Die casting alloy composition for battery terminal plate, method for manufacturing battery terminal plate using same, and battery terminal plate manufactured thereby
The die-casting alloy composition of silicon, iron, magnesium, and beryllium in aluminum alloys addresses the challenge of achieving high electrical conductivity in battery terminal plates, resulting in enhanced performance and manufacturing efficiency.
Patent Information
- Application Number
- PCT/KR2023/005267
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-17
AI Technical Summary
Existing aluminum alloys for battery terminal plates, while improving strength and thermal conductivity, fail to achieve high electrical conductivity due to alloying elements disrupting the crystal structure and scattering free electrons, leading to suboptimal performance.
A die-casting alloy composition comprising 4 to 6% silicon, 0.2 to 0.5% iron, 0.05 to 1.5% magnesium, and 0.001 to 0.003% beryllium, balanced with aluminum, is used, with a die-casting method at 680 to 750°C and 70 to 80 MPa pressure, followed by annealing at 300 to 500°C for 1 to 4 hours to enhance electrical conductivity.
The solution achieves electrical conductivity of 40% IACS or more, along with improved thermal conductivity and mechanical strength, while maintaining cost-effectiveness and ease of manufacturing through the die-casting process.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Die-casting alloy composition for battery terminal plate, method for manufacturing battery terminal plate using same, and battery terminal plate manufactured by the method for manufacturing same
[0001] The present invention relates to a die-casting alloy composition for a battery terminal plate having excellent electrical conductivity, a method for manufacturing a battery terminal plate using the same, and a battery terminal plate manufactured using the method for manufacturing the same.
[0002]
[0003] Globally, regulations on automobile exhaust emissions are becoming increasingly stringent, and carbon dioxide emissions are also being tightened. This is spurring innovative change in the automotive industry, and to meet these regulations, the industry is accelerating the development of eco-friendly vehicles and high-quality parts.
[0004]
[0005] Electric vehicles differ from internal combustion engine vehicles in their energy storage and propulsion systems, utilizing secondary batteries as their energy storage devices. As the development of eco-friendly vehicles accelerates, research and development is underway to maximize the performance of batteries themselves and their auxiliary materials.
[0006]
[0007] Automotive batteries use conductive battery terminal plates as a component for connecting multiple battery cells, and the electrical conductivity and thermal conductivity of the battery terminal plates are closely related to the performance and lifespan of the battery.
[0008]
[0009] Aluminum (Al) is widely used as a raw material for battery terminal plates across industries because it is easy to cast, forms alloys well with other metals, has strong corrosion resistance in the air, and has excellent electrical and thermal conductivity.
[0010]
[0011] Aluminum can generally be formed through press methods, die casting methods, etc., but the press method has limitations such as difficulty in shape implementation and thickness control, only one product is produced per press, and the cost of extruded materials for the press method is high. On the other hand, the die casting method has the advantage of being able to overcome the limitations of the press method.
[0012]
[0013] Die casting is a method of manufacturing a casting identical to the mold by injecting molten aluminum into a machined mold in the shape of the product. It is widely used for parts of electronic products, automobiles, and aircraft that require accurate dimensions and relatively complex designs.
[0014]
[0015] Pure aluminum can improve physical and chemical properties by adding various alloying elements to the aluminum base to address issues such as strength and formability, and the development of suitable materials is required to manufacture battery terminal plates using the die casting method.
[0016]
[0017] Recently, due to the high performance and lightweighting of automobile parts and electronic products, efforts have been made to improve the durability, thermal properties, and electrical properties of aluminum alloys.
[0018]
[0019] In this regard, Korean Patent No. 10-1133103 discloses an aluminum alloy for die casting that includes zinc (Zn), magnesium (Mg), copper (Cu), zirconium (Zr), and titanium (Ti), and can obtain excellent tensile strength through precipitation hardening heat treatment.
[0020]
[0021] In addition, Korean Patent Publication No. 10-2014-0034557 discloses a high thermal conductivity Al-Cu alloy for die casting by adding copper, magnesium, and iron to an aluminum base.
[0022]
[0023] Meanwhile, the electrical conductivity of pure aluminum is relatively high, but when alloying elements are incorporated into aluminum, the alloying elements lower the electrical conductivity of the aluminum alloy.
[0024]
[0025] Alloying elements create electric field inhomogeneity within the aluminum crystal structure, and as a result, free electrons that contribute to electrical conductivity are scattered by impurity atoms within the crystal, ultimately reducing the electrical conductivity of the aluminum alloy.
[0026]
[0027] However, the prior art has been limited in that it has focused on improving the strength and thermal conductivity of aluminum alloys and has not been able to propose a combination and composition ratio of alloys to achieve high electrical conductivity.
[0028]
[0029] The purpose of the present invention to solve the above problems is to provide a die-casting alloy composition for a battery terminal plate having excellent electrical conductivity, a method for manufacturing a battery terminal plate using the same, and a battery terminal plate manufactured using the method for manufacturing the same.
[0030]
[0031] The die-casting alloy composition for a battery terminal plate of the present invention for solving the above problem comprises 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), and the remainder aluminum (Al).
[0032]
[0033] The method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate of the present invention for solving the above problem includes a raw material preparation step of preparing a die-casting alloy composition for a battery terminal plate including 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), and the remainder aluminum (Al); and a molding step of supplying a molten mass of the die-casting alloy composition for a battery terminal plate to a die-casting mold for molding.
[0034]
[0035] It is characterized in that in the above molding step (S200), the casting temperature is 680 to 750°C and the casting pressure is 70 to 80 MPa.
[0036]
[0037] It is characterized in that it further includes an annealing treatment step of annealing at 300 to 500°C for 1 to 4 hours after the above molding step (S200).
[0038]
[0039] The battery terminal plate of the present invention for solving the above problem is characterized by casting a die-casting alloy composition for a battery terminal plate containing 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), and the remainder aluminum (Al) using a die-casting method.
[0040]
[0041] It is characterized in that the die casting temperature during casting of the above battery terminal plate is 680 to 750°C and the casting pressure is 70 to 80 MPa.
[0042]
[0043] It is characterized by annealing a cast battery terminal plate at 300 to 500°C for 1 to 4 hours.
[0044]
[0045] The above battery terminal plate is characterized by having an electrical conductivity of 40% IACS or more.
[0046]
[0047] As described above, the die-casting alloy composition for a battery terminal plate according to the present invention, the method for manufacturing a battery terminal plate using the same, and the battery terminal plate manufactured by the method for manufacturing the same have the effect of having excellent electrical conductivity and thermal conductivity.
[0048]
[0049] The specific features and advantages of the present invention are described in detail below. If a detailed description of the functions and configurations related to the present invention is deemed to unnecessarily obscure the gist of the invention, such detailed description will be omitted.
[0050]
[0051] The present invention relates to a die-casting alloy composition for a battery terminal plate having excellent electrical conductivity, a method for manufacturing a battery terminal plate using the same, and a battery terminal plate manufactured using the method for manufacturing the same.
[0052]
[0053] A die-casting alloy composition for a battery terminal plate according to the present invention contains 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), the remainder being aluminum (Al) and other unavoidable impurities.
[0054]
[0055] Silicon (Si), when added in an appropriate amount, reduces the melting point, increases the fluidity of the alloy in a molten state during the die casting process, and improves castability.
[0056]
[0057] Silicon (Si) reduces shrinkage, improves fatigue strength, hardness, wear resistance, and heat resistance, and in particular, when it coexists with magnesium (Mg), it forms Mg2Si, which can be strengthened by aging treatment.
[0058]
[0059] Silicon (Si) is added in an amount of 4 to 6 wt% based on 100 wt% of the total die-casting alloy composition for the battery terminal plate. If the amount of silicon (Si) is less than 4 wt%, appropriate strength and fluidity cannot be obtained, and if it exceeds 6 wt%, formability and impact resistance deteriorate. Therefore, it is preferable not to exceed the above weight range.
[0060]
[0061] Iron (Fe) prevents the alloy from sticking to the mold during the die casting process and contributes to improving strength and wear resistance.
[0062]
[0063] Iron (Fe) is added in an amount of 0.2 to 0.5 wt% based on 100 wt% of the total die-casting alloy composition for the battery terminal plate. If the iron is added in an amount less than 0.2 wt%, the anti-seizing and strength-enhancing effects are minimal, and if it exceeds 0.5 wt%, it causes precipitation and deterioration of corrosion resistance, ductility, thermal conductivity, surface gloss, processability, and castability. Therefore, it is preferable not to exceed the above weight range.
[0064]
[0065] Magnesium (Mg) improves mechanical strength through the solid solution effect and, in particular, forms a Mg2Si compound with silicon (Si) to provide age hardening properties.
[0066]
[0067] Magnesium (Mg) is added in an amount of 0.05 to 1.5 wt% based on 100 wt% of the total die-casting alloy composition for battery terminal plates. If the magnesium is added in an amount less than 0.05 wt%, the effects of improving corrosion resistance, elongation, and strength are minimal, and if it exceeds 1.5 wt%, fluidity and formability deteriorate, and the oxidation tendency of the molten metal increases, resulting in the generation of dross. In addition, since microbubbles may be generated on the alloy surface, it is preferable not to exceed the above weight range.
[0068]
[0069] More preferably, magnesium (Mg) may be added in an amount of 0.5 to 1 wt%.
[0070]
[0071] Beryllium (Be) prevents magnesium (Mg) from oxidizing in the die-casting alloy composition for battery terminal plates, thereby enhancing mechanical strength.
[0072]
[0073] Specifically, the alloy composition may be oxidized to MgO, Al2O3-MgO when exposed to air during the melting process. The oxide may act as an impurity in the aluminum alloy and reduce the mechanical strength.
[0074]
[0075] By adding beryllium (Be), the formation of magnesium oxide is suppressed, and in addition, by combining with iron (Fe) components, the formation of acicular Al3Fe precipitates is prevented, and the formation of a square Be2Fe phase can be formed, thereby improving ductility.
[0076]
[0077] Beryllium (Be) is added in an amount of 0.001 to 0.003 wt% based on 100 wt% of the die-casting alloy composition for the entire battery terminal plate. If the beryllium (Be) is added in an amount less than 0.001 wt%, the mechanical strength improvement and the magnesium oxide formation inhibition effects are minimal. If the beryllium (Be) is added in an amount exceeding 0.003 wt%, the mechanical strength improvement of the alloy due to the addition of beryllium is minimal, and since beryllium is expensive, the economic feasibility is poor. Therefore, it is preferable not to exceed the above weight range.
[0078]
[0079] The remainder, excluding the silicon, iron, magnesium and beryllium mentioned above, consists of aluminum and other unavoidable impurities.
[0080]
[0081] The above impurities are any one of copper (Cu), zinc (Zn), nickel (Ni), tin (Sn), lead (Pb), titanium (Ti) or a combination thereof, and are included in an amount of 0.1 wt% or less.
[0082]
[0083] Hereinafter, a method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate according to the present invention will be described.
[0084]
[0085] The method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate according to the present invention uses the die-casting alloy composition for a battery terminal plate described above, and the reasons for the raw material properties and content restrictions are the same as those described above, so a detailed description thereof will be omitted.
[0086]
[0087] A method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate of the present invention includes a raw material preparation step of preparing a die-casting alloy composition for a battery terminal plate and a molding step of supplying a molten product of the die-casting alloy composition for a battery terminal plate to a die-casting mold for molding.
[0088]
[0089] In the raw material preparation step, a die-casting alloy composition for a battery terminal plate is prepared. Specifically, a die-casting alloy composition for a battery terminal plate is prepared, which includes 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.001 to 0.003 wt% of beryllium (Be), 0.05 to 1.5 wt% of magnesium (Mg), and the remainder of aluminum (Al).
[0090]
[0091] The die-casting alloy composition for the above battery terminal plate may contain other unavoidable impurities in addition to the above-described raw materials, and the impurities may be any one of copper (Cu), zinc (Zn), nickel (Ni), tin (Sn), lead (Pb), titanium (Ti) or a combination thereof, and may be contained in an amount of 0.1 wt% or less.
[0092]
[0093] In the forming step, the die-casting alloy composition for the battery terminal plate is melted, and the molten material is supplied to a die-casting mold for forming.
[0094]
[0095] In the molding step, the remaining weight of aluminum (Al) is heated to 750 to 800°C to completely melt it, then the aluminum molten material is heated to 820 to 880°C, and then 4 to 6 wt% of silicon (Si) is added and the temperature is raised to 900 to 950°C.
[0096]
[0097] Afterwards, 0.2 to 0.5 wt% of iron (Fe) and 0.001 to 0.003 wt% of beryllium (Be) are added to the aluminum melt and dissolved for 3 to 6 hours, and then the temperature is reduced to 650 to 700°C, and 0.05 to 1.5 wt% of magnesium (Mg) is added to prepare a die-casting alloy melt for a battery terminal plate.
[0098]
[0099] Afterwards, a process may further be included to remove trace impurities such as oxides, carbides, and intermetallic compounds contained in the die-casting alloy composition for the battery terminal plate by injecting an inert gas such as nitrogen or argon to float the impurities and then filtering and removing the floated impurities.
[0100]
[0101] The casting temperature of the die-casting alloy composition for the prepared battery terminal plate can be controlled to 680 to 750°C, and the casting pressure can be controlled to 70 to 80 MPa, and preferably, the casting pressure is controlled to 75 MPa to complete the casting.
[0102]
[0103] The method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate according to the present invention may further include an annealing treatment step of annealing at 300 to 500°C for 1 to 4 hours after the molding step.
[0104]
[0105] The above annealing treatment relieves residual stress within the casting, and improves durability, thermal and electrical properties.
[0106]
[0107] Hereinafter, a battery terminal plate according to the present invention will be described.
[0108]
[0109] The battery terminal plate according to the present invention is manufactured by a method for manufacturing a battery terminal plate using the die-casting alloy composition for a battery terminal plate described above. The raw material properties and reasons for content restrictions are the same as those described above, and thus a detailed description thereof will be omitted.
[0110]
[0111] The battery terminal plate according to the present invention satisfies the tensile strength of 250 to 350 MPa, the yield strength of 160 to 200 Mpa, the elongation of 3 to 10%, the thermal diffusivity of 55 to 70 ㎟ / s, and the thermal conductivity of 150 to 180 W / mK.
[0112]
[0113] In addition, the battery terminal plate according to the present invention has excellent electrical conductivity, satisfying an electrical conductivity of 40% IACS (International Annealed Copper Standard) or higher, preferably 45 to 55% IACS.
[0114]
[0115] Hereinafter, the present invention will be described in detail with reference to a preferred embodiment. However, the following embodiment is intended to specifically illustrate the present invention and is not intended to be limited thereto.
[0116]
[0117] A die-casting alloy composition for a battery terminal plate was prepared with the composition ratio shown in Table 1 below, and a battery terminal plate specimen was manufactured, and the density, electrical conductivity, and thermal conductivity were measured.
[0118]
[0119] A die-casting alloy melt for a battery terminal plate was prepared by the following method.
[0120] After the remaining weight of aluminum (Al) was heated to 780°C and completely melted, the aluminum molten material was heated to 850°C, silicon (Si) was added, and the temperature was increased to 930°C. After that, iron (Fe) and beryllium (Be) were added and melted for 4 hours, and then the temperature was reduced to 650°C, and magnesium (Mg) was added to prepare a molten material. A battery terminal plate was cast using gravity die casting equipment at a casting temperature of 700°C and a casting pressure of 75 MPa.
[0121] Afterwards, the density, electrical conductivity, and thermal conductivity characteristics were confirmed according to the presence or absence of heat treatment (annealing). The heat treatment was performed at 400°C for 3 hours, and air cooling was performed under atmospheric pressure after the heat treatment.
[0122]
[0123] Separation heat treatment AlSiMgFeBe density g / cm 3 Electrical ConductivityIACS, %Experimental Example 1×Bal.61.50.30.0012.65034Experimental Example 1-1○Bal.61.50.30.0012.63042.5Experimental Example 2×Bal.61.00.30.0012.65037.7Experimental Example 2-1○Bal.61.00.30.0012.64643.6Experimental Example 3×Bal.60.50.30.0012.65036.4Experimental Example 3-1○Bal.60.50.30.0012.64840.9Experimental Example 4×Bal.51.00.30.0012.65037.5Experimental Example 4-1○Bal.51.00.30.0012.65246.5Experimental example 5×Bal.50.50.30.0012.65138.2Experimental example 5-1○Bal.50.50.30.0012.64245.7
[0124] As a result, it was confirmed that the amount of elements added and whether heat treatment was performed affected the electrical conductivity, and experimental example 4-1 showed the best electrical conductivity, showing an electrical conductivity of 46.5% IACS.
[0125]
[0126] Table 2 below shows the composition and composition ratio of commercially available aluminum alloys, and Table 3 compares the density, electrical conductivity, and thermal conductivity of commercially available aluminum alloys and Experimental Example 4-1 according to the present invention.
[0127]
[0128] ClassificationAlCuSiMgZnFeMnNiSnPbTiBeADC12Bal.1.5~3.59.6~12.00.3 or less1.0 or less1.3 or less0.5 or less0.5 or less0.2 or less0.2 or less0.3 or less-A380Bal.3.0~4.07.5~9.50.1 or less3.0 or less1.3 or less0.5 or less0.5 or less0.35 or less---A3003 H14Bal.0.05~0.20.6 or less-0.1 or less0.7 or less1.0~1.5-----Present inventionBal.-4.0~6.00.05~1.5-0.2~0.5-----0.001~0.003
[0129] Density (g / cm) 3 )ElectricalConductivity(IACS, %)Thermal conductivity(W / m·K)ADC122.7423.096A3802.7123.096A3003 H142.7427.3159Experimental Example 4-12.6546.5170
[0130] As a result, it was confirmed that Experimental Example 4-1 had superior electrical and thermal conductivity compared to commercial aluminum alloys. In addition, it was confirmed that the present invention can reduce manufacturing costs by satisfying superior electrical and thermal conductivity while minimizing the types of elements added compared to commercial aluminum alloys, and that the battery terminal plate can be manufactured using a die-casting method, making it easy to implement shape and control thickness and increasing production volume.
[0131]
[0132] While the present invention has been described with reference to preferred embodiments, those skilled in the art will appreciate that various modifications and variations can be made to the invention without departing from the technical spirit and scope of the claims. Therefore, the scope of the present invention should be construed in accordance with the claims, which are intended to encompass these numerous modifications.
Claims
1. Characterized in that it contains 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), and the remainder of aluminum (Al). Die-casting alloy composition for battery terminal plates.
2. A raw material preparation step for preparing a die-casting alloy composition for a battery terminal plate, which comprises 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), and the remainder of aluminum (Al); and A molding step characterized by including a molding step of supplying a molten die-casting alloy composition for the battery terminal plate to a die-casting mold; A method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate.
3. In paragraph 2, In the above molding step (S200), the casting temperature is 680 to 750°C, and the casting pressure is 70 to 80 MPa. A method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate.
4. In paragraph 2, It is characterized in that it further includes an annealing treatment step of annealing at 300 to 500°C for 1 to 4 hours after the above molding step (S200). A method for manufacturing a battery terminal plate using a die-casting alloy composition for a battery terminal plate.
5. A die-casting alloy composition for a battery terminal plate comprising 4 to 6 wt% of silicon (Si), 0.2 to 0.5 wt% of iron (Fe), 0.05 to 1.5 wt% of magnesium (Mg), 0.001 to 0.003 wt% of beryllium (Be), and the remainder aluminum (Al) is characterized by being cast using a die-casting method. Battery terminal plate.
6. In paragraph 5, The die casting temperature is 680 to 750℃, and the casting pressure is 70 to 80 MPa. Battery terminal plate.
7. In paragraph 5, It is characterized by annealing the cast battery terminal plate at 300 to 500°C for 1 to 4 hours. Battery terminal plate.
8. In any one of paragraphs 5 to 7, Characterized by an electrical conductivity of 40% IACS or more. Battery terminal plate.
Citation Information
Patent Citations
Aluminum alloy for die casting having excellent corrosion resistance
KR101606525B1
Corrosion resistant aluminium alloy for casting
KR1020170124963A
Encryption method of 128-bit lightweight block cipher suitable for side-channel countermeasures
KR1020210037945A
Aluminum alloy for die casting and die casting mold manufactured using the same
US20180169745A1
KR20220131800A