Composite base material and circuit board

By forming protrusions with specific roughness on the surface of the base layer and arranging an undulating resistance layer, the problem of poor uniformity of square resistance of the composite base material is solved, and the accuracy of the embedded resistor and the performance stability of the electronic component are improved.

WO2024216722A1PCT designated stage expired Publication Date: 2024-10-24GUANGZHOU FANGBANG ELECTRONICS +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/098455
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-06-06
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The sheet resistance uniformity of existing composite substrates is poor, which affects the accuracy of embedded resistors and the performance of electronic components, resulting in unstable circuit board structures.

Method used

By forming a number of protrusions on the surface of the base layer, controlling its roughness to 1μm-15μm, and setting the resistance layer into an undulating shape, ensuring that the resistance layer and the base layer are of the same shape, improving the uniformity of the resistance layer and the bonding between the composite substrate and the circuit board Peel strength.

Benefits of technology

It improves the sheet resistance uniformity of the embedded resistor, enhances the performance and structural stability of electronic components, and prevents the composite substrate from peeling off the circuit board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023098455_24102024_PF_FP_ABST
    Figure CN2023098455_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present invention are a composite base material and a circuit board. The composite base material comprises a substrate layer and a resistance layer, wherein the surface of one side of the substrate layer close to the resistance layer is provided with a plurality of protrusions, and the roughness Rz of the surface of one side of the substrate layer close to the resistance layer is 1-15 μm. By means of the technical solutions disclosed by the present application, sheet resistance uniformity of the resistance layer of the composite base material is improved, thereby facilitating preparation of an embedded resistor with relatively high precision, and facilitating improvement of performances of the circuit board and even electronic components.
Need to check novelty before this filing date? Find Prior Art

Description

Composite substrate and circuit board Technical Field

[0001] The present invention relates to the technical field of thin film resistors, and in particular to a composite substrate and a circuit board. Background Art

[0002] With the rapid development of wireless communications and electronic devices, electronic devices are evolving towards precision, miniaturization, and lightness. This requires that the components inside electronic devices be as small and light as possible. The resistor elements inside electronic devices have evolved from plug-in resistors with pins to chip resistors, and then from chip resistors to embedded resistors, gradually developing towards lightness and thinness. The application process of embedded resistors is roughly as follows: a composite substrate is attached to a circuit board, and an embedded resistor is etched out through an etching process. The composite substrate includes a base layer and a resistor layer located on one side surface of the base layer, and the surface of the resistor layer away from the base layer is suitable for attachment to the circuit board.

[0003] However, the existing composite substrates have poor uniformity in square resistance, which is not conducive to the preparation of embedded resistors with high precision.

[0004] Summary of the Invention

[0005] Therefore, the technical problem to be solved by the present invention is how to improve the uniformity of the square resistance of the embedded resistor, thereby providing a composite substrate and a circuit board.

[0006] The first aspect of the present invention provides a composite substrate, which includes a base layer and a first resistor layer, wherein the first resistor layer is stacked on at least one side surface of the base layer, and the side surface of the base layer facing the first resistor layer has a plurality of protrusions, and the roughness Rz of the side surface of the base layer having the protrusions is 1μm-15μm.

[0007] Optionally, at least some of the protrusions meet the following condition: the average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than the average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion.

[0008] Optionally, at least some of the protrusions meet the following condition: the minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than or equal to the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion.

[0009] Optionally, at least part of the protrusions meet the following condition: the minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is not less than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion.

[0010] Optionally, the average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than the average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion by at least 30%.

[0011] Optionally, the minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than or equal to the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion, accounting for at least 30% of the protrusion.

[0012] Optionally, the minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is not less than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion, accounting for at least 30%.

[0013] Optionally, the maximum value of the width of the protrusion at 1 / 2 of the height is 1 μm-10 μm.

[0014] Optionally, the height of the protrusion is 1 μm-15 μm.

[0015] Optionally, the thickness of the first resistance layer is 5 nm-3 μm.

[0016] Optionally, the thickness of the first resistance layer is 10 nm-200 nm.

[0017] Optionally, the composite substrate further includes a film layer located on a surface of the first resistor layer that is away from the base layer.

[0018] Optionally, the thickness of the film layer is 0.5 μm-100 μm.

[0019] Optionally, a conductive layer is provided on a side of the film layer away from the first resistance layer.

[0020] Optionally, the conductive layer is a single-layer conductive layer or a multi-layer conductive layer.

[0021] Optionally, a second resistance layer is provided between the film layer and the conductive layer.

[0022] Optionally, the material of the base layer is a conductive material or a dielectric material; the conductive material includes at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver or gold; the material of the resistance layer includes at least one element of Ni, Cr, Si, P, N, Ti, Pt, Ta, Mo, Sn or O.

[0023] A second aspect of the present invention provides a circuit board, comprising the composite substrate.

[0024] The technical solution of the present invention has the following advantages:

[0025] The composite substrate and circuit board provided by the present invention improve the uniformity of the sheet resistance of the resistor layer by controlling the surface roughness of the base layer near the resistor layer. This facilitates the preparation of highly precise embedded resistors and improves the performance of circuit boards and even electronic components. Furthermore, the resistor layer and base layer are arranged in the same shape, i.e., the resistor layer has an undulating shape, which enhances the peel strength between the composite substrate and the circuit board, making it difficult for the composite substrate to be peeled off from the circuit board and improving the structural stability of the electronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] FIG1 is a longitudinal cross-sectional SEM scan of a composite substrate;

[0028] FIG2 is a SEM scan of a protrusion of a composite substrate provided in an embodiment of the present invention;

[0029] FIG3 is a SEM scan of a longitudinal cross-section of a composite substrate provided in an embodiment of the present invention;

[0030] FIG4 is a schematic diagram of the stacking relationship of a composite substrate provided by an embodiment of the present invention;

[0031] FIG5 is a schematic diagram of the stacking relationship of another composite substrate provided by an embodiment of the present invention;

[0032] FIG6 is a schematic diagram of the stacking relationship of another composite substrate provided by an embodiment of the present invention;

[0033] FIG7 is a schematic diagram of the stacking relationship of another composite substrate provided by an embodiment of the present invention;

[0034] Description of reference numerals:

[0035] 1-base layer; 11-protrusion; 2-first resistance layer; 3-film layer; 4-conductive layer; 5-second resistance layer; 1′-base layer; 11′-protrusion. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0037] In the description of the present invention, it should be noted that the terms "upper", "lower", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limiting the present invention.

[0038] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0039] It should be understood that in order to improve the peel strength between the composite substrate and the circuit board and prevent the composite substrate from separating from the circuit board, a number of protrusions are usually formed on one surface of the base layer to give the surface of one side of the base layer a certain degree of roughness, so that the resistor layer formed on the rough surface of the base layer presents corresponding undulations.

[0040] The applicant discovered that, referring to FIG1 , when the minimum cross-sectional area of ​​the protrusion 11′ is located in the middle region of the protrusion 11′, and the maximum cross-sectional area from the middle region of the protrusion 11′ to the top of the protrusion 11′ is much larger than the minimum cross-sectional area, it is easy to cause the resistance material to be difficult to deposit relatively evenly on the rough surface of the base layer 1′ (see the area framed by the dotted line in FIG1 ), resulting in poor uniformity of the resistance layer deposited on the base layer 1′; and excessive roughness of the base layer will also lead to poor deposition uniformity of the resistance layer. The poor deposition uniformity of the resistance layer leads to poor uniformity of the square resistance of the resistance layer, which is not conducive to the preparation of embedded resistors with high precision, affecting the performance of circuit boards and even electronic components. It should be noted that a resistance layer is deposited on the surface of the side with the protrusion in the base layer of FIG1 , but because the resistance layer is relatively thin, it cannot be seen in FIG1 .

[0041] Based on this, referring to FIG. 2 to FIG. 4 , this embodiment provides a composite substrate, including:

[0042] A base layer 1, wherein at least one side surface of the base layer 1 has a plurality of protrusions 11, and the roughness Rz of the side surface of the base layer 1 having the protrusions 11 is 1 μm-15 μm;

[0043] The first resistor layer 2 is located on the surface of the side of the base layer 1 having the protrusion 11. The thickness of the first resistor layer is very thin, and the morphology of the first resistor layer is superimposed on the morphology of the base layer, and the morphologies of the two are basically the same. The roughness of the base layer of the present invention is measured from the side of the first resistor layer away from the base layer.

[0044] By setting the surface roughness Rz of the side of the base layer 1 with protrusions 11 to 1μm-15μm, the uniformity of the square resistance of the first resistor layer 2 is improved, facilitating the production of highly precise embedded resistors and improving the performance of circuit boards and even electronic components. Furthermore, the first resistor layer is configured in the same shape as the base layer, i.e., the first resistor layer has an undulating shape, which improves the peel strength between the composite substrate and the circuit board, making it difficult for the composite substrate to be peeled off from the circuit board and enhancing the structural stability of the electronic device.

[0045] In order to better achieve the technical effects of the present invention and further improve the uniformity of the square resistance, in one embodiment, on the basis that the roughness of the base layer meets the above-mentioned roughness requirements, at least some of the protrusions meet the following conditions: the average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than the average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion, and the extension direction of the protrusion is perpendicular to the base layer. Specifically, the number of protrusions that meet the above conditions can account for at least 30% of the total number of protrusions on one side of the base layer; illustratively, the number of protrusions that meet the above conditions accounts for more than 50% of the total number of protrusions on one side of the base layer. The greater the proportion of the number of protrusions that meet the above conditions, the better the uniformity of the square resistance of the first resistor layer.

[0046] Preferably, at least some of the protrusions meet the following conditions: the minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than or equal to the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion. This makes it easier for the resistor material to be evenly formed on the rough surface of the base layer, further optimizing uniformity and continuity. Specifically, the number of protrusions meeting the above conditions accounts for at least 30% of the total number of protrusions on one side of the base layer; illustratively, the number of protrusions meeting the above conditions accounts for more than 50% of the total number of protrusions on one side of the base layer. The greater the proportion of protrusions meeting the above conditions, the better the uniformity of the square resistance of the first resistor layer.

[0047] More preferably, at least some of the protrusions meet the following conditions: the minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is not less than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion, and the maximum width of the cross-section of the protrusion at each height is the width value at that height; in this case, the protrusion is "peak-shaped" as a whole, and the resistor material is more easily and evenly formed on the rough surface of the base layer, with better uniformity and continuity. Specifically, the number of protrusions that meet the above conditions can account for at least 30% of the total number of protrusions on one side of the base layer; illustratively, the number of protrusions that meet the above conditions accounts for more than 50% of the total number of protrusions on one side of the base layer. The greater the proportion of protrusions that meet the above conditions, the better the uniformity of the square resistance of the first resistor layer.

[0048] Furthermore, the width of the protrusion at 1 / 2 height is 1 μm-10 μm. For example, the width of the protrusion at 1 / 2 height can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and other values ​​within the above range. The width of the protrusion at 1 / 2 height refers to the maximum width at a cross section of the protrusion at 1 / 2 height.

[0049] Furthermore, the height h of the protrusion is 1 μm-15 μm. For example, the height of the protrusion can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm, and other values ​​within the above range. The height of the protrusion refers to the distance from the bottom of the protrusion to the top of the protrusion.

[0050] In this embodiment, the thickness of the base layer is 2μm-100μm, and the thickness of the base layer is preferably 8μm-35μm. The thickness of the first resistor layer is 5nm-3μm, and the thickness of the first resistor layer is preferably 10nm-200nm. Exemplarily, the thickness of the base layer can be 2μm, 4μm, 6μm, 8μm, 10μm, 20μm, 30μm, 35μm, 50μm, 60μm, 80μm or 100μm; the thickness of the first resistor layer is 5nm, 10nm, 25nm, 50nm, 75nm, 100nm, 125nm, 150nm, 175nm, 200nm, 1μm, 1.5μm, 2μm, 2.5μm, or 3μm.

[0051] It should be noted that the thickness of the base layer, the thickness of the first resistor layer, and the maximum width and other related parameters in this embodiment are obtained by preparing the composite substrate sample into slices and then measuring them under a scanning electron microscope. The magnification of the scanning electron microscope is 2000 times to 70,000 times. Figure 3 shows a longitudinal cross-sectional scan of a composite substrate. The first resistor layer is deposited on the surface of the side with a protrusion in the base layer of Figure 3. However, since the first resistor layer is relatively thin and the magnification is large, it cannot be seen in Figure 3. Figure 2 shows a schematic cross-sectional view of a protrusion. The magnification of Figure 2 is 50,000 times. The surface of the protrusion in Figure 2 has a resistor layer with a thickness of 58.1nm-61.9nm.

[0052] In this embodiment, the base layer is made of a conductive material or a dielectric material, and can be a single layer or a laminated multilayer structure. Conductive materials include, but are not limited to, at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver, and gold. Specifically, the base layer can be copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil, or gold foil. It can also be an alloy foil containing at least two of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver, and gold. It can also be a composite foil composed of at least two of copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil, and gold foil. Dielectric materials include, but are not limited to, PET, PP, PS, ABF film, BT resin, polyacrylic acid, polyurethane, polyimide, and the like. In a base layer having a multilayer structure, the materials of different layers can be the same or different.

[0053] The first resistor layer is a key functional layer of the composite substrate, which is used to realize the resistance function of the embedded resistor. The first resistor layer can be made of different materials according to the needs of different functions, and thus have different resistance characteristics. Specifically, the material of the first resistor layer includes at least one element of Ni, Cr, Si, P, N, Ti, Pt, Ta, Mo, Sn, and O. Specifically, the material can be at least one of NiCrSi, NiCrAlSi, NiP, NiCr, AlN, TiN, Pt, Cr, Cr-SiO, Cr-Si, Ti-Si, Ti-W, TaN, Mo, and Ni-Sn materials. The first resistor layer can be a single-layer structure or a multi-layer structure stacked together. In the first resistor layer with a multi-layer structure, the materials between different layers can be the same or different.

[0054] In this embodiment, the first resistor layer is formed by at least one process selected from electroplating, chemical plating, physical vapor deposition, and chemical vapor deposition. The sheet resistance of the first resistor layer is 1Ω-2000Ω.

[0055] As shown in Figure 5 , as an optional embodiment, the composite substrate further includes a film layer 3 located on the surface of the first resistive layer 2 facing away from the base layer 1. This film layer protects the first resistive layer 2 from damage by external forces. Furthermore, when the composite substrate is attached to a circuit board, the film layer adheres to the first resistive layer 2 and the circuit board, further enhancing the peel strength between the composite substrate and the circuit board, making it difficult to peel from the circuit board and improving the structural stability of the electronic device. Furthermore, the film layer can be used to prepare a foil-clad laminate for direct application in rigid or flexible PCBs.

[0056] Specifically, the thickness of the film layer is 0.5 μm-100 μm. Exemplarily, the thickness of the film layer can be 2 μm, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 20 μm, 30 μm, 40 μm, 55 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm. The film layer is selected from at least one of polystyrene thermoplastic resin, vinyl acetate thermoplastic resin, polyester thermoplastic resin, polyethylene thermoplastic resin, polyamide thermoplastic resin, rubber thermoplastic resin, acrylic thermoplastic resin, phenolic thermosetting resin, epoxy thermosetting resin, thermoplastic polyimide thermosetting resin, urethane thermosetting resin, melamine thermosetting resin, alkyd thermosetting resin and ABF resin. Illustratively, the film layer is selected from at least one of modified epoxy resin, modified acrylic resin, polyethylene terephthalate, polybutylene terephthalate, polyethylene, polyethylene naphthalate, polystyrene, polyvinyl chloride, polysulfone, polyphenylene sulfide, polyetheretherketone, polyphenylene oxide, polytetrafluoroethylene, liquid crystal polymer, polyoxaline, epoxy glass cloth, and BT resin. The specific thickness and material of the film layer can be selected and set by those skilled in the art based on actual needs.

[0057] Furthermore, referring to FIG6 , in one embodiment, a film layer 3 is provided in the composite substrate, and a conductive layer 4 is provided on the side of the film layer 3 away from the first resistor layer 2, thereby forming a foil-clad plate containing the first resistor layer. The foil-clad plate has a four-layer structure and can be directly applied to hard or soft boards. Specifically, the conductive layer can be a single-layer structure or a multi-layer structure. That is, the conductive layer can be copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil, or gold foil. It can also be an alloy foil containing at least two of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver, and gold. It can also be a composite foil composed of at least two of copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil, and gold foil. The material of the conductive layer can be the same as or different from the material of the base layer, and those skilled in the art can adjust it according to actual needs.

[0058] Furthermore, referring to FIG7 , in one embodiment, a second resistor layer 5 is disposed between the film layer 3 and the conductive layer 4, thereby forming an asymmetric structure. The material of the second resistor layer can be the same as or different from that of the first resistor layer 2, and those skilled in the art can configure the material based on actual needs.

[0059] This embodiment also provides a circuit board comprising the composite substrate. The circuit board has all the advantages of the composite substrate, which will not be described in detail here.

[0060] Specific examples and comparative examples are now provided as examples to support the technical effects of the present invention. The composite substrates in both the examples and comparative examples include a base layer and a first resistor layer, one surface of the base layer having a plurality of protrusions, and the first resistor layer is laminated on the side of the base layer having the protrusions. The base layer is 18 μm thick copper foil, and the first resistor layer is made of a NiCr alloy with a thickness of 22 nm.

[0061] Example 1

[0062] In this embodiment, the roughness Rz of the surface of the base layer with the protrusion is 5 μm. The average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than the average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion in 60%.

[0063] Example 2

[0064] In this embodiment, the roughness Rz of the surface of the base layer with the protrusion is 5 μm. The minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than or equal to the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion in 60%.

[0065] Example 3

[0066] In this embodiment, the roughness Rz of the surface of the base layer with the protrusion is 5 μm. The minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is not less than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion accounts for 60%.

[0067] Comparative Example 1

[0068] The only difference between the composite substrate provided in this comparative example and the composite substrate provided in Example 1 is that in the composite substrate provided in this comparative example, the surface roughness Rz of the side of the base layer having the protrusions is 0.5 μm.

[0069] Comparative Example 2

[0070] The only difference between the composite substrate provided in this comparative example and the composite substrate provided in Example 1 is that in the composite substrate provided in this comparative example, the average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is smaller than the average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion.

[0071] Comparative Example 3

[0072] The only difference between the composite substrate provided in this comparative example and the composite substrate provided in Example 2 is that in the composite substrate provided in this comparative example, the minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is smaller than the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion.

[0073] Comparative Example 4

[0074] The only difference between the composite substrate provided in this comparative example and the composite substrate provided in Example 3 is that in the composite substrate provided in this comparative example, the minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is smaller than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion.

[0075] Comparative Example 5

[0076] The only difference between the composite substrate provided in this comparative example and the composite substrate provided in Example 1 is that in the composite substrate provided in this comparative example, the surface roughness Rz of the side of the base layer having the protrusions is 20 μm.

[0077] Test example

[0078] The composite substrates provided in Examples 1-3 and Comparative Examples 1-5 were subjected to a sheet resistance uniformity test and a peeling force test. During the sheet resistance uniformity test, the sheet resistance M at different locations of the composite substrate was first tested. The sheet resistance test points were evenly distributed on the surface of the composite substrate, and the number of sheet resistance test points was 20. The average sheet resistance M at different locations of the composite substrate was then calculated. ave , and select the maximum square resistance M max and the minimum square resistance M min , then calculate the upper limit and lower limit of square resistance uniformity: Upper limit of square resistance uniformity = (M max -M ave ) / M ave ×100%; lower limit of square resistance uniformity = (M min -M ave ) / M ave ×100%; see Table 1 for test results:

[0079] Table 1

[0080] As can be seen from Table 1, the technical solution in this embodiment not only meets the required peeling force, but also has more outstanding uniformity and more stable performance.

[0081] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will readily appreciate that other variations or modifications based on the above descriptions are possible. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A composite substrate, characterized in that The composite substrate includes a base layer and a first resistor layer, the first resistor layer is stacked on at least one side surface of the base layer, the base layer has a plurality of protrusions on the side surface facing the first resistor layer, and the roughness Rz of the base layer having the protrusions is 1 μm-15 μm.

2. The composite substrate according to claim 1, characterized in that At least some of the protrusions satisfy the following condition: an average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than an average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion.

3. The composite substrate according to claim 1, characterized in that At least some of the protrusions meet the following condition: the minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than or equal to the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion.

4. The composite substrate according to claim 1, characterized in that At least some of the protrusions satisfy the following condition: the minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is not less than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion.

5. The composite substrate according to claim 2, characterized in that The average cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion is greater than the average cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion by at least 30%.

6. The composite substrate according to claim 3, characterized in that The proportion of protrusions having a minimum cross-sectional area from the bottom of the protrusion to 1 / 2 of the height of the protrusion greater than or equal to the maximum cross-sectional area from 1 / 2 of the height of the protrusion to the top of the protrusion is at least 30%.

7. The composite substrate according to claim 4, characterized in that The proportion of protrusions for which the minimum width from the bottom of the protrusion to 1 / 2 of the height of the protrusion is not less than the maximum width from 1 / 2 of the height of the protrusion to the top of the protrusion is at least 30%.

8. The composite substrate according to claim 4, characterized in that The maximum value of the width of the protrusion at 1 / 2 of the height is 1 μm to 10 μm.

9. The composite substrate according to any one of claims 1 to 8, characterized in that: The height of the protrusion is 1 μm-15 μm.

10. The composite substrate according to any one of claims 1 to 8, characterized in that: The thickness of the first resistance layer is 5 nm-3 μm.

11. The composite substrate according to claim 10, characterized in that The thickness of the first resistance layer is 10nm-200nm.

12. The composite substrate according to any one of claims 1 to 8, characterized in that: The composite substrate further includes a film layer located on a surface of the first resistor layer on a side away from the base layer.

13. The composite substrate according to claim 12, characterized in that The thickness of the film layer is 0.5 μm-100 μm.

14. The composite substrate according to claim 12, characterized in that A conductive layer is disposed on a side of the film layer away from the first resistance layer.

15. The composite substrate according to claim 14, characterized in that The conductive layer is a single conductive layer or a multi-layer conductive layer.

16. The composite substrate according to claim 14, characterized in that A second resistance layer is arranged between the film layer and the conductive layer.

17. The composite substrate according to any one of claims 1 to 8, characterized in that The material of the base layer is a conductive material or a dielectric material; the conductive material includes at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver or gold; the material of the resistance layer includes at least one element of Ni, Cr, Si, P, N, Ti, Pt, Ta, Mo, Sn or O.

18. A circuit board, characterized in that: The circuit board comprises the composite substrate according to any one of claims 1 to 17.

Citation Information

Patent Citations

  • Resistance-embedded metal foil

    CN114521049A

  • Composite metal foil and circuit board

    CN114554686A

  • Composite base material and circuit board

    CN116137197A

  • Resistance layer built-in copper clad laminated sheet and printed circuit board using the same

    JP2003200523A

  • Chip resistor, current sensor device, and manufacturing method of chip resistor