Alkenyl-group-containing polyoxyalkylene compound, silicone modifier, polyoxyalkylene-modified silicone, and emulsion composition
The synthesis of a polyether-based alkenyl group-containing polyoxyalkylene compound and its modification with a SiH group-containing organopolysiloxane addresses the stability and texture issues of conventional emulsifiers, providing a stable, fresh, and odor-controlled emulsifying composition for cosmetics.
Patent Information
- Application Number
- PCT/JP2024/014765
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional emulsifiers, such as polyoxyalkylene fatty acid esters, struggle to maintain stable emulsions, especially when dealing with large amounts of oil, and can cause cosmetic products to be sticky and have poor texture, while dehydration condensation reactions lead to coloration and odor issues due to degradation and hydrolysis.
A polyether-based alkenyl group-containing polyoxyalkylene compound is synthesized through dehydration condensation using a strong acid catalyst and diol, combined with a SiH group-containing organopolysiloxane to create a polyoxyalkylene-modified silicone, which acts as a surfactant in an emulsifying composition, enhancing emulsifying power and stability while suppressing coloration and odor.
The resulting emulsifying composition achieves high emulsifying power, a fresh feel upon application, excellent long-term stability, and controlled odor, suitable for cosmetic products requiring transparency and minimal coloration.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Alkenyl group-containing polyoxyalkylene compound, silicone modifier, polyoxyalkylene-modified silicone, and emulsion composition
[0001] The present invention relates to an alkenyl group-containing polyoxyalkylene compound, a silicone modifier, a polyoxyalkylene-modified silicone, and an emulsion composition. More specifically, the present invention relates to an alkenyl group-containing polyoxyalkylene compound capable of imparting surfactant properties to organopolysiloxanes; a silicone modifier comprising this compound; a polyoxyalkylene-modified silicone that is a reaction product of this silicone modifier and an organopolysiloxane; and an emulsion composition containing predetermined amounts of this polyoxyalkylene-modified silicone, an oil, and water.
[0002] Alkenyl-containing polyoxyalkylene compounds can be obtained by ring-opening addition polymerization of an initiator such as allyl alcohol containing active hydrogen with an alkylene oxide such as ethylene oxide or propylene oxide using an alkaline catalyst, or by reacting a polyoxyalkylene compound with an alkenyl halide. These alkenyl-containing polyoxyalkylene compounds contain both the reactive alkenyl group and a polyoxyalkylene group, which allows for a wide range of adjustments to the hydrophilicity and hydrophobicity of the resulting product. Therefore, they are used as silicone modifiers, polymerizable monomers, reactive emulsifiers, etc. Silicone modifiers, in particular, can impart surfactant properties to organopolysiloxanes, which have excellent heat resistance, weather resistance, mold releasability, water repellency, and physiological inertness.
[0003] For example, a modified organopolysiloxane can be obtained by chemically reacting a silicone modifier composed of a reactive group such as an alkenyl group and a hydrophilic functional group such as a polyoxyalkylene group with an organopolysiloxane having a reactive functional group such as a silylidyne group (hereinafter also referred to as an "SiH group"). The modified organopolysiloxane obtained by this method can impart excellent emulsion stability when incorporated, for example, as a surfactant component in an emulsion composition, and is therefore widely used in many industrial fields such as cosmetics, toiletries, and paints.
[0004] Emulsion compositions are broadly classified into oil-in-water and water-in-oil types based on their emulsification state, and are used for a variety of purposes, particularly in the cosmetics industry, such as skin care creams, emulsions, and sunscreens. Among these, water-in-oil types are superior to oil-in-water types as topical skin preparations because they can efficiently spread oil-soluble emollient oils, active ingredients, and UV absorbers onto the skin. However, because the continuous phase of water-in-oil types is oil, they can fully achieve moisturizing effects and the effects of active ingredients, but compared to oil-in-water types, they tend to be sticky upon application and can sometimes have a poor feel.
[0005] One solution to this problem of water-in-oil emulsions is to increase the water content. This method can impart a moisturizing feel, resulting in a refreshing sensation when used. Furthermore, by using silicone oil as the oil agent, it is possible to obtain a refreshing emulsion with little stickiness and high water repellency. However, it has been difficult to obtain a stable emulsion using conventional emulsifiers such as polyoxyalkylene fatty acid esters.
[0006] Against this background, for example, Patent Document 1 discloses a water-in-oil emulsion that has high stability by using a polyoxyalkyl-modified silicone that has both a polyglycerin group and a polyoxyalkyl group as an emulsifier.
[0007] Patent Document 2 discloses that by using a branched polyoxyalkylene-modified silicone as an emulsifier, excellent emulsification performance can be obtained for various oils such as silicone oil, and further that the resulting emulsion has a refreshing feel when used and is excellent in emulsion stability and transparency.
[0008] JP 2012-207078 A JP 2002-179797 A
[0009] Although the compositions described in Patent Documents 1 and 2 have excellent emulsion stability, there is a possibility that their emulsifying power may be insufficient when emulsifying a large amount of oil, and therefore there is a demand for an excellent emulsifier that has high emulsifying power and also provides a fresh feeling to the touch. Silicone modifiers that are generally used are those obtained by a polymerization reaction using an alkali catalyst and an alkylene oxide.
[0010] The following description is not publicly known, but rather is a matter investigated by the present inventors. During the development of the present invention, the present inventors focused on compounds obtained by a dehydration condensation reaction using a strong acid catalyst and a diol. It is known that compounds obtained by this dehydration condensation reaction are colored, and studies on coloration suppression have been conducted for a long time (see, for example, JP 2004-182974 A). Furthermore, in recent cosmetic developments, there has been a strong demand for improved color hue in formulations to enhance a sense of luxury. Highly transparent formulations such as lotions require colorless transparency, while opaque formulations such as emulsions and creams require a milky white color without any yellow tint. However, when surfactants containing silicone modifiers obtained by dehydration condensation reactions are used as cosmetic ingredients, color suppression may be insufficient. Furthermore, because dehydration condensation reactions are often performed under high-temperature conditions, silicone modifiers are prone to degradation, and they gradually hydrolyze in the presence of moisture in the air and traces of acid, producing odorous substances such as propionaldehyde, potentially resulting in the development of odorous products over time.
[0011] As a result of intensive research to solve the above problems, the present inventors have focused on using a specific polyether obtained by dehydration condensation of a diol as a silicone modifier, and have found that a surfactant obtained by reacting this silicone modifier with an organopolysiloxane having SiH groups suppresses coloration. Furthermore, the present inventors have also found that an emulsion composition using this surfactant has high emulsifying power, so that a large amount of water can be added, imparting a fresh feeling of use upon application, and exhibiting excellent emulsion stability and odor suppression over time.
[0012] The present invention includes the following aspects [1] to [4]: [1] An alkenyl group-containing polyoxyalkylene compound represented by the following formula (1): R 1 O-(AO)n-R 2 (1) (In formula (1), AO is an oxyalkylene group having 2 to 4 carbon atoms obtained by a dehydration condensation reaction using phosphinic acid or a phosphinic acid salt. n represents the average number of moles of AO added, and n is 3 to 90. R 1 is an alkenyl group having 3 to 5 carbon atoms, R 2 is an alkenyl group having 3 to 5 carbon atoms or a hydrogen atom. The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) calculated from a chromatogram obtained by gel permeation chromatography measurement is 1.20 to 5.00.
[0013] [2] A silicone modifier comprising the alkenyl group-containing polyoxyalkylene compound described in [1] above.
[0014] [3] A polyoxyalkylene-modified silicone which is a reaction product of the silicone modifier described in [2] above and a hydrogen organopolysiloxane represented by the following formula (2): (In formula (2), p is 1 to 100, q is 0 to 50, r is 0 to 100, and q / (p+r) is 0 to 1. R 3 are each independently an alkyl group having 1 to 8 carbon atoms. 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. When q=0, R 4 and R 5 At least one of is a hydrogen atom.
[0015] [4] An emulsion composition comprising (A) 0.1 to 40 mass% of the polyoxyalkylene-modified silicone according to [3] above, (B) 1 to 50 mass% of an oily agent that is liquid at 25°C, and (C) 10 to 98 mass% of water, wherein the mass ratio of component (B) to component (A) ((B) / (A)) is 0.5 to 30.
[0016] The polyoxyalkylene-modified silicone obtained by reacting the alkenyl group-containing polyoxyalkylene compound of the present invention with an organopolysiloxane having SiH groups is inhibited from discoloring, and therefore is less likely to cause discoloration problems when used in products such as cosmetic raw materials. Furthermore, emulsion compositions using this polyoxyalkylene-modified silicone as a surfactant have high emulsifying power, allowing the addition of large amounts of water, imparting a fresh feel upon application and exhibiting excellent emulsion stability over time and odor suppression.
[0017] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to the embodiments described herein and various modifications are possible without departing from the spirit and scope of the present invention. In this specification, numerical ranges defined using the symbol "to" are intended to include both the upper and lower limits of the symbol. For example, "2 to 5" means 2 or more and 5 or less. In multiple numerical ranges described in stages in this specification, each upper limit and each lower limit can be the upper or lower limit of any combined numerical range. For example, when the content of a certain component is described as "5 to 20 mass%, 10 to 15 mass%, "this can constitute the respective numerical ranges of "5 to 15 mass%, " "10 to 20 mass%, " "5 to 10 mass%, " and "15 to 20 mass%". Furthermore, in the numerical ranges described herein, the upper or lower limit of the numerical range can be replaced with a value shown in the examples or a value unambiguously derived from the examples. In this specification, unless otherwise specified, all numerical values should be understood to be modified in all cases by being preceded by the term "about." Numerical values should be construed herein given the inherent variation characteristic of the measurement technique employed to determine such values and should at least be construed in light of the number of significant digits and by applying rounding techniques.
[0018] <Alkenyl Group-Containing Polyoxyalkylene Compound> The alkenyl group-containing polyoxyalkylene compound of the present invention (hereinafter also referred to as "the compound of the present invention") is a polyether represented by the following formula (1): R 1 O-(AO)n-R 2 (1)
[0019] In formula (1), AO is an oxyalkylene group having 2 to 4 carbon atoms, and the oxyalkylene group may have a branched chain. Examples of AO include an oxyethylene group, an oxypropylene group, an oxytrimethylene group, a 1,2-oxybutylene (oxy-1-ethylethylene group), and a 1,4-oxybutylene group (oxytetramethylene group), and preferably an oxyethylene group, an oxypropylene group, or an oxytrimethylene group, and more preferably an oxyethylene group. Different oxyalkylene groups may be contained in the molecule of formula (1), and different oxyalkylene groups may be bonded in a block or random configuration.
[0020] Since the compound of the present invention is a composition containing two or more polyethers having different numbers of moles of oxyalkylene groups added, n in formula (1) represents the average number of moles of AO added. n is 3 to 90, preferably 6 to 70, more preferably 6 to 50, particularly preferably 7 to 30, and even more preferably 8 to 20. When two or more different types of oxyalkylene groups are contained in the molecule of formula (1), the sum of the average number of moles of oxyalkylene groups added may be within the above range.
[0021] In formula (1), R 1 is an alkenyl group having 3 to 5 carbon atoms, and R 2 is an alkenyl group having 3 to 5 carbon atoms or a hydrogen atom. These alkenyl groups may have a branched chain. R 2 When is an alkenyl group, R 1 and R 2 may be different alkenyl groups or may be the same alkenyl group. From the viewpoint of reactivity with silicone, R 1 and R 2 and are preferably both allyl groups which are alkenyl groups having 3 carbon atoms, or both methallyl groups which are alkenyl groups having 4 carbon atoms, and more preferably both allyl groups.
[0022] The compound of the present invention is specified by the molecular weight obtained from a chromatogram obtained by gel permeation chromatography (GPC) using a differential refractometer. This chromatogram is a graph showing the relationship between refractive index intensity and elution time. The ratio (Mw / Mn) of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) obtained from the chromatogram is in the range of 1.20 to 5.00. If the ratio (Mw / Mn) is too small, it is likely that an emulsion will not be obtained, while if the ratio (Mw / Mn) is too large, it is likely that a fresh feeling upon application will not be achieved. The ratio is preferably 1.25 to 3.00, more preferably 1.30 to 2.00, particularly preferably 1.40 to 1.80, and even more preferably 1.50 to 1.70.
[0023] In the present invention, gel permeation chromatography (GPC) for determining Mw and Mn is performed under the following conditions, and a chromatogram expressed as refractive index intensity and elution time is obtained using a Borwin GPC calculation program. System: SHODEX (registered trademark) GPC101 GPC dedicated system Differential refractometer: SHODEX (registered trademark) RI-71s Guard column: SHODEX (registered trademark) KF-G Column: Three SHODEX (registered trademark) KF804L columns installed in series Column temperature: 40°C Developing solvent: tetrahydrofuran Flow rate: 1 ml / min
[0024] [Method for Producing the Compound of the Present Invention] The compound of the present invention can be produced by first obtaining a reaction product by dehydration condensation of a diol represented by the following formula (3), and then alkenylating the reaction product: HO-(A'O)m-H (3)
[0025] In formula (3), A'O is an oxyalkylene group having 2 to 4 carbon atoms, and the oxyalkylene group may have a branched chain. Examples of A'O include an oxyethylene group, an oxypropylene group, an oxytrimethylene group, a 1,2-oxybutylene (oxy-1-ethylethylene group), and a 1,4-oxybutylene group (oxytetramethylene group), and preferably an oxyethylene group, an oxypropylene group, or an oxytrimethylene group, and more preferably an oxyethylene group. m is an integer of 1 to 3. When m is 2 or 3, different oxyalkylene groups may be contained in the molecule of formula (3).
[0026] Examples of diols represented by the above formula (3) include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, 1,2-butylene glycol, 1,4-butylene glycol, etc., and one selected from these diols can be used alone or two or more can be used in combination. From the viewpoint of the stability of the resulting emulsion, triethylene glycol and tripropylene glycol are preferred, and triethylene glycol is more preferred.
[0027] The reaction temperature during dehydration condensation is preferably 100 to 200° C., and from the viewpoints of reactivity and coloration of the resulting silicone modifier, more preferably 110 to 140° C. The pressure during production is atmospheric pressure or less, preferably about 10 kPa or less, and more preferably about 3 kPa or less.
[0028] A dehydration condensation catalyst is usually used for the dehydration condensation reaction. Examples of the dehydration condensation catalyst include homogeneous catalysts such as Lewis acids, Bronsted acids, super acids, and mixtures thereof. Examples include inorganic acids, organic sulfonic acids, heteropolyacids, and metal salts thereof. More specific examples include sulfuric acid, fluorosulfonic acid, phosphoric acid, p-toluenesulfonic acid, benzenesulfonic acid, phosphotungstic acid, phosphomolybdic acid, trifluoromethanesulfonic acid, 1,1,2,2-tetrafluoroethanesulfonic acid, 1,1,1,2,3,3-hexafluoropropanesulfonic acid, bismuth triflate, yttrium triflate, ytterbium triflate, neodymium triflate, lanthanum triflate, scandium triflate, and zirconium triflate. Heterogeneous catalysts such as zeolite, fluorinated alumina, acid-treated silica, acid-treated silica-alumina, heteropolyacids, heteropolyacids supported on zirconia, titania, alumina, and silica can also be used. The homogeneous catalysts described above are preferred, with sulfuric acid being more preferred. The amount of the dehydration condensation catalyst used is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, per 100 parts by mass of the diol used.
[0029] In the method according to the present invention, the presence of phosphinic acid or a phosphinic acid salt during dehydration condensation yields AO in formula (1), i.e., an oxyalkylene group having 2 to 4 carbon atoms. The phosphinic acid salt is preferably an alkali metal salt of phosphinic acid, such as sodium phosphinate or potassium phosphinate. From the standpoints of availability and suppression of coloration, it is preferable to use phosphinic acid or sodium phosphinate, and it is more preferable to use phosphinic acid. The amount of phosphinic acid or phosphinic acid salt used is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the diol used. Phosphinic acid and phosphinic acid salt may be used in combination, in which case the total amount of both used is preferably within the above range.
[0030] The reaction product after the dehydration condensation reaction preferably has a hydroxyl value of 25 to 750 mgKOH / g, more preferably 50 to 500 mgKOH / g, as measured in accordance with JIS K 1557-1.
[0031] The Hazen color number (APHA) of the reaction product is preferably 0 to 500, more preferably 0 to 300. The Hazen color number (APHA) is measured in accordance with JIS K 0071-1.
[0032] When the compound of the present invention has different oxyalkylene groups, the molar ratio of each oxyalkylene group can be determined, for example, by using a proton nuclear magnetic resonance (H-NMR) spectrometer. For example, when the compound of the present invention has an oxyethylene group and an oxypropylene group, the molar ratio of oxyethylene group:oxypropylene group can be determined by the integral value (P 1 ) and the integral value of the peaks of the methylene groups of the oxyethylene group and the oxypropylene group (P 2 ) can be calculated using the following formula. Furthermore, the total molecular weight can be calculated using the hydroxyl value, and the number of moles added can be calculated. Oxyethylene group: oxypropylene group = {(P 2 -P 1 ) / 4}: (P 1 / 3)
[0033] Next, alkenylation can be carried out by reacting the reaction product with an alkenyl halide. The alkenyl halide used is R 1 -X or R 2 '-X. 1 -X and R 2 '-X may be different or the same. 1 -X or R 2 Either one or both of R'-X can be used. 1 -R in X 1 is R in formula (1) 1 is synonymous with R 2 '-R in X 2 ' is R in formula (1)2 X is a halogen. Examples of halogen include fluorine, chlorine, bromine, and iodine, and any halogen selected from these can be used. The amount of the halogenated alkenyl used is preferably 4 to 120 parts by mass, and more preferably 8 to 75 parts by mass, per 100 parts by mass of the reaction product.
[0034] The alkenylation is carried out under basic conditions, for example, in the presence of a strong base. The reaction temperature during the alkenylation is preferably 60 to 200°C, more preferably 70 to 140°C. The pressure during the production is atmospheric pressure or less, preferably about 10 kPa or less, more preferably about 3 kPa or less.
[0035] The alkenyl group-containing polyoxyalkylene compound of the present invention thus obtained preferably has a degree of unsaturation of 0.40 to 13.00 meq / g, more preferably 0.90 to 8.90 meq / g, as measured in accordance with JIS K 1557-3.
[0036] The Hazen color unit number (APHA) of the compound of the present invention is preferably 0 to 500, more preferably 0 to 400. The Hazen color unit number (APHA) is measured in accordance with JIS K 0071-1.
[0037] In summary, the method for producing the alkenyl group-containing polyoxyalkylene compound represented by the above formula (1) comprises the steps of: subjecting the diol represented by the above formula (3) to a dehydration condensation reaction in the presence of a phosphinic acid or a phosphinic acid salt to obtain a reaction product; 1 -X and / or R 2 The method includes a step of reacting —X with
[0038] <Silicone Modifier> The silicone modifier of the present invention comprises an alkenyl group-containing polyoxyalkylene compound, which is the compound of the present invention, that functions as a silicone modifier.
[0039] <Polyoxyalkylene-Modified Silicone> The polyoxyalkylene-modified silicone of the present invention is a reaction product between the compound of the present invention, which functions as a silicone modifier, and a hydrogenorganopolysiloxane represented by the following formula (2): In other words, this reaction product is a hydrosilylation product of the compound of the present invention with the hydrogenorganopolysiloxane represented by the following formula (2):
[0040]
[0041] In formula (2), p is 1 to 100, q is 0 to 50, r is 0 to 100, and q / (p+r) is 0 to 1. From the viewpoint of the stability of the emulsion composition of the present invention, which will be described later, p is preferably 80 or less, more preferably 50 or less, and even more preferably 20 or less. q is preferably 30 or less, more preferably 10 or less, and particularly preferably 0. r is preferably 80 or less, more preferably 50 or less, and particularly preferably 20 or less. q / (p+r) is preferably 0.4 or less, and more preferably 0.
[0042] A plurality of R contained in formula (2) 3 are each independently an alkyl group having 1 to 8 carbon atoms, and the alkyl group may have a branched chain. 3 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a hexyl group, and an octyl group, and preferred are a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, and an isobutyl group.
[0043] R 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. However, when q=0, R 4 and R 5 At least one of the groups is a hydrogen atom. The alkyl group having 1 to 8 carbon atoms may have a branched chain. Examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a hexyl group, and an octyl group, and preferred are a methyl group and an ethyl group.
[0044] The hydrogen organopolysiloxane represented by formula (2) can be produced by a known method, but commercially available products can also be used. For example, a product of this type is "Methyl H Siloxane-Dimethyl Siloxane Copolymer" manufactured by Gelest, product code HMS-082 (where R 3 , R 4 and R 5 are all methyl groups, p is 75, q is 6.5, and r is 0.
[0045] The reaction between the compound of the present invention and the hydrogenorganopolysiloxane is usually carried out by mixing the two in the presence of a catalyst. Examples of the catalyst that can be used include chloroplatinic acid hexahydrate, alcohol-modified chloroplatinic acid, and chloroplatinic acid-vinylsiloxane complex. The amount of catalyst used is preferably 500 ppm or less, and particularly preferably 200 ppm or less, calculated as platinum, based on the total mass of the compound of the present invention and the hydrogenorganopolysiloxane.
[0046] The reaction temperature is preferably 50 to 130° C., more preferably 60 to 110° C. Completion of the reaction can be confirmed by FT-IR measurement, and a 2100 to 2300 cm radiative spectrum derived from the SiH group is observed. -1 The reaction is carried out until the absorption of
[0047] <Emulsion Composition> The emulsion composition of the present invention contains (A) 0.1 to 40 mass% of the polyoxyalkylene-modified silicone of the present invention, (B) 1 to 50 mass% of an oily agent that is liquid at 25° C., and (C) 10 to 98 mass% of water. In the emulsion composition of the present invention, the total amount of components (A), (B), and (C) is 100 mass%.
[0048] [Component (A): Polyoxyalkylene-Modified Silicone] Component (A) used in the emulsion composition of the present invention is the above-mentioned polyoxyalkylene-modified silicone that functions as a surfactant. The content of component (A) in the emulsion composition of the present invention is 0.1 to 40% by mass, preferably 0.5 to 30% by mass, more preferably 1 to 20% by mass, and particularly preferably 3 to 15% by mass. If the content of component (A) is too low, the surfactant activity of component (A) will be too low, and a stable emulsion composition may not be obtained. If the content is too high, the surfactant activity of component (A) will be too high, and partial gelation or the like may occur, and a stable emulsion composition may not be obtained.
[0049] [Component (B): Oil that is liquid at 25°C] The oil of component (B) is one or more oils selected from the group consisting of hydrocarbon oils that are liquid at 25°C, ester oils that are liquid at 25°C, triglycerides that are liquid at 25°C, animal and vegetable oils that are liquid at 25°C, and silicone oils that are liquid at 25°C.
[0050] Examples of hydrocarbon oils include liquid paraffin, hydrogenated polyisobutene, hydrogenated polydecene, squalane, squalene, pristane, light isoparaffin, light liquid isoparaffin, heavy liquid isoparaffin, liquid isoparaffin, tetradecene, isohexadecane, isododecane, α-olefin oligomers, etc. Preferred are liquid paraffin and hydrogenated polyisobutene, etc.
[0051] Examples of ester oils include ethyl oleate, ethyl linoleate, isopropyl myristate, isopropyl palmitate, isopropyl isostearate, cetyl 2-ethylhexanoate, cetyl palmitate, 2-ethylhexyl palmitate, isostearyl isostearate, myristyl myristate, cetyl myristate, isostearyl myristate, isocetyl myristate, hexyl laurate, decyl oleate, octyldodecyl oleate, isononyl isononanoate, and 2-ethylhexyl isononanoate.
[0052] Triglycerides are esters of glycerin and fatty acids, and examples of fatty acids include caproic acid, caprylic acid, capric acid, 2-ethylhexanoic acid, isotridecanoic acid, isopalmitic acid, isostearic acid, eicosanoic acid, and oleic acid. Examples of animal and vegetable oils include olive oil, sunflower oil, safflower oil, castor oil, and camellia oil. Examples of silicone oils include dimethicone, cyclomethicone, and phenyldimethicone, with dimethicone and cyclomethicone being preferred.
[0053] The oil agent of component (B) used is preferably silicone oil from the viewpoint of compatibility with the surfactant of component (A).
[0054] The content of component (B) in the emulsion composition of the present invention is 1 to 50% by mass, preferably 2 to 40% by mass, more preferably 5 to 30% by mass, and particularly preferably 10 to 25% by mass. If the content of component (B) is too low, the field in which component (A) functions may be too small, and a stable emulsion composition may not be obtained. If the content of component (B) is too high, the field in which component (A) functions may be too large, and a stable emulsion composition may not be obtained.
[0055] The total amount of component (A) and component (B) in the emulsion composition of the present invention is calculated to be 1.1 to 90% by mass, preferably 5 to 80% by mass, more preferably 10 to 70% by mass, and particularly preferably 15 to 60% by mass. If the total amount of component (A) and component (B) is too small, the content of component (C), which will be described later, will be too high, and a stable emulsion composition may not be obtained. If the total amount of component (A) and component (B) is too large, the content of component (C) will be too low, and a stable emulsion composition may not be obtained.
[0056] [Component (C): Water] Component (C) used in the emulsion composition of the present invention is water. The water is not particularly limited. For example, purified water such as distilled water or ion-exchanged water, physiological saline, phosphate buffer solution, etc. can be used.
[0057] The content of component (C) in the emulsion composition of the present invention is 10 to 98% by mass, preferably 20 to 90% by mass, more preferably 40 to 85% by mass, and particularly preferably 45 to 80% by mass. If the content of component (C) is too low or too high, excessive viscosity may be imparted, causing partial gelation, and therefore a stable emulsion composition may not be obtained.
[0058] The ratio of the mass of component (B) to the mass of component (A) ((B) / (A)) is preferably from 0.5 to 30, more preferably from 1 to 20, particularly preferably from 1 to 15, even more preferably from 1 to 10, and especially preferably from 1 to 6, from the viewpoints of emulsion stability and a fresh feeling upon application.
[0059] The emulsion composition of the present invention is prepared by blending the above-mentioned components (A) and (B) with water (component (C)). Various commonly used components can be blended into the emulsion composition of the present invention as needed. For example, in the field of cosmetic materials, moisturizers, preservatives, antioxidants, UV absorbers, cosmetic ingredients, fragrances, water-soluble polymers, coloring matter, pigments, organic powders, etc. can be blended.
[0060] The form of the emulsion composition of the present invention is not particularly limited, but it can be used in a wide range of applications such as cosmetic materials having excellent emulsion stability, paints, etc. In particular, in the field of cosmetic materials, oil-based cosmetics such as emulsions, cleansing oils, and hair oils are suitable.
[0061] The present invention has been described above by showing preferred embodiments for ease of understanding. Below, the present invention will be described in more detail and specifically by giving synthesis examples, examples, and comparative examples. However, the above description and the following synthesis examples, examples, and comparative examples are provided for illustrative purposes only and are not intended to limit the present invention. The intermediates, silicone modifiers, and surfactants shown in the following synthesis examples were analyzed by the methods described below. (Analytical methods) Hydroxyl value: JIS K 1557-1 Degree of unsaturation: JIS K 1557-3 Hazen color index (APHA): JIS K 0071-1
[0062] [Synthesis Example A-1] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 750 g of triethylene glycol (manufactured by Kanto Chemical Co., Ltd.), 9.8 g of sulfuric acid (manufactured by Kanto Chemical Co., Ltd.), and 6 g of phosphinic acid (manufactured by Kanto Chemical Co., Ltd.). After nitrogen substitution, the temperature was raised to 120 ° C., and the reaction was carried out for 23 hours under a vacuum of 6 kJ and nitrogen bubbling conditions. Five grams each of two adsorbents (Kyoward #700 and #1000, manufactured by Kyowa Chemical Industry Co., Ltd.) were added, and the mixture was subjected to adsorption treatment for 1 hour at 90 ° C., -0.097 MPa (gauge pressure) or less, with nitrogen bubbling. Filtration afforded 525 g of intermediate (A-1). The hydroxyl value was 251 mg KOH / g, the average number of moles of oxyethylene groups added was 10, and APHA was 60.
[0063] To 300 g of the obtained intermediate (A-1), 113 g of potassium hydroxide and 123 g of allyl chloride were charged. After purging with nitrogen, the reaction was carried out at 120°C for 3 hours. 450 g of water was added, and after stirring for 10 minutes, the mixture was allowed to stand at 80°C for 1 hour. The separated upper layer was recovered and neutralized, and then water was removed by nitrogen bubbling at 80°C. Thereafter, the mixture was treated with nitrogen bubbling at 80°C and -0.097 MPa (gauge pressure) or less for 2 hours, and then filtered to obtain silicone modifier (A-1). The degree of unsaturation was 3.36 meq / g, APHA was 150, and Mw / Mn = 1.45.
[0064] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 80 g (SiH equivalent: 85 meq) of hydrogendimethylpolysiloxane (HMS-082 (manufactured by Gelest), SiH equivalent per 1 g: 1.06 meq / g) and 35 g (unsaturated equivalent: 118 meq) of silicone modifier (A-1). A solution of chloroplatinic acid hexahydrate in isopropyl alcohol (1×10 -3 The reaction was carried out at 90°C with stirring under a nitrogen atmosphere. Sampling was carried out, and an isopropyl alcohol solution of N / 10 potassium hydroxide was added, and the reaction was continued until no more hydrogen gas was generated. FT-IR measurement revealed a peak of 2100 to 2300 cm3 derived from SiH groups. -1It was confirmed that the absorption of the surfactant (A-1) had disappeared.
[0065] [Synthesis Example A-2] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 375 g of triethylene glycol (manufactured by Kanto Chemical Co., Ltd.), 480 g of tripropylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd.), 9.8 g of sulfuric acid (manufactured by Kanto Chemical Co., Ltd.), and 6 g of phosphinic acid (manufactured by Kanto Chemical Co., Ltd.). After nitrogen substitution, the temperature was raised to 120 ° C., and the reaction was carried out for 23 hours under a vacuum of 6 kJ and nitrogen bubbling conditions. Five grams each of two adsorbents (Kyoward #700 and #1000, manufactured by Kyowa Chemical Industry Co., Ltd.) were added, and the mixture was subjected to adsorption treatment for 1 hour at 90 ° C., -0.097 MPa (gauge pressure) or less, with nitrogen bubbling. Filtration gave 550 g of intermediate (A-2). The hydroxyl value was 220 mgKOH / g, the average number of moles of oxyethylene groups added was 5, the average number of moles of oxypropylene groups added was 4, and the APHA was 80.
[0066] To 300 g of the obtained intermediate (A-2), 99 g of potassium hydroxide and 108 g of allyl chloride were charged. After purging with nitrogen, the reaction was carried out at 120°C for 3 hours. 396 g of water was added, and after stirring for 10 minutes, the mixture was allowed to stand at 80°C for 1 hour. The separated upper layer was recovered and neutralized, and then water was removed by nitrogen bubbling at 80°C. Thereafter, the mixture was treated with nitrogen bubbling at 80°C and -0.097 MPa (gauge pressure) or less for 2 hours, and then filtered to obtain silicone modifier (A-2). The degree of unsaturation was 3.11 meq / g, APHA was 200, and Mw / Mn = 1.30.
[0067] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 80 g (SiH equivalent: 85 meq) of hydrogendimethylpolysiloxane (HMS-082 (manufactured by Gelest), SiH equivalent per gram: 1.06 meq / g) and 38 g (unsaturated equivalent: 118 meq) of silicone modifier (A-2). A solution of chloroplatinic acid hexahydrate in isopropyl alcohol (1×10 -3The reaction was carried out at 90°C with stirring under a nitrogen atmosphere. Sampling was carried out, and an isopropyl alcohol solution of N / 10 potassium hydroxide was added, and the reaction was continued until no more hydrogen gas was generated. FT-IR measurement revealed a peak of 2100 to 2300 cm3 derived from SiH groups. -1 It was confirmed that the absorption of the surfactant (A-2) had disappeared.
[0068] Synthesis Example A-3: 75 g of potassium hydroxide and 112 g of methallyl chloride were charged to 200 g of the intermediate (A-1) from Synthesis Example A-1. After purging with nitrogen, the reaction was carried out at 120°C for 3 hours. 301 g of water was added, and the mixture was stirred for 10 minutes and then allowed to stand at 80°C for 1 hour. The separated upper layer was recovered and neutralized, after which moisture was removed by nitrogen bubbling at 80°C. Thereafter, the mixture was treated with nitrogen bubbling at 80°C and -0.097 MPa (gauge pressure) or less for 2 hours, and then filtered to obtain silicone modifier (A-3). The degree of unsaturation was 3.20 meq / g, APHA was 150, and Mw / Mn = 1.45.
[0069] A 500-milliliter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 80 g (SiH equivalent: 85 meq) of hydrogendimethylpolysiloxane (HMS-082 (manufactured by Gelest), SiH equivalent per gram: 1.06 meq / g) and 38 g (unsaturated equivalent: 118 meq) of silicone modifier (A-3). A solution of chloroplatinic acid hexahydrate in isopropyl alcohol (1×10 -3 The reaction was carried out at 90°C with stirring under a nitrogen atmosphere. Sampling was carried out, and an isopropyl alcohol solution of N / 10 potassium hydroxide was added, and the reaction was continued until no more hydrogen gas was generated. FT-IR measurement revealed a peak of 2100 to 2300 cm3 derived from SiH groups. -1 It was confirmed that the absorption of the surfactant (A-3) had disappeared.
[0070] [Synthesis Example A'-1] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 750 g of triethylene glycol (manufactured by Kanto Chemical Co., Ltd.) and 9.8 g of sulfuric acid (manufactured by Kanto Chemical Co., Ltd.). After nitrogen substitution, the temperature was raised to 120 ° C., and the reaction was carried out for 25 hours under vacuum conditions of 6 kJ and nitrogen bubbling. Five grams each of two adsorbents (Kyoward #700 and #1000, manufactured by Kyowa Chemical Industry Co., Ltd.) were added, and the mixture was subjected to adsorption treatment for one hour under nitrogen bubbling at 90 ° C. and -0.097 MPa (gauge pressure) or less. Filtration afforded 550 g of intermediate (A'-1). The hydroxyl value was 260 mg KOH / g, the average number of moles of oxyethylene groups added was 10, and the APHA was 500.
[0071] To 300 g of the obtained intermediate (A'-1), 117 g of potassium hydroxide and 128 g of allyl chloride were charged. After purging with nitrogen, the reaction was carried out at 120°C for 3 hours. 468 g of water was added, and the mixture was stirred for 10 minutes and then allowed to stand at 80°C for 1 hour. The separated upper layer was recovered and neutralized, after which moisture was removed by nitrogen bubbling at 80°C. Subsequently, the mixture was treated with nitrogen bubbling at 80°C and -0.097 MPa (gauge pressure) or less for 2 hours, and then filtered to obtain silicone modifier (A'-1). The degree of unsaturation was 3.45 meq / g, APHA was 500 or more, and Mw / Mn = 1.55.
[0072] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 80 g (SiH equivalent: 85 meq) of hydrogendimethylpolysiloxane (HMS-082 (manufactured by Gelest), SiH equivalent per gram: 1.06 meq / g) and 34 g (unsaturated equivalent: 117 meq) of silicone modifier (A'-1). A solution of chloroplatinic acid hexahydrate in isopropyl alcohol (1 x 10 -3 The reaction was carried out at 90°C with stirring under a nitrogen atmosphere. Sampling was carried out, and an isopropyl alcohol solution of N / 10 potassium hydroxide was added, and the reaction was continued until no more hydrogen gas was generated. FT-IR measurement revealed a peak of 2100 to 2300 cm3 derived from SiH groups. -1It was confirmed that the absorption of the compound had disappeared, and surfactant (A'-1) was obtained.
[0073] [Synthesis Example A'-2] Silicone modifier (A'-2) represented by formula (4) was obtained by a known production technique. The degree of unsaturation was 4.00 meq / g, APHA was 50, and Mw / Mn = 1.05. CH 2 =CH-CH 2 -O-(EO) 9 -CH 2 -CH=CH 2 (4)
[0074] A 1-liter four-neck flask equipped with a stirrer, a nitrogen inlet tube, a thermocouple, and a condenser was charged with 80 g (SiH equivalent: 85 meq) of hydrogendimethylpolysiloxane (HMS-082 (manufactured by Gelest), SiH equivalent per gram: 1.06 meq / g) and 30 g (unsaturated equivalent: 120 meq) of silicone modifier (A'-2). A solution of chloroplatinic acid hexahydrate in isopropyl alcohol (1 x 10 -3 The reaction was carried out at 90°C with stirring under a nitrogen atmosphere. Sampling was carried out, and an isopropyl alcohol solution of N / 10 potassium hydroxide was added, and the reaction was continued until no more hydrogen gas was generated. FT-IR measurement revealed a peak of 2100 to 2300 cm3 derived from SiH groups. -1 It was confirmed that the absorption of the compound had disappeared, and surfactant (A'-2) was obtained.
[0075] The silicone modifiers and surfactants produced in Synthesis Examples A-1 to A'-2 are shown in Table 1.
[0076]
[0077] Examples 1 to 6 Emulsion cosmetics were prepared using the compositions shown in Table 2 and the manufacturing method described below. Sensory evaluations were then conducted on the emulsion cosmetics of each composition for freshness upon application, emulsion stability, and odor over time, with the results shown in Table 2. The panelists conducting the evaluations were trained in a preliminary evaluation test conducted prior to the evaluation test to ensure that the level of evaluation corresponding to each score was roughly consistent, and differences in evaluation criteria between panelists were avoided.
[0078] Comparative Examples 1 to 4 Emulsion cosmetics were prepared by the following production method with the compositions shown in Table 3. Sensory evaluations were then conducted on the emulsion cosmetics of each composition regarding freshness upon application, emulsion stability, and odor over time, and the results are shown in Table 3.
[0079] <Manufacturing Method> Step I: Components (A) and (B) in each table were placed in a beaker and stirred at room temperature (25°C) until homogenous. Step II: Component (C) (water) was gradually added to the composition prepared in Step I while stirring with a homomixer to emulsify, thereby obtaining an emulsion cosmetic.
[0080] Component (B) is as follows: (B-1): KF-995 (decamethylcyclopentasiloxane, manufactured by Shin-Etsu Chemical Co., Ltd.) (B-2): Liquid paraffin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (B-3): Unistar MB-816 (ethylhexyl palmitate, manufactured by NOF Corporation)
[0081] <Moisture sensation upon application> Five panelists applied 0.5 g of the emulsion cosmetic to the forearms, and sensory evaluation of moisture sensation was performed according to the following criteria. 3 points: The panelists felt a strong moisture sensation, with almost no sticky sensation. 2 points: The panelists felt a slight moisture sensation, but the sensation was slightly sticky. 1 point: The panelists felt almost no moisture sensation, and the sensation was sticky. Furthermore, the total score of the five panelists' evaluations was judged according to the following criteria. ◎: 12 points or more ○: 9 points or more, less than 12 points △: Less than 9 points
[0082] <Emulsion Stability> 30 g of the emulsion composition was placed in a 50 ml transparent glass container, sealed, and stored at 0°C, 25°C, and 40°C for one month. After one month, the appearance of the sample stored at each temperature was observed and rated according to the following criteria. ∘: The appearance of the sample after storage remained unchanged at any temperature. ×: The appearance of the sample after storage changed from a uniform appearance to separation of an oil layer or an aqueous layer at any temperature.
[0083] <Changes in odor over time> 30 g of the emulsion composition was placed in a 50 ml transparent glass container, sealed, and stored at 40°C for one month. After one month, five panelists performed a sensory evaluation of the aldehyde odor according to the following criteria. 3 points: The panelists hardly noticed any odor. 2 points: The panelists noticed a slight odor. 1 point: The panelists noticed an odor. Furthermore, the total score of the five panelists' evaluations was judged according to the following criteria. ◎: 12 points or more ○: 9 points or more, less than 12 points △: Less than 9 points
[0084]
[0085]
[0086] The emulsified cosmetics of Examples 1 to 6 according to the present invention had a fresh feeling when applied, were excellent in emulsion stability, and suppressed the generation of odor over time.
[0087] The emulsion cosmetics of Comparative Examples 1 to 4, which do not conform to the present invention, were inferior to the emulsion cosmetics of the Examples in any one of freshness upon application, emulsion stability, and odor over time.
[0088] (Note) It is understood that the scope of the present invention should not be construed as being limited by the description in this specification, but should be construed only by the description in the claims. It is also understood that the contents of the patent applications and technical standards referenced in this specification should be incorporated by reference in their entirety as if the contents themselves were specifically set forth in this specification. Furthermore, the disclosure of Japanese Patent Application No. 2023-069682, filed on April 20, 2023, is incorporated herein by reference in its entirety.
Claims
1. An alkenyl-containing polyoxyalkylene compound represented by the following formula (1): R 1 O-(AO)n-R 2 (1) (In formula (1), AO is an oxyalkylene group having 2 to 4 carbon atoms obtained by a dehydration condensation reaction using phosphinic acid or a phosphinic acid salt. n represents the average number of moles of AO added, n = 3 to 90. R 1 is an alkenyl group having 3 to 5 carbon atoms, R 2 is an alkenyl group having 3 to 5 carbon atoms or a hydrogen atom. The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) calculated from a chromatogram obtained by gel permeation chromatography measurement is 1.20 to 5.
00.
2. A silicone modifier comprising the alkenyl-containing polyoxyalkylene compound according to claim 1.
3. A polyoxyalkylene-modified silicone which is a reaction product of the silicone modifier according to claim 2 with a hydrogen organopolysiloxane represented by the following formula (2): (In formula (2), p is 1 to 100, q is 0 to 50, r is 0 to 100, and q / (p+r) is 0 to 1. 3 are each independently an alkyl group having 1 to 8 carbon atoms. 4 and R 5 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. When q=0, R 4 and R 5 At least one of is a hydrogen atom.) 4. An emulsion composition comprising (A) 0.1 to 40 mass% of the polyoxyalkylene-modified silicone according to claim 3, (B) 1 to 50 mass% of an oil agent that is liquid at 25°C, and (C) 10 to 98 mass% water, wherein the mass ratio of component (B) to component (A) ((B) / (A)) is 0.5 to 30.
Citation Information
Patent Citations
Synthesis method of allyl alcohol polyether
CN109320712A
Cold-setting composition
JP1997296046A
Curable composition
JP2009046539A
Curable composition
JP2015183185A
Photocurable composition
JP2016132704A