Composite separator, and preparation method therefor and use thereof
By using fullerene materials as modified layers in lithium-ion battery separators, combined with doping and modification technologies, the problem of lightening the separators is solved, the mechanical properties and heat resistance are improved, and the overall performance of the separators is improved. .
Patent Information
- Application Number
- PCT/CN2023/131555
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-11-14
- Publication Date
- 2024-10-24
AI Technical Summary
It is difficult for existing lithium-ion battery separators to achieve lightweighting while ensuring mechanical properties and heat resistance, and reducing the thickness of the separator will affect the balance of other properties.
Fullerene material is used as the modified layer, which is placed between the base film layers through lamination. It is combined with doping heteroatoms, modified organic functional groups, composite inorganic materials and pore-making processing to form a layer with excellent mechanical rigidity, ions and electrons. Composite separator for electrical conductivity.
The mechanical properties, heat resistance and ionic conductivity of the composite separator are improved, and the lightweight design of the separator is achieved while maintaining the stability and performance of the battery.
Smart Images

Figure CN2023131555_24102024_PF_FP_ABST
Abstract
Description
Composite diaphragm and its preparation method and application
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 17, 2023, with application number 202310409508.6 and invention name “Composite diaphragm and its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of battery technology, and in particular to a composite diaphragm and a preparation method and application thereof. Background Art
[0003] With the continuous advancement and development of lithium-ion battery technology, it has been applied in a variety of fields, including digital electronics, energy storage, power, and new energy vehicles. Lithium-ion batteries inherently offer advantages such as light weight, high energy density, and excellent high-rate charge and discharge performance, but further improvements in performance and safety are still desired. One key factor influencing the performance and safety of lithium-ion batteries is the quality of their electrode materials; another is the battery separator. A separator is a porous, electrically insulating film that separates the positive and negative electrodes of a battery, preventing electrons from freely passing through while allowing ions to pass freely between the positive and negative electrodes. As a key component of lithium-ion batteries, the performance of the separator determines the battery's interface structure and internal resistance, directly impacting characteristics such as capacity, cycling, and safety. High-performance separators are crucial for improving a battery's overall performance. Therefore, the development of high-performance separators has become a key area for improving lithium-ion battery performance, with separator safety being a particular focus.
[0004] Currently, high-performance battery separators must not only possess excellent electrical insulation, high ion permeability, good mechanical properties, solvent resistance, high temperature resistance, and high wettability, but also reduce the separator's own weight, which plays a significant role in increasing the energy density of the battery cell and facilitating lightweighting. However, reducing the separator's thickness makes it difficult to balance the separator's mechanical properties, heat resistance, and other properties. Technical issues
[0005] One of the purposes of the embodiments of the present application is to provide a composite diaphragm to solve the technical problem that it is difficult to achieve lightweight while ensuring the performance of the diaphragm. Technical Solutions
[0006] The technical solution adopted in the embodiment of this application is:
[0007] In a first aspect, a composite membrane is provided, comprising a plurality of laminated base membrane layers and at least one modified layer disposed between two adjacent base membrane layers; the raw material components of the modified layer include fullerene materials.
[0008] In some embodiments, the raw material components of the modified layer include fullerenes modified by at least one of doping with heteroatoms, modifying organic functional groups, composite inorganic materials, and pore-forming treatment.
[0009] In some embodiments, the thickness of the modified layer is no greater than 5 μm.
[0010] In some embodiments, the thickness of the modified layer is no greater than 3 μm.
[0011] In some embodiments, the modified layer has a thickness of 0.5 μm to 2 μm.
[0012] In some embodiments, the base film layer has a thickness of 3 μm to 7 μm.
[0013] In some embodiments, the heteroatom includes a non-metallic element from Groups IIIA to VIA.
[0014] In some embodiments, the heteroatom includes at least one of N, S, O, B, and P.
[0015] In some embodiments, the organic functional group includes at least one of a pyrrole group, a thiophene group, and an aniline group.
[0016] In some embodiments, the inorganic material comprises a metal oxide.
[0017] In some embodiments, the inorganic material includes at least one of MoO2, MgO, and Al2O3.
[0018] In some embodiments, the pore-forming treatment comprises at least one of a pore-forming agent, chemical etching, and a template method.
[0019] In some embodiments, the average particle size of the fullerene material is 0.1 μm to 5 μm.
[0020] In some embodiments, the fullerene material comprises C 20 、C 60 、C 70 、C 76 、C 80 At least one of .
[0021] In some embodiments, the fullerene material has a shape including at least one of spherical, ellipsoidal, cylindrical, and tubular.
[0022] In some embodiments, the specific surface area of the fullerene material is 100 m 2 / g~500m 2 / g.
[0023] In some embodiments, the total pore volume of the fullerene material is 0.01 cm 3 / g~0.5cm 3 / g.
[0024] In some embodiments, the average pore size of the mesopores of the fullerene material is 2 nm to 20 nm.
[0025] In some embodiments, the modified layer further comprises a binder.
[0026] In some embodiments, the porosity of the base film layer is 30% to 70%.
[0027] In some embodiments, the average pore size of the base membrane layer is 100 nm to 800 nm.
[0028] In some embodiments, the surface density of the base film layer is 2 g / m 2 ~10g / m 2 .
[0029] In some embodiments, the base film layer includes at least one material selected from the group consisting of polypropylene, polyethylene, glass fiber, and polyvinylidene fluoride.
[0030] In some embodiments, the composite membrane has an air permeability of 300 s / (100 cc) to 500 s / (100 cc).
[0031] In some embodiments, the transverse tensile strength of the composite membrane is not less than 1000 kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm 2 .
[0032] In some embodiments, the transverse tensile strength of the composite membrane is not higher than 1700 kg / cm 2 , longitudinal tensile strength is not higher than 1500kg / cm 2 .
[0033] In some embodiments, the composite membrane has a thickness of no greater than 15 μm.
[0034] In some embodiments, the composite membrane has a thickness of 7 μm to 15 μm.
[0035] In some embodiments, the modified layer has a mass percentage of 10% to 20% in the composite membrane.
[0036] In a second aspect, a method for preparing a composite diaphragm is provided, comprising the following steps:
[0037] preparing a fullerene slurry;
[0038] At least two base film layers are obtained, and the fullerene slurry is made into a modified layer between two adjacent base film layers to obtain a composite diaphragm.
[0039] In some embodiments, the step of preparing the fullerene slurry includes: modifying the fullerene, and then preparing a mixed slurry of the fullerene material with a dispersant, a binder, and a solvent to obtain the fullerene slurry.
[0040] In some embodiments, the method of modifying the fullerene includes at least one of: doping with heteroatoms, modifying organic functional groups, composite inorganic materials, and pore-forming treatment.
[0041] In some embodiments, the heteroatom includes at least one of N, S, O, B, and P.
[0042] In some embodiments, the organic functional group includes at least one of a pyrrole group, a thiophene group, and an aniline group.
[0043] In some embodiments, the inorganic material includes at least one of MoO2, MgO, and Al2O3.
[0044] In some embodiments, the pore-forming treatment comprises at least one of a pore-forming agent, chemical etching, and a template method.
[0045] In some embodiments, in the fullerene slurry, the mass ratio of the fullerene material, the binder, and the dispersant is (60-90):(5-20):(1-20).
[0046] In some embodiments, in the fullerene slurry, the mass ratio of the total mass of the fullerene material, the binder, and the dispersant to the solvent is (0.1-0.6):1.
[0047] In some embodiments, the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylonitrile, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride, and polyimide.
[0048] In some embodiments, the dispersant includes at least one of polyacrylate, polyacrylamide, and long-chain fatty acid.
[0049] In some embodiments, the solvent includes at least one of deionized water, N-methylpyrrolidone, ethanol, dimethylformamide, dimethylacetamide, acetone, and dichloromethane.
[0050] In some embodiments, the preparation of the modified layer includes the steps of coating the fullerene slurry on one side of the base film layer, laminating the other base film layer to the coating slurry surface, and drying and curing to form the modified layer between the two base film layers.
[0051] In some embodiments, the modified layer has a thickness of 0.5 μm to 2 μm.
[0052] In some embodiments, the average particle size of the fullerene material is 0.1 μm to 5 μm.
[0053] In some embodiments, the fullerene material comprises C 20 、C 60 、C 70 、C 76 、C 80 At least one of .
[0054] In some embodiments, the fullerene material has a shape including at least one of spherical, ellipsoidal, cylindrical, and tubular.
[0055] In some embodiments, the porosity of the base film layer is 30% to 70%.
[0056] In some embodiments, the average pore size of the base membrane layer is 100 nm to 800 nm.
[0057] In some embodiments, the surface density of the base film layer is 2 g / m 2 ~10g / m 2 .
[0058] In some embodiments, the base film layer has a thickness of 3 μm to 7 μm.
[0059] In some embodiments, the base film layer includes at least one material selected from the group consisting of polypropylene, polyethylene, glass fiber, and polyvinylidene fluoride.
[0060] In some embodiments, the composite membrane has an air permeability of 300 s / (100 cc) to 500 s / (100 cc).
[0061] In some embodiments, the transverse tensile strength of the composite membrane is not less than 1000 kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm 2 .
[0062] In some embodiments, the composite membrane has a thickness of no greater than 15 μm.
[0063] In some embodiments, the modified layer has a mass percentage of 10% to 20% in the composite membrane.
[0064] In a third aspect, a battery cell is provided, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator comprises the composite separator described above, or a composite separator prepared by the method described above.
[0065] In a fourth aspect, a battery module is provided, wherein the battery module includes a plurality of the above-mentioned battery cells.
[0066] In a fifth aspect, a battery pack is provided, wherein the battery pack comprises a plurality of the above-mentioned battery modules.
[0067] In a sixth aspect, an electrical device is provided, wherein the electrical device includes the above-mentioned battery cell, or the above-mentioned battery module, or the above-mentioned battery pack. Beneficial effects
[0068] The beneficial effect of a composite membrane provided by an embodiment of the present application is that a fullerene material having excellent mechanical rigidity, excellent ionic and electronic conductivity, thermal conductivity, liquid absorption capacity, wettability, air permeability, and light weight is used as a modified layer in the composite membrane. This is beneficial for improving the comprehensive performance of the composite membrane, such as mechanical properties, heat resistance, ionic and electronic conductivity, and a small amount of fullerene material can meet the application requirements, which can reduce the thickness of the modified layer in the composite membrane, thereby facilitating the lightweight design of the composite membrane. In addition, the modified layer is arranged between two adjacent base film layers, and the base film layers on both sides can provide a load matrix for the modified layer and play a supporting and protective role, which is beneficial for maintaining the stability of the modified layer and avoiding the powdering of the modified layer during the charge and discharge process that affects the stability of the electrochemical performance of the battery. At the same time, the amount of adhesive material and the like in the modified layer can be reduced, avoiding the excessive introduction of other materials that affect the air permeability and ion migration efficiency of the composite membrane, which is beneficial for further reducing the thickness of the modified layer and reducing the overall thickness of the composite membrane, thereby facilitating lightweighting.
[0069] The beneficial effect of the preparation method of a composite diaphragm provided in an embodiment of the present application is that the prepared fullerene slurry is made into a modified layer between two base film layers, thereby obtaining a composite diaphragm with a base film layer-modified layer-base film layer laminated and bonded. The preparation process of the composite diaphragm is simple, the operation is simple, and it is suitable for industrial large-scale production and application. The prepared composite diaphragm introduces a fullerene modified layer with excellent mechanical rigidity, excellent ionic and electronic conductivity, thermal conductivity, strong stability, wettability and other characteristics in the middle of the base film layer, thereby improving the comprehensive performance of the composite diaphragm, such as mechanical properties, heat resistance, ionic and electronic conductivity, and liquid absorption rate. Moreover, based on the structural design of the fullerene modified layer as the intermediate layer, the composite diaphragm can achieve a lightweight design.
[0070] The battery cell provided in an embodiment of the present application has the beneficial effect of: the separator in the battery cell comprises the composite separator provided in the first aspect, or the composite separator prepared by the method provided in the second aspect. Because the separator employs the aforementioned composite separator, which simultaneously exhibits excellent mechanical properties, heat resistance, wettability, stability, ionic and electronic conductivity, and is capable of lightweight design, the battery cell's rate capability, energy density, cycling stability, and safety are improved.
[0071] The battery module provided by the embodiments of the present application has the beneficial effect of comprising a plurality of the aforementioned battery cells. Because the battery module comprises battery cells having the aforementioned specific characteristics of high rate performance, energy density, cycle stability, and safety, the battery module's rate performance, energy density, cycle stability, and safety are also improved.
[0072] The battery pack provided by the embodiments of the present application has the beneficial effect of comprising a plurality of the aforementioned battery modules. The inclusion of the aforementioned battery modules with high rate performance, energy density, cycle stability, and safety performance improves the rate performance, energy density, cycle stability, and safety performance of the battery pack.
[0073] The beneficial effect of an electrical device provided by an embodiment of the present application is that the electrical device includes the aforementioned battery cell, battery module, or battery pack. Because the electrical device includes the aforementioned battery cell, battery module, or battery pack having high rate performance, energy density, cycle stability, and safety performance, the electrical safety and stability of the electrical device are improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments or exemplary technical descriptions. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0075] FIG1 is a schematic flow chart of a method for preparing a composite diaphragm provided in an embodiment of the present application;
[0076] FIG2 is a schematic diagram of the composite diaphragm structure according to an embodiment of the present application;
[0077] FIG3 is a second schematic diagram of the composite diaphragm structure according to an embodiment of the present application;
[0078] FIG4 is a third schematic diagram of the composite diaphragm structure according to an embodiment of the present application;
[0079] FIG5 is a fourth schematic diagram of the composite diaphragm structure according to an embodiment of the present application;
[0080] FIG6 is a schematic structural diagram of an embodiment of a battery cell according to the present application;
[0081] FIG7 is an exploded schematic diagram of the battery cell shown in FIG6 ;
[0082] FIG8 is a schematic structural diagram of an embodiment of a battery module according to the present application;
[0083] FIG9 is a schematic structural diagram of an embodiment of a battery pack according to the present application;
[0084] FIG10 is a schematic diagram of the exploded structure of the battery pack shown in FIG9 ;
[0085] FIG11 is a schematic diagram of an embodiment of an electrical device including a battery cell, a battery module or a battery pack according to an embodiment of the present application as a power source.
[0086] The reference numerals in the specific embodiments are as follows: 05 - battery cell, 51 - housing, 52 - electrode assembly, 53 - cover plate; 06 - battery module; 07 - battery pack, 71 - box, 72 - lower box. Modes for Carrying Out the Invention
[0087] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit this application.
[0088] In this application, the term "and / or" describes the relationship between associated objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0089] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0090] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0091] The terms used in the embodiments of the present application are for the purpose of describing specific embodiments only and are not intended to limit the present application. The singular forms "a", "an", "the" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise.
[0092] The weights of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the mass described in the examples of this application may be a mass unit known in the chemical industry, such as μg, mg, g, kg, etc.
[0093] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0094] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0095] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0096] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0097] In order to illustrate the technical solution provided by this application, a detailed description is given below with reference to specific drawings and embodiments.
[0098] Currently, judging by market developments, separators, as key components of lithium-ion battery cells, determine the battery's interface structure and internal resistance, directly impacting its capacity, cycle life, and safety. High-performance separators are crucial for improving the battery's overall performance. The primary function of a battery separator is to separate the positive and negative plates in the battery, preventing direct contact and short circuits. Furthermore, because the separators contain numerous micropores, positive and negative ions in the battery can freely pass through them, migrating between the plates to form an internal conductive circuit within the battery. Electrons, on the other hand, migrate between the positive and negative electrodes through an external circuit, generating a current that is then used by electrical devices.
[0099] High-performance battery separators must not only possess excellent electrical insulation, high ion permeability, good mechanical properties, solvent resistance, high-temperature resistance, and high wettability, but also reduce the separator's own weight, which is crucial for increasing the energy density of the battery cell. Separator thickness is related to internal resistance: thinner separators reduce internal resistance, enabling high-power charging and discharging. While maintaining a certain mechanical strength, separator thickness should be minimized, especially for consumable lithium-ion batteries. The growing demand for portable devices such as mobile phones, laptops, and digital cameras is driving the demand for thinner separators. Furthermore, for power batteries, thinner separators reduce the resistance to solvated lithium ions traveling through them, resulting in better ion conductivity and lower impedance. Furthermore, thicker separators reduce the number of layers that can be wound, resulting in a corresponding decrease in capacity. However, excessively thin separators reduce their liquid retention and electronic insulation, negatively impacting battery performance. Therefore, separators must simultaneously achieve lightweight while maintaining high mechanical properties, heat resistance, and wettability. However, if the separator thickness is directly reduced, it is difficult to balance the mechanical properties, heat resistance and other properties of the separator.
[0100] Based on the above considerations, in order to solve the problem of the difficulty in achieving lightweighting while ensuring membrane properties such as mechanical properties, heat resistance, and wettability, a composite membrane was proposed. The fullerene material is used as a fullerene intermediate functional layer and applied between multiple base film layers to form a composite membrane.
[0101] In such a composite membrane, the fullerene material used in the modified layer not only possesses the excellent mechanical rigidity, superior ionic and electronic conductivity, thermal conductivity, stability, and good nonlinear optical properties of fullerenes described herein, but also, after modification, further enhances its ionic and electronic conductivity, porosity, liquid absorption, wettability, air permeability, and adhesion. Applying high-performance fullerene materials between the base membrane layers not only improves the composite membrane's overall performance, including mechanical properties, heat resistance, and ionic and electronic conductivity, but also allows for a smaller amount of fullerene material to meet application requirements, reducing the thickness of the modified layer in the composite membrane and thus facilitating a lightweight design. In addition, the modified layer is arranged between two adjacent base membrane layers. The base membrane layers on both sides can not only provide a load matrix for the modified layer, but also play a supporting and protective role, which is beneficial to maintaining the stability of the modified layer, and can reduce the amount of adhesive materials in the modified layer, etc., and avoid excessive introduction of other materials to affect the air permeability and ion migration efficiency of the composite diaphragm, which is beneficial to further reduce the thickness of the modified layer and reduce the overall thickness of the composite diaphragm, which is conducive to achieving lightweight.
[0102] Therefore, the composite diaphragm provided by this application not only has excellent electrical insulation, high ion transmission rate, good mechanical properties, solvent resistance, high temperature resistance, and high wettability, but also reduces the weight of the diaphragm itself, achieving a lightweight design. Its application in battery cells can help increase battery energy density and achieve high-power charging and discharging, making it particularly suitable for portable products that require consumable lithium-ion batteries.
[0103] For the convenience of description, the following embodiments of the present application are described by taking a composite diaphragm and its preparation method and application as an example.
[0104] In a first aspect, an embodiment of the present application provides a composite diaphragm, which includes a plurality of laminated base film layers and at least one modified layer disposed between two adjacent base film layers; the raw material components of the modified layer include fullerene materials.
[0105] In the composite diaphragm of the embodiment of the present application, the base film layer refers to the material layer used to separate the positive and negative electrodes in the battery, prevent the positive and negative electrodes from directly contacting each other to produce a short circuit, and prevent the electrons in the battery from passing freely, but at the same time allow ions to pass freely between the positive and negative electrodes. The composite diaphragm of the embodiment of the present application can be a laminated composite structure of multiple base film layers and at least one modified layer. For example, as shown in FIG2, the structure of the composite diaphragm can be base film layer-modified layer-base film layer-base film layer, or, as shown in FIG3, base film layer-base film layer-modified layer-base film layer-base film layer, etc. The composite diaphragm can also be a laminated composite structure of multiple base film layers and multiple modified layers. For example, as shown in FIG4, the structure of the composite diaphragm can be base film layer-modified layer-base film layer-modified layer-base film layer. The composite diaphragm can also be a composite structure of two base film layers and an intermediate modified layer. As shown in FIG5, the specific structure can be base film layer-modified layer-base film layer. In the above description, "-" indicates the connection relationship between the laminated bonding between the film layers. The structure and number of layers of the composite diaphragm can be flexibly designed according to actual application needs to meet the requirements of different battery systems for diaphragm performance.
[0106] Thus, the composite diaphragm of the embodiment of the present application has the following advantages:
[0107] First, fullerenes have a hollow molecular structure composed of carbon. Due to their unique zero-dimensional structure, fullerenes possess excellent physical and chemical properties, including superior mechanical rigidity, excellent ionic and electronic conductivity, thermal conductivity, and good nonlinear optical properties, all while being lightweight. Applying fullerenes to composite separators not only improves their mechanical properties, heat resistance, and stability, but also helps reduce their weight, enabling them to be lightweight while maintaining excellent mechanical and electrochemical properties.
[0108] Secondly, in order to form tubes or spheres, the sp hybrid orbitals in fullerenes are bent, resulting in a large bond angle tension. Once the carbon-carbon double bond is saturated through reaction, the bond angle tension is released. This shift in the atomic orbitals shifts the bond angle from approximately 120° (sp) to approximately 109.5° (sp), reducing the fullerene's Gibbs free energy and thus making it highly stable. Applying a modified layer between the two base film layers makes the composite separator less susceptible to reaction with the electrolyte during charge and discharge, further improving the separator's stability.
[0109] Third, the modified layer is positioned between two adjacent base film layers. The base film layers on both sides not only provide a load matrix for the modified layer but also provide support and protection, which helps maintain the stability of the modified layer and prevents the modified layer from shedding powder during charge and discharge, which could affect the stability of the battery's electrochemical performance. This also reduces the amount of adhesives and other materials used in the modified layer, preventing the excessive introduction of other materials that could affect the air permeability and ion migration efficiency of the composite membrane. This helps further reduce the thickness of the modified layer, reducing the overall thickness of the composite membrane and contributing to lightweighting.
[0110] In some possible implementations, the raw material components of the modified layer include fullerenes that have been modified by at least one of doping with heteroatoms, modifying organic functional groups, composite inorganic materials, and pore-forming treatment.
[0111] The fullerenes in the embodiments of the present application can produce chemical reactions such as oxidation, reduction, polymerization, photosensitization, affinity addition, and electrophilic addition. Fullerenes can form single addition products or multiple addition products. By using functionally modified fullerenes, not only can the ionic and electronic conductivity of fullerenes be improved, but also the porosity of fullerenes can be improved, and the liquid absorption capacity, wettability, air permeability, adhesion performance, etc. of fullerenes can be improved, so that it can meet the requirements of the membrane for air permeability, liquid absorption, etc. The application of fullerene materials with higher performance between the base film layers is beneficial to improving the comprehensive performance of the composite membrane, such as mechanical properties, heat resistance, ionic and electronic conductivity, and the application requirements can be met by a small amount of fullerene materials. The thickness of the modified layer in the composite membrane can be reduced, thereby facilitating the lightweight design of the composite membrane. For example, by doping heteroatoms in fullerenes, the heteroatoms partially replace carbon atoms in the fullerenes to form new aromatic rings, which can simultaneously improve the ionic and electronic conductivity of the fullerenes. In addition, by modifying fullerene with organic functional groups, the ionic and electronic conductivity of fullerene can also be improved. This not only improves the efficiency of ion migration in the composite membrane, weakens polarization, and reduces the internal resistance of the composite membrane; but also, when contacting the pierced lithium dendrite, since fullerene also has conductive properties, the electrons brought from the electrode by the lithium dendrite conduction will be transported and conducted through the surface of the modified layer, thereby changing the growth direction of the lithium dendrite, causing lithium ions to deposit along the fullerene surface, and reducing the risk of lithium dendrites piercing the membrane. For example, after the fullerene is composited with an inorganic material, the high flame retardancy and strong mechanical properties of the inorganic material are introduced on the basis of the fullerene properties, which is beneficial to improve the heat resistance, mechanical strength, safety performance and other properties of the modified layer. For example, by performing a pore-forming treatment on the fullerene, the specific surface area of the fullerene is increased, its mesopore volume is increased, the contact area between the modified layer and the electrolyte is increased, and the amount of electrolyte retained in the modified layer is increased, thereby improving the liquid absorption and liquid retention characteristics of the composite membrane. In addition, the high specific surface area and porosity of fullerene can enhance the charge transfer rate of the modified layer and reduce the internal resistance of the battery.
[0112] In some possible implementations, the heteroatom includes non-metallic elements from Groups IIIA to VIA. By doping fullerenes with non-metallic heteroatoms from Groups IIIA to VIA, the heteroatoms partially replace carbon atoms in the fullerene to form new aromatic rings such as pyrrole, pyridine, and thiophene, thereby simultaneously improving the fullerene's electronic conductivity. This increased electronic conductivity allows the modified layer to contact a lithium dendrite. Because the fullerene is also conductive, electrons carried by the lithium dendrite from the electrode are transported and conducted through the surface of the modified layer, thereby changing the growth direction of the lithium dendrite and causing lithium ions to deposit along the fullerene surface, reducing the risk of lithium dendrites piercing the separator.
[0113] In some possible implementations, the heteroatoms include at least one of N, S, O, B, and P; these heteroatoms are doped into fullerenes, and these heteroatoms partially replace the carbon atoms in the fullerenes to form new aromatic rings such as pyrrole, pyridine, and thiophene, which can improve the ionic and electronic conductivity of the fullerenes, improve the migration efficiency of ions in the composite membrane, and weaken the polarization phenomenon; at the same time, they can change the growth direction of lithium dendrites and improve the safety performance of the composite membrane.
[0114] In some possible implementations, the organic functional groups include at least one of pyrrole, thiophene, and aniline groups. These electron-rich organic functional groups are modified on the fullerene via a chemically bonded grafting method, allowing the composite separator to form ion pairs in the electrolyte. These ion pairs can conduct electricity in the electrolyte solution, thereby increasing the conductivity of the electrolyte solution and thus improving ionic conductivity. This also stabilizes the ion pairs, making the ionic charge distribution more stable and further improving ionic conductivity. This improves the efficiency of ion migration in the composite separator, weakens polarization, and reduces the internal resistance of the composite separator.
[0115] In some possible implementations, the inorganic material includes metal oxides; metal oxides have properties such as high flame retardancy and strong mechanical mechanics. After fullerenes are physically compounded with metal oxide inorganic materials, a composite material with close contact is formed. Based on the properties of fullerenes, it is beneficial to improve the heat resistance, mechanical strength, safety performance and other properties of the modified layer.
[0116] In some possible implementations, the inorganic material includes at least one of MoO2, MgO, and Al2O3. Among them, molybdenum dioxide is a transition metal oxide with high electrical conductivity, efficient charge transport properties, a high melting point, and high chemical stability. It is a metal oxide with high electrical conductivity and a high carrier conduction rate. The tunnel-like voids in its crystal structure are also conducive to the rapid insertion and extraction of charged particles. Therefore, the composite of MoO2 and fullerene can significantly improve the electrical conductivity and chemical stability of fullerene. Magnesium oxide has high fire-resistant insulation properties. It can be transformed into crystals after high-temperature calcination above 1000°C. When it rises to 1500-2000°C, it becomes dead-burned magnesium oxide (magnesia) or sintered magnesium oxide. Al2O3 is a compound with high hardness and a high melting point. Therefore, composite fullerene with magnesium oxide or aluminum oxide can improve the heat resistance of the modified layer, thereby improving the thermal stability of the composite diaphragm.
[0117] In some possible implementations, the pore-forming treatment includes at least one of a pore-forming agent, chemical etching, and a template method. In this case, by using at least one of these pore-forming agents, chemical etching, and a template method to create pores on the fullerene, the specific surface area and mesopore volume of the fullerene are increased, thereby increasing the contact area between the modified layer and the electrolyte, increasing the amount of electrolyte retained in the modified layer, and improving the wettability of the composite separator. Furthermore, the increased specific surface area and porosity of the fullerene can enhance the charge transfer rate of the modified layer and reduce the internal resistance of the battery.
[0118] In some possible implementations, the thickness of the modified layer is not higher than 5μm. Since the raw material component of the modified layer in the embodiment of the present application adopts fullerene material, and the modified layer is arranged between two adjacent base film layers as an intermediate functional layer. On the one hand, fullerene has excellent ionic and electronic conductivity, porosity, liquid absorption capacity, air permeability, adhesion performance and other properties. Therefore, a small amount of high-performance fullerene material applied to the composite diaphragm can effectively improve the mechanical properties, heat resistance, wettability, ion migration efficiency and other properties of the composite diaphragm, and can reduce the application thickness of the modified layer in the composite diaphragm. On the other hand, the modified layer is arranged between two adjacent base film layers, and the base film layers on both sides can support and protect the stability of the intermediate modified layer, which can reduce the proportion of other components such as binders in the modified layer, and further reduce the application thickness of the modified layer. Therefore, the thickness of the modified layer in the composite diaphragm of the embodiment of the present application can be no higher than 5μm, which is beneficial to the lightweighting of the composite diaphragm while improving the comprehensive performance of the composite diaphragm, thereby improving the energy density of the battery. For example, the thickness of the modified layer may be no greater than 5 μm, no greater than 4 μm, no greater than 3 μm, no greater than 2 μm, no greater than 1 μm, etc.
[0119] In some possible implementations, the thickness of the modified layer is no greater than 3 μm. This thickness is more conducive to lightweight applications of the composite diaphragm.
[0120] In some possible implementations, the modified layer has a thickness of 0.5 μm to 2 μm. In this case, by designing the modified layer as an intermediate layer in the raw material components, the modified layer can be designed to have a thickness of 0.5 μm to 2 μm, thereby effectively improving the mechanical properties, heat resistance, and wettability of the composite membrane. For example, in the composite membrane, the modified layer can have a thickness of 0.5 μm to 1 μm, 1 μm to 1.5 μm, 1.5 μm to 2 μm, etc.
[0121] In some possible implementations, the base film layer has a thickness of 3 μm to 7 μm. In this case, after laminating with the modified layer, the composite membrane simultaneously has excellent mechanical properties, air permeability, heat resistance, liquid absorption rate, and other characteristics, while reducing the overall thickness of the composite membrane, thereby achieving a lightweight membrane design. For example, the thickness of the base film layer can be 3 μm to 4 μm, 4 μm to 5 μm, 5 μm to 6 μm, 6 μm to 7 μm, etc.
[0122] In some possible implementations, the average particle size of the fullerene material is 0.1μm to 5μm; in this case, fullerenes with this average particle size are more conducive to forming a uniform film layer and a thin modified layer, improving the uniformity of the distribution of fullerene particles in the film layer, and facilitating the size design of the composite diaphragm. It reduces the risk of poor dispersion due to too small particles and the risk of easy puncture of the composite diaphragm base film due to too large particles, thereby improving the safety performance of the composite diaphragm in the battery. For example, the average particle size of the fullerene material can be 0.1μm to 0.5μm, 0.5μm to 1μm, 1μm to 1.5μm, 1.5μm to 2μm, 2μm to 2.5μm, 2.5μm to 3μm, 3μm to 3.5μm, 3.5μm to 4μm, 4μm to 4.5μm, 4.5μm to 5μm, etc.
[0123] In some possible implementations, the fullerene material has a specific surface area of 100 m 2 / g~500m 2 / g; Under this specific surface area, the fullerene material has a better contact area with the electrolyte, which is beneficial to improve the wettability of the modified layer to the electrolyte, enhance the ion migration efficiency and charge conduction rate of the modified layer, change the growth direction of lithium dendrites, and prevent lithium dendrites from piercing the composite separator. For example, the specific surface area of the fullerene material can be 100m 2 / g~150m 2 / g, 150m 2 / g~200m 2 / g, 200m 2 / g~250m 2 / g, 250m 2 / g~300m2 / g、300m 2 / g~350m 2 / g、350m 2 / g~400m 2 / g, 400m 2 / g~450m 2 / g, 450m 2 / g~500m 2 / g, etc.
[0124] In some possible implementations, the total pore volume of the fullerene material is 0.01 cm 3 / g~0.5cm 3 / g. In some possible implementations, the average mesopore diameter of the fullerene material is 2nm to 20nm. Under this total pore volume and average mesopore diameter, the fullerene material has better liquid absorption and retention properties for the electrode liquid, improves the wettability of the modified layer, is more conducive to the migration and transmission of ions in the diaphragm, and weakens the polarization phenomenon. For example, the total pore volume of the fullerene material can be 0.01cm 3 / g~0.05cm 3 / g, 0.05cm 3 / g~0.1cm 3 / g, 0.1cm 3 / g~0.2cm 3 / g, 0.2cm 3 / g~0.3cm 3 / g, 0.3cm 3 / g~0.4cm 3 / g, 0.4cm 3 / g~0.5cm 3 / g, etc. For example, the average pore diameter of the mesopores of the fullerene material can be 2nm-5nm, 5nm-8nm, 8nm-10nm, 10nm-13nm, 13nm-15nm, 15nm-18nm, 18nm-20nm, etc.
[0125] In some possible implementations, in the fullerene material, the fullerene includes C 20 、C 60 、C 70 、C 76 、C 80 At least one of the following. The fullerenes used in the present embodiment are not limited to C 60 , or it can be a combination of carbon atoms in different new molecular structures. 20 It is the smallest buckyball cluster (an unsaturated derivative of eicosane). 60The molecular structure of fullerene is a spherical 32-hedron. It is a soccer-shaped hollow symmetrical molecule with 30 carbon-carbon double bonds, composed of 60 carbon atoms connected by 20 six-membered rings and 12 five-membered rings. Therefore, fullerene is also called soccer ene. 60 It is a highly symmetrical cage structure with highly delocalized large π conjugation, which makes it highly stable. 70 It is an elongated cage-like structure. 76 The molecule is C 60 The molecules are close, it is in C 60 The molecule is formed on a hollow cage structure with 16 additional carbon atoms, making it one of the most basic and important fullerene molecules. These fullerenes have unique optical, electrical, and chemical properties due to their unique zero-dimensional structure.
[0126] In some possible implementations, the shape of the fullerene material includes at least one of spherical, ellipsoidal, cylindrical, and tubular. The shape of the fullerene and fullerene material in the embodiment of the present application is not limited to the conventional spherical shape, and can also be other configurations such as ellipsoidal, cylindrical, and tubular. Among them, the smallest spherical shape is C 20 (unsaturated derivatives of eicosane) and the most common C 60 . Ellipsoid type includes C 70 、C 76 Tubular carbon nanotubes include very small hollow tubes, which come in single-walled and multi-walled configurations. Columnar carbon nanotubes include giant carbon tubes (GCTs), which are larger than nanotubes and can be manufactured with walls of varying thicknesses, showing potential for transporting molecules of varying sizes.
[0127] In some possible implementations, the modified layer also contains a binder; by combining the binder with the fullerene material, the bonding stability of the fullerene material on the base film layer can be significantly improved, thereby improving the bonding stability of the fullerene film layer in the middle of the base film layer, avoiding the composite diaphragm from cracking, powdering, etc. during the battery charging and discharging process, and improving the operating stability of the composite diaphragm.
[0128] In some possible implementations, the weight percentage of the modified layer in the composite membrane is 10% to 20%. Under this weight percentage condition, the modified layer can effectively improve the mechanical properties, heat resistance, wettability, stability and other characteristics of the composite membrane, and is also conducive to the lightweight design of the composite membrane. In some specific embodiments, the weight percentage of the modified layer in the composite membrane can be 10% to 12%, 12% to 14%, 14% to 15%, 15% to 17%, 17% to 19%, 19% to 20%, etc.
[0129] In some possible implementations, the porosity of the base film layer is 30% to 70%. Porosity is the volume percentage of pores in the volume of the monomer base film layer. It is related to the density of the raw resin and the film, and reflects the number of micropores inside the separator. Under this porosity condition, the base film layer has good air permeability, which is conducive to the migration and transmission of ions in the separator, reducing the impedance of the battery. Exemplary, the porosity of the base film layer can be 30% to 40%, 40% to 50%, 50% to 60%, 60% to 70%, 40% to 60%, 50% to 70%, etc.
[0130] In some possible implementations, the average pore size of the base membrane layer is 100nm to 800nm; the pore size is related to the permeability of the separator. To prevent direct contact between electrode particles, it is necessary to prevent electrode particles from directly passing through the separator while maintaining low electrical resistance and high ionic and electronic conductivity. Excessively large pore sizes can cause perforation of the separator, resulting in micro-shorting of the battery and increased self-discharge; while too small pore sizes increase electrical resistance. Uneven pore size distribution leads to inconsistent current density within the battery, which over time can form local dendrites that pierce the separator. Under these conditions, a submicron pore size separator is sufficient to prevent direct passage of electrode particles. This ensures that the base membrane layer has an appropriate pore size, which facilitates ion transport and prevents direct contact between electrode particles, preventing them from directly passing through the separator. This avoids micro-shorting caused by excessively large pores, while also preventing increased electrical resistance caused by excessively small pores. This results in a separator with low electrical resistance and high ionic and electronic conductivity. Illustratively, the average pore size of the base membrane layer can be 100nm~200nm, 200nm~300nm, 300nm~400nm, 400nm~500nm, 500nm~600nm, 600nm~700nm, 700nm~800nm, 200nm~700nm, 300nm~600nm, 400nm~700nm, 500nm~800nm, etc.
[0131] In some possible implementations, the surface density of the base film layer is 2 g / m 2 ~10g / m 2 ; Surface density refers to the weight per unit area of the diaphragm. Since the diaphragm contains a large number of micropores, as the number of micropores decreases, the surface density of the diaphragm increases, and the porosity and air permeability decrease. Under this surface density condition, the porosity of the base membrane layer is ensured, which is conducive to improving the air permeability of the base membrane layer, facilitating the migration and transmission of ions in the diaphragm, avoiding short circuits, and facilitating the lightweight design of the composite diaphragm. For example, the surface density of the base membrane layer can be 2g / m 2 ~3g / m 2 , 3g / m 2 ~4g / m 2 , 4g / m 2 ~5g / m2 , 5g / m 2 ~6g / m 2 , 6g / m 2 ~7g / m 2 , 7g / m 2 ~8g / m 2 , 8g / m 2 ~9g / m 2 , 9g / m 2 ~10g / m 2 , 3g / m 2 ~9g / m 2 , 4g / m 2 ~8g / m 2 , 5g / m 2 ~7g / m 2 , 6g / m 2 ~8g / m 2 , 7g / m 2 ~9g / m 2 , 8g / m 2 ~10g / m 2 wait.
[0132] In some possible implementations, the base film layer comprises at least one of polypropylene, polyethylene, glass fiber, and polyvinylidene fluoride. These base film materials all possess excellent electrical insulation properties and maintain chemical stability over a wide temperature and voltage range. They are also advantageous for producing a thin, uniform base film layer with appropriate porosity and pore size, enabling rapid wetting of the electrolyte, isolating electrons while maintaining the free flow of ions to meet the battery's requirements for high energy, high power, and cycle performance. Furthermore, they possess a certain degree of mechanical strength and processing toughness to meet the battery's discharge requirements during assembly and use.
[0133] In some possible implementations, the composite membrane has a thickness of no greater than 15 μm. By utilizing a modified layer within the composite membrane and placing the modified layer between two adjacent base membrane layers, the membrane's mechanical properties, air permeability, heat resistance, and wettability are enhanced while also reducing its thickness to no greater than 15 μm, achieving a lightweight membrane. Furthermore, the thin membrane shortens the ion migration pathway, improving ion migration efficiency and reducing polarization.
[0134] In some possible implementations, the thickness of the composite membrane is 7 μm to 15 μm. At this thickness, the composite membrane has better comprehensive properties such as mechanical properties, air permeability, wettability, and heat resistance. For example, the thickness of the composite membrane can be 7 μm to 8 μm, 8 μm to 9 μm, 9 μm to 10 μm, 10 μm to 11 μm, 11 μm to 12 μm, 12 μm to 13 μm, 13 μm to 14 μm, 14 μm to 15 μm, 8 μm to 14 μm, 9 μm to 13 μm, 10 μm to 12 μm, etc.
[0135] In some possible implementations, the air permeability of the composite diaphragm is 300s / (100cc) to 500s / (100cc). The embodiment of the present application includes a composite diaphragm comprising a plurality of laminated base film layers and at least one modified layer disposed between two adjacent base film layers, and has high air permeability. Air permeability is an indicator of the gas permeability of the diaphragm and can indirectly reflect the permeability of ions. When the air permeability of the composite diaphragm is 300s / (100cc) to 500s / (100cc), it fully ensures the efficient migration and transmission efficiency of ions in the diaphragm, and avoids other substances such as electrons penetrating the composite diaphragm to affect the stability of the battery system. At the same time, it ensures that the composite diaphragm has good wettability to the electrolyte. Good wettability is conducive to improving the affinity between the diaphragm and the electrolyte, expanding the contact surface between the diaphragm and the electrolyte, thereby increasing ionic conductivity and improving the charge and discharge performance and capacity of the battery. In some specific embodiments, the air permeability of the composite membrane can be 300s / (100cc) to 350ss / (100cc), 350s / (100cc) to 400s / (100cc), 400s / (100cc) to 450s / (100cc), 450s / (100cc) to 500s / (100cc), etc.
[0136] In some possible implementations, the transverse tensile strength of the composite diaphragm is not less than 1000 kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm 2 Tensile strength refers to the ratio of the maximum force that the diaphragm can withstand before breaking under the action of pure tensile force to the cross-sectional area of the tested diaphragm. The greater the tensile strength, the lower the probability of damage and fracture of the composite diaphragm under the action of external force. The sufficient tensile strength in the transverse and longitudinal directions of the composite diaphragm of the embodiment of the present application can prevent the diaphragm from deforming and improve the operational stability of the diaphragm.
[0137] In some possible implementations, the transverse tensile strength of the composite diaphragm is not less than 1000 kg / cm 2 And not higher than 1700kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm2 And not higher than 1500kg / cm 2 Under the conditions of transverse and longitudinal tensile strength, the deformation requirements of the composite diaphragm are met and the composite diaphragm has a suitable shrinkage rate. For example, the transverse tensile strength of the composite diaphragm can be 1100 kg / cm 2 ~1200kg / cm 2 , 1200kg / cm 2 ~1300kg / cm 2 、1300kg / cm 2 ~1400kg / cm 2 、1400kg / cm 2 ~1500kg / cm 2 、1500kg / cm 2 ~1600kg / cm 2 、1600kg / cm 2 ~1700kg / cm 2 etc., the longitudinal tensile strength is 1250kg / cm 2 ~1300kg / cm 2 、1300kg / cm 2 ~1350kg / cm 2 、1350kg / cm 2 ~1400kg / cm 2 、1400kg / cm 2 ~1500kg / cm 2 wait.
[0138] The composite diaphragm of the above embodiment of the present application can be prepared by the following embodiment method.
[0139] In a second aspect, as shown in FIG1 , an embodiment of the present application provides a method for preparing a composite diaphragm, comprising the following steps:
[0140] S10. Prepare fullerene slurry.
[0141] S20. Obtain at least two base film layers, and prepare a modified layer with fullerene slurry between two adjacent base film layers to obtain a composite diaphragm.
[0142] The preparation method of the composite diaphragm provided in the embodiment of the present application is to prepare a modified layer between two base film layers using the prepared fullerene slurry, thereby obtaining a composite diaphragm with a laminated arrangement of base film layer-modified layer-base film layer, wherein "-" represents the laminated connection relationship between the film layers. The preparation process of the composite diaphragm is simple, easy to operate, and suitable for industrial large-scale production and application. The prepared composite diaphragm introduces a modified layer with excellent mechanical rigidity, excellent ionic and electronic conductivity, thermal conductivity, strong stability, wettability and other characteristics in the middle of the base film layer, thereby improving the comprehensive performance of the composite diaphragm, such as mechanical properties, heat resistance, ionic and electronic conductivity, and liquid absorption rate. Moreover, based on the structural design of the fullerene modified layer as the intermediate layer, the composite diaphragm can be designed to be lightweight.
[0143] The composite diaphragm prepared in the embodiment of the present application may include multiple base film layers, forming a laminated composite structure of multiple base film layers and at least one modified layer. For example, the structure of the composite diaphragm may be base film layer-modified layer-base film layer-base film layer, base film layer-base film layer-modified layer-base film layer-base film layer, etc. In addition, when there are multiple base film layers, modified layers may be prepared respectively between different adjacent base film layers, so that the prepared composite diaphragm forms a laminated composite structure of multiple base film layers and multiple modified layers. For example, the structure of the composite diaphragm may be base film layer-modified layer-base film layer-modified layer-base film layer. The structure and number of layers of the composite diaphragm can be flexibly designed according to actual application requirements so that it meets the requirements of different battery systems for diaphragm performance. In some specific embodiments, the composite diaphragm is a composite structure of two base film layers and an intermediate modified layer, and the specific structure is base film layer-modified layer-base film layer.
[0144] In step S10, a fullerene slurry is prepared. Fullerene has high ionic and electronic conductivity, porosity, liquid absorption capacity, wettability, air permeability, and adhesion properties, enabling it to meet the membrane's requirements for air permeability, liquid absorption, and other properties. Using modified, high-performance fullerene to prepare the slurry and applying it to the modified layer between the base membrane layers not only improves the composite membrane's overall performance, including mechanical properties, heat resistance, and ionic and electronic conductivity, but also allows the application requirements to be met with a small amount of fullerene material, reducing the thickness of the modified layer in the composite membrane, thereby facilitating a lightweight design of the composite membrane.
[0145] In some possible implementations, the steps of preparing a fullerene slurry include: after modifying the fullerene, mixing the fullerene material with a binder, a dispersant, and a solvent to form a mixed slurry to obtain the fullerene slurry. The binder can significantly improve the binding stability of the fullerene material on the base film layer and the binding stability of the fullerene film layer within the base film layer, thereby preventing cracking and powder loss in the modified layer of the composite separator during battery charging and discharging, and improving the operational stability of the composite separator. The dispersant is used to improve the dispersion stability of the fullerene material in the slurry, prevent fullerene agglomeration and sedimentation in the slurry, and facilitate subsequent preparation of the slurry into a smooth and uniform modified layer.
[0146] In some possible implementations, the binder includes: at least one of: carboxymethyl cellulose, styrene-butadiene rubber, polyacrylonitrile, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride, and polyimide; these binders can improve the bonding stability of the fullerene material on the base film layer, thereby improving the bonding stability of the fullerene film layer in the middle of the base film layer, avoiding the composite diaphragm from cracking, powdering, etc. during the battery charging and discharging process, and improving the operating stability of the composite diaphragm.
[0147] In some possible implementations, the dispersant includes: at least one of polyacrylate, polyacrylamide, and long-chain fatty acid; these dispersants can improve the dispersion stability of the fullerene material in the slurry, prevent the fullerene in the slurry from agglomerating and settling, and facilitate the subsequent preparation of a smooth and highly uniform modified layer from the slurry.
[0148] In some possible implementations, the solvent includes at least one of deionized water, N-methylpyrrolidone, ethanol, dimethylformamide, dimethylacetamide, acetone, and dichloromethane. These solvents have a good dissolving or dispersing effect on fullerene materials, binders, and dispersants, which is conducive to the preparation of a well-dispersed and stable fullerene slurry, and is conducive to the subsequent preparation of a uniform and smooth modified layer from the fullerene slurry.
[0149] In some possible implementations, the mass ratio of the fullerene material, binder, and dispersant in the fullerene slurry is (60-90):(5-20):(1-20). In some possible implementations, the mass ratio of the total mass of the fullerene material, binder, and dispersant to the solvent in the fullerene slurry is (0.1-0.6):1. With this ratio, the amount of solvent and dispersant in the slurry fully ensures the dispersion stability and viscosity of the fullerene slurry, which is beneficial for subsequent film formation. The amount of binder in the slurry fully ensures the bonding stability of the fullerene material with the base film layer during the film formation process, thereby ensuring the stability of the modified layer. For example, the mass ratio of the total mass of the fullerene material, the binder, and the dispersant to the solvent can be (0.1-0.2):1, (0.2-0.3):1, (0.3-0.4):1, (0.4-0.5):1, (0.5-0.6):1, etc.
[0150] In some possible implementations, the method of modifying fullerenes includes at least one of: doping with heteroatoms, modifying organic functional groups, composite inorganic materials, and pore-forming treatment. By doping heteroatoms in fullerenes or modifying organic functional groups on fullerenes, the ionic and electronic conductivity of fullerenes can be simultaneously improved. This improves the efficiency of ion migration in the composite diaphragm, weakens polarization, and reduces the internal resistance of the composite diaphragm. Furthermore, when contacting the pierced lithium dendrites, since fullerenes also have conductive properties, the electrons brought from the electrode by the lithium dendrites are transported and conducted through the surface of the modified layer, thereby changing the growth direction of the lithium dendrites and causing lithium ions to deposit along the fullerene surface, reducing the risk of lithium dendrites piercing the diaphragm. Composite inorganic materials can introduce high flame retardancy and strong mechanical properties of inorganic materials on the basis of fullerene properties, which is beneficial to improving the heat resistance, mechanical strength, safety performance and other characteristics of the modified layer. The fullerene is subjected to pore-forming treatment to increase the specific surface area of the fullerene, increase its mesopore volume, increase the contact area between the modified layer and the electrolyte, and increase the amount of electrolyte retained in the modified layer, thereby improving the liquid absorption and liquid retention characteristics of the composite membrane.
[0151] This application does not specifically limit the specific modification treatment method, and fullerenes can be modified by any method that can achieve the corresponding modification effect. Exemplary methods of doping fullerenes with heteroatoms include but are not limited to: after activating the fullerene with substances such as potassium hydroxide under a protective atmosphere, the heteroatom source substance is introduced and the heteroatoms are doped into the fullerene by high-temperature heat treatment. Exemplary methods of modifying fullerenes with organic functional groups include but are not limited to: after activating the fullerene surface, an organic substance containing the target organic functional group is introduced, and the organic active functional group is grafted to the fullerene surface through a chemical reaction. Exemplary methods of performing inorganic composite treatment on fullerenes include but are not limited to: after composite treatment of fullerenes with inorganic materials by ultrasound, coprecipitation, self-assembly, etc., the fullerenes and inorganic materials are fully and highly mixed to form a close physical contact interface, similar to a heterojunction structure, which is more conducive to the composite material to exert the characteristics of both.
[0152] In some possible implementations, the pore-forming treatment method includes at least one of using a pore-forming agent, chemical etching, and a template method, and any other method that can further increase the porosity and specific surface area of the fullerene can also be used. Among them, the method of using a pore-forming agent to form pores in fullerene includes but is not limited to, after mixing the fullerene with the pore-forming agent, under certain pore-forming conditions, the pore-forming agent generates a gaseous substance to form pores in the fullerene, thereby increasing its surface area and porosity. The chemical etching method includes but is not limited to, using a strong oxidizing chemical substance to destroy some carbon-hydrogen bonds in the fullerene, increase defects in the fullerene, and increase the specific surface area and porosity. The template method of pore-forming treatment uses a template agent as a template for the pore-forming structure to further increase the pore structure in the fullerene material, thereby increasing its specific surface area and porosity.
[0153] In some possible implementations, the heteroatoms include at least one of N, S, O, B, and P; doping with these heteroatoms can improve the ionic and electronic conductivity of fullerenes, improve the migration efficiency of ions in the composite membrane, and weaken the polarization phenomenon; at the same time, it can change the growth direction of lithium dendrites and improve the safety performance of the composite membrane.
[0154] In some possible implementations, the organic functional groups include at least one of a pyrrole group, a thiophene group, and an aniline group. Modification of these electron-rich organic functional groups allows the composite membrane to form ion pairs in the electrolyte. These ion pairs can conduct electricity in the electrolyte solution, thereby increasing the conductivity of the electrolyte solution and thus improving ionic conductivity. This improves the efficiency of ion migration in the composite membrane, weakens polarization, and reduces the internal resistance of the composite membrane.
[0155] In some possible implementations, the inorganic material includes at least one of MoO2, MgO, and Al2O3. Combining MoO2 with fullerenes can significantly improve the fullerene's electrical conductivity and chemical stability. Combining fullerenes with magnesium oxide or aluminum oxide can enhance the heat resistance of the modified layer, thereby improving the thermal stability of the composite separator.
[0156] In some possible implementations, the average particle size of the fullerene material in the modified layer is 0.1 μm to 5 μm; fullerenes with this average particle size are more conducive to forming a uniform film layer and a thin modified layer, improving the uniformity of the distribution of fullerene particles in the film layer, and facilitating the size design of the composite diaphragm.
[0157] In some possible implementations, the fullerene includes C 20 、C 60 、C 70 、C 76 、C 80 At least one of them; these fullerenes have special optical properties, electrical conductivity and chemical properties due to their unique zero-dimensional structure.
[0158] In some possible implementations, the shape of the fullerene material in the modified layer includes at least one of a spherical shape, an ellipsoidal shape, a columnar shape, and a tubular shape.
[0159] In the above step S20, two base film layers are obtained, and the fullerene slurry is made into a modified layer between the two base film layers to obtain a composite membrane. The modified layer is prepared between the two base film layers. The base film layers on both sides can not only provide a load matrix for the modified layer, but also play a supporting and protective role, which is conducive to maintaining the stability of the modified layer and avoiding the powdering of the modified layer during the charge and discharge process, which affects the stability of the battery's electrochemical performance. At the same time, it can reduce the amount of materials such as adhesives in the modified layer, avoid the excessive introduction of other materials that affect the air permeability and ion migration efficiency of the composite membrane, and help further reduce the thickness of the modified layer and the overall thickness of the composite membrane, which is conducive to achieving lightweighting.
[0160] In some possible implementations, the preparation of the modified layer includes the steps of: coating a fullerene slurry on one surface of a base film layer, laminating another base film layer to the surface of the coated slurry, and drying and curing the slurry to form a modified layer between the two base film layers, thereby obtaining a composite separator. In some specific embodiments, the two base film layers can be placed on separate unwinding rollers, and the fullerene slurry can be applied to the surface of one base film layer. The base film layer on the other unwinding roller can then be laminating to the coated surface of the slurry, followed by drying and pressing to form a modified layer between the two base film layers, thereby obtaining a composite separator.
[0161] In some possible implementations, the thickness of the modified layer is 0.5 μm to 2 μm; this thickness can effectively improve the comprehensive properties of the composite diaphragm, such as mechanical properties, heat resistance, and wettability, and is conducive to the lightweight design of the composite diaphragm.
[0162] In some possible implementations, the modified layer comprises 10% to 20% by weight of the composite membrane. At this weight percentage, the modified layer can effectively improve the mechanical properties, heat resistance, wettability, stability, and other characteristics of the composite membrane, and also facilitates lightweight design of the composite membrane.
[0163] In some possible implementations, the thickness of the base film layer is 3μm to 7μm; the base film layer of this thickness fully ensures the mechanical properties, air permeability, heat resistance, liquid absorption rate and other characteristics of the diaphragm, and is conducive to reducing the overall thickness of the composite diaphragm, thereby realizing a lightweight design of the composite diaphragm.
[0164] In some possible implementations, the thickness of the composite diaphragm is not higher than 15 μm; through the application of the modified layer in the composite diaphragm and the structural design of arranging the modified layer on two adjacent base membrane layers, the mechanical properties, air permeability, heat resistance, wetting properties and other characteristics of the composite diaphragm can be improved, and the thickness of the composite diaphragm can be reduced to no more than 15 μm, thereby achieving lightweight diaphragm.
[0165] In some possible implementations, the porosity of the base membrane layer is 30% to 70%; under this porosity condition, the base membrane layer has good air permeability, which is beneficial to the migration and transmission of ions in the diaphragm and reduces the impedance of the battery.
[0166] In some possible implementations, the average pore size of the base membrane layer is 100nm to 800nm. Under this average pore size condition, the submicron pore size of the separator is sufficient to prevent the direct passage of electrode particles. This allows the base membrane layer to have an appropriate pore size, which not only facilitates ion migration and transmission, but also helps prevent direct contact between electrode particles and prevent electrode particles from directly passing through the separator. This avoids the possibility of perforation of the separator due to excessively large pores, which could cause micro-short circuits in the battery, and also avoids the possibility of increased resistance due to excessively small pores.
[0167] In some possible implementations, the surface density of the base film layer is 2 g / m 2 ~10g / m 2 Under this surface density condition, the porosity of the base membrane layer is ensured, which is beneficial to improving the air permeability of the base membrane layer, facilitating the migration and transmission of ions in the diaphragm, avoiding short circuits, and is beneficial to the lightweight design of the composite diaphragm.
[0168] In some possible implementations, the base film layer comprises at least one of polypropylene, polyethylene, glass fiber, and polyvinylidene fluoride. These base film materials all possess excellent electrical insulation properties and maintain chemical stability over a wide temperature and voltage range. This facilitates the production of a thin, highly uniform base film layer with appropriate porosity and pore size. This allows for rapid wetting of the electrolyte, isolating electrons while maintaining the free flow of ions to meet the battery's requirements for high energy, high power, and cycle performance. Furthermore, the base film layer possesses a certain degree of mechanical strength and processing toughness to meet the battery's discharge requirements during assembly and use.
[0169] In some possible implementations, the composite separator has an air permeability of 300s / (100cc) to 500s / (100cc); this fully ensures efficient ion migration and transmission within the separator while preventing other substances, such as electrons, from penetrating the composite separator and affecting the stability of the battery system. This also ensures good wettability of the composite separator with the electrolyte. This improved wettability improves the separator's affinity with the electrolyte, expanding the contact surface between the separator and the electrolyte, thereby increasing ionic conductivity and improving the battery's charge and discharge performance and capacity.
[0170] In some possible implementations, the transverse tensile strength of the composite diaphragm is not less than 1000 kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm 2 The sufficient tensile strength of the composite diaphragm in the transverse and longitudinal directions can prevent the diaphragm from deforming and improve the operating stability of the diaphragm.
[0171] In a third aspect, an embodiment of the present application provides a battery cell, which includes a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator includes the above-mentioned composite separator, or the composite separator prepared by the above-mentioned method.
[0172] The battery cells of the present embodiment utilize a composite separator having excellent mechanical properties, heat resistance, wettability, stability, ionic and electronic conductivity, and lightweight design. This improves the rate capability, energy density, cycle stability, and safety of the battery cells.
[0173] This application does not specifically limit the positive electrode, negative electrode, electrolyte, etc. in the battery cells of the embodiments, and is applicable to any battery system.
[0174] In some possible implementations, the negative electrode materials in the battery cells include but are not limited to carbon materials such as graphite, soft carbon (such as coke), hard carbon, or nitrides, tin-based oxides, tin-based oxides, tin alloys, and silicon-based negative electrode materials.
[0175] In some possible implementations, the preparation of the negative electrode sheet includes the following steps: mixing the negative electrode material with a conductive agent such as conductive carbon black, a binder such as carboxymethyl cellulose and styrene-butadiene rubber, and a solvent such as water in a mass ratio of (80-99):(1-5):(2-10):100 to form a positive electrode mixed slurry, vacuum degassing, discharging, coating on a coating machine, and obtaining a negative electrode sheet after rolling, slitting, and die-cutting.
[0176] In some possible implementations, the positive electrode materials in the battery cells include metal oxides, such as lithium cobalt oxide, lithium nickel oxide, nickel-cobalt-manganese ternary materials, lithium nickel-cobalt-aluminum oxide, lithium-rich manganese-based materials, lithium manganese oxide, lithium nickel manganese oxide, ferroferric oxide, lithium vanadate, etc.; polyanionic salts such as phosphates, silicates, sulfates, borates, and titanates, such as lithium iron phosphate, lithium manganese phosphate, lithium iron manganese phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, lithium iron silicate, lithium iron fluorosulfate, lithium iron borate, and lithium iron titanate, etc.; and fluorides, sulfides, and selenides, such as iron trifluoride, cobalt trifluoride, nickel trifluoride (NiF3), titanium disulfide, iron disulfide, molybdenum disulfide, and niobium triselenide.
[0177] In some possible implementations, the preparation of the positive electrode sheet includes the following steps: mixing the positive electrode material with a conductive agent such as conductive carbon black, a binder such as polyvinylidene fluoride, and a solvent such as N-methylpyrrolidone in a mass ratio of (80-99):(1-5):(2-10):100 to form a positive electrode mixed slurry, vacuum degassing, discharging, coating on a coating machine, and obtaining a positive electrode sheet after rolling, slitting, and die-cutting.
[0178] In some possible implementations, the electrolyte in the battery cell includes at least one soluble metal salt.
[0179] In some possible implementations, battery cell types include lithium-ion batteries, as well as new types of batteries such as sodium-ion batteries, lithium-air batteries, and lithium metal batteries.
[0180] In some possible implementations, the present invention has no particular restrictions on the shape of the battery cell, which may be cylindrical, square, or any other shape. FIG6 shows a battery cell 05 with a square structure as an example.
[0181] In some embodiments, as shown in FIG7 , the outer packaging of the battery cell 05 may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 05 may be one or more, which can be adjusted according to actual needs. Among them, the composite diaphragm of the above embodiment is arranged between the positive electrode sheet and the negative electrode sheet.
[0182] In some possible implementations, the battery cells according to the present application may be assembled into a battery module. The battery module may contain multiple battery cells, and the specific number may be adjusted according to the application and capacity of the battery module.
[0183] In a fourth aspect, an embodiment of the present application provides a battery module, which includes a plurality of the above-mentioned battery cells.
[0184] The battery module of the embodiment of the present application includes battery cells with the above-mentioned specific high-rate performance, energy density, cycle stability and safety performance characteristics, thereby also improving the rate performance, energy density, cycle stability and safety performance of the battery module.
[0185] In one possible embodiment, as shown in FIG8 , a schematic diagram of an exemplary battery module 06 is shown. In the battery module 06 , multiple battery cells 05 may be arranged sequentially along the length of the battery module 06 . Alternatively, the arrangement may be arranged in any other manner. Furthermore, the multiple battery cells 05 may be secured using fasteners.
[0186] In a possible embodiment, the battery module 06 may further include a housing having a receiving space, and the plurality of battery cells 05 are received in the receiving space.
[0187] In a possible implementation, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0188] In a fifth aspect, an embodiment of the present application provides a battery pack, which includes a plurality of the above-mentioned battery cells or battery modules.
[0189] Since the battery pack of the embodiment of the present application includes the above-mentioned battery module with high rate performance, energy density, cycle stability and safety performance, the rate performance, energy density, cycle stability and safety performance of the battery pack are also improved.
[0190] In one possible embodiment, as shown in Figures 9 and 10 , a schematic diagram of an exemplary battery pack 07 may include a battery box and multiple battery modules 06 disposed within the battery box. The battery box includes an upper box body 71 and a lower box body 72. The upper box body 71 covers the lower box body 72 and forms an enclosed space for accommodating the battery modules 06. The multiple battery modules 06 may be arranged in any manner within the battery box.
[0191] In a sixth aspect, an embodiment of the present application provides an electrical device, which includes the above-mentioned battery cell, or the above-mentioned battery module, or the above-mentioned battery pack.
[0192] The electrical equipment of the embodiment of the present application includes the above-mentioned battery cells, battery modules or battery packs with high rate performance, energy density, cycle stability and safety performance, thereby improving the power safety and stability of the electrical equipment.
[0193] In a possible implementation, the electrical equipment may select the above-mentioned battery cells, battery modules or battery packs according to its usage requirements.
[0194] In one possible embodiment, the electrical device may be, but is not limited to, a mobile device, such as a mobile phone, a laptop computer, etc., or an electric vehicle, such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., or an electric train, a ship, a satellite, an energy storage system, etc.
[0195] In one possible embodiment, the electric device may be a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. In order to meet the high power and high energy density requirements of such electric devices, the above-mentioned battery pack or battery module may be used.
[0196] In some specific embodiments, a schematic diagram of an exemplary electric device is shown in FIG11 . The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electric device, a battery pack or battery module may be used.
[0197] In other possible implementations, the electrical device may be a tape recorder, a radio, an electronic learning machine, a mobile phone, a tablet computer, a laptop computer, etc. Such electrical devices are generally required to be lightweight and thin, and the battery cells in the above embodiments may be used as power sources.
[0198] Example
[0199] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0200] Example 1
[0201] An embodiment of the present application provides a composite diaphragm, comprising a polyethylene-based film layer with a thickness of 5 μm, an N / P co-doped fullerene material intermediate coating layer with a thickness of 1 μm, and a polypropylene-based film layer with a thickness of 6 μm, which are sequentially laminated and bonded.
[0202] Its preparation comprises the following steps:
[0203] ①N / P co-doped modified C 60 Preparation: 150 mg of C 60 Dissolve in 50ml of toluene and ultrasonicate for 30 minutes. Add ethylenediamine dropwise into the solution and ultrasonicate for 25 minutes. Then, add tetrabutylammonium hydroxide and 2ml of H2O2 dropwise into the mixed solution and stir at 60°C for 2 hours. The precipitate was collected by precipitation method and washed three times with ethanol. On this basis, 3ml of phytic acid (cyclohexanehexol hexaphosphate) solution of different volumes was added to the ethanol dispersion, stirred vigorously at room temperature for 12h, and the precipitate was collected. Maintain at 900°C for 2h under N2 atmosphere. N / P co-doped C with improved electronic conductivity was obtained. 60 , the average particle size is about 200nm.
[0204] ② Modify C 60 , polyacrylate, and carboxymethyl cellulose are uniformly mixed in a solvent in a mass ratio of 3:3:1 to form an aqueous slurry with a solid content of 25 wt % and a viscosity of 100 mPa·s to prepare a fullerene slurry.
[0205] ③ The fullerene slurry is coated onto a 5μm polyethylene PE base film through a coating machine. The other unwinding roller is a 6μm polypropylene PP base film. The slurry is applied to one surface of the PE base film by extrusion to form a wet coating with a thickness of about 1μm. It is transferred to an oven and baked at 60°C for 2 minutes. The roller is then reversed and the PP base film is pressed onto the wet coating with a pressure of 1000Mpa to obtain a composite diaphragm.
[0206] Example 2
[0207] This embodiment provides a composite separator comprising a 5-μm-thick polyethylene-based film layer, a 1-μm-thick N / P co-doped fullerene material intermediate coating layer, and a 6-μm-thick polypropylene-based film layer laminated in sequence. This embodiment differs from Example 1 in that the amount of phytic acid solution added in step ① is 5 ml.
[0208] Example 3
[0209] This embodiment provides a composite separator comprising a 5-μm-thick polyethylene-based film layer, a 1-μm-thick N / P co-doped fullerene material intermediate coating layer, and a 6-μm-thick polypropylene-based film layer laminated in sequence. This embodiment differs from Example 1 in that the amount of phytic acid solution added in step 1 is 8 ml.
[0210] Example 4
[0211] This embodiment provides a composite separator comprising a 5-μm-thick polyethylene-based film layer, a 1-μm-thick N / P co-doped fullerene material intermediate coating layer, and a 6-μm-thick polypropylene-based film layer laminated in sequence. This embodiment differs from Example 1 in that the amount of phytic acid solution added in step ① is 10 ml.
[0212] Example 5
[0213] This embodiment provides a composite membrane comprising a 5-μm-thick polyethylene-based film layer, a 0.5-μm-thick N / P-codoped fullerene material intermediate coating layer, and a 6-μm-thick polypropylene-based film layer laminated in sequence. This embodiment differs from Example 1 in that the N / P-codoped fullerene material intermediate coating layer is 0.5 μm thick.
[0214] Example 6
[0215] This embodiment provides a composite separator comprising a 5-μm-thick polyethylene-based film layer, a 2-μm-thick N / P co-doped fullerene material intermediate coating layer, and a 6-μm-thick polypropylene-based film layer laminated in sequence. This separator differs from Example 1 in that the N / P co-doped fullerene material intermediate coating layer is 2 μm thick.
[0216] Example 7
[0217] An embodiment of the present application provides a composite diaphragm, comprising a polyethylene-based film layer with a thickness of 5 μm, a composite α-alumina and N / P co-doped fullerene material intermediate coating with a thickness of 1 μm, and a polypropylene-based film layer with a thickness of 6 μm, which are laminated and bonded in sequence.
[0218] Its preparation comprises the following steps:
[0219] ① Preparation of composite α-alumina and N / P co-doped modified C60 coating: The N / P-doped modified C60 prepared in Example 1 was 60 , α-alumina, polyacrylate, and carboxymethyl cellulose were uniformly mixed in deionized water in a mass ratio of 4:2:1:0.5 to form an aqueous slurry with a solid content of 25 wt % and a viscosity of 100 mPa·s to prepare a fullerene slurry.
[0220] ② The fullerene slurry is coated onto a 5μm polyethylene PE base film through a coating machine. The other unwinding roller is a 5μm polypropylene PP base film. The slurry is applied to one surface of the PE base film by extrusion to form a wet coating with a thickness of about 1μm. It is transferred to an oven and baked at 60°C for 2 minutes. The roller is then reversed and the PP base film is pressed onto the wet coating with a pressure of 1000Mpa to obtain a composite diaphragm.
[0221] Example 8
[0222] An embodiment of the present application provides a composite diaphragm, comprising a polyethylene-based film layer with a thickness of 5 μm, a pore-forming fullerene material intermediate coating layer with a thickness of 1 μm, and a polypropylene-based film layer with a thickness of 6 μm, which are laminated and bonded in sequence.
[0223] Its preparation comprises the following steps:
[0224] ① Pore-forming modified C 60 Preparation: 0.3 mmol C 60 Fullerene and dimethoxymethane were mixed in a molar ratio of 10:1, and the mixture was added to 120ml of anhydrous nitrobenzene and 3.36mmol of aluminum chloride, and placed in an oven at 150℃ for 12h. After cooling, the solid was collected by centrifugation, washed with deionized water, and dried in a vacuum at 120℃. The dried solid was dissolved in a minimum of 6ml of CH2Cl2, and a large number of insoluble particles were filtered out. The clear CH2Cl2 solution was dropped into a mixture of 1:1 ether and hexane, stirred vigorously, and the monoadduct was precipitated. The precipitate was collected as a porous aromatic mixture composed of fullerene material molecules. Through the monoaddition organic coupling reaction of fullerene and dimethoxy compounds, C 60 Fullerene-based porous aromatic frameworks, in addition to being chemically and thermally stable, also have a high specific surface area.
[0225] ② Modify C 60 , polyacrylate, and carboxymethyl cellulose are uniformly mixed in a solvent in a mass ratio of 3:3:1 to form an aqueous slurry with a solid content of 25 wt % and a viscosity of 100 mPa·s to prepare a fullerene slurry.
[0226] ③ The fullerene slurry is coated onto a 5μm polyethylene PE base film through a coating machine. The other unwinding roller is a 5μm polypropylene PP base film. The slurry is applied to one surface of the PE base film by extrusion to form a wet coating with a thickness of about 1μm. It is transferred to an oven and baked at 60°C for 2 minutes. The roller is then reversed and the PP base film is pressed onto the wet coating with a pressure of 1000Mpa to obtain a composite diaphragm.
[0227] Example 9
[0228] An embodiment of the present application provides a composite diaphragm, comprising a polyethylene-based film layer with a thickness of 5 μm, a nitro-modified fullerene material intermediate coating layer with a thickness of 1 μm, and a polypropylene-based film layer with a thickness of 6 μm, which are laminated and bonded in sequence.
[0229] Its preparation comprises the following steps:
[0230] ①Nitro-modified C 60 Preparation: 0.6g C 60 Add 500ml of chlorobenzene and stir at 600rpm / min for 1h at room temperature. Use the gas from the reaction of Cu and concentrated nitric acid to continuously pass into the solution under stirring. After 3h of reaction, the solvent is continuously evaporated to obtain nitrofullerene material. Highly polar nitro-modified C 60 It has the function of improving the compatibility between the composite diaphragm and the electrolyte components, and increasing the lyophilicity of the diaphragm.
[0231] ② Modify the nitro group into C 60 , polyacrylate, and carboxymethyl cellulose are uniformly mixed in a solvent in a mass ratio of 3:3:1 to form an aqueous slurry with a solid content of 25 wt % and a viscosity of 100 mPa·s to prepare a fullerene slurry.
[0232] ③ The fullerene slurry is coated onto a 5μm polyethylene PE base film through a coating machine. The other unwinding roller is a 5μm polypropylene PP base film. The slurry is applied to one surface of the PE base film by extrusion to form a wet coating with a thickness of about 1μm. It is transferred to an oven and baked at 60°C for 2 minutes. The roller is then reversed and the PP base film is pressed onto the wet coating with a pressure of 1000Mpa to obtain a composite diaphragm.
[0233] Example 10
[0234] The present invention provides a fullerene composite membrane, comprising a polyethylene-based film layer with a thickness of 5 μm, an unmodified fullerene material C with a thickness of 1 μm, and a laminated film. 60 Intermediate coating and polypropylene base film layer with a thickness of 6μm.
[0235] Its preparation comprises the following steps:
[0236] ①C 60 , polyacrylate, and carboxymethyl cellulose are uniformly mixed in a solvent in a mass ratio of 3:3:1 to form an aqueous slurry with a solid content of 25 wt % and a viscosity of 100 mPa·s to prepare a fullerene slurry.
[0237] ② The fullerene slurry is coated onto a 5μm polyethylene PE base film through a coating machine. The other unwinding roller is a 5μm polypropylene PP base film. The slurry is applied to one surface of the PE base film by extrusion to form a wet coating with a thickness of about 1μm. It is transferred to an oven and baked at 60°C for 2 minutes. The roller is then reversed and the PP base film is pressed onto the wet coating with a pressure of 1000Mpa to obtain a composite diaphragm.
[0238] Comparative Example 1
[0239] This comparative example provides a double-layer composite diaphragm, using a 5μm thick PE microporous film and a 6μm thick PP microporous film as the substrate layer. First, a polycarbosilane PCS polymer coating is sprayed on a 5μm thick PE surface on one side, with a spraying amount of 0.5mg / m 2 To ensure consistency with the example, the membrane was first baked at 60° C. for 2 minutes and then pressed against the PP base film on the other side at a pressure of 1000 MPa to obtain a fullerene-free composite membrane.
[0240] The thickness, air permeability, specific surface area, surface density, thermal shrinkage, liquid absorption and other properties of the composite diaphragm in the above embodiments and comparative examples were tested respectively. The test method is as follows:
[0241] 1. Film thickness measurement: The film thickness of the separator was measured at five points within an area of 100 mm x 100 mm using a contact thickness gauge, and the average film thickness was calculated.
[0242] 2. Air permeability measurement: Air permeability (Gurley value) is measured in accordance with JIS P8117:2009, and the gas used in the measurement is air.
[0243] 3. Specific surface area measurement: The nitrogen adsorption isotherms of fullerene materials were measured on ASAP2020 (Micromeritics), and the specific surface area of the isotherm (SBET) was calculated using the Brunauer-Emmet-Teller method.
[0244] 4. Surface density measurement: Cut the isolation film into a circle with a radius R of 50 mm, and calculate its surface density after weighing it using an electronic balance.
[0245] 5. Thermal shrinkage measurement: Cut the isolation film into 100×50 mm in size and place it in an oven at 130°C / 1h. Use a vernier caliper to measure the shrinkage degree of the isolation film in the longitudinal direction (MD) and the transverse direction (TD).
[0246] 6. Liquid Absorption Test: Cut the separator sample into a 5cm x 5cm square and weigh it. Then, soak the separator in electrolyte for 30 minutes, remove it, and gently blot the electrolyte off the membrane surface with a dust-free paper. The electrolyte used was a 1 mol / L LiPF6 ethylene carbonate (EC) solution. Liquid Absorption = (Weight after immersion - Weight before immersion) / Weight before immersion × 100%.
[0247] The test results are shown in Table 1 below:
[0248] Table 1
[0249] From the test results in Table 1 above, it can be seen that the composite membranes prepared in the examples of the present application and provided with a fullerene material functional layer have shown improved performance in terms of air permeability, specific surface area, surface density, thermal shrinkage, and liquid absorption compared to the composite membrane of Comparative Example 1 that does not have a fullerene material layer. Specifically, the specific surface area of the composite membranes of Examples 1 to 4 containing a fullerene layer doped with heteroatoms is greater than that of the composite membrane of Comparative Example 1 that does not have a fullerene material layer, while the surface density is less than that of Comparative Example 1, and the liquid absorption rate thereof has also increased to a certain extent. The thickness of the fullerene material layer in the composite membrane of Example 5 is only 0.5 μm. Although the thickness of the intermediate coating is lower than that of Example 1 (1 μm), the air permeability, specific surface area, surface density, thermal shrinkage, liquid absorption and other properties are comparable to those of Example 1 in all aspects, and all aspects of the performance are significantly higher than those of the composite membrane of Comparative Example 1 that does not have a fullerene material modified layer. Therefore, even if the modified coating containing fullerenes is applied to a low thickness in the composite membrane, it can still significantly improve the composite membrane's properties, such as air permeability, thermal stability, and liquid absorption rate. This helps reduce the amount of fullerene material layer used in the composite membrane, thereby achieving a lightweight composite membrane design while maintaining membrane performance. Furthermore, increasing the thickness of the fullerene material layer in the composite membrane, as in Example 6, further improves various aspects of the composite membrane's performance.
[0250] In Example 7, fullerene is simultaneously compounded with α-alumina and N / P co-doped, and the heat resistance is better improved by modifying the fullerene double layer, while also showing the high specific surface area and good liquid absorption capacity of fullerene. Example 8 is formed by the monoaddition organic coupling reaction of fullerene and dimethoxy compound to form C 60 The fullerene-based porous aromatic framework has not only chemical and thermal stability but also a high specific surface area. Therefore, the composite membrane has the highest specific surface area, the lowest surface density and the best liquid absorption rate. 60 It has the function of improving the compatibility between the composite diaphragm and the electrolyte components, and increasing the lyophilicity of the composite diaphragm, thus having the best liquid absorption rate.
[0251] Furthermore, a comparison of Examples 1-9 and Example 10 demonstrates that the composite membranes prepared by modifying the fullerene material exhibit certain improvements in air permeability, specific surface area, areal density, thermal shrinkage, and liquid absorption. Applying the higher-performance modified fullerene material between the base membrane layers not only improves the composite membrane's overall performance, including mechanical properties, heat resistance, and ionic and electronic conductivity, but also allows for a smaller amount of fullerene material to meet application requirements, reducing the thickness of the modified layer within the composite membrane and thus facilitating a lightweight design.
[0252] By designing and preparing batteries, we analyze the effect of the fullerene P doping level on the inhibition of lithium deposition during the cycle. The battery preparation steps are as follows:
[0253] 1. The positive electrode uses lithium iron phosphate LFP material, with the active material accounting for 90%, the binder polyvinylidene fluoride PVDF accounting for 5%, and the conductive agent accounting for 5%. The coating weight of the electrode is 0.175mg / 1540mm 2 , compacted density is 1.65g / cm 3 The electrode is prepared through processes such as stirring, coating, and cold pressing.
[0254] 2. The negative electrode uses artificial graphite, with active materials accounting for 80%, binder styrene-butadiene rubber (SBR) and dispersant sodium carboxymethyl cellulose (CMC) accounting for 10wt%, and conductive agent accounting for 10wt%. The electrode is prepared through stirring, coating, cold pressing and other processes, and the final electrode coating weight is 0.265mg / 1540mm 2 The compacted density of the pole piece is 3.45g / cm 3 . Negative electrode area capacity ratio (N / P=1.01).
[0255] 3. The diaphragm is the composite diaphragm prepared in the above embodiment, and the electrolyte is an EC solution with a composition of 1M NaPF6.
[0256] 4. Assemble the above electrodes and electrolyte into a laminated battery cell, and use aluminum-plastic film as the packaging material.
[0257] Lithium plating inhibition test: At a test temperature of 25°C, the lithium-ion battery was charged to 3.6V at a constant current of 1.5C, left to stand for 5 minutes, and then discharged to 2.25V at a constant current of 1.0C. This cycle was repeated 100 times, and the occurrence of short circuits was counted. The test results are shown in Table 2 below:
[0258] Table 2
[0259] From the test results in Table 2 above, it can be seen that N / P co-doped fullerene materials can improve the conductivity of the battery. During the operation of the battery, the dendrite growth contacts the C60 Due to its strong electron-accepting properties and improved conductivity, it can change the direction of dendrite growth and prevent battery short circuits. Among them, the fullerene prepared by adding 10ml of phytic acid in Example 4 has the best effect in inhibiting lithium precipitation, indicating that effective element doping improves the conductivity of fullerene and has a better inhibitory effect when it comes into contact with lithium dendrites.
[0260] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A composite diaphragm, characterized in that: The composite diaphragm comprises a plurality of laminated base film layers and at least one modified layer arranged between two adjacent base film layers; the raw material components of the modified layer contain fullerene materials.
2. The composite diaphragm according to claim 1, characterized in that: The raw material components of the modified layer include fullerenes modified by at least one of doping with heteroatoms, modifying organic functional groups, composite inorganic materials, and pore-forming treatment.
3. The composite diaphragm according to claim 2, characterized in that: The thickness of the modified layer is not more than 5 μm.
4. The composite diaphragm according to claim 3, characterized in that: The thickness of the modified layer is not more than 3 μm.
5. The composite diaphragm according to claim 4, characterized in that: The thickness of the modified layer is 0.5 μm to 2 μm; And / or, the base film layer has a thickness of 3 μm to 7 μm.
6. The composite diaphragm according to any one of claims 2 to 5, characterized in that: The heteroatoms include non-metallic elements of the IIIA to VIA main groups; And / or, the organic functional group includes at least one of a pyrrole group, a thiophene group, and an aniline group; and / or, the inorganic material comprises a metal oxide; And / or, the pore-forming treatment method includes at least one of a pore-forming agent, chemical etching, and a template method.
7. The composite diaphragm according to claim 6, characterized in that: The heteroatom includes at least one of N, S, O, B, and P; And / or, the inorganic material includes at least one of MoO2, MgO, and Al2O3.
8. The composite diaphragm according to any one of claims 1 to 7, characterized in that: The fullerene material satisfies at least one of the following characteristics: The average particle size of the fullerene material is 0.1 μm to 5 μm; In the fullerene material, the fullerene includes C 20 , C 60 , C 70 , C 76 , C 80 At least one of; The shape of the fullerene material includes at least one of spherical, ellipsoidal, cylindrical, and tubular; The specific surface area of the fullerene material is 100 m 2 / g~500m 2 / g; The total pore volume of the fullerene material is 0.01 cm 3 / g~0.5cm 3 / g; The average pore diameter of the mesopores of the fullerene material is 2nm to 20nm.
9. The composite diaphragm according to any one of claims 1 to 8, characterized in that: The modified layer also contains a binder.
10. The composite diaphragm according to any one of claims 1 to 9, characterized in that: The base film layer satisfies at least one of the following characteristics: The porosity of the base film layer is 30% to 70%; The average pore size of the basement membrane layer is 100nm to 800nm; The surface density of the base film layer is 2g / m 2 ~10g / m 2 ; The base film layer includes at least one material selected from the group consisting of polypropylene, polyethylene, glass fiber, and polyvinylidene fluoride.
11. The composite diaphragm according to any one of claims 1 to 10, characterized in that: The composite diaphragm satisfies at least one of the following characteristics: The air permeability of the composite membrane is 300s / (100cc) to 500s / (100cc); The transverse tensile strength of the composite diaphragm is not less than 1000kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm 2 ; The thickness of the composite diaphragm is not more than 15 μm; The mass percentage of the modified layer in the composite diaphragm is 10% to 20%.
12. The composite diaphragm according to any one of claims 1 to 11, characterized in that: The transverse tensile strength of the composite diaphragm is not higher than 1700 kg / cm 2 , longitudinal tensile strength is not higher than 1500kg / cm 2 ; And / or, the thickness of the composite membrane is not higher than 7 μm to 15 μm.
13. A method for preparing a composite diaphragm, characterized in that: The following steps are involved: preparing a fullerene slurry; Obtain at least two base film layers, and prepare a modified layer by forming the fullerene slurry between two adjacent base film layers to obtain to the composite diaphragm.
14. The method for preparing a composite diaphragm according to claim 13, characterized in that: The step of preparing the fullerene slurry comprises: after modifying the fullerene, mixing the fullerene material with a dispersant, a binder and a solvent to form a mixed slurry to obtain the fullerene slurry.
15. The method for preparing a composite diaphragm according to claim 14, characterized in that: The method for modifying the fullerene includes at least one of: doping with heteroatoms, modifying organic functional groups, composite inorganic materials, and pore-forming treatment.
16. The method for preparing a composite diaphragm according to claim 15, characterized in that: The heteroatom includes at least one of N, S, O, B, and P; And / or, the organic functional group includes at least one of a pyrrole group, a thiophene group, and an aniline group; And / or, the inorganic material includes at least one of MoO2, MgO, and Al2O3; And / or, the pore-forming treatment method includes at least one of using a pore-forming agent, chemical etching, and a template method.
17. The method for preparing a composite diaphragm according to any one of claims 14 to 16, characterized in that: In the fullerene slurry, the mass ratio of the fullerene material, the binder and the dispersant is (60-90): (5-20): (1-20); and / or, in the fullerene slurry, the mass ratio of the total mass of the fullerene material, the binder, and the dispersant to the solvent is (0.1-0.6):1; And / or, the binder includes: at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylonitrile, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride, and polyimide; And / or, the dispersant includes: at least one of polyacrylate, polyacrylamide, and long-chain fatty acid; And / or, the solvent includes: at least one of deionized water, N-methylpyrrolidone, ethanol, dimethylformamide, dimethylacetamide, acetone, and dichloromethane.
18. The method for preparing a composite diaphragm according to any one of claims 13 to 17, characterized in that: The preparation of the modified layer includes the steps of: coating the fullerene slurry on one side of the base film layer, laminating the other base film layer with the coating slurry surface, drying and curing to form the modified layer between the two base film layers, and obtaining the composite diaphragm.
19. The method for preparing a composite diaphragm according to any one of claims 14 to 18, characterized in that: The thickness of the modified layer is 0.5 μm to 2 μm; And / or, the average particle size of the fullerene material is 0.1 to 5 μm; And / or, in the fullerene material, the fullerene includes C 20 , C 60 , C 70 , C 76 , C 80 At least one of; And / or, the shape of the fullerene material includes at least one of spherical, ellipsoidal, columnar, and tubular.
20. The method for preparing a composite diaphragm according to any one of claims 13 to 19, characterized in that: The base film layer satisfies at least one of the following characteristics: The porosity of the base film layer is 30% to 70%; The average pore size of the basement membrane layer is 100nm to 800nm; The surface density of the base film layer is 2g / m 2 ~10g / m 2 ; The thickness of the base film layer is 3 μm to 7 μm; The base film layer includes at least one material selected from the group consisting of polypropylene, polyethylene, glass fiber, and polyvinylidene fluoride.
21. The method for preparing a composite diaphragm according to any one of claims 13 to 20, characterized in that: The composite diaphragm satisfies at least one of the following characteristics: The air permeability of the composite membrane is 300 to 500 s / (100 cc); The transverse tensile strength of the composite diaphragm is not less than 1000kg / cm 2 , longitudinal tensile strength not less than 1200kg / cm 2 ; The thickness of the composite diaphragm is not more than 15 μm; The mass percentage of the modified layer in the composite diaphragm is 10% to 20%.
22. A battery cell, characterized in that: The battery cell comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator comprises the composite separator according to any one of claims 1 to 12, or a composite separator prepared by the method according to any one of claims 13 to 21.
23. A battery module, characterized in that: The battery module comprises a plurality of battery cells as claimed in claim 22 .
24. A battery pack, characterized in that: The battery pack includes a plurality of battery cells as described in claim 22 or a battery module as described in claim 23.
25. An electrical device, characterized in that: The electrical equipment includes the battery cell as claimed in claim 22, or the battery module as claimed in claim 23, or the battery pack as claimed in claim 24.
Citation Information
Patent Citations
Composite diaphragm as well as preparation method and application thereof
CN118825556A
Three-layer lithium battery diaphragm and preparation method thereof
CN104022249A
Lithium ion battery diaphragm, manufacturing method and application thereof
CN110828757A
Separator for electrochemical device, electrochemical device and electronic device
CN113261151A
Lithium metal battery diaphragm, preparation method thereof and lithium metal battery
CN113690544A