Photosensitive resin laminate and method for forming resist pattern
The photosensitive resin laminate, featuring polyglycerin-based (meth)acrylate and alkali-soluble resin, addresses the limitations of existing compositions by enhancing developability, flexibility, and adhesion, resulting in superior resist pattern formation for printed wiring boards.
Patent Information
- Application Number
- PCT/JP2024/014836
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
Existing photosensitive resin compositions for printed wiring boards face challenges in achieving optimal developability, flexibility, resolution, and adhesion, with existing solutions either improving one aspect at the expense of others.
A photosensitive resin laminate comprising a support film and a resist layer with a photosensitive resin composition containing polyglycerin-based (meth)acrylate and an alkali-soluble resin, along with specific structural units and photopolymerization initiators, to enhance developability, flexibility, resolution, and adhesion.
The proposed solution provides a photosensitive resin laminate with improved developability, flexibility, resolution, and adhesion, enabling the formation of high-quality resist patterns with enhanced performance in printed wiring board manufacturing.
Smart Images

Figure JP2024014836_17102024_PF_FP_ABST
Abstract
Description
Photosensitive resin laminate and method for forming resist pattern
[0001] The present invention relates to a photosensitive resin laminate and a method for forming a resist pattern.
[0002] Printed wiring boards are generally manufactured using a photolithography process. Photolithography is a method of forming a desired wiring pattern on a substrate by the following steps: First, a layer containing a photosensitive resin composition is formed on the substrate, and the coating film is subjected to pattern exposure and development to form a resist pattern. Next, a conductor pattern is formed by etching or plating. Thereafter, the resist pattern on the substrate is removed to form the desired wiring pattern on the substrate.
[0003] Generally, a resist pattern is formed in a photolithography process by, for example, applying a solution of a photosensitive resin composition to a substrate and drying it, or by laminating a resist layer of a dry film resist (a photosensitive resin laminate including a resist layer and a support film) onto a substrate.
[0004] Photosensitive resin laminates are often used in the manufacture of printed wiring boards. In the production and use of photosensitive resin laminates, performance such as developability, flexibility, resolution, adhesion, and peelability, and productivity, which are determined by the type and combination of compounds having ethylenically unsaturated bonds and the content thereof, are important.
[0005] For example, Patent Document 1 discloses that the use of glycerin triacrylate improves developability and removability, and Patent Document 2 discloses that the use of a (meth)acrylate compound having a skeleton derived from pentaerythritol improves resolution and adhesion.
[0006] JP 10-198031 A JP 2013-92693 A
[0007] However, although the photosensitive resin composition described in Patent Document 1 has predetermined developability and releasability, there is still room for further improvement in terms of resolution and adhesion. Also, although the curable resin composition described in Patent Document 2 has predetermined resolution and adhesion, there is still room for further improvement in terms of developability and flexibility.
[0008] An object of the present invention is to provide a photosensitive resin laminate that is excellent in developability, flexibility, resolution, and adhesion, and a method for forming a resist pattern.
[0009] The present invention is as follows.
[0010] [1] A photosensitive resin laminate comprising a support film and a resist layer containing a photosensitive resin composition, wherein the photosensitive resin composition contains the following components: (A) a compound having an ethylenically unsaturated bond, and (B) an alkali-soluble resin, and the component (A) is a compound represented by the following general formula (I): [wherein n is 2 to 20, each i is a natural number from 1 to n, k, each l i, and m are each independently 0 to 30, and R 1 , R 2i , and R 3 each independently represents a hydrogen atom or a methyl group; R 4 , R 5i , and R 6 are each independently an alkylene group having 1 to 10 carbon atoms, a group represented by the following formula (II): [In the formula, R 7 and R 8 are each independently an alkylene group having 1 to 10 carbon atoms.] and a group represented by the following formula (III): [In the formula, R 9is an alkylene group having 1 to 10 carbon atoms. ] is one selected from the group consisting of groups represented by the following formulas. ] A photosensitive resin laminate comprising: a polyglycerin-based (meth)acrylate represented by the following formula: and (A2) a compound having no carboxyl group and an ethylenically unsaturated bond. [2] The photosensitive resin laminate according to [1], wherein the total content of the component (A) and the component (B) in the photosensitive resin composition is 80 mass % or more and 98 mass % or less, based on the total solid content mass of the photosensitive resin composition. [3] The photosensitive resin laminate according to [1] or [2], wherein the content of the component (B) is 70 mass % or less, based on the total content of the component (A) and the component (B). [4] The photosensitive resin laminate according to any of [1] to [3], wherein the component (B) contains structural units derived from styrene and benzyl (meth)acrylate. [5] The photosensitive resin laminate according to any one of [1] to [4], wherein the component (B) contains a structural unit derived from styrene, and the styrene content in the component (B) is 35% by mass or more and 80% by mass or less. [6] The photosensitive resin laminate according to any one of [1] to [5], wherein the photosensitive resin composition further contains a photopolymerization initiator as the component (C). [7] The photosensitive resin laminate according to [6], wherein the content of the component (C) in the photosensitive resin composition is 25% by mass or less, based on the content of the component (A). [8] The photosensitive resin laminate according to [6] or [7], wherein the component (C) contains a hexaarylbiimidazole compound. [9] The photosensitive resin laminate according to any one of [1] to [8], wherein the photosensitive resin composition further contains a polymerization inhibitor (D).
[10] The photosensitive resin laminate according to any one of [1] to [9], wherein the component (A2) is a compound having 2 to 6 ethylenically unsaturated bonds.
[11] The photosensitive resin laminate according to any one of [1] to [9], wherein the component (A2) comprises a compound having two ethylenically unsaturated bonds.
[12] The photosensitive resin laminate according to any one of [1] to [9], wherein the component (A2) comprises a compound having one ethylenically unsaturated bond.
[13] The photosensitive resin laminate according to any one of [1] to
[12] , wherein the component (A2) comprises a di(meth)acrylate compound having a bisphenol A structure.
[14] R in the general formula (I). 1 , R 2i , and R 3
[15] The photosensitive resin laminate according to any one of [1] to
[13] , wherein R in the general formula (I) is a methyl group. 4 O, R 5i O and R 6 O into the formula R j O {where j=4, 5i, 6 (where i=1, 2, ..., n)}, j The photosensitive resin laminate according to any one of [1] to
[14] , wherein the ratio of the number of (meth)acryloyl groups to the total number of O is 20 or less.
[16] The photosensitive resin laminate according to any one of [1] to
[15] , wherein in the general formula (I), n is an integer of 2 to 15.
[17] The photosensitive resin laminate according to any one of [1] to
[15] , wherein in the general formula (I), n is a number average value of 2 to 15.
[18] The photosensitive resin laminate according to any one of [1] to
[15] , wherein the R 4 , R 5i , and R 6
[19] The photosensitive resin laminate according to any one of [1] to
[17] , wherein R is an alkylene group. 4 , R 5i , and R 6
[20] The photosensitive resin laminate according to any one of [1] to
[18] , wherein R contains an ethylene group and / or a propylene group. 4 , R 5i , and R 6
[21] The photosensitive resin laminate according to any one of [1] to
[18] , wherein R is an ethylene group and / or a propylene group. 4 , R 5i , and R 6is an ethylene group.
[22] The photosensitive resin laminate according to any one of [1] to
[21] , further comprising a protective film.
[23] A photosensitive resin laminate comprising a support film and a resist layer containing a photosensitive resin composition, wherein the photosensitive resin composition contains the following components: (A) a compound having an ethylenically unsaturated bond, and (B) an alkali-soluble resin, wherein the component (A) contains: (A3) a compound having no quaternary carbon and / or aromatic ring and having four or more ethylenically unsaturated bonds in one molecule; and (A4) a compound having a quaternary carbon and / or aromatic ring, no carboxyl group, and having an ethylenically unsaturated bond.
[24] The photosensitive resin laminate according to
[23] , wherein the (A4) compound contains a compound having one or two ethylenically unsaturated bonds.
[25] The photosensitive resin laminate according to
[23] or
[24] , wherein the amount of ethylenically unsaturated bonds per 100 g of the (A4) compound is 0.25 mol or less.
[26] The photosensitive resin laminate according to any of
[23] to
[25] , wherein the content of the (A) component is 20 mass% or more, based on the total mass of the solid content of the photosensitive resin composition.
[27] The photosensitive resin laminate according to any of
[23] to
[26] , wherein the (B) component comprises a copolymer containing structural units derived from (meth)acrylic acid as a monomer component, and the content of the structural units derived from (meth)acrylic acid in the (B) component is 27 mass% or less.
[28] The photosensitive resin laminate according to any of
[23] to
[26] , wherein the (B) component comprises a copolymer containing structural units derived from (meth)acrylic acid as a monomer component, and the content of the structural units derived from (meth)acrylic acid in the (B) component is 25 mass% or less.
[29] A method for forming a resist pattern using the photosensitive resin laminate according to any one of [1] to
[28] , comprising the following steps: a laminating step of laminating a resist layer on a substrate; an exposing step of exposing the resist layer; and a developing step of developing and removing an unexposed portion of the resist layer.
[30] A method for producing a wiring board using the photosensitive resin laminate according to any one of [1] to
[28] , comprising the following steps: a lamination step of laminating a resist layer on a substrate; an exposure step of exposing the resist layer to light; a development step of developing and removing unexposed portions of the resist layer to form a resist pattern; a conductor pattern formation step of etching or plating the substrate on which the resist pattern has been formed to form a conductor pattern; and a peeling step of peeling the resist pattern from the substrate.
[0011] According to the present invention, it is possible to provide a photosensitive resin laminate including a resist layer containing a photosensitive resin composition that is excellent in developability, flexibility, resolution, adhesion, and releasability, and a method for forming a resist pattern.
[0012] An exemplary embodiment of the present invention (hereinafter abbreviated as "the present embodiment") will be described in detail below. The present invention is not limited to this embodiment, and various modifications can be made within the scope of the gist of the present invention. In this specification, the upper and lower limits of each numerical range can be arbitrarily combined. Furthermore, in this embodiment, the upper or lower limit described in a certain numerical range can also be replaced with a value shown in the examples. In this specification, a numerical range indicated using "to" includes the upper and lower limit values. The term "step" in the following description can include an independent step, as well as a step that cannot be clearly distinguished from other steps, as long as the function of that "step" is achieved.
[0013] In addition, in this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid, "(meth)acryloyl group" means acryloyl group or methacryloyl group, and "(meth)acrylate" means "acrylate" or "methacrylate".
[0014] <Photosensitive Resin Laminate> In one aspect, the photosensitive resin laminate of the present embodiment includes a support film and a resist layer containing a photosensitive resin composition. The photosensitive resin composition constituting the photosensitive resin laminate, provided in particular in one aspect of the present embodiment, includes: (A) a compound having an ethylenically unsaturated bond; and (B) an alkali-soluble resin. In particular, in the photosensitive resin laminate of the present embodiment, the photosensitive resin composition of the present embodiment includes, as the (A) compound having an ethylenically unsaturated bond, (A1) a polyglycerin-based (meth)acrylate and (A2) a compound having no carboxyl group and an ethylenically unsaturated bond.
[0015] The present inventors have found that by combining a polyglycerol-based (meth)acrylate (A1) with a compound (A2) that does not have a carboxyl group and has an ethylenically unsaturated bond as components of the photosensitive resin composition of this embodiment, the developability, flexibility, resolution, adhesion, and releasability are improved. That is, this embodiment can provide a photosensitive resin composition and a method for forming a resist pattern that are excellent in developability, flexibility, resolution, adhesion, and releasability.
[0016] In another embodiment of the photosensitive resin laminate, the photosensitive resin composition of the present embodiment contains, as the compound (A) having an ethylenically unsaturated bond, (A3) a compound that does not have a quaternary carbon and / or an aromatic ring and has four or more ethylenically unsaturated bonds in one molecule, and (A4) a compound that has a quaternary carbon and / or an aromatic ring, does not have a carboxyl group, and has an ethylenically unsaturated bond.
[0017] <Support Film> The support film according to this embodiment is a layer or film for supporting the resist layer, and is preferably a transparent base film that transmits actinic rays.
[0018] Examples of transparent substrate films include films made of synthetic resins such as polyethylene, polypropylene, polycarbonate, polyethylene terephthalate (PET), cellulose triacetate, and cycloolefin polymer. Among these, it is preferable to use a high-quality film with few internal foreign matter. Specifically, high-quality films such as polyethylene terephthalate (PET) film, cellulose triacetate film, and cycloolefin polymer film are preferred, with polyethylene terephthalate (PET) film having appropriate flexibility and strength being more preferred. Among PET films, it is more preferable to use PET films synthesized using a Ti-based catalyst, small-diameter PET films with a low lubricant content, PET films containing lubricant on only one side of the film, thin-film PET films, PET films smoothed on at least one side, and PET films roughened on at least one side by plasma treatment or the like. This allows the exposure light to be irradiated onto the resist layer without being blocked by internal foreign matter, thereby improving the resolution of the photosensitive resin composition.
[0019] The thickness of the support film is preferably 5 μm to 25 μm, more preferably 6 μm to 20 μm. The thinner the support film, the fewer the number of internal foreign matter and the more effectively it can prevent a decrease in resolution. However, if the film is too thin, the film may be stretched and deformed in the winding direction due to tension or may be torn due to minute scratches during the coating and winding manufacturing process, or the strength of the film may be insufficient, causing wrinkles during lamination.
[0020] At least one surface of the support film may be subjected to a smoothing treatment using a calendering device, etc. This reduces the surface roughness of one surface of the support film, particularly the surface that comes into contact with a photosensitive resin composition layer described below, thereby further improving the effects of this embodiment.
[0021] The haze of the support film is preferably 0.01% to 1.5%, more preferably 0.01% to 1.2%, and even more preferably 0.01% to 0.95%, from the viewpoint of improving the parallelism of the light beam irradiated onto the resist layer and obtaining higher resolution after exposure and development of the photosensitive resin laminate.
[0022] <Resist Layer> The resist layer according to this embodiment contains a photosensitive resin composition. In one aspect, the resist layer according to this embodiment is a photosensitive resin composition layer. The thickness of the resist layer according to this embodiment is preferably 3 to 100 μm, and more preferably 3 to 50 μm. As the thickness of the resist layer approaches 3 μm, the resolution improves, and as the thickness approaches 100 μm, the film strength improves, so the thickness can be appropriately selected depending on the application. The thickness of the resist layer according to this embodiment may be greater than 100 μm and not greater than 500 μm. When the thickness of the resist layer is within the above range, it can also be suitably used for forming bumps and copper pillars.
[0023] <Photosensitive Resin Composition> The photosensitive resin composition of the present embodiment contains (A) a compound having an ethylenically unsaturated bond and (B) an alkali-soluble resin.
[0024] (A) Compound Having an Ethylenically Unsaturated Bond In this embodiment, the compound (A) having an ethylenically unsaturated bond (hereinafter referred to as component (A)) includes, as components, (A1) a polyglycerin-based (meth)acrylate and (A2) a compound having an ethylenically unsaturated bond and no carboxyl group. In one aspect, the component (A) includes a polyglycerin-based (meth)acrylate (A1) represented by general formula (I) described below and a compound having an ethylenically unsaturated bond and no carboxyl group (A2). By combining the polyglycerin-based (meth)acrylate (A1) and the compound having an ethylenically unsaturated bond and no carboxyl group (A2) as component (A) in the photosensitive resin composition of this embodiment, the developability, flexibility, resolution, adhesion, and releasability are improved.
[0025] (A1) Polyglycerin-Based (Meth)acrylate In this embodiment, (A1) polyglycerin-based (meth)acrylate refers to a compound having a polyglycerin skeleton and a (meth)acryloyl group, and refers to a compound having the following structural formula (I) (in one aspect, general formula (I) or formula (I)).
[0026] [wherein n is 2 to 20, each i is a natural number from 1 to n, k, each l i, and m are each independently 0 to 30, and R 1 , R 2i , and R 3 each independently represents a hydrogen atom or a methyl group; R 4 , R 5i , and R 6 are each independently an alkylene group having 1 to 10 carbon atoms, a group represented by the following formula (II): [In the formula, R 7 and R 8 are each independently an alkylene group having 1 to 10 carbon atoms.] and a group represented by the following formula (III): [In the formula, R 9 is an alkylene group having 1 to 10 carbon atoms.]
[0027] The polyglycerin-based (meth)acrylate (A1) may be used either as a single compound or as a combination of two or more compounds.
[0028] R 4 O, R 5i O and R 6 A polyglycerin-based (meth)acrylate having a repeating unit represented by O can be synthesized, for example, by the following method, but the synthesis method of the polyglycerin-based (meth)acrylate (A1) according to this embodiment is not limited to this. After reacting the hydroxyl group of polyglycerin with alkylene oxide, the terminal hydroxyl group is reacted with acrylic acid or methacrylic acid to form a polyglycerin-based (meth)acrylate having a repeating unit represented by O. 4 , R 5i and R 6In place of alkylene oxide, a compound having a leaving group and an epoxy group, such as epichlorohydrin, can be used in the reaction to obtain a polyglycerin-based (meth)acrylate in which the R 4 , R 5i and R 6 By using a lactone compound in place of an alkylene oxide in the reaction, it is possible to obtain a polyglycol-based (meth)acrylate represented by the chemical formula (II). 4 , R 5i and R 6 The polyglycerol-based (meth)acrylate represented by the chemical formula (III) can be obtained. These reactions may be freely combined. 4 O, R 5i O and R 6 It is also possible to react acrylic acid or methacrylic acid with the hydroxyl groups of polyglycerin without introducing a repeating unit represented by O. Specifically, SA-TE6, SA-TE60, etc. manufactured by Sakamoto Pharmaceutical Chemical Industry Co., Ltd. can be used as the polyglycerin-based (meth)acrylate.
[0029] From the viewpoint of flexibility and adhesion, k, each li, and m in formula (I) are each independently preferably 2 to 20, more preferably 2 to 15, even more preferably 2 to 12, even more preferably 2 to 10, particularly preferably 2 to 8, and most preferably 2 to 6. In the present disclosure, when the polyglycerin-based (meth)acrylate (A1) represented by formula (I) is composed of a single type of molecule, k, each li, and m can be expressed as an integer value. Furthermore, when the polyglycerin-based (meth)acrylate (A1) represented by formula (I) is composed of multiple types of molecules, k, each li, and m can be expressed as a number average value.
[0030] From the viewpoint of flexibility and releasability, n in structural formula (I) is preferably an integer of 2 to 15, more preferably 2 to 10, even more preferably 2 to 8, even more preferably 2 to 6, and particularly preferably 2 to 4. Furthermore, when the polyglycerin-based (meth)acrylate (A1) represented by general formula (I) is composed of multiple types of molecules, n can be expressed as a number average value. In one embodiment, n in formula (I) is a number average value, and is preferably 2 to 15, more preferably 2 to 10, even more preferably 2 to 8, even more preferably 2 to 6, and particularly preferably 2 to 4.
[0031] In the present disclosure, (k+l) in structural formula (I) 1 +l 2 +...+l n + m) / (n+2), i.e., the value of R in formula (I) 4 O, R 5i O and R 6 O into the formula R j O {where j=4, 5i, 6 (where i=1, 2, ..., n)}, R j From the viewpoint of resolution and adhesion, the ratio of the number of (meth)acryloyl groups to the total number of O is preferably 20 or less, more preferably 15 or less, even more preferably 10 or less, and particularly preferably 6 or less. In one embodiment, the value of (k+l+m) / (n+2) in structural formula (I) is preferably 2 or more. In the present disclosure, k, each l, and m in the formula of (A1) polyglycerin-based (meth)acrylate represented by formula (I) are referred to as repeating units. From the viewpoint of adhesion and resolution, the ratio of R in structural formula (I) is preferably 20 or less, more preferably 15 or less, even more preferably 10 or less, and particularly preferably 6 or less. In one embodiment, the value of (k+l+m) / (n+2) in structural formula (I) is preferably 2 or more. In the present disclosure, k, each l, and m in the formula of (A1) polyglycerin-based (meth)acrylate represented by formula (I) are referred to as repeating units. 1 , R 2i , and R 3 is preferably a methyl group.
[0032] From the viewpoint of adhesion and resolution, R 4 , R 5i , and R 6is preferably an alkylene group, more preferably an alkylene group having 1 to 10 carbon atoms, even more preferably an alkylene group containing one or more selected from the group consisting of an ethylene group, a propylene group, and a tetramethylene group, even more preferably containing an ethylene group and / or a propylene group, particularly more preferably an ethylene group and / or a propylene group, and extremely preferably an ethylene group.
[0033] The content of the polyglycerin-based (meth)acrylate (A1) in the photosensitive resin composition of this embodiment is, based on the total solids mass of the photosensitive resin composition, preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, even more preferably 7% by mass or more, particularly preferably 10% by mass or more, and most preferably 12% by mass or more. The content of the polyglycerin-based (meth)acrylate (A1) in the photosensitive resin composition of this embodiment is, based on the total solids mass of the photosensitive resin composition, preferably 50% by mass or less, more preferably 48% by mass or less, even more preferably 45% by mass or less, even more preferably 43% by mass or less, and particularly preferably 40% by mass or less.
[0034] (A2) Compound Having No Carboxyl Group and an Ethylenically Unsaturated Bond In this embodiment, the (A2) compound having no carboxyl group and an ethylenically unsaturated bond (hereinafter referred to as (A2) compound or (A2) component) is a compound other than (A1), and is not particularly limited as long as it is a compound having no carboxyl group and one or more ethylenically unsaturated bonds. The (A2) compound preferably contains a compound having two or more ethylenically unsaturated bonds. The (A2) compound may be used alone, or two or more compounds may be used in combination. When the (A) component contains the (A2) compound, the adhesion of the photosensitive resin composition of this embodiment to the substrate and the releasability of the resist pattern are improved.
[0035] The compound (A2) preferably has a (meth)acryloyl group, and more preferably a methacryloyl group.
[0036] The compound (A2) preferably has two ethylenically unsaturated bonds. Examples of the compound having two ethylenically unsaturated bonds include alkyl di(meth)acrylate, 1,3-bis(meth)acryloyloxy-2-propanol, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tricyclodecanol di(meth)acrylate, ethoxylated (hydrogenated) bisphenol A di(meth)acrylate, propoxylated (hydrogenated) bisphenol A di(meth)acrylate, tetramethylene glycoxylated (hydrogenated) bisphenol A di(meth)acrylate, and fluorene di(meth)acrylate.
[0037] Among these, from the viewpoint of excellent adhesion to the substrate, the compound having an ethylenically unsaturated bond preferably includes a di(meth)acrylate compound having a bisphenol A structure, and a compound represented by the following general formula (IV): (In the formula, R 10、 R 11 are each independently a hydrogen atom or a methyl group, R 12 O, R 13 O, R 14 O and R 15 O are each independently an oxyalkylene group, p, q, r and s are each independently an integer of 0 to 40, p+q is 1 to 40, and r+s is 0 to 20.
[0038] R 12 O, R 13 O, R 14 O and R 15Preferably, O is each independently an oxyethylene group or an oxypropylene group. In terms of resolution and adhesion, the compound having a bisphenol A structure preferably has an average value of p+q+r+s of 20 or less, more preferably 16 or less, even more preferably 12 or less, and particularly preferably 10 or less. The average value of p+q+r+s may be 2 or more. Preferably, p, q, r, and s are each independently 0 to 10, and more preferably 2 to 8.
[0039] Commercially available compounds having two ethylenically unsaturated bonds include, for example, NK Ester (registered trademark) A-HD-N, A-NOD-N, A-DOD-N, A-NPG, 701A, A-200, A-400, A-600, A-1000, APG-200, APG-400, APG-700, A-PTMG65, A-DCP, ABE-2, ABE-2.2, ABE-300, A-BPE-4, A-BPE-10, A-BPE-20, A-ABE-30, and A-BP. P-3, HD-N, NOD-N, DOD-N, NPG, 701, 2G, 3G, 4G, 9G, 14G, 23G, 9PG, DCP, BPE-80N, BPE-100, BPE-200, BPE-300, BPE-5 00, BPE-900, BPE-1300N, NK Oligo (registered trademark) UA-4200, UA-160TM, UA-290TM, UA-W2A, UA-4400, UA-122P, U-200PA (manufactured by Shin-Nakamura Chemical Co., Ltd.), Light Acrylate (registered trademark) 3EG-A, 4EG-A, 9EG-A, 14EG-A, PTMGA-250, NP-A, MPD-A, 1.6HX-A, 1.9ND-A, DCP-A, BP-4EAL, BP-4PA, HPP-A, Light Ester G-201P (all manufactured by Kyoeisha Chemical Co., Ltd.), FANCRIL (registered trademark) FA-124AS, FA-023M, FA-121M, FA-124M, FA-125M, FA-129AS, FA-137M, FA-220M, FA-222A, FA-240A, FA-240M, FA-320M, FA-3218M, FA-321A, FA-321M, FA-324A, FA-731A, FA-P240A, FA-P270A, FA-PTG9A, FA-PTG9M, FA-PTG28A, and FA-PTG49A (all manufactured by Showa Denko Materials Co., Ltd.), DPGDA, HDDA, TPGDA, EBECRYL 145, EBECRYL 150, PEG400DA, EBECRYL 11, IRR 214-K, EBECRYL 130, EBECRYL PEG200DMA (all manufactured by Daicel Allnex Co., Ltd.), SR212,SR213, SR230, SR238F, SR259, SR268, SR272, SR306H, SR344, SR349, SR508, CD560, CD561, CD564, SR601, SR602, SR610, SR833S, SR9003, SR9045, SR9209, SR205, SR206, SR209, SR210, SR214, SR231, SR239, SR248, SR252, SR297, SR348, SR480, CD540, CD541, CD542, SR603, SR644, SR9036 (all manufactured by Arkema Co., Ltd.), Examples of such surfactants include KAYARAD (registered trademark) NPGDA, KAYARAD PEG400DA, KAYARAD FM-400, KAYARAD R-167, KAYARAD HX-220, KAYARAD HX-620, KAYARAD R-551, KAYARAD R-712, KAYARAD R-604, and KAYARAD R-684 (all manufactured by Nippon Kayaku Co., Ltd.).
[0040] The compound (A2) may include a compound having three or more ethylenically unsaturated bonds. The compound (A2) may be, for example, a compound having three to six ethylenically unsaturated bonds. In other words, the compound (A2) may include a compound having three to six ethylenically unsaturated bonds.
[0041] Examples of compounds having three or more ethylenically unsaturated bonds include trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, 4,4',4''-ethylidinetrisphenol tri(meth)acrylate, isocyanuric acid tri(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, ditrimethylolpropane (tetra / penta / hexa)(meth)acrylate, and dipentaerythritol (tetra / penta / hexa)(meth)acrylate.
[0042] Examples of the compound having three or more ethylenically unsaturated bonds include alkylene oxide-modified tri(meth)acrylate of trimethylolpropane, alkylene oxide-modified tri(meth)acrylate of glycerin, alkylene oxide-modified 4,4',4''-ethylidinetrisphenol tri(meth)acrylate, alkylene oxide-modified isocyanuric acid tri(meth)acrylate, alkylene oxide-modified pentaerythritol (tri / tetra)(meth)acrylate, alkylene oxide-modified ditrimethylolpropane (tetra / penta / hexa)(meth)acrylate, and alkylene oxide-modified dipentaerythritol (tetra / penta / hexa)(meth)acrylate. From the viewpoint of excellent developability and flexibility, the compound (A2) preferably contains glycerin tri(meth)acrylate or alkylene oxide-modified glycerin tri(meth)acrylate.
[0043] Commercially available compounds having three or more ethylenically unsaturated bonds include, for example, NK Ester (registered trademark) A-TMPT, A-TMPT-9EO, AT-20E, A-GLY-3E, A-GLY-9E, A-GLY-20E, A-9300, A-9200YN, A-TMM-3, A-TMM-3L, and A-TMM- 3LM-N, A-TMMT, ATM-35E, AD-TMP, A-DPH, A-9550, A-DPH-12E, TPOA-50, NK Oligo (registered trademark) UA-7100, UA-1100H, U-6LPA, UA-33H, U-10HA, U-10PA, U-15HA (all manufactured by Shin-Nakamura Chemical Co., Ltd.), Light Acrylate (registered trademark) TMP-A, CPE-3A, PE-4A, and DPE-6A (all manufactured by Kyoeisha Chemical Co., Ltd.), FA-731A (manufactured by Resonac Co., Ltd.), TMPTA, EBECRYL 160S, OTA480, PETIA, PETRA, EBECRYL 40, PETA, EBECRYL 140, EBECRYL 1140, EBECRYL 1142, DPHA, EBECRYL 895, EBECRYL 896, and EBECRYL TMPTMA (all manufactured by Daicel-Allnex Co., Ltd.), Examples of the terpolymer include SR351S, SR368, SR415, SR444, SR454, SR492, SR499, CD501, SR502, SR9020, D9021, SR9035, SR295, SR355, SR399, SR494, and SR9041 (all manufactured by Arkema Co., Ltd.), KAYARAD (registered trademark) GPO-303, KAYARAD TMPTA, KAYARAD THE-330, KAYARAD TPA-330, KAYARAD PET-30, KAYARAD T-1420(T), KAYARAD RP-1040, KAYARAD DPHA, KAYARAD DPEA-12, KAYARAD D-310, and KAYARAD DPCA-20 (all manufactured by Nippon Kayaku Co., Ltd.).
[0044] From the viewpoint of improving resolution, the component (A2) is preferably a compound having 2 to 6 ethylenically unsaturated bonds, and more preferably contains a compound having 2 ethylenically unsaturated bonds.
[0045] From the viewpoint of improving releasability, the component (A2) may contain a compound having one ethylenically unsaturated bond.
[0046] For example, compounds having one ethylenically unsaturated bond include alkylene oxide-modified phenol (meth)acrylate, alkylene oxide-modified nonylphenol (meth)acrylate, alkylene oxide-modified 2-ethylhexyl (meth)acrylate, N-acryloyloxyethyl hexahydrophthalimide, 2-hydroxy-3-phenoxypropyl (meth)acrylate, ω-carboxy-polycaprolactone mono(meth)acrylate, monohydroxyethyl phthalate (meth)acrylate, m-phenoxybenzyl (meth)acrylate, 1-naphthalenemethyl (meth)acrylate, methylphenoxyethyl (meth)acrylate, isopropyl alcohol, methyliso ... Examples of the acrylates include methyl (meth)acrylate, hexyl (meth)acrylate, isodecyl (meth)acrylate, n-lauryl (meth)acrylate, tetradecyl (meth)acrylate, n-stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, 2-decyl-1-tetradecanyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, and 3,3,4,4,5,5,6,6,7,7,8,8-dodecafluorooctyl (meth)acrylate.
[0047] The upper limit of the ratio of component (A1) to component (A2) (i.e., the ratio of the content of component (A1) to the content of component (A2)) is preferably 4 or less, more preferably 3.5 or less, even more preferably 3 or less, even more preferably 2.75 or less, particularly preferably 2.5 or less, and most preferably 2 or less. The lower limit of the ratio of component (A1) to component (A2) is preferably 0.05 or more, more preferably 0.1 or more, even more preferably 0.12 or more, even more preferably 0.15 or more, and particularly preferably 0.20 or more.
[0048] In particular, the upper limit of the ratio of the total amount of compounds having one or two ethylenically unsaturated bonds in component (A2) to the total amount of compounds having one or two ethylenically unsaturated bonds in component (A2) (i.e., the ratio of the content of component (A1) to the total amount of compounds having one or two ethylenically unsaturated bonds in component (A2)) is preferably 4 or less, more preferably 3.5 or less, even more preferably 3 or less, even more preferably 2.75 or less, particularly preferably 2.5 or less, and most preferably 2 or less. The lower limit of the ratio of the total amount of compounds having one or two ethylenically unsaturated bonds in component (A2) is preferably 0.05 or more, more preferably 0.1 or more, even more preferably 0.12 or more, even more preferably 0.15 or more, and particularly preferably 0.20 or more.
[0049] The content of the compound (A) having an ethylenically unsaturated bond in the photosensitive resin composition of this embodiment is preferably 30% by mass or more, and more preferably 35% by mass or more, based on the total solid mass of the photosensitive resin composition, from the viewpoints of sensitivity, tackiness, and followability. Furthermore, the content of the compound (A) having an ethylenically unsaturated bond in the photosensitive resin composition is preferably 50% by mass or less, more preferably 45% by mass or less, and more preferably 43% by mass or less, based on the total solid mass of the photosensitive resin composition, from the viewpoints of edge fusion property, tackiness, and resolution. In one aspect, the content of the compound (A) having an ethylenically unsaturated bond in the photosensitive resin composition of this embodiment is preferably 20% by mass or more and 60% by mass or less, based on the total solid mass of the photosensitive resin composition, from the viewpoints of resolution, adhesion, and releasability.
[0050] Furthermore, from the viewpoints of flexibility, resolution, and adhesion, the ratio of the content of the compound having three or more ethylenically unsaturated groups to the content of the compound having an ethylenically unsaturated bond (A) contained in the photosensitive resin composition of the present embodiment (i.e., the ratio of the content of the compound having three or more ethylenically unsaturated groups / the content of the compound having an ethylenically unsaturated bond (A)) is preferably 0.95 or less, and more preferably 0.90 or less.
[0051] From the viewpoints of edge fusion property, tackiness, and resolution, the upper limit of the ratio of the content of the compound having an ethylenic unsaturated bond (A) to the content of the alkali-soluble resin (B) contained in the photosensitive resin composition of this embodiment (i.e., the ratio of the content of the compound having an ethylenic unsaturated bond (A) / the content of the alkali-soluble resin (B)) is preferably 1.4 or less, more preferably 1.3 or less, even more preferably 1.2 or less, even more preferably 1.1 or less, particularly preferably 1.0 or less, and most preferably 0.9 or less. The lower limit of the ratio of the content of the compound having an ethylenic unsaturated bond (A) / the content of the alkali-soluble resin (B) is preferably 0.50 or more, more preferably 0.60 or more, even more preferably 0.70 or more, even more preferably 0.75 or more, and particularly preferably 0.80 or more.
[0052] The photosensitive resin composition of this embodiment preferably has an ethylenically unsaturated bond content of 0.10 mol to 0.30 mol per 100 g of solids in the photosensitive resin composition. By setting the content to 0.10 mol or more, components of the photosensitive resin composition are eluted from the cured resist pattern in the water washing step after development, preventing contamination during the water washing step. By setting the content to 0.30 mol or less, the cured resist pattern is chipped and removed in the water washing step after development, preventing contamination during the water washing step.
[0053] The amount of ethylenically unsaturated bonds per 100 g of solids in the photosensitive resin composition of this embodiment is preferably 0.10 mol or more, more preferably 0.11 mol or more, even more preferably 0.12 mol or more, and even more preferably 0.13 mol or more. Furthermore, the amount of ethylenically unsaturated bonds per 100 g of solids in the photosensitive resin composition of this embodiment is preferably 0.30 mol or less, more preferably 0.28 mol or less, even more preferably 0.25 mol or less, even more preferably 0.22 mol or less, particularly preferably 0.20 mol or less, especially more preferably 0.18 mol or less, and extremely preferably 0.15 mol or less. The amount of ethylenically unsaturated bonds per 100 g of solids in the photosensitive resin composition of this embodiment is more preferably 0.10 mol to 0.25 mol, even more preferably 0.10 mol to 0.20 mol, even more preferably 0.11 mol to 0.20 mol, and extremely preferably 0.11 mol to 0.15 mol.
[0054] (B) Alkali-Soluble Resin In this embodiment, the (B) alkali-soluble resin (hereinafter referred to as component (B)) is preferably obtained by polymerizing at least one type of first monomer described later, and more preferably obtained by copolymerizing at least one type of first monomer with at least one type of second monomer described later.
[0055] The first monomer is a monomer having a carboxyl group in the molecule. Examples of the first monomer include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, 4-vinylbenzoic acid, maleic anhydride, and maleic acid half ester. Among these, (meth)acrylic acid is preferred, and methacrylic acid is more preferred, from the viewpoint of excellent adhesion and resolution.
[0056] The copolymerization ratio of the first monomer is preferably in the range of 10 to 50% by mass, based on the total mass of all monomer components. From the viewpoint of excellent adhesion and resolution, the copolymerization ratio is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 18% by mass or more, and even more preferably 21% by mass or more. From the viewpoint of excellent adhesion and resolution, the copolymerization ratio is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less, even more preferably 30% by mass or less, and particularly preferably 27% by mass or less. When two or more types of first monomers are polymerized and used, it is preferable that the total copolymerization ratio of each is within the above range.
[0057] The second monomer is a monomer having at least one ethylenically unsaturated bond in the molecule and having no carboxyl group. Examples of the second monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, pentamethylpiperidyl (meth)acrylate, tetramethylpiperidyl (meth)acrylates such as methyl methyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, methoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate; styrene derivatives such as styrene, methylstyrene, vinyltoluene, tert-butoxystyrene, acetoxystyrene, N-phenylmaleimide, styrene dimer, and styrene trimer; esters of vinyl alcohol such as vinyl acetate; and (meth)acrylonitrile.
[0058] The weight average molecular weight Mw of the alkali-soluble resin (B) is preferably 10,000 to 60,000. From the viewpoint of achieving both flexibility and resolution of the resist pattern, it is preferable to set the weight average molecular weight Mw to 60,000 or less, and from the same viewpoint, it is more preferable to set it to 55,000 or less, and even more preferable to set it to 50,000 or less. From the same viewpoint, it is preferable to set the weight average molecular weight Mw to 10,000 or more, more preferably 12,000 or more, and even more preferably 14,000 or more.
[0059] The polydispersity (Mw / Mn: weight average molecular weight / number average molecular weight) of the alkali-soluble resin (B) is preferably 1.0 to 6.0, more preferably 1.0 to 5.0, even more preferably 1.0 to 4.0, and particularly preferably 1.0 to 3.0.
[0060] The alkali-soluble resin (B) can be used alone or in a mixture of two or more. When two or more (B) components are used in combination, the monomer contents in the multiple (B) components are preferably selected so that the weighted average molecular weight and polydispersity, where the content ratio of each (B) component is taken as the weight, fall within the following ranges. In this disclosure, when two or more (B) components are used in combination, the weighted average value refers to the sum of the weight ratio of each alkali-soluble resin to the total weight of the mixed (B) components, multiplied by the weight average molecular weight or polydispersity of each alkali-soluble resin. The weighted average weight average molecular weight of the (B) component is preferably 10,000 or more, or 15,000 or more, or 20,000 or more, and preferably 60,000 or less, or 55,000 or less, or 50,000 or less. The weighted average polydispersity of component (B) is preferably 1.0 to 6.0, more preferably 1.0 to 5.0, even more preferably 1.0 to 4.0, and particularly preferably 1.0 to 3.0.
[0061] The synthesis of the alkali-soluble resin (B) is preferably carried out by adding an appropriate amount of a radical polymerization initiator such as benzoyl peroxide and azoisobutyronitrile to a solution obtained by diluting one or more of the above-described monomers with a solvent such as acetone, methyl ethyl ketone, or isopropanol, and then heating and stirring the solution. The synthesis may also be carried out by adding a portion of the mixture containing the monomer and solvent dropwise to a reaction solution containing the radical polymerization initiator. After the polymerization reaction is complete, further solvent may be added to adjust the concentration to the desired level. As a means for synthesizing the component (B), in addition to solution polymerization, living radical polymerization, bulk polymerization, suspension polymerization, or emulsion polymerization may also be used.
[0062] The content of the alkali-soluble resin (B) in the photosensitive resin composition of this embodiment may be 10% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, 45% by mass or more, 50% by mass or more, 55% by mass or more, or 60% by mass or more, based on the total solid mass of the photosensitive resin composition. Furthermore, the content of the alkali-soluble resin (B) in the photosensitive resin composition of this embodiment may be 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, or 50% by mass or less, based on the total solid mass of the photosensitive resin composition.
[0063] Based on the total solid content by mass of the photosensitive resin composition of this embodiment, it is preferable to set the content of the alkali-soluble resin (B) to 90% by mass or less from the viewpoint of controlling the development time, and it is preferable to set the content of the alkali-soluble resin (B) to 10% by mass or more from the viewpoint of suppressing protrusion of the resist layer from the edge surfaces of the film.
[0064] Among these, from the viewpoint of excellent adhesion to the substrate, it is preferable that the component (B) contains either one or both of styrene and benzyl (meth)acrylate. That is, it is preferable that the component (B) contains structural units derived from styrene and / or benzyl (meth)acrylate. When the alkali-soluble resin (B) contains multiple alkali-soluble resins, it may contain both an alkali-soluble resin containing styrene and an alkali-soluble resin containing benzyl (meth)acrylate.
[0065] From the viewpoints of flexibility, resolution, and adhesion, the total content of the components (A) and (B) contained in the photosensitive resin composition of this embodiment is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, based on the total solid mass of the photosensitive resin composition. From the viewpoints of sensitivity, resolution, and adhesion, the total content of the components (A) and (B) contained in the photosensitive resin composition of this embodiment is preferably 98% by mass or less, more preferably 96% by mass or less, based on the total solid mass of the photosensitive resin composition.
[0066] When component (B) contains a structural unit derived from styrene, from the viewpoint of adhesion, the styrene content in component (B) is preferably 25% by mass or more, or may be 30% by mass or more, or may be 35% by mass or more, and the styrene content in component (B) may be 80% by mass or less, or may be 75% by mass or less, or may be 70% by mass or less, or may be 65% by mass or less, or may be 60% by mass or less.
[0067] When the component (B) contains a structural unit derived from styrene, from the viewpoint of adhesion, the styrene content in the component (B) may be 25% by mass or more and 80% by mass or less, or 30% by mass or more and 80% by mass or less, or 35% by mass or more and 80% by mass or less.
[0068] From the viewpoints of developability, resolution, and adhesion, the content of component (B) contained in the photosensitive resin composition is preferably 70% by mass or less, more preferably 65% by mass or less, even more preferably 63% by mass or less, and particularly preferably 60% by mass or less, based on the total content of components (A) and (B). The content of component (B) contained in the photosensitive resin composition is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, based on the total content of components (A) and (B).
[0069] Photosensitive resin laminate according to another embodiment In one aspect, the photosensitive resin laminate according to another embodiment includes a support film and a resist layer containing a photosensitive resin composition. The photosensitive resin composition constituting the photosensitive resin laminate according to one aspect of the other embodiment includes (A) a compound having an ethylenically unsaturated bond, and (B) an alkali-soluble resin (hereinafter, referred to as component (B)). The support film included in the photosensitive resin laminate according to the other embodiment is the same as described above.
[0070] In another embodiment of the photosensitive resin laminate, the photosensitive resin composition preferably contains, as the compound (A) having an ethylenically unsaturated bond (in one aspect, component (A)), (A3) a compound that does not have a quaternary carbon and / or an aromatic ring and has four or more ethylenically unsaturated bonds in one molecule (hereinafter referred to as (A3) compound or (A3) component). In another embodiment of the photosensitive resin laminate, the photosensitive resin composition preferably contains, as the compound (A) having an ethylenically unsaturated bond, (A4) a compound that has a quaternary carbon and / or an aromatic ring, does not have a carboxyl group, and has an ethylenically unsaturated bond (hereinafter referred to as (A4) compound or (A4) component). In another embodiment of the photosensitive resin laminate, the component (A) of the photosensitive resin composition more preferably includes: (A3) a compound having no quaternary carbon and / or aromatic ring and having four or more ethylenically unsaturated bonds in one molecule; and (A4) a compound having a quaternary carbon and / or aromatic ring, having no carboxyl group, and having an ethylenically unsaturated bond.
[0071] (A3) Compound Having No Quaternary Carbon and / or Aromatic Ring and Four or More Ethylenically Unsaturated Bonds in One Molecule The (A3) compound is a compound having no quaternary carbon and / or aromatic ring and four or more ethylenically unsaturated bonds in one molecule. An example of the (A3) compound is the (A1) compound. The same applies as above for the (A1) compound. Furthermore, the (A3) compound is preferably a di(meth)acrylate compound having a bisphenol A structure, and preferably a compound represented by the following general formula (IV). Since the (A3) compound does not have a quaternary carbon and / or aromatic ring, it is presumed that a resist pattern formed using a photosensitive resin composition containing the (A3) compound as component (A) has high flexibility. Furthermore, since the (A3) compound has four or more ethylenically unsaturated bonds in one molecule, it is presumed that the structure of the (A3) compound is complexly bonded upon curing by exposure, thereby strengthening the resist pattern. For this reason, it is presumed that a resist pattern formed using a photosensitive resin composition containing the compound (A3) has excellent toughness, which in turn results in excellent flexibility, resolution, and adhesion.
[0072] When the content of structural units derived from (meth)acrylic acid, styrene, and benzyl (meth)acrylate in the component (B) is within the above-mentioned range, a good balance can be achieved between developability, flexibility, and rigidity when a photosensitive resin composition containing the compound (A3) is used, and the effects of excellent flexibility, resolution, and adhesion can be easily obtained.
[0073] (A4) Compound Having a Quaternary Carbon and / or an Aromatic Ring, No Carboxyl Group, and Having an Ethylenically Unsaturated Bond The (A4) compound is a compound having a quaternary carbon and / or an aromatic ring, no carboxyl group, and an ethylenically unsaturated bond. In another embodiment of the photosensitive resin laminate, the photosensitive resin composition preferably contains, as the (A) compound having an ethylenically unsaturated bond, and (A4) a compound having a quaternary carbon and / or an aromatic ring, no carboxyl group, and an ethylenically unsaturated bond.
[0074] Because the (A4) compound has a quaternary carbon and / or an aromatic ring, it is presumed that a resist pattern formed using a photosensitive resin composition containing the (A4) compound as component (A) is rigid. Therefore, it is presumed that by using a photosensitive resin composition containing both the (A3) compound and the (A4) compound, a balance between flexibility and rigidity can be achieved, and a strong resist pattern with excellent toughness can be formed. Therefore, a resist pattern obtained using a photosensitive resin composition containing both the (A3) compound and the (A4) compound is particularly excellent in resolution and adhesion.
[0075] Examples of the (A4) compound include the compounds listed as the (A2) component. The same applies to the (A2) compound as described above. Examples of the (A4) compound include, among the compounds listed as the (A2) component, alkylene oxide-modified phenol (meth)acrylate, alkylene oxide-modified nonylphenol (meth)acrylate, bisphenol A di(meth)acrylate, bisphenol di F (meth)acrylate, ethoxylated (hydrogenated) bisphenol A di(meth)acrylate, propoxylated (hydrogenated) bisphenol A di(meth)acrylate, tetramethyleneglycoxylated (hydrogenated) bisphenol A di(meth)acrylate, naphthalene di(meth)acrylate, fluorene di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and isocyanuric acid tri(meth)acrylate. , pentaerythritol (tri / tetra)(meth)acrylate, ditrimethylolpropane (tetra / penta / hexa)(meth)acrylate, dipentaerythritol (tetra / penta / hexa)(meth)acrylate, alkylene oxide-modified tri(meth)acrylate of trimethylolpropane, alkylene oxide-modified isocyanuric acid tri(meth)acrylate, alkylene oxide-modified pentaerythritol (tri / tetra)(meth)acrylate, alkylene oxide-modified ditrimethylolpropane (tetra / penta / hexa)(meth)acrylate, alkylene oxide-modified dipentaerythritol (tetra / penta / hexa)(meth)acrylate, etc. Among these, bisphenol A di(meth)acrylate is preferred as the (A4) compound.
[0076] Examples of commercially available products that can be used as the compound (A4) include A-1000, A-BPE-20, A-BPE-30, 23G, BPE-900, and BPE-1300N (all manufactured by Shin-Nakamura Chemical Co., Ltd.), 25PDC-900B, 30PDC-950B-H, and 40PDC-1700B (all manufactured by NOF Corporation), BP-1206A (manufactured by Toho Chemical Industry Co., Ltd.), FA-2100A, FA-2200A, FA-P2200M, FA-P2300M, FA-P2200A, FA-P2300A, FA-3218A, and FA-027M (all manufactured by Resonac Inc.).
[0077] The (A4) compound preferably contains a compound having one or two ethylenically unsaturated bonds. The amount of ethylenically unsaturated bonds per 100 g of the (A4) compound is preferably 0.25 mol or less. This makes it easier to achieve a balance between flexibility and rigidity when forming a resist pattern using a photosensitive resin composition containing both the (A3) compound and the (A4) compound, and thus makes it easier to form a resist pattern that is both excellent in toughness and strong, resulting in excellent flexibility and adhesion. From the above viewpoints, the amount of ethylenically unsaturated bonds per 100 g of the (A4) compound is more preferably 0.22 mol or less, and even more preferably 0.20 mol or less. The amount of ethylenically unsaturated bonds per 100 g of the (A4) compound may be 0.10 mol or more.
[0078] The photosensitive resin composition contained in the photosensitive resin laminate of another embodiment includes component (B). The same applies to component (B). Component (B) preferably includes a copolymer containing a structural unit derived from (meth)acrylic acid as a monomer component. In one aspect, the content of structural units derived from (meth)acrylic acid in the copolymer in component (B) is preferably 27% by mass or less, more preferably 25% by mass or less, and even more preferably 23% by mass or less. The content of structural units derived from (meth)acrylic acid in the copolymer in component (B) may be 10% by mass or more, or may be 15% by mass or more.
[0079] (C) Photopolymerization Initiator In this embodiment, the photosensitive resin composition preferably contains a (C) photopolymerization initiator (hereinafter referred to as component (C)). Examples of the (C) photopolymerization initiator include a hexaarylbiimidazole compound, an N-aryl-α-amino acid compound, a quinone compound, an aromatic ketone compound, an anthracene derivative, an acetophenone compound, an acylphosphine oxide compound, a benzoin compound, a benzoin ether compound, a dialkyl ketal compound, a thioxanthone compound, a dialkylaminobenzoic acid ester compound, an oxime ester compound, an acridine compound, a pyrazoline derivative, an N-arylamino acid ester compound, and a halogen compound. In one aspect, the (C) component preferably contains a hexaarylbiimidazole compound.
[0080] An example of the hexaarylbiimidazole compound is a lophine dimer, ie, a dimer of 2,4,5-triarylimidazole.
[0081] Lophine dimers, i.e., dimers of 2,4,5-triarylimidazole, include dimers of 2-(o-chlorophenyl)-4,5-diphenylimidazole (also known as 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole), 2-(o-chlorophenyl)-4,5-bis-(m-methoxyphenyl)biimidazole, 2-(p-methoxyphenyl)-4,5-diphenylbiimidazole, 2,2',5-tris-(o-chlorophenyl)-4-(3,4-dimethoxyphenyl)-4',5 '-diphenylbiimidazole, 2,4-bis-(o-chlorophenyl)-5-(3,4-dimethoxyphenyl)-diphenylbiimidazole, 2,4,5-tris-(o-chlorophenyl)-diphenylbiimidazole, 2-(o-chlorophenyl)-bis-4,5-(3,4-dimethoxyphenyl)-biimidazole, 2,2'-bis-(2-fluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3-difluoromethylphenyl)-4,4',5,5'-tetrakis-( 3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,4-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,5-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,6-difluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,4-trifluorophenyl)-4,4',5,5'-tetrakis- (3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,6-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,4,5-trifluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,4,6-trifluorophenyl)-4,4',5,Examples include 5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,4,5-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, 2,2'-bis-(2,3,4,6-tetrafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole, and 2,2'-bis-(2,3,4,5,6-pentafluorophenyl)-4,4',5,5'-tetrakis-(3-methoxyphenyl)-biimidazole.
[0082] From the viewpoint of high sensitivity, resolution, and adhesion, it is preferable to contain a lophine dimer as component (C), and in particular, 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer is preferred.
[0083] Examples of N-aryl-α-amino acid compounds include N-phenylglycine, N-methyl-N-phenylglycine, and N-ethyl-N-phenylglycine, etc. Among these, N-phenylglycine is preferred because of its high sensitizing effect.
[0084] Examples of quinone compounds include 2-ethylanthraquinone, octaethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, 2,3-dimethylanthraquinone, and 3-chloro-2-methylanthraquinone.
[0085] Examples of aromatic ketone compounds include benzophenone compounds. Examples of benzophenone compounds include benzophenone, Michler's ketone [4,4'-bis(dimethylamino)benzophenone], and 4-methoxy-4'-dimethylaminobenzophenone. From the viewpoints of sensitization effect and adhesion, examples of aromatic ketone compounds include 4,4'-bis(diethylamino)benzophenone.
[0086] In the present disclosure, the term "anthracene derivative" includes both anthracene and compounds derived therefrom. Examples of anthracene derivatives include anthracene, 9,10-dialkoxyanthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 9,10-dibutoxyanthracene, 9,10-diphenylanthracene, 2-ethylanthraquinone, octaethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, and 10-phenyl-9-anthraceneboronic acid. From the viewpoints of sensitization effect and adhesion, 9,10-dibutoxyanthracene and 9,10-diphenylanthracene are preferred, and 9,10-diphenylanthracene is particularly preferred.
[0087] Examples of acetophenone compounds include 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, etc. Commercially available acetophenone compounds include the Irgacure series (manufactured by Ciba Specialty Chemicals: Irgacure-907, Irgacure-369, and Irgacure-379, etc.).
[0088] Examples of acylphosphine oxide compounds include 2,4,6-trimethylbenzyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, etc. Commercially available acylphosphine oxide compounds include Lucirin TPO (manufactured by BASF) and Irgacure-819 (manufactured by Ciba Specialty Chemicals).
[0089] Examples of benzoin compounds and benzoin ether compounds include benzoin, benzoin ethyl ether, benzoin phenyl ether, methylbenzoin, and ethylbenzoin. Examples of dialkyl ketal compounds include benzyl dimethyl ketal and benzyl diethyl ketal. Examples of thioxanthone compounds include 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and 2-chlorothioxanthone. Examples of dialkylaminobenzoic acid ester compounds include ethyl dimethylaminobenzoate, ethyl diethylaminobenzoate, ethyl-p-dimethylaminobenzoate, and 2-ethylhexyl-4-(dimethylamino)benzoate.
[0090] Examples of oxime ester compounds include 1-phenyl-1,2-propanedione-2-O-benzoyloxime, 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime, etc. Commercially available oxime ester compounds include CGI-325, Irgacure-OXE01, and Irgacure-OXE02 (all manufactured by Ciba Specialty Chemicals).
[0091] As the acridine compound, 1,7-bis(9,9'-acridinyl)heptane or 9-phenylacridine is preferred in terms of sensitivity, resolution, availability, etc.
[0092] From the viewpoints of adhesion and rectangularity of the resist pattern, the pyrazoline derivatives are preferably 1-phenyl-3-(4-tert-butyl-styryl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-butyl-phenyl)-pyrazoline, 1-phenyl-3-(4-biphenyl)-5-(4-tert-octyl-phenyl)-pyrazoline, and 1-phenyl-3-(4-methoxystyryl)-5-(4-methoxyphenyl)-pyrazoline.
[0093] Examples of the ester compound of N-arylamino acid include methyl ester of N-phenylglycine, ethyl ester of N-phenylglycine, n-propyl ester of N-phenylglycine, isopropyl ester of N-phenylglycine, 1-butyl ester of N-phenylglycine, 2-butyl ester of N-phenylglycine, tert-butyl ester of N-phenylglycine, pentyl ester of N-phenylglycine, hexyl ester of N-phenylglycine, pentyl ester of N-phenylglycine, and octyl ester of N-phenylglycine.
[0094] Examples of halogen compounds include amyl bromide, isoamyl bromide, isobutylene bromide, ethylene bromide, diphenylmethyl bromide, benzyl bromide, methylene bromide, tribromomethylphenyl sulfone, carbon tetrabromide, tris(2,3-dibromopropyl)phosphate, trichloroacetamide, amyl iodide, isobutyl iodide, 1,1,1-trichloro-2,2-bis(p-chlorophenyl)ethane, chlorinated triazine compounds, and diaryliodonium compounds. Of these, tribromomethylphenyl sulfone is preferred.
[0095] The content of the (C) photopolymerization initiator in the photosensitive resin composition of this embodiment is preferably 0.01 to 20 mass %, and more preferably 0.5 to 10 mass %, based on the total mass of solids in the photosensitive resin composition. By adjusting the content of the (C) photopolymerization initiator within the above range, sufficient sensitivity can be easily obtained, making it easier to transmit light sufficiently to the bottom of the photosensitive resin composition layer, and ultimately making it easier to achieve improved resolution.
[0096] From the viewpoints of high sensitivity, resolution, and adhesion, it is preferable that the photopolymerization initiator (C) contains a lophine dimer. In this case, the content of the lophine dimer in the photosensitive resin composition is preferably 0.1 to 15 mass%, and more preferably 0.5 to 10 mass%, based on the total mass of the solid content of the photosensitive resin composition.
[0097] As the (C) photopolymerization initiator, it is preferable to use an anthracene derivative and a hexaarylbiimidazole compound in combination. In this case, the content of the anthracene derivative contained in the (C) photopolymerization initiator in the photosensitive resin composition of this embodiment is preferably 0.5 mass% or less, and more preferably 0.01 mass% to 0.4 mass%, based on the total solid mass of the photosensitive resin composition. Furthermore, the content of the hexaarylbiimidazole compound contained in the (C) photopolymerization initiator in the photosensitive resin composition of this embodiment is preferably 0.1 to 10 mass%, and more preferably 0.5 to 8 mass%, based on the total solid mass of the photosensitive resin composition.
[0098] The content of the (C) photopolymerization initiator in the photosensitive resin composition of this embodiment is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 18% by mass or less, based on the content of the (A) compound having an ethylenically unsaturated bond. The content of the (C) photopolymerization initiator in the photosensitive resin composition of this embodiment is preferably 2% by mass or more, more preferably 3% by mass or more, even more preferably 4% by mass or more, and particularly preferably 5% by mass or more, based on the content of the (A) compound having an ethylenically unsaturated bond.
[0099] (D) Polymerization Inhibitor In the present embodiment, the photosensitive resin composition may contain (D) a polymerization inhibitor. Examples of the (D) polymerization inhibitor include a free radical polymerization inhibitor, a phenolic polymerization inhibitor, hydroquinone, quinone, nitrobenzene, phenothiazine, phenoxazine, catechol, or a derivative thereof.
[0100] Examples of the free radical polymerization inhibitor include nitroso compounds such as p-nitrosophenol, nitrosobenzene, N-nitrosodiphenylamine, isononyl nitrite, N-nitrosocyclohexylhydroxylamine, N-nitrosophenylhydroxylamine, N,N'-dinitrosophenylenediamine, and salts thereof; and hindered amine compounds such as 2,2,6,6-tetramethylpiperidine-1-oxyl, 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl, 4-hydroxy-2,2,6,6-tetramethyl-1-hydroxypiperidine, 4-oxo-2,2,6,6-tetramethylpiperidine-1-oxyl, and 4-oxo-2,2,6,6-tetramethyl-1-oxypiperidine.
[0101] Examples of phenolic polymerization inhibitors include p-methoxyphenol, hydroquinone, pyrogallol, tert-butylcatechol, 2,6-di-tert-butyl-p-cresol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,6-di-tert-butyl-4-methylphenol, 2,5-di-tert-amylhydroquinone, 2,5-di-tert-butylhydroquinone, 2,2'-methylenebis(4-methyl-6- tert-butylphenol), bis(2-hydroxy-3-tert-butyl-5-ethylphenyl)methane, triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythrityl tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5 -di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-tert-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris-(3,5-di-te rt-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, styrenated phenol (for example, Antage SP, manufactured by Kawaguchi Chemical Industry Co., Ltd.), tribenzylphenol (for example, TBP, a phenol having 1 to 3 benzyl groups, manufactured by Kawaguchi Chemical Industry Co., Ltd.), and biphenol.
[0102] In the present disclosure, the term "hydroquinone, quinone, nitrobenzene, phenothiazine, phenoxazine, and catechol, and derivatives thereof" includes both hydroquinone, quinone, nitrobenzene, phenothiazine, phenoxazine, and catechol, and compounds derived therefrom. Examples of hydroquinone derivatives include methylhydroquinone, 2-tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, and 2,6-di-tert-butylhydroquinone. Examples of quinone derivatives include tert-butylbenzoquinone, 2,6-di-tert-butyl-1,4-benzoquinone, and 2,5-di-tert-butyl-1,4-benzoquinone.
[0103] Examples of nitrobenzene derivatives include 4-nitrotoluene, etc. Examples of phenothiazine derivatives include 2,8-dioctylphenothiazine, 2-methoxyphenothiazine, 3-methoxyphenothiazine, 2-methylphenothiazine, 2-ethylphenothiazine, 2-trifluoromethylphenothiazine, 3,7-dibutylphenothiazine, 3,7-dioctylphenothiazine, 3,7-dicumylphenothiazine, 2-cyano-8-methoxyphenothiazine, 2-cyanophenothiazine, 2-bromophenothiazine, 2-chlorophenothiazine, bis-(α-dimethylbenzyl)phenothiazine, and bis-(α-methylbenzyl)phenothiazine. Examples of phenoxazine derivatives include 1-methyl-phenoxazine, 2-methyl-phenoxazine, 3-methyl-phenoxazine, 4-methyl-phenoxazine, 10-methyl-phenoxazine, 2-hydroxy-phenoxazine, 3-hydroxy-phenoxazine, 4-hydroxy-phenoxazine, 10-bromo-phenoxazine, 3,7-dimethyl-phenoxazine, 2,8-dimethyl-phenoxazine, 1-amino-phenoxazine, 2-amino-phenoxazine, 3-amino-phenoxazine, 2-ethyl-phenoxazine, 3-ethyl-phenoxazine, 2-carbonitrile-phenoxazine, 3-carbonitrile-phenoxazine, 2-methoxy-phenoxazine, 3-methoxy-phenoxazine, and 12H-benzophenoxazine.
[0104] Examples of catechol derivatives include 2-methylcatechol, 3-methylcatechol, 4-methylcatechol, 2-ethylcatechol, 3-ethylcatechol, 4-ethylcatechol, 2-propylcatechol, 3-propylcatechol, 4-propylcatechol, 2-n-butylcatechol, 3-n-butylcatechol, 4-n-butylcatechol, 2-tert-butylcatechol, 3-tert-butylcatechol, 4-tert-butylcatechol, and 3,5-di-tert-butylcatechol.
[0105] By including phenothiazine or a phenothiazine derivative and a phenolic polymerization inhibitor, the NH group contained in the phenothiazine moiety and the OH group of the phenolic polymerization inhibitor form a hydrogen bond, thereby preventing the phenolic polymerization inhibitor from volatilizing or diffusing from the photosensitive resin composition layer. In other words, it is possible to provide a photosensitive resin composition and a method for forming a resist pattern that are excellent in sensitivity and resolution and are not affected by production conditions and storage conditions that are determined by the film thickness.
[0106] From the above viewpoint, the photosensitive resin composition of this embodiment preferably contains phenothiazine or a phenothiazine derivative as the polymerization inhibitor (D). In this case, the content of the phenothiazine or the phenothiazine derivative in the photosensitive resin composition of this embodiment is preferably 1% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.4% by mass or less, and particularly preferably 0.3% by mass or less, based on the total solid mass of the photosensitive resin composition of this embodiment. Furthermore, the content of the phenothiazine or the phenothiazine derivative in the photosensitive resin composition of this embodiment is preferably 0.0001% by mass or more, more preferably 0.0005% by mass or more, even more preferably 0.001% by mass or more, and even more preferably 0.002% by mass or more, based on the total solid mass of the photosensitive resin composition of this embodiment.
[0107] From the viewpoint of resolution, the photosensitive resin composition of this embodiment preferably contains catechol or a catechol derivative as the polymerization inhibitor (D), and particularly preferably contains 3-tert-butylcatechol or 4-tert-butylcatechol. In this case, the content of the catechol or catechol derivative in the photosensitive resin composition of this embodiment is preferably 1% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.4% by mass or less, and particularly preferably 0.3% by mass or less, based on the total solids mass of the photosensitive resin composition of this embodiment. Furthermore, the content of the catechol or catechol derivative in the photosensitive resin composition of this embodiment is preferably 0.0001% by mass or more, more preferably 0.0005% by mass or more, even more preferably 0.001% by mass or more, and even more preferably 0.002% by mass or more, based on the total solids mass of the photosensitive resin composition of this embodiment.
[0108] The content of the polymerization inhibitor (D) in the photosensitive resin composition of this embodiment is preferably 0.0001% by mass to 10% by mass, based on the total solids mass of the photosensitive resin composition of this embodiment. From the viewpoint of excellent adhesion and resolution, the content of the polymerization inhibitor (D) of this embodiment is preferably 0.0001% by mass or more, more preferably 0.0005% by mass or more, even more preferably 0.001% by mass or more, even more preferably 0.005% by mass or more, and particularly preferably 0.01% by mass or more. On the other hand, from the viewpoint of minimal sensitivity reduction and improved resolution, the content of the polymerization inhibitor (D) of this embodiment is preferably 10% by mass or less, more preferably 8% by mass or less, even more preferably 5% by mass or less, even more preferably 3% by mass or less, particularly preferably 2% by mass or less, and most preferably 1.5% by mass or less.
[0109] Additives The photosensitive resin composition according to this embodiment may contain additives such as dyes, adhesion aids, and plasticizers.
[0110] Dye In this embodiment, a dye may be contained in the photosensitive resin composition. In one aspect, a color-forming dye that develops color upon irradiation with light may be contained in the photosensitive resin composition. A dye is preferably added to the dry film resist, which is one aspect of the photosensitive resin laminate of this embodiment. Adding a dye improves the contrast of the resist pattern formed on the substrate after development, which also helps improve resolution.
[0111] A preferred dye is diamond green. Known color-forming dyes include, for example, combinations of leuco dyes and halogen compounds. Examples of leuco dyes include tris(4-dimethylamino-2-methylphenyl)methane (dye name: leuco crystal violet) and tris(4-dimethylamino-2-methylphenyl)methane (dye name: leucomalachite green). Examples of halogen compounds include amyl bromide, isoamyl bromide, isobutylene bromide, ethylene bromide, diphenylmethyl bromide, benzal bromide, methylene bromide, tribromomethylphenyl sulfone, carbon tetrabromide, tris(2,3-dibromopropyl)phosphate, trichloroacetamide, amyl iodide, isobutyl iodide, 1,1,1-trichloro-2,2-bis(p-chlorophenyl)ethane, and hexachloroethane.
[0112] Adhesion Aid In this embodiment, an adhesion aid may be contained in the photosensitive resin composition. It is preferable to add an adhesion aid to the dry film resist, which is one aspect of the photosensitive resin laminate of this embodiment. Adding an adhesion aid helps improve the adhesion of the resist pattern formed on the substrate to copper after development.
[0113] As the adhesion aid, triazoles and benzotriazoles are preferred, and carboxybenzotriazole is more preferred.
[0114] In this embodiment, if necessary, an additive such as a plasticizer may be contained in the photosensitive resin composition. Examples of additives such as a plasticizer include phthalate esters such as diethyl phthalate, o-toluenesulfonic acid amide, p-toluenesulfonic acid amide, tributyl citrate, triethyl citrate, triethyl acetyl citrate, tri-n-propyl acetyl citrate, tri-n-butyl acetyl citrate, polypropylene glycol, polyethylene glycol, polyethylene glycol alkyl ether, and polypropylene glycol alkyl ether.
[0115] <Photosensitive resin laminate> The photosensitive resin laminate of this embodiment includes a support film and a resist layer (in one embodiment, a photosensitive resin composition layer) containing a photosensitive resin composition, and the support film and resist layer are the same as described above. The photosensitive resin laminate of this embodiment may be, for example, formed by laminating at least one resist layer on a support film, or by laminating two or more resist layers on a support film. From the viewpoint of easily achieving the effects of this embodiment, the photosensitive resin laminate of this embodiment is preferably a dry film resist or a transfer film, and more preferably a dry film resist.
[0116] The photosensitive resin laminate of the present embodiment may include a protective film in addition to the support film and the resist layer. When the photosensitive resin laminate of the present embodiment includes the support film, the resist layer, and the protective film, the protective film is attached to the side of the resist layer on which the support film is not laminated, and functions as a cover.
[0117] In this embodiment, the adhesion between the photosensitive resin composition layer and the protective film is sufficiently smaller than the adhesion between the photosensitive resin composition layer and the support film, so the protective film can be easily peeled off from the photosensitive resin composition layer. For example, polyethylene film, polypropylene film, oriented polypropylene film, polyester film, etc. are preferably used as the protective film. Among these, polypropylene film and polyester film are more preferred, and as the polyester film, polyethylene terephthalate film is even more preferred. In addition, a release layer may be provided on the surface of the protective film.
[0118] The thickness of the protective film is preferably 10 to 100 μm, more preferably 10 to 50 μm. Examples of the protective film include Alphan (registered trademark) EM-501, E-200, E-201F, FG-201, and MA-411 (all manufactured by Oji F-Tex Co., Ltd.), Torayfan (registered trademark) KW37, 2578, 2548, 2500, and YM17S, Therapeel (registered trademark) PJ271, PJ111, HP2, PJ101, WZ, MDA, MFA, TK07, BKE, BX8A, and SY (all manufactured by Toray Industries, Inc.), and GF-18, GF-818, and GF-858 (all manufactured by Tamapoly Co., Ltd.).
[0119] The photosensitive resin laminate of this embodiment may further include an intermediate layer between the support film and the resist layer, or between the support film and the protective film.
[0120] [Photosensitive Resin Laminate Roll] The photosensitive resin laminate described above may be used as a roll of the photosensitive resin laminate in the form of a long photosensitive resin laminate wound around a core.
[0121] [Method for forming a resist pattern] A method for forming a resist pattern using the photosensitive resin laminate according to this embodiment includes, for example, the following steps: a lamination step of laminating a resist layer (in one embodiment, a photosensitive resin composition layer) constituting the photosensitive resin laminate according to this embodiment on a substrate; an exposure step of exposing the resist layer of the photosensitive resin laminate; and a development step of developing and removing unexposed portions of the resist layer. It is preferable to carry out the steps in the above order.
[0122] <Lamination Step> Specifically, in the lamination step, after peeling off the protective film from the photosensitive resin laminate of this embodiment, the resist layer is heated and pressed onto the surface of the substrate using a laminator, and laminated once or multiple times. Examples of the substrate material include copper, stainless steel (SUS), glass, indium tin oxide (ITO), etc., and a copper-clad laminate is preferred. If desired, for example, a H 2 SO 4 The substrate may be washed with an aqueous solution or the like to prepare the surface of the substrate. The heating temperature during lamination is generally 40°C to 160°C. Thermocompression bonding can be performed using a laminator equipped with rolls, or by repeatedly passing a laminate of the substrate and the photosensitive resin composition layer through rolls several times. Thermocompression bonding can be performed in a reduced pressure environment, if desired.
[0123] <Exposure Step> In the exposure step, the resist layer is exposed to an ultraviolet light source or the like using an exposure machine such as a contact aligner, mirror projection, or stepper, either directly or through a patterned photomask or reticle. The exposure step may be performed after peeling off the support film, as desired, or through the support film. When exposure is performed through a photomask, the exposure dose is determined by the illuminance of the light source and the exposure time, and may be measured using an actinometer. In the exposure step, direct imaging exposure may be performed. In direct imaging exposure, exposure is performed directly on the substrate using a drawing device without using a photomask. A semiconductor laser or an ultra-high pressure mercury lamp with a wavelength of 350 nm to 410 nm is used as the light source. When the drawing pattern is controlled by a computer, the exposure dose is determined by the illuminance of the exposure light source and the movement speed of the substrate.
[0124] The exposure method used in the exposure step is preferably at least one method selected from the group consisting of projection exposure, proximity exposure, contact exposure, direct imaging exposure, and electron beam direct writing, and more preferably projection exposure or direct imaging exposure.
[0125] <Heating Step> A heating step may be performed between the exposure step and the development step. The heating temperature is preferably 30°C to 200°C, more preferably 30°C to 150°C, and even more preferably 35°C to 120°C. By performing this heating step, it is possible to improve resolution and adhesion. For heating, a hot air, infrared, or far-infrared heating furnace, a thermostatic oven, a hot plate, a hot air dryer, an infrared dryer, a hot roll, or the like can be used. The heating time is preferably 1 to 300 seconds, more preferably 5 to 120 seconds.
[0126] The time elapsed from the exposure step to the heating step, more precisely the time elapsed from the time exposure is stopped to the time heating is started, is preferably 10 to 600 seconds, more preferably 20 to 300 seconds. The time elapsed from the time heating is started to the time heating is stopped is preferably 1 to 120 seconds, more preferably 5 to 60 seconds.
[0127] <Developing Step> In the developing step, the unexposed portions of the exposed resist layer are removed with a developer using a developing device to form a resist pattern. After exposure, if a support film is present on the resist layer, the support film is removed. Next, the unexposed portions are developed and removed using a developer consisting of an aqueous alkaline solution to obtain a resist pattern. As a developing method for developing the exposed (irradiated) resist layer, any method can be selected from conventionally known photoresist developing methods, such as a rotary spray method, a paddle method, and an immersion method accompanied by ultrasonic treatment.
[0128] The alkaline aqueous solution used as the developer is Na 2 CO 3 , K. 2 CO 3 The alkaline aqueous solution is selected depending on the characteristics of the resist layer, but a solution containing 0.2% to 2% by mass of Na 2 CO 3 An aqueous solution is generally used. The aqueous alkaline solution may contain a surfactant, an antifoaming agent, and a small amount of an organic solvent to promote development. The temperature of the developer in the development step is preferably kept constant within the range of 20°C to 40°C.
[0129] The development step preferably includes a water washing step for removing the developer contained in the resist pattern after development. The washing water may be pure water, industrial water, or other water selected according to the characteristics of the resist layer. In order to improve the resolution and the shape of the resist pattern, MgSO at a concentration of 0.001% by mass to 1% by mass is preferably used. 4 It is also possible to add polyvalent metal salts such as the following. The temperature of the washing water in the washing step is preferably kept constant within the range of 20°C to 40°C.
[0130] A resist pattern can be obtained by the above steps, but if desired, a heat treatment can be further carried out at 60°C to 300°C for 1 to 120 minutes. By carrying out this heat treatment, the chemical resistance of the resist pattern can be improved. For the heat treatment, a heating furnace using hot air, infrared rays, or far infrared rays can be used.
[0131] To obtain a conductive pattern, a conductive pattern forming step may be carried out after the developing step or heating step, in which the substrate on which the resist pattern has been formed is etched or plated.
[0132] <Conductive Pattern Forming Step> The conductive pattern forming step is a step of forming a conductive pattern by using a known etching method or plating method on the substrate surface (for example, copper surface) on which a resist pattern has been formed by development.
[0133] A method for forming a conductive pattern by plating is, for example, as follows: After the development step, the substrate is immersed in an acidic degreasing bath such as a 1 to 50% by mass aqueous sulfuric acid solution at 20 to 60° C. for 1 to 60 minutes, and the immersed substrate is washed with water, and then immersed in a 1 to 50% by mass aqueous sulfuric acid solution at room temperature for 1 to 60 minutes.
[0134] An aqueous solution containing 1 to 15% by mass of copper sulfate, 0.1 to 30% by mass of sulfuric acid, and 1 to 1,000 ppm of hydrochloric acid is prepared, followed by the addition of a brightener (in one embodiment, Cupracid HL and Cupracid GS manufactured by Atotech Corporation) at concentrations of 0.01 to 40 ml / L and 1 to 200 ml / L, respectively, to prepare a copper sulfate plating solution. The prepared copper sulfate plating solution is used for plating at an applied current of 0.01 to 10 A for 1 to 300 minutes using a Haring Cell uniform plating device (manufactured by Yamamoto Plating Tester Co., Ltd.) to form a conductor pattern. The thickness of the copper plating film depends on the thickness of the resist pattern, but is preferably 1 μm or more (resist pattern thickness (μm) - 2 μm). In this disclosure, the thickness of the resist pattern refers to the thickness of the resist layer after curing.
[0135] Examples of methods for forming a conductive pattern by etching include flash etching, which can remove the copper seed layer using a specific etching solution. Examples of the etching solution include, but are not limited to, a mixed etching solution of sulfuric acid and hydrogen peroxide (manufactured by Ebara Densan Co., Ltd.).
[0136] [Method for Producing Conductive Pattern] The method for producing a conductive pattern is carried out by, for example, using a metal plate or a metal-coated insulating plate as a substrate, forming a resist pattern by the resist pattern forming method described above, and then carrying out a conductive pattern forming step.
[0137] <Peeling Step> After the conductor pattern is produced by the above-described method for producing a conductor pattern, a peeling step may be performed in which the resist pattern is peeled off from the substrate using an aqueous solution that is more alkaline than the developer. By performing the peeling step, a wiring board (in one embodiment, a printed wiring board) having a desired wiring pattern can be obtained.
[0138] The alkaline aqueous solution used for stripping (hereinafter also referred to as "stripping solution") is not particularly limited, but an aqueous solution of NaOH or KOH with a concentration of 2% by mass to 20% by mass, or an organic amine-based stripping solution is generally used. A small amount of a water-soluble solvent may be added to the stripping solution. Examples of the water-soluble solvent include alcohol. The temperature of the stripping solution in the stripping step is preferably within the range of 40°C to 70°C, and the immersion time in the stripping solution is preferably 1 to 60 minutes.
[0139] [Method for manufacturing wiring board] In one aspect, a method for manufacturing a wiring board using the photosensitive resin laminate according to this embodiment comprises the following steps: a lamination step of laminating a resist layer on a substrate; an exposure step of exposing the resist layer; a development step of developing and removing unexposed portions of the resist layer to form a resist pattern; a conductor pattern formation step of etching or plating the substrate on which the resist pattern has been formed to form a conductor pattern; and a peeling step of peeling the resist pattern from the substrate. The lamination step, exposure step, development step, conductor pattern formation step, and peeling step, which are the steps included in the method for manufacturing a wiring board according to this embodiment, are the same as those described above.
[0140] The photosensitive resin laminate in this embodiment can be used in the manufacture of printed wiring boards, the manufacture of lead frames for mounting IC chips, precision processing of metal foils such as the manufacture of metal masks, the manufacture of packages such as ball grid arrays (BGAs) and chip size packages (CSPs), the manufacture of tape substrates such as chip-on-film (COFs) and tape automated bonding (TABs), the manufacture of semiconductor bumps, and the manufacture of partition walls of flat panel displays such as ITO electrodes, address electrodes, and electromagnetic wave shields. The values of the above-mentioned parameters are measured in accordance with the measurement methods in the examples described below, unless otherwise specified.
[0141] [Method for Producing Photosensitive Resin Laminate] The photosensitive resin laminate according to this embodiment can be produced by the method described below. That is, in one aspect, the method for producing the photosensitive resin laminate according to this embodiment is a method for producing a photosensitive resin laminate comprising a support film and a resist layer containing a photosensitive resin composition, and includes the following steps: a preparation step of preparing a photosensitive resin composition solution containing a compound having an ethylenically unsaturated bond as component (A), an alkali-soluble resin as component (B), and a solvent, a coating step of applying the photosensitive resin composition solution onto a support film, and a resist layer formation step of heating the support film coated with the photosensitive resin composition solution to form a resist layer. In one aspect, the component (A) comprises a polyglycerin-based (meth)acrylate (A1) and a compound having an ethylenically unsaturated bond (A2) that does not have a carboxyl group and has an ethylenically unsaturated bond.
[0142] The method for producing a photosensitive resin laminate according to this embodiment makes it possible to produce a photosensitive resin laminate that is excellent in sensitivity and resolution and is not affected by the production conditions and storage conditions that are determined by the film thickness of the resist layer.
[0143] <Preparation Step> This step is a step of adding a solvent to the above-mentioned (A) compound having an ethylenically unsaturated bond and (B) alkali-soluble resin to prepare a photosensitive resin composition solution.
[0144] Suitable solvents include ketones such as methyl ethyl ketone (MEK), and alcohols such as methanol, ethanol, and isopropyl alcohol. A single solvent may be used, or two or more solvents may be mixed. The solvent content is preferably 30 to 60% by mass, more preferably 33 to 55% by mass, and even more preferably 35 to 57% by mass, based on the photosensitive resin composition solution. The solvent is preferably added to the photosensitive resin composition so that the viscosity of the photosensitive resin composition solution is 500 to 4000 mPa·sec at 25°C. The viscosity was measured at 25°C using a Brookfield viscometer (manufactured by Eikosha, model number DVNext).
[0145] <Coating Step> This step is a step of coating a support film with a photosensitive resin composition solution. For coating the support film with the photosensitive resin composition solution, for example, a conventionally used method such as a coating method using a roll coater, spin coater, bar coater, blade coater, curtain coater, screen printing machine, or the like, or a spray coating method using a spray coater can be used.
[0146] <Resist Layer Formation Step> This step involves heating a support film coated with a photosensitive resin composition solution to distill off the solvent in the photosensitive resin composition solution, thereby forming a resist layer made of the photosensitive resin composition. The heating temperature of the support film coated with the photosensitive resin composition solution is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher. Heating to 90°C or higher accelerates the evaporation of the solvent contained in the photosensitive resin composition solution, thereby improving the production efficiency of the photosensitive resin laminate. The heating temperature of the support film coated with the photosensitive resin composition solution is preferably 140°C or lower, more preferably 130°C or lower, and even more preferably 120°C or lower. Maintaining the temperature at 140°C or lower can prevent the thermal polymerization of the photosensitive resin composition from progressing. The heating time of the support film coated with the photosensitive resin composition solution is preferably 1 to 10 minutes.
[0147] If necessary, a protection step may be performed after the resist layer forming step, in which a protection layer such as a protection film is laminated on the resist layer. The protection layer is attached to the side of the resist layer where the support film is not laminated, and functions as a cover. The protection film used in the protection step is the same as described above.
[0148] Next, the present embodiment will be described in more detail with reference to examples and comparative examples. However, the present embodiment is not limited to the following examples as long as it does not deviate from the gist of the present embodiment. Physical properties in the examples were measured by the following methods.
[0149] (B) The weight average molecular weight of the alkali-soluble resin was measured by gel permeation chromatography (GPC) and calculated using a calibration curve of standard polystyrene. The GPC conditions were as follows:
[0150] (GPC conditions) Pump: PU-980 manufactured by JASCO Corporation Column: Two columns in total (Shodex KF-80Y / KF-806M) Eluent: Tetrahydrofuran Measurement temperature: 40°C Flow rate: 2.05 mL / min Detector: RI-1530 manufactured by JASCO Corporation Standard monodisperse polystyrene: TSKgel standard polystyrene manufactured by Tosoh Corporation
[0151] Photosensitive resin laminates were prepared as follows. <Preparation of Photosensitive Resin Laminate> Photosensitive resin compositions (Examples 1 to 21 and Comparative Examples 1 to 5) were prepared by mixing the components (A) to (E) shown in Table 1 below (where the number for each component indicates the content (parts by mass) as solids). The photosensitive resin compositions of Examples 1 to 21 and Comparative Examples 1 to 5 and ethanol measured so that the solids concentration of these photosensitive resin compositions was 60% by mass were thoroughly stirred and mixed to obtain prepared solutions containing the photosensitive resin compositions of Examples 1 to 21 and Comparative Examples 1 to 5. A 16 μm-thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., QS71) was used as a support film, and these prepared solutions were uniformly applied to the surface of the film using a bar coater (product name: Type A Automatic Applicator, manufactured by Toyo Seiki Seisakusho, Ltd.). The film was then heated and dried in a dryer at 95°C for 2 minutes and 30 seconds to form a resist layer with a thickness of 25 μm. Next, a 19 μm thick polyethylene film (manufactured by Tamapoly Co., Ltd., GF-858) was laminated as a protective layer on the surface of the resist layer on the side on which the polyethylene terephthalate film was not laminated, and photosensitive resin laminates containing the photosensitive resin compositions of Examples 1 to 21 and Comparative Examples 1 to 5 were obtained.
[0152] [Preparation of Substrate for Performance Evaluation] A substrate for performance evaluation was prepared as follows.
[0153] <Substrate Surface Preparation> A copper-clad laminate having a thickness of 0.4 mm and a rolled copper foil having a thickness of 18 μm was prepared. The surface of this substrate was treated with a 10% by mass H 2 SO 4 Washed with aqueous solution.
[0154] <Lamination> While peeling off the polyethylene film from the photosensitive resin laminate prepared above, the photosensitive resin laminate prepared above was laminated onto a copper-clad laminate that had been preheated to 50°C after the substrate surface was prepared by the above method using a hot roll laminator (AL-700, manufactured by Asahi Kasei Corporation) at a roll temperature of 105°C to obtain a substrate for performance evaluation. The air pressure was 0.35 MPa and the lamination speed was 1.5 m / min.
[0155] <Exposure Step> Two hours after lamination, the performance evaluation substrate was exposed to light at a wavelength of 365 nm through a glass mask using a projection exposure machine (UX-44101SM, manufactured by Ushio Inc.). Similarly, the performance evaluation substrate was exposed to light at a wavelength of 402 nm using a predetermined drawing pattern for direct imaging (DI) exposure using a direct drawing exposure machine (FDi-3, manufactured by ORC Manufacturing Co., Ltd.).
[0156] <Heating Step> One minute after exposure, the performance evaluation substrate was heated for 30 seconds in a constant temperature incubator (manufactured by Yamato Scientific Co., Ltd., DKM600) set at 60°C.
[0157] <Developing Step> After peeling off the polyethylene terephthalate film (support film), the resulting film was developed using an alkaline developer (manufactured by Fuji Kiko Co., Ltd., a dry film developer) at a concentration of 1% by mass Na 2 CO 3 The aqueous solution was sprayed for a predetermined period of time to carry out development. The development spray time was twice the shortest development time, and the post-development washing spray time was twice the shortest development time.
[0158] <Plating Process> A substrate that had been subjected to the same surface preparation and lamination as above was exposed to light using a drawing pattern in which the line width (L) / space width (S) (hereinafter referred to as "L / S") was x / x (x = 1 to 20 (varying in 1 μm intervals)) (unit: μm) with an energy amount that resulted in 17 remaining steps on a Hitachi 41-step step tablet, followed by the same heating and development processes as above to form a resist pattern. After development, the substrate was immersed in an acidic degreasing FRX bath (a 10% by weight sulfuric acid aqueous solution, manufactured by Atotech Japan Co., Ltd.) at 40°C for 4 minutes. After rinsing with water, it was immersed in a 10% by weight sulfuric acid aqueous solution at room temperature for 2 minutes.
[0159] A 121 g / L copper sulfate solution was prepared and diluted 3.6 times with 19% by weight sulfuric acid, followed by the addition of concentrated hydrochloric acid at a concentration of 200 ppm. Next, Cupracid HL and Cupracid GS were added as brighteners at concentrations of 0.4 ml / L and 20 ml / L, respectively, to prepare a copper sulfate plating solution. After pretreatment, a 6 cm x 12.5 cm substrate for plating resistance evaluation was plated with the prepared copper sulfate plating solution for 65 minutes at an applied current of 0.4 A using a Haring Cell uniform plating apparatus (manufactured by Yamamoto Plating Tester Co., Ltd.). The resulting copper plating film was 20 μm thick.
[0160] <Removal Step> Products "Clean Etch (registered trademark) R-100S" (manufactured by Mitsubishi Gas Chemical Company, Inc.) and "Clean Etch (registered trademark) R-101" (manufactured by Mitsubishi Gas Chemical Company, Inc.) were mixed in a volume ratio of 2 / 1, and then diluted with pure water to prepare a stripper solution with a concentration of 20 mass %. A plated substrate for performance evaluation was immersed in the stripper solution heated to 50°C for 4 minutes without stirring, to strip and remove the resist pattern.
[0161] [Evaluation] <Developability> The prepared performance evaluation substrate was subjected to exposure and development steps according to the above method, and the shortest time required for the unexposed portion of the resist layer to completely dissolve was defined as the shortest development time. A shorter shortest development time means higher developability, and the shortest development time was evaluated according to the following criteria. If the evaluation is ◯ or Δ, the product can be suitably used as a photosensitive resin laminate for forming a resist pattern. ◯: Shortest development time less than 18 seconds "Good" Δ: Shortest development time 18 seconds or more but less than 20 seconds "Fair" ×: Shortest development time 20 seconds or more "Fail"
[0162] <Flexibility> A flexographic substrate that had been subjected to surface preparation and lamination according to the above method was exposed with an energy amount that left 17 steps on a Stouffer 41-step step tablet, and the substrate was then cut into 1-inch width samples to prepare samples. Using these samples, a mandrel test was carried out in accordance with JIS K5600-5-1, and flexibility was evaluated based on the smallest mandrel diameter that did not cause cracks in the exposed area. A smaller value indicates higher flexibility, and the evaluation was based on the following criteria. If the evaluation was ◯ or △, the product could be suitably used as a photosensitive resin laminate for forming a resist pattern. ◯: Diameter less than 6 mm "Good" △: Diameter 6 mm or more but less than 10 mm "Fair" ×: Diameter 10 mm or more "Fail"
[0163] <Adhesion> A resist pattern was formed on the prepared performance evaluation substrate by exposing the substrate to an energy amount sufficient to leave 17 steps on a 41-step step tablet manufactured by Hitachi, Ltd. using a drawing pattern in which the line width (L) / space width (S) (hereinafter referred to as "L / S") was x / 3x (x = 1 to 20 (varying in 1 μm intervals)) (unit: μm) with the exposure being carried out. The resist pattern was then heated and developed as described above. The resist pattern was observed under an optical microscope, and adhesion was evaluated based on the minimum line width formed without meandering or chipping of the line portion (exposed portion). A smaller value indicates higher adhesion, and the adhesion was evaluated according to the following criteria. A rating of ◯ or △ indicates that the product can be suitably used as a photosensitive resin laminate for forming a resist pattern. ◯: Minimum line width less than 6 μm ("Good") △: Minimum line width 6 μm or more but less than 8 μm ("Fair") ×: Minimum line width 8 μm or more ("Unacceptable"
[0164] <Resolution> A resist pattern was formed on the prepared performance evaluation substrate by exposing the substrate to an energy amount sufficient to leave 17 steps on a 41-step tablet manufactured by Hitachi, Ltd. using a drawing pattern in which the line width (L) / space width (S) (hereinafter referred to as "L / S") was x / x (x = 1 to 20 (varying in 1 μm intervals)) (unit: μm) with the exposure being carried out. The resist pattern was then heated and developed as described above. The resist pattern was observed under an optical microscope, and the resolution was evaluated based on the minimum line width at which the line portions (exposed portions) were removed without meandering or chipping and the space portions (unexposed portions) were removed without residue. A smaller value indicates higher resolution, and the evaluation was based on the following criteria. A rating of ◯ or △ indicates that the product can be suitably used as a photosensitive resin laminate for forming a resist pattern. ◯: Minimum line width less than 6 μm ("Good") △: Minimum line width 6 μm or more but less than 8 μm ("Fair") ×: Minimum line width 8 μm or more ("Unacceptable"
[0165] <Removability Evaluation> The prepared performance evaluation substrate was subjected to the plating step and then the peeling step. The minimum mask width at which the hardened resist lines between the plating patterns were completely peeled off was taken as the post-plating peelability value. The smaller this value, the higher the peelability, and it was evaluated according to the following criteria. If the evaluation was ⊚, ◯, or Δ, the substrate can be suitably used as a printed wiring board for plating after the formation of the resist pattern. ⊚: Minimum mask width less than 6 μm "Excellent" ○: Minimum mask width 6 μm or more but less than 7 μm "Good" Δ: Minimum mask width 7 μm or more but less than 9 μm "Fair" ×: Minimum mask width 9 μm or more "Fail"
[0166] The evaluation results for the performance evaluation substrates of the examples are shown in Table 1. Details of the components shown in Table 1 are shown in Table 2. Table 3 also shows the total value of k, each li, and m (the number of repeating units) in the formula of polyglycerin-based (meth)acrylate (A1) represented by formula (I), as well as the total value of the number of repeating units (k, each li, and m) / (n+2), and the value of n. Table 3 shows, from top to bottom, the total value of k, each li, and m, and the value of n for (A1-1) to (A1-5).
[0167]
[0168]
[0169]
[0170]
[0171]
[0172] As is clear from Table 1, in the examples that satisfied the requirements of this embodiment, the developability, flexibility, resolution, adhesion, and releasability were all good. On the other hand, when the component (A) did not contain either (A1) a polyglycerin-based (meth)acrylate or (A2) a compound that did not have a carboxyl group and had an ethylenically unsaturated bond, the developability, flexibility, resolution, adhesion, and releasability were all poor. Furthermore, when the component (A) contained (A3) a compound that had a carboxyl group and had an ethylenically unsaturated bond, the developability and resolution were inferior to those of the examples.
[0173] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the invention.
[0174] The photosensitive resin laminate of the present invention is excellent in developability, flexibility, resolution, adhesion, and releasability, and is not affected by the coating and drying conditions or storage conditions of the photosensitive resin laminate. That is, the photosensitive resin laminate can be widely used as a photosensitive resin laminate for forming a resist pattern, and is particularly suitable for use in forming a resist pattern for a printed wiring board, which requires plating after forming the resist pattern.
Claims
1. A photosensitive resin laminate comprising a support film and a resist layer containing a photosensitive resin composition, wherein the photosensitive resin composition contains the following components: (A) a compound having an ethylenically unsaturated bond, and (B) an alkali-soluble resin, and the component (A) is represented by the following general formula (I): [In the formula, n is 2 to 20, each i is a natural number from 1 to n, k, each li, and m are each independently 0 to 30, 1 , R 2i , and R 3 each independently represents a hydrogen atom or a methyl group; R 4 , R 5i , and R 6 each independently represents an alkylene group having 1 to 10 carbon atoms, the following formula (II): [In the formula, R 7 and R 8 are each independently an alkylene group having 1 to 10 carbon atoms.] and a group represented by the following formula (III): [In the formula, R 9 is an alkylene group having 1 to 10 carbon atoms.] is one selected from the group consisting of groups represented by the following formulas:] A polyglycerin-based (meth)acrylate represented by the following formula:]; and (A2) a compound having no carboxyl group and having an ethylenically unsaturated bond.
2. The photosensitive resin laminate described in claim 1, wherein the total content of the (A) component and the (B) component in the photosensitive resin composition is 80 mass% or more and 98 mass% or less, based on the total solid mass of the photosensitive resin composition.
3. A photosensitive resin laminate according to claim 1 or 2, wherein the content of the component (B) is 70 mass% or less based on the total content of the component (A) and the component (B).
4. The photosensitive resin laminate according to claim 1 or 2, wherein the component (B) contains structural units derived from styrene and benzyl (meth)acrylate.
5. A photosensitive resin laminate described in claim 1 or 2, wherein the (B) component contains a structural unit derived from styrene, and the styrene content in the (B) component is 35 mass% or more and 80 mass% or less.
6. The photosensitive resin laminate according to claim 1 or 2, wherein the photosensitive resin composition further contains a photopolymerization initiator as component (C).
7. The photosensitive resin laminate according to claim 6, wherein the content of the component (C) in the photosensitive resin composition is 25 mass % or less based on the content of the component (A).
8. The photosensitive resin laminate according to claim 6, wherein the component (C) comprises a hexaarylbiimidazole compound.
9. The photosensitive resin laminate according to claim 1 or 2, wherein the photosensitive resin composition further contains (D) a polymerization inhibitor.
10. The photosensitive resin laminate according to claim 1 or 2, wherein the component (A2) is a compound having 2 to 6 ethylenically unsaturated bonds.
11. The photosensitive resin laminate according to claim 1 or 2, wherein the component (A2) contains a compound having two ethylenically unsaturated bonds.
12. The photosensitive resin laminate according to claim 1 or 2, wherein the component (A2) contains a compound having one ethylenically unsaturated bond.
13. The photosensitive resin laminate according to claim 1 or 2, wherein the component (A2) contains a di(meth)acrylate compound having a bisphenol A structure.
14. In the general formula (I), R 1 , R 2i , and R 3 The photosensitive resin laminate according to claim 1 or 2, wherein is a methyl group.
15. R in the above general formula (I) 4 O, R 5i O and R 6 O into the formula R j O {wherein j=4, 5i, 6 (wherein i=1, 2, ..., n)}, j 3. The photosensitive resin laminate according to claim 1, wherein the ratio of the number of (meth)acryloyl groups to the total number of O is 20 or less.
16. The photosensitive resin laminate according to claim 1 or 2, wherein in said general formula (I), n is an integer of 2 to 15.
17. The photosensitive resin laminate according to claim 1 or 2, wherein in said general formula (I), n is a number average value of 2 to 15.
18. The above R 4 , R 5i , and R 6 The photosensitive resin laminate according to claim 1 or 2, wherein is an alkylene group.
19. The above R 4 , R 5i , and R 6 The photosensitive resin laminate according to claim 1 or 2, wherein contains an ethylene group and / or a propylene group.
20. The above R 4 , R 5i , and R 6 3. The photosensitive resin laminate according to claim 1 or 2, wherein represents an ethylene group and / or a propylene group.
21. The above R 4 , R 5i , and R 6 The photosensitive resin laminate according to claim 1 or 2, wherein is an ethylene group.
22. The photosensitive resin laminate according to claim 1 or 2, further comprising a protective film.
23. A photosensitive resin laminate comprising a support film and a resist layer containing a photosensitive resin composition, wherein the photosensitive resin composition contains the following components: (A) a compound having an ethylenically unsaturated bond, and (B) an alkali-soluble resin, and the component (A) contains: (A3) a compound having no quaternary carbon and / or aromatic ring, and having four or more ethylenically unsaturated bonds in one molecule; and (A4) a compound having a quaternary carbon and / or an aromatic ring, no carboxyl group, and having an ethylenically unsaturated bond.
24. The photosensitive resin laminate according to claim 23, wherein the compound (A4) includes a compound having one or two ethylenically unsaturated bonds.
25. The photosensitive resin laminate according to claim 23 or 24, wherein the amount of ethylenically unsaturated bonds per 100 g of the (A4) compound is 0.25 mol or less.
26. The photosensitive resin laminate according to claim 23 or 24, wherein the content of the component (A) is 20 mass % or more based on the total solid mass of the photosensitive resin composition.
27. The photosensitive resin laminate according to claim 23 or 24, wherein the component (B) contains a copolymer containing a structural unit derived from (meth)acrylic acid as a monomer component, and the content of the structural unit derived from (meth)acrylic acid in the component (B) is 27 mass% or less.
28. The photosensitive resin laminate according to claim 23 or 24, wherein the component (B) contains a copolymer containing a structural unit derived from (meth)acrylic acid as a monomer component, and the content of the structural unit derived from (meth)acrylic acid in the component (B) is 25 mass% or less.
29. A method for forming a resist pattern using the photosensitive resin laminate according to claim 1 or 2, comprising the following steps: a lamination step of laminating a resist layer on a substrate; an exposure step of exposing the resist layer to light; and a development step of developing and removing the unexposed portions of the resist layer.
30. A method for producing a wiring board using the photosensitive resin laminate according to claim 1 or 2, comprising the following steps: a lamination step of laminating a resist layer on a substrate; an exposure step of exposing the resist layer to light; a development step of developing and removing the unexposed parts of the resist layer to form a resist pattern; a conductor pattern formation step of etching or plating the substrate on which the resist pattern has been formed to form a conductor pattern; and a peeling step of peeling the resist pattern from the substrate.
Citation Information
Patent Citations
Dry film composition, which can undergo photopolymerization
JP1994110208A
Formation of thin film electrode
JP1999160864A
Photosensitive insulating resin composition, and product using the same
JP2015036416A
Photosensitive resin laminate and method for producing resist pattern
JP2022188113A
Cited By