Resin composition, multilayer structure, film, packaging material, pouch, secondary molded article, and method for producing resin composition
The resin composition, featuring EVOH, polyethylene resin with 1-hexene/1-octene units, and a polyolefin resin with a polar group, addresses the compatibility and property issues of recycled EVOH and polyolefin resins, achieving superior transparency and mechanical performance.
Patent Information
- Application Number
- PCT/JP2024/014203
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-17
AI Technical Summary
Recycled resin compositions made from EVOH and polyolefin resins exhibit poor compatibility and inferior appearance and mechanical properties, particularly when used as recycled raw materials, requiring further improvement in transparency and impact resistance.
A resin composition comprising EVOH, a polyethylene resin with specific structural units derived from 1-hexene and/or 1-octene, and a polyolefin resin with a polar group, optimized in terms of molecular weight, melt flow rate, and content ratios, to enhance compatibility and properties.
The resulting resin composition achieves excellent transparency and impact resistance, even when using recycled materials, with improved mechanical properties and appearance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Resin composition, multilayer structure, film, packaging material, pouch, secondary molded product, and method for producing resin composition
[0001] The present invention relates to a resin composition, a multilayer structure, a film, a packaging material, a pouch, a secondary molded product, and a method for producing a resin composition.
[0002] Ethylene-vinyl alcohol copolymers (hereinafter sometimes referred to as "EVOH"), polyolefin resins, and the like are generally used by being molded by a melt molding method into multilayer structures such as packaging films and containers for food and the like.
[0003] For the purpose of reducing the amount of plastic packaging waste and reducing the environmental load, used resin products using these EVOH and polyolefin resins, as well as resin scraps and ends generated in the manufacturing process of resin products, and defective products are collected and recycled into resin compositions containing EVOH and polyolefin from the collected products. However, since the EVOH and polyolefin resin in the resin composition obtained in this way are poorly compatible and have poor recyclability, a compatibilizer is added to improve the compatibility between EVOH and polyolefin resin.
[0004] For example, Patent Document 1 discloses a resin composition containing, as a compatibilizer, an ethylene-vinyl acetate copolymer and EVOH having an ethylene content of 70 mol% or more, in which the content of the EVOH is 1 to 30 parts by mass per 100 parts by mass of the ethylene-vinyl acetate copolymer.
[0005] Patent Document 2 also describes a polymeric composition containing a polyolefin, EVOH having an ethylene content of 20 to 60 mol% and a saponification degree of vinyl acetate units of 96% or more, a specific amount of a metal salt of a higher fatty acid having 8 to 22 carbon atoms, a conjugated polyene compound having a boiling point of 20°C or more, an ethylene-vinyl acetate copolymer (EVAc), and a saponified ethylene-vinyl acetate copolymer (S-EVOH) having an ethylene content of 68 to 98 mol% and a saponification degree of vinyl acetate units of 20% or more, and a weight ratio of the polyolefin to the EVOH. The resin composition disclosed has a ratio of 60:40 to 99.9:0.1, and contains a metal salt of a higher fatty acid in the range of 0.0001 to 10 parts by mass per 100 parts by mass of the total amount of polyolefin and EVOH, a conjugated polyene compound in the range of 0.000001 to 1 part by mass per 100 parts by mass of the total amount of polyolefin and EVOH, and EVAc and S-EVOH in a total amount of 0.3 parts by mass or more per 100 parts by mass of the total amount of polyolefin and EVOH.
[0006] JP 2009-97010 A International Publication No. 2010 / 079851
[0007] The techniques disclosed in Patent Documents 1 and 2 can improve the compatibility between EVOH and polyolefin resins, but are not sufficient, and further improvements are required in terms of appearance (transparency) and mechanical properties, particularly impact resistance. Furthermore, when a multilayer structure containing EVOH and polyolefin is used as a recycled raw material, the appearance and mechanical properties tend to be poor, so further improvements are required in terms of appearance and mechanical properties when recycled raw materials are used.
[0008] Therefore, the present invention provides a resin composition that is excellent in appearance and mechanical properties even when it contains EVOH and a polyolefin resin, and in particular, provides a resin composition that is excellent in transparency and mechanical properties even when EVOH or a polyolefin is used as a recycled raw material.
[0009] In view of the above circumstances, the present inventors have conducted extensive research and have found that the above problems can be solved by using EVOH, a polyethylene resin having a specific structural unit, a weight-average molecular weight, and a polyolefin resin containing a polar group and having a specific melt flow rate.
[0010] That is, the present invention has the following aspects. [1] A resin composition comprising EVOH (A), a polyethylene resin (B), and a polyolefin resin (C) having a polar group, wherein the polyethylene resin (B) contains structural units derived from 1-hexene and / or 1-octene, the polyethylene resin (B) has a weight-average molecular weight of 230,000 or more, and the polyolefin resin (C) having a polar group has a melt flow rate (190°C, 2160 g load) of 0.15 to 50 g / 10 min measured in accordance with JIS K7210:2014. [2] The resin composition according to [1], wherein the content ratio of EVOH (A) to polyethylene resin (B) [(A) / (B)] is 40 / 60 to 0.1 / 99.9 by mass. [3] The resin composition according to [1] or [2], wherein the content of structural units derived from 1-hexene and / or 1-octene in the polyethylene resin (B) is 2.0 mol% or more. [4] The density of the polyethylene resin (B) is 0.850 to 0.920 g / cm 3 [5] A multilayer structure having at least one layer comprising the resin composition according to any one of [1] to [4]. [6] A film comprising the resin composition according to any one of [1] to [4]. [7] A packaging material comprising the resin composition according to any one of [1] to [4]. [8] A pouch comprising the resin composition according to any one of [1] to [4]. [9] A secondary molded product comprising the resin composition according to any one of [1] to [4].
[10] A method for producing the resin composition according to any one of [1] to [4], comprising the step of mixing the EVOH (A), polyethylene resin (B), and polyolefin resin (C) having a polar group.
[0011] The resin composition of the present invention is excellent in transparency and impact resistance, and in particular, even when EVOH or polyolefin is used as a recycled raw material, the resin composition has excellent transparency and mechanical properties.
[0012] The present invention will be described in more detail below based on examples of the present invention, but the present invention is not limited to these examples.
[0013] In this specification, when "x to y" (x and y are any numbers) is used, it means "x or more and y or less," unless otherwise specified, and also includes "preferably greater than x" or "preferably smaller than y." Furthermore, when "x or more" (x is any number) is used, it also includes "preferably greater than x" unless otherwise specified, and when "y or less" (y is any number), it also includes "preferably smaller than y" unless otherwise specified. Furthermore, "x and / or y (x and y are any configurations)" means at least one of x and y, and can mean x only, y only, or both x and y. Regarding the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can be replaced with the value shown in the examples. Hereinafter, the monomer units contained in the copolymer resin may be simply referred to as "units." For example, a monomer unit based on ethylene may be referred to as an "ethylene unit."
[0014] A resin composition according to one embodiment of the present invention (hereinafter referred to as "the resin composition") contains EVOH (A), a polyethylene resin (B) having a specific structural unit, and a polyolefin resin (C) having a polar group. The EVOH (A), polyethylene resin (B), and polyolefin resin (C) having a polar group may be virgin products or recycled products. Of these, recycled products are preferred, and from the viewpoint of the effects of the present invention, it is particularly preferred to use a multilayer structure containing EVOH (A) and polyethylene resin (B), or scrap such as offcuts of a multilayer structure, as a raw material. Each component will be described below.
[0015] [EVOH (A)] The EVOH (A) is typically a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin. From an economical standpoint, vinyl acetate is generally used as the vinyl ester monomer. Polymerization of ethylene and a vinyl ester monomer can be carried out using any known polymerization method, such as solution polymerization, suspension polymerization, or emulsion polymerization, and solution polymerization using methanol as a solvent is generally used. The resulting ethylene-vinyl ester copolymer can also be saponified by a known method. EVOH (A) produced in this manner is primarily composed of ethylene-derived structural units and vinyl alcohol structural units, and typically contains a small amount of vinyl ester structural units remaining unsaponified.
[0016] As the vinyl ester monomer, vinyl acetate is typically used because of its commercial availability and the efficiency of impurity removal during production. Other vinyl ester monomers include, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate. Aliphatic vinyl esters having typically 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms, can be used. These can be used alone or in combination of two or more types.
[0017] The vinyl ester monomer is usually made from a petroleum-derived raw material such as naphtha, but it may also be made from a natural gas-derived raw material such as shale gas, or a plant-derived raw material purified from components such as sugar and starch contained in sugarcane, sugar beet, corn, potato, etc., or components such as cellulose contained in plants such as rice, wheat, and millet.
[0018] The ethylene unit content in EVOH (A) can be controlled by the ethylene pressure during copolymerization of the vinyl ester monomer with ethylene, and is preferably 20 to 60 mol%. It is more preferably 25 to 55 mol%, even more preferably 28 to 50 mol%, particularly preferably 30 to 45 mol%, and especially preferably 32 to 45 mol%. Furthermore, EVOH (A) preferably contains EVOH with such a content of 32 mol% or more, from the viewpoint of further improving mechanical properties and post-formability. If the content is too low, gas barrier properties and melt moldability under high humidity conditions tend to decrease, while if it is too high, gas barrier properties tend to decrease. The ethylene unit content can be measured, for example, according to ISO 14663.
[0019] The degree of saponification of the vinyl ester component in EVOH (A) can be controlled by the amount, temperature, time, etc. of a saponification catalyst (usually an alkaline catalyst such as sodium hydroxide is used) used when saponifying an ethylene-vinyl ester copolymer, and from the viewpoints of barrier property, thermal stability, and moisture resistance, it is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 98 mol% or more, and particularly preferably 99 mol% or more, and may even be 100 mol%. The degree of saponification of the vinyl ester unit of EVOH (A) is a value measured in accordance with JIS K6726 (wherein EVOH is a solution uniformly dissolved in a water / methanol solvent).
[0020] The melt flow rate (MFR) (210°C, 2160 g load) of EVOH (A) is usually 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, film-forming properties tend to become unstable, while if it is too low, the viscosity tends to become too high, making melt extrusion difficult. The MFR is an index of the degree of polymerization of EVOH (A) and can be adjusted by the amount of polymerization initiator and the amount of solvent used when copolymerizing ethylene and vinyl ester monomers.
[0021] EVOH (A) may be copolymerized with a polymerizable monomer other than ethylene and vinyl ester monomers within a range that does not impair the effects of the present invention, generally within a range of 5 mol % or less. Examples of such polymerizable monomers include α-olefins such as propylene, isobutene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, and 3-butene-1,2-diol, and hydroxyl-containing α-olefin derivatives such as esters and acylates thereof; hydroxymethylvinylidene diacetates such as 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyronyloxy-2-methylenepropane; unsaturated carboxylic acids or salts thereof, partial alkyl esters, complete alkyl esters, nitriles, amides, or anhydrides; unsaturated sulfonic acids or salts thereof; vinylsilane compounds; vinyl chloride; and styrene. These may be used alone or in combination of two or more.
[0022] The EVOH (A) used in the present invention may optionally be an EVOH having a primary hydroxyl group in the side chain. Examples of the EVOH having a primary hydroxyl group in the side chain include EVOH copolymerized with a hydroxy group-containing α-olefin and EVOH having a 1,2-diol structure in the side chain.
[0023] When EVOH having a primary hydroxyl group in a side chain is used, the content of the structural unit derived from the monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, and particularly preferably 1 to 10 mol % of the EVOH.
[0024] In the present invention, EVOH having no primary hydroxyl groups in the side chains is preferred.
[0025] Furthermore, as the EVOH (A), EVOH that has been "post-modified" by urethanization, acetalization, cyanoethylation, oxyalkylenation, or the like can also be used.
[0026] Only one type of EVOH (A) may be used, or two or more types differing in the type of vinyl ester, ethylene unit content, physical properties, etc. may be mixed and used. From the viewpoint of compatibility, it is preferable that only one type of EVOH is used, or when multiple types are used, it is preferable that all types have melting points of 170°C or higher, or all types have melting points of less than 170°C. In the present invention, the melting point is measured in accordance with the method described in JIS K7121 using a differential scanning calorimeter (DSC) by first heating a sample to 200°C, then cooling at a cooling rate of 30°C / min to a temperature about 50°C lower than the glass transition point, and then heating again at a heating rate of 10°C / min (second run).
[0027] The content of the EVOH (A) in the resin composition is usually 0.1 to 40% by mass, preferably 0.3 to 35% by mass, more preferably 0.5 to 30% by mass, and particularly preferably 0.7 to 25% by mass. When the content of EVOH (A) is within the above range, the molded product obtained tends to have a good appearance and excellent mechanical properties.
[0028] [Polyethylene Resin (B)] The polyethylene resin (B) used in the present invention contains structural units derived from ethylene and structural units derived from 1-hexene and / or 1-octene. When the polyethylene resin (B) contains structural units derived from 1-hexene and / or 1-octene, the mechanical properties can be improved.
[0029] The content of structural units derived from 1-hexene and / or 1-octene in the polyethylene resin (B) is preferably 2.0 mol% or more, more preferably 3.0 mol% or more, even more preferably 3.2 mol% or more, particularly preferably 3.4 mol% or more, and most preferably 3.6 mol% or more. There is no particular upper limit, but it is usually 15 mol%, preferably 13 mol%, more preferably 11 mol%, and particularly preferably 10 mol%. When the content of structural units derived from 1-hexene and / or 1-octene is within the above range, flexibility and mechanical properties tend to be good.
[0030] The density of the polyethylene resin (B) is 0.850 to 0.920 g / cm 3and preferably 0.860 to 0.920 g / cm 3 , more preferably 0.870 to 0.920 g / cm 3 , more preferably 0.880 to 0.920 g / cm 3 When the density is within the above range, the effects of the present invention tend to be easily obtained. The density can be measured with a densitometer.
[0031] Specific examples of the polyethylene resin (B) include, but are not limited to, linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, and high-density polyethylene. Examples of the polyethylene resin (B) also include modified polyethylene resins, such as unsaturated carboxylic acid-modified polyethylene resins obtained by graft-modifying polyethylene resins with unsaturated carboxylic acids or their esters. These may be used alone or in combination of two or more. Of these, linear low-density polyethylene is preferred. The raw material for the polyethylene resin may be derived from petroleum or plants.
[0032] The polyethylene resin (B) is obtained by polymerizing a copolymerization component containing ethylene and 1-hexene and / or 1-octene, but may contain an α-olefin other than 1-hexene and 1-octene as a copolymerization component.
[0033] Examples of the other α-olefins include α-olefins having 2 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-heptene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-ethyl-1-hexene, and 2,2,4-trimethyl-1-pentene. These may be used alone or in combination of two or more.
[0034] When the polyethylene resin (B) contains structural units derived from other α-olefins, the content thereof is usually 5 mol % or less, and preferably 2 mol % or less.
[0035] The weight average molecular weight of the polyethylene resin (B) is 230,000 or more, more preferably 235,000 or more, even more preferably 240,000 or more, particularly preferably 245,000 or more, especially preferably 250,000 or more, and most preferably 253,000 or more, in terms of polystyrene. The upper limit is not particularly limited, but is usually 400,000. When the weight average molecular weight of the polyethylene resin (B) is 230,000 or more in terms of polystyrene, the mechanical properties tend to be excellent. The weight average molecular weight of the polyethylene resin (B) can be measured by GPC.
[0036] The melt flow rate (MFR, 190°C, load 2160 g) of the polyethylene resin (B) measured in accordance with JIS K7210:2014 is not particularly limited, but from the viewpoint of moldability, it is usually 0.01 to 50 g / 10 min, more preferably 0.1 to 10 g / 10 min. The MFR can be measured using a melt indexer.
[0037] Commercially available polyethylene resins (B) suitable for use in the present invention include, for example, Innate (registered trademark) manufactured by The Dow Chemical Company, Exceed (registered trademark) manufactured by ExxonMobil Corporation, and Novatec (registered trademark) manufactured by Japan Polyethylene Corporation.
[0038] The content of the polyethylene resin (B) in the resin composition is usually 60 to 99.8 mass%, preferably 65 to 99.7 mass%, more preferably 70 to 99.5 mass%, and particularly preferably 75 to 99.3 mass%. When the content of the polyethylene resin (B) is within the above range, the obtained molded product tends to have good appearance and excellent mechanical properties.
[0039] The ratio of the EVOH (A) to the polyethylene resin (B) [(A) / (B)] by mass is preferably 40 / 60 to 0.1 / 99.9, more preferably 35 / 65 to 0.3 / 99.7, even more preferably 30 / 70 to 0.5 / 99.5, and particularly preferably 25 / 75 to 0.7 / 99.3. When the ratio of the polyethylene resin (B) to the EVOH (A) is within the above range, the molded product obtained tends to have a good appearance and excellent mechanical properties.
[0040] In the present resin composition, it is preferred that a sea-island structure be formed in which EVOH (A) is dispersed as an island phase in a sea phase (matrix) of polyethylene resin (B). When polyethylene resin (B) and EVOH (A) form a sea-island structure, the resulting molded article tends to have a good appearance and excellent mechanical properties.
[0041] [Polyolefin Resin (C) Having a Polar Group] Examples of the polyolefin resin containing a polar group include a polyolefin resin containing a carboxy group obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin by addition reaction, graft reaction, or the like.
[0042] Examples of the polyolefin resin having a carboxy group include maleic anhydride-modified polymers such as maleic anhydride-grafted polyethylene, maleic anhydride-grafted polypropylene, maleic anhydride-grafted ethylene-propylene (block and random) copolymers, maleic anhydride-grafted ethylene-ethyl acrylate copolymers, maleic anhydride-grafted ethylene-vinyl acetate copolymers, maleic anhydride-modified polycyclic olefin resins, and maleic anhydride-grafted polyolefin resins. These may be used alone or as a mixture of two or more.
[0043] As the polyolefin resin (C) having a polar group, maleic anhydride-modified polyolefin resins such as maleic anhydride-modified polyethylene and maleic anhydride-modified ethylene-α-olefin copolymer are particularly preferred, as they contribute to the effect of suppressing gel generation during melt heating and the effect of suppressing a decrease in transparency.
[0044] The melt flow rate (MFR, 190°C, 2160 g load) of the polar group-containing polyolefin resin (C), measured according to JIS K7210:2014, is 0.15 to 50 g / 10 min, preferably 0.4 to 40 g / 10 min, more preferably 0.7 to 30 g / 10 min, even more preferably 1 to 25 g / 10 min, and particularly preferably 1.2 to 20 g / 10 min. When the MFR of the polar group-containing polyolefin resin (C) is within the above range, the processability is excellent, and the resulting molded product has good appearance and excellent mechanical properties. On the other hand, when the melt flow rate of the polar group-containing polyolefin resin (C) is outside the above range, the processability, appearance, and mechanical properties are deteriorated.
[0045] The melt flow rate is expressed as a melt viscosity calculated from the following formula (1): MFR (190°C, load 2160g) = 3.6126[10 (log( η)−6.6928) / −1.1363]−9.31851 (1) where η is the melt viscosity at 350°F.
[0046] The acid value of the polar group-containing polyolefin resin (C) is usually 50 mgKOH / g or less, preferably 30 mgKOH / g or less, and particularly preferably 20 mgKOH / g or less. If the acid value is too high, the number of reaction sites with the hydroxyl groups in EVOH increases, resulting in the formation of highly polymerized products during the melt-kneading process, which reduces stability during extrusion processing and makes it difficult to obtain good molded products. The lower limit of the acid value is usually 1 mgKOH / g, preferably 2 mgKOH / g. The acid value is measured according to JIS K0070.
[0047] The content of the polyolefin resin (C) having a polar group in the resin composition is usually 0.1 to 40 mass%, preferably 0.3 to 35 mass%, more preferably 0.5 to 30 mass%, and particularly preferably 0.7 to 25 mass%. When the content of the polyolefin resin (C) having a polar group is within the above range, the molded product obtained tends to have good appearance and excellent mechanical properties.
[0048] The resin composition may contain other components besides those described above, such as antiblocking agents, processing aids, resins other than the EVOH (A), polyethylene resin (B), and polyolefin resin (C) having a polar group, carboxylic acid compounds, phosphoric acid compounds, boron compounds, metal salts, stabilizers, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, surfactants, desiccants, crosslinking agents, reinforcing agents such as various fibers, etc., as long as the effects of the present invention are not impaired. These may be used alone or in combination of two or more.
[0049] [Method for Producing Resin Composition] The resin composition can be produced by a production method including a step of mixing the EVOH (A), the polyethylene resin (B), the polyolefin resin (C) having a polar group, etc., such as a dry blending method, a melt mixing method, etc. These production methods can also be used in any combination.
[0050] As described above, the EVOH (A), the polyethylene resin (B), and the polyolefin resin (C) having a polar group may be virgin products or recycled products. In particular, it is particularly preferable to use, as raw materials, a multilayer structure containing the EVOH (A) and the polyethylene resin (B) or scraps such as scraps of the multilayer structure, in terms of the effects of the present invention.
[0051]
[0003] Generally, laminates comprising a layer containing EVOH and a layer containing polyethylene resin are widely used as packaging materials. When this laminate containing EVOH and polyethylene resin is recycled as it is to be used as a raw material for a resin composition, the compatibility between EVOH and polyethylene resin tends to be poor, resulting in poor appearance and mechanical properties. However, in the present invention, it has been found that the use of a specific polyethylene resin (B) and a polyolefin resin (C) having a polar group results in a good appearance and excellent mechanical properties.
[0052] When the recycled product is used, its content is 50% by mass or less, preferably 40% by mass or less, and particularly preferably 30% by mass or less of the resin composition. If the recycled product content is too high, the transparency and impact resistance tend to be poor.
[0053] The dry blending method may be, for example, (i) a method in which pellets of an EVOH resin (A), a polyethylene resin (B), and a polyolefin resin (C) having a polar group are dry blended using a tumbler or the like.
[0054] Examples of the melt-mixing method include (ii) a method of melt-kneading a dry blend obtained by dry-blending pelletized EVOH (A), polyethylene resin (B), and polyolefin resin (C) having a polar group, and (iii) a method of melt-kneading molten EVOH (A), polyethylene resin (B), and polyolefin resin (C) having a polar group.
[0055] As mentioned above, in the present invention, the above-mentioned different methods can be combined. Among them, the melt mixing method is preferred, and method (ii) is particularly preferred, in terms of productivity and the ability to obtain a resin composition in which the effects of the present invention are more pronounced. Furthermore, when using the other thermoplastic resins and other compounding agents, they may be compounded by a conventional method according to a known production method.
[0056] The resin composition obtained by each of the above-described production methods may have any shape, but is preferably in the form of pellets. The pellets may be, for example, spherical, oval, cylindrical, cubic, or rectangular, but are typically oval or cylindrical. From the viewpoint of convenience when subsequently used as a molding material, the size of the pellets is such that, in the case of an oval pellet, the minor axis is typically 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the major axis is typically 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. Furthermore, in the case of a cylindrical pellet, the diameter of the base is typically 1 to 6 mm, preferably 2 to 5 mm, and the length is typically 1 to 6 mm, preferably 2 to 5 mm. Furthermore, the pellet-shaped EVOH (A), polyethylene resin (B), and polyolefin resin (C) having a polar group used in each of the above-described production methods preferably have the same shape and size.
[0057] When the resin composition is in the form of pellets, it is also preferable to adhere a known lubricant to the surface of the pellets in order to stabilize the feedability during melt molding. Examples of lubricants include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, etc.; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, etc.; bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low-molecular-weight polyolefins (e.g., low-molecular-weight polyethylene or low-molecular-weight polypropylene having a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, and fluorinated ethylene resins. These compounds may be used alone or in combination of two or more. The content of such lubricants in the resin composition is usually 5% by mass or less, preferably 1% by mass or less. The lower limit is usually 0% by mass.
[0058] The resin composition thus obtained is excellent in transparency and impact resistance.
[0059] The total haze of the present resin composition is preferably 60% or less, more preferably 55% or less, and particularly preferably 50% or less. The total haze is determined by forming the present resin composition into a single-layer film having a thickness of 30 μm and measuring it using a haze meter.
[0060] The impact strength (g) of the present resin composition is preferably 50 g or more, more preferably 200 g or more, even more preferably 400 g or more, and particularly preferably 600 g or more. The impact strength (g) is the mass of the maximum weight that does not destroy the monolayer film when the present resin composition is formed into a monolayer film having a thickness of 30 μm, and a weight attached to a Bakelite dart (φ38 mm, 32 g) is dropped onto the monolayer film from a height of 0.66 m using a dart impact tester.
[0061] The resin composition is prepared in various forms, such as pellets, powder, or liquid, and is provided as a molding material for various molded products.
[0062] Examples of the molded article include a monolayer film molded from the present resin composition, as well as packaging materials, pouches, multilayer structures having at least one layer made of the present resin composition, etc. The molded article may also be subjected to secondary processing as described below to form a secondary processed product.
[0063] [Multilayer structure] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the multilayer structure") has at least one layer made of the resin composition. The layer made of the resin composition (hereinafter simply referred to as "the resin composition layer") can be laminated with a layer made of another resin composition containing a thermoplastic resin other than the resin composition as a main component (hereinafter simply referred to as "another resin layer") to impart further strength, protect the resin composition layer from the effects of moisture, etc., or impart other functions.
[0064] Examples of the thermoplastic resin include polyethylene resins such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-propylene (block and random) copolymers, and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and side chain); and polyolefins obtained by converting these polyolefins into unsaturated carboxylic acids. Examples of the polyolefin resin include polyolefin resins in the broad sense, including modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins graft-modified with carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.
[0065] Of these, hydrophobic resins such as polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred, and more preferred are polyolefin resins such as polyethylene resins, polypropylene resins, polycyclic olefin resins, and unsaturated carboxylic acid-modified polyolefin resins thereof.
[0066] The layer structure of the present multilayer structure can be any combination, such as a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, or b2 / b1 / a / b1 / a / b1 / b2, where a represents the resin composition layer and b represents the other resin layer. Furthermore, when R represents a recycled layer containing a mixture of the present resin composition and a thermoplastic resin other than the present resin composition, obtained by remelting and molding edges or defective products generated during the manufacturing process of the multilayer structure, the layer structure can also be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, or b / R / a / R / a / R / b. The total number of layers in the present multilayer structure is usually 2 to 15, and preferably 3 to 10. In the above layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the respective layers, if necessary.
[0067] Known adhesive resins can be used, and may be selected appropriately depending on the type of thermoplastic resin used in the other resin layer "b." Representative examples include carboxyl-containing modified polyolefin polymers obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin via addition reaction, graft reaction, or the like. Examples of the carboxyl-containing modified polyolefin polymers include maleic anhydride-grafted polyethylene, maleic anhydride-grafted polypropylene, maleic anhydride-grafted ethylene-propylene (block and random) copolymers, maleic anhydride-grafted ethylene-ethyl acrylate copolymers, maleic anhydride-grafted ethylene-vinyl acetate copolymers, maleic anhydride-modified polycyclic olefin resins, and maleic anhydride-grafted polyolefin resins. These may be used alone or in combination of two or more.
[0068] In the present multilayer structure, when an adhesive resin layer is used between the present resin composition layer and another resin layer, it is preferable to use an adhesive resin with excellent hydrophobicity, since the adhesive resin layers are located on both sides of the present resin composition layer.
[0069] The other resins and adhesive resins may contain conventionally known plasticizers, fillers, clays (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, waxes, etc., within a range that does not impair the spirit of the present invention (for example, 30% by mass or less, preferably 10% by mass or less, based on the total mass of the resin). These may be used alone or in combination of two or more.
[0070] The lamination of the present resin composition layer and the other resin layer (including the case where an adhesive resin layer is interposed) can be performed by a known method. For example, a method of melt-extrusion laminating another resin onto a film, sheet, etc. of the present resin composition, a method of melt-extrusion laminating the present resin composition onto another resin layer, a method of co-extruding the present resin composition with another resin, a method of dry-laminating the present resin composition (layer) with another resin composition or another resin layer using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, or a polyurethane compound, a method of applying a solution of the present resin composition onto another resin and then removing the solvent, etc. Among these, from the viewpoints of cost and environment, a manufacturing method including a step of melt-molding the present resin composition layer is preferred, and specifically, a co-extrusion method is preferred.
[0071] The multilayer structure may be subjected to a (heat) stretching treatment, if necessary. The stretching treatment may be either uniaxial stretching or biaxial stretching, and in the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. Furthermore, the stretching method may be a roll stretching method, tenter stretching method, tubular stretching method, stretch-blow method, vacuum pressure forming, or the like, whichever provides a higher stretch ratio. The stretching temperature is a temperature near the melting point of the multilayer structure, and is usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. If the stretching temperature is too low, the stretchability will be poor, and if it is too high, it will be difficult to maintain a stable stretched state.
[0072] The stretched multilayer structure may be heat-set to provide dimensional stability. Heat-setting can be performed by known means, for example, by subjecting the stretched multilayer structure to heat treatment while maintaining tension, typically at 80 to 180°C, preferably 100 to 165°C, for typically 2 to 600 seconds.
[0073] When the stretched multilayer structure is to be used as a shrink film, the heat-shrinkability can be imparted to the multilayer structure by, for example, cooling and fixing the multilayer structure by applying cold air thereto, without carrying out the heat-setting process described above.
[0074] The thickness of the present multilayer structure (including a stretched structure), as well as the thickness of the present resin composition layer, other resin layers, and adhesive resin layers constituting the multilayer structure, cannot be generally determined depending on the layer configuration, the type of other resin, the type of adhesive resin, the intended use, packaging form, required physical properties, etc., but the thickness of the present multilayer structure (including a stretched structure) is usually 10 to 5,000 μm, preferably 30 to 3,000 μm, and particularly preferably 50 to 2,000 μm. The present resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm. The other resin layers are usually 5 to 3,000 μm, preferably 10 to 2,000 μm, and particularly preferably 20 to 1,000 μm. The adhesive resin layers are usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.
[0075] Furthermore, the thickness ratio of the present resin composition layer to the other resin layers in the present multilayer structure (present resin composition layer / other resin layer), expressed as the ratio between the thickest layers when there are multiple layers of each type, is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60. Furthermore, the thickness ratio of the present resin composition layer to the adhesive resin layer (present resin composition layer / adhesive resin layer), expressed as the ratio between the thickest layers when there are multiple layers of each type, is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10.
[0076] The multilayer structure can also be used to produce multilayer containers such as cups, trays, packaging materials, and pouches. In this case, a drawing method is typically used, specifically vacuum forming, pressure forming, vacuum pressure forming, and plug-assisted vacuum pressure forming. Furthermore, blow molding is used to produce tube- or bottle-shaped multilayer containers (laminate structure) from a multilayer parison (a hollow tubular preform before blowing). Specific examples include extrusion blow molding (double-head, mold-moving, parison-shift, rotary, accumulator, horizontal parison, etc.), cold parison blow molding, injection blow molding, and biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection in-line biaxial stretch blow molding, etc.). Furthermore, the obtained multilayer container can be subjected to secondary processing such as heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making, deep drawing, box processing, tube processing, split processing, etc., as needed, to produce a secondary processed product.
[0077] Single-layer films formed from the present resin composition, and containers and lids formed from bags, cups, trays, tubes, bottles, packaging materials, pouches, etc. made from the present multilayer structure are useful as various packaging materials and containers for general foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc.
[0078] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following examples. Prior to the examples, the following materials were prepared.
[0079] <EVOH (A)> A1: "Soarnol (registered trademark) DC3203RB" manufactured by Mitsubishi Chemical Corporation (ethylene unit content 32 mol%, MFR 3.8 g / 10 min (210 ° C., load 2160 g), density 1.19 g / cm 3 ) <Polyethylene resin (B)> B1: ExxonMobil Corporation's "Exceed (registered trademark) 1012MA" (a copolymer of ethylene and 1-hexene, containing 3.9 mol% of structural units derived from 1-hexene, and having a density of 0.912 g / cm 3, MFR (190°C, load 2160 g) 1.0 g / 10 min, weight average molecular weight (polystyrene equivalent) 258,000) B2: ExxonMobil "Exceed (registered trademark) XP 8784" (ethylene and 1-hexene copolymer, content of structural units derived from 1-hexene 4.6 mol%, density 0.914 g / cm 3 , MFR (190 ° C, load 2160 g) 0.80 g / 10 min, weight average molecular weight (polystyrene equivalent) 269000) B3: "Innate (registered trademark) ST50" manufactured by Dow Chemical Company (ethylene and 1-octene copolymer, content of structural units derived from 1-octene 3.2 mol%, density 0.918 g / cm 3 , MFR (190 ° C, load 2160 g) 0.85 g / 10 min, weight average molecular weight (polystyrene equivalent) 251000) B4: "Innate (registered trademark) TH60" manufactured by The Dow Chemical Company (ethylene and 1-octene copolymer, content of structural units derived from 1-octene 4.0 mol%, density 0.912 g / cm 3 , MFR (190 ° C, load 2160 g) 0.85 g / 10 min, weight average molecular weight (polystyrene equivalent) 253000) B5: "Anteo (registered trademark) FK2715" manufactured by Borouge (ethylene and 1-hexene copolymer, content of structural units derived from 1-hexene 1.6 mol%, density 0.927 g / cm 3 , MFR (190°C, load 2160 g) 1.3 g / 10 min, weight average molecular weight (polystyrene equivalent) 240,000) B'1: "Novatec (registered trademark) UF641" manufactured by Japan Polyethylene Corporation (a copolymer of ethylene and 1-butene, density 0.927 g / cm 3 , MFR (190°C, load 2160 g) 2.1 g / 10 min, weight average molecular weight (polystyrene equivalent) 220,000) B'2: "Novatec (registered trademark) UF421" manufactured by Japan Polyethylene Co., Ltd. (ethylene and 1-butene copolymer, density 0.926 g / cm 3, MFR (190°C, load 2160 g) 0.9 g / 10 min, weight average molecular weight (polystyrene equivalent) 262000) B'3: "ELITE (registered trademark) 5400G" manufactured by The Dow Chemical Company (ethylene and 1-octene copolymer, content of structural units derived from 1-octene 3.6 mol%, density 0.916 g / cm 3 , MFR (190°C, load 2160 g) 1.0 g / 10 min, weight average molecular weight (polystyrene equivalent) 228000). The weight average molecular weight of the polyethylene resin (B) and the content of each copolymerization component are values measured by the evaluation method described below. <Polyolefin resin (C) having polar group> C1: "Modic (registered trademark) M533" manufactured by Mitsubishi Chemical Corporation (density 0.92 g / cm 3 , MFR (190°C, load 2160g) 2.5g / 10min)
[0080] Example 1 A dry blend of 5 parts by mass of EVOH (A1), 90 parts by mass of polyethylene resin composition (B1), and 5 parts by mass of polyolefin resin (C1) containing a polar group was melt-kneaded in a Φ40 mm single-screw extruder to obtain a resin composition. The obtained resin composition was used in a single-layer cast molding machine to produce a 30 μm single-layer film. The film-forming conditions were as follows: (Film-forming conditions) Φ40 mm single-screw extruder (barrel temperature: 220°C) Die temperature: 220°C Take-up speed: 2.0 to 2.5 m / min
[0081] Examples 2 to 5, Comparative Examples 1 to 3 Resin compositions of Examples 2 to 5 and Comparative Examples 1 to 3 were obtained in the same manner as in Example 1, except that the type of polyethylene resin (B) was changed as shown in Table 1 below. Furthermore, single-layer films having a thickness of 30 μm were produced from the obtained resin compositions of Examples 2 to 5 and Comparative Examples 1 to 3 in the same manner as in Example 1.
[0082] [Measurement of weight average molecular weight of polyethylene resin (B)] Each polyethylene resin was weighed and dissolved in 1,2,4-trichlorobenzene solvent by stirring at 140°C for 1 hour. Using the dissolved sample, high-temperature GPC measurement was carried out at 140°C. The calibration curve was prepared using standard polystyrenes manufactured by Tosoh Corporation (product numbers: 0005204, 0005205, 0005206, 0005207, 0005208, 0005209, 0005210, 0005211, 0005212, 0005213, 0005214, 0005215, 0005218, 0005220, 0005221). Therefore, the obtained value is the polystyrene-equivalent molecular weight.
[0083] [Structural Analysis of Polyethylene Resin (B)] Each polyethylene resin was weighed and dissolved in a heavy orthodichlorobenzene solvent at 130° C. The dissolved sample was used to perform structural analysis at 120° C. 13 The C NMR spectrum was measured, with the signal of the polyethylene resin main chain set at 30.0 ppm as the chemical shift reference.
[0084] The resulting monolayer films of Examples 1 to 5 and Comparative Examples 1 to 3 were evaluated for total haze and impact strength as described below. The results are shown in Table 1 below.
[0085] [Evaluation of Total Haze] The total haze of the monolayer film was measured using a haze meter ("NDH4000" manufactured by Nippon Denshoku Industries Co., Ltd.) The lower the value, the better the transparency.
[0086] [Evaluation of Impact Strength (Dart Impact)] Using a Dart Impact Tester (manufactured by Toyo Seiki Co., Ltd.), a Bakelite dart (Φ38 mm, 32 g) with a weight attached was dropped onto the monolayer film from a height of 0.66 m. The appearance of the monolayer film after the dart was visually confirmed, and the weight of the maximum weight at which no damage was observed was taken as the dart impact strength of the monolayer film.
[0087]
[0088] The results in Table 1 show that Examples 1 to 5, which used the specific polyethylene resin (B), were superior in transparency and impact strength compared to Comparative Examples 1 and 2, which used a polyethylene resin that did not contain structural units derived from 1-hexene and / or 1-octene. Furthermore, Comparative Example 3, which used a polyethylene resin that contained structural units derived from 1-hexene and / or 1-octene but had a weight-average molecular weight outside the specific range, exhibited poor total haze and was unable to achieve both transparency and mechanical properties.
[0089] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.
[0090] The present resin composition has excellent transparency and impact strength, and therefore can be suitably used as a packaging material, such as various packaging containers and packaging films, for general foods as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc.
Claims
1. A resin composition comprising an ethylene-vinyl alcohol copolymer (A), a polyethylene resin (B), and a polyolefin resin (C) having a polar group, wherein the polyethylene resin (B) contains structural units derived from 1-hexene and / or 1-octene, the weight average molecular weight of the polyethylene resin (B) is 230,000 or more, and the melt flow rate (190°C, load 2160 g) of the polyolefin resin (C) having a polar group measured in accordance with JIS K7210:2014 is 0.15 to 50 g / 10 min.
2. The resin composition according to claim 1, wherein the content ratio of the ethylene-vinyl alcohol copolymer (A) to the polyethylene resin (B) [(A) / (B)] is 40 / 60 to 0.1 / 99.9 by mass.
3. The resin composition according to claim 1 or 2, wherein the content of structural units derived from 1-hexene and / or 1-octene in the polyethylene resin (B) is 2.0 mol % or more.
4. The density of the polyethylene resin (B) is 0.850 to 0.920 g / cm 3 The resin composition according to claim 1 or 2, 5. A multilayer structure having at least one layer containing the resin composition according to claim 1 or 2.
6. A film comprising the resin composition according to claim 1 or 2.
7. A packaging material comprising the resin composition according to claim 1 or 2.
8. A pouch comprising the resin composition according to claim 1 or 2.
9. A secondary molded product comprising the resin composition according to claim 1 or 2.
10. A method for producing the resin composition according to claim 1 or 2, comprising the step of mixing the ethylene-vinyl alcohol copolymer (A), the polyethylene resin (B), and the polyolefin resin (C) having a polar group.
Citation Information
Patent Citations
Resin composition, molding resin composition prepared by using the same, laminate, and method for producing laminate thereof
JP2009097010A
Resin composition and multilayer structure using same
WO2010079851A2
Polyolefin multilayer thermally shrinkable film
JP1999254610A
Injection molded article
JP2002249595A
Photosensitive transfer material, method for producing resin pattern, method for producing circuit wiring, and method for producing touch panel
WO2022059418A1