Flexible metal-clad laminate plate and method for producing same
The flexible metal-clad laminate with a low-roughness copper foil and optimized surface structure, manufactured using a double belt press device, addresses the challenge of achieving high peel strength and environmental resistance for high-frequency applications, ensuring effective adhesion and electrical performance.
Patent Information
- Application Number
- PCT/JP2024/011537
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-24
AI Technical Summary
Existing flexible printed wiring boards face challenges in achieving sufficient peel strength and environmental resistance for high-frequency applications, particularly in harsh conditions, due to inadequate adhesion between the metal and insulating layers.
A flexible metal-clad laminate is developed using low-roughness copper foil with a specific surface structure characterized by peak density and arithmetic mean curvature, combined with a manufacturing method involving hot-press molding using a double belt press device, ensuring a peel strength of 0.8 N/mm or more between the metal and insulating layers.
The solution provides a flexible metal-clad laminate with excellent adhesion and electrical properties, capable of handling high-frequency bands while maintaining sufficient peel resistance, suitable for harsh environments.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Flexible metal-clad laminate and manufacturing method thereof
[0001] The present invention relates to a flexible metal-clad laminate and a method for manufacturing the same.
[0002] In recent years, as electronic devices such as smartphones move to higher frequencies (5G), there has been an increasing demand for low-transmission-loss flexible printed wiring boards with higher frequencies. Furthermore, with the advent of the IoT society, electronic devices such as sensors are being incorporated into a variety of fields and locations, requiring improved environmental resistance. For example, millimeter waves, which are used in sensors and other devices, are highly stable against light, weather, and the environment, and are therefore used in millimeter-wave radar in automobiles and other applications. However, they are likely to be installed in harsher environments than conventional electronic devices, and therefore require improved environmental resistance for transmitters and receivers.
[0003] Liquid crystal polymer resins are known for their high heat resistance, low dielectric constant, and low dielectric loss tangent, and flexible printed wiring boards compatible with high-frequency bands, including an insulating layer made of liquid crystal polymer, have been actively used in recent years. Patent Document 1 discloses a method for continuously thermo-compressing a liquid crystal polymer while applying surface pressure using a double-belt press equipped with a pair of endless belts. The metal foil used in this process is copper-plated to a surface roughness Rz of 0.5 to 4.0 μm to ensure sufficient adhesion with the insulating layer, the liquid crystal polymer.
[0004] However, in the copper foil examples disclosed in Patent Document 1, even if the Rz is within the above range, sufficient peel strength is not obtained without copper plating treatment (Example 7, Table 1).
[0005] Patent No. 5411656
[0006] Therefore, the inventors have aimed to provide a flexible metal-clad laminate of liquid crystal polymer with excellent adhesion and electrical properties by examining the copper foil surface structure from the perspective of area analysis rather than line analysis for metal foil, particularly low-roughness copper foil, that can handle high-frequency bands associated with the shift to high-frequency (5G) electronic devices such as smartphones, and have also conducted intensive research into a method for producing the same.
[0007] The inventors performed a surface structure analysis of the copper foil surface and calculated the number of bumps (protrusions) per unit area of the copper foil surface (unit: mm -2 ) and the curvature (unit: mm -1 ) multiplied by a parameter: Spd × Spc (unit: mm -3 ) is related to adhesiveness (adhesion), and this led to the completion of the present invention. That is, the present invention provides the following inventions [1] to [5]. [1] A flexible metal-clad laminate comprising an insulating layer made of a liquid crystal polymer and a metal layer formed on one or both sides of the insulating layer, wherein the surface of the metal layer that overlaps with the insulating layer has a peak density Spd (mm -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) product Spd × Spc (mm -3 ) is 10 x 10 7 mm -3 [2] A flexible metal-clad laminate according to [1] above, wherein the metal layer is a copper foil. [3] A method for producing a flexible metal-clad laminate by thermocompression molding an insulating layer formed of a liquid crystal polymer and a metal layer on one or both sides of the insulating layer, wherein the peak density Spd (mm) of the surface of the metal layer that overlaps with the insulating layer is measured in accordance with ISO 25178-2:2021. -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) The product Spd × Spc is 10 × 10 7 mm-3 [4] The method for producing a flexible metal-clad laminate according to [3] above, wherein the heating temperature during the thermo-compression molding is equal to or higher than the melting point of the liquid crystal polymer in the insulating layer. [5] The method for producing a flexible metal-clad laminate according to [3] above, wherein the thermo-compression molding is performed using a double belt press, the pressure during the thermo-compression molding is in the range of 0.5 to 5.5 MPa, and the heating and pressurizing time is in the range of 70 to 280 seconds. [6] The method for producing a flexible metal-clad laminate according to [3] above or [4] above, wherein the metal layer is copper foil.
[0008] According to the present invention, a flexible metal-clad laminate of a liquid crystal polymer having excellent adhesive (cohesion) properties and electrical properties, and a method for producing the same can be provided.
[0009] 1 is a schematic diagram showing a schematic configuration of an example of a thermocompression bonding step in a manufacturing method for a flexible metal-clad laminate of the present invention.
[0010] Preferred embodiments of the present invention will now be described.
[0011] The flexible metal-clad laminate of the present invention is a flexible laminate comprising an insulating layer made of a liquid crystal polymer and a metal layer formed on one or both sides of the insulating layer, and the surface of the metal layer that overlaps the insulating layer has a peak density Spd (mm -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) product Spd × Spc (mm -3 ) is 10 x 10 7 mm -3 The present invention is characterized in that the peel strength between the metal layer and the insulating layer is 0.8 N / mm or more.
[0012] <Insulating Layer> In the flexible metal-clad laminate of the present invention, the insulating layer is formed of a liquid crystal polymer. The type of liquid crystal polymer is not particularly limited, and examples include liquid crystal polymers having ethylene terephthalate and parahydroxybenzoic acid as structural units, liquid crystal polymers having phenol, phthalic acid, and parahydroxybenzoic acid as structural units, and liquid crystal polymers having 6-hydroxy-2-naphthoic acid and parahydroxybenzoic acid as structural units. Liquid crystal polymers having 6-hydroxy-2-naphthoic acid and parahydroxybenzoic acid as structural units and liquid crystal polymers having 6-hydroxy-2-naphthoic acid and terephthalic acid as structural units are preferred. In the present invention, the insulating layer may be in either a film or sheet form. The difference between "film" and "sheet" in the present invention is based on the JIS "Packaging Terminology" standard, in which a film is defined as a "plastic film having a thickness of less than 250 μm" and a sheet is defined as a "thin plastic plate having a thickness of 250 μm or more." Methods for forming a film- or sheet-like insulating layer include the T-die method, inflation method, etc. Among these, the T-die method is preferred from the viewpoints of excellent flatness and less thickness unevenness.
[0013] The thickness of the insulating layer is not particularly limited, and is preferably in the range of, for example, 6 to 300 μm. When an insulating film is used, the thickness is preferably in the range of, for example, 6 μm or more and less than 250 μm, more preferably in the range of 12 to 150 μm, and even more preferably in the range of 25 to 100 μm.
[0014] <Metal Layer> The material of the metal layer constituting the flexible metal-clad laminate of the present invention is not particularly limited as long as it is a metal, and copper, copper alloy, aluminum, stainless steel, etc. are used. Copper and copper alloy are preferred, and copper is more preferred. The form of the metal layer is preferably a metal foil, which can be selected from metal foils of the above materials, and copper foil is particularly preferred.
[0015] In the present invention, the surface of the metal layer overlapping the insulating layer has a peak density Spd (mm-2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) product Spd × Spc (mm -3 ) is 10 x 10 7 mm -3 The above is required.
[0016] In the present invention, the "peak density Spd" of the metal layer is a parameter representing the number of peaks per unit area measured in accordance with ISO 25178-2:2021. 2 A large value indicates a large number of contact points with other objects. The peak density Spd is the number of peaks per unit area of a given measurement area (e.g., 100 μm) on the treated surface. 2 In the present invention, the peak density Spd can be calculated by measuring the surface profile of the surface of the surface (region) using a commercially available laser microscope. 2 The upper limit is preferably 600,000 or less.
[0017] Meanwhile, in the present invention, the "arithmetic mean curvature of peaks Spc" of a metal layer is a parameter that represents the arithmetic mean of the principal curvatures of peaks on the surface of the metal layer, measured in accordance with the above ISO. A small value indicates that the point of contact with another object is rounded. On the other hand, a large value indicates that the point of contact with another object is sharp. In short, the arithmetic mean curvature of peaks Spc can be said to be a parameter that represents the roundness of bumps, which can be measured with a laser microscope. The arithmetic mean curvature of peaks Spc is a parameter that represents the roundness of bumps over a predetermined measurement area (for example, 100 μm ) on the treated surface. 2 The arithmetic mean curvature Spc of the peaks can be calculated by measuring the surface profile of the surface (two-dimensional area) using a commercially available laser microscope. The arithmetic mean curvature Spc of the peaks is defined by the following formula:
[0018] In the present invention, the arithmetic mean curvature Spc of the peaks of the metal layer is 200 mm -1 More than 1000 mm is preferable. -1 More preferably, 3000 mm or more -1 More preferably, the upper limit is 6000 mm.-1 It is preferable that the arithmetic mean curvature Spc of the peak is 200 mm or less. -1 If the thickness is 6000 mm or more, the adhesion between the insulating layer and the liquid crystal polymer is good. -1 If the length is less than 6000 mm, it is possible to prevent powder falling due to the sharp tip breaking off. -1 If the thickness exceeds this value, the tip of the metal layer surface becomes too sharp and is prone to breaking and falling off, which may result in the failure to achieve the designed adhesion (adhesion) properties.
[0019] In the present invention, the surface of the metal layer overlapping the insulating layer has a peak density Spd (mm -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) product Spd × Spc (mm -3 ) as a parameter, 10 x 10 7 mm -3 That is, 100 million mm -3 It must be 80 x 10 or more. 7 mm -3 More preferably, it is 100×10 7 mm -3 More preferably, it is 200×10 7 mm -3 Preferably, it is 150×10 or less. 7 mm -3 It is more preferable that Spd×Spc (mm -3 ) is 10 x 10 7 mm -3 If the value is equal to or greater than this, it is possible to maintain a sufficiently high peel strength between the insulating layer and the metal layer while exhibiting excellent high-frequency characteristics. -3 ) is 150 x 10 7 mm -3 If the thickness is less than this, there is no risk that the tip of the metal layer surface will become excessively sharp, causing the tip to break off and fall off, preventing the designed adhesion (adhesion) from being achieved. Note that the "adhesion (adhesion) between the insulating layer and the metal layer" in this invention is based on the strength of the peel strength between the two layers, and is not based on the concept of adhesive strength based on the type of adhesion in the narrow sense, such as "adhesion by chemical bonding."
[0020] In the present invention, the surface roughness (ten-point average roughness) Rz of the metal layer on the surface overlapping the insulating layer is preferably in the range of 0.5 to 4.0 μm as defined in JIS B0601: 1994. A surface roughness Rz in this range is preferable from the viewpoint of ensuring a sufficiently high adhesiveness (adhesion) with respect to the peel strength between the insulating layer and the metal layer in combination with the other surface properties described above.
[0021] The flexible metal-clad laminate of the present invention has a metal layer on one or both sides of an insulating layer. That is, either of the layer structure of embodiment 1, which is metal layer / insulating layer / metal layer, and embodiment 2, which is two layers, which is metal layer / insulating layer, can be selected depending on the application.
[0022] The flexible metal-clad laminate of the present invention requires that the peel strength between the metal layer and the insulating layer be 0.8 N / mm or more. It is more preferably 1.0 N / mm or more, and even more preferably 1.2 N / mm or more. If the peel strength between the metal layer and the insulating layer is 0.8 N / mm or more, peel resistance can be ensured when the flexible metal-clad laminate is mounted on a substrate.
[0023] The method for producing a flexible metal-clad laminate of the present invention will be described below. The method for producing a flexible metal-clad laminate of the present invention is a method for producing a flexible metal-clad laminate by overlaying an insulating layer made of a liquid crystal polymer and a metal layer on one or both sides of the insulating layer and thermocompressing the laminate. The method is characterized in that the peak density Spd (mm ) of the metal layer on the surface overlapping the insulating layer is measured in accordance with ISO 25178-2:2021. -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) The product Spd × Spc is 10 × 10 7 (mm -3 ) or higher, and the heating temperature during the thermocompression molding is equal to or higher than the melting point of the insulating layer.
[0024] The liquid crystal polymer and metal layer forming the insulating layer used in the manufacturing method of the present invention are those already described. The "peak density Spd (mm)" measured by a specific method on the surface of the metal layer overlapping the insulating layer is -2 ) and "arithmetic mean curvature of the peak Spc (mm -1Regarding the product "Spd × Spc" of the above formulas, a material that satisfies the respective values already described is selected and used from the viewpoint of exhibiting excellent high-frequency characteristics while maintaining a sufficiently high peel strength between the insulating layer and the metal layer. In addition, the heating temperature during thermocompression molding must be equal to or higher than the melting point of the liquid crystal polymer of the insulating layer in order to improve the adhesion (adhesion) between the metal layer and the insulating layer and ensure sufficient peel strength. Preferably, the heating temperature is at least 5°C higher than the melting point and not higher than 30°C higher than the melting point. If the heating temperature is lower than the melting point, the peel strength between the metal layer and the insulating layer is weak, and there is a concern that the circuit may peel off when the flexible metal-clad laminate is processed into a flexible circuit board.
[0025] In the method for producing a flexible metal-clad laminate of the present invention, the method of thermo-pressing may be either a method using a thermo-press roll or a method using a double belt press device for thermo-pressing between endless belts, as long as the method ensures the adhesion (tightness) between the metal layer and the insulating layer and the functionality of the metal-clad laminate. However, it is particularly preferable to perform the thermo-pressing using a double belt press device, from the viewpoint of being able to ensure continuous heating and pressing time while suppressing misalignment between the metal layer and the insulating layer when they are overlapped.
[0026] In the case of embodiment 2, in which the thermocompression molding is performed using a double-belt press, a flexible metal-clad laminate having a metal layer on only one side of the insulating layer is produced. To prevent the steel belt from being transferred to the softened insulating layer (film) during the thermocompression molding process, a release film may be superimposed on the insulating layer (film) to produce a release film / insulating layer / metal layer structure. As the release film, a known release film used in the manufacture of flexible metal-clad laminates can be used. In particular, it is preferable to use a release film made of a flexible material with high heat resistance and good releasability, such as at least one material selected from non-thermocompression-bondable heat-resistant aromatic polyimides, fluororesins, and silicone resins. The release film is appropriately peeled off when the flexible metal-clad laminate is used. In addition, in Figure 1, the metal foil 12 on the upper side can be replaced with a release film (not shown), and after running it through the double belt press device 20, a recovery roll for recovering the release film can be separately provided in the winding section 40, and the release film can be peeled off from the flexible metal-clad laminate 10 at the time it is transported out of the double belt press device 20, and the flexible metal-clad laminate 10 and the release film can be recovered separately.
[0027] In the manufacturing method of the present invention, the pressure applied during thermocompression molding may be set as appropriate, but is preferably in the range of 0.5 to 5.5 MPa, more preferably 2.0 to 5.0 MPa, and even more preferably 3.0 to 4.5 MPa. Setting the pressure applied during thermocompression molding within these ranges allows high peel strength to be maintained. Furthermore, in the manufacturing method of the present invention, the heating and pressurizing time during thermocompression molding may be set as appropriate, but is preferably in the range of 70 to 280 seconds, more preferably 80 to 240 seconds, and even more preferably 90 to 180 seconds. Within these ranges, the dimensional stability of the insulating layer can be improved.
[0028] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0029] The following materials were prepared and used in the Examples and Comparative Examples: Liquid crystal polymer film for insulating layer: AXSORDER liquid crystal polymer (LCP) film manufactured by Denka Co., Ltd., thickness 50 μm, melting point 280° C. Copper foil was used as the metal layer, and the type, thickness, surface roughness, and peak density Spd (mm -2 ), arithmetic mean curvature of the peak Spc (mm -1 ), and Spd × Spc (10 7 mm -3 The manufacturer, grade, type and thickness of the copper foil used as the metal layer in the examples and comparative examples are shown in Table 1.
[0030]
[0031] The surface characteristics of the copper foil used as the metal layer were evaluated using the method described below. Surface analysis (peak density Spd and arithmetic mean curvature Spc) of the matte copper foil surface (surface overlapping the insulating layer) was performed using a laser microscope (Keyence Corporation, Model VK-X210) at four arbitrary points on a copper foil cut to A4 size. Measurements were performed in accordance with ISO 25178-2:2021 using an S filter of 1 μm, F-operation surface tilt correction automatic, and an L filter of 0.1 mm. The values used in Table 2 are the average values of the four measured points. Surface roughness (ten-point average roughness) Rz of the matte copper foil surface was measured using the catalog value published by the copper foil manufacturer.
[0032] The peel strength, which represents the adhesiveness (adhesion) required for the flexible metal (copper)-clad laminates obtained in the Examples and Comparative Examples, was measured and evaluated by the method described below. Peel Strength: In accordance with JIS C6471:1995, the peel strength in the normal state was measured by Method A, i.e., a method of peeling in a 90° direction. The conductor width of the test piece was 3 mm. A peel strength of 0.8 N / mm or more was evaluated as good.
[0033] Example 1 Using a double belt press device 20 having the configuration shown in FIG. 1 , a liquid crystal polymer film 11 [AXSORDER (thickness 50 μm) manufactured by Denka Co., Ltd.] was used as the insulating film roll 31 suspended on the unwinding section 30, and an electrolytic copper foil (TQ-M7-VSP, thickness 12 μm) manufactured by Mitsui Mining & Smelting Co., Ltd. was used as the metal layer roll 32, with a surface roughness Rz of 1.2 μm and a peak density Spd of 368959 / mm 2 The arithmetic mean curvature Spc of the peak is 3391 mm -1 , Spd × Spc is 125 (× 10 7 mm -3 The resulting three-layer structure was fed into a double-belt press 20, sandwiched between an endless belt 23 stretched between upper drums 21 and 21 and an endless belt 24 stretched between lower drums 22 and 22, and then passed through the upper and lower zones of a heat press 25. The laminate was then subjected to heat press molding (lamination) at a maximum temperature of 295°C (15°C higher than the melting point of the liquid crystal film), a pressure of 4.0 MPa, and a press time of 124 seconds to produce a flexible copper-clad laminate 10, which was then wound into a roll by a winding section 40. The resulting flexible copper-clad laminate 10 had a three-layer structure, with metal layers made of copper foils 12, 12 laminated on top and bottom of an insulating layer made of a liquid crystal polymer film 11. The peel strength was evaluated using the method described above and found to be 1.10 (N / mm). The configurations of the insulating and metal layers, the heat press molding (lamination) conditions, and the evaluation results are summarized in Table 2.
[0034] (Examples 2 to 10, Comparative Examples 1 and 2) Copper foils with the manufacturer names and grade names shown in Table 1 were used for the metal layer in Examples 2 to 10 and Comparative Examples 1 and 2, and flexible copper-clad laminates were produced in the same manner as in Example 1, except that the maximum temperature of the thermocompression molding conditions was changed in Example 9 and Comparative Example 2. The configurations of the insulating layer and metal layer, the thermocompression molding (lamination) conditions, and the evaluation results are summarized in Table 2.
[0035]
[0036] As can be seen from Table 2, in Examples 1 to 10, high peel strength values of 0.82 to 1.28 N / mm were obtained. In contrast, when "Spd x Spc" was 2 x 10 7 mm -3 Comparative Example 1 exhibited a low peel strength of 0.44 N / mm, and Comparative Example 2, in which the maximum temperature under heat and pressure conditions was 5°C lower than the melting point of the liquid crystal polymer, 280°C, exhibited a low peel strength of 0.47 N / mm. Thus, it was demonstrated that the present invention can provide a flexible copper-clad laminate having excellent adhesion (tightness) between the insulating layer and the metal layer.
[0037] The flexible metal-clad laminate of the present invention has a high peel strength between the metal layer and the insulating layer of 0.8 N / mm or more, and therefore can be used to make flexible printed wiring boards that are compatible with high frequency bands. Furthermore, the method for producing a flexible metal-clad laminate of the present invention can be used as a method for producing the flexible metal-clad laminate in a stable, reproducible, and economical manner.
[0038] 10: Flexible metal-clad laminate (flexible copper-clad laminate) 11: Liquid crystal polymer film 12: Metal foil (copper foil) 20: Double belt press device 21: Upper drum 22: Lower drum 23, 24: Endless belts 25: Heat pressing (molding) device 30: Pay-out section 31: Insulating film roll 32: Metal layer roll 40: Winding section
Claims
1. A flexible metal-clad laminate comprising an insulating layer made of a liquid crystal polymer and a metal layer formed on one or both sides of the insulating layer, wherein the surface of the metal layer overlapping the insulating layer has a peak density Spd (mm -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) product Spd × Spc (mm -3 ) is 10 x 10 7 mm -3 or more, and the peel strength between the metal layer and the insulating layer measured by Method A in accordance with JIS C6471:1995 is 0.8 N / mm or more.
2. The flexible metal clad laminate of claim 1, wherein said metal layer is copper foil.
3. A method for producing a flexible metal-clad laminate comprising: an insulating layer formed of a liquid crystal polymer; and a metal layer on one or both sides of the insulating layer, and then thermocompressing the insulating layer; wherein the peak density Spd (mm -2 ) and the arithmetic mean curvature of the peak Spc (mm -1 ) The product Spd × Spc is 10 × 10 7 mm -3 the heating temperature during the thermocompression molding is equal to or higher than the melting point of the liquid crystal polymer of the insulating layer.
4. The method for producing a flexible metal-clad laminate according to claim 3, wherein the thermo-compression molding is performed using a double belt press device, the pressure during the thermo-compression molding is in the range of 0.5 to 5.5 MPa, and the heating and pressurizing time is in the range of 70 to 280 seconds.
5. The method for producing a flexible metal-clad laminate according to claim 3 or 4, wherein the metal layer is a copper foil.
Citation Information
Patent Citations
Metal clad laminated plate and method for manufacturing metal clad laminated plate
WO2020090688A1
Surface-treated copper foil, carrier-attached copper foil, copper-clad laminate, and printed wiring board
WO2020105289A1
Double-sided metal-clad laminate and production method therefor, insulating film, and electronic circuit base board
WO2020153391A1