Polymer crystallization method and additive manufactured powders made therefrom
The method of mixing thermoplastic polymers with inorganic submicron powders in polar aprotic solvents to control crystallization in additive manufacturing addresses the multiple melting point issue, resulting in improved melt behavior and printing efficiency for thermoplastic polymers in additive manufacturing.
Patent Information
- Application Number
- PCT/US2024/023544
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-17
AI Technical Summary
Existing additive manufacturing methods face challenges with thermoplastic polymers that exhibit multiple melting points or lack a single sharp melting point, leading to inefficient printing and poor feature resolution due to non-uniform powder distribution and thermal energy dissipation in powder bed fusion processes.
A method involving the mixing of a thermoplastic polymer with a polar aprotic solvent and an inorganic submicron powder to form a semi-crystalline powder with a singular distinct melt peak, achieved by dissolving the polymer in the solvent and precipitating it with the submicron powder, which can revert to an amorphous state under normal processing conditions.
This method produces semi-crystalline thermoplastic powders with a controlled crystallization process, enhancing the melt behavior and reducing the complexity of additive manufacturing by creating a single melt peak, thereby improving printing efficiency and feature resolution.
Smart Images

Figure US2024023544_17102024_PF_FP_ABST
Abstract
Description
POLYMER CRYSTALLIZATION METHOD AND ADDITIVE MANUFACTUREDPOWDERS MADE THEREFROMFIELD
[0001] The technology relates to a method to make polymer powders useful for additive manufacturing and in particular a method of controlling the crystallization in a polymer powder precipitated from a solution.BACKGROUND OF THE INVENTION
[0002] Various additive manufacturing processes, also known as three-dimensional (3D) printing processes, can be used to form three-dimensional objects by fusing certain materials at particular locations and / or in layers. Material can be joined or solidified under computer control, for example working from a computer-aided design (CAD) model, to create a three-dimensional object, with material being added together, such as liquid molecules or powder grains being fused together, typically layer-by-layer. Various types of additive manufacturing include binder jetting, directed energy deposition, material extrusion, material jetting, powder bed fusion, sheet lamination, and vat photopolymerization.
[0003] Certain additive manufacturing methods can be conducted using thermoplastic polymers (e.g., polycarbonate, polyamides, polyaryletherketones, and polyarylethersulfones), which include material extrusion, fused deposition modeling, and powder bed fusion. Powder bed fusion, in general, involves selective fusing of materials in a powder bed. The method can fuse parts of a layer of powder material, move upward in a working area, add another layer of powder material, and repeat the process until an object is built up therefrom. The powder bed fusion process can use unfused media to support overhangs and thin walls in the object being produced, which can reduce the need for temporary auxiliary supports in forming the object. In selective heat sintering, a thermal printhead can apply heat to layers of powdered thermoplastic; when a layer is finished, the powder bed moves down, and an automated roller adds a new layer of material which is sintered to form the next cross-section of the object. Selective lasersintering is another powder bed fusion process that can use one or more lasers to fuse powdered thermoplastic polymers into the desired three-dimensional object.
[0004] Materials for powder bed fusion processes preferably have a uniform shape, size, composition and melting behavior. The preparation of such powders from thermoplastic polymers on an economical and large scale is not straightforward. What is more, it can be difficult to use amorphous thermoplastic polymers, particularly in powder bed fusing processes such as selective laser sintering, because such thermoplastic polymers may not exhibit a single sharp melting point or have two melting points (e.g., has two or more crystalline phases). Problems may arise, because the powder bed is typically held just below the melting temperature of the polymer and non-uniform singular melting temperature may cause problems in distribution of the powder in each successive layer and dissipation of the applied thermal energy source (e.g., a laser beam) into the regions surrounding where the energy source contacts or strikes the powder bed. These problems can result in less efficient printing, unstable processing as well as poor feature resolution in the intended three-dimensional object being produced.
[0005] Preparations of thermoplastic such as polycarbonate and polyaryletherketone powders for powder bed fusion have been described, for example, in U.S. Pub. No. 2017 / 9567443 B2, Japanese Pat. No. 2017 / 095650 A, and U.S. Pub. No. 2018 / 0244863 Al. These describe methods that include dissolving polycarbonate in a suitable organic solvent, addition of a dispersing polymer to promote and sustain emulsion formation, and addition of a solvent that is miscible with the organic solvent but that is not a solvent for the polycarbonate, resulting in emulsion formation and subsequent precipitation of polycarbonate powder. WO 2018 / 071578 Al and U.S. Pub. No. 2018 / 0178413 Al describe the use of solvents to induce crystalline domain formation in pre-formed powder particles produced from grinding methods. U.S. pat. No. 11,365,284, describe dissolving polycarbonate in a solvent at elevated temperatures and precipitating of polycarbonate particles upon cooling from the elevated temperature. U.S. Pat. No. 3,214,407 describes forming a polycarbonate powder by the addition of a non- solvent.
[0006] Accordingly, it would be desirable to provide method to form semi-crystalline polymeric powders, wherein the method may control the crystallization, for example, to realize a singular distinct melt peak and other desirable characteristics useful for making additive manufactured articles.SUMMARY OF THE INVENTION
[0007] Applicant has discovered a method of forming semi-crystalline powders useful for additive manufacturing having a singular distinct melt peak even for those polymers that form more than one distinct melt peaks when crystallizing not using the method herein. The polymer may be an amorphous prior to the method and after crystallizing by the method, the induced crystallized polymer reverts to an amorphous polymer upon melting and cooling such as when forming an article by additive manufacturing (reverts to amorphous under normal thermoplastic polymer processing conditions, for example, heating and cooling rates of 1 °C / min to 100 °C / min, with 20 °C / min being standard for assessing such behavior). The method may also be used to shape a single melt peak that may be more advantageous for 3D printing (e.g., reduce the tail of the melt peak).
[0008] The crystallinity of the thermoplastic polymer may be determined by any suitable methods such as those known in the art. Illustratively, the percent crystallinity may be determined by x-ray diffraction including, for example, wide angle x-ray diffraction (WAXD), such as by using a Rigaku SmartLab x-ray diffractometer, or by differential scanning calorimetry (DSC), such as by using a TA Instruments DSC250 differential scanning calorimeter (ASTM D3418 - 15). The onset of the Tg, Tm and Tc peaks likewise are determined as per ASTM D3418 (i.e., deviation of the scan from linear) and unless otherwise stated herein any of these temperatures are to be understood to mean the onset temperatures. It is understood that amorphous means that the polymer essentially fails to display crystallinity in X-ray diffraction pattern or fails to display a melt peak in DSC. Herein, DSC is run at a heating rate of 20°C / min unless otherwise specified.
[0009] An illustration of the invention is a method of preparing a semi-crystalline thermoplastic polymer powder, the method comprising:(i) mixing, at a solubilization temperature, a thermoplastic polymer in a polar aprotic solvent and an inorganic submicron powder to form a mixture comprised of the thermoplastic polymer dissolved in the polar aprotic solvent and the inorganic submicron powder suspended therein; and(ii) Precipitating, at a precipitation temperature, a portion of the thermoplastic polymer dissolved in the polar aprotic solvent precipitates from the mixture to form a slurry comprised of the semi-crystalline thermoplastic powder.
[0010] The submicron powder means the powder has an average primary particle size of less than 2 micrometers whether the primary particles arc agglomerated into secondary particles (e.g., carbon black and hydroxyapatite) or individual unbonded primary particles (e.g., clay minerals). That is, there is a substantial portion of the submicron powder that has a diameter of at most 1 micrometer to realize a specific surface area that may desirably affect the arrangement of the polymer molecules during precipitation. The powders are particularly useful for making additive manufactured articles comprised of amorphous thermoplastic polymers having embedded therein the inorganic submicron powders at low concentrations.
[0011] Further areas of applicability will become apparent from the description provided herein. The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The drawings described herein are for illustrative purposes only of selected embodiments and are not intended to limit the scope of the present disclosure.
[0013] Figure 1 : is a differential scanning calorimetry (DSC) plot of a thermoplastic polymer not of this invention.
[0014] Figure 2: is an optical micrograph of a thermoplastic polymer of this invention.
[0015] Figure 3: is a DSC plot of a thermoplastic polymer of this invention.
[0016] Figure 4: is an optical micrograph of a thermoplastic polymer of this invention.
[0017] Figure 5 : is a DSC plot of a thermoplastic polymer of this invention.
[0018] Figure 6: is a DSC plot of a thermoplastic polymer of this invention.
[0019] Figure 7 : is a DSC plot of a thermoplastic polymer of this invention.DETAILED DESCRIPTION
[0020] The method is comprised of forming a mixture of a thermoplastic polymer dissolved in a polar aprotic solvent (“solution”) and an inorganic submicron powder (“submicron powder”) dispersed therein (suspension). The submicron powder is suspended and agitated sufficiently to be dispersed throughout the suspension. The agitation may be any suitable method such as those in the art rendering any reasonable shear rate including ultrasonic agitation. Generally, high shear is not required and low to moderate shear may be employed (e.g., 1 s'1to200 s’1). Agitation can be achieved with any commercially available mixers; for example, a mixer such as a Hci-Torquc 200 reactor stirring motor can be used.
[0021] The submicron inorganic powder has an average particle size of at most 2 micrometers and desirably at most 1.5 micrometer, 1 micrometer 0.5 micrometer or 0.3 micrometer in diameter. The powder may be comprised of primary particles that are chemically bound into secondary particles (e.g., carbon black) and or the primary particles may not be chemically bound other than by hydrogen or Van-der Waals forces (e.g., clay minerals).
[0022] Exemplary powders may include phosphate (e.g., hydroxyapatite) carbonates (e.g., calcium carbonate), talc, silica, wollastonite, clay, calcium sulfate, mica, inorganic glass (e.g., silica, alumino-silicate, borosilicate, alkali alumino silicate and the like), oxides (e.g., alumina, zirconia, magnesia, silica “quartz”, fumed silica, and calcia), carbides (e.g., boron carbide and silicon carbide), nitrides (e.g., silicon nitride, aluminum nitride), combinations of oxynitride, oxycarbides, or combination thereof. The powder desirably comprises an acicular mineral or platy mineral. Examples of useful powders include talc, clay minerals, flakes of inorganic glass, metal platelets, or graphite, mullite, mica, wollastanite, hydroxyapatite, carbon black or combination thereof. Desirably, the powder is a clay (e.g., of clays include those comprised of kaolin, or smectite clay minerals), carbon (e.g, graphene, graphite, carbon black, carbon fibers, and carbon nanotubes) or combination thereof.
[0023] Acicular herein means the particles of the powder have an aspect ratio that is at least 2 to 50, having needlelike or platy morphology, but preferably has a platy morphology. Needlelike meaning that there are two smaller equivalent dimensions (typically referred to as height and width) and one larger dimension (typically the length). Platy meaning that there are two larger somewhat equivalent dimensions (typically width and length) and one smaller dimension (typically height). More preferably, the aspect ratio is at least 3, 4 or 5 to 25, 20 or 15. The average aspect ratio may be determined by micrographic techniques measuring the longest and shortest dimension of a random representative sample of the particles (e.g., 100 to 200 particles).
[0024] Exemplary carbon blacks typically have an oil absorption number (OAN) of about 80 to 200 ccs per 100. (ASTM D-2414-09). The specific surface area (ISO 9277:2010) may be any useful, and generally is at least 10, 20 or 50 m2 / g to any practical including 1000, 500, 300 or 200 m2 / g.
[0025] The carbon black may be a standard carbon black which is not specially treated to render it nonconductivc. Standard carbon black is carbon black which is not specifically surface treated or oxidized. Alternatively, one or more conductive carbon blacks may be used exclusively or in conjunction with the standard carbon black. Conductive carbon blacks are generally recognized as having at a purity of at least 97% carbon, OAN of 100 or greater and specific surface area of 120 m2 / g or greater. Examples of standard carbon blacks include RAVEN 790, RAVEN 450, RAVEN 500, RAVEN 430, RAVEN 420 and RAVEN 410 carbon blacks available from Colombian and carbon blacks available from Cabot Corporation under the tradenames VULCAN, PROPEL, REGAL, STERLING, and SPHERON.
[0026] The amount of the powder may be any amount useful to impart the desired melt behavior. The amount of powder generally is from 0.05 %, 0.1 %, 0.25 %, 0.5 % or 1% to 5 % or 3% by weight of the polymer and powder.
[0027] The thermoplastic polymer may be any that is soluble in a polar aprotic solvent such as a thermoplastic polymer having a repeating unit comprised of one or more of a carbonyl, sulfur dioxide, and sulfone group. The carbonyl group may be a part of a carbonate, ester, amide, or imide in the thermoplastic polymer. The thermoplastic polymer may have one or more other repeating units such as an ether. Examples of useful thermoplastic polymers include polyamides, polycarbonates, polyketones, polysulfones, polyarylates and polyimides and combinations thereof. The thermoplastic polymer may be linear or branched. The thermoplastic polymer may be aliphatic or aromatic with it desirable for the polymer to have at least a portion of said polymer comprised of repeating aromatic units within the polymer backbone, where it generally is desirable for at least about 50% by mole of the polymer to be aromatic (i.e., aromatic groups make up 50% or more of the molar mass of the polymer).
[0028] The method is particularly useful to make composite thermoplastic polymer powders where the thermoplastic polymer is one that displays essentially no crystallinity when heated and cooled under conventional plastic processing heating rates (e.g., 1 to 200 °C / min, with 20 °C / min being a common rate when assessing the melt behavior of thermoplastic polymers by differential scanning calorimetry “DSC”). That is, the induced crystalline polymer upon melting and cooling reverts to an amorphous polymer aiding for example the suppression of two or more melt peaks. The thermoplastic polymer may be a homopolymer or a copolymer.Desirably, the thermoplastic polymer is comprised of a thermoplastic polymer having induced crystallinity (“induced crystalline polymer).
[0029] Examples of useful polycarbonates such as a polymer or copolymer having repeating structural carbonate units of formula (1):(1 )wherein at least 60 percent of the total number of R1groups are aromatic, or each R1contains at least one Ce-30 aromatic group. Specifically, each R1can be derived from a dihydroxy compound such as an aromatic dihydroxy compound of formula (2) or a bisphenol of formula (3), as follows:In formula (2), each Rhis independently a halogen atom, for example bromine, a Ci-io hydrocarbyl group such as a Ci-io alkyl, a halogen-substituted Ci-io alkyl, a Ce-io aryl, or a halogen- substituted Ce-io aryl, and n is 0 to 4.
[0030] In formula (3), Raand Rbare each independently a halogen, C1-12 alkoxy, or C1-12 alkyl, and p and q are each independently integers of 0 to 4, such that when p or q is less than 4, the valence of each carbon of the ring is filled by hydrogen. In certain embodiments, p and q areeach 0, or p and q are each 1 , and Raand Rbare each a C1-3 alkyl group, specifically methyl, disposed meta to the hydroxy group on each arylene group. Xais a bridging group connecting the two hydroxy-substituted aromatic groups, where the bridging group and the hydroxy substituent of each CY, arylene group are disposed ortho, meta, or para (specifically para) to each other on the C& arylene group, for example, a single bond, — O — , — S — , — S(=O) — , — S(=O)2 — (e.g., bisphenol-S polycarbonate, polysulfone), — C(=O) — (e.g., polyketone), or a C1-18 organic group, which can be cyclic or acyclic, aromatic or non-aromatic, and can further comprise heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon, or phosphorous. For example, Xacan be a substituted or unsubstituted C3-18 cycloalkylidene; a C1-25 alkylidene of the formula — C(Rc)(Rd) — wherein Rcand Rdare each independently hydrogen, C1-12 alkyl, C1-12 cycloalkyl, C7-12 arylalkyl, C1-12 heteroalkyl, or cyclic C7-12 heteroarylalkyl; or a group of the formula— C(=Re) — wherein Reis a divalent C1-12 hydrocarbon group. Certain illustrative examples of dihydroxy compounds that can be used are described, for example, in WO 2013 / 175448 Al, US 2014 / 0295363, and WO 2014 / 072923.
[0031] Specific dihydroxy compounds include resorcinol, 2,2-bis(4-hydroxyphenyl) propane (“bisphenol A” or “BPA”), 3,3-bis(4-hydroxyphenyl) phthalimidine, 2-phenyl-3,3'- bis(4-hydroxyphenyl) phthalimidine (also known as N-phenyl phenolphthalein bisphenol, “PPPBP”, or 3,3-bis(4-hydroxyphenyl)-2-phenylisoindolin-l-one), l,l-bis(4-hydroxy-3- methylphenyl)cyclohexane, and l,l-bis(4-hydroxy-3-methylphenyl)-3,3,5-trimethylcyclohexane (isophorone bisphenol).
[0032] Poly carbonates may also include copolymers comprising carbonate units and ester units (“poly(ester-carbonate)s”, also known as polyester-polycarbonates). Poly(ester- carbonate)s further contain, in addition to recurring carbonate chain units of formula (1), repeating ester units of formula (4):(4) O O- C - T — C — O - J - O - wherein J is a divalent group derived from a dihydroxy compound (which includes a reactive derivative thereof), and can be, for example, a C2-10 alkylene, a C6-20 cycloalkylene a C6-20arylene, or a polyoxyalkylene group in which the alkylene groups contain 2 to 6 carhon atoms, specifically, 2, 3, or 4 carbon atoms; and T is a divalent group derived from a dicarboxylic acid (which includes a reactive derivative thereof), and can be, for example, a C2-20 alkylene, a C6-20 cycloalkylene, or a C6- 0 arylene. Copolyesters containing a combination of different T or J groups can be used. The polyester units can be branched or linear.
[0033] Specific dihydroxy compounds include aromatic dihydroxy compounds of formula (2) (e.g., resorcinol), bisphenols of formula (3) (e.g., bisphenol A), a Ci-s aliphatic diol such as ethane diol, n-propane diol, i-propane diol, 1,4-butane diol, 1,6-cyclohexane diol, 1,6- hydroxymethylcyclohexane, or a combination comprising at least one of the foregoing dihydroxy compounds. Aliphatic dicarboxylic acids that can be used include C6-20 aliphatic dicarboxylic acids (which includes the terminal carboxyl groups), specifically linear Cs-i2 aliphatic dicarboxylic acid such as decanedioic acid (sebacic acid); and alpha, omega-Ctdicarboxylic acids such as dodecanedioic acid (DDDA). Aromatic dicarboxylic acids that can be used include terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, 1,6-cyclohexane dicarboxylic acid, or a combination comprising at least one of the foregoing acids. A combination of isophthalic acid and terephthalic acid wherein the weight ratio of isophthalic acid to terephthalic acid is 91:9 to 2:98 can be used.
[0034] Specific ester units include ethylene terephthalate units, n-propylene terephthalate units, n-butylene terephthalate units, ester units derived from isophthalic acid, terephthalic acid, and resorcinol (ITR ester units), and ester units derived from sebacic acid and bisphenol A. The molar ratio of ester units to carbonate units in the poly(ester-carbonate)s can vary broadly, for example 1:99 to 99:1, specifically, 10:90 to 90:10, more specifically, 25:75 to 75:25, or from 2:98 to 15:85.
[0035] The polycarbonates may have an intrinsic viscosity, as determined in chloroform at 25° C, of 0.3 to 1.5 deciliters per gram (dl / gm), specifically 0.45 to 1.0 dl / gm. The polycarbonates can have a weight average molecular weight of 5,000 to 200,000 Daltons, specifically 15,000 to 100,000 Daltons, as measured by gel permeation chromatography (GPC), using a crosslinked styrene-divinylbenzene column and calibrated to polycarbonate references. GPC samples are prepared at a concentration of 1 mg per mL (mg / mL) and are eluted at a flow rate of 1.5 mL per minute.
[0036] Examples of useful polysulfones may include polyarylethersulfones (PAES) which may be represented by:
[0037] wherein n is any integer value that gives rise to the PAES having an weight average molecular weight (Mw) anywhere from 1, 10, or 20 to 1000, 500 or 200 kDa, m typically varies from 0 to 10, each occurrence of R1represents an aromatic ring or fused rings of about 5- 10 carbon atoms, such as but not limited to: 1,2-, 1,3-, or 1,4-phenylene, or a diphenylene such as but not limited to 4,4’ -diphenylene, and each occurrence of R2is independently C1-C20 alkyl, C5- Cis or C5-C12 aromatic ring or fused rings consisting of 5-10 carbon atoms, or a combination thereof. The fragment structure -R1-S(=O)2-R1- may also represent either of the fused heterocyclic ring structures shown in formulas 2 and 3; and wherein at least 60% of the total number of R1groups are aromatic, or each R2contains at least one C6-30 aromatic group. The fragment structure -R1-S(=O)2-R1- may also represent either of the fused heterocyclic ring structures shown in formulas 2 and 3:
[0039] In another embodiment, the PAES of formula (1), m has an integer value greater than or equal to zero (typically from 1 to 10, 6, 5, 4, 3, or 2), and each R2is a residue of a dihydroxy compound such as an aromatic dihydroxy compound:
[0040] In formulas (3), (4), and (5), each R3, R4, and R5is independently, for example, but not limited to: a halogen atom (e.g., chlorine or bromine), a C3-20 alkoxy, a C1-20 hydrocarbyl group (e.g., a C1-20 alkyl, a halogen-substituted C1-10 alkyl, a Ce-io aryl, or a halogen-substituted Ce-io aryl); and p, q, and r are each independently integers of 0 to 4, such that when p, q, or r is less than 4, the valence of each unsubstituted carbon of the ring is filled by hydrogen; and X represents a bridging group connecting the two phenolic groups, where the bridging group and the hydroxy substituent of each Q, arylene group are disposed ortho, meta, or para (preferably para) to each other on the Ce arylene group, and the X group consists of, for example: a single bond; -O-; -S-; -S(=O)-; -S(=O)2- (e.g., bisphenol-S); -C(=O)-; or a C1-20 organic group, which can be cyclic or acyclic, aromatic or non-aromatic, and can further comprise heteroatoms such as: halogens; oxygen; nitrogen; sulfur; silicon; or phosphorous.
[0041] Specific dihydroxy compounds include but are not limited to: resorcinol; 2,2- bis(4-hydroxyphcnyl)propanc (“bisphenol A" or “BPA”, in which in which each of aryl rings is para-substituted and X is isopropylidene in formula (3)); 3,3-bis(4-hydroxyphenyl)phthalimid- ine; 2-phenyl-3,3-bis(4-hydroxyphenyl)phthalimidine (also known as ‘W-phenyl phenolphthalein bisphenol”, “PPPBP”, or 3,3-bis(4-hydroxyphenyl)-2-phenylisoindolin-l-one); 1 , l-bis(4- hydroxy-3-methylphenyl)cyclohexane; l,l-bis(4-hydroxy-3-methylphenyl)-3,3,5-trimethyl- cyclohexane (also known as “isophorone bisphenol”).
[0042] Examples of polyarylethersulfones that are suitable may any one or more of:
[0044] Examples of useful PAES polymers are: polyethersulfone (PSU, CAS # 25667-42, formula 7), poly ( 1 ,4-phcnylcnc-cthcr-cthcr- sulfone (PES or PEES, CAS # 28212-68-2, formula 8), polyphenylenesulfone (PPSU, CAS # 25839-81-0, formula 9) and poly(bisphenol-A sulfone) (PSF, CAS # 25135-51-7, formula 10), such as are available under the tradenames RADEL from Curbel Plastics Inc., Arlington TX, PARYLS from UJU New Materials, Ltd., and UDEL from Solvay Specialty Polymers USA, LLC, Alpharetta, GA.
[0045] The thermoplastic polymer may be polyketone including polyketones having ether repeating units such as polyetherketone, polyetheretherketone, polyetherketoneketone. An exemplary polyketone without ether repeating units may be formed by the reaction of carbon monoxide, an alkene monomer in the presence of a group 8 to 10 transition metal catalyst. In particular, the method may be any one of those described in US Pat. Nos. 4,835,250; 4,894,435 and 5,138,032 and US Pat. Publ. No. 2008 / 0058494 each incorporated by reference in its entirety. In particular, the method, reaction conditions and monomers are those described in US Pat. No. 5,138,032 from col. 2 line 52 to col. 5, line 17 specifically incorporated herein by reference. Such polyketones are typically comprised of repeating units represented by
[0046] where A is the residue of an alkene monomer converted to a saturated hydrocarbon group, m is from about 1 to 6 and n is at least about 2 to any practicable amount to realize the desired number average molecular weight (Mn) useful in the invention. Desirably, the alkene monomer is comprised of an olefin having from 2 to 12, 8 or 6 carbons. Illustratively, the alkene monomer is ethylene or the alkene monomer comprises ethylene and at least one other olefin monomer such as propylene. When the polyketone is a copolymer of ethylene and another olefin monomer (e.g., propylene), the amount of ethylene and other olefin is as described in US Pat. No. 5,138,032 from col. 2, line 17 to col. 3, line 14. The polyketone desirably is one that is a terpolymer of carbon monoxide, ethylene and another alkene monomer (e.g., olefin of 3 to 12, 8 or 6 carbons and in particular propylene). Such poly ketone may be represented by random repeating units:
[0047] Where G is the saturated residue of an olefin of 3 to 12, 8 or 6 carbons polymerized through the double bond and x / y is at least 2 to 100 or 50 or 20. Desirably, G is propylene. The polyketone may be terminated by any useful group such as alkyl group, hydroxyl, ester, carboxylic acid, ether or combination thereof. The particular terminating group may arise from using a solvent such as a low molecular alcohol such as methanol or water or combination thereof. Examples of commercially available polyketones include those available under the tradename POKETONE from Hyosung, Korea.
[0048] Generally, the polyketone may be a poly aryletherketone (PAES) such as those known in the ail. Illustratively, the PAES may be polyetherketoneketone (PEKK) such as those known in the art and, in particular, amorphous PEKK as described from col. 2, line 13 to 55 of U.S. Pat. No. 10,364,349, incorporated herein by reference. PEKKs may be made by known methods such as those described in U.S. Pat. Nos 3,065,205; 3,441,538; 3,442,857; 3,516,966; 4,704,448; 4,816,556 and 6,177,518.
[0049] The polyamide may be any of those known in the art and and commonly are semicrystalline as described from col. 4, line 7 to col. 5, line 22 of U.S. Pat. No. 5,391,640, incorporated herein by reference. In particular, the polyamide may be amorphous as described from col. 5, line 23 to col. 8, line 12 of U.S. Pat. No. 5,391,640, incorporated herein by reference. Examples of conventional polyamides include polypyrrolidone (nylon 4), polycaprolactam (nylon 6), polyheptanolactam (nylon 7), polycaprylactam (nylon 8), polynonanolactam (nylon 9), polyundecaneolactam (nylon 11), polydodecanolactam (nylon 12), poly(tet-ramethylenediamine-co-oxalic acid) (nylon 4,2), poly(-tetramethylenediamine-co-adipic acid) (nylon 4,6), poly(tctramcthylcncdiaminc-co-isophthalic acid) (nylon 4,1), polyhexamethylene azelaiamide (nylon 6,9), polyhexamethylene sebacamide (nylon 6,10), polyhexa- 5 methylene isophthalamide (nylon 6, IP), polymetaxyly-lene adipamide (nylon MXD6), the polyamide of n-dodecanedioic acid and hexamethylenediamine (nylon 6,12), the polyamide of dodecamethylenediamine and n-dodecanedioic acid (nylon 12,12), as well as copoly- 10 mers thereof which include: hexamethylene adipamide-caprolactam (nylon 6,6 / 6), hexamethylene adipamide / -hexamethylene-isophthalamide (nylon 6,6 / 6IP), hexa-methyleneadipamide / hexamethylene-terephthalamide (nylon 6,6 / 6T), trimethylene adipamide-hexamethy- 15 lenc-azclaicamidc (nylon trimcthyl 6, 2 / 6, 2), and hcxa-mcthylcnc adipamidc-hcxamcthylcnc- azelaicamide caprolactam (nylon 6, 6 / 6, 9 / 6) as well as others which are not particularly delineated here.
[0050] The polyimide may be any of those known in the art and desirably are known aromatic polyimides. Illustratively, Aromatic polyimides that may be suitable are described in U.S. Pat. Nos. 3,179,631; 3,249,588 and 4,755,555, each incorporated herein by reference. More particularly, the polyimide is amorphous such as those described by A. Rosenberg, et. al., in Optical Materials Express Vol. 8, No. 8, 1 Aug. 2018, 2159.
[0051] The polar aprotic solvent (solvent) may be any useful solvent that enables the dissolution of thermoplastic sufficiently to carry out the precipitating such as those described above, each incorporated herein by reference. The precipitating may be by any method that perturbs the dissolution of the polymer such as changing the temperature, adding a non-solvent, removing the solvent or any combination thereof.
[0052] In a particular illustration, the thermoplastic polymer (e.g., polycarbonate) dissolves in a halogenated solvent. The halogenated solvent may be, for example, a halogenated aliphatic or halogenated aromatic hydrocarbon and in particular, those having at most about 6 carbon atoms, or aromatic compounds that include one or more halogen atoms in the structure. In particular, the halogenated hydrocarbon may be a chlorinated hydrocarbon and in particular a chlorinated alkane or alkene such as chloromethane, dichloromethane, trichloromethane, 1,2- dichloroethane, or 1,1,1 -trichloroethane, or a chlorinated arene such as but not limited to chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, or 1,2,3-trichlorobenzene, or any combination thereof. Under agitation, the thermoplastic polymer is precipitated by the addition of a non- solvent comprised of a ketone such as methyl ethyl ketone, (2 butanone), ethyl ethyl ketone (3 pentanone), methyl propyl ketone (2 pentanone), di-isopropyl ketone and methyl isobutyl ketone. The amount of non-solvent may be any useful amount to cause the precipitation (10% to 200%, 100 %, or 50% by volume) in the absence of any other perturbance. Desirably, the non- solvent has a boiling point above the precipitating temperature and the solvent has a boiling point below the precipitating temperature, when precipitating by removing the solvent and adding a nonsolvent. After the addition of the non- solvent the temperature may be raised to simultaneously remove the solvent and separate it for reuse without further purification.
[0053] Another illustration is dissolving thermoplastic polymer such as an amorphous polycarbonate in a polar aprotic solvent to form a first solution of solubilized polycarbonate at a solubilizing temperature to form the suspension. The first solution is then cooled to a precipitation temperature that is lower than the solubilizing temperature, where a portion of the solubilized polycarbonate precipitates from the suspension to form the slurry with induced crystalline polycarbonate powder. Examples solvents useful in such a method may include dimethyl sulfoxide (DMSO), diphenyl ether, anisole or combination thereof.
[0054] The solubilizing temperature may include heating the amorphous polycarbonate in the polar aprotic solvent to form the suspension, the solubilizing temperature being greater than room temperature (~20 °C) and desirably less than the boiling point temperature, but a higher temperature may be employed, for example, by applying a pressure (e.g., greater than 1 bar to 500 bar). The precipitation temperature may be any temperature below the solubilizing temperature where precipitation occurs with room temperature being convenient.
[0055] The semi-crystalline thermoplastic powder may be separated by any suitable means such as those known in the art. Examples may include filtration, settling including by centrifugation, and removal of the solvent by any known technique (e.g., heating, vacuum drying, freeze drying, critical fluid drying or any combination thereof).
[0056] The semi-crystalline thermoplastic powder may exhibit the following physical characteristics. The powder desirably has a D90 particle size of less than about 150 pm; i.e., 90 vol % of the particles in the total distribution of the powder have a particle diameter of 150 pm or smaller. The powder desirably has an average particle diameter or D50 of 20 pm, or 30 pm to 70 pm, 50 pm or 40 pm. The powder may be in the form of spheroidal particles. Various crystallinity values are possible, where the powder may have at least about 20% crystallinity, at least about 25% to 50%, 40% or 35% crystallinity.
[0057] Powder bed fusing or powder bed fusion further includes all laser sintering and all selective laser sintering processes as well as other powder bed fusing technologies as defined by ASTM F2792-12a. For example, sintering of the powder composition can be accomplished via application of electromagnetic radiation other than that produced by a laser, with the selectivity of the sintering achieved, for example, through selective application of inhibitors, absorbers, susceptors, or the electromagnetic radiation (e.g., through use of masks or directed laser beams). The method has been found to be able to tailor the melt peaks of the induced crystallinethermoplastic polymer powder allowing for more efficient and effective additive manufacturing such as those employing fusion of a powder bed, including selective laser sintering (SLS), multi jet fusion (MJF), high speed sintering (HSS), and electrophotographic 3D-printing. In particular, the method allows for the crystallization of an amorphous polymer that in the absence of the inorganic particulates as described herein may have two or more distinct melt peaks when crystallized by precipitation. This allows for the making of amorphous manufactured articles using the induced crystalline powders described herein.
[0058] After separation the induced crystalline powder may be washed with a solvent (e.g., water and / or a volatile organic solvent such as alcohol, ketone, ether, ester or hydrocarbon in which the thermoplastic polymer does not significantly dissolve) to remove the solvent in which the thermoplastic polymer was dissolved and precipitated. The powder with or without washing may be further dried by any suitable method such as those known in the art. The drying, for example performed by heating to any temperature useful for removing the solvent. Illustratively, the temperature may be above 60 °C, 80 °C, 100 °C, 120 °C, 140 °C, to below the glass transition temperature of the induced crystalline polymer powder (e.g., -155 °C for polycarbonate), and preferably under reduced pressure. Desirably the temperature is at least 10 °C below the glass transition temperature.
[0059] After drying and separation, the powder may be further processed to realize the desired particle size and morphology by any suitable method such as one or more known in the art. For example, the induced crystalline thermoplastic powder may be subject to sieving, classification and grinding. Exemplary grinding may include grinding by pin mills, media mills, jet milling and hammer mills at ambient temperature (10 to 30 °C) or other temperatures such as common in cryogrinding.
[0060] Flowability herein means the flowability as determined by Method A of ASTM D 1895 using a 10 or 15 mm nozzle. Generally, the polycarbonate powder has a flowability of at least about 0.5 g / s, 1 g / s or 2 g / s to any practically achievable rate (e.g., 50 g / s) using a 15 mm nozzle.ILLUSTRATIONS
[0061] Illustration 1. A method of preparing a semi-crystalline thermoplastic polymer powder, the method comprising:(i) mixing, at a solubilization temperature, a thermoplastic polymer in a polar aprotic solvent and an inorganic submicron powder to form a mixture comprised of the thermoplastic polymer dissolved in the polar aprotic solvent and the inorganic submicron powder suspended therein; and(ii) precipitating, at a precipitation temperature, wherein a portion of the thermoplastic polymer dissolved in the polar aprotic solvent precipitates from the mixture to form a slurry comprised of the semi-crystalline thermoplastic polymer powder.
[0062] Illustration 2. The method of illustration 1, wherein the semi-crystalline thermoplastic polymer powder has the inorganic submicron powder embedded therein.
[0063] Illustration 3. The method of illustration 2, wherein the inorganic submicron powder is comprised of an acicular inorganic powder.
[0064] Illustration 4. The method of illustration 3, wherein the acicular inorganic submicron powder is platy.
[0065] Illustration 5. The method any one of the preceding illustrations, wherein the inorganic submicron powder is comprised of one or more of carbon black, graphene, carbon nano tubes, carbon fibers, clay, hydroxyapatite, talc, wollastonite and attapulgite.
[0066] Illustration 6. The method of any one of the preceding illustrations, wherein the precipitating is by cooling from the solubilization temperature to the precipitation temperature.
[0067] Illustration 7. The method of any one of illustrations 1 to 5, wherein the precipitating comprises adding a non- solvent, heating from the solubilization temperature to the precipitation temperature, and removing the polar aprotic solvent from the mixture.
[0068] Illustration 8. The method of illustration 7, wherein a reduced pressure is used when removing the polar aprotic solvent.
[0069] Illustration 9. The method of either illustration 7 or 8, wherein the polar aprotic solvent has a boiling point below the precipitation temperature.
[0070] Illustration 10. The method of illustration 9, wherein the non-solvent has a boiling point above the precipitation temperature.
[0071] Illustration 11. The method of any one of illustrations 7 to 11, wherein the boiling point of the non-solvent is at least 20 °C greater than the boiling point of the polar aprotic solvent.
[0072] Illustration 12. The method of illustration 11 , wherein the boiling point of the non- solvcnt is at least 40 °C greater than the boiling point of the polar aprotic solvent.
[0073] Illustration 13. The method of any one of illustrations 7 to 12, wherein the polar aprotic solvent after removing is sufficiently separated to be reused without further purification.
[0074] Illustration 14. The method of any one of illustrations 7 to 13, further comprising separating the semi-crystalline thermoplastic polymer powder having the inorganic submicron powder embedded therein from the non-solvent.
[0075] Illustration 15. The method of any one of the preceding illustrations, wherein the inorganic submicron powder is present in an amount of at most about 5% by weight of the thermoplastic polymer and inorganic submicron powder.
[0076] Illustration 16. The method of any one of the preceding illustrations, wherein the semi-crystalline thermoplastic polymer powder has one or more of: (i) a D90 particle size of less than about 300 pm, (ii) a D10 of at least 10 pm or (iii) an average particle size of about 20 pm to about 50 pm.
[0077] Illustration 17. The method of any one of the preceding illustrations, wherein a thermoplastic polymer subjected to the method in the absence of the inorganic submicron powder has at least two distinct melt peaks and the semi-crystalline thermoplastic polymer powder having the inorganic submicron powder embedded therein has one melt peak.
[0078] Illustration 18. The method of illustration 17, wherein the semi-crystalline thermoplastic polymer powder upon melting and cooling reverts to an amorphous thermoplastic polymer.
[0079] Illustration 19. An additive manufactured article comprising the semi-crystalline thermoplastic polymer powder fused together.
[0080] Illustration 20. The additive manufactured article of illustration 19, wherein the additive manufactured article’s fused semi-crystalline thermoplastic polymer powder has reverted to an amorphous polymer.
[0081] Illustration 21. An additive manufactured article comprised of an amorphous thermoplastic polymer having therein an inorganic submicron powder in an amount of 0.05% to 5% by weight of the amorphous thermoplastic polymer and inorganic submicron powder.
[0082] Illustration 22. The additive manufactured article of illustration 21 wherein the amount is 0.1% to 1%.
[0083] Illustration 23. The additive manufactured article of either illustration 21 or 22, wherein the inorganic submicron powder is comprised of one or more of carbon black, graphene, carbon nano tubes, carbon fibers, clay, hydroxyapatite, talc, wollastonite and attapulgite.EXAMPLESComparative Example 1
[0084] In a five liter reaction flask, 1.5 liters of dicloromethane (DCM) is added and stirred at 200 rpms at ambient temperature (~20 °C). TARFLON LC1500 polycarbonate (PC) available from Idemitsu Kosan Co., is added slowly until a concentration of about 15 g / 100 milliliters of DCM is realized. Upon complete dissolution of the PC in the DCM, methyl ethyl ketone (MEK) is added until precipitation occurs while stirring at 300 rpm. Typical amount of MEK added is about a 1 to 1 volume ratio as the DCM. Upon precipitation, the temperature is raised to - 40 °C for about 30 minutes and vacuum applied to preferentially remove the DCM and further the precipitation and concentrate the slurry of precipitated particles. The remaining solvent is removed by vacuum filtration leaving behind predominately MEK. The Particle size, shape and distribution (PSSD). PSSD was determined in air using a Microtrac S3500 instrument. Dio = 39.4 pm; D50 = 129.5 pm; D90 = 569.1 pm by volume and Dio = 17.76 pm; D50 = 27.73 pm; D90 = 55.25 pm by number.
[0085] Differential Scanning Calorimetry (DSC) and Crystallinity. The DSC was performed on a TA Instruments DSC 250 instrument scanning at 20 °C / min. and is shown in Figure 1. Onset of melting occurred in the first peak -190 °C and at 211.43 °C for the second peak. Upon cooling, a glass transition appeared at 142 °C, and again upon secondary heating at 147 °C, after which no melting behavior is observed.
[0086] Parts produced included thin discs, crosses, “window” test coupons, and ASTM D638 Type IV tensile bars. Parts featured a slight yellow tint but were mostly translucent and lacked the opaque appearance of typical laser sintering materials.Example 1
[0087] The method of Comparative Example 1 is repeated except prior to the addition of the MEK, an amount of GRAPHENEBLACK 3X, (Nanoxplorc) graphene powder is added to the solution equal to about 0.1% by weight of the PC and graphene.
[0088] ). The particle size is akin to the particle size of Comparative Example.1. An optical micrograph of the precipitated induced crystalline PC is shown in Figure 2. The DSC was performed on a TA Instruments DSC 250 instrument scanning at 20 °C / min. and is shown in Figure 3. Onset of melting of the sole peak occurs at 204.65 °C, and peaked at 236.09 °C. The sole peak displays a shoulder, but the DSC does not display an earlier melting peak. The cooling and subsequent melting displays the same amorphous behavior of the neat PC of Comparative Example 1.Example 2
[0089] The method of Comparative Example 1 is repeated except prior to the addition of the MEK, an amount of REGAL 660R (Cabot Corp.) carbon black powder is added to the solution equal to about 0.1% by weight of the PC and carbon black.
[0090] ) The particle size is akin to the particle size of Comparative Example.1. Differential Scanning Calorimetry (DSC) and Crystallinity. An optical micrograph of the precipitated induced crystalline PC is shown in Figure 4. The DSC was performed on a TA Instruments DSC 250 instrument scanning at 20 °C / min. and is shown in Figure 5. The sole peak displays a shoulder, but the DSC does not display an earlier melting peak. The onset and peak temperature are shown in Figure 5. The cooling and subsequent melting displays the same amorphous behavior of the neat PC of Comparative Example 1.Example 3
[0091] The method of Comparative Example 1 is repeated except prior to the addition of the MEK, an amount of hydroxyapatite (Sigma; CAS # 1306-06-05; Product # 900203) hydroxyapatite powder is added to the solution equal to about 0.4 % by weight of the PC and hydroxyapatite. The hydroxyapatite has a secondary particle size of 8 to 12 micrometers and asurface area of greater or equal to 100 m2 / g indicative of a primary particle size below 1 micrometer in diameter.
[0092] ). The particle size is akin to the particle size of Comparative Example.1. Differential Scanning Calorimetry (DSC) and Crystallinity. The DSC was performed on a TA Instruments DSC 250 instrument scanning at 20 °C / min. and is shown in Figure 6. The sole peak displays a shoulder, but the DSC does not display an earlier melting peak. The onset and peak temperature are shown in Figure 6. The cooling and subsequent melting displays the same amorphous behavior of the neat PC of Comparative Example 1.Example 4
[0093] The method of Comparative Example 1 is repeated except prior to the addition of the MEK, an amount of nanoclay (Sigma) nanoclay powder is added to the solution equal to about 1% by weight of the PC and nanoclay.
[0094] ). The particle size is akin to the particle size of Comparative Example.1. The DSC was performed on a TA Instruments DSC 250 instrument scanning at 20 °C / min. and is shown in Figure 7. The sole peak displays a tail, but no shoulder and the DSC does not display an earlier melting peak. The onset and peak temperature are shown in Figure 7. The cooling and subsequent melting displays the same amorphous behavior of the neat PC of Comparative Example 1. 1
Claims
CLAIMSWhat is claimed is:
1. A method of preparing a semi-crystalline thermoplastic polymer powder, the method comprising:(iii) mixing, at a solubilization temperature, a thermoplastic polymer in a polar aprotic solvent and an inorganic submicron powder to form a mixture comprised of the thermoplastic polymer dissolved in the polar aprotic solvent and the inorganic submicron powder suspended therein; and(iv) precipitating, at a precipitation temperature, wherein a portion of the thermoplastic polymer dissolved in the polar aprotic solvent precipitates from the mixture to form a slurry comprised of the semi-crystalline thermoplastic polymer powder.
2. The method of claim 1, wherein the semi-crystalline thermoplastic polymer powder has the inorganic submicron powder embedded therein.
3. The method of Claim 2, wherein the inorganic submicron powder is comprised of an acicular inorganic powder.
4. The method of claim 3, wherein the acicular inorganic submicron powder is platy.
5. The method any one of the preceding claims, wherein the inorganic submicron powder is comprised of one or more of carbon black, graphene, carbon nano tubes, carbon fibers, clay, hydroxyapatite, talc, wollastonite and attapulgite.
6. The method of any one of the preceding claims, wherein the precipitating is by cooling from the solubilization temperature to the precipitation temperature.
7. The method of any one of claims 1 to 5, wherein the precipitating comprises adding a non-solvcnt, heating from the solubilization temperature to the precipitation temperature, and removing the polar aprotic solvent from the mixture.
8. The method of claim 7, wherein a reduced pressure is used when removing the polar aprotic solvent.
9. The method of either claim 7 or 8, wherein the polar aprotic solvent has a boiling point below the precipitation temperature.
10. The method of claim 9, wherein the non-solvent has a boiling point above the precipitation temperature.
11. The method of any one of claims 7 to 11, wherein the boiling point of the non-solvent is at least 20 °C greater than the boiling point of the polar aprotic solvent.
12. The method of claim 11 , wherein the boiling point of the non-solvent is at least 40 °C greater than the boiling point of the polar aprotic solvent.
13. The method of any one of claims 7 to 12, wherein the polar aprotic solvent after removing is sufficiently separated to be reused without further purification.
14. The method of any one of claims 7 to 13, further comprising separating the semicrystalline thermoplastic polymer powder having the inorganic submicron powder embedded therein from the non- solvent.
15. The method of any one of the preceding claims, wherein the inorganic submicron powder is present in an amount of at most about 5% by weight of the thermoplastic polymer and inorganic submicron powder.
16. The method of any one of the preceding claims, wherein the semi-crystalline thermoplastic polymer powder has one or more of: (i) a D90 particle size of less thanabout 300 pm, (ii) a Dio of at least 10 pm or (iii) an average particle size of about 20 pm to about 50 pm.
17. The method of any one of the preceding claims, wherein a thermoplastic polymer subjected to the method in the absence of the inorganic submicron powder has at least two distinct melt peaks and the semi-crystalline thermoplastic polymer powder having the inorganic submicron powder embedded therein has one melt peak.
18. The method of claim 17, wherein the semi-crystalline thermoplastic polymer powder upon melting and cooling reverts to an amorphous thermoplastic polymer.
19. An additive manufactured article comprising the semi-crystalline thermoplastic polymer powder fused together.
20. The additive manufactured article of claim 19, wherein the additive manufactured article’s fused semi-crystalline thermoplastic polymer powder has reverted to an amorphous polymer.
21. An additive manufactured article comprised of an amorphous thermoplastic polymer having therein an inorganic submicron powder in an amount of 0.05% to 5% by weight of the amorphous thermoplastic polymer and inorganic submicron powder.
22. The additive manufactured article of claim 21, wherein the amount is 0.1% to 1%.
23. The additive manufactured article of either claim 21 or 22, wherein the inorganic submicron powder is comprised of one or more of carbon black, graphene, carbon nano tubes, carbon fibers, clay, hydroxyapatite, talc, wollastonite and attapulgite.
Citation Information
Patent Citations
Method for producing polycarbonate fine particles and polycarbonate resin powder
JP2017095650A
Assemblies containing polyetherketoneketone tie layers
US10364349B1
Producing semi-crystalline pulverulent polycarbonate and use thereof in additive manufacturing
US11365284B2
Process for preparing polyketone
US20080058494A1
Plastic flame housing and method of making the same
US20140295363A1