Adhesive sheet, laminate, and release sheet-attached adhesive sheet
The adhesive sheet, with a specific adhesive layer composition and gel fraction, addresses the issue of peeling on metal or metal oxide surfaces by providing strong and durable adhesion, preventing peeling and corrosion.
Patent Information
- Application Number
- PCT/JP2024/014615
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Adhesive sheets used on surfaces with metal or metal oxides tend to peel off easily due to thermal shrinkage, posing a challenge for reliable bonding.
A pressure-sensitive adhesive sheet with an adhesive layer composed of an acrylic polymer and a silane coupling agent, featuring an epoxy group, chelate functional group, or a mercapto group, with a gel fraction of 70% to 97%, which provides strong adhesion to metal or metal oxide surfaces without peeling.
The adhesive sheet effectively prevents peeling and corrosion on metal or metal oxide surfaces, ensuring durable bonding and improved adhesion, even under thermal stress.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Adhesive sheet, laminate, and adhesive sheet with release sheet
[0001] The present invention relates to a pressure-sensitive adhesive sheet, a laminate, and a pressure-sensitive adhesive sheet with a release sheet.
[0002] The pressure-sensitive adhesive sheet is a material formed with a pressure-sensitive adhesive layer whose main component is, for example, an acrylic polymer, and is used for bonding various optical components such as light-control films, touch panels, liquid crystal displays (LCDs), etc. When the pressure-sensitive adhesive layer is of an active energy ray-curable type, the pressure-sensitive adhesive layer is further cured by irradiating the pressure-sensitive adhesive layer with active energy rays such as UV, and various components (adherends) can be bonded together with high adhesive strength.
[0003] The pressure-sensitive adhesive sheet may be used by being attached to a substrate (e.g., a film with ITO) having a surface on which a metal oxide such as ITO (indium tin oxide) is formed. For example, Patent Document 1 describes a technology relating to a surface protection film that is attached to a surface on which ITO is formed.
[0004] JP 2013-72068 A
[0005] However, since a substrate (e.g., a resin film) having a surface on which a metal or metal oxide is formed tends to shrink due to heat, a pressure-sensitive adhesive sheet attached to the surface on which the metal or metal oxide is formed is likely to peel off from the surface. From this perspective, there has been a demand for a pressure-sensitive adhesive sheet that is less likely to peel off even when attached to a surface on which a metal or metal oxide is formed.
[0006] The present invention has been made in view of the above, and aims to provide an adhesive sheet that is less likely to peel off even when attached to a surface on which a metal or metal oxide is formed.
[0007] As a result of extensive research to achieve the above object, the inventors have discovered that the above object can be achieved by applying an adhesive layer formed using a specific adhesive composition to an adhesive sheet, and have thus completed the present invention.
[0008] That is, the present invention encompasses, for example, the subject matter described in the following items. Item 1: A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer contains an acrylic polymer and a silane coupling agent, the silane coupling agent having an epoxy group, a chelating functional group, a mercapto group, or a mercapto group protected by a protecting group, and the pressure-sensitive adhesive layer has a gel fraction of 70% or more and 97% or less. Item 2: The pressure-sensitive adhesive sheet according to Item 1, wherein the acrylic polymer has a content of carboxyl group-containing monomer units of 0.1% by mass or less. Item 3: The pressure-sensitive adhesive sheet according to Item 1 or 2, which is used for bonding to a surface having a metal or metal oxide. Item 4: The pressure-sensitive adhesive sheet according to Item 3, wherein the surface having a metal or metal oxide is a surface having indium tin oxide. Item 5: A laminate comprising the pressure-sensitive adhesive sheet according to any one of Items 1 to 4, wherein a first adherend having a metal or metal oxide surface is bonded to one surface thereof, and a second adherend made of a resin plate or glass is bonded to the other surface thereof. Item 6. A pressure-sensitive adhesive sheet with a release sheet, comprising the pressure-sensitive adhesive sheet according to any one of items 1 to 4 and a release sheet.
[0009] The pressure-sensitive adhesive sheet of the present invention is unlikely to peel off from a surface on which a metal or metal oxide is formed, even when the pressure-sensitive adhesive sheet is attached to the surface.
[0010]
[0023] In the present specification, the terms "contain" and "comprise" include the concepts of "contain," "comprise," "consist essentially of," and "consist only of."
[0011] 1. Pressure-sensitive adhesive sheet The pressure-sensitive adhesive sheet of the present invention includes a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer containing an acrylic polymer and a silane coupling agent, the silane coupling agent having an epoxy group, a chelating functional group, a mercapto group, or a mercapto group protected by a protecting group, and the pressure-sensitive adhesive layer having a gel fraction of 70% or more and 97% or less.
[0012] The pressure-sensitive adhesive sheet of the present invention is unlikely to peel off from a surface on which a metal or metal oxide is formed, even when the pressure-sensitive adhesive sheet is attached to the surface, and therefore can be suitably used for attachment to an adherend having a surface on which a metal or metal oxide is formed.
[0013] The pressure-sensitive adhesive layer contains at least an acrylic polymer and a silane coupling agent. Hereinafter, the acrylic polymer contained in the pressure-sensitive adhesive layer will be referred to as acrylic polymer (P1).
[0014] (Acrylic Polymer) The acrylic polymer (P1) can be, for example, a wide range of known acrylic polymers used to form pressure-sensitive adhesive sheets. For example, the acrylic polymer (P1) can be a polymer of a (meth)acrylic acid ester and a monomer having a crosslinkable functional group that is copolymerizable with the (meth)acrylic acid ester. That is, the acrylic polymer (P1) can contain a (meth)acrylic acid ester unit and a monomer unit having a crosslinkable functional group.
[0015] In this specification, "(meth)acrylic" means "acrylic" or "methacrylic", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)allyl" means "allyl" or "methallyl".
[0016] Examples of (meth)acrylic acid esters include (meth)acrylates having a linear or branched alkyl group, and (meth)acrylates having a ring structure. When the (meth)acrylate has a linear or branched alkyl group, the number of carbon atoms therein can be, for example, 1 to 20, preferably 1 to 15, and more preferably 2 to 10. When the (meth)acrylate has an aromatic ring, the number of carbon atoms therein can be, for example, 5 to 20, preferably 6 to 10.
[0017] Specific examples of (meth)acrylates having a linear or branched alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isopropyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate.
[0018] The (meth)acrylate having a ring structure is preferably a (meth)acrylic monomer having an alicyclic or aromatic ring, and more preferably a (meth)acrylic monomer having an alicyclic ring. Examples of the alicyclic ring include cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, cyclododecane, norbornene, norbornadiene, dicyclopentane, tetrahydrofuran, and tetrahydropyran. The alicyclic ring may have a spiro structure. Examples of the aromatic ring include benzene, naphthalene, anthracene, pyridine, furan, benzofuran, pyrrole, thiophene, imidazole, and oxazole. Among these, the ring structure is preferably an alicyclic ring, more preferably at least one selected from cyclohexane, dicyclopentane, isobornyl, and benzene, and particularly preferably cyclohexane. The above-mentioned ring structure may further have a substituent. Examples of the substituent include substitutable substituents selected from a halogen atom, a halogenated alkyl group, an alkyl group, an alkenyl group, an acyl group, a hydroxy group, a hydroxyalkyl group, an alkoxy group, an aryl group, a heteroaryl group, an alicyclic group, a cyano group, an epoxy group, an oxetanyl group, a mercapto group, an amino group, and a (meth)acryloyl group.
[0019] The (meth)acrylate having a ring structure preferably has a structure in which a functional group having a ring structure is bonded to an ester oxygen of the (meth)acrylate, and in this case, the functional group having a ring structure preferably has 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 4 to 8 carbon atoms.
[0020] Specific examples of the (meth)acrylate having a ring structure include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, O-phenylphenoxyethyl (meth)acrylate, etc. Among these, the (meth)acrylate having a ring structure is preferably one or more selected from the group consisting of cyclohexyl (meth)acrylate and isobornyl (meth)acrylate, and more preferably cyclohexyl (meth)acrylate.
[0021] The (meth)acrylic acid ester constituting the acrylic polymer (P1) is preferably at least one selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isopropyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate.
[0022] The (meth)acrylic acid ester unit contained in the acrylic polymer (P1) may be of one type alone or may be of two or more types.
[0023] On the other hand, the monomer for constituting the monomer unit having a crosslinkable functional group can be a wide variety of monomers other than the (meth)acrylic acid esters and having a crosslinkable functional group in the molecule. The type of the crosslinkable functional group is not particularly limited, and examples thereof include a carboxyl group, a hydroxyl group, an amino group, and a glycidyl group.
[0024] Examples of the monomer having a crosslinkable functional group in the molecule include a carboxyl group-containing monomer, a hydroxy group-containing monomer, an amino group-containing (meth)acrylate unit, and a glycidyl group-containing (meth)acrylate unit. More specifically, examples of the monomer having a crosslinkable functional group in the molecule include a carboxyl group-containing (meth)acrylate unit, a hydroxy group-containing (meth)acrylate unit, an amino group-containing (meth)acrylate unit, and a glycidyl group-containing (meth)acrylate unit.
[0025] Examples of the carboxyl group-containing (meth)acrylate include acrylic acid and methacrylic acid.
[0026] Examples of hydroxy group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2,2-dimethyl-2-hydroxyethyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and polyalkylene glycol mono(meth)acrylate.
[0027] Examples of the amino group-containing (meth)acrylate include (meth)acrylamide, allylamine, etc. Examples of the glycidyl group-containing (meth)acrylate unit include glycidyl (meth)acrylate, etc.
[0028] The monomer for constituting the monomer unit having a crosslinkable functional group is more preferably a hydroxy group-containing (meth)acrylate, and in particular, the hydroxy group-containing (meth)acrylate is preferably at least one selected from the group consisting of 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate.
[0029] Furthermore, the acrylic polymer (P1) preferably has a content of carboxyl group-containing monomer units of 0.1% by mass or less. In this case, the pressure-sensitive adhesive sheet of the present invention is particularly resistant to peeling even when bonded to a surface on which a metal or metal oxide is formed, and is also resistant to corrosion. The carboxyl group-containing monomer unit refers to a structural unit formed when a carboxyl group-containing monomer is polymerized. In order to easily suppress corrosion of the pressure-sensitive adhesive sheet when bonded to a surface on which a metal or metal oxide is formed, the content of the carboxyl group-containing monomer units in the acrylic polymer (P1) is preferably 0.05% by mass or less, and more preferably 0.01% by mass or less.
[0030] The acrylic polymer (P1) more preferably contains substantially no carboxyl group-containing monomer units, and even more preferably contains 0 mass% of carboxyl group-containing monomer units (i.e., no carboxyl group-containing monomer units are detected).
[0031] The acrylic polymer (P1) may contain one or more types of monomer units having a crosslinkable functional group.
[0032] In the acrylic polymer (P1), the content ratio of the (meth)acrylic acid ester unit and the monomer unit having a crosslinkable functional group is not particularly limited. For example, the acrylic polymer (P1) preferably contains 40% by mass or more of the (meth)acrylic acid ester unit, more preferably 50% by mass or more, even more preferably 60% by mass or more, particularly preferably 65% by mass or more, and also preferably contains 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less, particularly preferably 80% by mass or less. In these cases, the remaining monomer units of the acrylic polymer are preferably monomer units having a crosslinkable functional group, and are preferably hydroxyl group-containing (meth)acrylate units.
[0033] The acrylic polymer (P1) preferably contains a structural unit derived from the (meth)acrylate having the aforementioned ring structure. In this case, the pressure-sensitive adhesive sheet of the present invention has better adhesion to the adherend. When the acrylic polymer (P1) contains a structural unit derived from the (meth)acrylate having the aforementioned ring structure, the content ratio thereof is, for example, preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, and preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less, relative to the total mass of the acrylic polymer (P1).
[0034] The acrylic polymer (P1) may contain other monomer units other than those described above, as long as the effects of the present invention are not impaired. The content of the other monomer units may be 20% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The acrylic polymer may be composed only of (meth)acrylic acid ester units and monomer units having a crosslinkable functional group. The proportion (molar ratio) of each structural unit in the acrylic polymer can be considered to be the same as the molar ratio of each monomer used in producing the polymer.
[0035] The weight-average molecular weight of the acrylic polymer (P1) is preferably greater than 10,000, more preferably at least 100,000, and even more preferably at least 200,000. The weight-average molecular weight of the acrylic polymer (P1) is preferably at most 2,000,000, more preferably at most 1,500,000, and even more preferably at most 1,200,000.
[0036] The weight-average molecular weight referred to in the present invention refers to the weight-average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC). There are no particular limitations on the GPC apparatus used in the GPC method, and commercially available GPC measuring instruments, such as the LC-2000Plus series manufactured by JASCO Corporation, and detectors such as RI-2031Plus and UV-2075Plus, can be used. In this case, for example, a GPC column consisting of four columns connected together, namely, "Shodex KF801," "Shodex KF803L," "Shodex KF800L," and "Shodex KF800D" manufactured by Showa Denko K.K., can be used. The column temperature can be set to 40°C. Tetrahydrofuran is used as the eluent, and measurements are performed at a flow rate of 1.0 ml / min. Typically, a calibration curve is prepared using standard polystyrene, and the weight-average molecular weight (Mw) can be obtained in terms of polystyrene.
[0037] The acrylic polymer (P1) may be a random copolymer, or may have other structures such as a block polymer.
[0038] The acrylic polymer (P1) can be produced by a known method. For example, the acrylic polymer can be produced by polymerizing a monomer mixture for forming each structural unit by a known polymerization method. As the polymerization method, for example, solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, etc. can be used. The acrylic polymer can also be obtained from a commercially available product, etc.
[0039] The glass transition temperature (Tg) of the acrylic polymer (P1) is not particularly limited, and may be, for example, 0° C. or lower, preferably −10° C. or lower, more preferably −20° C. or lower, and even more preferably −30° C. or lower. The glass transition temperature of the acrylic polymer (P1) is, for example, preferably −80° C. or higher, more preferably −70° C. or higher, and even more preferably −60° C. or higher.
[0040] The method for adjusting the glass transition temperature of the acrylic polymer (P1) is not particularly limited, and the glass transition temperature can be adjusted to a desired range by, for example, changing the type and composition ratio of the monomers constituting the acrylic polymer (P1). In the present invention, the glass transition temperature of the acrylic polymer (P1) refers to Tg, which is calculated by the following Fox formula based on the composition of the monomers used in synthesizing the copolymer. Fox formula: 1 / Tg = (W1 / Tg1) + (W2 / Tg2) + ... + (Wm / Tgm), where W1 + W2 + ... + Wm = 1. In the formula, Tg is the glass transition temperature (unit: K) of the acrylic polymer (P1), Tg1, Tg2, ..., Tgm are the glass transition temperatures of the respective homopolymers of the m types of monomers (m is an integer) constituting the acrylic polymer (P1), and W1, W2, ..., Wm are the mass fractions of the respective structural units in the acrylic polymer (P1). Note that Tg1 and W1 correspond to each other, i.e., the monomer that constitutes the homopolymer exhibiting the glass transition temperature of Tg1 is the same as the monomer that forms the structural unit having the mass fraction of W1. Similarly, Tg2 and W2, ... Tgm and Wm correspond to each other.
[0041] The glass transition temperature of the homopolymer can be, for example, the value described in the Polymer Handbook 4th Edition (Wiley-Interscience 2003). If no such handbook is available, the glass transition temperature of the homopolymer can be measured, for example, by a differential scanning calorimeter (DSC). The DSC measurement conditions are as follows: 5 mg of sample in a nitrogen atmosphere; in the first measurement (1st RUN), the sample is heated from -100°C to 200°C at a heating rate of 5°C / min, then cooled to -100°C at a cooling rate of 5°C / min; and in the second measurement (2nd RUN), the sample is heated from -100°C to 200°C at a heating rate of 5°C / min. Here, the glass transition temperature refers to the intersection of an extension of the baseline on the lower temperature side of the region where the baseline of a DSC curve measured when the temperature is raised from −100° C. to 200° C. changes to a sigmoid shape in the endothermic direction, and a tangent to an inflection point in the sigmoid.
[0042] The acrylic polymer (P1) may be in the form of a solution (also called a syrup) in which it is dissolved in a polymerizable monomer M. Note that such a syrup may also include a form in which the acrylic polymer (P1) is a partial polymer obtained by partial bulk polymerization. In this case, the polymer fraction is not particularly limited. The polymer fraction is the content (% by mass) of the resin component relative to the total mass of the resin component (acrylic polymer (P)) and the monomer. The polymer fraction can be, for example, 1 to 80% by mass, and preferably 5 to 50% by mass.
[0043] The polymerizable monomer M preferably has the same composition as the monomer composition constituting the monomer units contained in the acrylic polymer (P1). Therefore, when the acrylic polymer (P1) is in the form of a solution (syrup) dissolved in the polymerizable monomer M, the content of the carboxyl group-containing monomer in the polymerizable monomer M is preferably 0.1% by mass or less. In this case, the pressure-sensitive adhesive sheet of the present invention is particularly resistant to peeling even when attached to a surface on which a metal or metal oxide is formed, and is also resistant to corrosion. The content of the carboxyl group-containing monomer in the polymerizable monomer M is preferably 0.05% by mass or less, and more preferably 0.01% by mass or less. It is more preferable that the polymerizable monomer M is substantially free of a carboxyl group-containing monomer, and even more preferably that the content of the carboxyl group-containing monomer is 0% by mass (i.e., no carboxyl group-containing monomer is detected).
[0044] (Silane Coupling Agent) The silane coupling agent has an epoxy group, a chelating functional group, a mercapto group, or a mercapto group protected by a protecting group. Specific examples of the silane coupling agent include alkoxysilanes having two or more, preferably three or more, alkoxy groups. In the alkoxysilane, the alkoxy group may be, for example, an alkoxy group having 1 to 6 carbon atoms, and among these, a methoxy group and an ethoxy group are preferred.
[0045] Examples of silane coupling agents having an epoxy group include a wide variety of known epoxy silane coupling agents. Specific examples include alkoxysilanes having an epoxy group, in which case the epoxy group is preferably located at the end of the molecule. Examples of alkoxysilanes having an epoxy group include 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 3-glycidoxypropyltrimethoxysilane. Commercially available alkoxysilanes having an epoxy group include Shin-Etsu Silicone KBE-402, KBE-403, KBM-303, KBE-402, and KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.
[0046] Examples of silane coupling agents having a chelating functional group include known chelating functional group-type silane coupling agents. Specific examples include N-2-pyridinyl-N'-[3-(trimethoxysilyl)propyl]-urea and [3-trimethoxysilyl)propyl]butane-thiourea. Commercially available alkoxysilanes having a chelating functional group include Shin-Etsu Silicone X-12-989MS and X-12-1116 manufactured by Shin-Etsu Chemical Co., Ltd.
[0047] Examples of silane coupling agents having a mercapto group include a wide variety of known mercapto-based silane coupling agents. Specific examples include alkoxysilanes having a mercapto group, in which case the mercapto group is preferably located at the end of the molecule. Examples of alkoxysilanes having a mercapto group include 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, and mercaptomethyltrimethoxysilane, and may also include alkoxy oligomers having a mercapto group. Commercially available alkoxysilanes having a mercapto group include Shin-Etsu Silicone X-12-1307, X-41-1810, X-41-1805, KBM-802, and KBM-803 manufactured by Shin-Etsu Chemical Co., Ltd.
[0048] In a silane coupling agent having a mercapto group protected by a protecting group, the term "mercapto group protected by a protecting group" can mean that the hydrogen atom of the mercapto group (-SH) is protected by a protecting group. The protecting group can be, for example, -Si(OR) 3 where OR is an alkoxy group, such as a methoxy group or an ethoxy group. Examples of the silane coupling agent having a mercapto group protected by a protecting group include alkoxysilanes having a mercapto group protected by a protecting group, such as triethoxysilylthiopropyltrimethoxysilane ((CH 3 O) 3 Si(CH 2 ) 3 S-Si(OC 2 H 5 ) 3 An example of a commercially available alkoxysilane having a mercapto group protected by a protecting group is Shin-Etsu Silicone X-12-1056ES manufactured by Shin-Etsu Chemical Co., Ltd.
[0049] The silane coupling agent preferably has an epoxy group, a chelating functional group, or a mercapto group protected by a protecting group, more preferably an alkoxysilane having an epoxy group, a chelating functional group, or a mercapto group protected by a protecting group, and particularly preferably an alkoxysilane having a mercapto group protected by a protecting group.
[0050] The silane coupling agent may contain other silane coupling agents in addition to the silane coupling agent having an epoxy group, a chelating functional group, a mercapto group, or a mercapto group protected by a protecting group, or the silane coupling agent may consist solely of a silane coupling agent having an epoxy group, a chelating functional group, a mercapto group, or a mercapto group protected by a protecting group.
[0051] The content of the silane coupling agent in the pressure-sensitive adhesive composition is not particularly limited. In order to easily improve the adhesion of the pressure-sensitive adhesive sheet to the adherend, the content of the silane coupling agent is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, particularly preferably 0.3 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, relative to 100 parts by mass of the total mass of the acrylic polymer (P1) and the polymerizable monomer M.
[0052] (Tackifier) The pressure-sensitive adhesive layer may contain a tackifier. In this case, the pressure-sensitive adhesive sheet is likely to have increased adhesive strength to a surface on which a metal or metal oxide is formed, and is likely to have excellent adhesion.
[0053] The type of tackifier is not particularly limited, and for example, a wide variety of tackifiers used in known PSA sheets can be used. For example, the tackifier can include an acrylic polymer (P2) different from the acrylic polymer (P1).
[0054] The type of acrylic polymer (P2) is not particularly limited, and examples thereof include a wide range of tackifier resins contained in known PSA sheets. Note that the acrylic polymer (P2) is different from the above-mentioned acrylic polymer (P1).
[0055] The acrylic polymer (P2) may be a resin having a glass transition temperature of 20° C. or higher, preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher. The glass transition temperature of the acrylic polymer (P2) is preferably 200° C. or lower, more preferably 180° C. or lower, and even more preferably 150° C. or lower. By adjusting the glass transition temperature of the acrylic polymer (P2) to fall within the above range, the adhesion of the PSA sheet to the adherend can be improved.
[0056] The acrylic polymer (P2) may contain a monomer unit having an alicyclic ring as a constituent unit. When the acrylic polymer (P2) contains a monomer unit having an alicyclic ring, the number of carbon atoms constituting the alicyclic ring is preferably 6 or more. Examples of the alicyclic ring having 6 or more carbon atoms include cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, cyclododecane, norbornene, norbornadiene, and dicyclopentane.
[0057] As the monomer having an alicyclic ring, for example, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, etc. can be preferably used.
[0058] The acrylic polymer (P2) can contain alkyl(meth)acrylate units in place of or in addition to the alicyclic monomer units. Examples of alkyl(meth)acrylates include alkyl(meth)acrylates such as methyl(meth)acrylate, ethyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, nonyl(meth)acrylate, decyl(meth)acrylate, lauryl(meth)acrylate, cetyl(meth)acrylate, stearyl(meth)acrylate, and behenyl(meth)acrylate. Among these, it is preferable that the acrylic polymer (P2) contains methyl(meth)acrylate.
[0059] The acrylic polymer (P2) is preferably a copolymer containing both an alicyclic monomer unit and an alkyl(meth)acrylate unit. In this case, the content of the alkyl(meth)acrylate unit relative to the total mass of the acrylic polymer (P2) is preferably 10% by mass or more, more preferably 15% by mass or more, in order to easily improve the adhesion between the pressure-sensitive adhesive sheet and the adherend. Also, it is preferably 95% by mass or less, more preferably 90% by mass or less.
[0060] The acrylic polymer (P2) may contain other monomer units as needed. The other monomers may be any monomers copolymerizable with the alkyl (meth)acrylates, such as (meth)acrylonitrile, vinyl acetate, vinyl chloride, and ethyl vinyl ether. The content of the other monomer units in the acrylic polymer (P2) is preferably 10% by mass or less, and more preferably 5% by mass or less.
[0061] The acrylic polymer (P2) preferably has substantially no crosslinkable functional groups, because in this case, the acrylic polymer (P2) does not form a crosslinked structure with the above-mentioned (meth)acrylic polymer.
[0062] The weight average molecular weight of the acrylic polymer (P2) is preferably 3,000 or more, more preferably 3,200 or more, and even more preferably 3,500 or more. The weight average molecular weight of the acrylic polymer (P2) may be 10,000 or less, more preferably 9,000 or less, and even more preferably 8,000 or less. The weight average molecular weight of the acrylic polymer (P2) is measured by gel permeation chromatography (GPC) and converted using a calibration curve prepared using standard polystyrenes with known molecular weights. Such resins may be commercially available or may be synthesized by known methods.
[0063] The content of the tackifier in the pressure-sensitive adhesive layer is not particularly limited. In order to easily improve the adhesion of the pressure-sensitive adhesive sheet to an adherend, the content of the tackifier is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 4 parts by mass or more, and particularly preferably 5 parts by mass or more, relative to 100 parts by mass of the total mass of the acrylic polymer (P1) and the polymerizable monomer M, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less.
[0064] In this specification, "the total mass of the acrylic polymer (P1) and the polymerizable monomer M" can be read as "the total mass of the acrylic polymer (P1)" when the acrylic polymer (P1) is not in the form of the above-mentioned syrup, since the polymerizable monomer M is not contained therein.
[0065] The content of the acrylic polymer (P2) in the pressure-sensitive adhesive layer is not particularly limited. In order to easily improve the adhesion of the pressure-sensitive adhesive sheet to an adherend, the content of the acrylic polymer (P2) is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 4 parts by mass or more, and particularly preferably 5 parts by mass or more, relative to 100 parts by mass of the total mass of the acrylic polymer (P1) and the polymerizable monomer M, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less.
[0066] The tackifier may be formed solely from the acrylic polymer (P2), or may contain components other than the acrylic polymer (P2). The acrylic polymer (P2) contained in the pressure-sensitive adhesive layer may be one type alone or two or more types.
[0067] <Adhesive Composition> The adhesive layer can be formed using an adhesive composition. For example, the adhesive layer can be formed by curing the adhesive composition, that is, the adhesive layer includes a cured product of the adhesive composition. When the adhesive composition is an active energy ray-curable adhesive described below, the adhesive layer can be formed by irradiating the adhesive with active energy rays to cure it.
[0068] The pressure-sensitive adhesive composition contains the acrylic polymer (acrylic polymer (P1)) and the silane coupling agent as essential components, and can also contain one or more selected from the group consisting of the tackifier, monofunctional monomer, polyfunctional monomer, and crosslinking agent.
[0069] (Monofunctional Monomer) The pressure-sensitive adhesive composition may contain a monofunctional monomer. In particular, when the pressure-sensitive adhesive composition is an active energy ray-curable pressure-sensitive adhesive described below, it preferably contains a monofunctional monomer.
[0070] The type of monofunctional monomer is not particularly limited, and examples thereof include a wide range of monofunctional monomers used to produce known pressure-sensitive adhesive sheets. Among them, it is preferable that the monofunctional monomer has a cyclic functional group. In this case, the pressure-sensitive adhesive sheet of the present invention is less likely to peel off even when it is attached to a surface on which a metal or metal oxide is formed.
[0071] The type of monofunctional monomer having a cyclic functional group is not particularly limited as long as it has a cyclic functional group, and examples thereof include a wide range of monomers having one reactive double bond in the molecule and having a cyclic functional group.
[0072] Examples of the monofunctional monomer having a cyclic functional group include the same types as the above-mentioned "(meth)acrylate having a ring structure." Therefore, the monofunctional monomer having a cyclic functional group preferably has a structure in which a functional group having a ring structure is bonded to the ester oxygen of a (meth)acrylate, and in this case, the functional group having a ring structure preferably has 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 4 to 8 carbon atoms.
[0073] Specific examples of monofunctional monomers having a cyclic functional group include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, O-phenylphenoxyethyl (meth)acrylate, etc. The monofunctional monomer having a cyclic functional group is preferably one or more selected from the group consisting of cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and isobornyl (meth)acrylate, since this makes it easier to obtain a pressure-sensitive adhesive sheet that is less likely to peel even when attached to a surface on which a metal or metal oxide is formed.
[0074] The monofunctional monomer having a cyclic functional group is preferably different from a monomer derived from a monomer unit forming the acrylic polymer (P1), i.e., the monofunctional monomer unit having a cyclic functional group contained in the PSA composition is preferably not contained in the constituent units of the acrylic polymer (P1).
[0075] The content of the monofunctional monomer in the pressure-sensitive adhesive composition is not particularly limited. In order to easily improve the adhesion of the pressure-sensitive adhesive sheet to the adherend, the content of the monofunctional monomer is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 1.5 parts by mass or more, relative to 100 parts by mass of the total mass of the acrylic polymer (P1) and the polymerizable monomer M, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, and particularly preferably 6 parts by mass or less.
[0076] The monofunctional monomer having a functional group contained in the pressure-sensitive adhesive composition may be one type alone or two or more types.
[0077] (Polyfunctional Monomer) The pressure-sensitive adhesive composition may contain a polyfunctional monomer. In particular, when the pressure-sensitive adhesive composition is an active energy ray-curable pressure-sensitive adhesive described below, it preferably contains a polyfunctional monomer.
[0078] The polyfunctional monomer may be, for example, a compound having two or more polymerizable double bonds in the molecule. The polyfunctional monomer has two or more polymerizable double bonds (e.g., radically polymerizable double bonds), preferably two or more but less than five, and more preferably two or more but less than four.
[0079] Examples of polyfunctional monomers include bifunctional monomers (monomers having two polymerizable double bonds), such as polyethylene glycol diacrylate, polypropylene diacrylate, alkyl diacrylate, polytetramethylene glycol diacrylate, polypropylene glycol diacrylate, dioxane diacrylate, tricyclodecanol diacrylate, and fluorene diacrylate. Examples of polyfunctional monomers include trifunctional or higher functional monomers, such as alkoxylated trimethylolpropane triacrylate, alkoxylated glycerin triacrylate, caprolactone-modified isocyanurate triacrylate, pentaerythritol acrylate, alkoxylated pentaerythritol acrylate, (alkoxylated) pentaerythritol acrylate, (alkoxylated) ditrimethylolpropane acrylate, (alkoxylated) dipentaerythritol acrylate, and (ethoxylated) polyglycerin acrylate.
[0080] The polyfunctional monomer may have a bisphenol skeleton in one molecule, such as a diacrylate of bisphenol A diglycidyl ether, a diacrylate of propoxylated bisphenol A, or a diacrylate of bisphenol F diglycidyl ether.
[0081] Commercially available polyfunctional monomers include, for example, "A-200" (polyethylene glycol #200 diacrylate) and "A-400" (polyethylene glycol #400 diacrylate) from the NK Ester series, which are bifunctional polyethylene glycol acrylates manufactured by Shin-Nakamura Chemical Co., Ltd., the trifunctional monomer A-TMPT ((alkoxylated) trimethylolpropane acrylate), the trifunctional monomer M310 (trimethylolpropane PO-modified triacrylate) and the trifunctional monomer M321 (trimethylolpropane propylene oxide-modified triacrylate) manufactured by Toagosei Co., Ltd., the bifunctional monomer M211B (bisphenol A EO-modified diacrylate) and M240 (polyethylene glycol diacrylate), and the tetrafunctional monomer M-408 (ditrimethylolpropane tetraacrylate), all manufactured by Toagosei Co., Ltd. Other commercially available polyfunctional monomers include, for example, A-DOG, A-DCP, A-9300, and A-9200YN manufactured by Shin-Nakamura Chemical Co., Ltd., FA-731A manufactured by Hitachi Chemical Co., Ltd., and AOMA manufactured by Nippon Shokubai.
[0082] In the pressure-sensitive adhesive composition, the content ratio of the polyfunctional monomer is not particularly limited. For example, in order to more easily improve adhesion, the content ratio of the polyfunctional monomer is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, particularly preferably 0.3 parts by mass or more, relative to 100 parts by mass of the total mass of the acrylic polymer (P1) and the polymerizable monomer M, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, particularly preferably 1.5 parts by mass or less. The polyfunctional monomer contained in the pressure-sensitive adhesive composition can be one type alone or two or more types.
[0083] <Photopolymerization initiator> The pressure-sensitive adhesive composition may further contain a photopolymerization initiator, which initiates polymerization of the monofunctional monomer and / or polyfunctional monomer when irradiated with active energy rays.
[0084] The type of photopolymerization initiator is not particularly limited, and a wide range of known photopolymerization initiators can be used. Examples of the photopolymerization initiator include acetophenone-based photopolymerization initiators such as 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-[4-(2-hydroxyethoxyl)-phenyl]-2-hydroxy-methylpropanone, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methyl-1-propanone; acylphosphine oxide-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 2,4,6-trimethylbenzoyl)phenylphosphine oxide; intramolecular hydrogen abstraction photopolymerization initiators such as methyl benzoylformate and 4-methylbenzophenone; and oil-soluble polymerization initiators such as oxime ester-based photopolymerization initiators and cationic photopolymerization initiators. Among these, the photopolymerization initiator is preferably at least one selected from the group consisting of acetophenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, and oxime ester-based photopolymerization initiators.
[0085] Commercially available acetophenone-based photopolymerization initiators include EsacureOne (oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenylpropanone], photoinitiator manufactured by IGM Resins B.V.), Omnirad 651 (2,2-dimethoxy-2-phenylacetophenone, manufactured by IGM Resins B.V.), Omnirad 184 (1-hydroxycyclohexylphenyl ketone, manufactured by IGM Resins B.V.), and Omnirad 1173 (2-hydroxy-2-methyl-1-phenylpropanone, manufactured by IGM Resins B.V.). Commercially available acylphosphine oxide-based photopolymerization initiators include Omnirad 819 (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, manufactured by IGM RESINS BV) and Omnirad TPO (2,4,6-trimethylbenzoyl-diphenylphosphine oxide, manufactured by IGM RESINS BV).
[0086] In the pressure-sensitive adhesive composition, the content ratio of the photopolymerization initiator is not particularly limited, and is, for example, preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the total mass of the acrylic polymer (P1) and the polymerizable monomer M, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, and particularly preferably 1.5 parts by mass or less.
[0087] (Crosslinking Agent) The pressure-sensitive adhesive composition may contain a crosslinking agent. In particular, when the pressure-sensitive adhesive composition is not an active energy ray-curable pressure-sensitive adhesive described below, it preferably contains a crosslinking agent instead of the monofunctional monomer and the polyfunctional monomer.
[0088] The crosslinking agent can be appropriately selected, for example, taking into consideration the reactivity with the crosslinkable functional group of the acrylic polymer (P1), and can be a wide variety of known crosslinking agents contained in pressure-sensitive adhesive sheets. Specific examples of the crosslinking agent can be selected from known crosslinking agents such as isocyanate compounds, epoxy compounds, oxazoline compounds, aziridine compounds, metal chelate compounds, and butylated melamine compounds. Of these, the crosslinking agent preferably contains at least one selected from isocyanate compounds, epoxy compounds, and metal chelate compounds.
[0089] (Solvent) When the pressure-sensitive adhesive composition contains a solvent, the coating property of the pressure-sensitive adhesive composition can be improved. Examples of the solvent include hydrocarbons such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, isobutyl alcohol, and diacetone alcohol; ethers such as diethyl ether, diisopropyl ether, dioxane, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, isophorone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, amyl acetate, and ethyl butyrate; polyols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate, and derivatives thereof.
[0090] (Adhesive Sheet) The method for producing the adhesive sheet of the present invention is not particularly limited, and the adhesive sheet of the present invention can be produced, for example, by a production method including a step of forming an adhesive layer using the adhesive composition.
[0091] The method for preparing the pressure-sensitive adhesive composition is not particularly limited, and for example, a wide variety of known methods can be employed. For example, the pressure-sensitive adhesive composition can be prepared by mixing an acrylic polymer (P1) or a syrup thereof, a silane coupling agent, a monofunctional monomer, a tackifier, a polyfunctional monomer, a photopolymerization initiator, and any other components in a predetermined mixing ratio. In this case, the pressure-sensitive adhesive composition is a so-called active energy ray-curable pressure-sensitive adhesive that has the property of being cured by irradiation with active energy rays. In this specification, "active energy rays" refers to electromagnetic waves or charged particle rays that have an energy quantum, and examples thereof include ultraviolet rays, electron beams, visible light, X-rays, and ion beams. Among these, ultraviolet rays or electron beams are preferred from the viewpoint of versatility, and ultraviolet rays are particularly preferred.
[0092] The pressure-sensitive adhesive composition can also be prepared by mixing, for example, the acrylic polymer (P1), a silane coupling agent, a tackifier, a crosslinking agent, and any other components in a predetermined mixing ratio. In this case, the pressure-sensitive adhesive composition can be cured, for example, by heat curing rather than by UV irradiation. The pressure-sensitive adhesive composition can also contain, for example, a plasticizer, an antioxidant, a metal corrosion inhibitor, a UV absorber, a light stabilizer, etc., as long as the effects of the present invention are not impaired. It may also contain a dye or pigment for coloring purposes.
[0093] The method for curing the pressure-sensitive adhesive composition is not particularly limited, and for example, known methods can be widely adopted. For example, when the pressure-sensitive adhesive composition is an active energy ray-curable pressure-sensitive adhesive, the method can include a step of applying the pressure-sensitive adhesive composition to a substrate to form a coating film, and a step of irradiating the coating film with active energy rays to obtain a cured product of the pressure-sensitive adhesive. This allows for the formation of a pressure-sensitive adhesive layer formed by curing the pressure-sensitive adhesive. When the pressure-sensitive adhesive composition is not an active energy ray-curable pressure-sensitive adhesive, the method can include a step of applying the pressure-sensitive adhesive composition to a substrate to form a coating film, and a step of heat-treating the coating film to obtain a cured product of the pressure-sensitive adhesive. Either method allows for the formation of a pressure-sensitive adhesive layer formed by curing the pressure-sensitive adhesive composition. Note that curing of the pressure-sensitive adhesive composition means that the reaction of some or all of the reactive components in the pressure-sensitive adhesive composition proceeds.
[0094] The PSA composition can be applied using a known coating device, such as a blade coater, air knife coater, roll coater, bar coater, gravure coater, microgravure coater, rod blade coater, lip coater, die coater, or curtain coater.
[0095] The substrate used for coating the pressure-sensitive adhesive composition is not particularly limited. For example, the pressure-sensitive adhesive composition can be coated onto various substrates such as resin substrates and glass substrates. When the substrate has a release sheet as described below, the pressure-sensitive adhesive composition can also be coated onto this release sheet. The pressure-sensitive adhesive composition can also be directly coated onto the member to be adhered. The thickness of the pressure-sensitive adhesive composition after coating is not particularly limited, and can be appropriately set depending on the desired thickness of the pressure-sensitive adhesive layer (or pressure-sensitive adhesive sheet). After forming the coating film, the coating film may be subjected to a heating treatment or a drying treatment, if necessary.
[0096] The step of irradiating the coating film with active energy rays can be, for example, a step similar to a known method. In this step, the photopolymerization initiator in the pressure-sensitive adhesive composition generates radicals due to the active energy rays, and the polymerizable components in the pressure-sensitive adhesive composition (e.g., monomers, polyfunctional monomers, etc. in the pressure-sensitive adhesive composition) initiate and progress a polymerization reaction due to the generated radicals, thereby forming a polymerized and cured product. This allows the formation of a pressure-sensitive adhesive layer and improving adhesive strength.
[0097] As mentioned above, ultraviolet rays are particularly preferred as the active energy rays. Examples of light sources that can be used for ultraviolet rays include chemical lamps, high-pressure mercury lamps, low-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, carbon arcs, xenon arcs, and electrodeless ultraviolet lamps. The irradiation output of ultraviolet rays is such that the cumulative light amount is 100 to 10,000 mJ / cm. 2 It is preferable to set the value to 200 to 5000 mJ / cm 2 It is more preferable that the active energy rays be irradiated in two stages in the step of irradiating the coating film with active energy rays. For example, the irradiation intensity in the second stage can be increased compared to that in the first stage. By performing such two-stage irradiation, the molecular weight of the polymer contained in the obtained pressure-sensitive adhesive sheet can be adjusted, and thermal shrinkage of the separator, etc. can be suppressed.
[0098] The pressure-sensitive adhesive layer formed using the pressure-sensitive adhesive composition as described above can be used as the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet of the present invention. The pressure-sensitive adhesive layer may consist of only the cured product of the pressure-sensitive adhesive composition, or may contain other components in addition to the cured product of the pressure-sensitive adhesive.
[0099] The pressure-sensitive adhesive sheet of the present invention may include other layers as long as it includes the pressure-sensitive adhesive layer, or may be formed only with the pressure-sensitive adhesive layer. That is, the pressure-sensitive adhesive sheet preferably consists of only the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer has, for example, a single-layer structure.
[0100] The pressure-sensitive adhesive sheet of the present invention may also be a pressure-sensitive adhesive sheet provided with a substrate such as a release sheet on one or both sides. That is, the present invention also encompasses a pressure-sensitive adhesive sheet with a release sheet that includes a pressure-sensitive adhesive sheet and a release sheet.
[0101] Examples of the release sheet include a release laminate sheet having a release sheet substrate and a release agent layer provided on one side of the release sheet substrate, or a polyolefin film such as a polyethylene film or a polypropylene film as a low-polarity substrate. Paper or a polymer film is used as the release sheet substrate in the release laminate sheet. Examples of the release agent that constitutes the release agent layer include general-purpose addition-type or condensation-type silicone-based release agents and long-chain alkyl group-containing compounds. Commercially available release laminate sheets may also be used. Examples include a heavy-duty separator film, which is a release-treated polyethylene terephthalate film manufactured by Teijin DuPont Films, and a light-duty separator film, which is a release-treated polyethylene terephthalate film manufactured by Teijin DuPont Films.
[0102] In the pressure-sensitive adhesive sheet of the present invention, the gel fraction of the pressure-sensitive adhesive layer is 70% or more and 97% or less. If the gel fraction is less than 70%, peeling is likely to occur when the pressure-sensitive adhesive sheet is adhered to a surface on which a metal or metal oxide is formed. If the gel fraction exceeds 97%, the pressure-sensitive adhesive sheet becomes too hard and adhesion is likely to decrease. The gel fraction of the pressure-sensitive adhesive layer is preferably 80% or more, and more preferably 90% or more. The gel fraction of the pressure-sensitive adhesive layer is measured by the following method. First, approximately 0.1 g of the pressure-sensitive adhesive sheet (pressure-sensitive adhesive layer) is collected in a sample bottle, 30 ml of ethyl acetate is added, and the mixture is shaken for 24 hours. The contents of the sample bottle are then filtered through a 150-mesh stainless steel wire mesh, and the residue on the mesh is dried at 120°C for 1 hour to measure the dry mass (g). The gel fraction can be calculated from the obtained dry mass using the following formula 1: Gel fraction (mass %) = (dry mass / collected mass of pressure-sensitive adhesive layer) × 100...Equation 1.
[0103] The gel fraction of the pressure-sensitive adhesive layer can be adjusted by changing the type and content of the acrylic polymer (P1) in the pressure-sensitive adhesive layer, the type or content of the polyfunctional monomer or crosslinking agent, etc. In particular, when a polyfunctional monomer or a crosslinking agent is contained, the gel fraction of the pressure-sensitive adhesive layer is easily adjusted to 70% or more and 97% or less.
[0104] The thickness of the pressure-sensitive adhesive sheet of the present invention can be appropriately set depending on the application, and is, for example, preferably 10 to 1000 μm, more preferably 20 to 500 μm, and even more preferably 50 to 400 μm.
[0105] By providing the pressure-sensitive adhesive layer, the pressure-sensitive adhesive sheet of the present invention has high adhesion even when attached to a surface on which a metal or metal oxide is formed, and is unlikely to peel off from the surface on which the metal or metal oxide is formed. Therefore, the pressure-sensitive adhesive sheet of the present invention is preferably used for attachment to an adherend having a surface on which a metal or metal oxide is formed. In this case, the pressure-sensitive adhesive sheet is directly attached to the surface on which the metal or metal oxide is formed of the adherend.
[0106] The type of surface on which the metal or metal oxide is formed is not particularly limited, and for example, a surface having indium tin oxide (ITO) can be mentioned. When the surface on which the metal or metal oxide is formed is ITO, the adhesiveness between the pressure-sensitive adhesive sheet of the present invention and the ITO surface is particularly high, so peeling is extremely unlikely to occur, and in addition, the appearance after a durability test is good, so corrosion is unlikely to occur and durability is also likely to be improved.
[0107] The pressure-sensitive adhesive sheet of the present invention has excellent adhesion to surfaces on which metals or metal oxides are formed and is not susceptible to peeling, and therefore can be suitably used as a pressure-sensitive adhesive sheet for various optical components, and is suitable for use in, for example, automotive dimming roofs.
[0108] 2. Laminate A laminate can be formed using the pressure-sensitive adhesive sheet of the present invention. In one embodiment of such a laminate, a first adherend having a metal or metal oxide surface is bonded to one surface of the pressure-sensitive adhesive sheet of the present invention, and a second adherend made of a resin plate or glass is bonded to the other surface.
[0109] The first adherend may have, for example, the aforementioned metal or metal oxide surface on a substrate. Examples of the substrate for the first adherend include various substrates such as glass, resin films, and metals. Examples of the first adherend include an ITO film in which an ITO film is provided on a transparent resin film, and an ITO glass in which an ITO film is provided on the surface of a glass plate. The first adherend may be a commercially available heat-shielding film, and examples thereof include a wide range of heat-shielding films having an ITO surface.
[0110] Examples of the second adherend include various substrates such as a glass plate, a resin film plate, a metal, etc. Examples of the resin film include polycarbonate, polyethylene terephthalate, polymethyl methacrylate, polyethylene naphthalate, cycloolefin polymer, triacetyl cellulose, polyimide, and cellulose acylate.
[0111] In specifying the inventions included in the present disclosure, the components (properties, structures, functions, etc.) described in each embodiment of the present disclosure may be combined in any manner. In other words, the present disclosure includes all subject matter consisting of all combinations of the components that can be combined as described in this specification.
[0112] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0113] (Acrylic Polymer (P1)) In the Examples and Comparative Examples, the following monomers were prepared for producing "acrylic polymer (P1)" or its syrup: 2EHA: 2-ethylhexyl acrylate, BA: butyl acrylate, 4HBA: 4-hydroxybutyl acrylate, CHMA: cyclohexyl methacrylate, AA: acrylic acid.
[0114] (Monofunctional Monomer) The following were prepared as "monofunctional monomers" to be used in the Examples and Comparative Examples: IBXA: isobornyl acrylate IBXMA: isobornyl methacrylate DCPA: dicyclopentanyl acrylate DCPMA: dicyclopentanyl methacrylate
[0115] (Silane Coupling Agent) The following were prepared as "silane coupling agents" used in the examples and comparative examples. Shin-Etsu Silicone KBM-403: 3-glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) Shin-Etsu Silicone KBM-402: 3-glycidoxypropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) Shin-Etsu Silicone KBE-403: 3-glycidoxypropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.) Shin-Etsu Silicone X-12-989MS: N-2-pyridinyl-N'-[3-(trimethoxysilyl)propyl]-urea (manufactured by Shin-Etsu Chemical Co., Ltd.) Shin-Etsu Silicone X-12-1056ES: alkoxysilane having a mercapto group protected by a protecting group (manufactured by Shin-Etsu Chemical Co., Ltd.) Shin-Etsu Silicone X-41-1810: reactive group is -C 3 H 6Alkoxysilane (SH) (manufactured by Shin-Etsu Chemical Co., Ltd.) Shin-Etsu Silicone KBM-9659: Tris(trimethoxysilylpropyl)isocyanurate (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0116] (Production Example 1: Production of Tackifier 1) 250 g of methyl methacrylate, 250 g of isobornyl methacrylate, 20 g of n-dodecyl mercaptan, 500 g of ethyl acetate, and 200 g of methyl ethyl ketone were added to a 2 L flask equipped with a stirrer, a nitrogen inlet tube, a cooling tube, and a thermometer. After nitrogen substitution at a nitrogen flow rate of 300 ml / min for 60 minutes, the nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 70 ° C. in a water bath and heating was stopped. 2 g of AIBN was added, and the mixture was reacted for 3 hours while controlling the heat generation, and then 3 g of AIBN was added, and the mixture was reacted for 4 hours, and then cooled to 30 ° C. Finally, the mixture was dried at 100 ° C. for 5 hours to remove the solvent, and a tackifier having a weight average molecular weight of 6,000 and a glass transition temperature of 95 ° C. was obtained.
[0117] (Production Example 2: Production of Tackifier 2) A tackifier having a weight average molecular weight of 6,000 and a glass transition temperature of 95°C was obtained in the same manner as in Production Example 1, except that dicyclopentanyl methacrylate was used instead of isobornyl methacrylate.
[0118] Example 1 Production of Acrylic Polymer (P1) An acrylic polymer (P1) was synthesized to have the monomer composition of the acrylic polymer (P1) shown in Table 1. Specifically, 100 parts by mass of a monomer mixture consisting of 2EHA, 4HBA, and CHMA (mass ratio 62:29:9) and 0.1 parts by mass of n-dodecyl mercaptan were added to a flask in the amounts of monomers shown in Table 1, and the atmosphere was purged with nitrogen at a nitrogen flow rate of 300 ml / min for 60 minutes. Thereafter, the nitrogen flow rate was reduced to 100 ml / min, and the mixture was heated to 65°C in a water bath. 0.15 g of AIBN was then added, and the mixture was allowed to react for 30 minutes while controlling the heat generation, and then cooled to room temperature. Additional polymerizable monomer M was added to the flask to achieve the monomer ratio of the aforementioned mass ratio, and the solids concentration was adjusted to 20%. In this manner, a syrup A containing an acrylic polymer (P1) having a solid content of 20% by mass and a weight-average molecular weight of 900,000 was obtained.
[0119] <Production of Pressure-Sensitive Adhesive Sheet> Next, as shown in Table 1, 0.3 parts by mass of a bifunctional monomer "polyethylene glycol #200 diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., NK Ester A-200" as a polyfunctional monomer, 3 parts by mass of isobornyl acrylate as a monofunctional monomer, 0.5 parts by mass of "KBM-403" as a silane coupling agent, and 0.3 parts by mass of a photopolymerization initiator (manufactured by IGM Resins B.V., Esacure One) were added to 100 parts by mass of the total amount of the syrup A (total amount of acrylic polymer (P1) and polymerizable monomer M), and the mixture was stirred and degassed to obtain a pressure-sensitive adhesive composition. The obtained pressure-sensitive adhesive composition was coated to a thickness of 175 μm on a 100 μm thick polyester film (release sheet) coated with a silicone release agent, and the resulting mixture was laminated with a 75 μm thick polyester film (release sheet) coated with a silicone release agent. The resulting composition was then heated at an illuminance of 5 mW / cm using a chemical lamp. 2 , cumulative illuminance 900 mJ / cm 2 Further, a high-pressure mercury lamp was used to irradiate the sample with an illuminance of 200 mW / cm 2 , cumulative illuminance 2000 mJ / cm 2 A pressure-sensitive adhesive layer (pressure-sensitive adhesive sheet) was obtained by irradiating the film so as to achieve the above condition.
[0120] (Example 2) A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the monomer composition of the acrylic polymer (P1) was changed to the conditions shown in Table 1, and the types and amounts of the polyfunctional monomer, monofunctional monomer, and silane coupling agent were changed to the conditions shown in Table 1.
[0121] (Example 3) A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the monomer composition of the acrylic polymer (P1) was changed to the conditions shown in Table 1, tackifier 2 was used in the blending amount shown in Table 1, and the types and amounts of the polyfunctional monomer, monofunctional monomer, and silane coupling agent were changed to the conditions shown in Table 1.
[0122] Example 4 Production of Acrylic Polymer (P1) An adhesive resin containing an acrylic polymer (P1) was synthesized according to the formulation conditions of the adhesive resin preparation formula shown in Table 1. Specifically, 335 g of BA, 125 g of 4HBA, 40 g of CHMA, and 750 g of ethyl acetate were charged into a 2 L flask equipped with a stirrer, nitrogen inlet tube, condenser, and thermometer in the amounts shown in Table 1. After nitrogen substitution at a nitrogen flow rate of 300 ml / min for 60 minutes, the nitrogen flow rate was reduced to 100 ml / min, and the temperature was raised to 70 ° C. in a water bath. 0.1 g of AIBN was added, and the reaction was allowed to proceed for 1 hour while controlling the heat generation. Thereafter, an additional 0.5 g of AIBN was added, and the reaction was allowed to proceed for 6 hours, after which the reaction was cooled to 50 ° C. In this manner, an acrylic polymer (P1) having a solids concentration of 40% by mass and a weight average molecular weight of approximately 600,000 was obtained.
[0123] Next, as shown in Table 1, 3 parts by mass of tackifier 2 obtained in Production Example 1, 0.5 parts by mass of a crosslinker (Tosoh Corporation, Coronate L), and 2 parts by mass of a silane coupling agent (Shin-Etsu Chemical Co., Ltd., KBE-403) were added to a total of 100 parts by mass of the acrylic polymer (P1), followed by stirring and degassing to obtain a pressure-sensitive adhesive composition. The obtained pressure-sensitive adhesive composition was applied to a 100 μm thick polyester film (release sheet) coated with a silicone release agent so that the thickness of the pressure-sensitive adhesive layer after drying would be 88 μm, and the coating was dried in a dryer at 90°C for 3 minutes. Thereafter, a pressure-sensitive adhesive layer obtained in the same manner was laminated and allowed to stand at room temperature for 7 days to obtain a pressure-sensitive adhesive layer (pressure-sensitive adhesive sheet) having a thickness of 175 μm.
[0124] (Example 5) <Production of acrylic polymer (P1)> A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 4, except that the monomer composition of the acrylic polymer (P1) was changed to the conditions shown in Table 1, and the types and amounts of the crosslinking agent and silane coupling agent used were changed to the conditions shown in Table 1.
[0125] (Example 6) A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the monomer composition of the acrylic polymer (P1) was changed to the conditions shown in Table 1, and the types and amounts of the polyfunctional monomer, monofunctional monomer, and silane coupling agent were changed to the conditions shown in Table 1.
[0126] Comparative Example 1 A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the monomer composition of the acrylic polymer (P1) was changed to the conditions shown in Table 1, tackifier 2 was used in the blending amount shown in Table 1, and the types and amounts of the polyfunctional monomer, monofunctional monomer, and silane coupling agent were changed to the conditions shown in Table 1.
[0127] (Comparative Example 2) A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the monomer composition of the acrylic polymer (P1) was changed to the conditions shown in Table 1, no polyfunctional monomer was used, and the types and amounts of the monofunctional monomer and silane coupling agent used were changed to the conditions shown in Table 1.
[0128] (Evaluation of Pressure-Sensitive Adhesive Sheet) <High-Temperature Constant Load Measurement> The obtained pressure-sensitive adhesive sheet was bonded to the ITO surface of a 50 μm-thick heat-shielding film (manufactured by Geomatec). The pressure-sensitive adhesive sheet was then cut so that the bonded portion was 25 mm wide and 50 mm long. A 1 mm-thick polycarbonate sheet (manufactured by Mitsubishi Gas Chemical Company, Iupilon MR58) was then bonded to the surface of the pressure-sensitive adhesive sheet opposite the heat-shielding film, and a laminate was obtained by rolling the sheet back and forth twice with a 2 kg roller. This laminate was then treated in an autoclave at a temperature of 30°C and a pressure of 0.5 MPa for 30 minutes, and then left to stand at atmospheric pressure and room temperature for 1 day to obtain a laminate for evaluation. The evaluation laminate was left to stand for 30 minutes in a thermo-hygrostat at 110°C, and then placed on a stand with the polycarbonate sheet side facing up. A 100g weight was then hooked onto the end of the heat shield film to apply a load, and the peel distance (peel distance between the polycarbonate sheet and the pressure-sensitive adhesive sheet) after 30 minutes was measured and evaluated according to the following criteria. <Evaluation criteria> ⊚: The peel distance after 30 minutes was less than 10mm, meaning that peeling was extremely difficult. ◯: The peel distance after 30 minutes was 10mm or more and less than 20mm, meaning that peeling was difficult. △: The peel distance after 30 minutes was 20mm or more and less than 40mm, meaning that there was no problem in practical use. ×: The peel distance after 30 minutes was 40mm or more, or the film fell off before 30 minutes had elapsed, meaning that peeling was extremely easy.
[0129] <Appearance Inspection> The obtained pressure-sensitive adhesive sheet was laminated to the ITO surface of a 50 μm-thick heat-shielding film (manufactured by Geomatec), and the other surface of the pressure-sensitive adhesive sheet was laminated to a 55 mm wide, 80 mm long, and 1 mm thick polycarbonate sheet (manufactured by Mitsubishi Gas Chemical Company, Iupilon MR58) to obtain a laminate. This laminate was autoclaved for 30 minutes at a temperature of 30°C and a pressure of 0.5 MPa, and then left to stand at atmospheric pressure and room temperature for 1 day. The obtained evaluation laminate was placed in a dryer at 110°C for 6 hours, removed, and visually inspected for the presence or absence of bubbles or peeling, and evaluated according to the following criteria. <Evaluation Criteria> ⊚: No bubbles or peeling, and the appearance was extremely good. ○: Bubbles were observed at a rate of 1 to less than 10 points, and the appearance was good. △: Bubbles were observed at a rate of 10 to less than 20 points, but the appearance was acceptable for practical use. x: 20 or more bubbles were observed or peeling was observed, and the appearance was extremely poor.
[0130] <Corrosion> The obtained pressure-sensitive adhesive sheet was laminated to the ITO surface of a 50 μm-thick heat-shielding film (manufactured by Geomatec), and the other surface of the pressure-sensitive adhesive sheet was laminated to a 55 mm wide, 80 mm long, 1 mm thick polycarbonate sheet (manufactured by Mitsubishi Gas Chemical Company, Iupilon MR58) to obtain a laminate. This laminate was treated in an autoclave at a temperature of 30°C and a pressure of 0.5 MPa for 30 minutes, and then left to stand at atmospheric pressure and room temperature for 1 day. The obtained evaluation laminate was placed in a dryer at 65°C and 95% humidity and removed after 168 hours. The presence or absence of corrosion on the ITO surface of the heat-shielding film was visually inspected and evaluated according to the following criteria. <Evaluation criteria> ○: No corrosion was observed. ×: Corrosion was observed.
[0131] Table 1 shows the pressure-sensitive adhesive compositions and pressure-sensitive adhesive sheet preparation conditions for each example and comparative example. Table 1 also shows the weight-average molecular weight and Tg of the acrylic polymer (P1) and the evaluation results of the pressure-sensitive adhesive sheets (pressure-sensitive adhesive layers). In Table 1, the notation "P1+M" means the total amount (parts by mass) of the acrylic polymer (P1) and the polymerizable monomer M. However, in Examples 4 and 5, the polymerizable monomer M was not used.
[0132] As can be seen from Table 1, as in Examples 1 to 6, adhesive sheets having an adhesive layer obtained using an adhesive composition containing a specified silane coupling agent were less likely to peel off even when attached to a surface (ITO surface) on which a metal or metal oxide was formed.
[0133]
Claims
1. An adhesive sheet having an adhesive layer, the adhesive layer containing an acrylic polymer and a silane coupling agent, the silane coupling agent having an epoxy group, a chelating functional group, a mercapto group, or a mercapto group protected by a protecting group, and the adhesive layer having a gel fraction of 70% or more and 97% or less.
2. The pressure-sensitive adhesive sheet according to claim 1, wherein the content of carboxyl group-containing monomer units in the acrylic polymer is 0.1 mass % or less.
3. The pressure-sensitive adhesive sheet according to claim 1, which is used for bonding to a surface having a metal or metal oxide.
4. The pressure-sensitive adhesive sheet according to claim 3, wherein the surface having a metal or metal oxide is a surface having indium tin oxide.
5. A laminate comprising a first adherend having a metal or metal oxide surface bonded to one side of the pressure-sensitive adhesive sheet according to any one of claims 1 to 4, and a second adherend made of a resin plate or glass bonded to the other side.
6. A release-sheet-attached adhesive sheet comprising the adhesive sheet according to any one of claims 1 to 4 and a release sheet.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition, pressure-sensitive adhesive and pressure-sensitive adhesive sheet
JP2014152312A
Adhesive composition, adhesive and adhesive sheet
JP2017141471A
Adhesive composition and polarizing plate with adhesive layer
JP2017171704A
Adhesive composition, adhesive layer, adhesive sheet, optical member, and touch panel
JP2018086846A
Optical adhesive sheet for polarizing plate and polarizing plate
JP2019059811A
Cited By
Optical adhesive sheet and laminate