Method for obtaining a material based on translucent paper and with barrier properties and material obtained

The method of processing biopolymers using electro-hydrodynamic and aero-hydrodynamic techniques creates a translucent paper with enhanced barrier properties, addressing the limitations of conventional paper packaging by improving biodegradability and recyclability while providing effective liquid, gas, and vapor barriers.

WO2024218419A1PCT designated stage expired Publication Date: 2024-10-24CONSEJO SUPERIOR DE INVESTIGACIONES CIENTIFICAS (CSIC)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/ES2024/070224
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-12
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional paper packaging materials have low barrier properties against liquids, gases, and vapors due to their porous structure, and are opaque, making them unsuitable for sustainable packaging applications, while existing solutions using synthetic polymeric coatings compromise biodegradability and recyclability.

Method used

A method involving electro-hydrodynamic and/or aero-hydrodynamic processing of biopolymers to create a translucent paper coating with enhanced barrier properties, using biodegradable polymers like polyhydroxyalkanoates, which are applied to cellulose-based paper through electrospinning and subsequent calendering or heat treatment to achieve improved optical and barrier properties.

Benefits of technology

The method produces a translucent paper with significantly improved barrier properties against water, oxygen, and grease, while maintaining biodegradability and recyclability, offering a sustainable alternative for packaging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000032
    Figure 000032
  • Figure 000033
    Figure 000033
  • Figure 000034
    Figure 000034
Patent Text Reader

Abstract

The present invention belongs to the area of biodegradable and / or compostable materials with liquid, gas and vapour barrier properties and improved optical properties, for use in the packing industry, among others. In particular, the invention relates to the coating of paper with a biopolymer layer to provide same with barrier properties and improved optical properties. The invention also relates to a method for producing same.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR OBTAINING A MATERIAL BASED ON TRANSLUCENT PAPER AND WITH BARRIER PROPERTIES AND MATERIAL OBTAINED

[0002] DESCRIPTION

[0003] SECTOR AND OBJECT OF THE INVENTION

[0004] The present invention falls within the field of biodegradable and / or compostable materials with barrier properties to liquids, gases, and vapors, and with improved optical properties, applicable in the packaging sector, among others. In particular, the invention relates to the coating of paper with a biopolymer layer to provide it with improved barrier and optical properties, and the method for obtaining it.

[0005] BACKGROUND OF THE INVENTION

[0006] Plastic represents a major environmental problem due to its petroleum-derived origin, its fundamental role in packaging production, and the high percentage of plastic waste it represents. For this reason, sustainable packaging alternatives are being sought, especially in food, medical, and cosmetic applications.

[0007] One of the most promising alternatives for these applications due to its abundant availability, biodegradability, renewability, and recyclability is paper made from cellulose fibers [Shen, Z.; Rajabi-Abhari, A.; Oh, K.; Yang, G.; Youn, H.J.; Lee, H.L. Improving the Barrier Properties of Packaging Paper by Polyvinyl Alcohol Based Polymer Coating — Effect of the Base Paper and Nanoclay. Polymers (Basel) 2021 , 13, 1334. ]. Furthermore, paper packaging is flexible, low-cost, safe, has good printing characteristics, and is easy to functionalize, making it competitive in the packaging sector. However, this material has disadvantages due to: 1) its low barrier properties, attributed to its porous structure, low resistance to water and grease; and 2) its opacity.

[0008] Intense efforts have been made to address some of these issues, such as improving barrier properties and resistance to water and grease through polymeric coatings [Kunam, P.K.; Ramakanth, D.; Akhila, K.; Gaikwad, K.K. Bio-Based Materials for Barrier Coatings on Paper Packaging. Biomass Convers Biorefin 2022, 1-16.], or through lamination with polymeric materials and aluminum, as is the case with Tetra Brik [Jinámar, C. Millions of Tetra-Brik Packages. Industries Alimentaires et Agricoles 1990, 107, 399-401]. As for reducing opacity, to date, translucent paper is obtained by impregnating the paper with mixtures of natural or synthetic resins and mineral oils or drying oils [Fang, Z.; Zhu, H.; Preston, C.; Hu, L. Development, Application and Commercialization of Transparent Paper.Translational Materials Research 2014, 1 , 015004], However, these approaches decrease the biodegradability of paper and make it difficult to recycle.

[0009] Despite improvements in these areas, the production of paper packaging with enhanced characteristics remains a goal. One alternative is to replace synthetic polymer coatings with sustainable and biodegradable biopolymers. However, these biopolymers have a narrower processing window, making them difficult to process using conventional technology. In this regard, techniques such as electrohydrodynamic and / or aerohydrodynamic processing offer advantages because they are processes that occur at room temperature and allow the generation of ultrathin biopolymer coating layers.

[0010] DESCRIPTION OF THE INVENTION

[0011] The present invention proposes a methodology based on electro-hydrodynamic, aero-hydrodynamic or a combination of both processing of biopolymers to generate translucent paper, with barrier properties to liquids, gases and vapors, and with biodegradation and / or compostability properties.

[0012] Method of obtaining the invention

[0013] In a first aspect, the present invention relates to a method for obtaining a translucent paper-based material with barrier properties, comprising the following steps: a) preparing a mixture of polymer in solvent at a concentration of between 0.01 and 99% w / v; b) subjecting the mixture prepared in step a) to an electrohydrodynamic process, aerohydrodynamic process or any combination of both; c) coating a paper with the material resulting from steps a) and b) and subjecting it to a calendering, annealing or heat treatment process with pressure, wherein said process is carried out at a temperature lower than 800 ° C; e C. The term “paper” refers in the present invention to a material consisting of a thin sheet made from cellulose pulp, prepared from a paste of ground vegetable fibers suspended in water, and subsequently dried and hardened.

[0014] The term “translucent” refers in the present invention to a material that allows light to pass through, but does not allow one to see clearly through it.

[0015] The term “enhanced optical properties” refers to a material that allows partial or complete light transmission, with relatively low absorption and reflection, and therefore allows one to see through it.

[0016] The term “barrier properties” refers to the properties of a material that prevent the transmission of liquids, gases, and vapors through it.

[0017] In the present invention, the mixture prepared in step (a) may be a solution, an emulsion, or a suspension. Thus, in a preferred embodiment of the method of preparation of the invention, the mixture prepared in step (a) is a solution, an emulsion, or a suspension.

[0018] The term "solution" can be defined as a homogeneous mixture in which one or more solutes are dissolved in a solvent. As understood by those skilled in the art, homogenization techniques or methods known in the art, such as magnetic stirring or the use of homogenizers, can be used to prepare the solution.

[0019] The term "emulsion," as used here, refers to a dispersion of a liquid (dispersed phase) in the form of small particles within another liquid (continuous phase) with which it is generally immiscible. Emulsions can be direct, inverse, or multiple. Direct emulsions are those in which the dispersed phase is a lipophilic substance and the continuous phase is hydrophilic. These emulsions are usually referred to as L / H or O / W. Inverse emulsions, on the other hand, are those in which the dispersed phase is a hydrophilic substance and the continuous phase is lipophilic. These emulsions are usually abbreviated as H / L or W / O. Multiple emulsions are those in which the dispersed phase contains an inverse emulsion and the continuous phase is an aqueous liquid. These emulsions are known as H / L / H or W / O / W.Pickering-type emulsions can also be formulated, using particles to separate the phases, and using any other type of emulsion technology. The term "suspension," as used here, refers to a heterogeneous mixture formed by small particles of an insoluble solid dispersed in a liquid medium.

[0020] As mentioned, the mixture prepared in step a) comprises polymer, preferably a biodegradable and / or compostable biopolymer and preferably biodegradable in the environment. Examples of biodegradable polymers include, but are not limited to, polyhydroxyalkanoates, such as polyhydroxybutyrate or polyhydroxybutyric acid (PHB), polyhydroxyvalerate (PHV), medium chain length PHA (mcl-PHA), and all possible copolymers thereof such as polyhydroxybutyrate-valerate (PHBV) among others, poly-8-caprolactone (PCL) and all copolymers thereof such as PEG-PCL, and PCLA, polylactic acid (PLA), all copolymers thereof such as poly(lactic-co-glycolic acid) (PLGA), polyphosphazenes, polyorthoesters, polyesters obtained from natural precursors such as polymethylene terephthalate (PTT), polybutylene terephthalate (PBT), polybutylene succinate (PBS),and all possible copolymers thereof such as poly(butylene succinate-co-adipate) (PBSA), poly(butylene adipate-co-terephthalate) (PBAT), polyvinyl alcohols (PVOH) and their copolymers with ethylene (EVOH), polyacrylates (PAC), polyacrylic acid (PAA), water-soluble polyacrylonitriles (PAN), acrylic / methacrylic ester polymers, proteins such as zein, gluten and its derivatives, collagen, gelatin, casein, whey protein, soy proteins and their derivatives, silk fibroin, elastin, among others, polysaccharides such as carrageenans and derivatives, alginates, pullulan, dextran, gum arabic, chitosan and its derivatives, cellulose and its derivatives such as ethylcellulose, hydroxypropylcellulose, methylcellulose, or hydroxypropylmethylcellulose, glycogen, starch, and polymers derived from it such as thermoplastic starch (TPS) and lipids such as waxes, resins, vegetable or mineral oils, acetoglycerides, fatty acids,lignin and derivatives such as sulfonated lignin (SL), among others, and any combination thereof.

[0021] More preferably, the selected biopolymers will be polyhydroxyalkanoates and / or mixtures of different polyhydroxyalkanoates. Even more preferably, copolymers based on polyhydroxybutyrate with contents of comonomers other than hydroxybutyrate greater than 10 mol % will be selected.

[0022] In a preferred embodiment, polymer grades with a mass molecular weight (Mw) of less than 2,000,000 Daltons will be selected. More preferably, grades with a molecular weight below 300,000 Daltons will be selected. The solvents used are selected from water, alcohol (preferably ethanol, isopropanol or butanol) and organic solvents such as, but not limited to, toluene, acetone, ethyl acetate, methylene chloride, chloroform, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), tetrahydrofuran (THF), trifluoroethanol (TFE), deep eutectic solvents (DES), natural deep eutectic solvents (NADES), ionic or inorganic solvents, and any combination of all of the foregoing.

[0023] On the other hand, the mixture prepared in step (a) may comprise other additives, including, but not limited to, plasticizers, surfactants, reinforcements, process additives, antioxidants, colorants and / or nanoreinforcements, among others.

[0024] Examples of plasticizers, which are compounds that increase the “free volume” between polymer chains thereby increasing the flexibility of the material, could include compounds such as acetylated monoglycerides, citrates such as triethyl citrate (TEC), trioctyl citrate (TOC), trihexyl citrate (THC), acetyl tributyl citrate (ATBC), and polyols such as glycerol, deep eutectic point solvents (DES) and natural deep eutectic point solvents (NADES) or combinations thereof.

[0025] Examples of surfactants, amphiphilic compounds used to modify surface tension, might include sorbitan esters and polysorbates (Span Tween, TEGO), poly(vinylpyrrolidone), polyglycerol, polyricinoleate, poly(vinyl alcohol), CTAB (cytyltrimethylammonium bromide), hexadecyltrimethylammonium bromide (HDTMAB), Triton (toctylphenesinpolyethoxyethanol), Lauryl Betaine, Pluronic (polaxomers) and block copolymers.

[0026] Examples of antioxidants include, but are not limited to, p-phenylenediamines, quinolines, phenols, or henna, among others.

[0027] Examples of colorants include, but are not limited to, oxides, sulfides, hydroxides, chromates and other metal-based complexes, such as cadmium, zinc, titanium, lead and molybdenum, phthalocyanine, quinacridones, dioxazines, isoindolines, pealenes, flavanthrones or anthraquinones, among others.

[0028] Examples of reinforcements, but not limited to, are carbon black, titanium dioxide, magnetite, calcium carbonate or silica.

[0029] Examples of nanoreinforcements are carbon nanotubes, graphene, fullerenes, metals, metal oxides, nanosilica, nanoclays, among others, and any combination thereof. In a second stage, step (b) of the method for obtaining the invention, comprises subjecting the mixture prepared in step (a) to an electro-hydrodynamic, aero-hydrodynamic process, or a combination thereof, obtaining a polymeric coating for the paper that provides it with barrier properties and / or improved optical properties.

[0030] Electrohydrodynamic processes are based on the use of electrohydrodynamic techniques, which are based on the formation of micro, submicro or ultrafine polymeric structures, from a polymeric solution to which an electric field is applied.

[0031] Examples of electro-hydrodynamic techniques include, but are not limited to, electrospinning, coaxial electrospinning, electrohydrodynamic jet (E-jet) printing, electrohydrodynamic direct writing, melt electrospinning, electrostatic-solution blow spinning, electrospraying, coaxial electrospraying, electrospraying assisted by pressurized gas.Thus, in a preferred embodiment, alone or in combination with the rest of the preferred embodiments, the electro-hydrodynamic process comprises the use of an electro-hydrodynamic technique selected from the list consisting of electrospinning, coaxial electrospinning, electrohydrodynamic jet (E-jet) printing, electrohydrodynamic direct writing, melt electrospinning, electrostatic-solution blow spinning, electrospraying, coaxial electrospraying, electrospraying assisted by pressurized gas.

[0032] Aero-hydrodynamic processes are based on the use of aero-hydrodynamic techniques, which are based on the formation of micro, sub-micro or ultra-fine polymeric structures, from a polymeric solution to which a pressurized air flow is applied through a jacket concentric to that of the solution.

[0033] Examples of aero-hydrodynamic techniques include, but are not limited to, centrifugal jet spinning, pull spinning, solution blow spinning, blown-centrifugal spinning, and solution blow spraying. Thus, in a preferred embodiment, alone or in combination with the rest of the preferred embodiments, the aero-hydrodynamic process comprises the use of an aero-hydrodynamic technique selected from the list consisting of: centrifugal jet spinning, pull spinning, solution blow spinning, blown-centrifugal spinning, and solution blow spraying, more preferably solution blow spinning.

[0034] In a more preferred embodiment, alone or in combination with the other preferred embodiments, the electrohydrodynamic process is electrospinning. Thus, in this most preferred embodiment of step (b) of the method for obtaining the invention, it comprises subjecting the mixture prepared in step (a) to an electrospinning process.

[0035] The term electrospinning or "electrospinning" can be defined as a type of electrohydrodynamic technique based on the use of electrostatic forces, such as the voltage applied between an emitter and a collector, promoting the formation of microfibers or nanofibers from polymer mixtures or solutions. Different parameters can determine the electrospinning process and its effects, such as the voltage applied between the emitter and the collector, the solution flow rate, the distance between the emitter and the collector, the temperature at which the process is carried out, the relative humidity, as well as other parameters related to the polymer solution such as solids concentration, viscosity of the mixture or solution, surface tension or conductivity.

[0036] In the present invention, the electrospinning process contemplates the use of a single emitter or a multi-emitter or multiple emitter, including but not limited to emitter / s with or without needles (needle-less also called free surface), and also including but not limited to emitter / s of monoaxial or coaxial structure.

[0037] In another preferred embodiment, alone or in combination with the other preferred embodiments, the electrospinning process is carried out using a multi-emitter system, with more than one emission point.

[0038] The present invention also contemplates, but is not limited to, fiber collection in a flat collector, a rotating collector, a disc-shaped collector, a collector ring, a roll-to-roll collector, or codeposition / layer-by-layer deposition. In a more preferred embodiment, the electrospinning process is preferably carried out on an industrial scale with multiple multi-emitters with or without needles, and with a roll-to-roll collection system. This system could optionally be purged with nitrogen or any other inert gas.

[0039] To carry out the electrospinning process, injectors can be used as emitters. The injector can be of different types depending on its configuration. Injector types include, but are not limited to, single, needle, or capillary injectors, coaxial injectors, needleless injectors (needle-less or free surface), multi-needle injectors, or similar injectors, or those made of porous materials. In a preferred embodiment, alone or in combination with the other preferred embodiments, the electrospinning process comprises the use of multi-needle or capillary injectors, or multi-needleless injectors.

[0040] In a preferred embodiment of the method for obtaining the invention, alone or in combination with the other preferred embodiments, the electrospinning process comprises an emitter voltage of between 0.01 kV and 5000 kV (including the extreme values ​​of the range), and a collector voltage of between 0.01 kV and -5000 kV (including the extreme values ​​of the range). More preferably, the electrospinning process comprises an emitter voltage of between 0.1 and 150 kV (including the extreme values ​​of the range) and a collector voltage of between -0.1 and -150 kV (including the extreme values ​​of the range).

[0041] In another preferred embodiment, alone or in combination with the rest of the preferred embodiments, the electrospinning process is carried out at a temperature between 1 e C and 100 e C, preferably at a temperature between 15 e C and 60 e C (including extreme values ​​of the range).

[0042] In another preferred embodiment, alone or in combination with the other preferred embodiments, the electrospinning process is carried out at a relative humidity of between 1 and 99% (including the extreme values ​​of the range), preferably at a relative humidity of between 1 and 60% (including the extreme values ​​of the range).

[0043] In another more preferred embodiment, alone or in combination with the rest of the preferred embodiments, the electrospinning process is carried out at a temperature less than or equal to 60 e C and at a relative humidity of less than or equal to 60%. In another preferred embodiment, alone or in combination with the other preferred embodiments, the electrospinning process is carried out at a flow rate of between 0.001 mL / min and 500 mL / min per emitter, and even more preferably, between 0.01 mL / min and 50 mL / min per emitter.

[0044] In another preferred embodiment, alone or in combination with the other preferred embodiments, when the injector is used in son mode, the electrospinning process is carried out with an injector speed of between 0.01 and 1000 mm / s.

[0045] In another preferred embodiment of the electrospinning process, alone or in combination with the other preferred embodiments, the emitter-collector distance is between 0.1 and 5000 cm (including the extreme values ​​of the range), more preferably, between 1 and 100 cm (including the extreme values ​​of the range).

[0046] In another preferred embodiment of the electrospinning process, alone or in combination with the other preferred embodiments, the electrospinning process is carried out using a roll-to-roll collector for fiber collection. The roll-to-roll speed is preferably between 0.01 m / minute and 10,000 m / minute, and more preferably above 100 m / minute.

[0047] The grammage of the coating applied to the paper obtained in step (b) is between 0.01 and 10,000 g / m 2 and more preferably between 0.2 and 500 g / m 2 .

[0048] In another preferred embodiment, the percentage by mass of coating should preferably be greater than 1%, more preferably greater than 20% and even more preferably greater than 40%.

[0049] In the present invention, the fibers may be, but are not limited to, smooth or pearlescent. These terms refer to different types of morphology found in the generated fibrous structure. Thus, in a preferred embodiment, alone or in combination with the other preferred embodiments, the fibers obtained are smooth fibers. In another preferred embodiment, the fibers are pearlescent fibers.

[0050] The term "smooth fibers" refers to fibers that have a smooth surface with a fairly regular cross-section in diameter. The term "pearled fibers" refers to fibers that have spherical, oblong, or other irregular beads or pearls interspersed throughout the fiber cross-section. Furthermore, the fibers can be arranged in a random or aligned orientation. In random orientation, each fiber has a distinct orientation, while in aligned orientation, all fibers have the same orientation.

[0051] The material obtained in step (b) of the method of obtaining the invention is placed on paper and both materials are subjected to a post-processing step. Therefore, the method of obtaining the invention comprises an additional post-processing step (c), which leads to the coalescence of the fibers obtained in step (b) to reduce their high surface energy, in which process they adhere to the paper substrate and at the same time reduce in a controlled manner and / or completely eliminate the porosity to obtain a continuous coating.

[0052] In a preferred embodiment of step (c) of the method for obtaining the invention, the post-processing step comprises subjecting the paper and the electrospun fiber coating obtained in step (b) to a process of calendering, annealing or heat treatment with pressure, preferably where said process is carried out at a temperature lower than 800 eC, obtaining a homogeneous, pore-free coating. More preferably, the calendering, annealing, or heat treatment process is carried out at a temperature below 300°C. e C, and even more preferably below 200°C. In another preferred embodiment, the calendering, annealing or heat treatment process is carried out at a pressure greater than 0.00001 Pa. In another preferred embodiment, the calendering, annealing or heat treatment process with pressure, is carried out between 0.0001 s and 60 min. In another preferred embodiment, step (c) of the method for obtaining the invention is carried out by means of the calendering process with pressure, at a speed of between 0.001 to 100,000 rpm (including the extreme values ​​of the range).

[0053] The term "calendering" refers to a material preparation process involving the use of two or more rollers, under pressure, with at least one of them at a specific required temperature. This process allows for the closure of pores between fibers, adhesion to the substrate, and filling of the porosity of the paper substrate, generating a continuous material with no or reduced porosity and greatly improved barrier properties.

[0054] Annealing or annealing of a material can be defined as a heat treatment at moderate temperatures under pressure that allows obtaining a material with reduced porosity or continuous with improved physical properties from the fibers. Heat treatment under pressure includes, but is not limited to, continuous and discontinuous processes, such as simultaneous thermal and pressure processes, or thermal and post-pressure processes in two steps. Heat treatment can be performed, but is not limited to, in a temperature chamber, such as an infrared chamber, a resistance chamber, an ultraviolet (UV) radiation chamber, a microwave chamber, a radiofrequency chamber, a convection heating chamber, a conduction heating chamber, an induction heating chamber, continuous dryers on a conveyor belt, vacuum dryers, through direct or indirect steam generators, and any combination thereof.

[0055] Thus, in a preferred embodiment, alone or in combination with the rest of the preferred embodiments, the heat treatment with pressure includes, but is not limited to, continuous and discontinuous processes, such as simultaneous thermal and pressure processes, or thermal and then pressure processes, in two steps. The heat treatment can be carried out, without limitation, in a temperature chamber, such as an infrared chamber, a resistance chamber, an ultraviolet (UV) radiation chamber, a microwave chamber, a radiofrequency chamber, a convection heating chamber, a conduction heating chamber, an induction heating chamber, continuous dryers on a conveyor belt, vacuum dryers, through direct or indirect steam generators, and any combination thereof.

[0056] In an even more preferred embodiment, alone or in combination with the other preferred embodiments, the heat treatment is carried out in a calender at a speed between 0.001 to 100,000 rpm (including the extreme values ​​of the range).

[0057] Translucent paper with barrier properties

[0058] In a second aspect, the invention relates to a paper-based material with barrier and translucent properties, hereinafter “the material of the invention”, comprising paper and a coating with at least one polymer, preferably wherein said polymer is biodegradable and / or compostable.

[0059] The term “paper” has been previously defined and explained in the previous aspect of the invention, and is also applicable to the present aspect of the invention.

[0060] Polymers, both biodegradable and non-biodegradable, may be comprised in the material of the invention. Examples of biodegradable polymers include, but are not limited to, polyhydroxyalkanoates, such as polyhydroxybutyrate or polyhydroxybutyric acid (PHB), polyhydroxyvalerate (PHV), medium chain length PHA (mcl-PHA), and all possible copolymers thereof such as polyhydroxybutyrate-valerate (PHBV) among others, poly-8-caprolactone (PCL) and all possible copolymers thereof such as PEG-PCL and PCLA, polylactic acid (PLA), all copolymers thereof such as poly(lactic-co-glycolic acid) (PLGA), polyphosphazenes, polyorthoesters, polyesters obtained from natural precursors such as polymethylene terephthalate (PTT), polybutylene terephthalate (PBT), polybutylene succinate (PBS), and all possible copolymers thereof such as poly(butylene succinate-co-adipate) (PBSA), poly(butylene adipate-co-terephthalate) (PBAT),polyvinyl alcohols (PVOH) and their copolymers with ethylene (EVOH), polyacrylates (PAC), polyacrylic acid (PAA), water-soluble polyacrylate nitriles (PAN), lignin and derivatives such as sulfonated lignin (SL), acrylic / methacrylic ester polymers, pullulan, zein, celluloses such as ethylcellulose, hydroxypropylcellulose, methylcellulose, or hydroxypropylmethylcellulose, glycogen, starch and polymers derived from this such as thermoplastic starch (TPS) among others.

[0061] In another preferred embodiment of the material of the invention, alone or in combination with the rest of the preferred embodiments, the material of the invention comprises at least one polymer selected from the list consisting of: polyethylene, propylene, poly(ethylene oxide) (PEO), polyethylene-co-vinyl acetate (EVA), polyethylene terephthalate (PET), PHB, PHV, medium chain length PHA (mcl-PHA), PHBV, poly-8-caprolactone (PCL), PEG-PCL, PCLA, PLA, PGLA, polyphosphazenes, polyorthoesters, PTT, PBT, PBS, poly(butylene adipate-co-terephthalate (PBAT), polyvinyl alcohols (PVOH), copolymers of polyvinyl alcohols with ethylene (EVOH), PAC, polyacrylic acid (PAA), water-soluble polyacrylate nitriles (PAN), lignin, sulfonated lignin (LS), acrylic / methacrylic ester polymers, pullulan, zein, ethylcellulose, hydroxypropylcellulose, methylcellulose, or hydroxypropylmethylcellulose, glycogen, starch, thermoplastic starch (TPS), PVP, silicone, PURs, polysulfones, PVDF, PTFE, PVDC, PVC,polycarbonates, acrylonitrile, butadiene, styrene, latex, polyimides, polysulfones, PA6, PA66, PA69, PA1010, thiolated polymers, polyanhydrides, polyethylene glycol PAA copolymers (PAA-co-PEG), and any combination thereof. The material of the invention may comprise at least two, three or more polymers, including any combination thereof.

[0062] On the other hand, the material of the invention may further comprise additives, including, but not limited to, plasticizers, surfactants, reinforcements, process additives, antioxidants, colorants, or nanoreinforcements, among others, as well as any combination thereof. Examples of plasticizers, which are compounds that increase the "free volume" between the polymer chains, thus increasing the flexibility of the material, could include compounds such as acetylated monoglycerides, citrates such as triethylcitrate (TEC), trioctylcitrate (TOC), trihexylcitrate (THC), acetyl tributyl citrate (ATBC), and polyols such as glycerol, deep eutectic point solvents (DES), and natural deep eutectic point solvents (NADES), or combinations thereof.

[0063] Examples of amphiphilic compounds used to modify surface tension might include sorbitan esters and polysorbates (Span Tween, TEGO), poly(vinylpyrrolidone), polyglycerol, polyricinoleate, poly(vinyl alcohol), CTAB (cytyltrimethylammonium bromide), hexadecyltrimethylammonium bromide (HDTMAB), Triton (toctylphenesinpolyethoxyethanol), Lauryl Betaine, Pluronic (polyomers) and block copolymers.

[0064] Examples of antioxidants include, but are not limited to, p-phenylenediamines, quinolines, phenols, or henna, among others.

[0065] Examples of colorants include, but are not limited to, oxides, sulfides, hydroxides, chromates and other metal-based complexes, such as cadmium, zinc, titanium, lead and molybdenum, phthalocyanine, quinacridones, dioxazines, isoindolines, perylenes, flavanthrones or anthraquinones, among others.

[0066] Examples of reinforcements, but not limited to, are carbon black, titanium dioxide, magnetite, calcium carbonate, and silica, among others.

[0067] Examples of nanoreinforcements include carbon nanotubes, graphene, fullerenes, metals, metal oxides, nanosilica, nanoclays, among others, as well as any combination thereof.

[0068] In a preferred embodiment, alone or in combination with the other preferred embodiments, the additives are encapsulated or in coaxial format in the material of the invention.

[0069] The material of the invention can be obtained by electrohydrodynamics, aerohydrodynamics, or any combination of both. Thus, in a preferred embodiment, the material of the invention is obtained by electrohydrodynamics and / or aerohydrodynamics. In another preferred embodiment, alone or in combination with the other preferred embodiments, the material of the invention is obtained by electrohydrodynamics. In a more preferred embodiment, alone or in combination with the other preferred embodiments, the electrohydrodynamic technique is electrospinning.

[0070] The terms “electro-hydrodynamics”, “aero-hydrodynamics” and “electrospinning” have been previously explained in the previous aspect of the invention, and both they and their preferred embodiments are applicable to the present aspect of the invention.

[0071] Furthermore, the material of the invention can be provided in the form of a paper coating, in the form of fibers, particles, or in the form of a film. In a preferred embodiment, alone or in combination with the other preferred embodiments, the coating material is provided in the form of a film.

[0072] As already discussed in the previous aspect of the invention, the fibers may be, but are not limited to, smooth or pearlescent. Thus, in a more preferred embodiment, the fibers are smooth fibers. In another more preferred embodiment, the fibers are pearlescent fibers.

[0073] In an even more preferred embodiment, alone or in combination with the other preferred embodiments, the size of the fibers is between 0.01 to 50 pm (including the extreme values ​​of the range), and more preferably between 0.1 and 10 pm (including the extreme values ​​of the range).

[0074] The grammage of the coating applied to the paper obtained in step (b) is between 0.01 and 10,000 g / m 2 and more preferably between 0.2 and 500 g / m 2 .

[0075] In another preferred embodiment, the percentage by mass of coating should preferably be greater than 1%, more preferably greater than 20% and even more preferably greater than 40%.

[0076] In another preferred embodiment, the material of the invention has water barrier properties of interest, which can be characterized according to the ASTM E96-9 standard method [ASTM-E96 / E96M Standard Test Methods for Water Vapor Transmission of Materials, West Conshohocken. 2016, 14p], or any other, using Payne permeability cups with relative humidity up to 100% (RH) or any other typical equipment that allows measuring water vapor permeability at different temperatures and relative humidities. In another preferred embodiment, the water permeability values ​​at 25°C and 100%RH of the material of the invention are less than 500 g / m 2 d, and more preferably less than 100 g / m 2 d, and even more preferably less than 5 g / m 2 d.

[0077] In another preferred embodiment, the material of the invention has oxygen barrier properties, which can be characterized according to the standard method ASTM D3985-05 using an oxygen permeability analyzer with temperature and humidity control.

[0078] In another preferred embodiment, the oxygen permeability values ​​of the material of the invention are less than 500 cm 3 / m 2 d measured at 23 e C and 50% relative humidity, preferably below 80 cm 3 / m 2 d measured at 23 e C and 50% relative humidity, and even more preferably less than 5 cm 3 / m 2 d measured at 23 e C and 50% relative humidity.

[0079] In another preferred embodiment, alone or in combination with the above preferred embodiments, the material of the invention exhibits water resistance, which can be characterized according to the TAPPI standard method T441 om-13 [Jayaweera, TM; Yu, H.-Z. Water Absorption in Horizontal Corrugated Boards under Water Sprays. Fire Saf J 2006, 41 , 335-342].

[0080] In another preferred embodiment, the water resistance values ​​of the material of the invention are less than 100 g / m 2 , and more preferably less than 5 g / m 2 .

[0081] In another preferred embodiment, alone or in combination with the previous preferred embodiments, the material of the invention has grease resistance, which can be characterized according to the TAPPI standard method T559 cm-12 [Wang, W.; Gu, F.; Deng, Z.; Zhu, Y.; Zhu, J.; Guo, T.; Song, J.; Xiao, H. Multilayer Surface Construction for Enhancing Barrier Properties of Cellulose-Based Packaging. Carbohydr Polym 2021 , 255, 1 17431 ] or similar.

[0082] In another preferred embodiment, the grease resistance values ​​of the material of the invention are higher than a kit 0, more preferably higher than a kit 6, and even more preferably higher than a kit 10. In another preferred embodiment, alone or in combination with the previous preferred embodiments, the material of the invention has improved optical properties, which can be characterized through contact transparency or through transparency calculation. Transparency (T) can be calculated for example using equation (1 ) [Han, JH; Floros, JD Casting Antimicrobial Packaging Films and Measuring Their Physical Properties and Antimicrobial Activity. Journal of Plastic Film & Sheeting 1997, 13, 287-298.].

[0083] T=A6OO / L (1 )

[0084] Where A6oo is the absorbance value at 600 nm and L is the film thickness (mm). According to this equation, the improvement in optical properties of visibility through the film is greater the lower the T value.

[0085] In another preferred embodiment, the transparency values ​​(T) of the material of the invention are lower than those of uncoated paper, more preferably lower than 50 mnr 1 , and even more preferably less than 12 million pesos 1 .

[0086] On the other hand, the material of the invention is preferably a heat-sealable system, resistant to bending, with printing capacity, mechanical resistance and / or flexibility, among others.

[0087] The terms used to define the material of the invention have been previously explained in the previous aspect of the invention, and both they and their preferred embodiments may be applicable to the material of the invention.

[0088] DESCRIPTION OF THE FIGURES

[0089] Figure 1: A) Scanning electron microscopy (SEM) image in front view of the uncoated paper, B) Scanning electron microscopy (SEM) image in front view of the PHBV 35% HV fibers.

[0090] Figure 2: A) Photograph of the uncoated paper, B) Photograph of the paper coated with a layer of PHBV 35%HV of 80 g / m 2 , C) Scanning electron microscopy image of a cross-section of the coated sample.

[0091] Figure 3: A) Photograph of the uncoated paper, B) Photograph of the paper coated with a 130 g / m 35%HV PHBV layer 2 , C) Scanning electron microscopy image of a cross-section of the coated sample. Figure 4: Cobb test values ​​for the paper sample and the coated paper.

[0092] Figure 5: A) Photograph of the uncoated paper, B) Photograph of the paper coated with a 130 g / m 35%HV PHBV layer2 , C) Scanning electron microscopy image of a cross-section of the coated sample.

[0093] Figure 6: A) Scanning electron microscopy (SEM) image in front view of the uncoated paper, B) Scanning electron microscopy (SEM) image in front view of the PHBV 3% HV fibers.

[0094] Figure 7: A) Photograph of the uncoated paper, B) Photograph of the paper coated with a 53 g / m 3%HV PHBV layer 2 , C) Scanning electron microscopy image of a cross-section of the coated sample.

[0095] Figure 8: A) Photograph of the uncoated paper, B) Photograph of the paper coated with a layer of PHBV 3%HV of 80 g / m 2 , C) Scanning electron microscopy image of a cross-section of the coated sample.

[0096] Figure 9: A) Photograph of the uncoated paper, B) Photograph of the paper coated with a 130 g / m 3%HV PHBV layer2 , C) Scanning electron microscopy image of a cross-section of the coated sample.

[0097] Figure 10: Cobb test values ​​for the paper and coated paper samples.

[0098] EXAMPLES

[0099] The invention will now be illustrated by examples provided by the inventors, which demonstrate the effectiveness of the method and product of the invention.

[0100] Example 1

[0101] A solution of PHBV 35% HV (Mw: 205,200 Daltons) with a concentration of 15% by weight in CHCh / BuOH 75:25 vol. / vol was prepared for 24 h at room temperature by magnetic stirring. The electrospinning process was carried out in a high-performance Fluidnatek LE-100 equipment (Bioinicia SL) with environmental conditions control using a multi-injector system, with movement on the X axis and with a rotating collector. The process parameters were: injector voltage 12 kV, collector voltage -6.5 kV, needle-collector distance of 23.5 cm, flow rate of 15 mL / h per needle (5-needle injector), injector speed of 50 mm / s. The process was carried out at a temperature of 20 e C and 30% relative humidity (RH). The deposition time was 1 h 40 min to obtain a coating of 80 g / m 2 .

[0102] The material obtained in the electrospinning process was then deposited on Kraft paper with a weight of 63 g / m2 and heat treated using a Carver Inc. hot plate press (model 4122). The treatment was carried out at 140 e C for 6 s with contact between the plates, but without applying additional pressure above the weight of the upper plate.

[0103] Results

[0104] Figure 1 shows scanning electron microscopy (SEM) images taken with a Hitachi S-4800 microscope of the uncoated paper (A) and the electrospun 35% HV PHBV fibers (B). The PHBV fibers are observed to be nonwoven and have an average fiber size of 2.5 µm.

[0105] Figure 2 shows photographs of uncoated paper (A) and coated paper (B), showing that the coated sample exhibits greater transparency. The improved optical properties are explained by the diffusion of the coating biopolymer, which partially fills the paper pores and reduces light scattering. Figure 2C shows a scanning electron microscopy image of a cross-section of the coated sample. It can be observed that the heat treatment allows the polymer to penetrate the paper pores, generating transparency.

[0106] To quantify the degree of transparency, light absorption at 600 nm was measured on a Dinko Instruments VIS3000 UV-VIS spectrophotometer. Transparency (T) was calculated by dividing the absorbance value at 600 nm by the sample thickness, expressed in millimeters. Table 1 shows the transparency (T) values ​​for both samples. Table 1. Transparency (T) values ​​of uncoated paper samples and paper coated with a 80 g / m 35%HV PHBV layer. 2 .

[0107] Sample T (mm')

[0108] Kraft paper 63 g / m 2 17

[0109] Coated paper 10

[0110] Example 2

[0111] A solution of PHBV 35% HV (Mw: 205,200 Dalton) with a concentration of 15% by weight in CHCl3 / BuOH 75:25 vol / vol was prepared for 24 h at room temperature by magnetic stirring.

[0112] The electrospinning process was carried out in a high-performance Fluidnatek LE-100 (Bioinicia SL) equipment with controlled environmental conditions using a multi-injector system, with movement on the X axis and with a rotating collector. The process parameters were: injector voltage 12 kV, collector voltage -6.5 kV, needle-collector distance of 23.5 cm, flow rate of 15 mL / h per needle (5-needle injector), injector speed of 50 mm / s. The process was carried out at a temperature of 20 e C and 30% relative humidity (RH). The deposition time was 2 h and 40 min to obtain a coating of 130 g / m 2 .

[0113] The material obtained in the electrospinning process was then deposited on Kraft paper with a weight of 63 g / m 2 and heat treated using a Carver Inc. hot plate press (model 4122). The treatment was carried out at 140 eC for 10 s with contact between the plates but without applying additional pressure above the weight of the upper plate.

[0114] Results

[0115] Figure 3 shows photographs of uncoated paper (A) and coated paper (B), showing that the coated sample exhibits better optical light transmission properties. Figure 3C shows a scanning electron microscopy image of a cross-section of the coated sample. It can be seen that the heat treatment allows the polymer to penetrate the paper pores, generating transparency.

[0116] To quantify the degree of transparency, light absorption at 600 nm was measured using a Dinko Instruments VIS3000 UV-VIS spectrophotometer. Transparency (T) was calculated by dividing the absorbance at 600 nm by the sample thickness, expressed in millimeters. Table 2 shows the transparency values ​​for both samples, with the coated paper showing approximately twice the light transmission.

[0117] Table 2. Transparency values ​​(T) of uncoated paper samples and paper coated with a 130 g / m3 PHBV 35%HV layer 2 .

[0118] Sample f (mnr 1 )

[0119] Kraft paper 63 g / m 2 i 7

[0120] Coated paper 9

[0121] The water vapor transmission rate (WVTR) and oxygen transmission rate (OTR) values ​​were determined. The water vapor transmission rate (WVTR) was determined by an ASTM E96-9 test using Payne permeation cups with 100% relative humidity (RH) on one side of the material and 0% RH on the other. The Payne cups were stored at 25 °C and their weight was measured periodically until a constant weight was reached. Aluminum foils were used as controls to estimate water vapor loss through the seal. Oxygen barrier properties were characterized according to the ASTM D3985-05 standard method using an Oxygen Permeation Analyzer M8001 from Systech Illinois (Thame, UK) at 53% RH and 25 q C. Table 3 shows the results obtained. The coated paper sample showed a very good barrier to water vapor and oxygen compared to paper.

[0122] Table 3. Water vapor transmission rate (WVTR) and oxygen transmission rate (OTR) values ​​of coated paper

[0123] WVTR sample (g / m 2 d) OTR (cm 3 / m 2 d)

[0124] Kraft paper 63 g / m 2 >800 Out of range

[0125] Coated paper 9.25 ± 1 .41 10.5 ± 0.3

[0126] The water absorption of both the paper sample and the coated paper was determined using the TAPPI method T441 cm-13. The water absorption value, indicated by the Cobb index, was calculated by measuring the amount of water absorbed by the paper for 60 s. The Cobb value or water absorption value is represented by the amount of water absorbed by the paper per unit area (g / m 2 ). The results are shown in Figure 4. While the paper showed a water absorption of more than 40 g / m 2 , the coated paper showed a value of less than 5 g / m 2. Grease resistance was evaluated for both the paper and coated paper samples using TAPPI method T559 cm-12. The test involves depositing a series of numbered solutions, which exhibit different surface tensions and viscosities, onto the sample surface. The solutions are numbered from 1 (least aggressive) to 12 (most aggressive). The highest-numbered solution that leaves no mark on the sample surface corresponds to its rating according to this Kit. The results are shown in Table 4. While the uncoated paper had no resistance, the coated sample showed the highest resistance.

[0127] Table 4. KIT values ​​of the grease resistance test for paper and coated paper Sample KIT VALUE

[0128] Kraft paper 63 g / m 2 EITHER

[0129] Coated paper 12

[0130] Example 3

[0131] A solution of PHBV 35% HV (Mw: 205,200 Dalton) with a concentration of 15% by weight in CHCh / BuCH 75:25 vol / vol was prepared for 24 h at room temperature by magnetic stirring.

[0132] The electrospinning process was carried out in a high-performance Fluidnatek LE-100 (Bioinicia SL) equipment with controlled environmental conditions using a multi-injector system, with movement on the X axis and with a rotating collector. The process parameters were: injector voltage 12 kV, collector voltage -6.5 kV, needle-collector distance of 23.5 cm, flow rate of 15 mL / h per needle (5-needle injector), injector speed of 50 mm / s. The process was carried out at a temperature of 20 e C and 30% relative humidity (RH). The deposition time was 2 h and 40 min to obtain a coating of 130 g / m 2 .

[0133] The material obtained in the electrospinning process was then deposited on Kraft paper with a weight of 74 g / m 2 and heat treated using a Carver Inc. hot plate press (model 4122). The treatment was carried out at 140 e C for 10 s with contact between the plates but without applying additional pressure above the weight of the upper plate.

[0134] Results

[0135] Figure 5 shows images of uncoated paper (A) and coated paper (B), with the coated sample showing greater transparency. Figure 5C shows a scanning electron microscopy image of a cross-section of the coated sample. It can be seen that the heat treatment allows the polymer to penetrate the pores of the paper, generating transparency.

[0136] To quantify the degree of transparency, light absorption at 600 nm was measured using a Dinko Instruments VIS3000 UV-VIS spectrophotometer. Transparency (T) was calculated by dividing the absorbance at 600 nm by the sample thickness, expressed in millimeters. Table 5 shows the transparency values ​​for both samples, with twice the light transmission observed compared to the coated paper.

[0137] Table 5. Transparency values ​​(T) of uncoated paper samples and paper coated with a 130 g / m3 PHBV 35%HV layer 2 .

[0138] Sample T (mnv 1 )

[0139] Kraft paper 74 g / m 2 15

[0140] Coated paper 8

[0141] Eiemolo 4

[0142] A solution of PHBV 2% HV (M w : 280,000 Dalton) with a concentration of 10% by weight in TFE for 24 h at room temperature by magnetic stirring.

[0143] The electrospinning process was carried out in a high-performance Fluidnatek LE-100 (Bioinicia SL) equipment with controlled environmental conditions using a multi-injector system, with movement on the X axis and with a rotating collector. The process parameters were: injector voltage 23 kV, collector voltage -15 kV, needle-collector distance of 24.5 cm, flow rate of 20 mL / h per needle (5-needle injector), injector speed of 50 mm / s. The process was carried out at a temperature of 30 e C and 30% relative humidity (RH). The deposition time was 1 h 30 min to obtain a coating of 53 g / m 2 .

[0144] The material obtained in the electrospinning process was then deposited on Kraft paper with a weight of 63 g / m 2 and heat treated using a Carver Inc. hot plate press (model 4122). The treatment was carried out at 170 eC for 8 s and 5.86 MPa of additional pressure to the weight of the upper plate.

[0145] Results

[0146] Figure 6 shows scanning electron microscopy (SEM) images taken with a Hitachi S-4800 microscope of the uncoated paper (A) and the electrospun 3% HV PHBV fibers (B). The PHBV fibers are observed to be nonwoven, with an average fiber size of 1.8 pm.

[0147] Figure 7 shows photographs of uncoated paper (A) and coated paper (B), observing that the coated sample has greater transparency. Figure 6C shows a scanning electron microscopy image of a cross-section of the coated sample. It is observed that the heat treatment allows the polymer to penetrate the pores of the paper, generating greater light transmission. Since the polymer has a higher molecular weight and a lower HV content (2% HV) compared to the polymer in the previous examples, it diffuses less well and therefore requires higher pressure to produce an improvement in optical properties.

[0148] To quantify the degree of transparency, light absorption at 600 nm was measured using a Dinko Instruments VIS3000 UV-VIS spectrophotometer. Transparency (T) was calculated by dividing the absorbance at 600 nm by the sample thickness, expressed in millimeters. Table 6 shows the transparency values ​​for both samples, with greater light transmission observed for the coated paper.

[0149] Table 6. Transparency values ​​(T) of uncoated paper samples and paper coated with a 53 g / m 3%HV PHBV layer 2 .

[0150] Sample T (mnr 1 )

[0151] Kraft paper 63 g / m 2 17

[0152] Coated paper 16

[0153] Example 5

[0154] A solution of PHBV 2% HV (M w : 280,000 Dalton) with a concentration of 10% by weight in TFE for 24 h at room temperature by magnetic stirring.

[0155] The electrospinning process was carried out in a high-performance Fluidnatek LE-100 (Bioinicia SL) equipment with controlled environmental conditions using a multi-injector system, with movement on the X axis and with a rotating collector. The process parameters were: injector voltage 23 kV, collector voltage -15 kV, needle-collector distance of 24.5 cm, flow rate of 20 mL / h per needle (5-needle injector), injector speed of 50 mm / s. The process was carried out at a temperature of 30 e C and 30% relative humidity (RH). The deposition time was 3 h to obtain a coating of 80 g / m 2 The material obtained from the electrospinning process was then deposited on Kraft paper with a weight of 63 g / m 2 and heat treated using a Carver Inc. hot plate press (model 4122). The treatment was carried out at 170 eC for 10 s and 5.86 MPa of additional pressure to the weight of the upper plate.

[0156] Results

[0157] Figure 8 shows photographs of the uncoated paper (A) and the coated paper (B), showing that the coated sample exhibits greater transparency. Figure 8C shows a scanning electron microscopy image of a cross-section of the coated sample. It can be seen that the heat treatment allows the polymer to penetrate the pores of the paper, generating transparency.

[0158] To quantify the degree of transparency, light absorption at 600 nm was measured using a Dinko Instruments VIS3000 UV-VIS spectrophotometer. Transparency (T) was calculated by dividing the absorbance at 600 nm by the sample thickness, expressed in millimeters. Table 7 shows the transparency values ​​for both samples, with greater light transmission observed for the coated paper.

[0159] Table 7. Transparency values ​​(T) of uncoated paper samples and paper coated with a 80 g / m 3%HV PHBV layer 2 .

[0160] Sample T (mnr 1 )

[0161] Kraft paper 63 g / m 2 17

[0162] Coated paper 1 1

[0163] Example 6

[0164] A solution of PHBV 2% HV (M w : 280,000 Dalton) with a concentration of 10% by weight in TFE for 24 h at room temperature by magnetic stirring.

[0165] The electrospinning process was carried out on a high-performance Fluidnatek LE-100 (Bioinicia SL) equipment with controlled environmental conditions using a multi-injector system, with movement on the X axis and with a rotating collector. The process parameters were: injector voltage 23 kV, collector voltage -15 kV, needle-collector distance 24.5 cm, flow rate of 20 mL / h per needle (5-needle injector), injector speed of 50 mm / s. The process was carried out at a temperature of 30 e C and 30% relative humidity (RH). The deposition time was 4 h 20 min to obtain a coating of 130 g / m 2 The material obtained from the electrospinning process was then deposited on Kraft paper with a weight of 63 g / m 2 and heat treated using a Carver Inc. hot plate press (model 4122). The treatment was carried out at 170 eC for 15 s and 5.86 MPa of additional pressure to the weight of the upper plate.

[0166] Results

[0167] Figure 9 shows photographs of uncoated paper (A) and coated paper (B), showing that the coated sample has greater transparency. Figure 9C shows a scanning electron microscopy image of a cross-section of the coated sample. It is observed that the heat treatment allows the polymer to diffuse into the pores of the paper, generating greater light transmission for the coated paper.

[0168] To quantify the degree of transparency, light absorption at 600 nm was measured using a Dinko Instruments VIS3000 UV-VIS spectrophotometer. Transparency (T) was calculated by dividing the absorbance at 600 nm by the sample thickness, expressed in millimeters. Table 8 shows the transparency values ​​for both samples, with greater light transmission observed for the coated paper.

[0169] Table 8. Transparency values ​​(T) of uncoated paper samples and paper coated with a 130 g / m 3%HV PHBV layer 2 .

[0170] Sample T (mrrr 1 )

[0171] Kraft paper 63 g / m 2 17

[0172] Coated paper 14

[0173] Water vapor transmission rate (WVTR) values ​​were determined. The water vapor transmission rate (WVTR) value was determined using an ASTM E96-9 test using Payne permeability cups with 100% relative humidity (RH) on one side of the material and 0% RH on the other. The Payne cups were stored at 25°C, and their weight was measured periodically until a constant weight was reached. Aluminum foil was used as a control to estimate water vapor loss through the seal. Table 9 shows the results obtained. The coated paper sample showed a much higher water vapor barrier than the paper.

[0174] Table 9. Water vapor transmission rate (WVTR) values. Sample WVTR (g / m 2 d)

[0175] Kraft paper 63 g / m 2 >800 Coated paper 6.5 ± 2.7

[0176] The water absorption of both the paper sample and the coated paper was determined using the TAPPI method T441 cm-13. The water absorption value, indicated by the Cobb index, was calculated by measuring the amount of water absorbed by the paper for 60 s. The Cobb value or water absorption value is represented by the amount of water absorbed by the paper per unit area (g / m 2 ). The results are shown in Figure 9. While the paper showed a water absorption of more than 40 g / m 2 , the coated paper showed a value of less than 6 g / m 2 .

[0177] Grease resistance was evaluated for both the paper and coated paper samples using TAPPI Method T559 cm-12. The test involves depositing a series of numbered solutions, each with different surface tensions and viscosities, onto the sample surface. The solutions are numbered from 1 (least aggressive) to 12 (most aggressive). The highest-numbered solution that leaves no mark on the sample surface corresponds to its rating according to this Kit. The results are shown in Table 10. While the uncoated paper showed no resistance, the coated sample showed resistance up to Kit 10.

[0178] Table 10. KIT values ​​of the grease resistance test for paper and coated paper

[0179] Sample VALUE KIT

[0180] Kraft paper 63 g / m 2 EITHER

[0181] Coated paper 10

Claims

CLAIMS 1.- Method for obtaining a translucent paper-based material with barrier properties, comprising the following steps: a) preparing a mixture of polymer in solvent at a concentration of between 0.01 and 99% w / v b) subjecting the mixture prepared in step a) to an electrohydrodynamic process, aerohydrodynamic process or any combination of both, c) coating the paper with the material resulting from steps a) and b) and subjecting it to a calendering, annealing or heat treatment process with pressure, wherein said process is carried out at a temperature lower than 800 e C. 2.- Method according to claim 1, wherein the mixture prepared in step a) is a solution, emulsion or suspension. 3.- Method according to claims 1 or 2, wherein the polymer of the mixture prepared in step a) is a biodegradable and / or compostable biopolymer. 4.- Method according to claim 3, wherein the biopolymer is selected from: - polyhydroxyalkanoates, such as polyhydroxybutyrate or polyhydroxybutyric acid (PHB), polyhydroxyvalerate (PHV), polyhydroxybutyrate-valerate (PHBV), medium chain length PHA (mcl-PHA), and all their possible copolymers - poly-8-caprolactone (PCL) and all its copolymers - polylactic acid (PLA) and all its copolymers - polyphosphazenes - polyorthoesters - polyesters obtained from precursors such as polymethylene terephthalate (PTT), polybutylene terephthalate (PBT), polybutylene succinate (PBS), and all possible copolymers of these - polyvinyl alcohols (PVOH) and their copolymers with ethylene (EVOH) - polyacrylates (PAC) and polyacrylic acid (PAA) - water-soluble polyacrylonitriles (PAN) - acrylic / methacrylic aster polymers - proteins such as zein, gluten and its derivatives, collagen, gelatin, casein, whey protein, soy proteins and their derivatives, silk fibroma or elastins - polysaccharides such as carrageenans and derivatives, alginates, pullulan, dextran, gum arabic, chitosan and their derivatives - cellulose and its derivatives such as ethylcellulose, hydroxypropylcellulose, methylcellulose, or hydroxypropylmethylcellulose - glycogen, starch, and polymers derived from it such as thermoplastic starch (TPS) and - lipids such as waxes, resins, vegetable or mineral oils, acetoglycerides, fatty acids, lignin and derivatives such as sulfonated lignin (SL) and any combination thereof. 5.- Method according to claim 4, wherein the biopolymer has a molecular weight by mass (Mw) of less than 2,000,000 Daltons. 6.- Method according to claim 5, wherein the biopolymer has a molecular weight by mass of less than 300,000 Daltons. 7.- Method according to claim 4, wherein the biopolymer is a polyhydroxyalkanoate or any combination of polyhydroxyalkanoates. 8.- Method according to claim 7, wherein the biopolymer is a polyhydroxyalkanoate with comonomer contents other than hydroxybutyrate greater than 10% molar. 9.- Method according to any one of claims 1 to 8, wherein the mixture prepared in step a) comprises other additives that are selected from among plasticizers, surfactants, reinforcements, process additives, antioxidants, colorants, nanoreinforcements or any combination thereof. 10.- Method according to any one of claims 1 to 9, wherein the mixture is subjected to an electrohydrodynamic process.

11. - Method according to claim 10, wherein the electro-hydrodynamic process comprises the use of an electro-hydrodynamic technique selected from the list consisting of electrospinning, coaxial electrospinning, electrohydrodynamic jet printing, electrohydrodynamic direct writing, melt electrospinning, electrostatic solution blowing, electrospraying, coaxial electrospraying and pressurized gas assisted electrospraying. 12.- Method according to claim 1 1, wherein the electro-hydrodynamic technique is electrospinning. 13.- Method according to claim 12, wherein the technique is electrospinning with multi-injectors, with or without needles. 14.- Method according to claims 12 or 13, wherein the electrospinning process comprises a voltage at the emitter of between 0.01 and 5000 kV, and a voltage at the collector of between 0.01 and -5000 kV. 15.- Method according to any one of claims 12 to 14, wherein the electrospinning process is carried out at a temperature between 1 e C and 100 e C. 16.- Method according to any one of claims 12 to 15, wherein the electrospinning process is carried out at a relative humidity of between 1 and 99%. 17.- Method according to any one of claims 12 to 16, wherein the electrospinning process is carried out at a flow rate per emitter of between 0.001 ml / min and 500 ml / min. 18.- Method according to any one of claims 12 to 17, wherein the electrospinning process is carried out with a roll-to-roll collector system at a speed of between 0.01 m / min and 10,000 m / min. 19.- Method according to any one of claims 1 to 9, wherein the mixture is subjected to an aero-hydrodynamic process.

20. Method according to claim 16, wherein the aero-hydrodynamic process comprises the use of an aero-hydrodynamic technique selected from the list consisting of: centrifugal jet spinning, draw-assisted spinning, solution-blown spinning, centrifugal blow-blown spinning and solution-blown spray spinning, more preferably solution-blown spinning. 21.- Method according to any one of claims 1 to 20, wherein step c) is carried out by means of a pressure calendering process at a temperature lower than 800 e C and at a speed between 0.001 and 100,000 rpm. 22.- Method according to any one of the preceding claims, wherein the grammage of the coating applied to the paper is between 0.01 and 10,000 g / m 2 and more preferably between 0.2 and 500 g / m 2 . 23.- Method according to any one of the preceding claims, wherein the percentage by mass of coating must preferably be greater than 1%, more preferably greater than 20% and even more preferably greater than 40%. 24.- Translucent paper-based material with barrier properties, obtained by a method according to claims 1 to 23, comprising paper and a coating with at least one polymer and having: - a transparency value (T) lower than that of the paper substrate. - a water vapour transmission rate between 0 and 500 g / m 2 d - an oxygen transmission rate between 0 and 500 cm 3 / m 2 d - a water absorption between 0 and 500 g / m 2 - a grease resistance with a kit value greater than 0. 25.- Material according to claim 24, further comprising additives selected from plasticizers, surfactants, reinforcements, process additives, antioxidants, colorants, nanoreinforcements or any combination thereof.