Yarn membrane, preparation method therefor and use thereof

By generating a polyamide film on the surface of the yarn and combining the "wicking" and "siphoning" effects, the problems of high cost and low efficiency of filter materials in the existing technology are solved, and a high-efficiency filtration effect without external driving force is achieved, which is suitable for Various application scenarios.

WO2024217090A1PCT designated stage expired Publication Date: 2024-10-24WUYI UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/072321
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-01-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing filter materials are high in cost and have low filtration efficiency. They require external factors such as pressure, gravity or vacuum environment to effectively filter. Most of them can only perform intermittent filtration, which cannot meet the demand for high-efficiency and low-cost filtration.

Method used

Interfacial polymerization technology is used to generate a polyamide film on the surface of the yarn, which is combined with the traditional "wicking" and "siphoning" effects of the roving to form a yarn film that can efficiently intercept salt ions and dyes without the need for external driving force.

Benefits of technology

It achieves high-efficiency filtration without external driving force, improves filtration efficiency and cost-effectiveness, simplifies the preparation process and reduces costs, and is suitable for seawater desalination, dye waste liquid treatment and soil desalination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024072321-FTAPPB-I100001
    Figure PCTCN2024072321-FTAPPB-I100001
  • Figure PCTCN2024072321-FTAPPB-I100002
    Figure PCTCN2024072321-FTAPPB-I100002
  • Figure 00000008_0000
    Figure 00000008_0000
Patent Text Reader

Abstract

A yarn membrane, a preparation method therefor and a use thereof. The preparation method for the yarn membrane comprises the following steps: sequentially immersing yarns into an aqueous solution containing amine monomers and an oil phase solution containing acyl chloride monomers, taking out the yarns, and drying same to obtain the yarn membrane. By using an interfacial polymerization technology, the surface of a roving is coated with a polyamide membrane, and by using the characteristics of the polyamide membrane formed by polymerization of allowing for free penetration of water molecules but retaining salt ions and dye macromolecules, and the advantages of "wicking" and "siphoning" effects of a traditional roving, the prepared yarn membrane can achieve excellent salt ion retention and dye retention functions without additional pressure.
Need to check novelty before this filing date? Find Prior Art

Description

Yarn film and its preparation method and application Technical Field

[0001] The present invention belongs to the field of membrane technology, and in particular relates to a yarn membrane and a preparation method and application thereof. Background Art

[0002] As people's demand for the performance of filter materials continues to increase, the variety of filter materials is increasing, and the research and development of high-performance and high-efficiency filter materials has also received attention, striving to find a high-efficiency, low-cost filtering method.

[0003] Traditional filtration systems utilize high-cost filter materials and exhibit slow filtration performance, leading to the shift from traditional filtration systems to composite filters. Currently, commercially available filtration technologies require external factors to operate (such as pressure, gravity, centrifugal force, and vacuum), resulting in high costs, limited intermittent filtration, and low filtration efficiency. Therefore, the development of a low-cost filter material with minimal application requirements is crucial.

[0004] Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a yarn membrane, a preparation method, and an application thereof. The present invention utilizes interfacial polymerization technology to coat the surface of roving with a polyamide membrane. The polyamide membrane formed by interfacial polymerization is free to pass water molecules but retains salt ions and dye macromolecules. This, combined with the advantages of the "wicking" and "siphoning" effects of traditional roving, enables the resulting yarn membrane to achieve excellent salt ion and dye retention without the need for external driving pressure.

[0006] A first aspect of the present invention provides a method for preparing a yarn film, comprising the following steps:

[0007] The yarn is immersed in an aqueous solution containing an amine monomer and an oil phase solution containing an acyl chloride monomer in sequence, taken out, and dried to obtain the yarn.

[0008] Interfacial polymerization refers to a condensation reaction that occurs at the interface (or on the organic side of the interface) between two immiscible solutions containing two monomers. Prior art methods typically utilize an aqueous solution containing an amine monomer and an oily solution containing an acyl chloride monomer to react at their interface, forming a thin polyamide membrane on a support (typically polysulfone or polyethersulfone). This membrane retains ions and dyes while allowing water molecules to pass through. However, it is a pressure-driven membrane.

[0009] Wicking is the process of spontaneously absorbing liquid into a porous medium through the capillary effect. During the wicking process, the surface tension of the liquid (caused by the cohesive force within the liquid) and the adhesive force between the liquid and the porous medium work together to drive the capillary to draw the liquid into the porous medium. The wicking effect occurs in fabrics or rovings composed of wettable fibers, and the geometry of the pores allows the formation of a curved liquid surface. The arrangement and material of the fibers in the yarn are key factors in determining the wicking properties of the fabric. At the same time, the wicking effect can conduct not only water molecules, but also solute molecules of the solution such as salt ions, dye molecules, etc.

[0010] To enhance the wicking effect of the roving and give it a certain ability to intercept ions or dyes, the present invention uses interfacial polymerization technology to form a complete polyamide membrane on the surface of the roving. On the one hand, the wicking effect of the roving can absorb liquid, and then the polyamide membrane intercepts salt ions and dyes. On the other hand, the formation of the polyamide membrane helps to reduce the pores between the fibers inside the yarn, thereby further enhancing the wicking effect of the roving. The reasons are: (1) After being immersed in the aqueous solution, the roving will shrink after being removed; (2) the generated polyamide membrane will also shrink during the heating process, further promoting the compaction between the fibers.

[0011] According to some embodiments of the present invention, the mass concentration of the aqueous solution containing the amine monomer is 0.5 wt% to 5.0 wt%, preferably 0.5 wt% to 4 wt%, and more preferably 1 wt% to 2 wt%.

[0012] According to some embodiments of the present invention, the amine monomer is an aromatic amine and / or an aliphatic amine; preferably, the aromatic amine is selected from at least one of p-phenylenediamine, m-phenylenediamine and o-phenylenediamine; and the aliphatic amine is selected from at least one of ethylenediamine, propylenediamine, butylenediamine, pentamethylenediamine, N-(2-hydroxyethyl)ethylenediamine, hexamethylenediamine, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine and 4-aminomethylpiperazine.

[0013] According to some embodiments of the present invention, the mass concentration of the oil phase solution containing the acyl chloride monomer is 0.1 wt% to 2 wt%, preferably 0.2 wt% to 1.5 wt%, and more preferably 0.2 wt% to 1.0 wt%.

[0014] According to some embodiments of the present invention, the acyl chloride monomer is an aromatic acyl chloride and / or a fatty acyl chloride; preferably, the aromatic acyl chloride is selected from at least one of phthaloyl chloride, isophthaloyl chloride, biphenyl dichloride, benzene disulfonyl chloride and trimesoyl chloride; the fatty acyl chloride is selected from at least one of succinyl chloride, succinoyl chloride, glutaryl chloride, glutaryl chloride, adipoyl chloride, adipoyl chloride, sebacoyl chloride, sebacoyl chloride, cyclopropanetrichloride, cyclobutanedichloride and cyclopentanedichloride.

[0015] The concentration of amine monomers and acyl chloride monomers has a certain influence on the membrane retention performance. If the concentration is too low, the polyamide membrane will have poor cross-linking, large flux but low desalination rate; if the concentration is too high, the reaction will be too fast and the polyamide membrane will become thicker, which is not conducive to the membrane separation performance.

[0016] The solvent in the oil phase solution can be selected from at least one of n-hexane, cyclohexane and n-heptane.

[0017] According to some embodiments of the present invention, the yarn is selected from at least one of cotton, bamboo fiber, viscose fiber, and polypropylene filament; preferably, the yarn is viscose fiber. Viscose fiber material has good retention ability due to its unique skin-core structure and serrated cross-section.

[0018] According to some embodiments of the present invention, the fineness of the yarn is 500-1000tex.

[0019] According to some embodiments of the present invention, the twist coefficient of the yarn is 4 to 5.4.

[0020] According to some embodiments of the present invention, the yarn is a roving, which is composed of a plurality of fiber lines; further, the fiber lines are arranged approximately in parallel along the axial direction of the roving.

[0021] The yarn used in the present invention has excellent wicking capacity and significantly expands upon absorbing moisture, making it an ideal material for applications. The yarn of the present invention can enhance wicking height and moisture conduction through the siphon effect, achieving the goal of enabling applications without the need for external conditions. The resulting yarn membrane can retain dyes and salt ions in the original solution while transferring purified water to the other end, thereby achieving excellent filtration effects.

[0022] According to some embodiments of the present invention, the yarn is immersed in the aqueous solution for 2 to 20 minutes, preferably 2 to 10 minutes, and more preferably 2 to 5 minutes.

[0023] According to some embodiments of the present invention, the yarn is immersed in the oil phase solution for 2 to 10 minutes, preferably 2 to 8 minutes, and more preferably 2 to 6 minutes.

[0024] As the immersion time in the aqueous solution and the interfacial polymerization time increase, the polyamide membrane continues to improve and the charge density on the membrane increases, thereby improving the membrane's water permeability and ion and dye retention rate. However, excessively long reaction times hinder the further diffusion of monomers from the two phases toward the interface, resulting in less than ideal improvements in the membrane's separation performance.

[0025] According to some embodiments of the present invention, the drying temperature is 50°C to 80°C, preferably 50°C to 70°C, and more preferably 60°C to 65°C.

[0026] According to some embodiments of the present invention, the drying time is 8 to 20 minutes, preferably 8 to 15 minutes, and more preferably 8 to 10 minutes.

[0027] After the oil phase monomer and the water phase monomer are combined to form a film on the yarn surface by soaking, the film is reinforced by drying technology.

[0028] According to some embodiments of the present invention, the yarn is hydro-twisted to reduce its hairiness before dipping.

[0029] The second aspect of the present invention provides a yarn membrane prepared by the above-mentioned preparation method.

[0030] According to some embodiments of the present invention, the pore size of the yarn membrane is 1 to 2 nm, and the thickness is 6 to 8 nm.

[0031] The third aspect of the present invention provides the use of the yarn membrane in seawater desalination, dye waste liquid treatment, and soil desalination.

[0032] The yarn membrane of the present invention can freely pass water molecules and efficiently intercept dyes and salt ions in seawater, dye waste liquid and soil.

[0033] Beneficial effects of the present invention:

[0034] (1) The yarn of the present invention itself has good filtering and wicking effects. When combined with a film prepared by interfacial polymerization, the pore structure is more compact, which can more efficiently filter impurities such as dyes and salt ions and extract pure water;

[0035] (2) The present invention utilizes pressure difference as a driving force to achieve continuous filtration and membrane separation, without the need for external power as a driving force in the prior art;

[0036] (3) The preparation process of the yarn membrane of the present invention is simple, time-saving, easy to control, and low-cost.

[0037] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:

[0039] FIG1 is a morphology diagram of the yarn film prepared in Example 1 of the present invention, wherein FIGa is a morphology diagram of the original roving, and FIGb is a morphology diagram of the roving after being coated with a polyamide film. DETAILED DESCRIPTION

[0040] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0041] The present invention adopts an interfacial polymerization method, in which an oil-phase monomer trimesoyl chloride solution (TMC) reacts with a water-phase monomer piperazine to form a nanofiltration membrane on the surface of the yarn. The membrane prepared by this method is thinner, has a higher degree of cross-linking, and has smaller pores. At the same time, it can enhance the wicking capacity and siphon effect of the yarn, thereby improving the flux and the retention rate of dyes and salts.

[0042] The yarn used in the embodiments of the present invention can be made of cotton, bamboo fiber, viscose fiber or polypropylene filament, etc., wherein the fineness of the yarn used in embodiments 1 to 3 is 500 to 1000 tex.

[0043] Example 1

[0044] The yarn material used in this embodiment is viscose fiber.

[0045] The preparation of the yarn film of this embodiment includes the following steps:

[0046] First, immerse the roving in deionized water and soak it thoroughly. Then, remove it and twist it slightly to squeeze out excess water from the surface of the roving, so that the hairiness on the yarn surface adheres to the yarn surface, and a certain amount of deionized water is retained in the core of the roving (to prevent the subsequent aqueous monomer from penetrating too deeply into the yarn body). Then, immerse the roving in a 1% piperazine aqueous solution for 3 minutes, so that the outside of the yarn is the aqueous monomer solution and the core is deionized water, so as to control the depth of immersion of the aqueous monomer. Then immerse it in a prepared 0.2% benzyl chloride n-hexane solution, and carry out polymerization reaction at the interface for 4 minutes. A nanofiltration membrane with a pore size of 1-2nm and a thickness of 7nm is formed.

[0047] The film was placed in a drying oven for heating and curing for 8 minutes at a temperature of 65° C. to obtain a yarn film.

[0048] The structure of the yarn membrane is shown in Figure 1, where a nanofiltration membrane is generated on the yarn surface.

[0049] Example 2

[0050] The preparation steps of Reference Example 1 are as follows:

[0051] The concentration of the piperazine aqueous solution used in this embodiment is 2%, the concentration of the benzene trimesoyl chloride n-hexane solution is 1%, the heating curing time is 10 minutes, and the temperature is 60°C.

[0052] Example 3

[0053] The preparation steps of Reference Example 1 are as follows:

[0054] The yarn material used in this embodiment is polypropylene filament.

[0055] Example 4

[0056] The preparation steps of Reference Example 1 are as follows:

[0057] The yarn fineness used in this embodiment is 2000-3000 tex.

[0058] Comparative Example 1

[0059] The polysulfone-based membrane was immersed in a 1% piperazine aqueous solution for 2 minutes, and then the liquid on the membrane surface was removed. The membrane was then immersed in a 0.2% benzene trimethylene chloride n-hexane solution for interfacial polymerization. The reaction time was 3 minutes and the reaction temperature was 35°C. The liquid on the membrane surface was removed and the membrane was placed in an 80°C oven for heat treatment for 6 minutes to obtain a polyamide nanofiltration membrane.

[0060] Comparative Example 2

[0061] The polyacrylonitrile-based membrane was immersed in a 1% piperazine aqueous solution for 2 minutes, and then the liquid on the membrane surface was removed. The membrane was then immersed in a 0.2% benzene trimethylene chloride n-hexane solution for interfacial polymerization. The reaction time was 3 minutes and the reaction temperature was 25°C. The liquid on the membrane surface was removed and the membrane was placed in a 75°C oven for heat treatment for 6 minutes to obtain a polyamide nanofiltration membrane.

[0062] Test Case

[0063] The separation performance of the yarn membrane was analyzed by detecting the water flux and the retention rate of salt and dye.

[0064] The test conditions for the salt retention rate are as follows: the feed liquid is 1500 ppm NaCl aqueous solution, 2000 ppm MgCl2 aqueous solution, 1500 ppm KCl aqueous solution, and the feed liquid temperature is 20-25°C.

[0065] The test conditions for dye retention rate are as follows: the feed liquid is 100 mg / L methylene blue, 150 mg / L Congo red, and the feed liquid temperature is 20-25°C.

[0066] The calculation formula of retention rate is: R = (1-C p / C r)×100%, where R represents the retention rate, C p and C r are the concentrations of the permeate and feed liquid, respectively.

[0067] In addition, when performing performance tests on the polyamide nanofiltration membranes of Comparative Examples 1 and 2, an additional pressure of 0.45 MPa was required.

[0068] Table 1 Separation performance of yarn membranes prepared in Examples 1 to 4 and polyamide nanofiltration membranes prepared in Comparative Examples 1 and 2

[0069] The present invention uses interfacial polymerization technology to impart a polyamide layer to the surface of conventional roving yarns, imparting them with not only strong wicking and siphoning effects but also the ability to intercept salt ions and dyes. In Examples 1-4, using specific interfacial polymerization parameters and roving yarns, yarn membranes with salt ion rejection rates of 93.5% to 99.2% and dye rejection rates of 96.1% to 99.4% were prepared. These membranes can be used for seawater desalination, dye wastewater treatment, and soil desalination.

[0070] Comparative Examples 1 and 2 do not use yarn but adopt conventional polysulfone-based membrane and polyacrylonitrile-based membrane respectively, so they do not have "wicking" and "siphon" effects and both require external driving force to perform membrane separation.

[0071] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.

Claims

1. A method for preparing a yarn film, characterized in that: The steps include: The yarn is immersed in an aqueous solution containing an amine monomer and an oil phase solution containing an acyl chloride monomer in turn, taken out, and dried to obtain the yarn.

2. The preparation method according to claim 1, wherein the mass concentration of the aqueous solution containing the amine monomer is 0.5wt% to 5.0wt%.

3. The preparation method according to claim 1, wherein the mass concentration of the oil phase solution containing the acyl chloride monomer is 0.1wt% to 2wt%.

4. The preparation method according to claim 1, characterized in that: The yarn is selected from at least one of cotton, bamboo fiber, viscose fiber and polypropylene filament.

5. The preparation method according to claim 1, characterized in that: The fineness of the yarn is 500-1000tex.

6. The preparation method according to claim 1, characterized in that: The immersion time of the yarn in the aqueous solution is 2 to 20 minutes, and the immersion time of the yarn in the oil phase solution is 2 to 10 minutes.

7. The preparation method according to claim 1, characterized in that: The drying temperature is 50-80° C., and the drying time is 8-20 min.

8. A yarn film, characterized in that: The method is prepared according to any one of claims 1 to 7.

9. The yarn membrane according to claim 8, characterized in that The pore size of the yarn membrane is 1 to 2 nm, and the thickness is 6 to 8 nm.

10. Use of the yarn membrane as claimed in claim 8 or 9 in seawater desalination, dye waste liquid treatment and soil desalination.

Citation Information

Patent Citations

  • Filtration membrane with tubular support

    CN102202772A

  • Three-channel ultra-filtration membrane and endothelial layer high-chlorine-resistant nano-filtration membrane preparation method

    CN107754617A

  • Composite polyamide film with salt concentration responsiveness, preparation method and use of composite polyamide film

    CN110339724A

  • Nanofiltration membrane material with multi-scale surface structure as well as preparation method and application of nanofiltration membrane material

    CN113230902A

  • Special filter cloth for polypropylene fiber monofilament beer

    CN114682004A