Laminate and sanitary article including said laminate

The laminate, composed of a nonwoven fabric and polyurethane resin layers, addresses the balance of waterproofness and breathability in disposable diapers, enhancing comfort and fit while reducing material usage and environmental impact.

WO2024219309A1PCT designated stage expired Publication Date: 2024-10-24NITTO DENKO CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014587
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-10
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Disposable diapers face challenges in achieving a balance between waterproofness and breathability, leading to discomfort and potential skin issues, while also requiring elastic properties to fit various body types and reduce material usage.

Method used

A laminate comprising a nonwoven fabric layer and a polyurethane resin layer with specific thickness and adhesive configurations, providing excellent waterproofness, breathability, and elastic recovery properties, which is suitable for use in disposable diapers.

Benefits of technology

The laminate enhances the comfort and fit of disposable diapers by ensuring excellent waterproofness and breathability while reducing material usage and environmental impact, accommodating a wider range of body types with fewer sizes and improving tactile sensation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014587_24102024_PF_FP_ABST
    Figure JP2024014587_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a laminate that has excellent waterproofness and air permeability and also has excellent expansion / contraction recovery properties. A laminate according to an embodiment of the present invention comprises: a nonwoven fabric layer of fibers; and a polyurethane resin layer having a thickness of 5-15 μm. A sanitary article according to an embodiment of the present invention includes said laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and sanitary product containing said laminate

[0001] The present invention relates to a laminate and to a sanitary article comprising said laminate.

[0002] Disposable diapers are used not only by infants but also by adults, and demand for them is increasing. Disposable diapers are required to prevent leakage of body waste and to provide a comfortable wearing experience. To prevent leakage, openings around the legs and waist must fit the body well. Furthermore, highly waterproof materials are used for the components that make up disposable diapers. On the other hand, if a diaper is only highly waterproof, the inside may become damp, causing rashes and itching in the wearer, or may produce a foul odor. Therefore, materials that are both waterproof and breathable are used for disposable diapers (see, for example, Patent Document 1). On the other hand, materials that are both waterproof and breathable can result in disposable diapers that are unpleasant to the touch and feel like paper. Disposable diapers that are not only waterproof and breathable but also pleasant to the touch and have an excellent feel are desired.

[0003] JP 2023-44181 A

[0004] The present invention has been made to solve the above-mentioned problems of the prior art, and an object of the present invention is to provide a laminate having excellent waterproofness and breathability, as well as excellent stretch recovery properties.

[0005] 1. A laminate according to an embodiment of the present invention comprises a fibrous nonwoven fabric layer and a polyurethane resin layer having a thickness of 5 μm or more and 15 μm or less. 2. The water vapor permeability of the laminate described in 1 above is 1500 g / (m 23. The laminate according to 1 or 2 above may be stretched 100% under conditions of a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 300 mm / min, fixed in the stretched state and held for 1 minute, and then released from the stretched state. The coefficient of variation (%) calculated from the initial chuck distance (A) (mm) and the length of the laminate after the test (B) (mm) = [{(B) - (A)} / (A)] x 100 may be 10% or less. 4. In the laminate according to any one of 1 to 3 above, the nonwoven fabric layer may be a nonwoven fabric that stretches 50% or more in the CD direction. 5. The laminate according to any one of 1 to 4 above may be a laminate obtained by extrusion laminating the nonwoven fabric layer and the polyurethane resin layer. 6. The laminate according to any one of 1 to 4 above may be a laminate obtained by laminating the nonwoven fabric layer and the polyurethane resin layer via a pressure-sensitive adhesive layer. 7. In the laminate described in 6 above, the pressure-sensitive adhesive layer may be a layer formed on the entire surface of at least one of the nonwoven fabric layer or the polyurethane resin layer. 8. In the laminate described in 6 above, the pressure-sensitive adhesive layer may be a layer formed intermittently on the surface of at least one of the nonwoven fabric layer or the polyurethane resin layer. 9. In the laminate described in any one of 1 to 8 above, the nonwoven fabric layer may be a nonwoven fabric of olefin-based fibers. 10. In another aspect of the present invention, a sanitary product is provided. This sanitary product includes the laminate described in any one of 1 to 9 above.

[0006] According to an embodiment of the present invention, a laminate having excellent waterproofness and breathability, as well as excellent stretch recovery, can be provided.

[0007] 1 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention.

[0008] A. Overall Structure of the Laminate FIG. 1 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention. The laminate 100 according to an embodiment of the present invention includes a polyurethane resin layer 10 and a fibrous nonwoven fabric layer (hereinafter also referred to as the nonwoven fabric layer) 20. The thickness of the polyurethane resin layer is 5 μm or more and 15 μm or less. In the illustrated example, the nonwoven fabric layer is laminated on only one side of the polyurethane resin layer, but nonwoven fabric layers may be laminated on both sides of the polyurethane resin layer. Components used in sanitary products such as disposable diapers, particularly components used for backsheets, are required to be waterproof and breathable. However, laminates with excellent waterproofness and breathability may have a poor feel and may not provide a satisfactory tactile sensation. The laminate according to an embodiment of the present invention includes a polyurethane resin layer with a thickness of 5 μm or more and 15 μm or less and a nonwoven fabric layer. A laminate having a thin polyurethane resin layer as described above not only has excellent waterproofness and breathability, but also excellent stretch recovery. When the laminate of the embodiment of the present invention is applied to, for example, a disposable diaper, it can provide not only excellent waterproofness and breathability, but also a comfortable fit to the body and suppress leakage around the legs and waist. Furthermore, the disposable diaper can have a pleasant feel and improved tactile sensation. Because disposable diapers are required to fit the body well, they are available in a wide range of sizes, which can require a large amount of storage space in retail stores, hospitals, nurseries, kindergartens, etc. By using the laminate of the embodiment of the present invention, the stretchability of the disposable diaper can be improved, allowing it to suit a wide range of body types even with a limited number of sizes. Furthermore, the polyurethane resin layer used in the laminate is thin, allowing for a reduction in the amount of plastic material used in the laminate and the size of the disposable diaper itself using the laminate. As a result, the amount of plastic used can be reduced, contributing to a reduction in environmental impact.

[0009] The polyurethane resin layer 10 and the nonwoven fabric layer 20 may be laminated directly, i.e., without any adhesive layer, or may be laminated via any appropriate adhesive layer (not shown). The adhesive layer may be an adhesive layer or a pressure-sensitive adhesive layer. The adhesive layer is preferably a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer may be formed on the entire surface of at least one of the polyurethane resin layer 10 and the nonwoven fabric layer 20, or may be formed intermittently, for example, in a striped or dotted pattern. Preferably, the polyurethane resin layer 10 and the nonwoven fabric layer 20 are laminated directly. A directly laminated laminate can further improve breathability.

[0010] The laminate preferably has a water vapor permeability of 1500 g / (m 2 ·day) or more, and more preferably 1800 g / (m 2 ·day) or more, and more preferably 2000 g / (m 2 ·day) or more, and particularly preferably 2500 g / (m 2 -day) or more. If the water vapor permeability is within the above range, a laminate with excellent breathability can be obtained. The higher the water vapor permeability, the more preferable. In this specification, the water vapor permeability of the laminate refers to a value measured using an 8 mm x 8 mm sample in accordance with ISO 15106-1 under conditions of a temperature of 23°C and a humidity of 100% RH.

[0011] The laminate was stretched 100% under conditions of a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 300 mm / min, fixed in the stretched state and held for 1 minute, and then released from the stretched state. The coefficient of variation (%) calculated from the initial chuck distance (A) (mm) and the length of the laminate after the test (B) (mm) = [{(B) - (A)} / (A)] x 100 (hereinafter also referred to as stretch recovery) is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, and particularly preferably 5% or less. A stretch recovery within the above range can provide excellent stretch recovery. The coefficient of variation is, for example, 2% or more.

[0012] The laminate may be decorated with any suitable decoration. For example, the polyurethane resin layer and / or the nonwoven fabric layer may be colored, or may have any suitable printed portion.

[0013] B. Polyurethane Resin Layer The polyurethane resin layer is a layer having a thickness of 5 μm or more and 15 μm or less. When the thickness of the polyurethane resin layer is within the above range, a laminate can be obtained that not only has excellent waterproofness and breathability, but also has excellent stretch recovery. Furthermore, even when the thickness is within the above range, the polyurethane resin layer has excellent strength and can prevent the laminate from breaking even when stretched. A polyurethane resin layer having a thickness exceeding 15 μm can reduce breathability and deteriorate the tactile feel. This can also lead to increased material costs and increased environmental impact due to the increased use of materials (e.g., plastic materials). The thickness of the polyurethane resin layer is preferably 5 μm to 12 μm, more preferably 5 μm to 10 μm. In one embodiment, the thickness of the polyurethane resin layer is 5 μm or more. Furthermore, the thickness of the polyurethane resin layer is 15 μm or less, preferably 12 μm or less, more preferably 10 μm or less. The polyurethane resin layer may be a single layer or a laminate of two or more layers.

[0014] B-1. Polyurethane Resin Any appropriate polyurethane resin can be used. Polyurethane has a soft segment phase and a hard segment phase. The soft segment phase is formed from a high-molecular-weight polyol compound, and the hard segment phase can be formed by the reaction of a low-molecular-weight diol compound and an organic diisocyanate compound.

[0015] The high molecular weight polyol compound is, for example, a diol compound having a weight-average molecular weight of 500 to 6000. Any appropriate diol can be used as the high molecular weight polyol compound. Examples include polyester diols, polyether diols, polycarbonate diols, and co-condensates thereof (e.g., polyester ether diols). High molecular weight polyol compounds can be obtained, for example, by addition polymerization of alkylene oxides such as propylene oxide and ethylene oxide with low molecular weight compounds having two or more hydroxyl groups in the molecule, such as glycol and glycerin, or by condensation of dibasic acids such as adipic acid with polyhydric alcohols such as ethylene glycol. The high molecular weight polyol compound may be one type or two or more types.

[0016] As the polyester diol, any appropriate polyester diol can be used, preferably a saturated polyester diol obtained from a diol compound of an alkane having 2 to 10 carbon atoms, such as propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, or 2-methylpropanediol, and an aliphatic or aromatic dicarboxylic acid having 4 to 12 carbon atoms, such as glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, terephthalic acid, or isophthalic acid; or a polylactone diol, such as polycaprolactone glycol or polyvalerolactone glycol.

[0017] As the polyether diol, any suitable polyether diol can be used, and preferably, a polyalkylene ether diol such as polyethylene ether glycol, polypropylene ether glycol, polytetramethylene ether glycol, or polyhexamethylene ether glycol is used.

[0018] The low-molecular-weight diol compound is, for example, a diol compound having a weight-average molecular weight of less than 500. Any appropriate diol compound can be used as the low-molecular-weight diol compound. Examples include aliphatic or aromatic diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentane glycol, 3-methylpentane glycol, 1,6-hexanediol, and 1,4-bishydroxyethylbenzene. Only one type of low-molecular-weight diol compound may be used, or two or more types may be used in combination.

[0019] Any appropriate diisocyanate compound can be used as the organic diisocyanate compound. Examples include aliphatic or aromatic diisocyanate compounds such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, xylylene diisocyanate, 2,6-diisocyanate methyl caproate, and hexamethylene diisocyanate. Only one organic diisocyanate compound may be used, or two or more organic diisocyanate compounds may be used in combination.

[0020] Any suitable additive may be further used in the polymerization of the polyurethane resin. Examples include hindered phenol and amine antioxidants, benzotriazole and hindered amine UV absorbers, smoothing agents such as amide wax and montanic acid wax, hydrolysis inhibitors such as carbodiimide compounds, pigments such as titanium oxide and red iron oxide, and polymer additives such as gas yellowing inhibitors. These additives may be used alone or in combination of two or more.

[0021] The polyurethane resin can be obtained by polymerizing the high-molecular-weight polyol compound, the low-molecular-weight diol compound, and the organic diisocyanate compound, and optionally other suitable monomer components and additives, by any suitable method, such as continuous melt polymerization, kneader polymerization, vat curing, or belt polymerization.

[0022] As the polyurethane resin, commercially available products may be used, for example, trade names "Elastollan E SP806," "Elastollan E 1170 A," and "Elastollan E 1385 A" manufactured by BASF.

[0023] B-2. Filler The polyurethane resin layer may further contain a filler. If the polyurethane resin layer further contains a filler, the breathability of the laminate may be further improved. Any appropriate filler may be used. Specific examples include inorganic particles and organic particles. Examples of inorganic particles include talc, titanium oxide, calcium oxide, magnesium oxide, zinc oxide, calcium carbonate, silica, clay, mica, barium sulfate, whiskers, magnesium hydroxide, etc. Examples of organic particles include acrylic beads, styrene beads, silicone resin particles, etc. One type of filler may be used alone, or two or more types may be used in combination.

[0024] The average particle size of the filler may be any appropriate average particle size. The average particle size of the filler is preferably 0.5 μm or more, more preferably 0.6 μm or more, and even more preferably 0.7 μm or more. The average particle size of the filler is preferably 50 μm or less, more preferably 30 μm or less, even more preferably 10 μm or less, and particularly preferably 5 μm or less. In one embodiment, the average particle size of the filler is preferably 0.5 μm to 50 μm, more preferably 0.6 μm to 30 μm, even more preferably 0.7 μm to 10 μm, and particularly preferably 0.7 μm to 5 μm. When the average particle size of the filler is within the above range, the breathability of the laminate can be further improved.

[0025] The filler can be used in any appropriate content. The filler content is preferably 50 parts by weight or more, more preferably 70 parts by weight or more, and even more preferably 100 parts by weight or more, relative to 100 parts by weight of the polyurethane resin contained in the composition forming the polyurethane resin layer. The filler content is preferably 400 parts by weight or less, more preferably 350 parts by weight or less, and even more preferably 300 parts by weight or less. In one embodiment, the filler content is preferably 50 parts by weight to 400 parts by weight, more preferably 70 parts by weight to 350 parts by weight, and even more preferably 100 parts by weight to 300 parts by weight, relative to 100 parts by weight of the polyurethane resin. When the filler content is within the above range, the breathability of the laminate can be further improved.

[0026] The filler may be coated with a release agent. Any suitable release agent may be used. Examples of the release agent include fatty acid amide-based release agents, silicone-based release agents, fluorine-based release agents, and long-chain alkyl-based release agents. The release agent may be used in any suitable amount.

[0027] B-3. ​​Other Additives The polyurethane resin layer may further contain any appropriate other additives. Examples of the other additives include ultraviolet absorbers, heat stabilizers, release agents, lubricants, colorants such as dyes, antioxidants, anti-emulsion agents, anti-blocking agents, foaming agents, other polymers, tackifiers, plasticizers, anti-degradants, antistatic agents, and light stabilizers. Only one type of other additive may be used, or two or more types may be used in combination. The other additives are used in any appropriate content.

[0028] In one embodiment, a commercially available polyurethane film may be used as the polyurethane resin layer. Examples include "SMF-10" manufactured by Seiren Co., Ltd. and "TX2060" manufactured by Argotec. Furthermore, examples of commercially available products in which a pressure-sensitive adhesive is laminated on a polyurethane resin layer include "Permirollite" manufactured by Nitto Denko Corporation.

[0029] C. Fiber Nonwoven Fabric Layer Any suitable nonwoven fabric can be used as the fiber nonwoven fabric layer. The nonwoven fabric layer may be a single nonwoven fabric layer or a laminate of two or more nonwoven fabrics. The nonwoven fabric is preferably a nonwoven fabric that can stretch by 50% or more in the CD direction. That is, the machine direction during the manufacture of the nonwoven fabric is the MD direction, and the direction perpendicular to the MD direction is the CD direction. A nonwoven fabric is cut into a length of 50 mm in the longitudinal direction and used as a sample. The sample is set in a tensile tester (e.g., Shimadzu Corporation, product name "AG-20kNG") with a chuck distance of 50 mm and stretched in the CD direction at a tensile speed of 300 mm / min under the condition of 100% elongation. When the value calculated from the formula (CD length of nonwoven fabric after stretching (mm) - CD length of nonwoven fabric before stretching (mm)) / CD length of nonwoven fabric before stretching (mm) x 100(%) is 50%, the nonwoven fabric exhibits a strength of 10 N / 50 mm or less. If the strength of the nonwoven fabric when stretched 50% in the CD direction is 10 N / 50 mm or less, the nonwoven fabric layer can follow the stretch recovery of the polyurethane resin layer, and the stretch recovery of the laminate can be improved.

[0030] Examples of fibrous nonwoven fabrics include spunbond nonwoven fabrics, thermalbond nonwoven fabrics, pointbond nonwoven fabrics, air-through nonwoven fabrics, meltblown nonwoven fabrics, spunlace nonwoven fabrics, spunbond-meltblown spunbond nonwoven fabrics, spunbond-meltblown-meltblown spunbond nonwoven fabrics, non-bonded nonwoven fabrics, electrospun nonwoven fabrics, carded nonwoven fabrics, etc. Preferred are nonwoven fabrics that can be stretched in the CD direction, such as spunlace nonwoven fabrics, air-through nonwoven fabrics, meltblown nonwoven fabrics, and carded nonwoven fabrics.

[0031] Any suitable fibers can be used as the fibers constituting the nonwoven fabric. Examples include fibers of olefins such as polypropylene and polyethylene, polyester, polyamide, polyurethane, elastomer, rayon, cellulose, acrylic, copolymers thereof, or mixtures thereof. Olefin-based fibers are preferred, and polypropylene fibers and polyethylene fibers are preferred from the standpoint of cost. Core-sheath fibers made of polyester and olefin resin may also be used.

[0032] Examples of olefin-based fibers include polypropylene fibers, polyethylene fibers, α-olefin copolymer fibers, etc. Preferred olefin-based fibers are polypropylene fibers and polyethylene fibers.

[0033] The fibers constituting the nonwoven fabric may further contain any appropriate other components. Examples of the other components include other polymers, tackifiers, plasticizers, antidegradants, pigments, dyes, antioxidants, antistatic agents, lubricants, foaming agents, heat stabilizers, light stabilizers, inorganic fillers, and organic fillers. The other components may be used alone or in combination of two or more. The content ratio of the other components in the fibers constituting the nonwoven fabric may be set to any appropriate amount.

[0034] The density of the nonwoven fabric can be set to any appropriate value. The density of the nonwoven fabric is preferably 0.90 kg / m 3 ~0.99 kg / m 3 and more preferably 0.92 kg / m 3 ~0.98 kg / m 3 and more preferably 0.93 kg / m 3 ~0.98 kg / m 3 In one embodiment, the density of the nonwoven fabric is preferably 0.90 kg / m 3 More preferably, it is 0.92 kg / m or more. 3 More preferably, it is 0.93 kg / m or more. 3 The density of the nonwoven fabric is preferably 0.99 kg / m 3 More preferably, it is 0.98 kg / m or less. 3 If the density of the nonwoven fabric is within the above range, a laminate having an excellent feel to the touch can be provided. In this specification, the density of the nonwoven fabric (kg / m 3 ) is the basis weight of the nonwoven fabric (X g / m 2 ) and the thickness (Y mm) of the nonwoven fabric measured by the following method. 3 ) is X / Y (kg / m 3) <Thickness of nonwoven fabric> Using a digital microscope (for example, Keyence Corporation, product name "VHX-1000"), the cross section of the nonwoven fabric is photographed at 100x magnification, and the thickness of the nonwoven fabric is measured using the image analysis software of the same microscope. In measuring the thickness, parallel lines at the top and bottom of the nonwoven fabric cross section, which intersect with the fibers at 10 points, are defined as the upper and lower sides, respectively, and the length between the upper and lower sides is defined as the thickness of the nonwoven fabric.

[0035] The basis weight of the nonwoven fabric is preferably 0.15 g / m 2 ~0.40g / m 2 and more preferably 0.15 g / m 2 ~0.35g / m 2 and more preferably 0.15 g / m 2 ~0.30g / m 2 In one embodiment, the basis weight of the nonwoven fabric is preferably 0.15 g / m 2 The basis weight of the nonwoven fabric is preferably 0.40 g / m 2 More preferably, it is 0.35 g / m or less. 2 More preferably, it is 0.30 g / m or less. 2 If the basis weight of the nonwoven fabric is within the above range, the feel of the laminate can be further improved. The basis weight of the nonwoven fabric can be measured by any appropriate method. For example, it can be measured by the following method. 2 The weight of the sample cut into pieces was measured using an electronic balance, and the weight was calculated using the following formula: g / m 2 The basis weight of the nonwoven fabric can be measured by converting it into units (gsm).

[0036] D. Manufacturing Method of Laminate The laminate of the embodiment of the present invention can be manufactured by any appropriate method. For example, it can be manufactured by preparing a resin film that will become the polyurethane resin layer and laminating it to a fibrous nonwoven fabric layer by any appropriate method. When laminating the resin film that will become the polyurethane resin layer and the nonwoven fabric, for example, they can be laminated via a pressure-sensitive adhesive layer. Any appropriate pressure-sensitive adhesive can be used to form the pressure-sensitive adhesive layer. Examples include acrylic pressure-sensitive adhesives and hot-melt pressure-sensitive adhesives. The pressure-sensitive adhesive can be formed on the surface (one side surface) of at least one of the resin film and the nonwoven fabric. The pressure-sensitive adhesive layer may be formed over the entire surface of the resin film or nonwoven fabric on which the pressure-sensitive adhesive layer is to be formed, or it may be formed intermittently, for example, in a striped or dotted pattern. Preferably, the pressure-sensitive adhesive layer is an intermittent layer. If the pressure-sensitive adhesive layer is an intermittent layer, the breathability of the resulting laminate can be improved.

[0037] The adhesive layer can be formed by applying the adhesive by any suitable method, for example, by solidly applying the adhesive to the resin film or nonwoven fabric, or by intermittently applying the adhesive by spray coating.

[0038] The laminate may be produced by extruding the composition forming the polyurethane resin layer directly onto a fibrous nonwoven fabric through the die of an extruder and then extrusion laminating the extrusion. Production by extrusion lamination can further improve the breathability of the laminate. Furthermore, the process from composition preparation to laminate production can be carried out continuously, thereby improving production efficiency. More specifically, a method can be used in which the composition forming the polyurethane resin layer is extruded through a T-die of an extruder and a laminate of the nonwoven fabric and the polyurethane resin layer is formed. The extrusion temperature of the composition forming the polyurethane resin layer is preferably 180°C to 250°C, more preferably 180°C to 230°C, and even more preferably 200°C to 230°C. In one embodiment, the extrusion temperature is preferably 180°C or higher, more preferably 200°C or higher. Furthermore, the extrusion temperature is preferably 250°C or lower, more preferably 230°C or lower. When performing direct extrusion lamination with the nonwoven fabric, the adhesion of the laminate can be further improved within the above range.

[0039] The laminate of the embodiment of the present invention can have high breathability without undergoing a pre-stretching process. For example, a laminate including a resin layer formed from an olefin-based resin can have improved breathability by pre-stretching the resin layer. On the other hand, the strength of the resin layer that has undergone pre-stretching can be reduced, which can reduce the handleability of the resin layer in the laminate manufacturing process after pre-stretching. In the laminate of the embodiment of the present invention, the polyurethane resin layer can exhibit excellent breathability and strength even without pre-stretching. Therefore, manufacturing processes such as pre-stretching can be omitted, improving manufacturing efficiency. Furthermore, a laminate having excellent waterproofness and breathability can be manufactured without reducing yield. Furthermore, when used in, for example, disposable diapers, the laminate can be prevented from breaking when stretched during wear, etc.

[0040] E. Uses of the Laminate The laminate of the embodiment of the present invention can be used in any appropriate application. In one embodiment, the laminate of the embodiment of the present invention can be suitably used in a sanitary product. Examples of sanitary products include disposable diapers. Disposable diapers typically include a topsheet that contacts the wearer's body, a backsheet that is on the outside of the disposable diaper, and an absorbent disposed between the topsheet and the backsheet. The laminate of the embodiment of the present invention is preferably used in a backsheet. As described above, the laminate of the embodiment of the present invention has excellent waterproofness and breathability, and can also have excellent stretch recovery. Using the laminate of the embodiment of the present invention as a backsheet can prevent leakage of excrement and provide a disposable diaper that fits the wearer better. Furthermore, the tactile feel of the disposable diaper can be improved, providing a disposable diaper that is more comfortable to the touch. Furthermore, a disposable diaper with excellent stretch recovery and that can fit a wider range of body types can be provided. As a result, a smaller number of sizes can accommodate a wider range of body types, thereby enabling space savings during storage.

[0041] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0042] [Example 1] A polyurethane film with an adhesive layer (manufactured by Nitto Denko Corporation, trade name "Permilorlite", urethane film thickness 8 μm, adhesive layer thickness 25 μm) and a carded type nonwoven fabric of propylene (PP) resin fiber (manufactured by Nitto Denko Corporation, trade name "ThermoStrain 22 HI", basis weight 22 g / m) were used. 2 ) was attached to the adhesive layer of the polyurethane film with an adhesive layer therebetween using a hand roller to obtain a laminate.

[0043] [Example 2] Pellets of urethane resin A (manufactured by BASF, trade name "Elastollan E SP806") were thoroughly dried, and an 8 μm-thick polyurethane resin layer was melt-extruded using an extruder. The extruded PP resin fiber was then fed out into a carded-type nonwoven fabric (manufactured by Nitto Denko Corporation, trade name "Thermotrain 22 HI", basis weight 22 g / m). 2 The polyurethane resin layer immediately after extrusion was brought into contact with the laminated sheet, and extrusion lamination was carried out to obtain a laminate.

[0044] Example 3 A laminate was obtained in the same manner as in Example 2, except that the thickness of the polyurethane resin layer was 15 μm.

[0045] Example 4 A laminate was obtained in the same manner as in Example 2, except that the urethane resin A was replaced with a polyurethane resin B (manufactured by BASF under the trade name "Elastollan E 1385A").

[0046] [Example 5] Carded type nonwoven fabric of PP resin fiber (manufactured by Nitto Denko Corporation, product name "Thermotrain 22 HI", basis weight 22 g / m 2 ) and a hot melt adhesive (manufactured by Nitto Denko Corporation, product name "olefin hot melt adhesive AC600") was applied at a rate of 8 g / m 2 A laminate was obtained in the same manner as in Example 4, except that the hot-melt adhesive was spray-coated so as to form a polyurethane resin layer on the surface on which the hot-melt adhesive had been spray-coated.

[0047] (Comparative Example 1) Linear low-density polyethylene (manufactured by Prime Polymer Co., Ltd., trade name "Ultzex ​​2022L", density 0.919 g / cm 3A mixture of 63 parts by weight of ethylene-propylene terpolymer (manufactured by Mitsui Chemicals, Inc., trade name "K-9720"), 77 parts by weight of ethylene-propylene terpolymer (manufactured by Mitsui Chemicals, Inc., trade name "K-9720"), and 210 parts by weight of calcium carbonate was fed into an extruder. The mixture was then melt-extruded from a T-die and stretched in the machine direction (MD) at a stretching temperature of 60°C and a stretch ratio of 2 by a uniaxial roll stretching method to obtain a porous film with a thickness of 20 μm. A carded type nonwoven fabric of propylene (PP) resin fiber (manufactured by Nitto Denko Corporation, trade name "ThermoStrain 22 HI", basis weight 22 g / m) was also prepared. 2 ) on one side of which a hot melt adhesive (manufactured by Nitto Denko Corporation, product name "olefin hot melt adhesive AC600") was applied at a coating amount of 8 g / m 2 The surface of the nonwoven fabric on which the hot melt adhesive had been spray coated was then spray laminated with the porous film to obtain a laminate.

[0048] (Comparative Example 2) Metallocene polypropylene elastomer (manufactured by ExxonMobil Corporation, trade name "Vistamax 7010", density 0.861 g / cm 3 A mixture of 140 parts by weight of cellulose acetate (melt flow rate (MFR) 3 g / 10 min), 200 parts by weight of calcium carbonate (average particle size 1.1 μm), 1 part by weight of stearic acid, and 1 part by weight of antioxidant was fed into an extruder. Next, melt extrusion was carried out from a T-die, and the mixture was stretched in the longitudinal (MD) direction by a uniaxial roll stretching method at a stretching temperature of 60 ° C. and a stretching ratio of 2 to obtain a porous film having a thickness of 50 μm. A laminate was obtained in the same manner as in Comparative Example 1, except that the obtained porous film was used.

[0049] Comparative Example 3 A laminate was obtained in the same manner as in Comparative Example 2, except that the thickness of the porous film was 15 μm.

[0050] (Comparative Example 4) Metallocene polypropylene elastomer (manufactured by ExxonMobil Corporation, trade name "Vistamax 7010", density 0.861 g / cm 3A mixture of 140 parts by weight of cellulose acetate (with a MFR of 3 g / 10 min), 1 part by weight of stearic acid, and 1 part by weight of an antioxidant was fed into an extruder. The mixture was then melt-extruded through a T-die and stretched in the machine direction (MD) at a stretching temperature of 60°C and a stretching ratio of 2 by a uniaxial roll stretching method to obtain a porous film having a thickness of 50 μm. A laminate was obtained in the same manner as in Comparative Example 1, except that the obtained porous film was used.

[0051] (Comparative Example 5) As the nonwoven fabric, a spunbond nonwoven fabric of PP resin fiber (basis weight 19 g / m 2 A laminate was obtained in the same manner as in Example 1, except that the above-mentioned acrylic resin was used instead of the above-mentioned acrylic resin.

[0052] <Evaluation> The following evaluations were carried out using the laminates obtained in the Examples and Comparative Examples. The results are shown in Table 1. 1. Water Vapor Transmission Rate In accordance with ISO15106-1, the water vapor transmission rate of the laminate was measured using a water vapor transmission rate measuring device (manufactured by Lyssy, device name "L80-5000") under measurement conditions of a temperature of 23°C and a humidity of 100% RH. Samples of 8 mm x 8 mm were used for the measurement. Measurement was carried out using 10 samples, and the average value was taken as the water vapor transmission rate of the laminate. The obtained value was measured in m according to the ISO water vapor transmission rate measurement method. 2 The measured values ​​were converted into water vapor transmission rates per unit area.

[0053] 2. Stretch Recovery The laminates obtained in the Examples and Comparative Examples were cut into 30 mm pieces in the machine direction and set in a tensile tester (manufactured by Shimadzu Corporation, product name "AG-20kNG") with a chuck distance of 50 mm in the width direction. The laminates were stretched to 100% at a tensile speed of 300 mm / min, and the stretched state was released, and the initial chuck distance of 50 mm (A) and post-test film length (mm) (B) were measured. The rate of variation was calculated from the obtained values ​​using the following formula. A rate of variation exceeding 10% was marked x, and a rate of 10% or less was marked ◯. The rate of variation was measured using the formula: Rate of variation (%) = [{(B) - (A)} / (A)] x 100.

[0054] 3. Touch The laminates obtained in the examples and comparative examples were cut into 100 mm x 100 mm samples. 3A resin composition containing 100 parts by weight of propylene (PP) resin fiber and 100 parts by weight of calcium carbonate as a filler was extruded using an extruder to produce a film with a thickness of 30 μm. The obtained film was stretched twice in the machine direction to obtain a breathable backsheet with a thickness of 15 μm. A carded type nonwoven fabric of propylene (PP) resin fiber (manufactured by Nitto Denko Corporation, trade name "ThermoStrain 22 HI", basis weight 22 g / m) was used. 2 ) and a hot melt adhesive (manufactured by Nitto Denko Corporation, product name "olefin hot melt adhesive AC600") was applied at a rate of 8 g / m 2 The sample and the comparative laminate were touched with the hand, and those judged to be soft were rated as ◯ (good), and those judged to be the same or hard were rated × (room for improvement).

[0055] 4. Productivity: The laminate manufacturing process including a pre-stretching step was rated as × (room for improvement), and the laminate manufacturing process not including a pre-stretching step was rated as 1500 g / (m 2 A laminate having a water vapor permeability of 0.05% or more (0.05% water vapor permeability) was evaluated as ◯ (good).

[0056] 5. Nonwoven Fabric Elongation The machine direction during the production of the nonwoven fabric is defined as the MD direction, and the direction perpendicular to the MD direction is defined as the CD direction. The nonwoven fabric was cut into a 50 mm length in the MD direction to prepare a sample. The obtained sample was set in a tensile tester (Shimadzu Corporation, product name "AG-20kNG") with a chuck distance of 50 mm and stretched in the CD direction at a tensile speed of 300 mm / min under the condition of 100% stretch. The strength (N / 50 mm) was measured when the value calculated as (CD length of nonwoven fabric after stretching - CD length of nonwoven fabric before stretching) / CD length of nonwoven fabric before stretching x 100 (%) reached 50%. Nonwoven fabrics with a strength of 10 N / 50 mm or less were rated as ◯ (good), and nonwoven fabrics with a strength exceeding 10 N / 50 mm were rated as × (room for improvement).

[0057]

[0058] The laminates of the examples of the present invention had excellent moisture permeability and excellent stretchability. They also had an excellent feel to the touch. Furthermore, they were highly productive and could be produced efficiently.

[0059] The laminate according to the embodiment of the present invention can be suitably used in sanitary products, particularly as a backsheet for disposable diapers.

[0060] 10 Polyurethane resin layer 20 Fiber nonwoven fabric layer 100 Laminate

Claims

1. A laminate having a fibrous nonwoven fabric layer and a polyurethane resin layer having a thickness of 5 μm or more and 15 μm or less.

2. The water vapor permeability of the laminate is 1500 g / (m 2 2. The laminate according to claim 1, wherein the average thermal expansion coefficient is 1.0-1.0 days.

3. The laminate according to claim 1 or 2, in which the laminate is stretched to 100% under conditions of a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 300 mm / min, fixed in the stretched state and held for 1 minute, and then released from the stretched state, the rate of variation (%) calculated from the initial chuck distance (A) (mm) and the length of the laminate after the test (B) (mm) = [{(B) - (A)} / (A)] x 100 is 10% or less.

4. The laminate according to any one of claims 1 to 3, wherein the nonwoven fabric layer is a nonwoven fabric that stretches in the CD direction by 50% or more.

5. The laminate according to any one of claims 1 to 4, wherein the nonwoven fabric layer and the polyurethane resin layer are extrusion laminated.

6. The laminate according to any one of claims 1 to 4, wherein the nonwoven fabric layer and the polyurethane resin layer are laminated via a pressure-sensitive adhesive layer.

7. The laminate according to claim 6, wherein the pressure-sensitive adhesive layer is a layer formed on the entire surface of at least one of the nonwoven fabric layer and the polyurethane resin layer.

8. The laminate according to claim 6, wherein the pressure-sensitive adhesive layer is a layer intermittently formed on the surface of at least one of the nonwoven fabric layer and the polyurethane resin layer.

9. The laminate according to any one of claims 1 to 8, wherein the nonwoven fabric layer is a nonwoven fabric made of olefin-based fibers.

10. A sanitary article comprising a laminate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Material for extensible clothing

    JP1986225364A

  • Expandable, moisture-permeable and waterproofing sheet

    JP1994134000A

  • Composite nonwoven sheet

    JP1999115127A

  • Manufacture of laminated sheet