Diamond spin sensor and method for manufacturing same

The diamond spin sensor with an inclined surface and CVD-formed NV centers on specific crystal planes addresses alignment issues, achieving improved sensitivity and independent field/temperature measurement, leveraging large (100) crystal plane substrates for cost-effective production.

WO2024219050A1PCT designated stage expired Publication Date: 2024-10-24NISSIN ELECTRIC CO LTD +1

Patent Information

Application Number
PCT/JP2024/003395
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-02-02
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing diamond spin sensors face challenges in aligning NV centers for enhanced detection sensitivity due to the small size of substrates with (111) crystal planes, leading to high costs and difficulties in synthesizing thick films with aligned NV axes, as well as issues with patterning substrates with (100) crystal planes resulting in NV centers pointing in multiple directions.

Method used

A diamond spin sensor with an inclined surface on the substrate, where the number of color centers with axes perpendicular to the surface is significantly higher than those not perpendicular, allowing for improved alignment and detection sensitivity, and a manufacturing method involving CVD to form NV centers on (111) and (-1-11) crystal planes, enabling independent detection of magnetic and electric fields and temperature measurement without magnetic field interference.

Benefits of technology

The solution results in a diamond spin sensor with aligned color centers, enhancing detection sensitivity and allowing for accurate measurement of magnetic, electric fields, and temperature without magnetic field interference, using readily available large (100) crystal plane substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024003395_24102024_PF_FP_ABST
    Figure JP2024003395_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This diamond spin sensor includes: a diamond substrate; and inclined surfaces formed on the diamond substrate. Color centers having electron spin are formed on the inclined surfaces. Among the color centers formed on the inclined surfaces, the color centers having a color center axis perpendicular to the inclined surfaces exist at a proportion of at least two times the existence of color centers having a color center axis which is not perpendicular to the inclined surfaces.
Need to check novelty before this filing date? Find Prior Art

Description

Diamond spin sensor and its manufacturing method

[0001] This disclosure relates to a diamond spin sensor and a method for manufacturing the same. This application claims priority to Japanese Application No. 2023-067532, filed on April 18, 2023, and incorporates by reference all of the contents of said Japanese application.

[0002] A diamond spin sensor using the NV center of diamond (hereinafter referred to as NV center) is known. When the NV center, which consists of nitrogen (i.e., N) that has entered the substitution position of carbon (i.e., C) in diamond and a vacancy (i.e., V: Vacancy) adjacent to the nitrogen, becomes negatively charged, its ground state becomes a triplet state (i.e., spin S=1). The negatively charged NV center is NV - Although the term "NV center" is used in the present specification, it will also be referred to as an NV center below. When a charged NV center is excited with a wavelength of 532 nm (i.e., green light), it emits fluorescence with a wavelength of 637 nm (i.e., red light). The intensity of the fluorescence changes depending on the spin state, and the spin state changes due to magnetic resonance between a magnetic field applied to the NV center and microwaves or radio waves, so it can be used as a magnetic sensor.

[0003] For detection, a diamond substrate containing an NV center, which is a diamond spin sensor, is used; an optical system that transmits excitation light from a light source and irradiates the NV center; an optical system that collects fluorescence from the NV center and transmits it to a photodetector; and a waveguide that transmits microwaves from a power source and irradiates the NV center.

[0004] M. Lesik, J.-P. Tetienne, A. Tallaire, J. Achard, V. Mille, A. Gicquel, J.-F. Roch, V. Jacques, “Perfect preferential orientation of nitrogen-vacancy defects in a synthetic diamond sample”, Appl. Phys. Lett. 104, 113107 (2014). Y. Nakano, H. Inagaki, K. Kobayashi, M. Haruyama, C. Kato, K. Christoph E. Nebel1, Xufang Zhang, T. Matsumoto, T. Inokuma, S. Yamazaki, N. Tokuda, N. Tokuda, “Development of a technique for the growth of highly nitrogen-doped diamond by suppressing two-dimensional nucleation”, Proceedings of the 69th Spring Meeting of the Japan Society of Applied Physics (2022) 25a-E204-1. M. W. Doherty, V. M. Acosta, A. Jarmola, M. J. Barson, N. B. Manson, D. Budker, and L. C. Hollenberg, “Temperature shifts of the resonances of the NV- center in diamond”, PHYSICAL REVIEW B 90, 041201(R) (2014)

[0005] A diamond spin sensor according to one aspect of the present disclosure includes a diamond substrate and an inclined surface formed on the diamond substrate, wherein color centers having electronic spins are formed on the inclined surface, and among the color centers formed on the inclined surface, color centers whose color center axes are perpendicular to the inclined surface are present at a ratio of at least twice the ratio of color centers whose color center axes are not perpendicular to the inclined surface.

[0006] FIG. 1 is a perspective view of a diamond spin sensor according to an embodiment. FIG. 2 is a schematic diagram showing the crystal planes of diamond. FIG. 3 is a block diagram showing the configuration of an apparatus used for measurements using the diamond sensor shown in FIG. 1. FIG. 4 is a sequence diagram showing the timing of irradiation of excitation light and electromagnetic waves, and the timing of measurement of synchrotron radiation during measurements using the diamond spin sensor shown in FIG. 1. FIG. 5 is a graph showing the relationship between the observed signal intensity (i.e., the radiation light intensity) and the frequency of the electromagnetic wave (i.e., the microwave). FIG. 6 is a perspective view showing measurements of magnetic and electric fields using the diamond spin sensor shown in FIG. 1. FIG. 7 is a schematic diagram showing the NV center of diamond. FIG. 8 is a perspective view showing the relationship between the four possible directions of the NV axis of diamond and the magnetic field in the <100> direction. FIG. 9 is a graph showing the relationship between the signal intensity observed in the state shown in FIG. 8 and the electromagnetic wave frequency. FIG. 10 is a perspective view showing the relationship between the four possible directions of the NV axis of diamond and the magnetic field in the <110> direction. Fig. 11 is a graph showing a schematic relationship between the signal intensity and the electromagnetic wave frequency observed in the state of Fig. 10. Fig. 12 is a perspective view showing the relationship between the four directions of the NV axis that diamond can take and the magnetic field in the <111> direction. Fig. 13 is a graph showing a schematic relationship between the signal intensity and the electromagnetic wave frequency observed in the state of Fig. 12. Fig. 14 is a schematic diagram showing a method for manufacturing a diamond spin sensor. Fig. 15 is a schematic diagram showing a method for manufacturing a diamond spin sensor, different from that of Fig. 14.

[0007] [Problem to be Solved by the Present Disclosure] The axis passing through N and V of the NV center formed in diamond (hereinafter referred to as the NV axis) can take four directions based on the diamond's crystal structure. Since the sensitivity as a sensor depends on the direction of the NV axis relative to the detection target (e.g., a magnetic field or electric field), it is preferable to align the NV axis. For example, the NV axis can be aligned perpendicular to the (111) crystal plane using CVD (Chemical Vapor Deposition). However, since the total number of NV centers is small and the amount of fluorescence is weak, a sufficient S / N ratio cannot be obtained. In addition, abnormal growth is likely to occur during CVD growth, making it difficult to synthesize a thick film with NV centers with aligned NV axis directions. Diamonds with a (111) crystal plane on their surface are small in size, making it difficult to obtain large substrates and resulting in high costs. There is also a method of patterning a substrate with a large (100) crystal plane and growing NV-oriented crystals, but this results in the formation of NV centers pointing in four directions, making it difficult to align the NV axes and provide anisotropy. These problems occur not only with NV centers, but also with diamonds that have color centers with electron spin.

[0008] Therefore, an object of the present disclosure is to provide a diamond spin sensor having color centers with aligned color center axes and capable of improving detection sensitivity, and a method for manufacturing the same.

[0009] Effect of the Present Disclosure According to the present disclosure, it is possible to provide a diamond spin sensor having color centers with aligned color center axes and capable of improving detection sensitivity, and a method for manufacturing the same.

[0010] [Description of Embodiments of the Present Disclosure] The contents of the embodiments of the present disclosure will be listed and described below. At least some of the embodiments described below may be combined in any combination.

[0011] (1) A diamond spin sensor according to a first aspect of the present disclosure includes a diamond substrate and an inclined surface formed on the diamond substrate, wherein color centers having electron spins are formed on the inclined surface, and among the color centers formed on the inclined surface, color centers whose color center axes are perpendicular to the inclined surface exist at a ratio of at least twice as large as color centers whose color center axes are not perpendicular to the inclined surface. This makes it possible to realize a diamond spin sensor that has multiple color centers with aligned color center axes and can improve detection sensitivity.

[0012] (2) In the above (1), the color center is NV - This allows NV - Multiple NVs with aligned center axes - A diamond spin sensor having a center and capable of improving detection sensitivity can be realized.

[0013] (3) In the above (1) or (2), the inclined surface may include a first inclined surface and a second inclined surface. The second inclined surface may be disposed on the back surface of the first inclined surface. The first inclined surface may have a (111) crystal plane, and the second inclined surface may have a (-1-11) crystal plane. Among the color centers formed on the first inclined surface, color centers whose color center axes are perpendicular to the first inclined surface may exist at a ratio of at least twice the number of color centers whose color center axes are not perpendicular to the first inclined surface. Among the color centers formed on the second inclined surface, color centers whose color center axes are perpendicular to the second inclined surface may exist at a ratio of at least twice the number of color centers whose color center axes are not perpendicular to the second inclined surface. This allows sensitivity in two directions and enables independent detection of magnetic and electric fields. Furthermore, temperature can be measured without being affected by magnetic fields. The notation "-1" corresponds to a notation in which a bar (horizontal bar) is added to a "1."

[0014] (4) In the above (3), when measuring the electric field formed by the current flowing through a predetermined portion of the conductive wire, the diamond spin sensor may be positioned relative to the conductive wire so that the predetermined portion is located within a plane defined by the <111> direction, which is the normal direction of the first inclined plane, and the <-1-11> direction, which is the normal direction of the second inclined plane. This allows the electric field formed by the current flowing through the predetermined portion of the conductive wire to be measured with high accuracy.

[0015] (5) A method for manufacturing a diamond spin sensor according to a second aspect of the present disclosure includes a preparation step of preparing a single-crystal diamond substrate having a (001) crystal face on its surface, a crystal face formation step of forming (111) and (-1-11) crystal faces on the surface of the substrate, and an NV formation step of forming NV centers on the (111) and (-1-11) crystal faces by CVD. This makes it possible to manufacture a diamond spin sensor having multiple color centers with aligned color center axes, thereby improving detection sensitivity. Diamond substrates having a (100) crystal face are easily available in relatively large sizes, making it easy to manufacture diamond spin sensors.

[0016] (6) In the above (5), the method may further include, between the preparation step and the crystal plane formation step, a step of forming a mask of a predetermined width on the (001) crystal plane extending along the <1-10> direction, a step of etching the (001) crystal plane on which the mask is formed, and a step of removing the mask remaining after etching, and the crystal plane formation step may include a step of performing CVD in an environment containing methane and hydrogen, with the substrate at a predetermined temperature. This allows color centers to be formed on the (111) crystal plane and the (-1-11) crystal plane with larger areas than conventional color centers, thereby improving detection sensitivity.

[0017] (7) In the above (6), the CVD in the CVD step may be performed so that the α parameter, which represents the ratio of the growth rate in the <100> direction to the growth rate in the <111> direction, is 2 or more and 3.5 or less, thereby forming (111) crystal planes and (−1-11) crystal planes with wider areas.

[0018] (8) In the above (6) or (7), the volume ratio of methane to hydrogen may be 1% or more and 20% or less, and the predetermined temperature may be 600° C. or more and 1100° C. or less. This allows the (111) crystal plane and (−1-11) crystal plane to be formed with larger areas.

[0019] (9) In the above (5), between the preparation step and the crystal plane formation step, the method may further include the steps of forming a mask of a predetermined width on the (001) crystal plane and extending along the <1-10> direction, etching the (001) crystal plane on which the mask is formed, and removing the mask remaining after etching, and the crystal plane formation step may include a step of performing hydrogen plasma etching. This allows color centers to be formed on the (111) crystal plane and the (-1-11) crystal plane with larger areas than conventional color centers, thereby improving detection sensitivity.

[0020] [Details of the embodiments of the present disclosure] In the following embodiments, the same components are denoted by the same reference numerals, and their names and functions are also the same. Therefore, detailed descriptions thereof will not be repeated.

[0021] 1, a diamond spin sensor 100 according to an embodiment of the present disclosure includes a diamond substrate 102 and a plurality of protrusions 104 formed on the diamond substrate 102. The surface 112 is a (001) crystal plane. The protrusions 104 include a first slant surface 106 and a second slant surface 108 located on the back surface thereof. The first slant surface 106 is a (111) crystal plane, and the second slant surface 108 is a (-1-11) crystal plane. The protrusions 104 are triangular prisms, with one side surface of the triangular prism abutting the surface 112. The protrusions 104 extend along the <1-10> direction indicated by arrow 114.

[0022] Referring to Figure 2, the (001) crystal plane in diamond is the plane defined by points A5, A6, A7, and A8. The (111) crystal plane is the plane defined by points A5, A2, and A4. The (-1-11) crystal plane is the plane defined by points B2, B4, and A5. The <1-10> direction is, for example, the direction passing through points A1 and C1.

[0023] As will be described later, the convex portion 104 may extend along the <110> direction. In that case, the first inclined surface 106 is a (1-11) crystal plane, and the second inclined surface 108 is a (-111) crystal plane. With reference to FIG. 2 , the <110> direction is, for example, a direction passing through points A1 and A3. The (1-11) crystal plane is a plane defined by points A5, B4, and A2. The (-111) crystal plane is a plane defined by points A5, A4, and B2. As described above, there are two combinations of the extension direction of the convex portion 104 and the crystal planes of the first inclined surface 106 and the second inclined surface 108, but these are rotationally symmetric (specifically, four-fold symmetric) and are therefore the same.

[0024] The first slope 106 and the second slope 108 include NV centers 110 composed of nitrogen N and vacancies V. In most of the NV centers 110 included in the first slope 106, the axis passing through N and V (hereinafter referred to as the NV axis) is arranged perpendicular to the first slope 106. In most of the NV centers 110 included in the second slope 108, the NV axis is arranged perpendicular to the second slope 108.

[0025] As will be described later, the position of N substituting for C in a diamond single crystal can take four positions relative to V. Therefore, the NV axis can take four directions. As described above, many of the NV centers included in the first inclined surface 106 and the second inclined surface 108 have their NV axes aligned perpendicular to each surface. As will be described later, the number of NV centers whose NV axes are aligned perpendicular to each surface depends on the manufacturing process. For example, it is preferable that the ratio of the number of NV centers whose NV axes are aligned perpendicular to each surface be approximately twice or more the number of NV centers whose NV axes are aligned in the other three directions. This makes it possible to realize a diamond spin sensor 100 that has multiple NV centers whose NV axes are aligned and can improve detection sensitivity.

[0026] Measurement using the diamond spin sensor 100 is performed, for example, by the configuration shown in Fig. 3. The control unit 230 includes a CPU (Central Processing Unit) and a storage unit (neither of which are shown). The processing performed by the control unit 230, which will be described later, is realized by the CPU reading and executing a program stored in advance in the storage unit.

[0027] The excitation light generating unit 210 generates excitation light for exciting the NV centers of the diamond spin sensor 100 under the control of the control unit 230. The control unit 230 supplies, for example, a voltage to the excitation light generating unit 210 at a predetermined timing to cause the excitation light generating unit 210 to emit light. The excitation light 204 is green light (i.e., wavelength 490 to 560 nm). The excitation light 204 is preferably laser light, and the excitation light generating unit 210 is preferably a semiconductor laser (e.g., emitted light wavelength 532 nm).

[0028] The filter 212 is an element for separating the excitation light 204 incident from the excitation light generating unit 210 and the light (i.e., fluorescent light) emitted from the diamond spin sensor 100, as will be described later. For example, the filter 212 is a filter that cuts off (i.e., reflects) light with wavelengths equal to or less than a predetermined wavelength and passes light with wavelengths greater than the predetermined wavelength, or a bandpass filter that passes light with wavelengths within a predetermined wavelength range and cuts off (i.e., reflects) light with wavelengths outside the predetermined wavelength range. Generally, excitation light has a shorter wavelength than fluorescent light, so such a configuration is preferable. The filter 212 is preferably a dichroic mirror with this function.

[0029] The focusing element 214 focuses the excitation light 204 input from the filter 212. The focusing element 214 is, for example, a spherical lens. The focusing element 214 inputs as much of the excitation light diffused and output from the excitation light generating unit 210 as possible into the end of the optical waveguide 216. The optical waveguide 216 includes a medium for transmitting light and transmits light in both directions. That is, the optical waveguide 216 has a first end and a second end, and transmits the excitation light 204 incident on the first end to the second end located near the diamond spin sensor 100. The optical waveguide 216 also transmits the emitted light (i.e., fluorescence) from the diamond spin sensor 100 incident on the second end to the first end and outputs it. The optical waveguide 216 is, for example, an optical fiber.

[0030] The electromagnetic wave irradiating unit 202 irradiates the diamond spin sensor 100 with electromagnetic waves (e.g., microwaves). The electromagnetic wave irradiating unit 202 is, for example, a coil formed including an electric conductor. The electromagnetic waves are supplied from the electromagnetic wave generating unit 232 to the electromagnetic wave irradiating unit 202 by, for example, a coaxial cable. The irradiation of the excitation light and electromagnetic waves to the diamond spin sensor 100 is controlled by the control unit 230, and is performed, for example, at the timing shown in FIG. 4.

[0031] Referring to Fig. 4, the control unit 230 controls the excitation light generating unit 210 to output excitation light for a predetermined time (e.g., period t1) at a predetermined timing. The control unit 230 controls the electromagnetic wave generating unit 232 to output electromagnetic waves for a predetermined time (e.g., period t2) at a predetermined timing. Any appropriate pulse sequence may be used during period t2. This allows the excitation light and the electromagnetic waves to be irradiated onto the diamond in a temporally and spatially combined manner. As will be described later, the control unit 230 captures the output signal of the light detecting unit 220 at a predetermined timing (e.g., within period t3) and stores it in the memory unit.

[0032] The NV center transitions from the ground state to an excited state when exposed to green light with a wavelength of 490 nm to 560 nm (e.g., laser light of 532 nm), and then emits red light with a wavelength of 630 nm to 800 nm (e.g., fluorescent light of 637 nm) and returns to the ground state. The NV center captures one electron (i.e., NV - ) the magnetic quantum number m s forms a spin triplet state of -1, 0, or +1, and in the presence of a magnetic field, m s The energy levels of the state of = ±1 are separated according to the magnetic field strength (i.e., Zeeman separation). s = 0 state is m s After causing a transition to a state of ∑ = ±1 (i.e., electron spin resonance), the diamond is excited by irradiating it with green light. As a result, the transition when returning to the ground state includes a transition that does not emit light (i.e., fluorescence), so the intensity of the observed emitted light decreases. Therefore, a valley (i.e., a drop in the signal) is observed in the ESR (Electron Spin Resonance) spectrum. As described above, the control unit 230 controls the excitation light generator 210 and the electromagnetic wave generator 232 to measure a spectrum such as that shown in FIG. 5. The distance Δf between the two observed valleys depends on the magnetic field strength at the position of the diamond spin sensor 100. The control unit 230 can calculate the magnetic field from Δf.

[0033] The LPF (Long Pass Filter) 218 ​​is a long-pass filter that passes light with wavelengths equal to or greater than a predetermined wavelength and cuts (e.g., reflects) light with wavelengths shorter than the predetermined wavelength. The fluorescent light 206, which is the emitted light of the diamond spin sensor 100, is red light and passes through the LPF 218, but the excitation light 204 output from the excitation light generator 210 has a shorter wavelength and does not pass through the LPF 218. This prevents the excitation light 204 emitted from the excitation light generator 210 from being detected by the photodetector 220 and becoming noise, which reduces the detection sensitivity of the fluorescent light 206, which is the emitted light of the diamond spin sensor 100. The photodetector 220 generates and outputs an electrical signal corresponding to the incident light. The photodetector 220 is, for example, a photodiode. The output signal from the photodetector 220 is acquired by the control unit 230.

[0034] It has been explained above that the magnetic field can be calculated from changes in the ESR spectrum, but it is known that the resonance frequency of the NV center has temperature dependence in the range from 120 K to 700 K. For example, as disclosed in Non-Patent Document 3, it is possible to measure temperature from changes in the frequency of an ODMR (Opticaly Detected Magnetic Resonance) signal.

[0035] Referring to FIG. 6 , when measuring an electric field generated by a current using the diamond spin sensor 100, the extension direction of the convex portion 104 of the diamond spin sensor 100 is positioned perpendicular to the conductive line 300, which is a predetermined portion of the conductive line through which the current flows. The predetermined portion is not limited to a portion of the conductive line, but may be the entire conductive line. That is, as described above, the first inclined surface 106 and the second inclined surface 108 are (111) and (-1-11) crystal planes, respectively, and the diamond spin sensor 100 is positioned so that the conductive line 300 is located within a plane defined by the <111> and <-1-11> directions perpendicular to these crystal planes. Note that a plane defined by two directions refers to a plane that includes these two directions. As described above, the multiple NV centers 110 present on each of the first inclined surface 106 and the second inclined surface 108 of the convex portion 104 have NV axes aligned perpendicular to each plane, and there are two directions in which the NV axes are aligned on the convex portion 104. That is, the first slant surface 106 is a (111) crystal plane, and the NV axes of each NV center formed on the first slant surface 106 are aligned in the <111> direction, which is perpendicular to the first slant surface 106. The second slant surface 108 is a (-1-11) crystal plane, and the NV axes of each NV center formed on the second slant surface 108 are aligned in the <-1-11> direction, which is perpendicular to the second slant surface 108. When the diamond spin sensor 100 is positioned in this manner, the NV centers 110 present on the first slant surface 106 and the second slant surface 108 are included in a plane 302 passing through the conductive line 300.

[0036] A current flowing through the conductive wire 300 forms a magnetic field vector around the conductive wire 300 in the tangential direction of a concentric circle centered on the conductive wire 300, and the magnetic field vector formed at a position within the plane 302 is perpendicular to the plane 302. Referring to FIG. 7, the magnetic field detected by the NV center has a component in the NV axis direction. That is, the diamond spin sensor 100 detects a change in signal intensity (i.e., fluorescence intensity) according to B cos θ, where θ is the angle formed between the magnetic field vector B and the NV axis. As shown in FIG. 6, when the diamond spin sensor 100 is positioned relative to the conductive wire 300, the magnetic field formed in the plane 302 has no component within the plane 302. Therefore, since the angle θ is 90 degrees and cos θ = 0, the diamond spin sensor 100 (i.e., the NV center 110) cannot detect the magnetic field formed by the current flowing through the conductive wire 300.

[0037] On the other hand, with regard to the electric field, the NV center can detect components in a direction perpendicular to the NV axis. As shown in Figure 6, when the diamond spin sensor 100 is placed relative to the conductive wire 300, the electric field formed on the plane 302 has a component perpendicular to the NV axis. Therefore, the electric field can be detected by the diamond spin sensor 100 (i.e., the NV center 110). In other words, by placing the diamond spin sensor 100 relative to the conductive wire 300 as shown in Figure 6, the diamond spin sensor 100 can measure the electric field without being affected by the magnetic field.

[0038] Similarly, when measuring temperature, as shown in Fig. 6, by placing the diamond spin sensor 100 relative to the conductive wire 300, the diamond spin sensor 100 (i.e., the NV center 110) can measure the temperature around the conductive wire 300 without being affected by the magnetic field formed by the current flowing through the conductive wire 300. Therefore, if the magnetic field direction is known or can be predicted in advance, the diamond spin sensor 100 can be placed so that the extension direction of its convex portion 104 is perpendicular to the magnetic field and the temperature is measured, allowing accurate measurement without being affected by the magnetic field.

[0039] As mentioned above, there are four possible directions for the NV axes of the NV centers. In the diamond spin sensor 100, the proportion of NV centers whose NV axes are oriented perpendicular to the first inclined surface 106 and the second inclined surface 108 is approximately twice or more the number of NV centers whose NV axes are oriented in the other three directions. This proportion can be evaluated by measurement. With reference to Figures 8 to 13, it will be explained that the distribution of the NV axes of the NV centers arranged on the convex portion 104 and the first inclined surface 106 of the diamond spin sensor 100 can be estimated by changing the direction of the magnetic field applied externally to the diamond spin sensor 100, performing ODMR, and observing the detected signals.

[0040] FIG. 8 shows the state in which a magnetic field B is applied in the <100> direction in the diamond crystal structure. The crystal axis is shown in the lower right. In FIG. 8, the bracketed [V] represents a vacancy, and the bracketed numbers [1] to [4] represent the four positions where nitrogen (N) can be located relative to [V]. By performing ODMR using a diamond containing N at the same ratio at positions [1] to [4] and applying a magnetic field B as shown in FIG. 8, a graph including two valleys as shown in FIG. 9 is obtained. This is because the angle θ between the NV axis and the magnetic field B in the <100> direction when N is at each position [1] to [4] is θ = 54.7 (degrees). In other words, since the same magnetic field strength is detected by the NV sensors where N is at each position [1] to [4], the frequency proportional to the magnetic field strength (i.e., the distance between the two valleys) is equal.

[0041] Figure 10 shows the state in which a magnetic field B is applied in the <110> direction in the diamond crystal structure. The crystal axes are the same as those in Figure 8. Similarly, by performing ODMR using a diamond containing N at the same ratio at positions [1] to [4] and applying a magnetic field B as shown in Figure 10, a graph containing three valleys is obtained, as shown in Figure 11. This is because the angles θ between the NV axis and the magnetic field B in the <110> direction when N is at each position from [1] to [4] are 35.3 degrees, 90.0 degrees, 35.3 degrees, and 90.0 degrees, respectively. θ is either 35.3 degrees or 90.0 degrees. In other words, two types of magnetic field strength are detected by the NV sensors where N is at each position from [1] to [4], and therefore two types of frequencies proportional to the magnetic field strength (i.e., the distance between the two valleys) are detected. The valleys on both sides of Figure 11 are detected by NV centers with NV axes of θ = 35.3 (degrees). The central valley is detected by the NV center with the NV axis at θ=90.0 (degrees), and is the overlap of two valleys (Δf=0 in FIG. 5).

[0042] Figure 12 shows the state in which a magnetic field B is applied in the <111> direction in the diamond crystal structure. The crystal axes are the same as those in Figure 8. Similarly, by performing ODMR using a diamond containing N at the same ratio at positions [1] to [4] and applying a magnetic field B as shown in Figure 12, a graph containing four valleys as shown in Figure 13 is obtained. This is because the angles θ between the NV axis and the magnetic field B in the <111> direction when N is at each position from [1] to [4] are 0.0 degrees, 70.5 degrees, 70.5 degrees, and 70.5 degrees, respectively. In other words, θ is either 0.0 degrees or 70.5 degrees. The valleys on the left and right ends of Figure 13 are detected by NV centers with NV axes of θ = 0.0 (degrees). The two inner valleys are detected by NV centers with NV axes of θ = 70.3 (degrees). When θ = 70.3 (degrees), the value of cosθ is smaller than when θ = 0.0 (degrees), and the drop in signal strength is smaller; however, since the signal is detected by the NV center where N is located at each of the three positions [2] to [4], the drop in signal strength is greater than at the valleys on both the left and right ends.

[0043] The magnitude of the valley depression (i.e., signal intensity) shown in Figures 9, 11, and 13 corresponds to the intensity of the fluorescence emitted from the NV center and depends on the proportion of the four NV axis directions of the diamond. Therefore, by performing ODMR while changing the direction of the magnetic field applied to the diamond crystal structure, the proportion of the NV axis directions can be calculated from the observed valley (specifically, the degree of depression).

[0044] (First Manufacturing Method of Diamond Spin Sensor) A manufacturing method for the diamond spin sensor shown in FIG. 1 will be described. Referring to FIG. 14, in step (A), a diamond substrate 500 of a predetermined size is prepared. Specifically, a type Ib diamond single crystal synthesized by the high-pressure, high-temperature (HPHT) method is cut and polished with a laser so that the (001) plane becomes the main surface. The diamond substrate 500 is then prepared by cleaning using a mixture of concentrated sulfuric acid and concentrated nitric acid. Diamonds are classified according to the presence or absence of impurities and the type of impurity. Type Ib diamonds contain nitrogen atoms as impurities (i.e., they have NV centers).

[0045] Following step (A), in step (B), an aluminum (Al) film is formed on the surface (i.e., the (001) plane) of the diamond substrate 500, for example, by sputtering, a pattern is formed by photolithography, and a rectangular mask 502 (i.e., an Al mask) is formed by etching using buffered hydrofluoric acid. The mask 502 is formed, for example, so as to extend in the <1-10> direction relative to the diamond crystal. The dimensions of the mask 502 are, for example, 3 μm wide and 100 μm long. Multiple masks 502 may be formed in parallel. Ten masks 502 may be formed, for example, spaced 10 μm apart from each other. Note that the mask 502 may also be formed so as to extend in the <110> direction relative to the diamond crystal.

[0046] The mask material is not limited to Al, but may be tungsten (W) or SiO 2The etching material is not limited to buffered hydrofluoric acid, but may be alkali or the like, and may be an appropriate material depending on the mask material.

[0047] Following step (B), in step (C), the diamond substrate 500 is etched by dry etching using the RIE (Reactive Ion Etching) method to form a wall surface along the rectangular mask 502. The gas used for dry etching is carbon tetrafluoride (CF 4 ) and oxygen (O 2 The mixture ratio (volume ratio) can be, for example, CF 4 / O 2 = 2%. The pressure of the mixed gas is, for example, 1 Pa. The RF power is, for example, 300 W, and dry etching is performed for, for example, 1 hour. The mask 502 remaining after dry etching is removed. CF 4 The diamond substrate 500 is etched by the cations 504. The diamond substrate 500a shows the diamond substrate 500 after etching. The etching conditions are not limited to those described above. The etching conditions include a mixture ratio of CF 4 / O 2 = 1% to 50%, the pressure of the mixed gas may be 0.1 Pa to 100 Pa, and the RF power may be 100 W to 3 kW.

[0048] In step (D), the diamond substrate 500a formed in step (C) is placed in a microwave plasma CVD apparatus and (001) oriented growth is performed. This forms a first slope 506 having a long (111) crystal plane along the wall surface formed in step (C), and a second slope 508 having a (-1-11) crystal plane on the back side of the first slope 506. For example, methane (CH 4 ) and hydrogen (H 2 ) mixed gas (mixing ratio is CH 4 / H 2The first and second oblique surfaces 506 and 508 are grown in an environment with a pressure of 100 Torr (approximately 13.3 kPa), a microwave power of 2 kW, and a substrate temperature of 800° C. To form the (111) and (−1-11) crystal planes by (001) oriented growth, a low temperature and high concentration of CH 4 It is preferable to carry out CVD using

[0049] As described above, when the mask 502 is formed so as to extend in the <1-10> direction relative to the diamond crystal, a first inclined surface 506 having a (111) crystal plane and a second inclined surface 508 having a (-1-11) crystal plane are formed. When the mask 502 is formed so as to extend in the <110> direction relative to the diamond crystal, a first inclined surface 506 having a (1-11) crystal plane and a second inclined surface 508 having a (-111) crystal plane are formed.

[0050] Following step (D), in step (E), (111) oriented growth is performed in a microwave plasma CVD apparatus while adding nitrogen (N), to form a first NV layer 510 and a second NV layer 512 having oriented NV centers on the surface of the first slant surface 506 (i.e., the (111) crystal plane) and the second slant surface 508 (i.e., the (-1-11) crystal plane), respectively. That is, in the first NV layer 510, an NV center having an NV axis perpendicular to the surface of the first NV layer 510 is formed. In the second NV layer 512, an NV center having an NV axis perpendicular to the surface of the second NV layer 512 is formed. For example, CH 4 , H 2 and N 2 The gas mixture is CH 4 / H 2 = 0.05%, N 2 / CH 4 The growth is performed under the conditions of 10% vapor pressure, 80 Torr (approximately 10.7 kPa), microwave power of 3 kW, and substrate temperature of 900°C. Note that the CVD conditions for forming NV centers with NV axes perpendicular to the surface are not limited to those described above. The CVD conditions are as follows: gas composition: CH 4 / H 2 = 0.01% to 1%, and N 2 / CH 4=0.1% to 50%, pressure 50 Torr to 200 Torr (approximately 6.67 kPa to 26.7 kPa), microwave power 1 kW to 5 kW, substrate temperature 600°C to 1000°C, etc. may be used.

[0051] This completes the manufacture of the diamond spin sensor 100 shown in Figure 1. That is, it is possible to manufacture a diamond spin sensor 100 that has multiple NV centers with aligned NV axes, thereby improving detection sensitivity. Diamond substrates with a (100) crystal face are readily available in relatively large sizes, making it easy to manufacture diamond spin sensors.

[0052] As described above, the first manufacturing method for a diamond spin sensor includes, between step (A) and the crystal plane formation step (D), step (B) of forming a mask 502 of a predetermined width extending along the <110> direction on the (001) crystal plane. It also includes an etching step of etching the (001) crystal plane on which the mask 502 is formed, and a step (C) of removing the mask 502 remaining after etching, and the crystal plane formation step (D) includes a step of performing CVD in an environment containing methane and hydrogen at a predetermined temperature. This allows NV centers to be formed on the (111) crystal plane and the (-1-11) crystal plane, which have larger areas than conventional ones, thereby improving the detection sensitivity of the diamond spin sensor.

[0053] In step (D), the CVD growth condition is set such that the α parameter, which represents the ratio of the growth rates in the <100> direction and the <111> direction, is α≧2, thereby forming a surface oriented to the (111) plane and the (−1−11) plane. The growth rate in the <100> direction (i.e., the direction perpendicular to the (100) plane) is V 100 , the growth rate in the <111> direction (i.e., the direction perpendicular to the (111) plane) is V 111 Then, the α parameter is defined by the following equation:

[0054]

[0055] More preferably, α≧2.5. However, if α>3.5, the surface shape becomes rough, so α≦3.5 is preferable. As for specific synthesis conditions, the volume ratio of methane to hydrogen is not limited to the above value, and may be 1% or more and 20% or less. Furthermore, the substrate temperature is not limited to the above value, and may be 600°C or more and 1100°C or less. This allows the formation of (111) crystal planes and (−1-11) crystal planes with wider areas.

[0056] Using the diamond spin sensor manufactured as described above, the temperature of a sample in an environment where a magnetic field is present can be measured by placing the diamond spin sensor in a direction perpendicular to the NV axis and performing ODMR measurement. For example, the diamond spin sensor 100 is brought into contact with the sample to equalize their temperatures, and in the configuration shown in FIG. 3, an electromagnetic wave (e.g., microwave) is irradiated onto the diamond spin sensor 100 by the electromagnetic wave irradiator 202. The electromagnetic wave irradiator 202 may be, for example, a coil formed with an electrical conductor or a resonator such as a λ / 4 open stub made of copper foil and ceramic, and may irradiate microwaves with an intensity of, for example, 0.5 mW or more. The excitation light output from the light-emitting element may be irradiated onto the diamond spin sensor 100 through an optical waveguide 216 such as an optical fiber at an intensity of, for example, 0.1 mW or more.

[0057] (Second Manufacturing Method of Diamond Spin Sensor) The diamond spin sensor shown in Fig. 1 may be manufactured using a method other than the manufacturing method shown in Fig. 14. For example, the manufacturing method shown in Fig. 15 may be used. The manufacturing method shown in Fig. 15 includes the same processes as the manufacturing method shown in Fig. 14. Therefore, the following description will not be repeated and will mainly focus on the differences.

[0058] Referring to Fig. 15, in step (A), a diamond substrate 500 of a predetermined size is prepared, similar to step (A) of Fig. 14. Subsequently, in step (B), an aluminum (Al) film is formed on the surface (i.e., the (001) plane) of the diamond substrate 500, similar to step (B) of Fig. 14, and a pattern is formed by photolithography, followed by etching to form a rectangular mask 520 (i.e., an Al mask). The mask 520 is formed so as to extend in the <110> direction relative to the diamond crystal. However, the mask 520 is wider than the mask 502 of Fig. 14. The width of the mask 520 is, for example, 4 µm. A plurality of masks 520 may be formed in parallel. Ten masks 520 may be formed, spaced apart from each other by, for example, 10 µm.

[0059] 14, the diamond substrate 500 is etched by dry etching using the RIE method to form wall surfaces along the rectangular mask 520. The mask 520 remaining after the dry etching is removed.

[0060] In step (D), the diamond substrate 500a formed in step (C) is placed in a microwave plasma CVD apparatus and anisotropic etching (e.g., plasma etching) is performed. This forms a first slope 522 having a long (111) crystal plane along the wall surface formed in step (C), and a second slope 524 having a (-1-11) crystal plane on the back surface of the first slope 522. For example, anisotropic etching (i.e., hydrogen plasma etching) is performed using a single hydrogen gas (concentration 100%) at a pressure of 80 Torr (approximately 10.7 kPa), a microwave power of 3 kW, and a substrate temperature of 950°C.

[0061] 14, in step (E), (111)-oriented growth is performed in a microwave plasma CVD apparatus while adding nitrogen (N). As a result, a first NV layer 526 and a second NV layer 528 having oriented NV centers are formed on the first slant surface 522 (i.e., the (111) crystal plane) and the second slant surface 524 (i.e., the (-1-11) crystal plane), respectively. That is, in the first NV layer 526, an NV center having an NV axis perpendicular to the surface of the first NV layer 526 is formed. In the second NV layer 528, an NV center having an NV axis perpendicular to the surface of the second NV layer 528 is formed.

[0062] This completes the manufacture of the diamond spin sensor 100 shown in Figure 1. That is, it is possible to manufacture a diamond spin sensor 100 that has multiple NV centers with aligned NV axes, thereby improving detection sensitivity. Diamond substrates with a (100) crystal face are readily available in relatively large sizes, making it easy to manufacture diamond spin sensors.

[0063] As described above, the second manufacturing method for a diamond spin sensor includes, between step (A) and the crystal plane formation step (D), step (B) of forming a mask 520 of a predetermined width extending along the <110> direction on the (001) crystal plane. It also includes an etching step of etching the (001) crystal plane on which the mask 520 is formed, and a step (C) of removing the mask 520 remaining after etching, and the crystal plane formation step (D) includes a step of performing hydrogen plasma etching. This allows NV centers to be formed on the (111) crystal plane and the (-1-11) crystal plane, which have larger areas than conventional ones, thereby improving the detection sensitivity of the diamond spin sensor.

[0064] In the above, a case where a diamond having an NV center is used as the diamond has been described, but this is not limiting. Any diamond having a color center with electronic spin will suffice. A color center with electronic spin is a center that forms a spin triplet state and emits light when excited, with the NV center being a representative example. It is also known that color centers with electronic spin exist in silicon-vacancy centers (i.e., Si-V centers), germanium-vacancy centers (i.e., Ge-V centers), and tin-vacancy centers (i.e., Sn-V centers). Therefore, a diamond spin sensor may be constructed using a diamond containing any of these. This makes it possible to realize a diamond spin sensor that has multiple color centers with aligned color center axes and can improve detection sensitivity.

[0065] Using the diamond spin sensor manufactured as described above, for a sample in an environment where an AC magnetic field and an AC electric field are present, the diamond spin sensor is placed in a direction perpendicular to the NV axis, and electric field measurements are performed using a pulse sequence, thereby enabling the electric field applied to the sample to be measured without being affected by the magnetic field. A free induction decay (FID) signal can be used as the magnetic resonance signal. For example, in the configuration shown in FIG. 3, the diamond spin sensor 100 is placed near or within the sample, and an electromagnetic wave (e.g., microwave) is irradiated to the diamond spin sensor 100 by the electromagnetic wave irradiation unit 202. The electromagnetic wave irradiation unit 202 may be, for example, a coil formed with an electrical conductor or a resonator such as a λ / 4 open stub made of copper foil and ceramic, and may irradiate microwaves with an intensity of, for example, 0.5 mW or more. The excitation light output from the light-emitting element may be irradiated to the diamond spin sensor 100 through an optical waveguide 216 such as an optical fiber at an intensity of, for example, 0.1 mW or more.

[0066] Although the present disclosure has been described above by explaining the embodiments, the above-described embodiments are merely examples, and the present disclosure is not limited to only the above-described embodiments. The scope of the present disclosure is defined by the claims in the scope of the claims, taking into consideration the description of the detailed description of the invention, and includes all modifications within the meaning and scope equivalent to the wording described therein.

[0067] 100 Diamond spin sensor 102, 500, 500a Diamond substrate 104 Convex portion 106, 506, 522 First inclined surface 108, 508, 524 Second inclined surface 110 NV center 112 Surface 114 Arrow 202 Electromagnetic wave irradiation unit 204 Excitation light 206 Fluorescence 210 Excitation light generation unit 212 Filter 214 Light-collecting element 216 Optical waveguide 218 LPF 220 Light detection unit 230 Control unit 232 Electromagnetic wave generation unit 300 Conductive wire 302 Plane 502, 520 Mask 504 Cations 510, 526 First NV layer 512, 528 Second NV layer (A), (B), (C), (D), (E) Steps A1, A2, A3, A4, A5, A6, A7, A8, B2, B3, B4, B6, B7, B8, C1 Point N Nitrogen V Vacancy X, Y, Z axis

Claims

1. A diamond spin sensor comprising: a diamond substrate; and an inclined surface formed on the diamond substrate, wherein color centers having electronic spins are formed on the inclined surface, and among the color centers formed on the inclined surface, color centers whose color center axes are perpendicular to the inclined surface are present at a ratio of at least twice as high as color centers whose color center axes are not perpendicular to the inclined surface.

2. The color center is NV - The diamond spin sensor of claim 1 including a center.

3. A diamond spin sensor as described in claim 1 or claim 2, wherein the inclined surface includes a first inclined surface and a second inclined surface, the second inclined surface is disposed on the rear surface of the first inclined surface, the first inclined surface has a (111) crystal plane, the second inclined surface has a (-1-11) crystal plane, among the color centers formed on the first inclined surface, color centers whose color center axes are perpendicular to the first inclined surface exist at a ratio of at least twice as many as color centers whose color center axes are not perpendicular to the first inclined surface, and among the color centers formed on the second inclined surface, color centers whose color center axes are perpendicular to the second inclined surface exist at a ratio of at least twice as many as color centers whose color center axes are not perpendicular to the second inclined surface.

4. A diamond spin sensor as described in claim 3, wherein, when measuring the electric field formed by a current flowing through a predetermined portion of the conductive wire, the diamond spin sensor is positioned with respect to the conductive wire so that the predetermined portion is located within a plane defined by the <111> direction, which is the normal direction of the first inclined surface, and the <-1-11> direction, which is the normal direction of the second inclined surface.

5. A method for manufacturing a diamond spin sensor, comprising: a preparation step of preparing a substrate of single crystal diamond having a (001) crystal plane on its surface; a crystal plane formation step of forming a (111) crystal plane and a (-1-11) crystal plane on the surface of the substrate; and an NV formation step of forming NV centers on the (111) crystal plane and the (-1-11) crystal plane by CVD.

6. A method for manufacturing a diamond spin sensor as described in claim 5, further comprising, between the preparation step and the crystal face formation step, a step of forming a mask of a predetermined width extending along a <1-10> direction on the (001) crystal face, an etching step of etching the (001) crystal face on which the mask is formed, and a step of removing the mask remaining after the etching, and the crystal face formation step includes a CVD step of performing CVD by heating the substrate to a predetermined temperature in an environment containing methane and hydrogen.

7. A method for manufacturing a diamond spin sensor as described in claim 6, wherein the CVD in the CVD step is performed so that the α parameter, which represents the ratio of the growth rate in the <100> direction to the growth rate in the <111> direction, is 2 or more and 3.5 or less.

8. A method for manufacturing a diamond spin sensor as described in claim 6 or 7, wherein the volume ratio of methane to hydrogen is 1% or more and 20% or less, and the predetermined temperature is 600°C or more and 1100°C or less.

9. A method for manufacturing a diamond spin sensor as described in claim 5, further comprising, between the preparation step and the crystal face forming step, a step of forming a mask of a predetermined width extending along a <1-10> direction on the (001) crystal face, an etching step of etching the (001) crystal face on which the mask is formed, and a step of removing the mask remaining after the etching, wherein the crystal face forming step includes a step of performing hydrogen plasma etching.

Citation Information

Patent Citations

  • Drier, heat exchanging ventilator and drying control method

    JP2023067532A

  • Electromagnetic field near-field imaging system and method based on pulsed light detection magnetic resonance

    CN107356820A

  • Synthetic diamonds of high crystalline quality

    JP2009518273A

  • Magnetic measuring device

    JP2020063960A

  • Proteome assay using quantum sensor

    JP2021193377A

Cited By

  • Diamond sensor

    WO2025182849A1