Mesoporous molecular sieve-based solid acid-base catalyst, preparation method therefor, and application thereof in synthesis of transformer insulating oil
Through the use of mesoporous molecular sieve-based solid acid-base catalysts, the problem of single alkali catalyst poisoning of active sites in cottonseed oil transesterification is solved, efficient transesterification and esterification of cottonseed oil are achieved, the raw material grade requirements are reduced, and the Preparation efficiency and cost of insulating oil.
Patent Information
- Application Number
- PCT/CN2024/070549
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-01-04
- Publication Date
- 2024-10-24
AI Technical Summary
When the existing technology uses a single alkali catalyst to transesterify cottonseed oil, it is difficult to effectively process raw oil with high acid value, which leads to poisoning of active sites in the transesterification reaction and affects the preparation efficiency and quality of insulating oil.
A mesoporous molecular sieve-based solid acid-base catalyst is used. The catalyst separates acidic and basic sites through the nanosphere hard template and silicon-oxygen network structure, forming a topological structure in which macropores and mesopores are interconnected to avoid free oleic acid from affecting basic sites. Points are poisoned, and the soft template is removed through high-temperature roasting to generate metal oxides to form an MCM-type mesoporous molecular sieve-based solid acid-base catalyst.
It achieves effective transesterification and esterification of high acid value cottonseed oil, extends the grade requirements of raw materials, reduces the cost of insulating oil synthesis, and maintains the long life and high activity of the catalyst.
Smart Images

Figure CN2024070549_24102024_PF_FP_ABST
Abstract
Description
A mesoporous molecular sieve-based solid acid-base catalyst, its preparation method, and its application in transformer insulating oil synthesis
[0001] This application claims priority to a Chinese patent application filed with the Patent Office of China on April 20, 2023, with application number 202310424569.X and invention name “Application of mesoporous molecular sieve-based solid acid-base catalysts in the synthesis of transformer insulating oil”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The invention belongs to the technical field of insulating oil preparation, and particularly relates to a mesoporous molecular sieve-based solid acid-base catalyst, a preparation method thereof, and application thereof in the synthesis of transformer insulating oil. Background Art
[0003] Insulating oil is typically formulated from a highly refined lubricating base oil with antioxidants. It is widely used in high-voltage power equipment such as transformers, circuit breakers, oil-filled cables, power capacitors, and bushings. Insulating oil impregnates and protects transformers, cables, capacitors, and other components, preventing the ingress of air and moisture and ensuring reliable insulation. Insulating oil also cools transformers and other power equipment. The hot oil is cooled by a radiator and then returned to the transformer, circulating the insulating oil within the box and cooling it, maintaining the transformer's temperature within a certain range. In addition to serving as an insulating medium, insulating oil also acts as an arc extinguishing medium, preventing the spread of arcs and extinguishing them quickly.
[0004] Transformer insulating oil can be mainly divided into several categories, including mineral insulating oil, vegetable insulating oil, silicone oil insulating oil, synthetic ester insulating oil and modified insulating oil. However, mineral insulating oil is prone to leakage pollution and has poor fire resistance. Silicone oil insulating oil, synthetic ester insulating oil and modified insulating oil have high manufacturing costs. Vegetable insulating oil is becoming an increasingly hot research topic in the industry.
[0005] At present, the preparation of vegetable insulating oil mainly uses raw materials such as rapeseed oil and camellia seed oil, while there is little research on using cottonseed oil as raw material. The acid value and other indicators of cottonseed oil are relatively high, and the use of a single alkaline catalyst cannot avoid problems such as active site poisoning in the ester exchange reaction.
[0006] Chinese patent CN 106635432A discloses a method for producing vegetable insulating oil using swill oil. The method uses refined swill oil as a main raw material, ethanol as a reaction raw material, KOH or NaOH as a catalyst, and phosphoric acid as a neutralizing agent. The swill oil is transesterified with ethanol to reduce the viscosity of the swill oil and remove impurities in the swill oil to obtain high-purity fatty acid ethyl ester. Then, using fatty acid ethyl ester as a main raw material, pentaerythritol as a reaction raw material, monobutyltin oxide as a catalyst, diatomaceous earth, white clay, and activated carbon as a filter, and nitrogen as a protective gas, the fatty acid ethyl ester reacts with pentaerythritol to obtain high-quality vegetable insulating oil through a refining process.
[0007] Chinese patent CN 113817525A discloses a method for preparing natural ester insulating oil. The method comprises degumming raw oil, including recycled oil, to remove phospholipids to reduce the effect of phospholipids on the pour point and facilitate the subsequent separation of fatty acids. The oil is then transesterified to obtain mixed fatty acid monoesters after impurities removal. The monoesters are then separated by solvent crystallization to obtain various high-purity single-component fatty acid monoesters. The monoesters are then transesterified with glycerol in the presence of a catalyst to obtain corresponding high-purity single-component triglycerides. The resulting mixtures are then mixed to obtain a natural ester insulating oil having a low pour point, suitable for use in low-temperature areas, low kinematic viscosity, high fluidity, and high heat dissipation capacity.
[0008] The above patents all use a single alkaline catalyst for transesterification, but the single alkaline catalyst is sensitive to the acid value and moisture in the crude oil, resulting in separation difficulties.
[0009] Summary of the Invention
[0010] The purpose of the present invention is to provide a mesoporous molecular sieve-based solid acid-base catalyst, a preparation method thereof, and application in the synthesis of transformer insulating oil. The mesoporous molecular sieve-based solid acid-base catalyst synthesized by the present invention has the advantages of high activity, long performance retention life, and no requirements for the acid value of the raw materials. It can be used for cottonseed oil ester exchange to produce transformer insulating oil.
[0011] In order to achieve the above object, the present invention provides the following technical solutions:
[0012] The present invention provides a method for preparing a mesoporous molecular sieve-based solid acid-base catalyst, comprising the following steps:
[0013] (1) Synthesis of hard template
[0014] A polymer monomer and pure water are prepared into a polymer monomer aqueous solution; under inert gas protection, the polymer monomer aqueous solution, a modified dispersant and an initiator are stirred to react to obtain nanospheres, which are then washed and dried to obtain a nanosphere hard template I;
[0015] (2) Preparation of catalyst skeleton
[0016] The soft template, nitrate, silane derivative, pore-enlarging agent and pure water are stirred to obtain precursor II; the nanosphere hard template I and precursor II are mixed and aged to obtain catalyst skeleton III;
[0017] (3) Preparation of precursor
[0018] The catalyst skeleton III is leached with a solvent to obtain a catalyst precursor IV after removing the hard template I; under inert gas protection, the catalyst precursor IV, an organic solvent and a transition metal alkoxide are stirred and reacted, vacuum filtered to obtain a filter cake and dried, then the filter cake is hydrolyzed, and vacuum filtered and dried again to obtain a powder precursor V;
[0019] (4) Preparation of solid acid-base catalyst
[0020] The powder precursor V is impregnated with an ammonium persulfate solution, vacuum filtered, dried, and calcined to obtain a mesoporous molecular sieve-based solid acid-base catalyst.
[0021] Preferably, the raw materials of the nanosphere hard template I in step (1) further include a modified dispersant.
[0022] Preferably, the raw materials of the precursor II in step (2) further include a pore-enlarging agent.
[0023] Preferably, the polymer monomer in step (1) is one or two of 4-methylstyrene, 1-ethylene-4-(2-methylpropyl)benzene, 4-tert-butylstyrene and vinyl acetate.
[0024] Preferably, the mass ratio of the polymer monomer to pure water in step (1) is 1:5-9.
[0025] Preferably, the modified dispersant in step (1) is 2-acrylamide-2-methylpropanesulfonic acid.
[0026] Preferably, the amount of the modified dispersant in step (1) is 0-1% of the total mass of the polymer monomers.
[0027] Preferably, the initiator in step (1) is a single initiator or a redox composite initiator; the single initiator is H2O2, ammonium persulfate or potassium persulfate; the redox composite initiator is a persulfate-sodium sulfite system composite initiator, a persulfate-sodium bisulfite system composite initiator, a persulfate-sodium dithionite system composite initiator, a persulfate-vitamin C system composite initiator, an H2O2-sodium sulfite system composite initiator, an H2O2-sodium bisulfite system composite initiator, an H2O2-sodium dithionite system composite initiator or an H2O2-vitamin C system composite initiator; the persulfate in the redox composite initiator is ammonium persulfate or potassium persulfate.
[0028] Preferably, the amount of the initiator added in step (1) is 0.5-6% of the total mass of the polymer monomers.
[0029] Preferably, the temperature of the stirring reaction in step (1) is 50-80°C.
[0030] Preferably, the washing times in step (1) are 3-4 times; and the drying temperature is 80-100°C.
[0031] Preferably, the soft template in step (2) is a polyoxyethylene nonionic surfactant; the polyoxyethylene nonionic surfactant is a long-chain alkyl secondary alcohol polyoxyethylene ether series surfactant (C m H 2m+1 O(C2H4O) n H, where m = 11-15, n = 3, 5, 7, 9, 12, 15, 20, 30, 40) and alkyl aryl polyoxyethylene ether series surfactants (C8H 17 -C6H4-O(C2H4O) n H, wherein n=3, 4.5, 7.5, 9.5, 12) or two thereof.
[0032] Preferably, the nitrate in step (2) is one or more of Group II metal nitrates and rare earth metal nitrates, such as Ca(NO3)2·4H2O, Mg(NO3)2·6H2O, La(NO3)3·6H2O, Ce(NO3)3·6H2O, etc.
[0033] Preferably, the silane derivative in step (2) is one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane and tetrabutoxysilane.
[0034] Preferably, the pore-enlarging agent in step (2) is one or two of mesitylene, linear alkane and tert-amyl alcohol; and the molar ratio of the pore-enlarging agent to the soft template is 0-1:1.
[0035] Preferably, the molar ratio of the soft template, nitrate, silane derivative and pure water in step (2) is 1:2-8:14-31:400-500.
[0036] Preferably, the stirring temperature in step (2) is room temperature-55°C, preferably 40-45°C; the stirring speed is 800-1200 rpm, and the stirring time is 15-60 minutes.
[0037] Preferably, the mass ratio of the nanosphere hard template I to the precursor II in step (2) is 2:3-5.
[0038] Preferably, the mixing time in step (2) is 20-30 minutes; and the aging time is 36-96 hours.
[0039] Preferably, the solvent in step (3) is methyl ethyl ketone, ethyl acetate or toluene.
[0040] Preferably, the mass ratio of the catalyst skeleton III to the solvent in step (3) is 1:5-8.
[0041] Preferably, the leaching temperature in step (3) is -3-5°C, and the leaching time is 15-30 seconds.
[0042] Preferably, the organic solvent in step (3) is isooctane, heptane, isobutanol, n-butanol, butyl acetate, toluene, p-xylene, propanol or methyl isobutyl ketone.
[0043] Preferably, the transition metal alkoxy compound in step (3) is a zirconium alkoxy compound, a titanium alkoxy compound or a hafnium alkoxy compound; the alkoxy group in the transition metal alkoxy compound is tetraethoxy, tetrapropoxy, tetraisopropoxy or tetrabutoxy.
[0044] Preferably, in step (3), the mass ratio of the catalyst precursor IV to the organic solvent is 1:14-24; the mass ratio of the transition metal alkoxide to the catalyst precursor IV is 1:1-2.
[0045] Preferably, the stirring reaction temperature in step (3) is 60-80° C., and the stirring reaction time is 24-36 hours.
[0046] Preferably, the concentration of the ammonium persulfate solution in step (4) is 1-2 mol / L.
[0047] Preferably, the immersion time in step (4) is 4-8 hours.
[0048] Preferably, the calcination temperature in step (4) is 400-600° C., and the calcination time is 4-8 hours.
[0049] Preferably, the preparation method of the mesoporous molecular sieve-based solid acid-base catalyst comprises the following specific steps:
[0050] (1) Synthesis of hard template
[0051] The polymer monomers from which the polymerization inhibitor has been removed and pure water are prepared into a polymer monomer aqueous solution; the polymer monomer aqueous solution and a modified dispersant (whether to be added depends on whether a block hard template is to be synthesized) are added into a reaction device equipped with an inert gas protection system and a stirrer, and an initiator is added dropwise at a certain temperature while stirring to polymerize into nanospheres, which are then centrifuged at high speed, washed, and dried to obtain a nanosphere hard template I.
[0052] In the present invention, the stirring rate is preferably 200-800 rpm, the initiator addition time is preferably 30-60 minutes, and the centrifugal speed is preferably 10000-20000 rpm.
[0053] In the present invention, a modified dispersant is added when synthesizing the block hard template, and the molar ratio of the polymer monomer aqueous solution to the modified dispersant is preferably 1:5-5:1.
[0054] (2) Preparation of catalyst skeleton
[0055] A soft template, nitrate, silane derivative, and pore-enlarging agent (their inclusion depends on the desired pore size) are added to pure water in appropriate proportions. The mixture is then placed in a stirring mixer and mixed at a controlled temperature to produce Precursor II. The related groups in the soft template's molecular structure self-assemble into micelles through hydrogen bonding with water molecules and hydrophilic-hydrophobic interactions. The nitrate is encapsulated within the micelles, while the silane derivative, after hydrolysis, forms a three-dimensional MCM-type mesoporous silica network outside the micelles.
[0056] The nanosphere hard template I and the precursor II synthesized in step (1) are stirred in proportion for 20-30 minutes to homogenize, and the hydrolysis small molecule products are removed by rotary evaporation. The catalyst skeleton III is obtained by gelation aging in air at room temperature for 36-96 hours.
[0057] (3) Preparation of precursor
[0058] At a stirring speed of 500-1000 rpm, the catalyst skeleton III is leached with a solvent at a low temperature (-3-5°C) for 15-30 seconds, and a filter cake is obtained by suction filtration. The solvent is washed at a low temperature three times, and the leaching process is repeated 3-4 times to obtain a catalyst precursor IV after the hard template I is removed; the catalyst precursor IV, an organic solvent, and a transition metal alkoxide are added to a device equipped with an inert gas protection system and a stirrer to react, the temperature is controlled at 60-80°C, the reaction is stirred for 24-36 hours, and a filter cake is obtained by vacuum filtration and drying. The filter cake is then hydrolyzed at a stirring speed of 500-1000 rpm for 2-4 hours, and then vacuum filtered and dried for 6 hours to obtain a powder precursor V;
[0059] (4) Preparation of solid acid-base catalyst
[0060] The powder precursor V is impregnated with ammonium persulfate solution at room temperature for 4-8 hours at a stirring speed of 500-1000 rpm, and then vacuum filtered to obtain a filter cake, which is vacuum dried at 90°C for 4 hours and then calcined at 400-600°C for 4-8 hours to burn off the soft template therein to obtain a mesoporous molecular sieve-based solid acid-base catalyst.
[0061] The present invention also provides a mesoporous molecular sieve-based solid acid-base catalyst obtained by the preparation method described in the above scheme. The mesoporous molecular sieve-based solid acid-base catalyst has a topological structure in which macropores and mesopores are interconnected, the macropores are located on the catalyst surface, the mesopores are located inside the catalyst, the acidic sites exist in the macropores, the basic sites exist in the mesopores, and the acidic sites and the basic sites are confined and separated from each other in space.
[0062] The present invention also provides an application of a mesoporous molecular sieve-based solid acid-base catalyst in the synthesis of transformer insulating oil. The mesoporous molecular sieve-based solid acid-base catalyst is used to synthesize transformer insulating oil by cottonseed oil ester exchange; the mesoporous molecular sieve-based solid acid-base catalyst is the mesoporous molecular sieve-based solid acid-base catalyst described in the above scheme.
[0063] The present invention provides a mesoporous molecular sieve-based solid acid-base catalyst. The soft template used in the present invention is a polyoxyethylene nonionic surfactant. The related groups in its molecular structure self-assemble to form micelles through hydrogen bonding with water molecules and hydrophilic-hydrophobic interactions. Nitrates are encapsulated within the micelles, and silane derivatives, after hydrolysis, form a three-dimensional MCM-type mesoporous silica network structure outside the micelles. High-temperature calcination then removes the soft template, and the nitrate decomposes to form metal oxides that adhere to the pores of the MCM-type mesoporous silica. As can be seen in Table 2 and Figure 2, the mesopore diameter of the catalyst of the present invention is approximately 4-5 nm. The wide-angle X-ray diffraction pattern in Figure 1 (b) shows that the metal oxide exists in the mesopores in an amorphous, highly dispersed state.
[0064] On the other hand, when the prepared catalyst skeleton III is solvent-extracted to remove the nanosphere hard template I, a large number of open macroporous structures are formed on the surface of the material. Then, the transition metal alkoxide compound is hydrolyzed and loaded in these macroporous structures, and then immersed in ammonium persulfate solution and calcined to obtain a persulfate-activated macroporous solid acid material.
[0065] The present invention also provides a mesoporous molecular sieve-based solid acid-base catalyst obtained by the preparation method described in the above scheme. The structure of the MCM-type mesoporous molecular sieve-based solid acid-base catalyst prepared by the present invention is a topological structure with interconnected macropores and mesopores. The macropores are located on the catalyst surface, the mesopores are located inside the catalyst, the acidic sites are present in the macropores, and the basic sites are present in the mesopores. The acidic sites and basic sites are confined and separated from each other in space.
[0066] When high-acidity crude oil enters from the macropores on the surface, most of the free oleic acid is esterified at the acidic sites of this structure, and then migrates along the channels between the macropores and mesopores into the MCM mesopores, where the ester exchange reaction occurs. This topological spatial separation of different functional active sites effectively prevents free oleic acid from poisoning the alkaline active sites.
[0067] The present invention also provides the use of the mesoporous molecular sieve-based solid acid-base catalyst described in the above solution in the synthesis of transformer insulating oil. The mesoporous molecular sieve-based solid acid-base catalyst provided by the present invention can be used for the synthesis of transformer insulating oil.
[0068] The topological spatial separation of alkaline and acidic active sites in the mesoporous molecular sieve-based solid acid-base catalyst synthesized by the present invention effectively prevents free fatty acids from poisoning the alkaline active sites, reduces the grade requirements of raw materials, greatly expands the source of raw materials, and reduces the cost of transformer insulating oil synthesis. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0070] FIG1 is an X-ray diffraction pattern of the MCM-type mesoporous molecular sieve-based solid acid-base catalyst prepared in Example 1; wherein a is a small-angle X-ray diffraction pattern, and b is a wide-angle X-ray diffraction pattern;
[0071] FIG2 is a pore size distribution diagram of the MCM-type mesoporous molecular sieve-based solid acid-base catalyst prepared in Example 1;
[0072] FIG3 is a N2 physical adsorption-desorption isotherm diagram of the MCM-type mesoporous molecular sieve-based solid acid-base catalyst prepared in Example 1. DETAILED DESCRIPTION
[0073] In order to further illustrate the present invention, the scheme of the present invention is further described below in conjunction with the drawings and embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0074] The present invention uses cottonseed oil as a raw material and produces a cottonseed oil-derived insulating oil with high flash and ignition points and excellent low-temperature performance through an ester exchange reaction between cottonseed oil and a long-branched alcohol. The long-branched alcohol selected is isotridecanol. Two representative cottonseed oils, designated Cottonseed Oil I (low acid value) and Cottonseed Oil II (high acid value), were selected for use in the examples. Their compositions and parameters are shown in Table 1.
[0075] Table 1 Cottonseed oil composition selected in the embodiment
[0076] Example 1
[0077] A 1-vinyl-4-(2-methylpropyl)benzene aqueous solution (11.1%, w / w) was prepared by removing the inhibitor from the polymer monomer 1-vinyl-4-(2-methylpropyl)benzene and adding pure water. 900 g of this 1-vinyl-4-(2-methylpropyl)benzene aqueous solution (11.1%, w / w) was added to a reaction apparatus equipped with an inert gas system and a stirrer. An initiator (H2O2-vitamin C redox system) was added dropwise at 70°C while stirring at 600 rpm. The amounts of H2O2 and vitamin C added were 2% and 0.5% of the monomer mass, respectively, over a period of 50 minutes. After the initiator addition was complete, the stirring speed was adjusted to 300 rpm. After the polymer nanospheres formed, stirring was continued for 12 hours. The mixture was then centrifuged at 20,000 rpm, washed three times, and dried in vacuo at 100°C to obtain nanosphere hard template I.
[0078] Add 15.2 g of soft template long chain alkyl secondary alcohol polyoxyethylene ether C to 90 g of pure water m H 2m+1 O(C2H4O) n H (wherein m = 12, n = 30), 20.4 g of Mg(NO3)2·6H2O and 45 mL of tetramethoxysilane were placed in a stirring mixer and mixed and stirred at 45°C and 1000 rpm for 60 minutes to obtain precursor II.
[0079] 20 g of nanosphere hard template I and 50 g of precursor II were mixed, stirred for 20 minutes to mix evenly, and the hydrolysis small molecular products were removed by rotary evaporation. The mixture was gelled and aged in air at room temperature for 72 hours to obtain catalyst skeleton III.
[0080] At a stirring speed of 800 rpm, 30 g of catalyst skeleton III was leached with 178 mL of toluene at low temperature (-3°C) for 20 seconds, the filter cake was filtered and washed three times with cold toluene at low temperature. The leaching process was repeated three times to obtain the catalyst precursor IV after removing the hard template I.
[0081] 8 g of catalyst precursor IV, 198 mL of n-butanol and 4 g of tetrabutoxyzirconium were added to a device equipped with an inert gas protection system and a stirrer for reaction. The temperature was controlled at 80°C and stirred for 24 hours. The filter cake was vacuum filtered and dried. The filter cake was then hydrolyzed at a stirring speed of 800 rpm for 4 hours, and then vacuum filtered and dried for 6 hours to obtain a powder precursor V.
[0082] At a stirring speed of 1000 rpm, the powder precursor V was impregnated with 1.5 mol / L ammonium persulfate solution at room temperature for 8 hours, and then vacuum filtered to obtain a filter cake, which was vacuum dried at 90 ° C for 4 hours and then calcined at 400 ° C for 6 hours to burn off the soft template to obtain "mesoporous MgO-macroporous ZrO2 / S2O8 2- "MCM-type mesoporous molecular sieve-based solid acid-base catalyst.
[0083] 30g cottonseed oil I (acid value is 1.0), 250mL isotridecanol and 3.9g "mesoporous MgO--macroporous ZrO2 / S2O8 2- An MCM-type mesoporous molecular sieve-based solid acid-base catalyst was added to a reaction apparatus equipped with an inert gas protection system and a stirrer. The temperature was raised to 80°C while stirring (800-1000 rpm). After reacting for 4 hours, the catalyst was filtered off. The filtrate was allowed to stand and separate into layers. The upper layer mainly contained isotridecanol and isotridecanol, while the lower layer mainly contained glycerol and isotridecanol. The isotridecanol in the upper oil phase was recovered using molecular distillation technology. The isotridecanol was then refined through adsorption decolorization and filtration unit operations to obtain the isotridecanol fatty acid product.
[0084] Example 2
[0085] A 14.3% w / w aqueous solution of 4-tert-butylstyrene (4-tert-butylstyrene) was prepared by adding 798 g (14.3% w / w) of the polymer monomer 4-tert-butylstyrene to pure water. The mixture was then added dropwise to a reactor equipped with an inert gas system and a stirrer. An initiator (potassium persulfate + sodium sulfite redox system) was added dropwise at 50°C while stirring at 800 rpm. The amounts of potassium persulfate and sodium sulfite added were 4% and 1% of the monomer mass, respectively, over a period of 60 minutes. After the initiator addition was complete, the stirring speed was adjusted to 400 rpm. After the polymer nanospheres formed, stirring was continued for 18 hours. The mixture was then centrifuged at 15,000 rpm, washed four times, and dried under vacuum at 80°C to obtain the nanosphere hard template I.
[0086] Add 6.24 g of soft template alkyl aryl polyoxyethylene ether C8H 17 -C6H4-O(C2H4O) 9.5 H, 1.2 g of mesitylene, 9.4 g of Ca(NO3)2·4H2O and 58 mL of tetrapropoxysilane were placed in a stirring mixer and mixed and stirred at 35°C and 800 rpm for 15 minutes to obtain precursor II.
[0087] 20 g of nanosphere hard template I and 30 g of precursor II were mixed, stirred for 30 minutes to mix evenly, and the hydrolysis small molecular products were removed by rotary evaporation. The mixture was gelled and aged in air at room temperature for 36 hours to obtain catalyst skeleton III.
[0088] At a stirring speed of 600 rpm, 30 g of catalyst skeleton III was leached with 225 mL of methyl ethyl ketone at low temperature (0°C) for 30 seconds, the filter cake was filtered out, and washed three times with cold methyl ethyl ketone at low temperature. The leaching process was repeated three times to obtain the catalyst precursor IV after removing the hard template I.
[0089] 8 g of catalyst precursor IV, 130 mL of butyl acetate and 8 g of tetrabutoxytitanium were added to a device equipped with an inert gas protection system and a stirrer for reaction. The temperature was controlled at 60°C and the reaction was stirred for 30 hours. The filter cake was vacuum filtered and dried. The filter cake was then hydrolyzed at a stirring speed of 600 rpm for 2 hours, and then vacuum filtered and dried for 6 hours to obtain a powder precursor V.
[0090] At a stirring speed of 500 rpm, the powder precursor V was impregnated with 1 mol / L ammonium persulfate solution at room temperature for 6 hours, and then vacuum filtered to obtain a filter cake, which was vacuum dried at 90 ° C for 4 hours and then calcined at 600 ° C for 4 hours to burn off the soft template and obtain "mesoporous CaO-macroporous TiO2 / S2O8 2- "MCM-type mesoporous molecular sieve-based solid acid-base catalyst.
[0091] Other steps are the same as in Example 1.
[0092] Example 3
[0093] A polymer monomer aqueous solution was prepared by removing the inhibitor from the polymer monomer 4-methylstyrene (151.2 g), vinyl acetate (19 g), and pure water (1370 g). This aqueous solution and 1.7 g of 2-acrylamido-2-methylpropanesulfonic acid were added to a reaction apparatus equipped with an inert gas protection system and a stirrer. An initiator (H₂O₂ + sodium bisulfite redox system) was added dropwise at 80°C while stirring (400 rpm). The amounts of H₂O₂ and sodium bisulfite were 3% and 0.75% of the polymer monomer mass, respectively, over a period of 30 minutes. After the initiator addition was complete, the stirring speed was adjusted to 200 rpm. After the polymer nanospheres were formed, stirring was continued for 6 hours, followed by high-speed centrifugation at 10,000 rpm, washing four times, and vacuum drying at 90°C to obtain block copolymer nanosphere hard template I.
[0094] Add 4.3 g of soft template long chain alkyl secondary alcohol polyoxyethylene ether C to 90 g of pure water m H 2m+1 O(C2H4O) n H (wherein m = 12, n = 30), 4.43 g of alkyl aryl polyoxyethylene ether C8H 17 -C6H4-O(C2H4O) 9.5 H, 5.12 g of Mg(NO3)2·6H2O and 50 mL of tetrabutoxysilane were placed in a stirring mixer and mixed and stirred at 55°C and 1200 rpm for 30 minutes to obtain precursor II.
[0095] 16 g of nanosphere hard template I and 40 g of precursor II were mixed, stirred for 25 minutes to mix evenly, and the hydrolysis small molecular products were removed by rotary evaporation. The mixture was gelled and aged in air at room temperature for 96 hours to obtain catalyst skeleton III.
[0096] At a stirring speed of 1000 rpm, 30 g of catalyst skeleton III was leached with 235 mL of ethyl acetate at low temperature (5°C) for 15 seconds, the filter cake was filtered and washed three times with cold ethyl acetate at low temperature. The leaching process was repeated three times to obtain the catalyst precursor IV after removing the hard template I.
[0097] 8 g of catalyst precursor IV, 240 mL of methyl isobutyl ketone and 5 g of tetraisopropoxy zirconium were added to a device equipped with an inert gas protection system and a stirrer for reaction. The temperature was controlled at 70°C and stirred for 36 hours. The filter cake was vacuum filtered and dried. The filter cake was then hydrolyzed at a stirring speed of 1000 rpm for 3 hours, and then vacuum filtered and dried for 6 hours to obtain a powder precursor V.
[0098] At a stirring speed of 800 rpm, the powder precursor V was impregnated with 2 mol / L ammonium persulfate solution at room temperature for 4 hours, and then vacuum filtered to obtain a filter cake, which was vacuum dried at 90 ° C for 4 hours and then calcined at 500 ° C for 8 hours to burn off the soft template and obtain "mesoporous MgO-macroporous ZrO2 / S2O8 2- "MCM-type mesoporous molecular sieve-based solid acid-base catalyst.
[0099] Other steps are the same as in Example 1.
[0100] Comparative Example 1
[0101] The polymer monomer 1-vinyl-4-(2-methylpropyl)benzene, from which the polymerization inhibitor had been removed, was mixed with pure water to prepare an aqueous solution of 1-vinyl-4-(2-methylpropyl)benzene (11.1%, w / w). 900 g of the aqueous solution (11.1%, w / w) was added to a reaction apparatus equipped with an inert gas protection system and a stirrer. An initiator (H2O2-vitamin C redox system) was added dropwise at 70°C while stirring (600 rpm). The amounts of H2O2 and vitamin C added were 2% and 0.5% of the mass of the polymer monomer, respectively, over a period of 50 minutes. After the initiator was added, the stirring speed was adjusted to 300 rpm. After the polymer nanospheres were formed, stirring was continued for 12 hours, followed by high-speed centrifugation at 20,000 rpm, washing three times, and vacuum drying at 100°C to obtain nanosphere hard template I. * .
[0102] Add 15.2 g of soft template long chain alkyl secondary alcohol polyoxyethylene ether C to 90 g of pure water m H 2m+1 O(C2H4O) nH (wherein m = 11-15, n = 30), 20.4 g of Mg(NO3)2·6H2O and 45 mL of tetramethoxysilane were placed in a stirring mixer and stirred at 45°C and 1000 rpm for 60 minutes to obtain precursor II * .
[0103] 20 g of nanosphere hard template I * and 50g of precursor II * Mix and stir for 20 minutes to mix thoroughly, remove the hydrolysis small molecular products by rotary evaporation, and gel aging in air at room temperature for 72 hours to obtain catalyst skeleton III * .
[0104] At a stirring speed of 800 rpm, 30 g of catalyst skeleton III was leached with 178 mL of toluene at low temperature (-3 ° C). * 20 seconds, filter to obtain the filter cake, and wash it 3 times with cold toluene at low temperature. Repeat the leaching process 3 times to obtain the hard template I * Catalyst precursor IV * , vacuum dried at 90℃ for 4 hours, and then calcined at 400℃ for 6 hours to burn out the soft template to obtain "mesoporous MgO-macroporous unmodified" MCM type solid base catalyst.
[0105] Other steps are the same as in Example 1.
[0106] Comparative Example 2
[0107] The polymer monomer 1-vinyl-4-(2-methylpropyl)benzene, from which the polymerization inhibitor had been removed, was mixed with pure water to prepare an aqueous solution of 1-vinyl-4-(2-methylpropyl)benzene (11.1%, w / w). 900 g of the aqueous solution (11.1%, w / w) was added to a reaction apparatus equipped with an inert gas protection system and a stirrer. An initiator (H2O2-vitamin C redox system) was added dropwise at 70°C while stirring (600 rpm). The amounts of H2O2 and vitamin C added were 2% and 0.5% of the mass of the polymer monomer, respectively, over a period of 50 minutes. After the initiator was added, the stirring speed was adjusted to 300 rpm. After the polymer nanospheres were formed, stirring was continued for 12 hours, followed by high-speed centrifugation at 20,000 rpm, washing three times, and vacuum drying at 100°C to obtain nanosphere hard template I. # .
[0108] Add 15.2 g of soft template long chain alkyl secondary alcohol polyoxyethylene ether C to 90 g of pure water m H 2m+1 O(C2H4O) nH (wherein m = 11-15, n = 30) and 45 mL of tetramethoxysilane were placed in a stirring mixer and mixed at 45 ° C and 1000 rpm for 60 minutes to obtain precursor II # .
[0109] 20 g of nanosphere hard template I # and 50g of precursor II # Mix and stir for 20 minutes to mix thoroughly, remove the hydrolysis small molecular products by rotary evaporation, and gel aging in air at room temperature for 72 hours to obtain catalyst skeleton III # .
[0110] At a stirring speed of 800 rpm, 30 g of catalyst skeleton III was leached with 178 mL of toluene at low temperature (-3 ° C). # 20 seconds, filter to obtain the filter cake, and wash it 3 times with cold toluene at low temperature. Repeat the leaching process 3 times to obtain the hard template I # Catalyst precursor IV # .
[0111] 8 g of precursor IV # A mixture of 198 mL of n-butanol and 4 g of tetrabutoxyzirconium was added to a device equipped with an inert gas protection system and a stirrer to react, the temperature was controlled at 80°C, the reaction was stirred for 24 hours, vacuum filtered to obtain a filter cake and dried, and then the filter cake was hydrolyzed at a stirring speed of 800 rpm for 4 hours, and then vacuum filtered and dried for 6 hours to obtain a powder precursor V. # .
[0112] At a stirring speed of 1000 rpm, the powder precursor V was impregnated with 1.5 mol / L ammonium persulfate solution at room temperature. # After 8 hours, the filter cake was vacuum filtered and dried at 90℃ for 4 hours, and then calcined at 400℃ for 6 hours to burn out the soft template and obtain "mesoporous unmodified-macroporous ZrO2 / S2O8 2- "MCM type macroporous solid acid catalyst.
[0113] Other steps are the same as in Example 1.
[0114] The specific surface area (BET) and pore structure (mercury intrusion) data of the catalysts prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 are shown in Table 2, Figures 2 and 3; the X-ray diffraction crystal phase information is shown in Figure 1; and the element content analysis and acidic and basic site loading (titration analysis) data are shown in Table 3.
[0115] Table 2 Specific surface area and pore structure parameters of the catalysts of Examples 1-3 and Comparative Examples 1-2
[0116] Table 3 Active element ratio and active site loading of the catalysts of Examples 1-3 and Comparative Examples 1-2
[0117] As can be seen from the data in Table 2, the MCM-type mesoporous molecular sieve-based solid acid-base catalyst synthesized in the present invention has a large number of mesopores and macropores, and has a high specific surface area value, which meets the basic requirements for excellent catalytic performance.
[0118] From the data in Table 3, it can be seen that the catalyst synthesized in Comparative Example 1 only has basic sites that catalyze the transesterification reaction, and the catalyst prepared in Comparative Example 2 only has acidic sites that catalyze the esterification reaction.
[0119] The catalyst synthesized in Example 1 was tested and characterized, and the results are shown in Figures 1, 2 and 3.
[0120] According to Figure 1a, the characteristic peak of the MCM mesoporous material (100) crystal plane appears in the small-angle X-ray diffraction pattern, which is located near the diffraction angle of 1.7°, indicating that the present invention has successfully prepared a catalyst with an MCM mesoporous channel structure.
[0121] As can be seen from Figure 1 b, the wide-angle X-ray diffraction pattern does not show the characteristic peaks of the crystalline phase of magnesium and zirconium compounds, indicating that in the catalyst material synthesized by the present invention, magnesium and zirconium exist in a highly dispersed amorphous state.
[0122] As shown in Figure 2, the mesopore size data on the pore size distribution diagram reflects the typical MCM mesopore characteristics, which is consistent with Table 2.
[0123] The catalyst prepared in Example 1 was subjected to N2 physical adsorption-desorption experiments, and a type IV adsorption-desorption isotherm with an H1-type hysteresis loop was obtained (see Figure 3), which is a typical feature of MCM-type mesoporous materials with a relatively narrow pore size distribution. This once again proves that a mesoporous structure is indeed prepared in the catalyst of the present invention.
[0124] Example 4
[0125] 30 g cottonseed oil II, 250 mL isotridecanol and 3.9 g catalyst ("mesoporous MgO-macroporous ZrO2 / S2O8" prepared in Example 1) were added. 2- An MCM-type mesoporous molecular sieve-based solid acid-base catalyst was added to a pilot reactive distillation apparatus and heated to 105°C while stirring (800-1000 rpm). A certain vacuum was maintained in the apparatus to periodically remove water generated by the esterification reaction. After 4 hours of reaction, the catalyst was filtered out and the filtrate was allowed to stand and separate into layers. The upper layer mainly contained isotridecanol, isotridecanol, and trace amounts of oleic acid, while the lower layer mainly contained glycerol, isotridecanol, and trace amounts of water. The isotridecanol in the upper oil phase was recovered using molecular distillation technology. The product was then refined through alkali refining, water washing, adsorption decolorization, filtration, and water removal.
[0126] Comparative Example 3
[0127] The catalyst is the "mesoporous MgO-macroporous unmodified" MCM type solid base catalyst prepared in Comparative Example 1, and the other steps are the same as those in Example 4.
[0128] Comparative Example 4
[0129] The catalyst is the "mesoporous unmodified-macroporous ZrO2 / S2O8" prepared in Comparative Example 2. 2- MCM macroporous solid acid catalyst, other steps are the same as Example 4.
[0130] Table 4 Comparison of catalytic performance of cottonseed oil transesterification and esterification in Example 1, Example 4 and Comparative Examples 1-4
[0131] From Table 4 we can see that:
[0132] (1) When the raw material is low acid value cottonseed oil I, the cottonseed oil transesterification conversion rates of Comparative Example 1 and Example 1 are equivalent, namely 97.2% and 97.5%, respectively. This shows that the catalytic performance of the solid base catalyst synthesized in Comparative Example 1 for transesterification reaction is comparable to that of the "mesoporous MgO-macroporous ZrO2 / S2O8" synthesized in Example 1. 2- The catalytic performance of the MCM solid acid-base catalysts was comparable, while the cottonseed oil transesterification conversion rate in Comparative Example 2 was only 7.2%, which was very poor. This indicates that the basic sites have excellent catalytic activity for the transesterification reaction.
[0133] (2) When the raw material is high-acid cottonseed oil II, the transesterification conversion rate of Example 4 is 95.8%, which is very close to the 97.5% of Example 1, and the oleic acid esterification conversion rate thereof also reaches 96.0%. The catalytic activities for transesterification and esterification reactions come from the basic and acidic sites in the catalyst, respectively. The presence of free oleic acid in cottonseed oil II does not affect the catalytic activity of the catalyst for transesterification (i.e., the free oleic acid molecules do not cause the deactivation of the basic sites). This is closely related to the topological structure of the prepared MCM-type solid acid-base catalyst. The basic and acidic sites in the catalyst are confined and separated from each other in space, and are respectively located in the mesopores of the MCM and in the macropores on the surface.
[0134] (3) The transesterification conversion rate of cottonseed oil II with high acid value in Comparative Example 3 was only 12.3%, which was much lower than the transesterification conversion rate of cottonseed oil I with low acid value in Comparative Example 1 (97.2%). This was because the macroporous structure on the surface of the solid base catalyst was not acid-treated, i.e., there were no acidic active sites required for the esterification reaction. Free oleic acid could not be esterified. When it diffused into the mesoporous channels of the MCM, it would occupy the active alkaline sites therein, resulting in catalyst poisoning.
[0135] (4) Comparative Example 4 uses a surface macroporous solid acid catalyst, which has a good catalytic effect on the esterification of free oleic acid, with an esterification conversion rate of up to 97.3%. However, due to the lack of alkaline sites in the mesopores, the catalytic conversion rate for the transesterification reaction is only 5.9%.
[0136] The low pour point cottonseed oil separated by freezing was first blended with the refined isotridecyl fatty acid product synthesized in Example 4. 0.3% butylated hydroxytoluene, 0.2% methylbenzotriazole, and 1% polyalphaolefin were then added to prepare cottonseed insulating oil. Table 5 lists the physical, chemical, and electrical performance parameters of the cottonseed insulating oil evaluated according to general standards.
[0137] Table 5 Performance parameters of cottonseed insulating oil
[0138] As shown in Table 5, the cottonseed insulating oil prepared by the present invention has excellent indicators. Among them, the breakdown voltage (70 kV, 2.5 mm), flash point (302° C.), and ignition point (330° C.) are far superior to those of mineral oil, and it is safe to use. In addition, the low-temperature performance is also excellent (pour point -37° C.).
[0139] Catalyst performance decay experiment:
[0140] 1. The catalyst in Example 1 was filtered off and recovered. The recovered catalyst was first vacuum-dried at 100° C. for 4 hours, and then catalytically reacted according to the operating conditions of Example 1. The above steps were repeated 6 times, and the cottonseed oil transesterification conversion rate decreased to 81.5%.
[0141] 2. The catalyst in Example 1 was filtered off and recovered. The recovered catalyst was first washed three times with acetone, then vacuum-dried at 100°C for 4 hours, and then subjected to a catalytic reaction according to the operating conditions of Example 1. The above steps were repeated six times, and the cottonseed oil transesterification conversion rate decreased to 90.6%. The recovered catalyst after repeating the above steps six times was calcined at 400°C for 10 minutes with air, cooled to room temperature, and then subjected to a catalytic reaction according to the operating conditions of Example 1, and the cottonseed oil transesterification conversion rate became 95.4%.
[0142] 3. The catalyst in Example 4 was filtered off and recovered. The recovered catalyst was first vacuum-dried at 100° C. for 4 hours, and then catalytically reacted according to the operating conditions of Example 4. The above steps were repeated 6 times. The cottonseed oil transesterification conversion rate and oleic acid conversion rate decreased to 78.6% and 79.2%, respectively.
[0143] 4. The catalyst in Example 4 was filtered off and recovered. The recovered catalyst was first washed three times with acetone and then vacuum-dried at 100°C for 4 hours. The catalytic reaction was then carried out according to the operating conditions of Example 4. The above steps were repeated six times. The cottonseed oil transesterification conversion rate and oleic acid conversion rate decreased to 89.3% and 90.5%, respectively. The recovered catalyst after repeating the above steps six times was calcined at 400°C for 10 minutes in air, cooled to room temperature, and then catalytically reacted according to the operating conditions of Example 4. The cottonseed oil transesterification conversion rate and oleic acid conversion rate increased to 94.2% and 93.7%, respectively.
[0144] The results of the catalyst performance attenuation experiment of the present invention show that the MCM-type mesoporous molecular sieve-based solid acid-base catalyst synthesized by the present invention can still maintain excellent catalytic performance during repeated use, and the catalytic performance can be better restored by an acetone washing method; supplemented by a short-time air roasting, the catalytic performance is almost equivalent to that of the initial catalyst.
[0145] Although the above embodiment provides a detailed description of the present invention, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a mesoporous molecular sieve-based solid acid-base catalyst, comprising the following steps: (1) Synthesis of hard template The polymer monomer and pure water are prepared into a polymer monomer aqueous solution; under the protection of inert gas, the polymer monomer aqueous solution and the initiator are stirred to react to obtain nanospheres, and the nanosphere hard template I is obtained by washing and drying. (2) Preparation of catalyst skeleton The soft template, nitrate, silane derivative and pure water are stirred to obtain precursor II; the nanosphere hard template I and precursor II are mixed and aged to obtain catalyst skeleton III; (3) Preparation of precursor The catalyst skeleton III is leached with a solvent to obtain a catalyst precursor IV after the hard template I is removed; under the protection of inert gas, the catalyst precursor IV, an organic solvent and a transition metal alkoxide are stirred for reaction, a filter cake is obtained by vacuum filtration and dried, and then the filter cake is hydrolyzed, and then vacuum filtration and drying are performed to obtain a powder precursor V; (4) Preparation of solid acid-base catalyst The powder precursor V is impregnated with an ammonium persulfate solution, vacuum filtered, dried, and calcined to obtain a mesoporous molecular sieve-based solid acid-base catalyst.
2. The preparation method according to claim 1, characterized in that: The raw materials of the nanosphere hard template I in step (1) also include a modified dispersant.
3. The preparation method according to claim 1 or 2, characterized in that: The raw materials of the precursor II in step (2) also include a pore expanding agent.
4. The preparation method according to claim 1, characterized in that: The polymer monomers in step (1) are one or two of 4-methylstyrene, 1-ethylene-4-(2-methylpropyl)benzene, 4-tert-butylstyrene and vinyl acetate.
5. The preparation method according to claim 2, characterized in that: The modified dispersant in step (1) is 2-acrylamide-2-methylpropane sulfonic acid.
6. The preparation method according to claim 1, characterized in that: The initiator in step (1) is a single initiator or a redox composite initiator; the single initiator is H2O2, ammonium persulfate or potassium persulfate; the redox composite initiator is a persulfate-sodium sulfite system composite initiator, a persulfate-sodium bisulfite system composite initiator, a persulfate-sodium dithionite system composite initiator, a persulfate-vitamin C system composite initiator, a H2O2-sodium sulfite system composite initiator, a H2O2-sodium bisulfite system composite initiator, a H2O2-sodium dithionite system composite initiator or a H2O2-vitamin C system composite initiator; the persulfate in the redox composite initiator is ammonium persulfate or potassium persulfate.
7. The preparation method according to claim 1, 4 or 6, characterized in that: The mass ratio of the polymer monomer to pure water in step (1) is 1:5-9; The amount of the initiator added is 0.5-6% of the total mass of the polymer monomers.
8. The preparation method according to claim 2 or 5, characterized in that: The amount of the modified dispersant in step (1) is 0-1% of the total mass of the polymer monomer.
9. The preparation method according to claim 1, characterized in that: The stirring reaction temperature in step (1) is 50-80°C.
10. The preparation method according to claim 1, characterized in that: The soft template in step (2) is a polyoxyethylene nonionic surfactant; the polyoxyethylene nonionic surfactant is one or both of a long-chain alkyl secondary alcohol polyoxyethylene ether series surfactant and an alkyl aryl polyoxyethylene ether series surfactant.
11. The preparation method according to claim 1, characterized in that: The nitrate in step (2) is one or more of Group II metal nitrates and rare earth metal nitrates; the silane derivative is one or more of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane and tetrabutoxysilane.
12. The preparation method according to claim 3, characterized in that: The pore-enlarging agent in step (2) is one or two of mesitylene, straight-chain alkane and tert-amyl alcohol.
13. The preparation method according to claim 3 or 12, characterized in that: The molar ratio of the pore-enlarging agent to the soft template in step (2) is 0-1:
1.
14. The preparation method according to claim 1, characterized in that: The molar ratio of the soft template, nitrate, silane derivative and pure water in step (2) is 1:2-8:14-31:400-500.
15. The preparation method according to claim 1, characterized in that: The stirring temperature in step (2) is room temperature-55°C, the stirring speed is 800-1200rpm, and the stirring time is 15-60 minutes.
16. The preparation method according to claim 1, characterized in that: The mass ratio of the nanosphere hard template I and the precursor II in step (2) is 2:3-5.
17. The preparation method according to claim 1, characterized in that: The mixing time in step (2) is 20-30 minutes; the aging time is 36-96 hours.
18. The preparation method according to claim 1, characterized in that: The solvent in step (3) is methyl ethyl ketone, ethyl acetate or toluene.
19. The preparation method according to claim 1 or 18, characterized in that: The mass ratio of the catalyst skeleton III to the solvent in step (3) is 1:5-8.
20. The preparation method according to claim 1 or 19, characterized in that: The leaching temperature in step (3) is -3-5°C, and the leaching time is 15-30 seconds.
21. The preparation method according to claim 1, characterized in that: The organic solvent in step (3) is isooctane, heptane, isobutanol, n-butanol, butyl acetate, toluene, p-xylene, propanol or methyl isobutyl ketone; the transition metal alkoxy compound is a zirconium alkoxy compound, a titanium alkoxy compound or a hafnium alkoxy compound; the alkoxy group in the transition metal alkoxy compound is tetraethoxy, tetrapropoxy, tetraisopropoxy or tetrabutoxy.
22. The preparation method according to claim 1 or 21, characterized in that: In step (3), the mass ratio of the catalyst precursor IV to the organic solvent is 1:14-24; the mass ratio of the transition metal alkoxide compound to the catalyst precursor IV is 1:1-2.
23. The preparation method according to claim 1 or 22, characterized in that: The stirring reaction temperature in step (3) is 60-80° C., and the stirring reaction time is 24-36 hours.
24. The preparation method according to claim 1, characterized in that: The concentration of the ammonium persulfate solution in step (4) is 1-2 mol / L.
25. The preparation method according to claim 1 or 24, characterized in that: The impregnation time in step (4) is 4-8 hours; the calcination temperature is 400-600° C., and the calcination time is 4-8 hours.
26. The preparation method according to claim 1, characterized in that: The washing times in step (1) are 3-4 times; and the drying temperature is 80-100°C.
27. The mesoporous molecular sieve-based solid acid-base catalyst obtained by the preparation method according to any one of claims 1 to 26, characterized in that: The mesoporous molecular sieve-based solid acid-base catalyst has a topological structure in which macropores and mesopores are interconnected, the macropores are located on the catalyst surface, the mesopores are located inside the catalyst, the acidic sites exist in the macropores, the basic sites exist in the mesopores, and the acidic sites and the basic sites are confined and separated from each other in space.
28. Application of a mesoporous molecular sieve-based solid acid-base catalyst in the synthesis of transformer insulating oil, characterized in that: Mesoporous molecular sieve-based solid acid-base catalysts are used for cottonseed oil transesterification to synthesize transformer insulating oil; The mesoporous molecular sieve-based solid acid-base catalyst is the mesoporous molecular sieve-based solid acid-base catalyst according to claim 27.
29. The use according to claim 28, characterized in that The mesoporous molecular sieve-based solid acid-base catalyst is used for synthesizing transformer insulating oil through ester exchange of cottonseed oil and then the catalyst is recovered; The catalyst recovery method comprises: filtering the cottonseed oil ester exchange synthetic transformer insulating oil to obtain a mesoporous molecular sieve-based solid acid-base catalyst, then washing the mesoporous molecular sieve-based solid acid-base catalyst with acetone, and then vacuum drying, air-blow roasting and cooling in sequence.
Citation Information
Patent Citations
Method for producing biofuel from high-acid-value Comus wilsoniana fruit oil under co-catalysis of solid acid and solid base
CN102250694A
A solid acid catalyst for esterification reaction and its preparation method
CN102259008A
Preparation method of rare-earth modified MCM-48 loaded double-function catalyst
CN103551192A
Modified macroporous / mesoporous molecular sieve catalyst as well as preparation method and application thereof
CN114515596A
Application of mesoporous molecular sieve-based solid acid-base catalyst in synthesis of transformer insulating oil
CN116139911A
Cited By
Preparation method of composite alcohol-base catalyst suitable for transesterification
CN121945027A