Transparent deketoxime-type silicone sealant

By using high viscosity and low viscosity α,ω-dihydroxypolydimethylsiloxane compound and basic amino acid modified silica in transparent silicone sealant, the problem of reduced transparency is solved and high mechanical properties are achieved. High performance and short drying time ensure transparency stability after long-term storage.

WO2024216837A1PCT designated stage expired Publication Date: 2024-10-24ANHUI JINGKANG BUILDING MATERIALS CO LTD

Patent Information

Application Number
PCT/CN2023/119896
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-09-20
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The transparency of transparent silicone sealants on the market is average, especially after long-term storage, the transparency drops significantly, mainly because the aggregation tendency of hydrophilic silica affects the transparency after curing.

Method used

High-viscosity and low-viscosity α,ω-dihydroxypolydimethylsiloxane compound is used as the base gum, and silica is modified with basic amino acids to weaken its aggregation tendency and improve the transparency after curing. At the same time, it uses enhanced Plasticizers and cross-linkers improve mechanical properties and cure speed.

Benefits of technology

The transparency and mechanical properties of the transparent ketone oxime silicone sealant are significantly improved, the surface drying time is shortened, and the transparency does not decrease significantly after long-term storage, and the light transmittance is maintained above 85%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to the technical field of sealants, and in particular relates to a transparent deketoxime-type silicone sealant. The transparent deketoxime-type silicone sealant comprises the following components in parts by mass: 80-160 parts of high-viscosity α,ω-dihydroxy polydimethylsiloxane, 20-40 parts of low-viscosity α,ω-dihydroxy polydimethylsiloxane, 5-10 parts of modified white carbon black, 25-45 parts of a plasticizer, 10-20 parts of a crosslinking agent and 0.1-0.3 parts of a catalyst, wherein the modified white carbon black is obtained by grafting white carbon black with a basic amino acid. The basic amino acid changes the surface energy of the white carbon black, such that the aggregation tendency of the modified white carbon black in the transparent deketoxime-type silicone sealant before curing is weakened, and the modified white carbon black does not aggregate during long-term storage, thereby improving the transparency after curing.
Need to check novelty before this filing date? Find Prior Art

Description

A transparent deketoxime type silicone sealant Technical Field

[0001] The present invention relates to the technical field of sealants, in particular to a transparent deketoxime type silicone sealant. Background Art

[0002] Transparent silicone sealant is a one-component, neutral-curing, high-quality sealant widely recognized for its unique advantages, including high transparency, excellent thixotropy, and high elongation. As a type of room-temperature vulcanized silicone rubber, it exhibits excellent resistance to cold, heat, aging, water, and moisture.

[0003] Currently, all transparent silicone sealants on the market use hydrophilic silica as a reinforcing agent and thixotropic agent, resulting in a translucent appearance. Ketoxime-based transparent silicone sealants dominate the transparent sealant market. Silica particle size, specific surface area, surface properties, and dosage significantly influence the performance of the vulcanized sealant. Generally, smaller specific surface area (larger particle size) or excessive dosage results in lower transparency and correspondingly poorer mechanical properties. Larger specific surface area (smaller particle size) results in higher transparency.

[0004] The base glue of silicone sealant is α,ω-dihydroxypolydimethylsiloxane, which itself has a large number of silanol groups. The surface of hydrophilic silica contains a large number of silanol groups, which can cross-link with the base glue during the curing process, have better compatibility, and help improve transparency. However, the transparency of transparent silicone sealants currently on the market is average, especially after long-term storage, its transparency decreases significantly. This is mainly because the surface of hydrophilic silica before curing contains a large number of silanol groups and has a tendency to aggregate. Especially after long-term storage, its aggregation phenomenon becomes more serious, affecting the transparency after curing. Summary of the Invention

[0005] In view of this, the purpose of the present invention is to provide a transparent deketoxime silicone sealant to solve the problem that the transparency of transparent silicone sealants currently on the market is generally poor, especially after long-term storage, its transparency decreases significantly.

[0006] Based on the above purpose, the present invention provides a transparent deketoxime silicone sealant, comprising the following components in parts by mass: 80-160 parts of high-viscosity α,ω-dihydroxypolydimethylsiloxane, 20-40 parts of low-viscosity α,ω-dihydroxypolydimethylsiloxane, 5-10 parts of modified silica, 25-45 parts of a plasticizer, 10-20 parts of a crosslinking agent, and 0.1-0.3 parts of a catalyst;

[0007] Preferably, the viscosity of the high-viscosity α,ω-dihydroxypolydimethylsiloxane is 30,000 mPa·s-80,000 mPa·s (25°C);

[0008] Preferably, the viscosity of the low-viscosity α,ω-dihydroxypolydimethylsiloxane is 2000-5000 mPa·s (25°C);

[0009] Preferably, the specific synthesis steps of the modified silica are as follows:

[0010] (1) Adding silica to a mixed solution of deionized water and ethanol, then adding γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stirring at room temperature for 3-5 hours, washing and drying to obtain epoxidized silica;

[0011] (2) Add epoxidized silica to ethyl acetate, then add basic amino acid and 4-dimethylaminopyridine, heat to 115-120 °C, stir for 7-9 hours, wash and dry to obtain modified silica.

[0012] Preferably, the white carbon black has a specific surface area of ​​100-120m 2 / g of hydrophilic fumed silica and a specific surface area of ​​20-100m 2 / g of precipitated silica.

[0013] Preferably, the white carbon black preferably has a specific surface area of ​​20-50m 2 / g of precipitated silica.

[0014] Preferably, in the specific synthesis steps of the modified silica, the mass ratio of silica, deionized water, ethanol and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in step (1) is 5-10:40-100:10-20:0.005-0.01.

[0015] Preferably, in the specific synthesis steps of the modified silica, the mass ratio of epoxidized silica, ethyl acetate, basic amino acid and 4-dimethylaminopyridine in step (2) is 5-10:50-100:0.01-0.02:0.001-0.002.

[0016] Preferably, the basic amino acid is one of arginine, lysine and histidine.

[0017] Preferably, the plasticizer is dimethyl silicone oil with a viscosity of 100-500 mPa·s (25°C).

[0018] Preferably, the crosslinking agent is one or more of methyltributylanoximesilane, vinyltributylanoximesilane, and tetrabutylketoximesilane.

[0019] Preferably, the catalyst is one of dibutyltin dilaurate, dibutyltin diacetate, and dimethyltin diceneodecanoate.

[0020] Furthermore, the present invention also provides a method for preparing the transparent deketoxime-type silicone sealant. The specific preparation method is as follows:

[0021] S1: low viscosity α,ω-dihydroxy polydimethylsiloxane and modified silica are added to a reactor and stirred for 30-60 minutes under vacuum to obtain a mixture A;

[0022] S2: Add high viscosity α,ω-dihydroxy polydimethylsiloxane and plasticizer to mixture A, and stir under vacuum for 20-40 minutes to obtain mixture B;

[0023] S3: Add the crosslinking agent and catalyst to the mixture B, and stir for 20-40 minutes under a vacuum environment to obtain a transparent deketoxime type silicone sealant.

[0024] Beneficial effects of the present invention:

[0025] The present invention utilizes basic amino acids to modify silica to prepare modified silica. Since the basic amino acids change the surface energy of silica, the aggregation tendency of the modified silica in a transparent deketoxime-type silicone sealant before curing is weakened, and aggregation will not occur even after long-term storage, thereby improving the transparency after curing.

[0026] The base glue of the present invention is compounded with high-viscosity α,ω-dihydroxy polydimethylsiloxane and low-viscosity α,ω-dihydroxy polydimethylsiloxane. The high-viscosity α,ω-dihydroxy polydimethylsiloxane helps to improve the overall mechanical properties of the sealant after curing, while the molecular chain of the low-viscosity α,ω-dihydroxy polydimethylsiloxane has better flexibility and is not affected by the steric hindrance of the basic amino acids on the surface of the modified silica. It helps to combine with the remaining hydroxyl groups on the surface of the modified silica during curing, thereby improving the dispersion of the modified silica after curing and further improving the transparency.

[0027] After the white carbon black is grafted with the basic amino acid, the adhesion between the sealant and the substrate is improved due to the influence of the amino groups on the surface of the basic amino acid, and the catalytic effect of the amino groups themselves increases the curing speed and shortens the surface drying time. Implementation Method

[0028] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below with reference to specific embodiments.

[0029] The sources or properties of the raw materials used in the present invention are as follows:

[0030] The viscosity of high viscosity α,ω-dihydroxy polydimethylsiloxane is 50000mPa·s (25℃), the viscosity of low viscosity α,ω-dihydroxy polydimethylsiloxane is 3000mPa·s (25℃), and the specific surface area of ​​white carbon black is 30m2 / g of precipitated silica, and the viscosity of dimethyl silicone oil is 200mPa·s (25℃). Example

[0031] S1: 5 g of silica was added to a mixed solution of 40 g of deionized water and 10 g of ethanol, and then 0.005 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane was added. The mixture was stirred at room temperature for 3 h, washed and dried to obtain epoxidized silica.

[0032] S2: 5 g of epoxidized silica was added to 50 g of ethyl acetate, followed by 0.01 g of lysine and 0.001 g of 4-dimethylaminopyridine. The mixture was heated to 115°C, stirred for 7 h, washed, and dried to obtain modified silica.

[0033] S3: 20 g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 5 g of modified silica were added to a reactor and stirred under vacuum for 30 min to obtain a mixture A;

[0034] S4: 80 g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 25 g of dimethyl silicone oil were added to mixture A, and the mixture was stirred under vacuum for 20 min to obtain mixture B;

[0035] S5: 10 g of methyltributylidene oxime silane and 0.1 g of dibutyltin dilaurate were added to mixture B, and the mixture was stirred under vacuum for 20 min to obtain a transparent deketoxime silicone sealant. Example

[0036] S1: 7.5 g of silica was added to a mixed solution of 70 g of deionized water and 15 g of ethanol, and then 0.007 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane was added. The mixture was stirred at room temperature for 4 h, washed and dried to obtain epoxidized silica.

[0037] S2: 7.5 g of epoxidized silica was added to 75 g of ethyl acetate, followed by 0.015 g of lysine and 0.002 g of 4-dimethylaminopyridine. The mixture was heated to 115°C, stirred for 8 h, washed, and dried to obtain modified silica.

[0038] S3: 30 g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 7.5 g of modified silica were added to a reactor and stirred under vacuum for 45 min to obtain a mixture A.

[0039] S4: 120 g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 35 g of dimethyl silicone oil were added to mixture A, and the mixture was stirred under vacuum for 30 min to obtain mixture B;

[0040] S5: 15 g of methyltributylidene oxime silane and 0.2 g of dibutyltin dilaurate were added to mixture B, and stirred under vacuum for 30 min to obtain a transparent deketoxime silicone sealant. Example

[0041] S1: 10 g of silica was added to a mixed solution of 100 g of deionized water and 20 g of ethanol, and then 0.01 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane was added. The mixture was stirred at room temperature for 5 h, washed and dried to obtain epoxidized silica.

[0042] S2: 10 g of epoxidized silica was added to 100 g of ethyl acetate, followed by 0.02 g of lysine and 0.002 g of 4-dimethylaminopyridine. The mixture was heated to 120°C, stirred for 9 h, washed, and dried to obtain modified silica.

[0043] S3: 40 g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 10 g of modified silica were added to a reactor and stirred under vacuum for 60 min to obtain a mixture A;

[0044] S4: 160 g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 45 g of dimethyl silicone oil were added to mixture A, and the mixture was stirred under vacuum for 40 min to obtain mixture B;

[0045] S5: 20 g of methyltributylidene oxime silane and 0.3 g of dibutyltin dilaurate were added to mixture B, and stirred under vacuum for 40 min to obtain a transparent deketoxime silicone sealant. Example

[0046] S1: Same as Example 2;

[0047] S2: 7.5 g of epoxidized silica was added to 75 g of ethyl acetate, followed by 0.015 g of arginine and 0.002 g of 4-dimethylaminopyridine. The mixture was heated to 115°C, stirred for 8 h, washed, and dried to obtain modified silica.

[0048] S3: Same as Example 2;

[0049] S4: Same as Example 2;

[0050] S5: Same as Example 2. Example

[0051] S1: Same as Example 2;

[0052] S2: 7.5 g of epoxidized silica was added to 75 g of ethyl acetate, followed by 0.015 g of histidine and 0.002 g of 4-dimethylaminopyridine. The mixture was heated to 115°C, stirred for 8 h, washed, and dried to obtain modified silica.

[0053] S3: Same as Example 2;

[0054] S4: Same as Example 2;

[0055] S5: Same as Example 2.

[0056] S1: 30 g of low-viscosity α,ω-dihydroxypolydimethylsiloxane and 7.5 g of white carbon black were added to a reactor and stirred under vacuum for 45 min to obtain a mixture A;

[0057] S2: 120 g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 35 g of dimethyl silicone oil were added to mixture A, and the mixture was stirred under vacuum for 30 min to obtain mixture B;

[0058] S3: 15 g of methyltributylidene oxime silane and 0.2 g of dibutyltin dilaurate were added to mixture B, and the mixture was stirred under vacuum for 30 min to obtain a deketoxime silicone sealant.

[0059] S1: Same as Example 2;

[0060] S2: Same as Example 2;

[0061] S3: 30 g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 7.5 g of modified silica were added to a reactor and stirred under vacuum for 45 min to obtain a mixture A.

[0062] S4: 120 g of high-viscosity α,ω-dihydroxypolydimethylsiloxane and 35 g of dimethyl silicone oil were added to mixture A, and the mixture was stirred under vacuum for 30 min to obtain mixture B;

[0063] S5: Same as Example 2.

[0064] Performance Testing

[0065] Surface drying time: The test was conducted in accordance with GB / T 13477.5-2017 "Test Methods for Building Sealing Materials". After storing Examples 1-5 and Comparative Examples 1-2 in a cool environment for 0 and 30 days, adhesive strips were extruded. The end of a finger was gently touched at different locations on the adhesive strip, and the time required for the finger to no longer adhere to the sample was recorded. The results are shown in Table 1.

[0066] Mechanical properties: According to the standard GB / T13477.8-2017 "Test Methods for Building Sealing Materials", Examples 1-5 and Comparative Examples 1-2 were placed in a cool environment and stored for 0 days and 30 days, and then cured to obtain dumbbell-shaped standard test pieces. The dumbbell-shaped standard test pieces were tensile tested using a tensile testing machine at a speed of 6 mm / min to obtain tensile strength and elongation at break. The results are shown in Table 1.

[0067] Light transmittance: According to the standard GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics", Examples 1-5 and Comparative Examples 1-2 were placed in a cool environment and stored for 0 days and 30 days, and then cured to obtain standard test pieces. The light transmittance of the standard test pieces was measured using a transmittance and haze meter (Saicheng WGT-S). The results are shown in Table 1.

[0068] Tensile Adhesion: According to GB / T 13477.5-2017 "Test Methods for Building Sealing Materials", Examples 1-5 and Comparative Examples 1-2 were stored in a cool environment for 0 days and 30 days, then cured on colorless transparent float glass. The tensile bond strength was measured using a tensile testing machine at a speed of 6 mm / min. The results are shown in Table 1.

[0069] Table 1 Performance test results of Examples 1-5 and Comparative Examples 1-2

[0070] Data analysis: It can be seen from Examples 1-5 that the transparent deketoxime type silicone sealant prepared by the present invention has excellent mechanical properties and a short surface drying time, and its light transmittance can reach more than 89%. After storage for 30 days and then curing, its light transmittance can still be maintained below 85%, and the decline is not obvious. Among them, the light transmittance of Examples 4 and 5 decreases more, which may be because different basic amino acids give different surface energies to silica, and the change in surface energy helps to disperse silica during storage. It can be seen from Example 2 and Comparative Examples 1-2 that the low-viscosity base glue and modified silica synergistically stabilize the uniform dispersion of silica during storage, among which the modification of silica has the greatest influence on the stability of silica during storage.

[0071] It should be understood by those skilled in the art that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Within the scope of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0072] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A transparent deketoxime type silicone sealant, characterized in that: The invention comprises the following components in parts by weight: 80-160 parts of high viscosity α,ω-dihydroxy polydimethylsiloxane, 20-40 parts of low viscosity α,ω-dihydroxy polydimethylsiloxane, 5-10 parts of modified white carbon black, 25-45 parts of plasticizer, 10-20 parts of crosslinking agent and 0.1-0.3 parts of catalyst; The viscosity of the high-viscosity α,ω-dihydroxy polydimethylsiloxane is 30000 mPa·s-80000 mPa·s (25°C); The viscosity of the low-viscosity α,ω-dihydroxy polydimethylsiloxane is 2000-5000 mPa·s (25°C); The specific synthesis steps of the modified silica are as follows: (1) Adding silica to a mixed solution of deionized water and ethanol, then adding γ-(2,3-epoxypropoxy)propyltrimethoxysilane, stirring at room temperature for 3-5 hours, washing and drying to obtain epoxidized silica; (2) Add epoxidized silica to ethyl acetate, then add basic amino acid and 4-dimethylaminopyridine, heat to 115-120°C, stir for 7-9 hours, wash and dry to obtain modified silica.

2. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: The white carbon black has a specific surface area of ​​100-120m 2 / g of hydrophilic fumed silica and a specific surface area of ​​20-100m 2 / g of precipitated silica.

3. The transparent deketoxime type silicone sealant according to claim 2, characterized in that: The white carbon black preferably has a specific surface area of ​​20-50 m 2 / g of precipitated silica.

4. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: In the specific synthesis steps of the modified white carbon black, the mass ratio of white carbon black, deionized water, ethanol and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in step (1) is 5-10:40-100:10-20:0.005-0.

01.

5. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: In the specific synthesis steps of the modified silica, the mass ratio of the epoxidized silica, ethyl acetate, basic amino acid and 4-dimethylaminopyridine in step (2) is 5-10:50-100:0.01-0.02:0.001-0.

002.

6. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: The basic amino acid is one of arginine, lysine and histidine.

7. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: The plasticizer is dimethyl silicone oil with a viscosity of 100-500 mPa·s (25°C).

8. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: The crosslinking agent is one or more of methyltributylacetoximine silane, vinyltributylacetoximine silane and tetrabutylketoneximine silane.

9. The transparent deketoxime type silicone sealant according to claim 1, characterized in that: The catalyst is one of dibutyltin dilaurate, dibutyltin diacetate and dimethyltin diceneodecanoate.

10. A method for preparing a transparent deketoxime type silicone sealant according to any one of claims 1 to 9, characterized in that: The specific preparation method is as follows: S1: adding low viscosity α,ω-dihydroxy polydimethylsiloxane and modified white carbon black into a reaction kettle, stirring for 30-60 minutes under a vacuum environment to obtain a mixture A; S2: adding high viscosity α,ω-dihydroxy polydimethylsiloxane and plasticizer to mixed material A, stirring for 20-40 minutes under vacuum environment to obtain mixed material B; S3: Add the crosslinking agent and the catalyst into the mixed material B, and stir for 20-40 minutes under a vacuum environment to obtain a transparent deketoxime type silicone sealant.

Citation Information

Patent Citations

  • Low-modulus monocomponent de-ketoxime type room temperature sulfurized silicone sealant and preparation method thereof

    CN106833503A

  • Deoximation oil-resistant fluorosilicone sealant and preparation method thereof

    CN107189753A

  • Two-component acidic silicone rubber vulcanized at room temperature and preparation method thereof

    CN107286668A

  • Acid silicone adhesive for simulated dinosaur crafts and preparing method thereof

    CN107353869A

  • Preparing method of anti-static glue

    CN110172316A

Cited By

  • High-temperature-resistant single-component silicone adhesive and preparation method thereof

    CN119391362A

  • Tear-resistant and fatigue-resistant silicone sealant and preparation method thereof

    CN122213912A