Small-particle-diameter embolization microsphere and preparation method therefor
By adding unsaturated bonds and water-soluble molecules with an aldehyde structure to the polyvinyl alcohol aqueous solution for reaction, and through cross-linking and modification treatments, narrow and elastic small-particle polyvinyl alcohol embolization microspheres are prepared, which solves the current problem. There are problems with the large particle size and wide distribution range of microspheres, and efficient drug loading and drug release effects are achieved.
Patent Information
- Application Number
- PCT/CN2024/082078
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-24
AI Technical Summary
Existing drug-loaded embolization microspheres have large particle sizes and wide particle size distribution ranges, resulting in slow drug loading and poor embolization effect. It is difficult to target small blood vessel sites and the prepared microspheres lack elasticity and uniformity.
By adding unsaturated bonds, water-soluble molecules with aldehyde or acetal structures to the polyvinyl alcohol aqueous solution and reacting with the catalyst, after cross-linking and modification treatment, small particle size polyethylene with a particle size of 5-40 microns and a narrow distribution range is prepared. Alcohol embolized microspheres increase hydrophobicity through linear aldehyde modification, reduce the water content of microspheres, and improve particle size uniformity and elasticity.
It has achieved high yield, small particle size microspheres with uniform particle size, fast drug loading speed, slow drug release speed, good elastic properties, and is suitable for fine embolization of capillaries and long-term local chemotherapy.
Smart Images

Figure CN2024082078_24102024_PF_FP_ABST
Abstract
Description
Small-size embolic microspheres and preparation method thereof Technical Field
[0001] The present invention relates to drug-loaded embolic microspheres, in particular to small-diameter embolic microspheres with a narrow particle size distribution range, and belongs to the technical field of medical materials. Background Art
[0002] In recent years, interventional embolization therapy has played an increasingly important role in clinical medicine, especially in the treatment of vascular-rich tumors such as liver cancer, and has been increasingly widely used. It has become the preferred alternative for treating tumors that cannot be surgically removed. Drug-loaded embolic microspheres are one of the most common embolic carriers and have received increasing attention due to their high targeting to specific tissues and organs, good embolic properties, ability to combine with chemotherapy drugs, and ability to release drugs slowly. Currently available microspheres (such as DC Bead, CalliSphere, etc.) have a smooth surface, good elasticity and elasticity, and good hydrophilicity and suspension properties. They are easy to guide with blood flow, can block the entire cross-section of blood vessels, and can slowly release drugs at the lesion site, maintain local effective drug concentrations for a long time, and produce significant cytotoxic effects on tumor cells.
[0003] Recent studies have shown that using embolic microspheres with small particle sizes (5-100 microns, particularly 5-40 microns) can better target capillaries for embolization. This is because the small size of these microspheres allows them to more precisely target the target vessels, which helps improve the accuracy of embolization and thus achieve better therapeutic effects. However, microspheres prepared by existing technologies (such as the commercially available microspheres mentioned above) mostly have a particle size range of 100-1000 microns, with large particle sizes and a wide size distribution. The yield of small-sized microspheres is extremely low. Moreover, due to the wide range and uneven particle size of the microspheres prepared by these methods, the drug loading rate of the microspheres is slow, the embolic effect is poor, and it is difficult to treat some small blood vessels.
[0004] Chinese patent CN114306724B discloses a type of embolic microsphere capable of sustained-release drugs and a method for preparing the same. The microspheres prepared by this method have good elasticity, drug loading capacity, and sustained-release properties, but the microspheres are relatively large in size, which limits their use scenarios.
[0005] Chinese patent CN 106729953 B describes functionalized modified polyvinyl alcohol embolic microspheres and their preparation method. These modified microspheres are capable of elastic deformation and loading with anti-tumor drugs. However, the embolic microspheres prepared by this method have a particle size range of 100-1000 microns, which is too large and has a wide size distribution. Furthermore, the microspheres cannot load the drug quickly enough and release the drug too quickly, making them inconvenient for clinical use and impractical for long-term local chemotherapy in vivo.
[0006] CN 106902716 B introduces a method for preparing small-particle starch microspheres. This method uses a polyvinyl pyrrolidone solution as the continuous phase and a soluble starch solution as the dispersed phase. A high-speed shear emulsifier is used for emulsification to form a two-phase aqueous emulsion. The starch retrogradation properties are then utilized to solidify the starch solution droplets into spheres to prepare small-particle starch microspheres with a median particle size of less than 10 μm. However, when this method is used to prepare starch microspheres, the viscosity of the reactants is low, and the resulting microspheres exhibit significant agglomeration and lack elasticity. The reactants used to prepare polyvinyl alcohol embolic microspheres have high viscosity, and the microspheres must not agglomerate and must possess good elasticity. Therefore, this method cannot be used to prepare embolic microspheres.
[0007] Therefore, there is an urgent need in this field to develop drug-loaded embolic microspheres with small particle size and narrow distribution range.
[0008] Summary of the Invention
[0009] To overcome the limitations of existing drug-loaded embolic microspheres, which have large particle sizes and a wide particle size range, the present invention provides small-particle polyvinyl alcohol embolic microspheres and a method for preparing them. The polyvinyl alcohol embolic microspheres provided by the present invention have a particle size range of 5-40 microns, a small size distribution, and can be used for embolization of finer capillaries. They also exhibit faster drug loading, more sustained drug release, and excellent elasticity, resulting in faster and more efficient use.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] A method for preparing small-size embolic microspheres, characterized by comprising the following steps:
[0012] S1: adding a water-soluble molecule containing an unsaturated bond and an aldehyde or acetal structure and a first catalyst to a polyvinyl alcohol aqueous solution for reaction; after the reaction is completed, adjusting the pH of the reaction system to 7-9, and concentrating the solution to obtain a polyvinyl alcohol embolic microsphere intermediate; the polyvinyl alcohol has a weight average molecular weight of 55,000-70,000 g / mol;
[0013] S2: adding the polyvinyl alcohol embolic microsphere intermediate, crosslinking agent, and initiator prepared in step S1 into water and dissolving them, then adding a solvent and a surfactant, and then stirring / mixing them in an inert gas atmosphere using a homogenizer; after the reaction is completed, washing to obtain polyvinyl alcohol embolic microspheres;
[0014] S3: dissolving the C3-C6 straight-chain aldehyde in a solvent, adding the polyvinyl alcohol embolic microspheres prepared in step S2 and the second catalyst, stirring and reacting, and washing after the reaction to obtain small-size polyvinyl alcohol embolic microspheres.
[0015] Furthermore, the water-soluble molecule containing an unsaturated bond and an aldehyde or acetal structure is N-(2,2-dimethoxyethyl)-2-acrylamide or 4-acrylamidobutyraldehyde dimethyl acetal.
[0016] Furthermore, the first catalyst is an inorganic acid, preferably at least one of concentrated hydrochloric acid, concentrated nitric acid or perchloric acid.
[0017] Furthermore, the cross-linking agent is sodium 2-acrylamide-2-methylpropanesulfonate or potassium 3-sulfopropylacrylate.
[0018] Furthermore, the initiator is at least one of V-50 (azobisisobutylamidine hydrochloride), potassium persulfate, and sodium persulfate.
[0019] Furthermore, the solvent in step S2 is at least one of liquid paraffin, ethyl acetate or butyl acetate; the surfactant is at least one of Tween 80 or cellulose acetate butyrate; and the second catalyst is an organic acid.
[0020] Furthermore, the concentration of the polyvinyl alcohol aqueous solution described in step S1 is 0.15-0.25 g / mL; the concentration of the water-soluble molecules containing unsaturated bonds and aldehyde or acetal structures described in step S1 in the polyvinyl alcohol aqueous solution is 4-6 mg / mL, preferably 5 mg / mL; the concentration of the first catalyst in the polyvinyl alcohol aqueous solution is 52-72 mg / mL, preferably 62 mg / mL; and the concentrated solution is concentrated to a viscosity of 1500 cps.
[0021] Furthermore, the concentration of the polyvinyl alcohol aqueous solution is preferably 0.2 g / mL; and the weight average molecular weight of the polyvinyl alcohol is preferably 65,000 g / mol.
[0022] Furthermore, the concentrations of the polyvinyl alcohol embolic microsphere intermediate, cross-linking agent, initiator, water, and surfactant in the solvent in step S2 are 0.15-0.18 g / mL, 0.03-0.05 g / mL, 0.7-1.75 mg / mL, 0.09-0.17 g / mL, and 0.07-0.09 g / mL, respectively; preferably, they are 0.17 g / mL, 0.04 g / mL, 1.2 mg / mL, 0.12 g / mL, and 0.08 g / mL, respectively.
[0023] Furthermore, the reaction temperature of step S1 is 10-35° C., and the reaction time is 3-8 h; the reaction temperature of step S2 is 40-55° C., and the reaction time is 1-2 h; and the reaction of step S3 is carried out at room temperature.
[0024] Furthermore, the homogenizing apparatus in step S2 is an ultrasonic homogenizer with a power of 1.0 kW and a frequency of 20 kHz.
[0025] Furthermore, in step S3, the concentration of the solution after the linear aldehyde is dissolved in the solvent is 0.05-0.1 g / mL; the solvent is at least one of dimethyl sulfoxide, butyl acetate, ethyl acetate, n-heptane or cyclohexane; the second catalyst is at least one of methanesulfonic acid or trichloroacetic acid, and the concentration is 0.06-0.14 g / mL solvent, preferably 0.10 g / mL, preferably methanesulfonic acid; the linear aldehyde is n-butyraldehyde, propionaldehyde or n-valeraldehyde, preferably n-butyraldehyde.
[0026] Furthermore, in step S3, the mass ratio of the linear aldehyde to the polyvinyl alcohol embolic microspheres is (1-2):1.
[0027] The present invention further protects the small-size polyvinyl alcohol embolic microspheres prepared by the above method, wherein the particle size of the microspheres ranges from 5 to 40 microns.
[0028] The present invention has the following beneficial effects:
[0029] 1. The method of the present invention adds a linear aldehyde to react with the microspheres, whereby the microsphere macromolecules are modified with linear alkanes and hydrophobic molecules are attached to the polyvinyl alcohol skeleton, thereby increasing the hydrophobicity and reducing the water content of the microspheres. This significantly reduces the water content of the microspheres, which already contain a large amount of water, and further reduces the particle size of the microspheres.
[0030] 2. The small-size embolic microspheres prepared by the method of the present invention have a high yield, and more than 90% of the microspheres have a particle size in the range of 5-40 microns. The microspheres have a small particle size, a narrow distribution range, and a relatively uniform particle size.
[0031] 3. The embolic microspheres of the present invention have a faster drug loading speed and a slower release speed; the drug loading rate can reach about 90% in 3 minutes, and the release rate can reach a minimum of 58.5% in 28 days.
[0032] 4. The embolic microspheres of the present invention have good mechanical properties and are elastic; the minimum elastic modulus can reach 2.5 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG1 is a microscope image of the microspheres prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The following embodiments of the present invention are described in further detail with reference to the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0035] Example 1
[0036] S1. 100 g of polyvinyl alcohol (65,000 weight-average molecular weight) was dissolved in 500 mL of purified water at 80°C. 2.5 g of N-(2,2-dimethoxyethyl)-2-acrylamide and 70 mL of 37 wt% concentrated hydrochloric acid (62.16 mg / mL) were added and reacted at 25°C for 4 h. After the reaction, the pH of the system was adjusted to 7.2 with sodium hydroxide solution and the mixture was concentrated to a viscosity of 1500 cps to obtain a polyvinyl alcohol embolic microsphere intermediate.
[0037] S2. Completely dissolve 10.2 g of the microsphere intermediate prepared in step S1, 2.4 g of sodium 2-acrylamido-2-methylpropanesulfonate, and 0.07 g of V-50 initiator in 7.2 mL of deionized water. Add 60 mL of liquid paraffin and 4.8 g of Tween 80. Finally, stir the mixture under a helium atmosphere using an ultrasonic homogenizer (1.0 kW power, 20 kHz frequency) at 47°C for 1.5 h. After completion of the reaction, wash the mixture with ethyl acetate, acetone, and deionized water to obtain polyvinyl alcohol embolic microspheres.
[0038] S3. Add 1 g of microspheres to 20 mL of dimethyl sulfoxide solution containing 1.5 g of n-butyraldehyde, add 1.5 mL of methanesulfonic acid (concentration of 0.10 g / mL), and stir at room temperature for 30 minutes. After the reaction is completed, wash with ethanol and deionized water to obtain small-particle polyvinyl alcohol embolic microspheres.
[0039] A microscope image (40 times magnification) of the drug-loaded embolic microspheres prepared in this example is shown in FIG1 . Most of the microspheres have a particle size range of 5-40 μm, with a small particle size and a narrow particle size distribution.
[0040] Example 2
[0041] S1. 110 g of polyvinyl alcohol (68,000 weight-average molecular weight) was added to 500 mL of purified water and dissolved at 80°C. 2.7 g of N-(2,2-dimethoxyethyl)-2-acrylamide and 74 mL of 37 wt% concentrated hydrochloric acid (65.71 mg / mL) were added and reacted at 25°C for 4 h. After the reaction, the pH of the system was adjusted to 7.4 with sodium hydroxide solution and the mixture was concentrated to a viscosity of 1500 cps to obtain a polyvinyl alcohol embolic microsphere intermediate.
[0042] S2. Completely dissolve 10.5 g of the microsphere intermediate prepared in step S1, 2.8 g of sodium 2-acrylamido-2-methylpropanesulfonate, and 0.08 g of V-50 initiator in 8.5 mL of deionized water. Add 60 mL of liquid paraffin and 5 g of Tween 80. Finally, stir the mixture under a helium atmosphere using an ultrasonic homogenizer (1.0 kW power, 20 kHz frequency) at 50°C for 1.5 h. After completion of the reaction, wash the mixture with ethyl acetate, acetone, and deionized water to obtain polyvinyl alcohol embolic microspheres.
[0043] S3. Add 1 g of microspheres to 20 mL of dimethyl sulfoxide solution containing 1.5 g of n-butyraldehyde, add 1.5 mL of methanesulfonic acid (concentration of 0.10 g / mL), and stir at room temperature for 30 minutes. After the reaction is completed, wash with ethanol and deionized water to obtain small-particle polyvinyl alcohol embolic microspheres.
[0044] Example 3
[0045] S1. 125 g of polyvinyl alcohol (70,000 weight-average molecular weight) was added to 500 mL of purified water and dissolved at 80°C. 3 g of N-(2,2-dimethoxyethyl)-2-acrylamide and 80 mL of 37 wt% concentrated hydrochloric acid (71.04 mg / mL) were added and reacted at 30°C for 3 h. After the reaction, the pH of the system was adjusted to 7.6 with sodium hydroxide solution and the mixture was concentrated to a viscosity of 1500 cps to obtain a polyvinyl alcohol embolic microsphere intermediate.
[0046] S2. Completely dissolve 10.8 g of the microsphere intermediate prepared in step S1, 3 g of sodium 2-acrylamido-2-methylpropanesulfonate, and 0.095 g of V-50 initiator in 10.2 mL of deionized water. Add 60 mL of liquid paraffin and 5.4 g of Tween 80. Finally, stir the mixture under a helium atmosphere using an ultrasonic homogenizer (1.0 kW power, 20 kHz frequency) at 55°C for 1 h. After completion of the reaction, wash the mixture with ethyl acetate, acetone, and deionized water to obtain polyvinyl alcohol embolic microspheres.
[0047] S3. Add 1 g of microspheres to 20 mL of n-heptane solution containing 1 g of propionaldehyde, add 2 mL of methanesulfonic acid (concentration of 0.135 g / mL), and stir at room temperature for 30 minutes. After the reaction is completed, wash with ethanol and deionized water to obtain small-particle polyvinyl alcohol embolic microspheres.
[0048] Example 4
[0049] S1. 75 g of polyvinyl alcohol (60,000 weight-average molecular weight) was added to 500 mL of purified water and dissolved at 80°C. 2 g of N-(2,2-dimethoxyethyl)-2-acrylamide and 60 mL of 37 wt% concentrated hydrochloric acid (53.28 mg / mL) were added and reacted at 15°C for 6 h. After the reaction, the pH of the system was adjusted to 7.5 with sodium hydroxide solution and the mixture was concentrated to a viscosity of 1500 cps to obtain a polyvinyl alcohol embolic microsphere intermediate.
[0050] S2. Completely dissolve 9 g of the microsphere intermediate prepared in step S1, 1.8 g of sodium 2-acrylamido-2-methylpropanesulfonate, and 0.042 g of V-50 initiator in 5.4 mL of deionized water. Add 60 mL of liquid paraffin and 4.2 g of Tween 80. Finally, stir the mixture under a helium atmosphere using an ultrasonic homogenizer (1.0 kW power, 20 kHz frequency) at 40°C for 2 h. After completion of the reaction, wash the mixture with ethyl acetate, acetone, and deionized water to obtain polyvinyl alcohol embolic microspheres.
[0051] S3. Add 1 g of microspheres to 20 mL of cyclohexane solution containing 2 g of n-valeraldehyde, add 1 mL of methanesulfonic acid (concentration of 0.0675 g / mL), and stir at room temperature for 30 minutes. After the reaction is completed, wash with ethanol and deionized water to obtain small-size polyvinyl alcohol embolic microspheres.
[0052] Example 5
[0053] S1. 100 g of polyvinyl alcohol (60,000 weight-average molecular weight) was added to 500 mL of purified water and dissolved at 80°C. 2.5 g of 4-acrylamidobutyraldehyde dimethyl acetal and 31.6 mL of 68 wt% concentrated nitric acid (concentration: 61.12 mg / mL) were added and reacted at 25°C for 4 h. After the reaction, the pH of the system was adjusted to 7.2 with sodium hydroxide solution and the mixture was concentrated to a viscosity of 1500 cps to obtain a polyvinyl alcohol embolic microsphere intermediate.
[0054] S2. Completely dissolve 10.2 g of the microsphere intermediate prepared in step S1, 2.4 g of potassium 3-sulfopropylacrylate, and 0.07 g of potassium persulfate initiator in 7.2 mL of deionized water. Then, add 60 mL of ethyl acetate and 4.8 g of cellulose acetate butyrate (weight-average molecular weight, 65,000 g / mol). Finally, stir the mixture under a helium atmosphere using an ultrasonic homogenizer (1.0 kW power, 20 kHz frequency) at 47°C for 1.5 h. After completion of the reaction, wash with ethyl acetate, acetone, and deionized water to obtain polyvinyl alcohol embolic microspheres.
[0055] S3. Add 1 g of microspheres to 20 mL of cyclohexane solution containing 2 g of n-hexanal, add 1.5 mL of trichloroacetic acid (concentration of 0.10 g / mL), and stir at room temperature for 30 minutes. After the reaction is completed, wash with ethanol and deionized water to obtain small-particle polyvinyl alcohol embolic microspheres.
[0056] Example 6
[0057] S1. 110 g of polyvinyl alcohol (60,000 weight-average molecular weight) was added to 500 mL of purified water and dissolved at 80°C. 2.7 g of 4-acrylamidobutyraldehyde dimethyl acetal and 60 mL of 72 wt% perchloric acid (concentration: 61.12 mg / mL) were added and reacted at 25°C for 4 h. After the reaction, the pH of the system was adjusted to 7.5 with sodium hydroxide solution and the mixture was concentrated to a viscosity of 1500 cps to obtain a polyvinyl alcohol embolic microsphere intermediate.
[0058] S2. Completely dissolve 10.5 g of the microsphere intermediate prepared in step S1, 2.8 g of potassium 3-sulfopropylacrylate, and 0.08 g of sodium persulfate initiator in 8.5 mL of deionized water. Then, add 60 mL of butyl acetate and 5 g of cellulose acetate butyrate (weight-average molecular weight, 65,000 g / mol). Finally, stir the mixture under a helium atmosphere using an ultrasonic homogenizer (1.0 kW power, 20 kHz frequency) at 50°C for 1.5 h. After completion of the reaction, wash the mixture with ethyl acetate, acetone, and deionized water to obtain polyvinyl alcohol embolic microspheres.
[0059] S3. Add 1 g of microspheres to 20 mL of dimethyl sulfoxide solution containing 1 g of n-hexanal, add 1 mL of trichloroacetic acid (concentration of 0.0675 g / mL), and stir at room temperature for 30 minutes. After the reaction is completed, wash with ethanol and deionized water to obtain small-particle polyvinyl alcohol embolic microspheres.
[0060] Comparative Example 1
[0061] Compared with Preparation Example 1, polyvinyl alcohol with a weight average molecular weight of 100,000 g / mol was used, and other conditions remained unchanged.
[0062] Comparative Example 2
[0063] Compared with Preparation Example 1, mechanical stirring was used instead of the ultrasonic homogenizer, and other conditions remained unchanged.
[0064] Comparative Example 3
[0065] Compared with Preparation Example 1, n-octanal was used instead of n-butyraldehyde, and other conditions remained unchanged.
[0066] Comparative Example 4
[0067] Compared with Preparation Example 1, no straight-chain aldehyde was added in Step 3, and other conditions remained unchanged.
[0068] Comparative Example 5
[0069] Compared with Preparation Example 1, isobutyraldehyde was used instead of n-butyraldehyde, and other conditions remained unchanged.
[0070] Test Example 1
[0071] Small-particle microsphere yield test: The microspheres obtained in the experiment were sieved and the weight ratio of microspheres in the 5-40 μm particle size range to the total weight was calculated. The results are shown in Table 1.
[0072] Table 1 Comparison of small-size microsphere yields by different methods
[0073] As shown in Table 1, over 90% of the embolic microspheres prepared in Examples 1-6 had a particle size range of 5-40 μm, and the yield of small-sized microspheres was significantly higher than that of the small-sized microspheres prepared in Comparative Examples 1, 2, 4, and 5. Comparative Example 3, similar to Examples 1-6, also used a linear aldehyde, and achieved a yield of 97% of small-sized microspheres.
[0074] Compared with ultrasonic homogenizers, mechanical stirring provides relatively smaller shear force, resulting in larger particle size of the produced microspheres and a wider particle size distribution, resulting in a low yield of microspheres with the target particle size (5-40 microns).
[0075] Test Example 2
[0076] Elastic modulus test: Polyvinyl alcohol embolic microspheres were placed in a nanoindenter and compressed in compression mode at a rate of 1% strain per second. The elastic modulus of the microspheres was calculated based on the data. This was repeated for five microspheres and the average value was taken. The test results are shown in Table 2.
[0077] Table 2 Comparison of elastic modulus of different methods
[0078] As shown in Table 2, the polyvinyl alcohol embolic microspheres prepared in Examples 1-6 have extremely low elastic moduli and excellent compression deformation properties. In particular, Example 1 exhibits an elastic modulus of only 2.5 MPa, demonstrating excellent compression deformation properties. Comparative Example 1, due to the use of polyvinyl alcohol with an excessively high molecular weight, and Comparative Example 3, due to the use of n-octanal with an excessively long carbon chain, both microspheres have excessively high elastic moduli and poor compression deformation properties.
[0079] The weight-average molecular weight of polyvinyl alcohol affects the cross-linking degree of the microspheres, thereby affecting the particle size and elasticity of the microspheres. The larger the molecular weight of polyvinyl alcohol, the longer the molecular chain, the higher the cross-linking degree of the microspheres, the lower the water content, the smaller the particle size, and the larger the elastic modulus.
[0080] Test Example 3
[0081] Drug Loading Rate Test: Embolic microspheres were collected, and surface moisture was removed. 1 g of microspheres were weighed into a vial. 4 mL of a 20 mg / mL doxorubicin hydrochloride aqueous solution was added. The vial was sealed and placed on a plate shaker at 180 rpm. After 3 minutes, 10 μl of the sample was aspirated and diluted to 2 mL. The concentration of the doxorubicin hydrochloride solution was measured using a UV spectrophotometer at 480 nm. The drug adsorption and loading rate of the embolic microspheres after 3 minutes were calculated. The test results are shown in Table 3.
[0082] Table 3 Comparison of drug loading rates of different microspheres in 3 minutes
[0083] As can be seen from the data in Table 3, the polyvinyl alcohol embolic microspheres prepared in Examples 1-6 can load a very high amount of chemotherapy drugs in the same period of time, providing great convenience in clinical use.
[0084] Test Example 4
[0085] Drug release rate testing: 1 g of doxorubicin-loaded microspheres was added to the dissolution apparatus vessel, 1000 mL of PBS was added, the microspheres were placed in the dissolution apparatus basket, and the basket was mounted on the dissolution rod. The apparatus was set to 100 rpm, the instrument was started, and the timing was commenced. At three designated time points (1 day, 7 days, and 28 days), approximately 2 mL of release medium was pipetted into a clean 10 mL vial. After the test was completed, the volume was returned to the sample vessel. At the time of medium change, the dissolution apparatus was paused, the vessel removed, the old medium in the vessel discarded, the vessel rinsed with purified water, and reinstalled. Subsequently, 1000 mL of PBS was measured using a graduated cylinder and added to the vessel as the new release medium, and the dissolution apparatus was restarted. The doxorubicin concentration in the dissolved samples was measured using a UV spectrophotometer at 480 nm, with the sampling time and results clearly recorded. The test results are shown in Table 4.
[0086] Table 4 Comparison of drug release rates of different microspheres
[0087] It can be seen from the data in Table 4 that the polyvinyl alcohol embolic microspheres prepared in Examples 1-6 release chemotherapy drugs for a longer duration and can achieve a longer-lasting local chemotherapy effect.
Claims
1. A method for preparing small-size embolic microspheres. It is characterized in that The following steps are involved: S1: adding a water-soluble molecule containing an unsaturated bond and an aldehyde or acetal structure and a first catalyst to a polyvinyl alcohol aqueous solution for reaction, and after the reaction is completed, adjusting the pH of the reaction system to 7-9, concentrating the solution, and obtaining a polyvinyl alcohol embolization microsphere intermediate; the weight average molecular weight of the polyvinyl alcohol is 55000-70000 g / mol; S2: adding the polyvinyl alcohol embolic microsphere intermediate, the crosslinking agent, and the initiator obtained in step S1 into water to dissolve, then adding a solvent and a surfactant, and then stirring / mixing the microspheres using a homogenizer under an inert gas atmosphere; after the reaction is completed, washing the microspheres to obtain polyvinyl alcohol embolic microspheres; S3: dissolving C3-C6 straight-chain aldehyde in a solvent, adding the polyvinyl alcohol embolic microspheres prepared in step S2 and a second catalyst, stirring for reaction, and washing after the reaction to obtain small-diameter polyvinyl alcohol embolic microspheres.
2. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The water-soluble molecule containing an unsaturated bond and an aldehyde or acetal structure is N-(2,2-dimethoxyethyl)-2-acrylamide or 4-acrylamidobutyraldehyde dimethyl acetal; the first catalyst is an inorganic acid; the cross-linking agent is sodium 2-acrylamide-2-methylpropane sulfonate or potassium 3-sulfopropyl acrylate; the initiator is at least one of V-50, potassium persulfate, and sodium persulfate; the solvent in step S2 is at least one of liquid paraffin, ethyl acetate, or butyl acetate; the surfactant is at least one of Tween 80 or cellulose acetate butyrate; and the second catalyst is an organic acid.
3. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The concentration of the polyvinyl alcohol aqueous solution described in step S1 is 0.15-0.25 g / mL; the concentration of the water-soluble molecules containing unsaturated bonds and aldehyde or acetal structures in the polyvinyl alcohol aqueous solution is 4-6 mg / mL; the first catalyst is at least one of concentrated hydrochloric acid, concentrated nitric acid or perchloric acid, and the concentration in the polyvinyl alcohol aqueous solution is 52-72 mg / mL.
4. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The concentration of the water-soluble molecules containing unsaturated bonds and aldehyde or acetal structures in the polyvinyl alcohol aqueous solution described in step S1 is 5 mg / mL; the concentration of the first catalyst in the polyvinyl alcohol aqueous solution is 62 mg / mL; the concentration of the polyvinyl alcohol aqueous solution is 0.2 g / mL; the weight average molecular weight of the polyvinyl alcohol is 65000 g / mol; and the concentrated solution is concentrated to a viscosity of 1500 cps.
5. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The concentrations of the polyvinyl alcohol embolic microsphere intermediate, crosslinking agent, initiator, water and surfactant in the solvent in step S2 are 0.15-0.18 g / mL, 0.03-0.05 g / mL, 0.7-1.75 mg / mL, 0.09-0.17 g / mL and 0.07-0.09 g / mL respectively.
6. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The concentrations of the polyvinyl alcohol embolic microsphere intermediate, cross-linking agent, initiator, water and surfactant in the solvent in step S2 are 0.17 g / mL, 0.04 g / mL, 1.2 mg / mL, 0.12 g / mL and 0.08 g / mL respectively.
7. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The reaction temperature of step S1 is 10-35°C, and the reaction time is 3-8h; the reaction temperature of step S2 is 40-55°C, and the reaction time is 1-2h.
8. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The straight-chain aldehyde in step S3 is n-butyraldehyde, propionaldehyde or n-valeraldehyde.
9. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The straight-chain aldehyde in step S3 is n-butyraldehyde.
10. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The concentration of the solution after the straight-chain aldehyde is dissolved in the solvent in step S3 is 0.05-0.1 g / mL.
11. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that The solvent in step S3 is at least one of dimethyl sulfoxide, butyl acetate, ethyl acetate, n-heptane or cyclohexane.
12. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that In step S3, the second catalyst is at least one of methanesulfonic acid or trichloroacetic acid, and the concentration is 0.06-0.14 g / mL solvent.
13. The method for preparing small-size embolic microspheres according to claim 1, It is characterized in that In step S3, the mass ratio of the linear aldehyde to the polyvinyl alcohol embolic microspheres is (1-2):1; and the stirring reaction is carried out at room temperature.
14. Small-diameter polyvinyl alcohol embolic microspheres prepared by the method for preparing small-diameter embolic microspheres according to any one of claims 1 to 13.
Citation Information
Patent Citations
Grain size controllable monodisperse polyvinyl alcohol gel microsphere, preparation method thereof and applied device
CN102895927A
Embolism microsphere having controllable particle size range and preparation method of embolism microsphere
CN109847091A
Photo-initiated cross-linked polyvinyl alcohol drug-loaded embolism microsphere and preparation method thereof
CN114099765A
Embolization microsphere and gradient cross-linking preparation method
CN114478927A
Three polymer microspheres as well as preparation method and application thereof
CN114917399A