Metal reinforced polytetrafluoroethylene membrane, manufacturing method, and use
By using metal-reinforced polytetrafluoroethylene membranes in guided bone regeneration, and using a combination of microporous structure and implantable metal scaffolds, the problem of insufficient or excessive adhesion of the existing membrane layer is solved, and a new method is achieved in bone regeneration. Stable osteogenic effect and easy separation characteristics.
Patent Information
- Application Number
- PCT/CN2023/089811
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-24
AI Technical Summary
In clinical use, existing titanium-reinforced polytetrafluoroethylene membranes have problems such as insufficient adhesion, which makes separation difficult, or excessive adhesion, which causes soft tissue damage and affects the osteogenesis effect.
A metal-reinforced polytetrafluoroethylene membrane is used, which is composed of micro-stretched expanded polytetrafluoroethylene material and an implantable metal stent. A membrane layer with a suitable microporous structure is formed through a hot pressing process to ensure good adhesion to soft tissue at the same time. Easy to separate, and grooved stripes are designed on the surface of the film layer to enhance adhesion.
It provides a stable osteogenic space during guided bone regeneration, promotes new bone formation, avoids soft tissue damage, and improves the membrane's ease of retrieval and osteogenic effect.
Smart Images

Figure CN2023089811_24102024_PF_FP_ABST
Abstract
Description
Metal reinforced polytetrafluoroethylene membrane, manufacturing method and application Technical Field
[0001] The present application relates to the field of medical device technology, and in particular to a metal-reinforced polytetrafluoroethylene membrane, a manufacturing method and an application thereof. Background Art
[0002] Middle-aged and elderly people generally have problems such as poor periodontal conditions, high tooth loss rates and low dental implant penetration rates. As people pay more attention to oral problems, the size of the oral dental implant market will continue to increase.
[0003] In oral implant surgery, maintaining the stability of the implant is very important. If you want to maintain the stability of the implant, you need to have a certain bone thickness around the implant. However, most cases of tooth loss are generally accompanied by periodontal bone loss, which makes it insufficient to maintain the stability of the implant. Therefore, bone augmentation surgery has become a key part of implant restoration. Existing bone augmentation technologies include: Guide Bone Regeneration (GBR), Bone lock onlay grafting (Onlay bone grafting), Alveolar ridge split technique, Distraction Osteogenesis and Tenting technique, among which Guide Bone Regeneration (GBR) is more widely used.
[0004] Guided bone regeneration (GBR) involves placing a barrier membrane between soft tissue and bone defects to create a biological barrier. This prevents rapidly migrating connective tissue and epithelial cells, which interfere with bone formation, from entering the bone defect. This allows slower-migrating precursor osteoblasts, which have the potential for growth, to preferentially enter the defect and complete induction and growth. In GBR, preventing connective tissue from invading the alveolar ridge in the edentulous area and providing a stable three-dimensional space for bone tissue growth is crucial, and GBR barrier membranes play a decisive role in this process.
[0005] There are two common types of GBR barrier membranes on the market: absorbable barrier membranes and non-absorbable barrier membranes. Absorbable barrier membranes include animal-derived collagen membranes, allogeneic collagen membranes, and synthetic polymer oral barrier membranes. Absorbable barrier membranes do not need to be removed a second time and have excellent biocompatibility, but their ability to maintain space is poor, resulting in insufficient bone volume after GBR surgery. Non-absorbable membrane barrier membranes include titanium mesh stents, pure polytetrafluoroethylene membranes, and titanium-reinforced polytetrafluoroethylene membranes. The best of these is titanium-reinforced polytetrafluoroethylene membrane. Polytetrafluoroethylene has good biocompatibility with titanium, excellent mechanical properties, and can provide a stable space. However, because it is non-degradable, it requires a second surgery to remove.
[0006] For large-area bone defects or vertical bone defects, it is crucial to maintain bone formation space during GBR surgery. Since it is impossible to obtain initial stability of the implant during bone grafting surgery, staged implantation is generally performed (i.e. bone grafting first, then implantation). In this case, non-absorbable barrier membranes with strong space maintenance capabilities have absolute advantages. The use of non-absorbable barrier membranes for GBR surgery can predict better bone formation than using other absorbable barrier membranes, and the bone formation effect can also be observed when the non-absorbable barrier membrane is removed during the second-stage implantation surgery.
[0007] Regarding the titanium-reinforced polytetrafluoroethylene membrane with good application prospects, although it has the advantages of good biocompatibility and strong space maintenance ability, the performance of the common titanium-reinforced polytetrafluoroethylene membrane products on the market is not perfect. For example, there is a common expanded polytetrafluoroethylene membrane. During clinical use, the barrier membrane has good adhesion to the soft tissue, but it is also easy to cause the soft tissue to grow into the pores, making it difficult to bluntly separate the barrier membrane during a secondary operation. Sharp separation must be performed, which can easily damage the soft tissue, causing difficulties in clinical operations and greater trauma to patients. In terms of osteogenesis, due to the growth of soft tissue, a layer of pseudoperiosteum with a thickness of 1-3 mm is formed between the membrane and the osteogenesis area, thereby reducing the final osteogenesis height; for example, there is also a dense polytetrafluoroethylene membrane, which is easy to peel off, but its adhesion to the soft tissue is too poor. During clinical use, after the soft tissue covers the barrier membrane, the soft tissue is prone to rupture, resulting in membrane exposure, and it must be removed early, which ultimately affects the osteogenesis effect.
[0008] Summary of the Invention
[0009] According to various embodiments of the present application, a metal-reinforced polytetrafluoroethylene membrane, a manufacturing method, and an application are provided.
[0010] An embodiment of the present application provides a metal-reinforced polytetrafluoroethylene membrane, comprising a first membrane layer, a second membrane layer, and a metal bracket, wherein the metal bracket is located between the first membrane layer and the second membrane layer and is enclosed by the first membrane layer and the second membrane layer;
[0011] The materials of the first film layer and the second film layer are independently selected from micro-stretched expanded polytetrafluoroethylene with a stretching range of about 20% to 100%, and the micro-stretched expanded polytetrafluoroethylene has a microporous structure;
[0012] The formed metal reinforced polytetrafluoroethylene membrane has micropores with an overall average pore size of about 0.03 μm to 0.50 μm;
[0013] The material of the metal stent includes implantable metal.
[0014] In one embodiment, the metal reinforced polytetrafluoroethylene membrane as a whole satisfies one or more of the following properties (1) to (3):
[0015] (1) The pore size range of micropores is approximately 0.01 μm to 1.00 μm;
[0016] (2) The total thickness of the film layer area not covered with the metal bracket is about 0.10 mm to 0.50 mm;
[0017] (3) The total thickness of the film layer area covered with the metal bracket is about 0.20 mm to 0.80 mm.
[0018] In one embodiment, the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is smaller than the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer.
[0019] In one embodiment, the micro-stretched expanded polytetrafluoroethylene used to form the first film layer satisfies one or more of the following properties (1) to (3):
[0020] (1) The thickness is about 0.10mm to 0.40mm;
[0021] (2) The pore size of the micropores ranges from approximately 0.05 μm to 5.0 μm;
[0022] (3) The average pore size of the micropores is about 0.2 μm to 1.0 μm.
[0023] In one embodiment, the micro-stretched expanded polytetrafluoroethylene used to form the second film layer satisfies one or more of the following properties (1) to (3):
[0024] (1) The thickness is about 0.05mm to 0.3mm;
[0025] (2) The pore size of the micropores ranges from approximately 0.01 μm to 2.50 μm;
[0026] (3) The average pore size of the micropores is about 0.1 μm to 0.5 μm.
[0027] In one embodiment, the implantable metal includes pure titanium, titanium alloy or stainless steel.
[0028] In one embodiment, the thickness of the metal bracket is about 0.05 mm to 0.2 mm.
[0029] In one embodiment, the metal bracket is a prefabricated metal bracket.
[0030] In one embodiment, the metal bracket includes a metal center bar and a plurality of metal branch bars, wherein the plurality of metal branch bars are distributed on both sides of the metal center bar, and each of the metal branch bars is connected to the metal center bar respectively.
[0031] In one embodiment, a surface of the first film layer facing away from the metal support has groove-shaped stripes.
[0032] In one embodiment, there are multiple stripes arranged in parallel.
[0033] In one embodiment, each of the stripes includes a plurality of first stripes arranged along a first direction and a plurality of second stripes arranged along a second direction;
[0034] The first direction and the second direction are perpendicular to each other.
[0035] In one embodiment, in each of the stripes, the first stripes and the second stripes are arranged alternately.
[0036] In one embodiment, among the stripes, the length of each first stripe is greater than the length of each second stripe, and the width of each first stripe is the same as the width of each second stripe;
[0037] A plurality of the first stripes are arranged in a straight line, and a plurality of the second stripes are arranged in parallel;
[0038] The depth of each of the first stripes and each of the second stripes independently decreases from the middle to both ends.
[0039] In one embodiment, the depth of each of the first stripes and the depth of each of the second stripes are independently approximately 0 mm to 0.15 mm.
[0040] An embodiment of the present application further provides a method for manufacturing a metal-reinforced polytetrafluoroethylene membrane as described in any of the above embodiments, comprising the following steps:
[0041] Providing a mold, the mold comprising a mold base and a mold cover;
[0042] A first film, the metal bracket, and a second film are sequentially stacked on the mold base, wherein the metal bracket does not extend beyond the outer edges of the first film and the second film; the material of the first film and the second film are independently selected from micro-stretched expanded polytetrafluoroethylene with a stretching range of 20% to 100%, and the micro-stretched expanded polytetrafluoroethylene has a microporous structure;
[0043] covering the mold cover plate on the second film;
[0044] hot pressing the mold containing the first film, the metal bracket, and the second film;
[0045] After the hot pressing is completed and the temperature is lowered, the mold is removed; the formed metal reinforced polytetrafluoroethylene membrane has micropores with an overall average pore size of about 0.03 μm to 0.50 μm.
[0046] In one embodiment, the method further includes forming stripes on a surface of the first film facing away from the metal support.
[0047] In one embodiment, the step of forming stripes on the surface of the first film facing away from the metal support comprises:
[0048] A stripe template corresponding to the preset stripes is placed between the first film and the mold bottom plate.
[0049] In one embodiment, the step of hot pressing comprises:
[0050] The mold containing the first film, the metal bracket and the second film is pressed, heated and kept warm in sequence.
[0051] In one embodiment, the pressing method is locking pressing, and the locking torque is about 0.5N·m to 10N·m.
[0052] In one embodiment, the heating rate is about 30°C / min to 60°C / min, and the heating temperature is about 300°C to 380°C.
[0053] In one embodiment, the holding time is about 1 hour to 5 hours.
[0054] In one embodiment, the cooling rate is about 2°C / h to 10°C / h.
[0055] An embodiment of the present application further provides a barrier membrane, comprising the metal-reinforced polytetrafluoroethylene membrane as described in any of the above embodiments.
[0056] An embodiment of the present application further provides a use of the barrier membrane as described in the above embodiment in guided bone regeneration.
[0057] The details of one or more embodiments of the present application are set forth in the accompanying drawings and the description below. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the conventional technology, the following briefly introduces the drawings required for use in the embodiments or the conventional technology descriptions. Obviously, the drawings described below are merely embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the disclosed drawings without any creative work.
[0059] FIG1 is a schematic structural diagram of a metal-reinforced polytetrafluoroethylene membrane in one embodiment;
[0060] FIG2 is a top view of a metal-reinforced polytetrafluoroethylene membrane in one embodiment;
[0061] FIG3 is a scanning electron microscope image of the second film layer in one embodiment;
[0062] FIG4 is a schematic structural diagram of groove-shaped stripes on the surface of the first film layer facing away from the metal support in one embodiment;
[0063] FIG5 is a scanning electron microscope image of a surface of the first film layer facing away from the metal support in one embodiment;
[0064] FIG6 is a further magnified scanning electron microscope image of the surface of the first film layer facing away from the metal support in one embodiment;
[0065] FIG7 is a scanning electron microscope image of a cross-sectional position of a metal-reinforced polytetrafluoroethylene membrane in one embodiment;
[0066] FIG8 is a process flow chart for preparing a metal-reinforced polytetrafluoroethylene membrane in one embodiment;
[0067] FIG9 is a schematic diagram of a process for preparing a metal-reinforced polytetrafluoroethylene membrane using a mold containing a fixing clip in one embodiment;
[0068] Figure 10 is a schematic structural diagram of the mold in Figure 9, wherein a in Figure 10 is a front view of the mold after compaction, b in Figure 10 is a top view of the mold after compaction; and c in Figure 10 is a left view of the mold after compaction;
[0069] FIG11 is a schematic diagram of a process for preparing a metal-reinforced polytetrafluoroethylene membrane using a mold containing a fixing screw that does not cooperate with a nut in one embodiment;
[0070] FIG12 is a schematic structural diagram of the mold in FIG11 , wherein FIG12 a is a front view of the mold cover before pressing, FIG12 b is a top view of the mold after pressing; FIG12 c is a left view of the mold after pressing;
[0071] FIG13 is a schematic diagram of a process for preparing a metal-reinforced polytetrafluoroethylene membrane using a mold containing a fixing screw that cooperates with a nut in one embodiment;
[0072] FIG14 is a schematic structural diagram of the mold in FIG13 , wherein a in FIG14 is a front view of the mold after compaction; b in FIG14 is a top view of the mold after compaction; and c in FIG14 is a left view of the mold after compaction;
[0073] FIG15 shows the maximum peel force test results of Examples 1 to 6, Comparative Examples 1 and 2;
[0074] FIG16 is the histological observation results of H&E staining of the rabbit skull defect models in Example 2, Comparative Example 1 and Comparative Example 2;
[0075] FIG17 shows the new bone volume and area ratio results of the rabbit skull defect models in Example 2, Comparative Example 1, and Comparative Example 2;
[0076] FIG18 shows the osteogenesis height results of the beagle mandibular defect models in Example 4, Comparative Example 1, and Comparative Example 2;
[0077] FIG19 shows the bone formation rate results of the beagle mandibular defect models of Example 4, Comparative Example 1, and Comparative Example 2.
[0078] Explanation of the figure marks: 10: Metal reinforced polytetrafluoroethylene film; 110: First film layer; 111: Stripe; 111a: First stripe; 111b: Second stripe; 120: Second film layer; 130: Metal bracket; 20: Mold; 210: Mold base plate; 220: Mold cover plate; 230: Fixing clip; 240: Fixing screw; 250: Nut; 260: Threaded hole; 30: First film; 40: Second film; 50: Striped film plate. DETAILED DESCRIPTION
[0079] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0080] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" as used in this application includes any and all combinations of one or more of the relevant listed items.
[0081] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0082] Referring to FIG. 1 and FIG. 2 , an embodiment of the present application provides a metal-reinforced polytetrafluoroethylene membrane 10 , comprising a first membrane layer 110 , a second membrane layer 120 , and a metal bracket 130 . The metal bracket 130 is located between the first membrane layer 110 and the second membrane layer 120 , and is enclosed by the first membrane layer 110 and the second membrane layer 120 .
[0083] The materials of the first film layer 110 and the second film layer 120 are independently selected from micro-stretched expanded polytetrafluoroethylene with a stretching range of about 20% to 100%, and the micro-stretched expanded polytetrafluoroethylene has a microporous structure;
[0084] The formed metal reinforced polytetrafluoroethylene membrane 10 has micropores with an overall average pore size of about 0.03 μm to 0.50 μm;
[0085] The material of the metal stent 130 includes implantable metal.
[0086] FIG3 shows a scanning electron microscope image of the second membrane layer in one embodiment of the present application, showing its microporous structure. It can be understood that the first membrane layer also has a similar microporous structure.
[0087] The metal-reinforced polytetrafluoroethylene (PTFE) membrane 10 provided in one embodiment of the present application comprises a first membrane layer 110 and a second membrane layer 120 made of micro-stretched expanded polytetrafluoroethylene (EPTFE), and an implantable metal stent 130. The micro-stretched expanded polytetrafluoroethylene (EPTFE) membrane layer has a microporous structure, which provides good adhesion to soft tissue and is not easily exposed during clinical use. Furthermore, the micro-stretched expanded polytetrafluoroethylene (EPTFE) material and the metal stent 130 have good biocompatibility. The resulting metal-reinforced polytetrafluoroethylene membrane 10 can create a space for maintaining regeneration required for osteogenesis, fix bone, and / or perform other fixation and space maintenance functions. The resulting metal-reinforced polytetrafluoroethylene membrane 10 has a microporous structure with an average pore size of approximately 0.03 μm to 0.50 μm. This appropriate pore size facilitates the diffusion of nutrients and promotes effective bone reconstruction in the underlying osteogenic zone, while avoiding the problem of a dense polytetrafluoroethylene membrane with a non-porous structure that blocks nutrient diffusion and hinders osteogenesis. Furthermore, the appropriate micropore size ensures good adhesion between the membrane layer and soft tissue while also facilitating easy removal. The metal-reinforced polytetrafluoroethylene membrane 10 provided in the present application can be used as a barrier membrane in guided bone regeneration, and can be used in oral surgery, craniofacial surgery, and maxillofacial surgery to treat periodontal tissue defects.
[0088] It can be understood that the overall average pore size of the micropores on the metal reinforced polytetrafluoroethylene membrane 10 can be, for example but not limited to, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.10 μm, 0.11 μm, 0.12 μm, 0.13 μm, 0.14 μm, 0.15 μm, 0.16 μm, 0.17 μm, 0.18 μm, 0.19 μm, 0.20 μm, 0.21 μm, 0.22 μm, .23μm, 0.24μm, 0.25μm, 0.26μm, 0.27μm, 0.28μm, 0.29μm, 0.30μm, 0.31μm, 0.32μm, 0.33μm, 0.34μm, 0.35μm, 0.36μm, 0.37μm, 0.38μm, 0.39μm, 0.40μm, 0.41μm, 0.42μm, 0.43μm, 0.44μm, 0.45μm, 0.46μm, 0.47μm, 0.48μm, 0.49μm, 0.50μm, etc. In one embodiment, the overall average pore size of the micropores on the metal reinforced polytetrafluoroethylene membrane 10 is about 0.15μm to 0.2μm.
[0089] In one embodiment, the overall pore size of the metal reinforced polytetrafluoroethylene membrane 10 is in the range of about 0.01 μm to 1.00 μm.
[0090] The pore size range of the micropores on the metal reinforced polytetrafluoroethylene membrane 10 can completely block soft tissue cells, eliminate stimulation that may hinder bone formation, and provide stable space required for bone regeneration.
[0091] In one embodiment, the total thickness of the film layer area of the metal reinforced polytetrafluoroethylene film 10 not covered with the metal bracket 130 is about 0.10mm to 0.50mm. It is understandable that the total thickness of the film layer area of the metal reinforced polytetrafluoroethylene film 10 not covered with the metal bracket 130 can be, for example but not limited to, 0.10mm, 0.11mm, 0.12mm, 0.13mm, 0.14mm, 0.15mm, 0.16mm, 0.17mm, 0.18mm, 0.19mm, 0.20mm, 0.21mm, 0.22mm, 0.23mm, 0.24mm, 0.25mm, 0.26mm, 0.27mm, 0.28mm, 0.29mm, 0.30mm, 0.31mm, 0.32mm, 0.33mm, 0.34mm, 0.35mm, 0.36mm, 0.37mm, 0.38mm, 0.39mm, 0.40mm, 0.41mm, 0.42mm, 0.43mm, 0.44mm, 0.45mm, 0.46mm, 0.47mm, 0.48mm, 0.49mm, 0.50mm, 0.51mm, 0.52mm, 0.53mm, 0.54mm, 0.55mm, 0.56mm, 0.57mm, 0.58mm, 0.59mm, 0.60mm, 0.61mm, 0.62mm, 0.63mm, 0.64mm, 0.65mm, 0.66mm, 0.67mm, 0.68mm 0.27mm, 0.28mm, 0.29mm, 0.30mm, 0.31mm, 0.32mm, 0.33mm, 0.34mm, 0.35mm, 0.36mm, 0.37mm, 0.38mm, 0.39mm, 0.40mm, 0.41mm, 0.42mm, 0.43mm, 0.44mm, 0.45mm, 0.46mm, 0.47mm, 0.48mm, 0.49mm, 0.50mm, etc. In one embodiment, the total thickness of the film layer area of the metal-reinforced polytetrafluoroethylene film 10 not covered with the metal bracket 130 is about 0.10mm-0.30mm. In one embodiment, the total thickness of the film layer area of the metal-reinforced polytetrafluoroethylene film 10 not covered with the metal bracket 130 is about 0.20mm-0.25mm.
[0092] In one embodiment, the total thickness of the metal reinforced polytetrafluoroethylene membrane 10 where the metal bracket 130 is covered is about 0.20 mm to 0.80 mm. It can be understood that the total thickness of the film layer area covered with the metal bracket 130 in the metal reinforced polytetrafluoroethylene film 10 can be, for example but not limited to, 0.20mm, 0.22mm, 0.24mm, 0.25mm, 0.28mm, 0.30mm, 0.31mm, 0.35mm, 0.38mm, 0.39mm, 0.40mm, 043mm, 0.45mm, 0.46mm, 0.48mm, 0.50mm, 0.53mm, 0.55mm, 0.58mm, 0.59mm, 0.60mm, 0.62mm, 0.65mm, 0.66mm, 0.67mm, 0.70mm, 0.71mm, 0.73mm, 0.75mm, 0.77mm, 0.78mm, 0.80mm, etc. In one embodiment, the total thickness of the metal reinforced polytetrafluoroethylene membrane 10 covering the metal bracket 130 is about 0.30 mm to 0.50 mm. In one embodiment, the total thickness of the metal reinforced polytetrafluoroethylene membrane 10 covering the metal bracket 130 is about 0.40 mm.
[0093] In one embodiment, the stretching range of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is smaller than the stretching range of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer.
[0094] In one embodiment, the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is smaller than the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer.
[0095] In one embodiment, the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer is about 0.10 mm to 0.40 mm. It is understood that the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer can be, for example, but not limited to, about 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.20 mm, 0.21 mm, 0.22 mm, 0.23 mm, 0.24 mm, 0.25 mm, 0.26 mm, 0.27 mm, 0.28 mm, 0.29 mm, 0.30 mm, 0.31 mm, 0.32 mm, 0.33 mm, 0.34 mm, 0.35 mm, 0.36 mm, 0.37 mm, 0.38 mm, 0.39 mm, 0.40 mm, etc. In one embodiment, the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer is about 0.15 mm to 0.25 mm. In one embodiment, the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer is about 0.20 mm to 0.22 mm.
[0096] In one embodiment, the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer have a pore size range of about 0.05 μm to 5.0 μm.
[0097] In one embodiment, the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the first membrane layer is approximately 0.2 μm to 1.0 μm. The micro-stretched expanded polytetrafluoroethylene used to form the first membrane layer has a microporous structure, which facilitates adhesion between the membrane and soft tissue. It is understood that the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the first membrane layer can be, but is not limited to, approximately 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, etc.
[0098] In one embodiment, the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is about 0.05 mm to 0.3 mm. It is understood that the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer can be, for example, but not limited to, about 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.10 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.20 mm, 0.21 mm, 0.22 mm, 0.23 mm, 0.24 mm, 0.25 mm, 0.26 mm, 0.27 mm, 0.28 mm, 0.29 mm, 0.30 mm, etc. In one embodiment, the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is about 0.05 mm to 0.2 mm. In one embodiment, the thickness of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is about 0.05 mm to 0.15 mm.
[0099] In one embodiment, the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the second membrane layer have a pore size range of approximately 0.01 μm to 2.5 μm. In one embodiment, the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the second membrane layer have a pore size range of approximately 0.01 μm to 2.0 μm.
[0100] In one embodiment, the average pore size of the micropores of the microstretched expanded polytetrafluoroethylene used to form the second film layer is approximately 0.1 μm to 0.5 μm. The micropores of the microstretched expanded polytetrafluoroethylene used to form the second film layer are small microporous structures. Overall, the average pore size of the micropores of the microstretched expanded polytetrafluoroethylene used to form the second film layer is smaller than the average pore size of the micropores of the microstretched expanded polytetrafluoroethylene used to form the first film layer. This can completely block the growth of connective tissue or fibrous tissue into the bone formation area, which helps reduce stimuli that may hinder bone formation. It is understood that the average pore size of the micropores of the microstretched expanded polytetrafluoroethylene used to form the second film layer can be, for example, but not limited to, approximately 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, etc. In one embodiment, the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is about 0.1 μm to 0.3 μm.
[0101] In one embodiment, the implantable metal comprises pure titanium, a titanium alloy, or stainless steel.
[0102] In one embodiment, the implantable metal includes TA1 medical pure titanium, TC4 titanium alloy, or high nitrogen stainless steel.
[0103] In one embodiment, the thickness of the metal bracket 130 is approximately 0.05 mm to 0.2 mm. It is understood that the thickness of the metal bracket 130 may be, for example, but not limited to, 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.10 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.20 mm, etc. In one embodiment, the thickness of the metal bracket 130 is approximately 0.10 mm to 0.15 mm. It is understood that the thickness of the metal bracket 130 refers to the maximum thickness of the metal bracket 130 in the thickness direction.
[0104] In one embodiment, the metal stent 130 provided herein is a preformed metal stent 130. The preformed metal stent 130 can be prefabricated into a corresponding shape based on the shape and size of the bone defect, making the metal stent 130 more compatible with the defect and more conducive to fixing the submembranous bone filler. The metal stent 130 also has better support against gingival pressure, which helps protect the submembranous bone filler and promotes new bone formation in the defect area. It is understood that the metal stent 130 can be a conventional prefabricated stent for conventional defect types, or it can be customized based on the patient's specific defect size and shape.
[0105] In one embodiment, the metal bracket 130 is shaped as follows: comprising a metal center bar and a plurality of metal branch bars, wherein the plurality of metal branch bars are distributed on both sides of the metal center bar, and each metal branch bar is connected to the metal center bar respectively.
[0106] In one embodiment, the shape of the metal bracket 130 is: composed of an H-shaped metal support bar in the middle and symmetrical K-shaped metal supports on both sides, wherein the vertical metal supports on both sides of the H-shaped overlap with the two K-shaped vertical metal supports, and the metal bracket 130 has a symmetrical structure.
[0107] In one embodiment, the metal bracket 130 is manufactured by laser cutting or stamping, wherein the laser cutting needs to be protected by an inert gas to avoid burns.
[0108] It is understandable that the ends of the metal branches in the metal bracket 130 may be semi-circular to avoid sharp angles.
[0109] The inventors also discovered that when faced with special alveolar bone defect sizes and shapes, traditional barrier membranes with prefabricated stents need to be trimmed before use. Trimming the titanium stent inevitably results in sharp metal edges, which can cause the metal stent to penetrate the gingival soft tissue, leading to gingival recession and membrane exposure, thus affecting the osteogenesis effect. Based on this, in one embodiment, the metal stent 130 is a personalized stent. The method for making the personalized stent includes the following steps: three-dimensionally scanning the patient's oral and mandibular conditions to model the defect and confirm the defect size and shape. Based on the patient's special defect size and shape, finite element analysis is used to analyze the force distribution of the defect site and design a special personalized metal stent. The special personalized metal stent is then made using 3D printing technology. When the final product is used, trimming of the titanium stent is avoided, reducing the probability of membrane exposure due to sharp edges. Membrane pin fixing holes can also be set on the metal stent 130 to optimize membrane pin fixation during surgery.
[0110] In one embodiment, as shown in Figures 4 to 7 , the surface of the first film layer 110 facing away from the metal stent 130 has groove-shaped stripes 111. The stripes 111 facilitate adhesion between the metal-reinforced polytetrafluoroethylene film 10 and soft tissue, further overcoming the problem of poor adhesion between the film and soft tissue, which can lead to soft tissue cracking and membrane exposure, while also preventing excessive adhesion to the soft tissue and preventing inconvenient removal.
[0111] In one embodiment, there are multiple stripes 111 arranged in parallel.
[0112] In one embodiment, each stripe 111 includes a plurality of first stripes 111a arranged along a first direction and a plurality of second stripes 111b arranged along a second direction;
[0113] The first direction and the second direction are perpendicular to each other.
[0114] In one embodiment, in each stripe 111 , the first stripes 111 a and the second stripes 111 b are arranged alternately.
[0115] In one embodiment, the length of each first stripe 111a is greater than the length of each second stripe 111b, and the width of each first stripe 111a is the same as the width of each second stripe 111b. Multiple first stripes 111a are arranged in a straight line, and multiple second stripes 111b are arranged in parallel. The depth of each first stripe 111a and each second stripe 111b decreases independently from the center toward the ends. These stripes 111 enable the first film layer 110 to better adhere to soft tissue fibers.
[0116] In one embodiment, the depth of each first stripe 111 a and the depth of each second stripe 111 b are independently approximately 0 mm to 0.15 mm.
[0117] It is understood that the metal-reinforced polytetrafluoroethylene membrane 10 can be cut into various shapes as needed, such as, but not limited to, rectangular, square, semicircular, circular, or racetrack shapes. In one embodiment, the metal-reinforced polytetrafluoroethylene membrane 10 is rectangular, with a length of 15 mm to 50 mm and a width of 15 mm to 40 mm. It is understood that to avoid sharp corners in the rectangular or square shape of the metal-reinforced polytetrafluoroethylene membrane 10, the corners may be chamfered, with a chamfer radius of, for example, but not limited to, approximately 2 mm to 6 mm.
[0118] An embodiment of the present application further provides a method for manufacturing the metal-reinforced polytetrafluoroethylene membrane 10 as in any of the above embodiments, comprising the following steps S1 to S5.
[0119] FIG8 shows a process flow chart of a method for manufacturing a metal reinforced polytetrafluoroethylene membrane 10 provided in one embodiment of the present application. It should be understood that although the steps in the flow chart shown in FIG8 are displayed in sequence as indicated by the arrows, these steps are not necessarily performed in the order indicated by the arrows. Unless otherwise specified in the present application, there is no strict order restriction for the execution of these steps, and they can be performed in other orders. Moreover, at least a portion of the steps in FIG8 may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily performed at the same time, but can be performed at different times. The order of execution is not necessarily sequential, but can be performed in turn or alternately with other steps or at least a portion of other sub-steps or stages.
[0120] Step S1: providing a mold 20 , wherein the mold 20 includes a mold base 210 and a mold cover 220 .
[0121] Step S2: The first film 30, the metal bracket 130 and the second film 40 are stacked in sequence on the mold base plate 210, and the metal bracket 130 does not extend beyond the outer edges of the first film 30 and the second film 40; the materials of the first film 30 and the second film 40 are independently selected from micro-stretched expanded polytetrafluoroethylene with a stretching range of 20% to 100%, and the micro-stretched expanded polytetrafluoroethylene has a microporous structure.
[0122] Step S3 : Covering the mold cover plate 220 on the second film 30 .
[0123] Step S4 : hot pressing the mold 20 including the first film 30 , the metal bracket 130 and the second film 40 .
[0124] Step S5: After the hot pressing is completed, the mold 20 is removed after the temperature is lowered; the formed metal reinforced polytetrafluoroethylene membrane 10 has micropores with an overall average pore size of about 0.03 μm to 0.50 μm.
[0125] It can be understood that in the above embodiment, the first film 30 and the second film 40 are respectively the aforementioned micro-stretched expanded polytetrafluoroethylene for forming the first film layer 110 and the micro-stretched expanded polytetrafluoroethylene for forming the second film layer 120. After the above method is used for production, the first film 30 and the second film 40 are hot-pressed to form the first film layer 110 and the second film layer 120 respectively.
[0126] In one embodiment, the stretching amplitude of the second film 40 is smaller than the stretching amplitude of the first film 30 .
[0127] In one embodiment, the average pore size of the micropores in the second film 40 is smaller than the average pore size of the micropores in the first film 30 .
[0128] In one embodiment, the thickness of the first film 30 is about 0.10 mm to 0.40 mm. It is understood that the thickness of the first film 30 can be, for example, but not limited to, 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.20 mm, 0.21 mm, 0.22 mm, 0.23 mm, 0.24 mm, 0.25 mm, 0.26 mm, 0.27 mm, 0.28 mm, 0.29 mm, 0.30 mm, 0.31 mm, 0.32 mm, 0.33 mm, 0.34 mm, 0.35 mm, 0.36 mm, 0.37 mm, 0.38 mm, 0.39 mm, 0.40 mm, etc. In one embodiment, the thickness of the first film 30 is about 0.15 mm to 0.25 mm. In one embodiment, the thickness of the first film 30 is about 0.20 mm to 0.22 mm.
[0129] In one embodiment, the pores of the first film 30 have a pore size ranging from about 0.05 μm to about 5.0 μm.
[0130] In one embodiment, the average pore size of the micropores of the first film 30 is approximately 0.2 μm to 1.0 μm. The first film 30, comprised of a slightly stretched expanded polytetrafluoroethylene material, has a microporous structure that facilitates adhesion between the film and soft tissue. It is understood that the average pore size of the micropores of the first film 30 can be, but is not limited to, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, and the like.
[0131] In one embodiment, the thickness of the second film 40 is approximately 0.05 mm to 0.3 mm. It is understood that the thickness of the second film 40 may be, for example, but not limited to, 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.10 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.20 mm, 0.21 mm, 0.22 mm, 0.23 mm, 0.24 mm, 0.25 mm, 0.26 mm, 0.27 mm, 0.28 mm, 0.29 mm, 0.30 mm, etc. In one embodiment, the thickness of the second film 40 is approximately 0.05 mm to 0.2 mm. In another embodiment, the thickness of the second film 40 is approximately 0.05 mm to 0.15 mm.
[0132] In one embodiment, the pore size of the micropores of the second film 40 ranges from about 0.01 μm to about 2.50 μm.
[0133] In one embodiment, the pore size of the micropores of the second film 40 ranges from about 0.01 μm to about 2.0 μm.
[0134] In one embodiment, the average pore size of the micropores of the second film 40 is about 0.1μm to 0.5μm. The average pore size of the second film 40 made of micro-stretched expanded polytetrafluoroethylene is smaller than the average pore size of the first film 30, and the overall structure is a small microporous structure, which can completely block the growth of connective tissue or fibrous tissue into the bone formation area, which is conducive to reducing stimuli that may hinder bone formation. It can be understood that the average pore size of the second film 40 can be, for example, but not limited to, 0.1μm, 0.15μm, 0.2μm, 0.25μm, 0.3μm, 0.35μm, 0.4μm, 0.45μm, 0.5μm, etc. In one embodiment, the average pore size of the second film 40 is about 0.1μm to 0.3μm.
[0135] In one embodiment, the step further includes forming stripes 111 on the surface of the first film 30 facing away from the metal support 130 .
[0136] In one embodiment, the step of forming the stripes 111 on the surface of the first film 30 facing away from the metal support 130 includes:
[0137] A stripe template 50 corresponding to the preset stripes 111 is placed between the first film 30 and the mold base 210 .
[0138] In one embodiment, step S2 includes: stacking the stripe template 50, the first film 30, the metal bracket 130 and the second film 40 in sequence on the mold base plate 210, and the metal bracket 130 does not extend beyond the outer edges of the first film 30 and the second film 40; the material of the first film 30 and the second film 40 each independently includes micro-stretched expanded polytetrafluoroethylene with a stretching range of 20% to 100%.
[0139] It can be understood that the stripe template 50 can be, for example but not limited to, a metal mesh.
[0140] In one embodiment, in step S4, the hot pressing step includes:
[0141] The mold 20 including the first film 30 , the metal support 130 and the second film 40 is pressed, heated and kept warm in sequence.
[0142] In one embodiment, the clamping method is locking clamping, and the locking torque is about 0.5N·m to 10N·m. It is understandable that the locking torque can be, for example, but not limited to, 0.5N·m, 1N·m, 1.5N·m, 2N·m, 2.5N·m, 3N·m, 3.5N·m, 4N·m, 4.5N·m, 5N·m, 5.5N·m, 6N·m, 6.5N·m, 7N·m, 7.5N·m, 8N·m, 8.5N·m, 9N·m, 9.5N·m, 10N·m, etc.
[0143] In one embodiment, referring to Figures 9 and 10 , the locking and pressing method is to use a fixing clamp 230 to clamp the mold base plate 210 and the mold cover plate 220 and to lock them by torsion. The fixing clamp 230 can be, for example, but not limited to, a C-shaped clamp.
[0144] In one embodiment, please refer to Figures 11 to 14, the locking and tightening method is to use a fixing screw 240 to fix the mold base plate 210 and the mold cover plate 220, and torsion locking. As shown in Figures 11 and 12, the fixing screw 240 can be, for example, a fixing screw 240 that does not need to be matched with the nut 250. As shown in Figures 13 to 14, the fixing screw 240 can also be a fixing screw 240 that requires a nut to be matched. It can be understood that when the fixing screw 240 is used to fix the mold base plate 210 and the mold cover plate 220, in order to ensure that the mold base plate 210 and the mold cover plate 220 are firmly fixed, the mold base plate 210 and the mold cover plate 220 are correspondingly provided with threaded holes 260.
[0145] By using a fixing clamp 230 to clamp the mold base plate 210 and the mold cover plate 220, or using a fixing screw 240 to fix the mold base plate 210 and the mold cover plate 220 and then torsionally locking the locking and clamping method, it is more convenient to adjust the pressure of the hot pressing, and after adjusting to the appropriate pressure, the mold 20 will be placed in a high temperature environment without causing adverse effects such as deformation. Compared with ordinary hydraulic or other clamping methods, the clamping method provided in this application has better high temperature tolerance and uniformity, and the thickness of the metal reinforced polytetrafluoroethylene film 10 prepared by hot pressing is more uniform.
[0146] In one embodiment, the heating temperature is increased at a rate of about 30°C / min to 60°C / min, and the heating temperature is about 300°C to 380°C. It is understood that the heating temperature can be, but is not limited to, 30°C / min, 35°C / min, 40°C / min, 45°C / min, 50°C / min, 55°C / min, 60°C / min, etc. It is understood that the heating temperature can be, but is not limited to, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, etc.
[0147] In one embodiment, the holding time is about 1 hour to 5 hours. It is understandable that the holding time can be, but is not limited to, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, etc.
[0148] In one embodiment, the cooling rate is about 2°C / h to 10°C / h. It is understood that the cooling rate can be, for example but not limited to, 2°C / h, 3°C / h, 4°C / h, 5°C / h, 6°C / h, 7°C / h, 8°C / h, 9°C / h, 10°C / h, etc.
[0149] An embodiment of the present application further provides a barrier membrane, comprising the metal-reinforced polytetrafluoroethylene membrane 10 as in any of the above embodiments.
[0150] In one embodiment, the barrier membrane further comprises a collagen membrane.
[0151] An embodiment of the present application further provides a use of the barrier membrane in the above embodiment in guided bone regeneration.
[0152] In one embodiment, the first membrane layer 110 of the metal reinforced polytetrafluoroethylene membrane 10 contacts the soft tissue surface, and the second membrane layer 120 contacts the bone graft.
[0153] The metal-reinforced polytetrafluoroethylene membrane 10 provided in this application can be used in oral surgery, craniofacial surgery, and maxillofacial surgery, etc., for treatments involving guided bone regeneration, for example, for the treatment of periodontal tissue defects. As a barrier membrane in guided bone regeneration, the metal-reinforced polytetrafluoroethylene membrane 10 can be used to create a stable space for bone regeneration, prevent connective tissue fibers from growing into bone tissue, stabilize the bone, eliminate stimuli that may hinder bone formation, and / or serve other purposes of fixing and maintaining space. The metal-reinforced polytetrafluoroethylene membrane 10 has the following main advantages:
[0154] (1) The materials of the first membrane layer 110 and the second membrane layer 120 are independently selected from micro-stretched expanded polytetrafluoroethylene. Micro-stretched expanded polytetrafluoroethylene has a microporous structure. The average pore size of the micropores formed on the metal reinforced polytetrafluoroethylene membrane 10 is about 0.03μm to 0.50μm. The pore size is appropriate, which is conducive to the diffusion of nutrients and promotes effective bone reconstruction in the submembrane osteogenic area. When used in guided bone regeneration surgery, the metal reinforced polytetrafluoroethylene membrane 10 has good adhesion to soft tissue and is easy to separate.
[0155] (2) The microporous structure of the first membrane layer 110 facilitates contact with soft tissue, allowing the gum soft tissue to fit within the first membrane layer 110. Furthermore, during secondary surgical removal, blunt separation is relatively easy without damaging the soft tissue. The average pore size of the second membrane layer 120 is smaller than that of the first membrane layer 110, which helps prevent connective tissue fibers from growing into bone tissue. This avoids the problem of excessive soft tissue ingrown into the expanded polytetrafluoroethylene membrane due to excessive pore size, making removal difficult and damaging the soft tissue. Furthermore, it eliminates stimuli that may hinder bone formation and promotes new bone formation.
[0156] (3) The metal stent 130 is plastic and can be molded into a corresponding shape according to the shape and size of the bone defect. In practical applications, it can be divided into conventional prefabricated stents and personalized stents. Conventional prefabricated stents are used for conventional defect types. Personalized stents are made according to the patient's special defect size and shape through 3D printing and finite element analysis technology. When the metal stent 130 is in use, there is no need to trim the metal stent 130 additionally, reducing the probability of membrane exposure caused by sharp edges. In addition, membrane nail fixing holes can be set on the metal stent 130 to optimize membrane nail fixation during surgery.
[0157] (4) The surface of the first film layer 110 facing away from the metal bracket 130 has groove-shaped stripes 111. When used in guided bone regeneration surgery, the first film layer 110 contacts the soft tissue. The groove-shaped stripes 111 can make the soft tissue fit more closely in the first film layer 110, avoiding the problem of soft tissue cracking and exposure caused by the poor adhesion of the dense polytetrafluoroethylene film to the soft tissue due to its almost non-porous and smooth surface.
[0158] The following are specific examples.
[0159] Example 1
[0160] A metal reinforced polytetrafluoroethylene membrane 10:
[0161] 1 to 7 , the metal reinforced polytetrafluoroethylene membrane 10 includes a first membrane layer 110 , a second membrane layer 120 and a metal bracket 130 . The metal bracket 130 is located between the first membrane layer 110 and the second membrane layer 120 and is enclosed by the first membrane layer 110 and the second membrane layer 120 .
[0162] Regarding the first film layer 110:
[0163] The first film layer 110 is made of slightly stretched expanded polytetrafluoroethylene with a stretching range of 80% and a microporous structure.
[0164] The surface of the first film layer 110 facing away from the metal support 130 includes a plurality of parallel groove-shaped stripes 111 .
[0165] Each stripe 111 includes a plurality of first stripes 111a arranged along a first direction and a plurality of second stripes 111b arranged along a second direction. The first direction and the second direction are perpendicular to each other. In each stripe, the first stripes 111a and the second stripes 111b are alternately arranged.
[0166] Each first stripe 111a is deepest in the middle, with a depth of 0.1 mm, and gradually becomes shallower toward both ends to a depth of 0 mm. Each first stripe 111a has a width of 0.1 mm and a length of 0.5 mm.
[0167] Each second stripe 111b is deepest in the middle, with a depth of 0.1 mm, and gradually becomes shallower toward both ends to a depth of 0 mm. Each second stripe 111b has a width of 0.1 mm and a length of 0.3 mm.
[0168] The distance between each two adjacent first stripes 111a is 0.4 mm, and the distance between each two adjacent second stripes 111b is 0.6 mm.
[0169] Regarding the second film layer 120:
[0170] The second film layer 120 is made of slightly stretched expanded polytetrafluoroethylene with a stretching range of 30% and a microporous structure.
[0171] About Metal Bracket 130:
[0172] The metal stent 130 is made of TA1 medical pure titanium prefabricated stent with a thickness of 0.15 mm and a surface roughness of less than 0.08 μm.
[0173] The metal bracket 130 includes a metal center bar and a plurality of metal branch bars. The plurality of metal branch bars are symmetrically distributed on both sides of the metal center bar, and each metal branch bar is connected to the metal center bar respectively.
[0174] The metal bracket 130 is manufactured by laser cutting or stamping. Laser cutting requires protection with inert gas to avoid burns. The end of the metal bracket is semi-circular to avoid sharp angles.
[0175] About the metal reinforced polytetrafluoroethylene membrane 10 overall:
[0176] The pore size ranges from 0.01 μm to 1.00 μm, with an average pore size of 0.15 μm. The total thickness of the film region not covered with the metal bracket 130 is approximately 0.25 mm, and the total thickness of the film region covered with the metal bracket 130 is approximately 0.40 mm.
[0177] The first film layer 110 , the metal bracket 130 and the second film layer 120 are bonded together by heat pressing without any other additives.
[0178] The metal reinforced polytetrafluoroethylene membrane 10 is formed in a rectangular shape.
[0179] The method for manufacturing the metal reinforced polytetrafluoroethylene membrane 10 comprises the following steps:
[0180] (1) Two pieces of slightly stretched expanded polytetrafluoroethylene membranes with stretching amplitudes of 80% and 30% were cut into 5 cm × 6 cm films as the first film 30 and the second film 40, respectively. They were ultrasonically cleaned three times each using purified water, alcohol, and injection water as cleaning agents, and then dried in a 60°C oven for 3 hours. The TA1 medical pure titanium prefabricated stent used as the metal stent was cleaned using the same method; the pore size range of the first film 30 was 0.2 μm to 1.0 μm, the average pore size was about 0.5 μm, and the thickness was about 0.22 mm. The pore size range of the second film 40 was 0.2 μm to 1.2 μm, the average pore size was 0.25 μm, and the thickness was 0.1 mm;
[0181] (2) Referring again to FIG. 9 and FIG. 10 , a mold 20 for hot pressing is provided. The mold 20 includes a mold base 210 and a mold cover 220. A metal mesh, a first film 30, a metal bracket 130, and a second film 40 corresponding to the preset stripes 111 are sequentially stacked on the mold base 210. The metal bracket 130 does not extend beyond the outer edges of the first film 30 and the second film 40. The mold cover 220 is covered on the second film 40. Fixing clamps 230 are used around the mold 20 to clamp the mold base 210 and the mold cover 220. A torque wrench is used to fix the clamping torque to 2.5 Nm.
[0182] (3) Place the assembled mold 20 in a high-temperature oven and set the temperature control program. First, set the program to heat up at a rate of 50°C / min until the temperature reaches 360°C and maintain the temperature for 2 hours. Then set the program to cool down at a rate of 5°C / h until the temperature reaches 100°C. Take out the mold 20 and cool it to room temperature. Then, open the mold and take out the semi-finished product.
[0183] (4) Cut the semi-finished product after hot pressing into products, and ensure that the TA1 medical pure titanium prefabricated stent is centered through visual positioning or mold positioning, and the position deviation is controlled within ±0.5mm;
[0184] (5) The cut products are ultrasonically cleaned three times using purified water, alcohol, and injection water, placed in a 60°C oven for drying for 3 hours, and then inner and outer packaging, sterilized, and made into finished products.
[0185] Example 2
[0186] A metal reinforced polytetrafluoroethylene membrane 10:
[0187] 1 to 7 , the metal reinforced polytetrafluoroethylene membrane 10 includes a first membrane layer 110 , a second membrane layer 120 and a metal bracket 130 . The metal bracket 130 is located between the first membrane layer 110 and the second membrane layer 120 and is enclosed by the first membrane layer 110 and the second membrane layer 120 .
[0188] Regarding the first film layer 110:
[0189] The first film layer 110 is made of slightly stretched expanded polytetrafluoroethylene with a stretching range of 100% and a microporous structure.
[0190] The surface of the first film layer 110 facing away from the metal support 130 includes a plurality of parallel groove-shaped stripes 111 .
[0191] Each stripe 111 includes a plurality of first stripes 111a arranged along a first direction and a plurality of second stripes 111b arranged along a second direction. The first direction and the second direction are perpendicular to each other. In each stripe, the first stripes 111a and the second stripes 111b are alternately arranged.
[0192] Each first stripe 111a is deepest in the middle, with a depth of 0.05 mm, and gradually becomes shallower toward both ends to a depth of 0 mm. Each first stripe 111a has a width of 0.05 mm and a length of 0.25 mm.
[0193] Each second stripe 111b is deepest in the middle, with a depth of 0.05mm, and gradually becomes shallower to a depth of 0mm toward both ends. Each second stripe 111b has a width of 0.05mm and a length of 0.15mm.
[0194] The distance between each two adjacent first stripes 111a is 0.3 mm. The distance between each two adjacent second stripes 111b is 0.3 mm.
[0195] Regarding the second film layer 120:
[0196] The second film layer 120 is made of slightly stretched expanded polytetrafluoroethylene with a stretching range of 30% and a microporous structure.
[0197] About Metal Bracket 130:
[0198] The metal bracket 130 is made of a TC4 titanium alloy prefabricated bracket with a thickness of 0.10 mm and a surface roughness of less than 0.05 μm.
[0199] The metal bracket 130 is shaped like an H-shaped metal support bar in the middle and symmetrical K-shaped metal support bars on both sides. The vertical metal support bars on both sides of the H-shaped support bar overlap with the two vertical metal support bars of the K-shaped support bar, and the metal bracket 130 has a symmetrical structure.
[0200] The metal bracket 130 is manufactured by laser cutting or stamping. Laser cutting requires protection with inert gas to avoid burns. The end of the metal bracket is semi-circular to avoid sharp angles.
[0201] About the metal reinforced polytetrafluoroethylene membrane 10 overall:
[0202] The pore size ranges from 0.01 μm to 0.8 μm, with an average pore size of 0.2 μm. The total thickness of the film region not covered with the metal bracket 130 is approximately 0.2 mm, and the total thickness of the film region covered with the metal bracket 130 is approximately 0.40 mm.
[0203] The first film layer 110 , the metal bracket 130 and the second film layer 120 are bonded together by heat pressing without any other additives.
[0204] The metal reinforced polytetrafluoroethylene membrane 10 is formed in a rectangular shape.
[0205] The method for manufacturing the metal reinforced polytetrafluoroethylene membrane 10 comprises the following steps:
[0206] (1) Two pieces of slightly stretched expanded polytetrafluoroethylene membranes with stretching amplitudes of 100% and 30% were cut into 4 cm × 5 cm films as the first film 30 and the second film 40, respectively. They were ultrasonically cleaned three times each using purified water, alcohol, and injection water as cleaning agents, and then dried in a 60°C oven for 3 hours. The TC4 titanium alloy prefabricated stent used as the metal stent was cleaned using the same method. The pore size of the first film 30 ranged from approximately 0.5 μm to 5.0 μm, the average pore size was approximately 1.0 μm, and the thickness was approximately 0.20 mm. The pore size of the second film 40 ranged from 0.03 μm to 1.0 μm, the average pore size was 0.30 μm, and the thickness was 0.15 mm.
[0207] (2) Referring again to FIG. 11 and FIG. 12 , a mold 20 for hot pressing is provided. The mold 20 includes a mold base 210 and a mold cover 220. A metal mesh, a first film 30, a metal bracket 130, and a second film 40 corresponding to the preset stripes 111 are sequentially stacked on the mold base 210. The metal bracket 130 does not extend beyond the outer edges of the first film 30 and the second film 40. The mold cover 220 is covered on the second film 40. Fixing screws 240 are used in threaded holes 260 provided in the mold to lock the mold base 210 and the mold cover 220. A torque wrench is used to fix the screws, and the torque is set to 5 N.m.
[0208] (3) Place the assembled mold 20 in a high-temperature oven and set the temperature control program. First, set the program to heat up at a rate of 60°C / min until the temperature reaches 380°C, maintain heating for 1 hour, then set the program to cool down at a rate of 10°C / h until the temperature reaches 80°C. Take out the mold 20 and cool it to room temperature. Open the mold and take out the semi-finished product.
[0209] (4) Cut the semi-finished product after hot pressing into products, and ensure that the TA4 titanium alloy bracket is centered through visual positioning or mold positioning, and the position deviation is controlled within ±0.5mm;
[0210] (5) The cut products are ultrasonically cleaned three times using purified water, alcohol, and injection water, placed in a 60°C oven for drying for 3 hours, and then inner and outer packaging, sterilized, and made into finished products.
[0211] Example 3
[0212] Example 3 is substantially the same as Example 2, with the difference being that the metal bracket 130 is made of a high-nitrogen stainless steel prefabricated bracket.
[0213] Example 4
[0214] Example 4 is substantially the same as Example 2, except that: 1. the overall pore size and specifications of the metal-reinforced polytetrafluoroethylene membrane 10 are different; 2. the manufacturing method of the metal-reinforced polytetrafluoroethylene membrane is different.
[0215] 1. The overall pore size of the metal reinforced polytetrafluoroethylene membrane 10 ranges from 0.05 μm to 0.8 μm, with an average pore size of 0.5 μm. The total thickness of the membrane area not covered with the metal bracket 130 is approximately 0.12 mm, and the total thickness of the membrane area covered with the metal bracket 130 is approximately 0.30 mm.
[0216] 2. The method for manufacturing the metal reinforced polytetrafluoroethylene membrane 10 comprises the following steps:
[0217] (1) Two pieces of slightly stretched expanded polytetrafluoroethylene membranes with stretching amplitudes of 100% and 50% were cut into 5 cm × 6 cm films as the first film 30 and the second film 40, respectively. They were ultrasonically cleaned three times each using purified water, alcohol, and injection water as cleaning agents, and then dried in a 60°C oven for 3 hours. The TC4 titanium alloy prefabricated stent used as the metal stent was cleaned using the same method. The pore size range of the first film 30 was approximately 0.05 μm to 5.0 μm, the average pore size was approximately 0.2 μm, and the thickness was approximately 0.10 mm. The pore size range of the second film 40 was 0.01 μm to 2.0 μm, the average pore size was 0.1 μm, and the thickness was 0.05 mm.
[0218] (2) Referring again to FIG. 13 and FIG. 14 , a mold 20 for hot pressing is provided. The mold 20 includes a mold base 210 and a mold cover 220. A metal mesh, a first film 30, a metal bracket 130, and a second film 40 corresponding to the preset stripes 111 are sequentially stacked on the mold base 210. The metal bracket 130 does not extend beyond the outer edges of the first film 30 and the second film 40. The mold cover 220 is covered on the second film 40. A fixing screw 240 is used in conjunction with a nut 250 in a threaded hole 260 provided in the mold 20 to lock the mold base 210 and the mold cover 220. A torque wrench is used to fix the screws, and the torque is set to 10 N.m.
[0219] (3) Place the assembled mold 20 in a high-temperature oven and set the temperature control program. First, set the program to heat up at a rate of 60°C / min until the temperature reaches 350°C and maintain the temperature for 3 hours. Then set the program to cool down at a rate of 6°C / h until the temperature reaches 120°C. Take out the mold 20 and cool it to room temperature. Open the mold and take out the semi-finished product.
[0220] (4) Cut the semi-finished product after hot pressing into products, and ensure that the TC4 titanium alloy prefabricated bracket is centered through visual positioning or mold positioning, and the position deviation is controlled within ±0.5mm;
[0221] (5) The cut products are ultrasonically cleaned three times using purified water, alcohol, and injection water, placed in a 50°C oven for drying for 4 hours, and then inner and outer packaging, sterilized, and made into finished products.
[0222] Example 5
[0223] Example 5 is similar to Example 2, except that the metal bracket 130 is customized. The specific preparation method of the metal bracket 130 is as follows:
[0224] (1) Obtaining a model of the patient's alveolar bone defect by performing a CT scan on the patient, and then designing a titanium stent model that matches the defect model. The titanium stent model includes the design of the membrane pin fixation point and the shape of the main bearing area;
[0225] (2) Perform finite element analysis on the titanium stent, import finite element analysis software, determine the fixed points, set the load conditions, perform mechanical analysis and solve, determine the distribution of the load-bearing capacity of the personalized titanium stent, thicken the main load-bearing area, perform transition processing between different thicknesses, and finally obtain a better titanium stent design model;
[0226] (3) Through additive manufacturing technology, personalized titanium stents are prepared, and annealing and surface treatment are performed to obtain the final titanium stent.
[0227] Example 6
[0228] Example 6 is substantially the same as Example 2, except that: 1. the overall pore size and specifications of the metal-reinforced polytetrafluoroethylene membrane are different; 2. the manufacturing method of the metal-reinforced polytetrafluoroethylene membrane is different.
[0229] 1. The overall pore size of the metal reinforced polytetrafluoroethylene membrane 10 ranges from 0.01 μm to 0.1 μm, with an average pore size of 0.03 μm. The total thickness of the membrane area not covered with the metal bracket 130 is approximately 0.12 mm, and the total thickness of the membrane area covered with the metal bracket 130 is approximately 0.30 mm.
[0230] 2. The method for manufacturing the metal reinforced polytetrafluoroethylene membrane 10 comprises the following steps:
[0231] (1) Two pieces of slightly stretched expanded polytetrafluoroethylene membranes with stretching amplitudes of 50% and 20% were cut into 5 cm × 6 cm films as the first film 30 and the second film 40, respectively. They were ultrasonically cleaned three times each using purified water, alcohol, and injection water as cleaning agents, and then dried in a 60°C oven for 3 hours. The TC4 titanium alloy prefabricated stent used as the metal stent was cleaned using the same method. The pore size of the first film 30 ranged from approximately 0.01 μm to 2.0 μm, the average pore size was approximately 0.1 μm, and the thickness was approximately 0.10 mm. The pore size of the second film 40 ranged from 0.01 μm to 1.0 μm, the average pore size was 0.05 μm, and the thickness was 0.05 mm.
[0232] (2) Referring again to FIG. 13 and FIG. 14 , a mold 20 for hot pressing is provided. The mold 20 includes a mold base 210 and a mold cover 220. A metal mesh, a first film 30, a metal bracket 130, and a second film 40 corresponding to the preset stripes 111 are sequentially stacked on the mold base 210. The metal bracket 130 does not extend beyond the outer edges of the first film 30 and the second film 40. The mold cover 220 is covered on the second film 40. A fixing screw 240 is used in conjunction with a nut 250 in a threaded hole 260 provided in the mold 20 to lock the mold base 210 and the mold cover 220. A torque wrench is used to fix the screws, and the torque is set to 10 N.m.
[0233] (3) Place the assembled mold 20 in a high-temperature oven and set the temperature control program. First, set the program to heat up at a rate of 30°C / min until the temperature reaches 300°C and maintain the temperature for 3 hours. Then set the program to cool down at a rate of 6°C / h until the temperature reaches 120°C. Take out the mold 20 and cool it to room temperature. Then, open the mold and take out the semi-finished product.
[0234] (4) Cut the semi-finished product after hot pressing into products, and ensure that the TC4 titanium alloy prefabricated bracket is centered through visual positioning or mold positioning, and the position deviation is controlled within ±0.5mm;
[0235] (5) The cut products are ultrasonically cleaned three times using purified water, alcohol, and injection water, placed in a 50°C oven for drying for 4 hours, and then inner and outer packaging, sterilized, and made into finished products.
[0236] Comparative Example 1
[0237] Comparative Example 1 is a commercially available titanium-reinforced macroporous expanded polytetrafluoroethylene membrane, the average pore diameter of which reaches 30 μm, and the stretching amplitude of the expanded polytetrafluoroethylene is greater than 200%.
[0238] Comparative Example 2
[0239] Comparative Example 2 is a commercially available titanium-reinforced dense polytetrafluoroethylene membrane, which has almost no micropores and a smooth surface.
[0240] Test Example 1
[0241] The adhesion of the metal reinforced polytetrafluoroethylene membranes prepared in Examples 1 to 6, the commercially available titanium reinforced macroporous expanded polytetrafluoroethylene membrane in Comparative Example 1, and the commercially available titanium reinforced dense polytetrafluoroethylene membrane in Comparative Example 2 to the wound surface was compared.
[0242] The adhesion between eight membranes and the wound surface was evaluated using the standard YY / T 1477.4-2017 in vitro model. The specific test methods are as follows:
[0243] (1) Remove the metal brackets from the eight metal-reinforced polytetrafluoroethylene membranes and cut them into 30 mm × 40 mm test pieces, two for each test. Place the wound model (fibrin clot) between the two test pieces, with the wound model in contact with the soft tissue contact surface of the product. Place the membrane on a horizontal tray, apply a 98 g pressure block, and transfer to a constant temperature and humidity chamber at (37 ± 2) ° C and a relative humidity of 85% for 24 h.
[0244] (2) Take out the above sample, place it in a drying oven at (37±2)℃ and dry it for 3h~4h, take it out and let it cool to room temperature;
[0245] (3) The above samples were subjected to a peel test in a 90° handheld manner according to Figure A.2b) of standard YY / T 1477.4. The initial distance between the clamps was about 40 mm. The samples were stretched at a tensile rate of 100 mm / min until they were completely peeled off from the wound model. The potential soft tissue adhesion of the samples was evaluated and the maximum peeling force required for peeling was recorded.
[0246] (4) Repeat the above experimental steps 6 times.
[0247] The test results are shown in Table 1 and Figure 15.
[0248] Table 1 Maximum peel force test results
[0249] As can be seen from Table 1 and Figure 15, the maximum peeling forces of Examples 1 to 6 are (1.12±0.23) N / 30 mm, (1.39±0.22) N / 30 mm, (1.60±0.19) N / 30 mm, (1.17±0.18) N / 30 mm, (1.37±0.21) N / 30 mm, and (1.07±0.15) N / 30 mm, respectively. The maximum peeling forces are appropriate, indicating that the metal-reinforced polytetrafluoroethylene films prepared in Examples 1 to 6 can contact the wound model, have certain adhesion, and are relatively easy to peel off.
[0250] The maximum peeling force of Comparative Example 1 is (2.74±0.22) N / 30 mm, which is too large. This indicates that although the commercially available titanium-reinforced macroporous expanded polytetrafluoroethylene membrane in Comparative Example 1 can contact the wound model, the adhesion force is large and peeling is difficult.
[0251] The maximum peeling force of Comparative Example 2 was (0.14±0.04) N / 30 mm, which was extremely small. In addition, separation occurred during the test without natural peeling, indicating that the commercially available titanium-reinforced dense polytetrafluoroethylene membrane in Comparative Example 2 was not in firm contact with the wound model.
[0252] The peeling force of Comparative Example 1 is significantly greater than that of Examples 1 to 6, indicating that the adhesion of Comparative Example 1 is stronger than that of Examples 1 to 6. During use, Comparative Example 1 may have the risk of adhesion to soft tissue; while the peeling force of Comparative Example 2 is too small, and the combination with the wound model is not firm, and natural peeling may occur. During use, Comparative Example 2 may have the risk of exposure due to the incompatibility between the metal-reinforced polytetrafluoroethylene film and the soft tissue; in comparison, Examples 1 to 6 have an appropriate maximum peeling force, are easier to peel, and can stabilize the wound model, which can avoid the risk of adhesion to soft tissue and is not easy to be exposed.
[0253] Test Example 2:
[0254] A rabbit skull defect model was established to compare the osteogenesis effects of the metal-reinforced polytetrafluoroethylene membrane prepared in Example 2, the commercially available titanium-reinforced macroporous expanded polytetrafluoroethylene membrane in Comparative Example 1, and the commercially available titanium-reinforced dense polytetrafluoroethylene membrane in Comparative Example 2. The specific method is as follows:
[0255] Twelve 3 kg New Zealand rabbits were selected and divided into two groups: 4-week observation group I and 12-week observation group II. Two 8 mm defect models were made for each rabbit, for a total of 12 models in each group. Each group was randomly assigned 4 of each of the three metal-reinforced polytetrafluoroethylene film products of Example 2, Comparative Example 1, and Comparative Example 3.
[0256] (1) The animals were fasted but not watered for 12 h one day before surgery. On the day of the experiment, the animals were weighed and anesthetized with an intramuscular injection of 0.15-0.2 ml / kg of Zotalitol to induce anesthesia.
[0257] (2) Shaving: Shave the hair on the rabbit's head.
[0258] (3) Disinfection: Place the animal in lateral position, disinfect the head and face with 2% iodine tincture, and cover with a sterile sheet.
[0259] (4) Local anesthesia: 2% lidocaine hydrochloride (1:100,000 epinephrine) was used for local infiltration anesthesia in the surgical area to reduce bleeding during the operation.
[0260] (5) Modeling: A 3.0-4.0 cm incision was made along the middle of the skull. The scalp and subcutaneous tissue were carefully pulled apart to facilitate drilling with a grinder and a contra-angle drill. A 7 mm diameter hollow drill bit was used to drill holes, creating an 8 mm defect on each side of the rabbit skull. During the drilling process, a large amount of saline was used to cool the skull, and care was taken to avoid damaging the dura mater. After the modeling was completed, the skull at the modeling site was removed.
[0261] (6) Placement of materials: Use sterile instruments to clamp the barrier membrane product with a diameter of 12 mm, carefully apply medical glue 1-2 mm around the periphery of the membrane, and be careful not to apply it in the central area, and then cover the product on the rabbit skull defect.
[0262] (7) Suture: Use interrupted suture to completely close the wound.
[0263] (8) Record abnormal conditions and solutions during the operation.
[0264] (9) Postoperatively: intramuscular injection of penicillin (400,000 U / d) and tolfenamic acid for anti-inflammatory and analgesic purposes.
[0265] (10) After surgery, the animal was kept warm and its vital signs were monitored until it fully regained consciousness.
[0266] (11) Anti-infection and analgesia. Anti-infection: intramuscular injection of penicillin (400,000 U / d), once a day for 3 consecutive days; analgesia: tolfenamic acid sodium 0.1 ml / kg, once a day for 3 consecutive days.
[0267] (12) At 4 and 12 weeks after surgery, the animals in groups I and II were killed, and the whole skull specimens were removed and fixed in 4% neutral formalin / 1% calcium chloride solution. Three-dimensional CT was performed to analyze the new bone volume (NBV) (mm) in the defect area. 3 ), followed by H&E staining for histological observation and histomorphometric analysis of the new bone percentage (NBA%). P < 0.05 indicated a significant difference, indicated by *, and p < 0.001 indicated an extremely significant difference between the groups, indicated by ***.
[0268] The test results are shown in Table 2, Table 3, Figure 16 and Figure 17.
[0269] Table 2 Analysis results of new bone volume in defect area
[0270] Table 3 Analysis results of the proportion of new bone area in the defect area
[0271] From the H&E staining histological observation in Figure 16, it was found that the submembranous bone formation volume of the three groups of products 12 weeks after implantation was greater than the bone formation volume at 4 weeks; at 4 weeks, in Example 2, a small amount of soft tissue was attached to the first membrane layer of Example 2, and a certain amount of new bone filled the defect; in Comparative Example 1, more soft tissue was attached to the membrane, a certain amount of soft tissue cells penetrated the membrane, a certain amount of new bone was generated under the membrane, and the defect was filled; in Comparative Example 2, the soft tissue was basically not attached to the membrane, and some new bone was generated under the membrane, which did not fill the defect. At the 12th week, in Example 2, more soft tissue was attached to the first membrane layer of Example 2, a small amount was embedded in the interior of the membrane, and the new bone under the membrane was plump; in Comparative Example 1, more soft tissue was attached to the membrane, a large number of soft tissue cells penetrated the membrane, a certain amount of new bone was generated under the membrane, the defect was filled, there was a layer of soft tissue between the membrane and the bone, the new bone under the membrane filled the defect site, and the bone wall was thicker; in Comparative Example 2, the soft tissue was basically not attached to the membrane, some new bone was generated under the membrane, filling the defect position, but the new bone wall was thin.
[0272] Table 3, Table 4 and Figure 17 show the new bone volume and new bone area ratio. At 4 weeks, the new bone volume and new bone area ratio of Example 2 and Comparative Example 1 were significantly greater than those of Comparative Example 2, and Example 2 was significantly greater than that of Comparative Example 1. At 12 weeks, the overall trend of the new bone volume and new bone area ratio was the same as that at 4 weeks, among which the new bone volume and new bone area ratio of Example 2 12 weeks after surgery were significantly greater than those at 4 weeks after surgery, and the bone mass growth was most obvious.
[0273] Based on the above analysis, it can be seen that the metal-reinforced polytetrafluoroethylene barrier membrane provided in Example 2 has a better osteogenesis effect than the existing commercially available titanium-reinforced macroporous expanded polytetrafluoroethylene membrane and the commercially available titanium-reinforced dense polytetrafluoroethylene membrane.
[0274] Test Example 3
[0275] A beagle dog mandibular defect model was established to compare the differences in osteogenesis, soft tissue adhesion and exposure between the metal reinforced polytetrafluoroethylene membrane prepared in Example 4, the commercially available titanium reinforced macroporous expanded polytetrafluoroethylene membrane in Comparative Example 1, and the commercially available titanium reinforced dense polytetrafluoroethylene membrane in Comparative Example 2.
[0276] Design: Six male beagle dogs, aged 9-12 months and weighing 10-12 kg, were selected. Mandibular P1-P4 was extracted and the wounds were closed and healed for 2 months. A saddle-shaped defect measuring 8 mm (mesiodistal) × 5 mm (croon-root) × (5-7) mm (buccally and lingually) was created. Each dog had two sites on each side of the mandible. The dogs were divided into four groups: Example 4, Comparative Example 1, Comparative Example 2, and a blank group. Bone powder was then implanted. Three groups were fixed with the three membranes described above, while the blank group was not fixed with a membrane. CT scans were performed immediately, 13 weeks, and 26 weeks after surgery to assess bone formation height (H). The bone formation rate (26-week bone formation height H / immediate bone formation height H after surgery × 100%) was used to assess product exposure. After CT testing at 26 weeks, the mucosa was opened and the material was removed. The adhesion of the membrane to soft tissue was evaluated using the Rydell score.
[0277] The specific method is as follows:
[0278] I. One-stage surgical procedure (extraction socket formation)
[0279] (1) Disinfection: Use 2% iodine tincture to disinfect the oral cavity and face, and lay a sterile sheet.
[0280] (2) Local anesthesia: 2% lidocaine hydrochloride (1:100000 epinephrine) was used for local infiltration anesthesia in the surgical area to reduce bleeding during the operation.
[0281] (3) Gingival incision: Use a bone stripper to peel off the gums, turn over the mucoperiosteal flap, and use a spacer to increase the gap between the tooth root and the alveolar bone, and loosen the tooth root.
[0282] (4) Crown division: Use a tungsten carbide split drill to divide the first, second, third, and fourth premolars (P1-P4) on the left and right sides of the mandible into two mesiodistal halves at the root bifurcation.
[0283] (5) Tooth extraction: Extract the tooth and scrape the extraction socket to create a well-blooded receiving bed. Rinse with sterile saline.
[0284] (6) Suturing: After taking photos and recording, use 4-0 sutures to suture the extraction socket tightly and then take photos.
[0285] (7) After the tooth extraction on one side is completed, the animal is placed in a lateral position and the tooth extraction on the other side is performed in the same manner as above to complete the operation. The experimental animal is then returned to the breeding cage.
[0286] (8) Record abnormal conditions and solutions during the operation.
[0287] (9) Postoperatively: intramuscular injection of penicillin (800,000 U / d) and tolfenamic acid for anti-inflammatory and analgesic purposes.
[0288] (10) Suture removal: The surgical sutures of all animals were uniformly removed about 14 days after surgery.
[0289] II-stage surgical procedure (alveolar bone defect)
[0290] Eight to twelve weeks after tooth extraction surgery, animals were fasted for 12 hours but not water on the day before surgery. On the day of the experiment, the animals were weighed and the extraction sockets were observed by X-ray after anesthesia. After the sockets were basically healed and the density of the new bone was close to that of the surrounding bone tissue, anesthesia was induced by intramuscular injection of Zotalitol 0.1 ml / kg. After endotracheal intubation, general anesthesia was maintained with sevoflurane.
[0291] (1) Disinfection: Place the animal in lateral position, disinfect the oral cavity and face with 2% iodine tincture, and cover with a sterile sheet.
[0292] (2) Local anesthesia: 2% lidocaine hydrochloride (1:100000 epinephrine) was used for local infiltration anesthesia in the surgical area to reduce bleeding during the operation.
[0293] (3) Flap opening: Cut the gingival tissue to expose the alveolar bone. Make an incision on the outer side of the gingiva in the extraction area, separate and open the mucosal flap to expose the outer side of the alveolar bone. Note: The flap should be fully relaxed to facilitate suturing after implantation and reduce the risk of membrane exposure.
[0294] (4) Modeling: Use a drill bit for drilling and grinding, and use a large amount of physiological saline to cool the patient during the drilling and grinding process. Use a 3mm diameter drill bit to drill and enlarge the hole at a speed of less than 1500rpm. Use a circular saw to cut the tooth extraction socket to prepare a saddle-shaped alveolar bone defect with a uniform depth, extent, and range. The defect has a mesiodistal width of 8mm, a vertical width of 5mm, and a buccal-lingual width of 5-7mm (the width of the mandibular bone of a beagle dog).
[0295] (5) Implantation of bone material: In a sterile container, artificial bone powder and beagle autologous bone (1:1) are pre-soaked and mixed with sterile saline to form a mixture. The mixture is then filled into the alveolar defect and squeezed with a filler to loosen the filling, avoiding crushing the trabeculae, until the bone powder is flush with the outer ridge of the alveolar bone.
[0296] (6) Covering film: Under sterile conditions, the metal reinforced polytetrafluoroethylene barrier film was cut into a suitable size, about 15×22 mm, and the products of Example 4, Comparative Example 1, and Comparative Example 2 were respectively covered on the buccal and lingual sides of the filling part at the corresponding sites and fixed with film pins. No film was used in the blank group.
[0297] (7) Suturing: All sites are turned back to the mucoperiosteal flap, and after fully loosening the flap, double-layer suture (such as horizontal suture + interrupted suture) is used to completely close the wound.
[0298] (8) After the tooth extraction on one side is completed, the animal is placed in a lateral position and the tooth extraction on the other side is performed in the same manner as above to complete the operation. The experimental animal is then returned to the breeding cage.
[0299] (9) Record any abnormal conditions and solutions during the operation.
[0300] (10) Postoperatively: intramuscular injection of penicillin (800,000 U / d) and tolfenamic acid for anti-inflammatory and analgesic purposes, and observation of exposure.
[0301] Suture removal: The surgical sutures of all animals were uniformly removed around 21 days after surgery.
[0302] CBCT scans were performed under anesthesia immediately after surgery, 13 weeks, and 26 weeks after surgery. After the CT scan was completed 26 weeks after surgery, the gums were cut open and the implant was removed. The degree of adhesion during implant removal was graded according to the Rydell scale, which is categorized into four levels: Grade 0: No obvious adhesion between the product and soft tissue; Grade I: The product is easily separated from the soft tissue by blunt dissection; Grade II: The product is easily separated from the soft tissue by blunt dissection, but the resistance is high, and the soft tissue remains intact after separation; Grade III: The product cannot be separated from the soft tissue by blunt dissection, and the soft tissue cannot remain intact after sharp dissection.
[0303] Table 5 Test results of soft tissue adhesion and exposure
[0304] Table 6 Osteogenesis effect test results
[0305] p<0.05, there is a significant difference between the groups, indicated by *; p<0.01, there is a very significant difference between the groups, indicated by **; p<0.001, there is an extremely significant difference between the groups, indicated by ***.
[0306] As shown in Table 5, the metal-reinforced polytetrafluoroethylene membrane product prepared in Example 2 was implanted in the oral cavity of beagle dogs for guided bone regeneration without membrane exposure. However, two cases of membrane exposure occurred in the commercially available product, Comparative Example 2, with an exposure rate of 33.3%. This may be because the dense structure of Comparative Example 2 affected the blood supply, resulting in soft tissue rupture.
[0307] According to the Rydell scoring system, the products of Example 4, Comparative Example 1, and Comparative Example 2 were removed and observed for soft tissue adhesion 26 weeks after implantation. All six test samples from Example 4 were easily dissected with blunt dissection, and the soft tissue remained intact after separation. In Comparative Example 1, two cases showed significant resistance to blunt dissection, with the soft tissue remaining intact after separation. In three cases, sharp dissection was required, resulting in damage to the mucosal tissue. Comparative Example 2 was relatively easy to separate from the soft tissue. The difficulty in separating Comparative Example 1 was primarily due to its large pore size, which easily allowed soft tissue to grow into the barrier membrane product, resulting in a tight bond with the barrier membrane, making removal difficult and easily damaging the mucosal tissue.
[0308] As shown in Table 6, Figures 18 and 19, the metal-reinforced polytetrafluoroethylene membrane products of Example 4, Comparative Example 1, and Comparative Example 2 all effectively induced osteogenesis in the vertical bone defect model, with the height of the formed bones being statistically different from that of the blank group. After 26 weeks of implantation, the height of the formed bones in Example 4 was significantly greater than that in Comparative Examples 1 and 2, and the osteogenesis rate in Example 4 was significantly greater than that in Comparative Examples 1 and 2. The superior osteogenesis in Example 4 is attributed to the microporous structure of the first and second membrane layers of the metal-reinforced polytetrafluoroethylene membrane, which are made of micro-stretched expanded polytetrafluoroethylene. This microporous structure facilitates soft tissue adhesion without adhesion, and facilitates nutrient penetration, thus promoting osteogenesis.
[0309] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0310] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A metal reinforced polytetrafluoroethylene membrane, characterized in that: It comprises a first film layer, a second film layer and a metal bracket, wherein the metal bracket is located between the first film layer and the second film layer and is covered by the first film layer and the second film layer; The materials of the first film layer and the second film layer are independently selected from micro-stretched expanded polytetrafluoroethylene with a stretching range of about 20% to 100%, and the micro-stretched expanded polytetrafluoroethylene has a microporous structure; The formed metal reinforced polytetrafluoroethylene membrane has micropores with an overall average pore size of about 0.03 μm to 0.50 μm; The material of the metal stent includes implantable metal.
2. The metal reinforced polytetrafluoroethylene membrane according to claim 1, characterized in that: The metal reinforced polytetrafluoroethylene film as a whole satisfies one or more of the following properties (1) to (3): (1) The pore size range of micropores is about 0.01 μm to 1.00 μm; (2) The total thickness of the film layer area not covered with the metal bracket is about 0.10 mm to 0.50 mm; (3) The total thickness of the film layer area coated with the metal bracket is about 0.20 mm to 0.80 mm.
3. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 2, characterized in that: The average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the second film layer is smaller than the average pore size of the micropores of the micro-stretched expanded polytetrafluoroethylene used to form the first film layer.
4. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 3, characterized in that: The micro-stretched expanded polytetrafluoroethylene used to form the first film layer satisfies one or more of the following properties (1) to (3): (1) The thickness is about 0.10mm to 0.40mm; (2) The pore size of the micropores ranges from about 0.05 μm to 5.0 μm; (3) The average pore size of the micropores is about 0.2 μm to 1.0 μm.
5. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 4, characterized in that: The micro-stretched expanded polytetrafluoroethylene used to form the second film layer satisfies one or more of the following properties (1) to (3): (1) The thickness is about 0.05mm to 0.3mm; (2) The pore size of the micropores ranges from about 0.01 μm to 2.50 μm; (3) The average pore size of the micropores is about 0.1 μm to 0.5 μm.
6. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 5, characterized in that: The implantable metal includes pure titanium, titanium alloy or stainless steel.
7. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 6, characterized in that: The thickness of the metal bracket is about 0.05 mm to 0.2 mm.
8. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 7, characterized in that: The metal bracket is a prefabricated metal bracket.
9. The metal reinforced polytetrafluoroethylene membrane according to claim 8, characterized in that: The metal support comprises a metal central bar and a plurality of metal branch bars, wherein the plurality of metal branch bars are distributed on both sides of the metal central bar, and each of the metal branch bars is respectively connected to the metal central bar.
10. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 9, characterized in that: The surface of the first film layer facing away from the metal support has groove-shaped stripes.
11. The metal reinforced polytetrafluoroethylene membrane according to claim 10, characterized in that: There are multiple stripes arranged in parallel.
12. The metal reinforced polytetrafluoroethylene membrane according to claim 11, characterized in that: Each of the stripes includes a plurality of first stripes arranged along a first direction and a plurality of second stripes arranged along a second direction; The first direction and the second direction are perpendicular to each other.
13. The metal reinforced polytetrafluoroethylene membrane according to claim 12, characterized in that: In each of the stripes, the first stripes and the second stripes are arranged alternately.
14. The metal reinforced polytetrafluoroethylene membrane according to claim 13, characterized in that: Among the stripes, the length of each first stripe is greater than the length of each second stripe, and the width of each first stripe is the same as the width of each second stripe; A plurality of the first stripes are arranged in a straight line, and a plurality of the second stripes are arranged in parallel; The depth of each of the first stripes and each of the second stripes decreases independently from the middle to both ends.
15. The metal reinforced polytetrafluoroethylene membrane according to any one of claims 12 to 14, characterized in that: The depth of each of the first stripes and the depth of each of the second stripes are independently approximately 0 mm to 0.15 mm.
16. A method for producing a metal reinforced polytetrafluoroethylene membrane according to any one of claims 1 to 15, characterized in that: The steps include: Providing a mold, the mold comprising a mold bottom plate and a mold cover plate; A first film, a metal bracket and a second film are sequentially stacked on the mold bottom plate, wherein the metal bracket does not extend beyond the outer edges of the first film and the second film; the materials of the first film and the second film are independently selected from micro-stretched expanded polytetrafluoroethylene with a stretching range of 20% to 100%, and the micro-stretched expanded polytetrafluoroethylene has a microporous structure; Covering the mold cover plate on the second film; hot pressing the mold containing the first film, the metal support and the second film; After the hot pressing is completed, the mold is removed after the temperature drops; the formed metal reinforced polytetrafluoroethylene film has an overall average pore size. Micropores with a diameter of about 0.03μm to 0.50μm.
17. The method for manufacturing a metal reinforced polytetrafluoroethylene membrane according to claim 16, characterized in that: The method further includes the step of forming stripes on a surface of the first film facing away from the metal support.
18. The method for manufacturing a metal reinforced polytetrafluoroethylene membrane according to claim 17, characterized in that: The step of forming stripes on the surface of the first film facing away from the metal support comprises: A stripe template corresponding to the preset stripes is placed between the first film and the mold bottom plate.
19. The method for producing a metal reinforced polytetrafluoroethylene membrane according to any one of items 16 to 18, characterized in that: The steps of heat pressing include: The mold containing the first film, the metal support and the second film is pressed, heated and kept warm in sequence.
20. The method for preparing the metal reinforced polytetrafluoroethylene membrane according to 19, characterized in that: The clamping method is locking clamping, and the locking torque is about 0.5N·m to 10N·m.
21. The method for producing a metal reinforced polytetrafluoroethylene membrane according to any one of items 19 to 20, characterized in that: The heating rate during heating is about 30°C / min to 60°C / min, and the heating temperature is about 300°C to 380°C.
22. The method for producing a metal-reinforced polytetrafluoroethylene membrane according to any one of items 19 to 21, characterized in that: The insulation time is about 1h to 5h.
23. The method for producing a metal reinforced polytetrafluoroethylene membrane according to any one of items 16 to 22, characterized in that: The cooling rate is about 2℃ / h~10℃ / h.
24. A barrier film, characterized in that: It comprises the metal reinforced polytetrafluoroethylene membrane as claimed in any one of claims 1 to 15.
25. Use of the barrier membrane according to claim 24 in guided bone regeneration.
Citation Information
Patent Citations
A high strength surgical patch
CN209574958U
Reinforced PTFE medical barriers
US20100217392A1
Reinforced multi-layered membrane
US20150245911A1
Perforated membrane for guided bone and tissue regeneration
US20170189159A1
Composite perforated implant structures
US5380328A