High-chemical-resistance positive photosensitive resin composition, preparation method therefor, and use thereof
By adding an aliphatic flexible compound containing unsaturated bonds to a positive photosensitive resin, the problem of insufficient chemical resistance of the resin in the erosion of high-temperature resist stripping liquids is solved, and high resistance to resist stripping liquids is achieved. and high resolution to meet the multiple performance needs of semiconductor manufacturing.
Patent Information
- Application Number
- PCT/CN2023/128139
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-24
AI Technical Summary
Existing positive-working photosensitive resins have poor chemical resistance when faced with erosion by high-temperature resist stripping solutions, and their resolution is insufficient to meet the needs of advanced packaging fields.
By adding an aliphatic flexible compound containing unsaturated bonds to the positive photosensitive resin composition, the residual stress and chemical resistance of the cured film are improved, and the high-temperature erosion performance of the resist stripping solution is improved.
Significantly improves the resistance of the resin film to highly polar organic reagents and resist stripping solutions, prevents pattern cracking, and improves bonding performance with metal to meet high resolution and heat resistance requirements in the semiconductor manufacturing and packaging fields. .
Smart Images

Figure PCTCN2023128139-APPB-I100001 
Figure PCTCN2023128139-APPB-I100002 
Figure PCTCN2023128139-APPB-I100003
Abstract
Description
A high chemical resistance positive photosensitive resin composition and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to a high-chemical-resistant positive photosensitive resin composition, a preparation method thereof, and an application thereof. Background Art
[0002] Photosensitive polyimide / polybenzoxazole resin solution has excellent photolithography processability, and the cured resin has the advantages of high heat resistance, high electrical insulation, high strength and toughness. It is widely used in chip surface passivation and interlayer insulation of multi-layer metal interconnect structures in the semiconductor manufacturing process, multi-layer wiring and bump / micro-solder ball manufacturing processes of advanced electronic packaging (BGA, CSP, SiP, etc.) substrates, stress buffer inner coating protective layer films for plastic-encapsulated circuits, and multi-layer wiring processes for optoelectronic display devices.
[0003] In order to meet the complex process requirements of semiconductor manufacturing, photosensitive polyimide / polybenzoxazole cured resin films are generally required to have excellent chemical resistance and excellent adhesion to the substrate. Although negative photosensitive polyimide has excellent chemical resistance and can withstand the erosion of high-temperature resist stripping solutions, the organic solvents used in its development process are not conducive to environmental protection, and the photolithography resolution is poor, which cannot meet the needs of high-resolution application scenarios in the advanced packaging field. Although positive photosensitive resins have high resolution, their chemical resistance is poor, which also limits their practical application. Currently, there are few reports on positive photosensitive resins with high chemical resistance. SUMMARY OF THE INVENTION
[0004] The present invention improves the residual stress of the cured film by adding an unsaturated bond-containing aliphatic flexible compound to a positive photosensitive resin composition, thereby increasing its resistance to high-temperature erosion by an anti-etching stripping solution, and in particular preventing cracking of rectangular patterns due to corner stress concentration. The present invention improves the chemical resistance of the cured resin film and is suitable for use in fields such as semiconductor manufacturing and packaging.
[0005] Specifically, the positive photosensitive resin composition of the present invention includes the following components in parts by mass: 100 parts of alkali-soluble resin; 3-40 parts of photosensitizer; 1-30 parts of aliphatic flexible compound containing unsaturated bonds; 1-30 parts of crosslinking agent and 100-1000 parts of organic solvent.
[0006] The unsaturated bond-containing aliphatic flexible compound refers to an aliphatic compound having two or more unsaturated olefinic bond groups in the molecule. Technical issues
[0007] The purpose of the present invention is to provide a highly chemical-resistant positive photosensitive resin composition, a preparation method and an application thereof. The polybenzoxazole resin film of the present invention has excellent tolerance to chemicals such as highly polar organic reagents and resist stripping solutions.
[0008] The present invention first provides a positive photosensitive resin composition, which includes the following components in parts by weight:
[0009] 100 parts of alkali-soluble resin; 3-40 parts of photosensitizer; 1-30 parts of aliphatic flexible compound containing unsaturated bonds; 1-30 parts of cross-linking agent and 100-1000 parts of organic solvent.
[0010] The positive photosensitive resin composition comprises the following components in parts by mass: 100 parts of an alkali-soluble resin; 8 to 15 parts of a photosensitizer; 10 to 15 parts of an aliphatic flexible compound containing an unsaturated bond; 2 to 8 parts of a crosslinking agent; and 100 to 250 parts of an organic solvent.
[0011] The positive photosensitive resin composition comprises the following components in parts by mass: 100 parts of an alkali-soluble resin; 12 parts of a photosensitizer; 10-15 parts of an aliphatic flexible compound containing an unsaturated bond; 5 parts of a crosslinking agent and 180 parts of an organic solvent.
[0012] In the above-mentioned positive photosensitive resin composition, the alkali-soluble resin is polymerized by components 1 and 2 in an organic solvent under the action of a capping agent; the alkali-soluble resin GPC weight-average molecular weight is 10,000 to 60,000, preferably 10,000 to 40,000. When the resin weight-average molecular weight is lower than 10,000, the mechanical properties and chemical resistance of the cured film are affected; when it is higher than 60,000, the photolithographic performance and processing performance are affected.
[0013] The component 1 is an aromatic diacyl chloride or a derivative thereof, which can be selected from at least one of diphenyl ether dicarboxyl chloride, isophthaloyl chloride, terephthaloyl chloride, biphenyl dicarboxyl chloride, diphenyl sulfone dicarboxyl chloride, diphenylmethane dicarboxyl chloride and benzophenone dicarboxyl chloride; more specifically, it can be 4,4'-diphenyl ether dicarboxyl chloride;
[0014] The component 2 is a phenolic hydroxyl-containing aromatic diamine, or a small amount of at least one of an aliphatic diamine, a phenolic hydroxyl-free aromatic diamine and a silicon-containing diamine is added to the phenolic hydroxyl-containing aromatic diamine to improve the mechanical properties, thermal properties and adhesion properties of the resin to the substrate; wherein the molar ratio of the total amount of the aliphatic diamine, the phenolic hydroxyl-free aromatic diamine and the silicon-containing diamine to the total diamine is not higher than 20%, otherwise it will affect the heat resistance of the cured film, the photosensitivity and storage stability of the resin composition and other properties.
[0015] The phenolic hydroxyl aromatic diamine is selected from 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methane, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 4,4'-di At least one of amino-3,3'-dihydroxydiphenyl ether, bis(3-amino-4-hydroxy)biphenyl, bis(3-amino-4-hydroxyphenyl)fluorene, 3,3'-diamino-4,4'-dihydroxybenzophenone, 4,4'-diamino-3,3'-dihydroxybenzophenone, 1,4-diamino-2,5-dihydroxybenzene, 1,3-diamino-2,4-dihydroxybenzene, and 1,3-diamino-4,6-dihydroxybenzene;
[0016] The aliphatic diamine refers to a linear aliphatic diamine having 2 to 20 carbon atoms, a cycloalkane diamine, or a linear aliphatic diamine having 2 to 20 carbon atoms and containing oxygen atoms in the structure; specifically, it can be selected from at least one of 1,4-butanediamine, hexanediamine, octanediamine, nonanediamine, decanediamine, dodecanediamine, 1,4-cyclohexanediamine, 1,3-cyclobutanediamine, 1,8-diamino-3,6-dioxaoctane, 4,7,10-trioxo-1,13-tridecanediamine, 4,9-dioxa-1,12-dodecanediamine, and ethylene glycol bis(3-aminopropyl) ether; specifically, it can be hexanediamine;
[0017] The aromatic diamine containing no phenolic hydroxyl group may be selected from 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl} At least one of 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, and 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl; specifically, 4,4'-diaminodiphenyl ether;
[0018] The silicon-containing diamine can be selected from 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminobutyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(2-aminoethyl)-1,1-dimethyl-3,3-diethyl-disiloxane, 1,5-bis(2-aminoethyl)-1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-bis(3-aminopropyl)-1,1,3,3,5,5-hexamethyltrisiloxane, 1-aminopropyl-5-aminoethyl-1,1 ,3,3,5,5-hexamethyltrisiloxane, 1,7-bis(2-aminoethyl)-1,1,3,3,5,5,7,7-octamethyltetrasiloxane, 1,3-bis(3-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminopropyl)-1,3-dimethyl-1,3-diphenyldisiloxane; specifically, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.
[0019] The end-capping agent is at least one of maleic anhydride, nadic anhydride, methylnadic anhydride, 4-ethynylphthalic anhydride, 4-phenylethynylphthalic anhydride, 4-vinylaniline, norbornenamine, allylamine, 4-ethynylaniline, 3-ethynylaniline, 3-phenylethynylaniline, 4-phenylethynylaniline, 4-(4-aminophenylethynyl)phenylacetylene, 4-[(trimethylsilyl)-ethynyl]aniline, 4-(4-amino-phenyl)-2-methyl-but-3-yn-2-ol, (E)-3-aminocinnamic acid and propargylamine; specifically, it can be nadic anhydride or 4-ethynylphthalic anhydride;
[0020] The organic solvent is N'N-dimethylformamide, N'N-dimethylacetamide, N-methyl-ε-caprolactam, N-methylpyrrolidone, γ-butyrolactone, ethyl lactate, 1,3-dimethyl-2-imidazolidinone, dimethyl sulfoxide, dimethyl sulfone, tetramethylene sulfone, tetramethyl urea, phenol, m-cresol, methyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, ethyl acetate, ethyl acetate At least one of butyl acrylate, sulfolane, p-cresol, 3-chlorophenol, 4-chlorophenol, tetrahydrofuran, ethyl 3-ethoxypropionate, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol monomethyl ether acetate; specifically, N-methylpyrrolidone.
[0021] In the above-mentioned positive photosensitive resin composition, the photosensitizer is at least one of a diazonaphthoquinone compound, an iodonium salt compound, and a sulfonium salt compound;
[0022] The diazonaphthoquinone compound is any one of the following 1) to 3): 1) a compound formed by an esterification reaction between a diazonaphthoquinone sulfonic acid and a polyhydroxy compound; 2) a compound formed by a sulfonylation reaction between a diazonaphthoquinone sulfonic acid and a polyamine compound; 3) a compound formed by an esterification and / or sulfonylation reaction between a diazonaphthoquinone sulfonic acid and a polyhydroxy polyamine compound; wherein the proportion of the polyhydroxy polyamine compound substituted by the diazonaphthoquinone sulfonic acid is 50% to 100%;
[0023] The naphthoquinone diazo compounds include 1,2-naphthoquinone diazo-5-sulfonyl compounds and / or 1,2-naphthoquinone diazo-4-sulfonyl compounds; the polyhydroxy compounds include Bis-Z, BisP-EZ, BisP-AP, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, Methylene tris-FR-CR, BisRS-26X, DML-MBPC, DML-MBOC, DML-OCHP, DML-PCHP, DML-PC, DML-PTBP, DML-34X, DML-EP, DML-POP, Dimethylol-BisOC -P, DML-PFP, DML-PSBP, DML-MTrisPC, TriML-P, TriML-35XL, TML-BP, TML-HQ, TML-PP-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP (these are trade names, available from Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (these are trade names, products of Asahi Organic Materials Industry Co., Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, 2,3,4-trihydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, pyrogallol acetone resin, m-cresol resin, and phenolic resin;
[0024] The iodonium salt compounds include bis(4-tert-butylphenyl)iodonium hexafluorophosphate, diphenyliodonium hexafluoroarsenate, diphenyliodonium hexafluorophosphate, 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nitrate, [4-(trifluoromethyl)phenyl](2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, [3-(trifluoromethyl)phenyl](2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, iodonium trifluoromethanesulfonate, [(4-trifluoromethyl)phenyl](2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, phenyl(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, phenyl[3-(trifluoromethyl)phenyl]iodonium trifluoromethanesulfonate, (4-nitrophenyl)(phenyl)iodonium trifluoromethanesulfonate, (4-tolyl)(2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, (3-tolyl) (2,4,6-Trimethylphenyl)iodonium trifluoromethanesulfonate, (2-methylphenyl)(2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate, [4-[(2-hydroxytetradecyl)oxy]phenyl]phenyliodonium hexafluoroantimonate, (5-fluoro-2-nitrophenyl)(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, diphenyliodonium hexafluorophosphate, Diphenyliodonium hexafluoroarsenate, (3,5-dichlorophenyl)(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, (3-bromophenyl)(mesityl)iodonium trifluoromethanesulfonate, [4-(bromomethyl)phenyl](2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, bis(2,4,6-trimethylpyridinium)iodonium hexafluorophosphate, 4,4'-ditolyliodonium hexafluorophosphate, and mixtures thereof in any proportion;
[0025] The sulfonium salt compounds include 1,3-benzodithiopyrrole tetrafluoroboron salt, cyclopropyldiphenylsulfonium tetrafluoroborate, dimethyl (methylthio) sulfonium tetrafluoroborate, diphenyl (methyl) sulfonium tetrafluoroborate, (difluoromethyl) bis (2,5-dimethylphenyl) sulfonium tetrafluoroborate, 2-[4-(3-ethoxy-2-hydroxypropoxy)phenylcarbamoyl] ethyl dimethylthio toluenesulfonate, 4-hydroxyphenyldimethylsulfonium methanesulfonate, triphenylsulfonium tetrafluoroborate, tri (4-tolyl) sulfonium hexafluorophosphate, tri (4-tolyl) sulfonium trifluoromethanesulfonate, triethylsulfonium bis (trifluoromethylsulfonyl) imide and mixtures thereof in any proportion.
[0026] More preferably, the photosensitizer is , wherein R is 1,2-naphthoquinonediazidesulfonyl and / or H.
[0027] In the positive photosensitive resin composition, the unsaturated bond-containing aliphatic flexible compound refers to an aliphatic compound having two or more unsaturated olefinic groups in the molecule; specifically, it may be any of the following:
[0028]
[0029] wherein R1, R2, R3, R4, R5 and R6 are all H or methyl; R7 is H, hydroxyl, alkyl or alkoxy; n1 is an integer from 1 to 10; n2 is an integer from 0 to 10;
[0030] Specifically, the alkyl group or alkoxy group is an alkyl group or alkoxy group having 1 to 6 carbon atoms;
[0031] The present invention improves the residual stress of the cured film and its resistance to high-temperature erosion of the resist stripping solution by adding an unsaturated bond-containing aliphatic flexible compound to the positive photosensitive resin composition, and can especially prevent the cracking of rectangular patterns caused by corner stress concentration.
[0032] The aliphatic flexible compound containing unsaturated bonds is preferably ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,3-propylene glycol diacrylate, 1,3-propylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,5-pentanediol diacrylate, 1,5-pentanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, 1,7-heptanediol diacrylate, 1,7-heptanediol dimethacrylate, 1,8-octanediol diacrylate, 1,8-octanediol dimethacrylate, 1,9-nonanediol diacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol diacrylate, 1,10-decanediol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, at least one of triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, pentaethylene glycol diacrylate, pentaethylene glycol dimethacrylate, hexaethylene glycol diacrylate, hexaethylene glycol dimethacrylate, polypropylene glycol dimethacrylate (degree of polymerization of 1-10), ethoxylated trimethylolpropane triacrylate, ethoxylated trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol tetramethacrylate, dipentaerythritol triacrylate, dipentaerythritol trimethacrylate, dipentaerythritol tetraacrylate, dipentaerythritol tetramethacrylate, dipentaerythritol pentaenoate, dipentaerythritol pentamethenoate, polydipentaerythritol hexaacrylate, polydipentaerythritol hexamethacrylate, and tris(2-hydroxyethyl)isocyanuric acid triacrylate;
[0033] More preferably, the unsaturated bond-containing aliphatic flexible compound is selected from any one of the following:
[0034]
[0035] In the above-mentioned positive photosensitive resin composition, the crosslinking agent refers to a compound that can undergo a crosslinking reaction under heating conditions or under the action of a Lewis acid, including a compound containing an epoxy group, a compound containing a hydroxymethyl group or an alkoxymethyl group, etc.;
[0036] The epoxy group-containing compound includes any one of bisphenol A epoxy resin, bisphenol F epoxy resin, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polymethyl (glycidyloxypropyl) and epoxy group-containing silicone; more preferably 3,3'-[oxybismethylene]bis[3-ethyl]oxetane, 1,4-butanediol diglycidyl ether, 2,2-bis(4-epoxypropyloxyphenyl)propane, 9,9-bis(4-epoxypropyloxy-3-methylphenyl)fluorene, 9,9-bis(4-epoxypropyloxyphenyl)fluorene, 1,3-bis[2-(7-oxabicyclo[4.1.0]hept-3-yl)ethyl]-1,1,3,3-tetramethyldisiloxane, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, 1,2,7,8-diepoxyoctane, 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, triglycidyl isocyanurate, 4,4'-methylenebis(N,N-dicyclopropyloxyaniline), neopentyl glycol diglycidyl ether, 2,2'-(2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl)bis(ethylene oxide), pentaerythritol diglycidyl ether, vinylcyclohexene diglycidyl ether, polyethylene glycol diglycidyl ether ( degree of polymerization of 1-15), polypropylene glycol diglycidyl ether (degree of polymerization of 1-15), polydimethylsiloxane diglycidyl ether (degree of polymerization of 1-15), butanediol diglycidyl ether, diglycidyl aniline, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, 5,5-dimethyl-1,3-bis(oxiranylmethyl)imidazolidine-2,4-dione, 2,2',2''-[methylene-tris(phenyleneoxymethylene)]tri(oxirane), 1,1,1-tris(4-hydroxyphenyl)ethyl triglycidyl ether, bis(2,3-epoxycyclopentyl) ether, 3 ,4-epoxy-6-methylcyclohexylcarboxylic acid-3',4'-epoxy-6'-methylcyclohexyl methyl ester, vinylcyclohexene and epoxy compound, 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, diisoprene diepoxide, tetraphenyl glycidyl ether ethane, triphenyl glycidyl ether methane, triglycidyl-p-aminophenol, triglycidyl triisocyanate, tetraglycidyl diaminodiphenylmethane, tetraglycidyl xylenediamine or tetraglycidyl-1,3-bisaminomethylcyclohexane; products with trade names include H P-850, HP-4032, HP-7200, HP-820, HP-4700, EXA-4710, HP-4770, EXA-859CRP, EXA-1514, EXA-4880, EXA-4850-150, EXA-4850-1000, EXA-4816, EXA-4822, BEO-60E, BPO-20E, HBE-100, DME-100, NC-3000, NC-6000 (Nippon Kayaku Co., Ltd.), and mixtures thereof in any proportion.
[0037] The compounds containing hydroxymethyl or alkoxymethyl include 46DMOC, 46DMOEP (the above are trade names, manufactured by Asahi Organic Materials Industry Co., Ltd.), DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DMLMBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DMLBisOC-P, DMOM-PC, DMOMPTBP, DMOM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML -pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPA, HMOM-TPHAP (these are trade names, available from Honshu Chemical Industry Co., Ltd.), "NIKALAC" MX-290, "NIKALAC" MX-280, "NIKALAC" MX-270, "NIKALAC" MX-279, "NIKALAC" MW-100LM, "NIKALAC" MX-750LM (Sanwa Chemical Co., Ltd.), and mixtures thereof in any proportion.
[0038] More preferably, the cross-linking agent is any one of the following:
[0039]
[0040] In the positive photosensitive resin composition, the organic solvent is at least one of N-methylpyrrolidone, N,N'-dimethylacetamide, N,N'-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, ethyl acetate, butyl acetate, n-propyl acetate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate;
[0041] Specifically, the organic solvent consists of γ-butyrolactone (GBL) and propylene glycol methyl ether acetate (PGEMA); more specifically, the mass ratio of GBL to PGEMA is 9:1.
[0042] The positive photosensitive resin composition further comprises, in addition to the above components, 0.1 to 20 parts by weight of other components, including at least one of an adhesion promoter and a development inhibitor;
[0043] Preferably, the other components are adhesion promoters and development inhibitors.
[0044] In the positive photosensitive resin composition, the adhesion promoter can be selected from γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptomethyltrimethoxysilane, 3-mercaptomethyldimethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyltributoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, Alkane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexane)ethyltriethoxysilane, epoxybutyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, p-aminophenyltrimethoxysilane, aminophenyltrimethoxysilane, 3-(m-aminophenoxy)trimethoxysilane, 3-methacryloyloxypropyldimethoxymethylsilane, 3- Methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acetoxypropyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldiethoxysilane, vinyltriethoxysilane, hydroxymethyltrimethoxysilane, hydroxymethyltriethoxysilane, 2-hydroxyethyltrimethoxysilane, 2-hydroxyethyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 4- At least one of hydroxybutyltrimethoxysilane, 4-hydroxybutyltriethoxysilane, 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane, 3-[bis(2-hydroxyethyl)amino]propane-trimethoxysilane, isocyanatepropyltrimethoxysilane, isocyanatepropyltriethoxysilane, 3-isothiocyanatopropyltrimethoxysilane, 3-isothiocyanatopropyltriethoxysilane, 2-cyanoethyltrimethoxysilane, 2-cyanoethyltriethoxysilane, and 3-piperazinylpropylmethyldimethoxysilane;
[0045] More preferably, the adhesion promoter is any one of the following: .
[0046] The mass ratio of the adhesion promoter to the alkali-soluble resin is 1 to 20:100, and can be specifically 3:100.
[0047] The development inhibitor is a compound that can inhibit the dissolution of a positive photosensitive resin in an alkaline aqueous solution after exposure, thereby helping to adjust film retention and development time. The development inhibitor is selected from at least one of diphenyliodonium nitrate, bis(p-tert-butylphenyl)iodonium nitrate, diphenyliodonium bromide, diphenyliodonium chloride, and diphenyliodonium iodide; preferably, diphenyliodonium nitrate.
[0048] The mass ratio of the development inhibitor to the alkali-soluble resin is 0.1 to 20:100, and can be specifically 2 to 3:100.
[0049] The positive photosensitive resin composition is composed of the following components in parts by mass: 100 parts of an alkali-soluble resin; 3 to 40 parts of a photosensitizer; 1 to 30 parts of an aliphatic flexible compound containing an unsaturated bond; 1 to 20 parts of an adhesion promoter; 0.1 to 20 parts of a development inhibitor; 1 to 30 parts of a crosslinking agent; and 100 to 1000 parts of an organic solvent.
[0050] The present invention also provides a method for preparing the positive photosensitive resin composition, comprising the following steps:
[0051] (1) mixing the alkali-soluble resin with the organic solvent, and stirring in a yellow light region under nitrogen protection to form a homogeneous solution;
[0052] (2) Adding the photosensitizer, the unsaturated bond-containing aliphatic flexible compound, the crosslinking agent and / or the other components to the homogeneous solution of step (1) and mixing to form a homogeneous solution; adding the organic solvent to adjust the solution viscosity, and filtering to obtain the positive photosensitive resin composition.
[0053] The present invention further provides a patterned polybenzoxazole resin film, which is obtained by coating, exposing, developing and curing the positive photosensitive resin composition.
[0054] Specifically, the method for preparing the patterned polybenzoxazole resin film comprises the following steps:
[0055] 1) coating the positive photosensitive resin composition on a wafer substrate to obtain a liquid adhesive film;
[0056] 2) Bake at 80-130°C for 1-30 minutes to obtain a solid film;
[0057] 3) Cover the mask and expose using ultraviolet i-line or (i-line and g-line) exposure equipment;
[0058] 4) Develop with a developer to dissolve and remove the exposed area;
[0059] 5) washing with a rinse solution to obtain an uncured patterned resin film;
[0060] 6) heating and curing the uncured patterned resin film to convert it into a patterned polybenzoxazole resin film.
[0061] In the above method, the developer and rinse solution are conventional additives in the prior art. The developer is preferably an aqueous solution of an alkaline compound such as tetramethylammonium hydroxide, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, choline hydroxide, diethanolamine, diethylaminoethanol, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and 1,6-hexanediamine. The rinse solution is preferably water or an aqueous solution containing an alcohol such as methanol, ethanol, or isopropyl alcohol, or an ester such as ethyl lactate or propylene glycol monomethyl ether acetate. Beneficial effects
[0062] The patterned polybenzoxazole resin film of the present invention has excellent tolerance to chemicals such as highly polar organic reagents and resist stripping solutions; it also has excellent adhesion to metals Cu and Au. In addition, it has high resolution, low water absorption, and excellent mechanical properties, heat resistance, and dielectric properties. Its main properties are shown in Table 1.
[0063] BRIEF DESCRIPTION OF THE DRAWINGS
[0064] FIG1 is a FIB pattern obtained by immersing the positive photosensitive resin composition solution provided by Experimental Group 1 in a DMSO / MEA (3 / 7) solution at 85° C. for 60 minutes after the stereolithographic pattern was obtained by photolithographic development and curing.
[0065] FIG2 is a FIB pattern obtained by immersing the stereolithographic pattern obtained by photolithographic development and curing of the positive photosensitive resin composition solution provided by Control Group 1 in a DMSO / MEA (3 / 7) solution at 85° C. for 60 minutes. Modes for Carrying Out the Invention
[0066] The present invention is described in further detail below in conjunction with specific embodiments. The examples provided are only for illustrating the present invention, not for limiting the scope of the invention. The experimental methods in the following examples are conventional methods unless otherwise specified. The materials, reagents, instruments, etc. used in the following examples are all commercially available unless otherwise specified. The quantitative tests in the following examples were performed in triplicate, and the results were averaged.
[0067] The test or evaluation methods for each performance index in the following embodiments are as follows:
[0068] (1) Molecular weight test
[0069] The weight-average molecular weight was determined by GPC using PS as the standard. An NMP solution containing LiBr (0.03 mol / L) and H3PO4 (0.06 mol / L) was used as the eluent, and the polymer concentration was 1 mg / mL.
[0070] (2) Lithography performance evaluation
[0071] A. Film retention rate
[0072] A positive photosensitive resin composition solution was spin-coated onto a 6-inch Si wafer. Pre-baking was performed at 80-130°C for 1-30 minutes to obtain an 8-10 μm solid film. A mask was placed on the surface and exposed using an ultraviolet (i-ray) exposure device. Development was then performed using a 2.38 wt% aqueous solution of tetramethylammonium hydroxide. After rinsing with deionized water, an uncured patterned resin film was obtained. The film thickness of the unexposed portion after development was measured using an optical interferometer. The film retention rate was calculated by comparing the thickness of the unexposed portion to the pre-development thickness.
[0073] B. Resolution and Sensitivity
[0074] Use an optical microscope to observe the pattern with L / S = 10μm / 10μm after development. The development time when the pattern edge is smooth and there is no scum is set as the benchmark. The minimum pattern size that can be observed under this benchmark is set as the resolution L / S (μm). The minimum exposure energy required for this resolution is the sensitivity (mJ / mm2).
[0075] (3) Chemical resistance evaluation
[0076] A positive photosensitive resin composition solution was spin-coated onto a 6-inch silicon wafer and heated at 80-130°C for 1-30 minutes to form a solid film. A mask was placed on the surface and exposed using a UV i-ray exposure device. The film was then developed with a 2.38wt% tetramethylammonium hydroxide aqueous solution and rinsed with deionized water to produce an uncured positive resin pattern. The silicon wafer with the resin pattern was then cured in a nitrogen-protected forced-air oven (oxygen concentration below 100 ppm) at 150°C for 30 minutes, then heated to 350°C for 1 hour, resulting in a 10μm-thick stereolithographic pattern. The patterned silicon wafers were immersed in the organic reagents acetone, N-methylpyrrolidone (NMP), and 2.38% tetramethylammonium hydroxide (TMAH) aqueous solution at RT for 30 minutes, immersed in the resist stripping liquid dimethyl sulfoxide (DMSO) / monoethanolamine (MEA) solution (mass ratio 3 / 7) at 85°C for 60 minutes, immersed in dimethyl sulfoxide (DMSO) / monoethanolamine (MEA) (mass ratio 9 / 1) at 90°C for 30 minutes, and immersed in NMP / DMSO (mass ratio 1 / 1) at 90°C for 30 minutes. Then, after water washing and air drying, the change in film thickness before and after immersion of the patterned silicon wafers was measured with a film thickness meter. The 50μm square holes were observed with an optical microscope to evaluate their chemical resistance.
[0077] The chemical resistance was evaluated as A when the film thickness change before and after immersion was less than ±5%. The chemical resistance was evaluated as B when the film thickness change before and after immersion was greater than ±5% and less than ±10%. The chemical resistance was evaluated as C when cracks occurred on the film surface, cracks occurred at the pattern corners, the chemical penetrated the pattern edge, or the cured film peeled off from the substrate.
[0078] (4) Adhesion evaluation
[0079] A positive photosensitive resin composition solution was spin-coated onto a 6-inch wafer sputtered with 100nm thick Cu and Au layers (hereinafter referred to as the Cu and Au substrates). The films were cured in a nitrogen-protected forced-air oven at 150°C for 30 minutes, followed by curing at 350°C for 1 hour to produce cured films. The films were then aged in an aging oven using Uhast 96 (130°C / 85% RH / 96 hours). Following the national standard "GB / T 9286-1998 Cross-cut Test for Paint and Varnish Films," the cured films were cross-cut with a cutter to create a 10-row x 10-column grid. A peel test was then performed using specialized 3M tape, with the number of squares peeled off recorded as "X / 100," with "X" representing the total number of squares peeled off. Adhesion was evaluated as good if no more than 5 squares were peeled off on either substrate. Adhesion was evaluated as poor if more than 5 squares were peeled off on either substrate.
[0080] Example 1
[0081] In a 1L three-necked round-bottom flask equipped with a mechanical stirrer, a thermometer, and a nitrogen protection device, 36.63g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 146.5g of NMP were added sequentially and stirred to dissolve to form a homogeneous transparent diamine solution. The solution was cooled to below 5°C in an ice bath. A mixed solution of 4,4'-diphenyl ether dicarbonyl chloride (25.97g) and NMP (103.9g) was added dropwise to the diamine solution while stirring for 0.5h. The solution was then allowed to react at room temperature for 3h. 3.94g of nadic anhydride was then added and stirring continued for 1h. The reaction solution was poured into 5L of deionized water, the precipitated solid was filtered, and vacuum dried to obtain polybenzoxazole precursor resin A1. GPC analysis showed a weight-average molecular weight Mw = 17800 and a molecular weight distribution of 1.60.
[0082] Example 2
[0083] In a 1L three-necked round-bottom flask equipped with a mechanical stirrer, a thermometer, and a nitrogen protection device, 32.96g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1.16g of hexamethylenediamine, and 136g of NMP were added in sequence and stirred to dissolve to form a homogeneous transparent diamine solution. The solution was cooled to below 5°C in an ice bath, and a mixed solution of 4,4'-diphenylether dicarbonyl chloride (25.97g) and NMP (103.9g) was added dropwise to the diamine solution while stirring for 0.5h. The reaction was then allowed to proceed at room temperature for 3h. 3.94g of nadic anhydride was then added and stirring continued for 1h. The reaction solution was poured into 5L of deionized water, the precipitated solid was filtered, and vacuum dried to obtain polybenzoxazole precursor resin A2. GPC analysis showed a weight-average molecular weight (Mw) of 18800 and a molecular weight distribution (MDD) of 1.78.
[0084] Example 3
[0085] In a 1L three-necked round-bottom flask equipped with a mechanical stirrer, a thermometer, and a nitrogen protection device, 29.30g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1.74g of hexamethylenediamine, 1.24g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, and 139g of NMP were added in sequence and stirred to dissolve to form a homogeneous transparent diamine solution; the solution was cooled to below 5°C in an ice bath, and a mixed solution of 4,4'-diphenylether dicarbonyl chloride (25.97g) and NMP (103.9g) was added dropwise to the diamine solution while stirring for 0.5h; then, the mixture was reacted at room temperature for 3h; and 4.13g of 4-Ethynylphthalic anhydride, and continue stirring for 1 hour; the reaction solution is poured into 5 L of deionized water, the precipitated solid is filtered, and vacuum dried to obtain polybenzoxazole precursor resin A3. GPC test shows a weight average molecular weight Mw=18300 and a molecular weight distribution of 1.84.
[0086] Example 4
[0087] In a 1L three-necked round-bottom flask equipped with a mechanical stirrer, a thermometer, and a nitrogen protection device, 32.96g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1.00g of 4,4'-diaminodiphenyl ether, 1.24g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, and 141g of NMP were added in sequence and stirred to dissolve to form a homogeneous transparent diamine solution; the solution was cooled to below 5°C in an ice bath, and a mixed solution of 4,4'-diphenyl ether dicarbonyl chloride (25.97g) and NMP (103.9g) was added dropwise to the diamine solution while stirring for 0.5h; then, the mixture was reacted at room temperature for 3h; and 4.13g of 4-ethynylphthalic anhydride, and continue stirring for 1 hour; the reaction solution is poured into 5 L of deionized water, the precipitated solid is filtered, and vacuum dried to obtain polybenzoxazole precursor resin A4. GPC test shows a weight average molecular weight Mw=17500 and a molecular weight distribution of 1.70.
[0088] Example 5
[0089] A polybenzoxazole precursor resin and solvent G (solvent G is a mixture of γ-butyrolactone (GBL) and propylene glycol methyl ether acetate (PGMEA) in a mass ratio of 9 / 1) were mixed in the amounts specified in Table 2 below, and stirred under nitrogen protection in a yellow light zone to form a homogeneous solution. Subsequently, an aliphatic flexible compound containing an unsaturated bond (hereinafter referred to as the "flexible component"), a photosensitizer, a crosslinker, and other components (adhesion promoter, development inhibitor) were added to the above solution and mixed to form a homogeneous solution. Solvent G was then added to adjust the solution viscosity, and the solution was filtered through a 0.5 μm pore size filter to obtain a positive photosensitive resin composition solution.
[0090] Aliphatic flexible compounds containing unsaturated bonds:
[0091]
[0092] Flexible components used in the control group:
[0093]
[0094] Among them, B7 viscosity is 900~1300cps, and B8 average Mn is 640.
[0095] Photosensitizer C:
[0096]
[0097] Crosslinking agent:
[0098]
[0099] Adhesion promoter:
[0100]
[0101] Development inhibitor F is diphenyliodonium nitrate.
[0102]
[0103] Note: In Table 2, parentheses represent the amount (parts by mass) added per 100 parts by weight of the benzoxazole precursor resin.
[0104] The experimental groups 1 to 12 and the control groups 1 to 6 were evaluated according to the chemical resistance evaluation method. The evaluation results are listed in Table 3.
[0105]
[0106] The chemical resistance evaluation results for experimental groups 1-12 and control groups 1-6 indicate that the patterned resin films prepared from the positive photosensitive resin composition of the present invention not only withstand room-temperature etching with highly polar organic reagents but also withstand high-temperature etching with resist stripping solutions, demonstrating outstanding chemical resistance. Control groups 1-2 and 5-6 exhibited poor resistance to high-temperature etching with resist stripping solutions, while control group 3-4 exhibited poor resistance to both room-temperature and high-temperature etching with organic reagents. This demonstrates that the combined use of an unsaturated bond-containing aliphatic flexible compound and a crosslinker significantly improves the chemical resistance of the cured film.
[0107] FIG1 is a FIB pattern obtained by immersing the positive photosensitive resin composition solution provided by Experimental Group 1 in a DMSO / MEA (3 / 7) solution at 85° C. for 60 minutes after the stereolithographic pattern was obtained by photolithographic development and curing.
[0108] Figure 2 shows a stereolithographic pattern obtained by photolithographic development and curing using the positive photosensitive resin composition solution provided in Control Group 1, then immersed in a DMSO / MEA (3 / 7) solution at 85°C for 60 minutes. Figures 1 and 2 demonstrate that the addition of an unsaturated aliphatic flexible compound to the polybenzoxazole precursor resin composition significantly improves the chemical resistance of the patterned resin film.
[0109] The experimental groups 1 to 12 and the control groups 1 to 6 were evaluated according to the adhesion performance evaluation method. The evaluation results are listed in Table 4.
[0110]
[0111] As can be seen from Table 4, the positive photosensitive resin composition of the present invention (experimental groups 1 to 12) has good adhesion to metal Cu and Au, while the comparative examples 2, 5 and 6 have poor adhesion to Au, indicating that the aliphatic flexible compound containing an unsaturated bond can enhance the adhesion to Au.
[0112] In summary, the most prominent feature of the positive photosensitive resin composition of the present invention is that the resin film formed after exposure, development, and thermal curing has excellent tolerance to chemicals such as strongly polar organic reagents and resist stripping solutions, and has excellent bonding properties with metals Cu and Au. In addition, it has high resolution, low water absorption, excellent mechanical properties, heat resistance, and dielectric properties, and has excellent comprehensive performance, which can meet the use requirements in the semiconductor manufacturing and packaging fields. Industrial Applicability
[0113] The patterned polybenzoxazole resin film of the present invention can be used as a surface protection film, a passivation film, a stress buffer layer for bump production, etc. of a chip during semiconductor manufacturing, and has good application prospects.
Claims
1. A positive photosensitive resin composition, Features: The positive photosensitive resin composition comprises the following components in parts by mass: 100 parts of alkali-soluble resin; 3-40 parts of photosensitizer; 1-30 parts of aliphatic flexible compounds containing unsaturated bonds; 1-30 parts of crosslinking agents and 100-1000 parts of organic solvents.
2. The positive photosensitive resin composition according to claim 1, Features: The alkali-soluble resin is polymerized by component 1 and component 2 in an organic solvent under the action of a capping agent; The component 1 is an aromatic diacid chloride or a derivative thereof; The component 2 is a phenolic hydroxyl-containing aromatic diamine, or at least one of an aliphatic diamine, a non-phenolic hydroxyl-containing aromatic diamine and a silicon-containing diamine is added to the phenolic hydroxyl-containing aromatic diamine; The alkali-soluble resin GPC weight average molecular weight is 10,000-60,000.
3. The positive photosensitive resin composition according to claim 2, Features: The component 1 is selected from at least one of diphenyl ether dicarboxyl chloride, isophthaloyl chloride, terephthaloyl chloride, biphenyl dicarboxyl chloride, diphenyl sulfone dicarboxyl chloride, diphenylmethane dicarboxyl chloride and benzophenone dicarboxyl chloride; The molar ratio of the total amount of the aliphatic diamine, the aromatic diamine without phenolic hydroxyl group and the silicon-containing diamine to the total diamine is not higher than 20%; The phenolic hydroxyl-containing aromatic diamine is selected from 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methane, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 4,4'-di At least one of amino-3,3'-dihydroxydiphenyl ether, bis(3-amino-4-hydroxy)biphenyl, bis(3-amino-4-hydroxyphenyl)fluorene, 3,3'-diamino-4,4'-dihydroxybenzophenone, 4,4'-diamino-3,3'-dihydroxybenzophenone, 1,4-diamino-2,5-dihydroxybenzene, 1,3-diamino-2,4-dihydroxybenzene and 1,3-diamino-4,6-dihydroxybenzene; The aliphatic diamine refers to a straight-chain aliphatic diamine with 2 to 20 carbon atoms, a cycloalkane diamine, or a straight-chain aliphatic diamine with 2 to 20 carbon atoms containing an oxygen atom in the structure; The aromatic diamine containing no phenolic hydroxyl group is selected from 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis(4-aminophenoxy)benzene, At least one of {4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, and 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl; The silicon-containing diamine is selected from 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminobutyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(2-aminoethyl)-1,1-dimethyl-3,3-diethyl-disiloxane, 1,5-bis(2-aminoethyl)-1,1,3,3,5,5-hexamethyltrisiloxane, 1,5-bis(3-aminopropyl)-1,1,3,3,5,5-hexamethyltrisiloxane, At least one of 1-aminopropyl-5-aminoethyl-1,1,3,3,5,5-hexamethyltrisiloxane, 1,7-bis(2-aminoethyl)-1,1,3,3,5,5,7,7-octamethyltetrasiloxane, 1,3-bis(3-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminophenyl)-1,1,3,3-tetramethyldisiloxane, and 1,3-bis(3-aminopropyl)-1,3-dimethyl-1,3-diphenyldisiloxane; The end-capping agent is selected from at least one of maleic anhydride, nadic anhydride, methylnadic anhydride, 4-ethynylphthalic anhydride, 4-phenylethynylphthalic anhydride, 4-vinylaniline, naphthaleneamine, allylamine, 4-ethynylaniline, 3-ethynylaniline, 3-phenylethynylaniline, 4-phenylethynylaniline, 4-(4-aminophenylethynyl)phenylethynyl, 4-[(trimethylsilyl)-ethynyl]aniline, 4-(4-amino-phenyl)-2-methyl-but-3-yn-2-ol, (E)-3-aminocinnamic acid and propargylamine; The organic solvent is selected from N'N-dimethylformamide, N'N-dimethylacetamide, N-methyl-ε-caprolactam, N-methylpyrrolidone, γ-butyrolactone, ethyl lactate, 1,3-dimethyl-2-imidazolidinone, dimethyl sulfoxide, dimethyl sulfone, tetramethylene sulfone, tetramethyl urea, phenol, m-cresol, methyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone , ethyl acetate, butyl acetate, cyclopentane, p-cresol, 3-chlorophenol, 4-chlorophenol, tetrahydrofuran, ethyl 3-ethoxypropionate, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol monomethyl ether acetate.
4. The positive photosensitive resin composition according to claim 1, Features: The photosensitizer is at least one of a diazonaphthoquinone compound, an iodonium salt compound, and a sulfonium salt compound; The unsaturated bond-containing aliphatic flexible compound refers to an aliphatic compound having two or more unsaturated olefinic bond groups in the molecule; The cross-linking agent refers to a compound that can undergo a cross-linking reaction under heating conditions or under the action of a Lewis acid; The organic solvent is selected from at least one of N-methylpyrrolidone, N,N'-dimethylacetamide, N,N'-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, ethyl acetate, butyl acetate, n-propyl acetate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, toluene, xylene, mesitylene, diacetone alcohol, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, methyl propyl ketone, tetrahydrofuran, tetrahydropyran, dioxane, dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol monomethyl ether acetate.
5. The positive photosensitive resin composition according to claim 1, Features: The positive photosensitive resin composition further comprises 0.1 to 20 parts by weight of other components; The other components include at least one of an adhesion promoter and a development inhibitor; The mass ratio of the adhesion promoter to the alkali-soluble resin is 1-20:100; The mass ratio of the development inhibitor to the alkali-soluble resin is 0.1-20:
100.
6. The positive photosensitive resin composition according to claim 5, Features: The adhesion promoter is selected from γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, 3-mercaptopropyl trimethoxysilane, 3-mercaptopropyl triethoxysilane, 3-mercaptopropyl methyl dimethoxysilane, 3-mercaptomethyl trimethoxysilane, 3-mercaptomethyl dimethoxysilane, 3-mercaptopropyl ethoxy dimethoxysilane, 3-mercaptopropyl tripropoxysilane, 3-mercaptopropyl tributoxysilane, 3-ureidopropyl trimethoxysilane, 3-ureidopropyl triethoxysilane, γ-glycidyl ether oxypropyl trimethoxysilane, gamma-glycidyloxypropyl triethoxysilane, 2-(3,4-epoxycyclohexane)ethyl trimethoxysilane, 2-(3,4-epoxycyclohexane)ethyl triethoxysilane, epoxybutyl trimethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane, p-aminophenyl trimethoxysilane, aminophenyl trimethoxysilane, 3-(m-aminophenoxy) trimethoxysilane, 3-methacryloxypropyl dimethoxymethylsilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-acetoxypropyl trimethoxysilane, vinyl trimethoxysilane, vinyl methyl diethoxysilane, vinyl triethoxysilane, hydroxymethyl trimethoxysilane, hydroxymethyl triethoxysilane, 2-hydroxyethyl trimethoxysilane, 2-hydroxyethyl triethoxysilane, 3-hydroxypropyl trimethoxysilane, 3-hydroxypropyl triethoxysilane, 4-hydroxybutyl at least one of trimethoxysilane, 4-hydroxybutyltriethoxysilane, 3-[bis(2-hydroxyethyl)amino]propane-triethoxysilane, 3-[bis(2-hydroxyethyl)amino]propane-trimethoxysilane, isocyanatepropyltrimethoxysilane, isocyanatepropyltriethoxysilane, 3-isothiocyanatopropyltrimethoxysilane, 3-isothiocyanatopropyltriethoxysilane, 2-cyanoethyltrimethoxysilane, 2-cyanoethyltriethoxysilane and 3-piperazinylpropylmethyldimethoxysilane; The development inhibitor refers to a compound that can hinder the dissolution of a positive photosensitive resin in an alkaline aqueous solution after exposure and helps to adjust the film retention rate and the development time, and is selected from at least one of diphenyliodonium nitrate, bis(p-tert-butylphenyl)iodonium nitrate, diphenyliodonium bromide, diphenyliodonium chloride and diphenyliodonium iodide.
7. The positive photosensitive resin composition according to claim 6, Features: The adhesion promoter is any of the following: ; The development inhibitor is diphenyliodonium nitrate.
8. The positive photosensitive resin composition according to claim 1, Features: The unsaturated bond-containing aliphatic flexible compound is selected from any one of the following structures: ; The cross-linking agent is any of the following: ; The photosensitizer is , wherein R is 1,2-naphthoquinonediazidesulfonyl and / or H; The organic solvent consists of gamma-butyrolactone and propylene glycol methyl ether acetate.
9. A method for preparing a positive photosensitive resin composition according to any one of claims 1 to 8, Features: The method comprises the following steps: (1) mixing the alkali-soluble resin with the organic solvent, and stirring in a yellow light region under nitrogen protection to form a homogeneous solution; (2) adding the photosensitizer, the unsaturated bond-containing aliphatic flexible compound, the crosslinking agent and / or the other components to the homogeneous solution of step (1) to form a homogeneous solution; adding the organic solvent to adjust the solution viscosity, and filtering to obtain the positive photosensitive resin composition.
10. A patterned polybenzoxazole resin film, Features: The patterned polybenzoxazole resin film is obtained by coating, exposing, developing and curing the positive photosensitive resin composition according to any one of claims 1 to 8.
11. The patterned polybenzoxazole resin film according to claim 10, Features: The method for preparing the patterned polybenzoxazole resin film comprises the following steps: 1) coating the positive photosensitive resin composition according to any one of claims 1 to 8 on a wafer substrate to obtain a liquid adhesive film; 2) Bake at 80-130°C for 1-30 min to obtain a solid film; 3) Cover the mask and use ultraviolet i-line or (i-line and g-line) exposure equipment for exposure; 4) Develop with a developer to dissolve and remove the exposed area; 5) washing with a rinse solution to obtain an uncured patterned resin film; 6) The uncured patterned resin film is heated and cured to be converted into a patterned polybenzoxazole resin film.
12. Use of the positive photosensitive resin composition according to any one of claims 1 to 8 in semiconductor manufacturing and / or packaging.
Citation Information
Patent Citations
Positive-type photosensitive resin compositions
CA2114461A1
High toughness, high heat resistance and weak alkaline wat developable polyimide / photosensitive epoxy acrylic resin composition
CN109270792A
Chemical amplification type positive photosensitive polyimide coating adhesive as well as preparation method and application thereof
CN114874441A
Positive photosensitive resin composition and preparation method and application thereof
CN115220305A
Positive photosensitive resin composition with high chemical resistance as well as preparation method and application of positive photosensitive resin composition
CN116149140A
Cited By
Alkali-soluble polyimide precursor, preparation method thereof and positive photosensitive resin composition