Copolyamide resin
The copolyamide resin, formed from specific diamines and dicarboxylic acids, addresses the challenges of water absorption and wear resistance in polyamide resins, achieving high bio-content and environmental compatibility, suitable for sustainable applications.
Patent Information
- Application Number
- PCT/JP2024/014956
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional polyamide resins derived from fossil materials face challenges in achieving low water absorption, excellent wear resistance, and high bio-content ratios, which are essential for meeting environmental sustainability standards and consumer quality demands.
A copolyamide resin is developed using equimolar amounts of pentamethylene diamine or decamethylene diamine with specific dicarboxylic acids, such as adipic and sebacic acid, to create structural units with a high bio-content, resulting in a resin with improved melting points, crystallization temperatures, and reduced water absorption.
The copolyamide resin exhibits low water absorption, enhanced wear resistance, and a high bio-content, making it suitable for environmentally friendly applications while maintaining properties comparable to conventional polyamide resins.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Copolymer polyamide resin
[0001] The present invention relates to a copolyamide resin, and particularly to a copolyamide resin containing a high proportion of raw materials derived from biomass.
[0002] Polyamide resins are polymers formed by assembling structural units containing amide bonds. The structural units of polyamides are generally derived from aminocarboxylic acids or lactams, or from diamines and dicarboxylic acids. Aliphatic polyamide resins derived from the aliphatic species of these compounds have versatile and beneficial properties, such as chemical resistance, toughness, heat resistance, and oil resistance. Therefore, aliphatic polyamide resins are useful as raw materials for molded products in a variety of applications. For example, they are used as substrates for monolayer or laminate films, particularly in packaging films that require pinhole resistance and gas barrier properties, particularly in the food packaging field, and as structural materials for multilayer films coextruded with other resins.
[0003] One of the advantages of resins is that their properties can be controlled in various ways by selecting the monomer or by using multiple types of monomers. Copolymer polyamide resins that give molded articles with properties suited to their intended use are produced by combining two or more types of structural units (Patent Document 1).
[0004] Polyamide resins provide molded products with excellent properties, and therefore are produced as homopolymers of various structural units or copolymers of combinations of structural units. However, many of the monomers used to produce polyamide resins are industrially derived from fossil fuels. For example, ε-caprolactam, a well-known raw material for Nylon (registered trademark), is synthesized from naphtha-derived benzene. With the recent rise in environmental awareness, which calls for the reduction of carbon dioxide emissions, there is a demand for a shift from fossil fuels to biomass-derived raw materials for polyamide resins. Pentamethylenediamine, which can be obtained from starch or sugarcane through enzyme reactions, yeast reactions, and fermentation reactions, is known as a biomass-derived compound that can be used as a polyamide raw material. Patent Document 2 attempts to produce polyamide resins with fewer impurities derived from biomass materials using pentamethylenediamine as a raw material. Patent Documents 3 and 4 attempt to produce polyamide resins for large molded products with improved thermal retention stability using pentamethylenediamine as a raw material.
[0005] International Publication No. 2022 / 071013 International Publication No. 2015 / 076233 JP 2006-348057 A JP 2007-332353 A
[0006] The replacement of conventional products with resins derived from biomass raw materials is one of the global efforts to build a sustainable society, and in Japan too, legislation is being put in place to set certain standards for the content of bio-based polymers, and efforts are being made to establish recycling processes and reduce CO2 emissions. 2 Demonstration experiments are underway to achieve this. However, replacing raw resin materials often involves changes to the molecular structure of the resin, which inevitably leads to changes in physical properties. Consumers are highly concerned about the quality of resins, along with the price, and there is a strong demand for resins that are of equal or higher quality than the resins they are replacing.
[0007] The inventors have found that the polyamide resin described in Patent Document 2 has a high crystallization temperature and a large heat of fusion, making it difficult to handle during the extrusion molding process in which the resin is melted and molded. Furthermore, aliphatic polyamide resins are hygroscopic due to the presence of amide bonds, making them useful as fibers, but high hygroscopicity can lead to durability problems. The inventors have found that the polyamide resin described in Patent Document 3 does not exhibit sufficient abrasion resistance. While it is possible to produce copolymers with conventional raw materials, Patent Document 4 does not adequately replace biomass raw materials. Therefore, there is a need to produce resins with a high bio content in accordance with regulatory requirements and certification bodies such as RSB and ISCC.
[0008] Therefore, an object of the present invention is to provide a copolymer polyamide resin that has low water absorption, excellent abrasion resistance, and a high bio content, and a molded article containing the same.
[0009] Specific means for solving the above problems are as follows: [1] A copolymer polyamide resin (excluding polyamide 56 / 510) having at least two types of structural units derived from a reaction product of equimolar amounts of at least one selected from pentamethylene diamine or decamethylene diamine with a dicarboxylic acid having 6 to 13 carbon atoms; [2] The copolymer polyamide resin of [1] above having at least one selected from the following: a structural unit derived from a reaction product of equimolar amounts of pentamethylene diamine and adipic acid, a structural unit derived from a reaction product of equimolar amounts of pentamethylene diamine and sebacic acid, a structural unit derived from a reaction product of equimolar amounts of decamethylene diamine and adipic acid, a structural unit derived from a reaction product of equimolar amounts of decamethylene diamine and sebacic acid, and a structural unit derived from a reaction product of equimolar amounts of a mixture of pentamethylene diamine and decamethylene diamine with sebacic acid. [3] The copolymer polyamide resin of [1] or [2] above, having as the structural unit [A] a structural unit derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid, or a structural unit derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid. [4] The copolymer polyamide resin of any of [1] to [3] above, containing the structural unit [A] in an amount of 50 to 95 mass% based on the total mass of the copolymer polyamide resin. [5] The copolymer polyamide resin of any of [1] to [4] above, wherein the melting point of the copolymer polyamide resin is 145 to 250°C as measured by DSC. [6] The copolymer polyamide resin of any of [1] to [5] above, wherein the crystallization temperature of the copolymer polyamide resin is 90 to 195°C as measured by DSC. [7] A polyamide resin composition comprising the copolymer polyamide resin of any of [1] to [6] above. [8] A molded article comprising the copolymer polyamide resin of any one of [1] to [6]. [9] A film comprising the copolymer polyamide resin of any one of [1] to [6].
[10] A monofilament comprising the copolymer polyamide resin of any one of [1] to [6].
[0010] The copolyamide resin of the present invention has low water absorption, excellent abrasion resistance, and a high bio content, and therefore can provide molded articles using an environmentally friendly resin.
[0011] The copolymerized polyamide resin of the present invention will be described in detail below for each of its constituent components. In this specification, the symbol "to" indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits. For example, "50.00 to 90.00 mass%" means "50.00 mass% or more and 90.00 mass% or less."
[0012] The copolyamide resin according to an embodiment of the present invention is a copolyamide resin having at least two types of structural units derived from equimolar amounts of a reaction product of at least one selected from pentamethylenediamine or decamethylenediamine with a dicarboxylic acid having 6 to 13 carbon atoms. However, polyamide 56 / 510 is excluded. Hereinafter, polyamide resin may be abbreviated as "PA."
[0013] Polyamide resin is a polymer in which many monomers are bonded together through amide bonds (-NHC(=O)-). Polyamides synthesized from equimolar amounts of linear diamines and linear dicarboxylic acids have structural units represented by the following general formula: In the formula, m represents the number of carbon atoms in the alkylene group derived from the dicarboxylic acid, and n represents the number of carbon atoms in the alkylene group derived from the diamine. Polyamides synthesized from linear diamines and linear dicarboxylic acids are represented by the number of carbon atoms (including the carbonyl carbon of the dicarboxylic acid) of the raw diamine and dicarboxylic acid. For example, a polyamide represented by "PA56" means a polyamide composed of structural units derived from the equimolar reaction product of a C5 diamine (pentamethylenediamine) and a C6 dicarboxylic acid (adipic acid). In the above formula, PA56 means a polyamide composed of structural units where n is 5 and m is 4. Copolymer polyamide resins are represented by listing multiple structural units, such as PA56 / 510. PA56 / 510 is a resin containing the PA56 structural unit and structural units derived from the equimolar reaction product of a C5 diamine (pentamethylenediamine) and a C10 dicarboxylic acid (sebacic acid).
[0014] The copolymerized polyamide resin according to an embodiment of the present invention has at least two types of structural units represented by the above general formula. Hereinafter, these structural units will be referred to as structural unit [A] and structural unit [B]. Structural units [A] and [B] are structural units derived from equimolar amounts of a reaction product of at least one selected from pentamethylenediamine or decamethylenediamine with a dicarboxylic acid having 6 to 13 carbon atoms.
[0015] The diamine constituting the structural units [A] and [B] is at least one selected from pentamethylenediamine and decamethylenediamine. The same diamine may be used for both structural units [A] and [B], or a mixture of pentamethylenediamine and decamethylenediamine may be used. Therefore, the copolyamide resin according to an embodiment of the present invention has a structural unit in which n is 5 or 10 in the above general formula.
[0016] The dicarboxylic acids constituting the structural units [A] and [B] are dicarboxylic acids having 6 to 13 carbon atoms. Therefore, the copolymerized polyamide resin according to an embodiment of the present invention has structural units in which m is 4 to 11 in the above general formula. Examples of dicarboxylic acids include adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, and brassylic acid. These dicarboxylic acids may be used alone or in combination. As dicarboxylic acids, it is preferable to use adipic acid (m = 4), which is industrially important and has an established production method, or sebacic acid (m = 8), which is a biomass material that can be produced from castor oil. It is even more preferable to use sebacic acid at least in part.
[0017] Specific examples of structural units [A] and [B] include structural units derived from the equimolar reaction product of pentamethylenediamine and adipic acid, structural units derived from the equimolar reaction product of pentamethylenediamine and sebacic acid, structural units derived from the equimolar reaction product of decamethylenediamine and adipic acid, structural units derived from the equimolar reaction product of decamethylenediamine and sebacic acid, and structural units derived from the equimolar reaction product of a mixture of pentamethylenediamine and decamethylenediamine with sebacic acid. The copolymerized polyamide resin according to the present invention preferably contains at least one selected from these structural units. Furthermore, structural unit [A] is more preferably a structural unit derived from the equimolar reaction product of pentamethylenediamine and adipic acid, or a structural unit derived from the equimolar reaction product of pentamethylenediamine and sebacic acid. Structural unit [B] is not particularly limited as long as it is a structural unit formed from a combination of a diamine and a dicarboxylic acid different from those of structural unit [A]. Furthermore, three or more types of structural units may be contained.
[0018] Specific examples of copolymer polyamide resins that satisfy the above requirements include copolymers containing PA56, such as PA56 / 57, PA56 / 58, PA56 / 59, PA56 / 511, PA56 / 512, PA56 / 513, PA56 / 106, PA56 / 107, PA56 / 108, PA56 / 109, PA56 / 1010, PA56 / 1011, PA56 / 1012, and PA56 / 1013; copolymers containing PA56, such as PA510 / 57, PA510 / 58, PA510 / 59, PA510 / 511, PA510 / 512, PA510 / 513, PA510 / 106, PA510 / 107, PA510 / 108, PA510 / 109, and PA510 / 1011. copolymers containing PA510 such as PA510 / 010, PA510 / 1011, PA510 / 1012, PA510 / 1013; copolymers containing PA106 such as PA106 / 57, PA106 / 58, PA106 / 59, PA106 / 511, PA106 / 512, PA106 / 513; copolymers containing PA1010 such as PA57 / 1010, PA58 / 1010, PA59 / 1010, PA511 / 1010, PA512 / 1010, PA513 / 1010, PA107 / 1010, PA108 / 1010, PA109 / 1010, PA1010 / 1011, PA1010 / 1012, PA1010 / 1013;PA57 / 58, PA57 / 59, PA57 / 511, PA57 / 512, PA57 / 513, PA57 / 107, PA57 / 108, PA57 / 109, PA57 / 1011, PA57 / 1012. PA57 / 1013, PA58 / 59, PA58 / 511, PA58 / 512, PA58 / 513, PA58 / 107, PA58 / 108, PA58 / 109, PA5 8 / 1011, PA58 / 1012, PA58 / 1013, PA59 / 511, PA59 / 512, PA59 / 513, PA59 / 107, PA59 / 108, PA5 9 / 109, PA59 / 1011, PA59 / 1012, PA59 / 1013, PA511 / 512, PA511 / 513, PA511 / 107, PA511 / 108 , PA511 / 109, PA511 / 1011, PA511 / 1012, PA511 / 1013, PA512 / 513, PA512 / 107, PA512 / 108, PA 512 / 109, PA512 / 1011, PA512 / 1012, PA512 / 1013, PA106 / 107, PA106 / 108, PA106 / 109, PA10 6 / 1011, PA106 / 1012, PA106 / 1013, PA107 / 108, PA107 / 109, PA107 / 1011, PA107 / 1012, PA107 Examples of copolymers that are not made from adipic acid or sebacic acid include copolymers that are not made from adipic acid or sebacic acid, such as PA108 / 109, PA108 / 1011, PA108 / 1012, PA108 / 1013, PA109 / 1011, PA109 / 1012, PA109 / 1013, PA1011 / 1012, PA1011 / 1013, and PA1012 / 1013. To increase the proportion of bio-derived components (hereinafter referred to as the "bio-ratio") while maintaining the physical properties of conventionally known polyamides, it is preferable to include PA56, PA510, PA106, or PA1010 in the structural units.
[0019] A particularly preferred structural unit of the copolyamide resin according to an embodiment of the present invention is represented by the following formula: The copolyamide resin may contain at least a portion of the structural units represented by these formulas, or may consist of these structural units.
[0020] The copolyamide resin according to an embodiment of the present invention is a polyamide resin having at least two types of structural units [A] and [B]. The present invention is based in part on the discovery that copolymers having two or more types of structural units exhibit superior physical properties compared to resins alone or simple mixtures of these units. Copolymers form polymers with different sequences depending on the polymerization method, and may be either block copolymers or random copolymers. The copolyamide resin of this embodiment is preferably a random copolymer from the viewpoint of obtaining a desirable melting point and crystallization temperature. A block copolymer is a copolymer in which repeating units with two or more different structures are linked together. Generally, it is obtained by polymerizing a monomer from which a certain structural unit is derived alone, followed by the addition of a different type of monomer and further polymerization. A random copolymer is a copolymer in which the structural units are arranged in a random manner. A copolyamide resin obtained by mixing and polymerizing the components from which the structural units are derived in the monomer state is usually a random copolymer. Copolyamides obtained by preparing multiple types of salts of diamines and dicarboxylic acids as raw materials and then mixing and polymerizing these also usually result in random copolymers. Block copolymers or random copolymers can be confirmed by nuclear magnetic resonance spectroscopy. 13 This can be confirmed by checking the bonding probability of each component from a C-NMR spectrum.
[0021] The content ratio of the structural units [A] and [B] is not particularly limited, but it is preferable that the structural unit [A] is contained in the range of 50% by mass to 95% by mass based on the entire copolymerized polyamide resin.
[0022] The copolyamide resin according to an embodiment of the present invention is preferably designed to have a high bio-derived component content, i.e., a high bio-ratio, within a range that does not impair the properties of the resulting copolyamide resin. The bio-ratio may be any ratio as long as it satisfies the standards set for each product in regulations such as the Act on Promotion of Procurement of Environmental Goods and Services by the State (Green Purchasing Act), but it is preferable that the weight ratio of the raw materials be 25% or more of bio-derived components, and more preferably 50% or more of bio-derived components. A copolyamide resin with a bio-derived component ratio close to 100% is even more preferable, and it is most preferable that the copolyamide resin be obtained solely from bio-derived components, provided that the functions and properties of the resulting copolyamide resin are not impaired.
[0023] The copolyamide resin of the present invention may contain structural units other than the above structural units, as long as the properties of the resulting copolyamide resin are not impaired. Components from which such structural units are derived may be non-bio-derived components, such as lactams, aminocarboxylic acids, non-bio-derived diamines, non-bio-derived dicarboxylic acids, monoamines, or monocarboxylic acids. Examples of lactams include enantholactam, undecane lactam, α-pyrrolidone, and α-piperidone. Examples of aminocarboxylic acids include 7-aminoheptanoic acid, 9-aminononanoic acid, and 11-aminoundecanoic acid. Examples of diamines include aliphatic diamines such as ethylenediamine, tetramethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, and 2,2,4 / 2,4,4-trimethylhexamethylenediamine; alicyclic diamines such as cyclohexyldiamine, bis(4-aminocyclohexyl)methane, bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, (3-methyl-4-aminocyclohexyl)propane, 1,3- / 1,4-bisaminomethylcyclohexane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, and norbornanedimethyleneamine; and the like. Examples of dicarboxylic acids include dicarboxylic acids with a small number of carbon atoms, such as oxalic acid, malonic acid, succinic acid, and glutaric acid; long-chain aliphatic dicarboxylic acids, such as tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosanedioic acid; and alicyclic dicarboxylic acids, such as 1,3- / 1,4-cyclohexanedicarboxylic acid, dicyclohexanemethane-4,4'-dicarboxylic acid, and norbornanedicarboxylic acid.Examples of monoamines include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, 2-ethylhexylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, octadecylamine, octadecyleneamine, eicosylamine, and docosylamine; alicyclic monoamines such as cyclohexylamine and methylcyclohexylamine; benzylamine, β-phenylamine, and the like. aromatic monoamines such as N,N-dimethylamine, N,N-diethylamine, N,N-dipropylamine, N,N-dibutylamine, N,N-dihexylamine, N,N-dioctylamine, and the like; symmetrical secondary amines such as N-methyl-N-ethylamine, N-methyl-N-butylamine, N-methyl-N-dodecylamine, N-methyl-N-octadecylamine, N-ethyl-N-hexadecylamine, N-ethyl-N-octadecylamine, N-propyl-N-hexadecylamine, N-propyl-N-benzylamine, and the like. Examples of monocarboxylic acids include aliphatic monocarboxylic acids such as monoacetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, capric acid, pelargonic acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, myristoleic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, arachic acid, behenic acid, and erucic acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid and methylcyclohexanecarboxylic acid; and aromatic monocarboxylic acids such as benzoic acid, toluic acid, ethylbenzoic acid, and phenylacetic acid.
[0024] The amount of each component of the copolymerized polyamide resin of the present invention corresponds to the amount of each component charged during the production of the copolymerized polyamide resin, but can also be determined by measuring the obtained copolymerized polyamide resin directly or after hydrolysis using high performance liquid chromatography, gas chromatography, gas chromatograph / atomic emission detector (GC / AED), gel permeation chromatography, etc. Since the values may differ depending on the measurement method, the amount of each component of the copolymerized polyamide resin described in the specification and claims of this application is defined as the amount determined by measurement using gas chromatograph / atomic emission detector (GC / AED) when determined from the copolymerized polyamide resin.
[0025] The copolymer polyamide resin of this embodiment has a melting point of 145°C or higher and 250°C or lower as measured by differential scanning calorimetry (DSC). The lower limit of the melting point is preferably 147°C or higher, more preferably 150°C or higher. The upper limit of the melting point is preferably 240°C or lower, more preferably 230°C or lower, and even more preferably 220°C or lower. This makes it possible to suppress thermal degradation of the molded product during molding of the copolymer polyamide resin. The melting point of the copolymer polyamide resin as measured by differential scanning calorimetry (DSC) can be increased or decreased depending on the composition ratio, relative viscosity, and molecular weight of each component.
[0026] The copolymer polyamide resin of this embodiment has a crystallization temperature of 90°C or higher and 195°C or lower as measured by differential scanning calorimetry (DSC). The lower limit of the crystallization temperature is preferably 95°C or higher, more preferably 100°C or higher. The upper limit of the crystallization temperature is preferably 185°C or lower, more preferably 175°C or lower. This is particularly advantageous when a plurality of resins are used in combination to form a film that includes a heating process. For example, when a multilayer film containing the copolymer polyamide resin is formed by an inflation method, curling of the film can be suppressed. The crystallization temperature of the copolymer polyamide resin as measured by differential scanning calorimetry (DSC) can be increased or decreased depending on the composition ratio, relative viscosity, and molecular weight of each component.
[0027] The copolyamide resin of this embodiment has a relative viscosity of 1.5 or more and 5.0 or less. The lower limit of the relative viscosity is preferably 1.6 or more, more preferably 1.8 or more. The upper limit of the relative viscosity is preferably 4.7 or less, more preferably 4.5 or less. When the relative viscosity is equal to or less than the upper limit, extrusion molding is facilitated. When the relative viscosity is equal to or more than the lower limit, extrusion molding is facilitated and the mechanical strength of the molded product is improved. In this specification, ηr (relative viscosity) is the measured value (JIS K 6810) at 25°C of a solution of 1 g / 100 ml of polyamide dissolved in 96% by mass concentrated sulfuric acid as a solvent.
[0028] The copolymerized polyamide resin of this embodiment preferably has a moisture content of 1000 ppm or less, more preferably 800 ppm or less. A moisture content of 1000 ppm or less can suppress foaming during molding. The moisture content can be measured using a known method. As a specific example of the method, a Karl Fischer moisture content meter is used to measure the moisture content in 1 g of polyamide resin by heating and vaporizing it at 215°C under a nitrogen stream.
[0029] Due to the synthesis method of the polyamide resin, the polyamide resin has an amino group or a carboxy group at the molecular terminal. In order to obtain a preferable relative viscosity by increasing the molecular weight of the copolymerized polyamide resin of the present embodiment, the lower limit of the terminal amino group concentration is 1.20 × 10 -5 eq / g or more, and preferably 1.50×10 -5 eq / g or more, and more preferably 1.80×10 -5 eq / g or more, more preferably 2.00 x 10 -5 The upper limit of the terminal amino group concentration is particularly preferably 4.50×10 -5 eq / g or less, and preferably 4.00×10 -5 eq / g or less, more preferably 3.50 × 10 -5eq / g or less. A specific example of a method for measuring the terminal amino group concentration is to dissolve the polyamide resin in a mixed solution of phenol and methanol in a volume ratio of 7:3, and titrate with 0.05 N hydrochloric acid. Furthermore, with regard to the terminal carboxy group concentration of the copolyamide resin of this embodiment, from the viewpoint of suppressing hydrolysis, the lower limit of the terminal carboxy group concentration is 2.00 × 10 -5 eq / g or more, and preferably 2.50×10 -5 eq / g or more, more preferably 2.80×10 -5 eq / g or more, more preferably 3.00 x 10 -5 The upper limit of the terminal carboxyl group concentration is particularly preferably 8.00×10 -5 eq / g or less, and preferably 7.60×10 -5 eq / g or less, more preferably 7.20×10 -5 eq / g or less. A specific example of a method for measuring the terminal carboxyl group concentration is to dissolve the polyamide resin in benzyl alcohol and titrate it with a 0.05N sodium hydroxide solution.
[0030] In order to satisfy the standards of the Food Sanitation Act, the copolymerized polyamide resin of this embodiment preferably has an EC (Extactable Content), which is an index of the amount of hot water soluble components, of 1.0% by mass or less. Furthermore, when caprolactam, a well-known polyamide raw material, is used in combination, in order to satisfy the standards of the Food Sanitation Act, the amount of caprolactam eluted in a 20% ethanol solution as measured by GC-FID is preferably 15 μg / mL or less, more preferably 10 μg / mL or less. A specific example of a method for measuring EC is to boil 10 g of polyamide resin with pure water for 6 hours, vacuum-dry the sample for 16 hours, measure the mass of the dried sample, and use the weight loss as the amount of hot water soluble components (g). EC (%) can be calculated as EC (g) / 10 (g) × 100.
[0031] [Method for Producing Copolymerized Polyamide Resin] The copolymerized polyamide resin of this embodiment can be produced by known polymerization methods such as melt polymerization, solution polymerization, interfacial polymerization, solid-state polymerization, and combinations thereof. Typically, melt polymerization, which is carried out at a temperature higher than the melting point of the resulting copolymerized polyamide resin, is preferably used. Furthermore, the copolymerized polyamide resin of this embodiment can be produced using known polymerization equipment, and can be produced by a batch or continuous method, appropriately combining operations such as normal pressure, reduced pressure, and increased pressure, as needed. For example, the diamine and dicarboxylic acid from which each structural unit is derived can be introduced at once.
[0032] Furthermore, although not particularly limited, since the copolymer polyamide resin of the present embodiment may have a high viscosity, in some cases, in order to avoid difficulty in extracting the resin during polymerization, it is possible to synthesize a copolymer polyamide resin having a lower viscosity than that of the present embodiment by melt polymerization, and then increase the viscosity by solid-state polymerization to obtain the copolymer polyamide resin of the present embodiment.
[0033] The copolymer polyamide resin of this embodiment can contain other components to form a polyamide resin composition, provided that the effects of the present invention are not impaired. A further embodiment of the present invention is a polyamide resin composition containing the copolymer polyamide resin. Examples of other components include plasticizers, heat resistance agents, foaming agents, weathering agents, crystal nucleating agents, crystallization accelerators, mold release agents, lubricants, antistatic agents, flame retardants, flame retardant auxiliaries, and functionality-imparting agents such as pigments and dyes. Polyamide resin compositions containing these other components can be formed into pellets, films, and the like. For the purpose of producing molded articles with various functions and properties, resin compositions can be prepared by further blending the copolymer polyamide resin or polyamide resin composition obtained as described above with the other components described above, polyamide resins other than the copolymer polyamide resin of the present invention, or any resin component other than polyamide resins. The method for producing the polyamide resin composition is not particularly limited. For example, the polyamide resin can be produced by mixing the polyamide resin and other components using a known melt kneader such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader, or a mixing roll. A further embodiment of the present invention is a molded article comprising the polyamide resin composition described above.
[0034] [Uses of Copolymer Polyamide Resin] The copolymer polyamide resin of this embodiment has excellent water resistance and abrasion resistance, and is therefore suitable for use in molded articles, including the molding of various films for food packaging, etc. The copolymer polyamide resin of this embodiment is also suitable for use in inflation molding. In particular, when used in inflation molding to mold a multilayer film containing a layer made of the copolymer polyamide resin of this embodiment and a low-melting-point thermoplastic resin layer, thermal degradation and curling of the film can be suppressed, which is preferable. Another embodiment of the present invention is a molded article containing the copolymer polyamide resin.
[0035] Taking advantage of their excellent properties, molded articles containing copolymerized polyamide resins and compositions thereof are used in a variety of applications, such as electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, sporting goods, etc. Preferred applications for electronic components include, for example, connectors, coils, sensors, LED lamps, sockets, resistors, relay cases, small switches, coil bobbins, capacitors, variable capacitor cases, optical pickup chassis, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, transformer components, parabolic antennas, and computer-related parts. Preferred applications for electrical components include, for example, generators, electric motors, transformers, current transformers, voltage regulators, rectifiers, inverters, relays, power contacts, switches, circuit breakers, knife switches, opposite-pole rods, electrical components, motor cases, notebook computer housings and internal components, CRT display housings and internal components, printer housings and internal components, mobile terminal housings and internal components for mobile phones, mobile personal computers, handheld mobile devices, etc., various gears, various cases, cabinets, etc. Preferred applications for household and office supplies include, for example, VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts, acoustic parts, audio / visual equipment parts such as laser discs (registered trademark), compact discs, and DVDs, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, electronic device housings for personal computers and notebook computers, etc., office computer-related parts, telephone-related parts, facsimile-related parts, copier-related parts, cleaning jigs, motor parts, lighters, typewriters, microscopes, binoculars, cameras, and clocks.Automotive and vehicle-related part applications include, for example, alternator terminals, alternator connectors, IC regulators, light dimmer potentiometer bases, various valves such as exhaust gas valves, various pipes, hoses, and tubes for fuel, cooling, brake, wiper, exhaust, and intake systems, air intake nozzle snorkels, intake manifolds, fuel pumps, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake pad wear sensors, battery peripherals, air conditioner thermostat bases, heating hot air flow control valves, radiator motor brush holders, water pump impellers, turbine vanes, wiper motor-related parts, distributors, starter switches, starter relays, transmission wire harnesses, transmission oil pans, windshield washer nozzles, and air conditioners. It is preferably used in panel switch boards, coils for fuel-related electromagnetic valves, various connectors such as wire harness connectors, SMJ connectors, PCB connectors, door grommet connectors, and fuse connectors, horn terminals, insulating plates for electrical components, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil pans, engine oil filters, ignition device cases, torque control levers, safety belt parts, register blades, washer levers, window regulator handles, window regulator handle knobs, passing light levers, sun visor brackets, instrument panels, airbag peripheral parts, door pads, pillars, console boxes, various motor housings, roof rails, fenders, garnishes, roof panels, hood panels, trunk lids, door mirror stays, spoilers, hood louvers, wheel covers, wheel caps, grill apron cover frames, lamp bezels, door handles, door moldings, rear finishers, and wipers.As building material applications, it is preferably used, for example, in civil engineering building wall, roof, and ceiling material-related parts, window material-related parts, heat insulating material-related parts, flooring material-related parts, seismic isolation and vibration damping material-related parts, lifeline-related parts, etc. As sporting goods applications, it is preferably used, for example, in golf-related goods such as golf clubs and shafts, sports personal protective equipment such as masks, helmets, breast pads, elbow pads, and knee pads for American football, baseball, softball, etc., shoe-related goods such as soles of sports shoes, fishing tackle-related goods such as fishing rods and fishing lines, summer sports related goods such as surfing, winter sports related goods such as skiing and snowboarding, and other indoor and outdoor sports related goods.
[0036] [Polyamide Film] The copolymer polyamide resin of the present invention can be used in a single-layer or multilayer film. In the case of a multilayer film, the copolymer polyamide resin of the present invention may be contained in at least one layer. In addition to a layer containing a copolymer polyamide resin (also simply referred to as a "copolymer polyamide resin layer"), the polyamide film of this embodiment may further include a layer containing a low-melting point thermoplastic resin (also simply referred to as a "low-melting point thermoplastic resin layer" or "thermoplastic resin layer"), a layer containing a resin other than the copolymer polyamide resin layer and the low-melting point thermoplastic resin layer (also simply referred to as an "other resin layer other than the copolymer polyamide resin layer and the low-melting point thermoplastic resin layer," "other resin layer," or "resin layer"), or a layer containing an adhesive or adhesive resin (also simply referred to as an "adhesive or adhesive resin layer" or "adhesive resin layer"). The low-melting point thermoplastic resin layer is preferably the innermost layer.
[0037] The low-melting-point thermoplastic resin layer is a layer that can be heat-sealed to the packaging lid material, and keeping the heat-sealing temperature as low as possible is preferable for production efficiency, so it is preferable to use a low-melting-point thermoplastic resin. Here, low-melting point refers to a melting point of 165°C or less, preferably 160°C or less, and more preferably 150°C or less. Furthermore, the low-melting point preferably refers to a melting point of 100°C or more, and more preferably 120°C or more. Examples of low-melting-point thermoplastic resins contained in the low-melting-point thermoplastic resin layer include ethylene-based resins such as low-density polyethylene, linear low-density polyethylene, ionomers, ethylene-vinyl alcohol copolymers (EVOH), ethylene-acrylic acid copolymers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid ester copolymers, and ethylene-methacrylic acid copolymers, and particularly those with low melting points can be used.
[0038] The layer structure of the polyamide film of this embodiment can include a monolayer film consisting of a copolymer polyamide resin layer alone, a two-layer film consisting of a copolymer polyamide resin layer and a low-melting-point thermoplastic resin layer, a three-layer film consisting of a copolymer polyamide resin layer / (adhesive or adhesive resin layer) / low-melting-point thermoplastic resin layer, at least three layers consisting of a copolymer polyamide resin layer, a low-melting-point thermoplastic resin layer, and a resin layer other than these layers, or at least four layers consisting of a copolymer polyamide resin layer, a thermoplastic resin layer, and (adhesive or adhesive resin layer) and a resin layer other than these layers.Specific examples include a copolymer polyamide resin layer / (adhesive or adhesive resin layer) / resin layer, a copolymer polyamide resin layer / (adhesive or adhesive resin layer) / resin layer / (adhesive or adhesive resin layer) / low-melting-point thermoplastic resin layer, or a resin layer / (adhesive or adhesive resin layer) / copolymer polyamide resin layer / (adhesive or adhesive resin layer) / low-melting-point thermoplastic resin layer, and the like, and the adhesive or adhesive resin layer can be provided as needed.
[0039] In the polyamide-based film of this embodiment, other resin layers besides the copolymer polyamide resin layer and the low-melting point thermoplastic resin layer include layers containing ethylene-based resins such as low-density polyethylene, linear low-density polyethylene, ionomers, ethylene-vinyl alcohol copolymer (EVOH), ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-methacrylic acid copolymer, polyolefins such as polypropylene, polyesters, polyvinyl alcohol, polyamides, polyamide elastomers, and films thereof. Biomass plastics such as polylactic acid (PLA) and polyhydroxyalkanoates (PHA) can also be used.
[0040] The adhesive resin layer may be made of an acid-modified polyolefin resin such as acid-modified polyethylene grafted with at least one monomer selected from unsaturated carboxylic acids or derivatives thereof.
[0041] The polyamide film of this embodiment, the copolymer polyamide resin layer constituting this film and the copolymer polyamide resin or composition thereof constituting this layer, the thermoplastic resin layer and the thermoplastic resin or composition thereof constituting this layer, the other resin layer and the other resin or composition thereof constituting this layer, the adhesive resin layer and the adhesive resin or composition thereof constituting this layer, etc. may contain heat stabilizers, antioxidants, ultraviolet absorbers, weathering agents, lubricants, fillers, nucleating agents, plasticizers, foaming agents, antiblocking agents, antifogging agents, flame retardants, dyes, pigments, stabilizers, coupling agents, etc., within ranges that do not impair the properties of the resulting film, resin, etc.
[0042] The thickness of the layers of the polyamide-based film of this embodiment is as follows: (1) When a copolymer polyamide resin layer is used alone, the copolymer polyamide resin layer is preferably in the range of 10 to 100 μm, and (2) When a film has two layers, a copolymer polyamide resin layer and a thermoplastic resin layer, or three or more layers, a copolymer polyamide resin layer / (adhesive or adhesive resin layer) / thermoplastic resin layer, the copolymer polyamide resin layer is preferably in the range of 2 to 80 μm, and the thermoplastic resin layer is preferably in the range of 8 to 120 μm. The thickness of the adhesive or adhesive resin can be appropriately selected depending on the purpose.
[0043] [Film Production] In the polyamide-based film of this embodiment, the copolymerized polyamide resin layer and the thermoplastic resin layer may be laminated directly by coextrusion, lamination, or the like, or may be laminated via an adhesive or adhesive resin layer. Coextrusion is preferred due to its excellent productivity. The polyamide-based film of this embodiment can be produced by a molding method such as a T-die molding method, an air-cooled inflation molding method, a water-cooled inflation molding method, or a triple bubble molding method. When the polyamide-based film of this embodiment is produced by coextrusion, for example, a coextrusion T-die molding method in which a copolymerized polyamide resin or a composition thereof, a thermoplastic resin or a composition thereof, etc. are melted in separate extruders and continuously extruded through a T-die and cooled with a casting roll to form a film; a coextrusion air-cooled inflation molding method in which the resins are continuously extruded through a circular die and cooled by air; or a coextrusion water-cooled inflation molding method in which the resins are continuously extruded through a circular die and cooled by contact with water, etc., to produce a substantially unoriented unstretched film. That is, the polyamide film in one embodiment is an unstretched film.
[0044] Among these, air-cooled inflation molding and water-cooled inflation molding (also simply referred to as "inflation molding" or "inflation molding") require simple equipment and allow easy film width adjustment by simply adjusting the blow-up ratio, resulting in good workability and high productivity for film production. When used in air-cooled inflation molding and water-cooled inflation molding, the copolymerized polyamide resin of the present invention can suppress film curling. Furthermore, the polyamide film of the present invention can suppress curling when produced by coextrusion inflation molding. In particular, when the polyamide film is a multilayer film containing a copolymerized polyamide resin layer and a low-melting-point thermoplastic resin layer, thermal degradation and curling of the film can be suppressed, which is preferable. That is, in a preferred embodiment, the copolymerized polyamide resin of the present invention can be used in inflation molding. Furthermore, in a preferred embodiment, the polyamide film is used for inflation molding.
[0045] The conditions for forming an inflation-molded film are not particularly limited, but the resin temperature is preferably above the melting point of the raw resin used but less than 300°C. In the present invention, because the melting point of the copolymerized polyamide resin is low, the resin temperature can be, for example, 160°C to 250°C, preferably 160°C to 200°C. The blow-up ratio (also referred to as the blow ratio) refers to the ratio of the maximum bubble diameter to the die diameter, and is preferably 1.1 to 3.0, more preferably 1.2 to 2.5. The take-up speed is determined by the film thickness, width, and extrusion rate, and can be adjusted within a range that maintains film formation stability. Generally, the take-up speed is preferably 1 to 150 m / min, more preferably 5 to 100 m / min.
[0046] [Biaxially Stretched Film] The polyamide film of the present invention may be a biaxially stretched film. A biaxially stretched film is produced by stretching an unstretched film biaxially in the machine direction (MD) of film formation and in the direction perpendicular to the machine direction (TD), followed by heat treatment under specific conditions. The stretching method is not particularly limited, but examples thereof include sequential biaxial stretching, simultaneous biaxial stretching, and tubular simultaneous biaxial stretching.
[0047] Furthermore, the polyamide film of the present embodiment can be subjected to surface treatments such as corona discharge treatment, plasma treatment, flame treatment, acid treatment, etc., in order to improve printability, lamination, and adhesive application properties. After such treatments are performed as necessary, the film can be used for the intended purpose through secondary processing steps such as printing, lamination, adhesive application, and heat sealing.
[0048] [Applications of the film] The polyamide film of this embodiment has excellent water resistance and abrasion resistance, and can be used as a food packaging film. The polyamide film of this embodiment is also used as an inflation-molded film. In particular, a multilayer polyamide film including a copolymer polyamide resin layer and a low-melting-point thermoplastic resin layer is preferred because it can suppress thermal degradation and curling of the film.
[0049] [Production of a three-layer film including a copolymer polyamide resin layer and a low-melting point thermoplastic resin layer] Although not particularly limited, for example, using a three-type three-layer coextrusion air-cooled multilayer inflation molding machine (die diameter 100 mmφ) manufactured by Dr. Colin Co., Ltd., the copolymer polyamide resin of the present invention is used as the first layer (outermost layer), an adhesive resin layer as the second layer, and a low-melting point thermoplastic resin layer as the third layer (innermost layer), under conditions of an ambient temperature of 25 ° C, a resin temperature of 160 ° C to 250 ° C, and a blow-up ratio of 1.53, a three-layer film including a copolymer polyamide resin layer and a low-melting point thermoplastic resin layer with a total film thickness of 100 μm (first layer: 30 μm, second layer: 5 μm, third layer: 65 μm) can be produced. During film production, the resin temperature must be set above the melting point of the copolymer polyamide resin; when using conventional polyamide resins, it was necessary to set it to at least 230 ° C. Therefore, during the production of a multilayer film, deterioration of the adhesive resin layer and the low-melting-point thermoplastic resin layer occurs. On the other hand, by using the copolymer polyamide resin of the present invention, the resin temperature can be set lower than conventionally, for example, to 160°C to 250°C, preferably 160°C to 200°C, and therefore deterioration of the adhesive resin layer and the low-melting-point thermoplastic resin layer can be suppressed.
[0050] [Polyamide Monofilament] Yet another aspect of the present invention is a monofilament comprising a copolymerized polyamide resin or a polyamide resin composition. The diameter of the monofilament is not particularly limited, but is preferably 0.5 to 20 mm, more preferably 1 to 5 mm. The monofilament may be a continuous fiber or a staple fiber.
[0051] [Production of Monofilaments] Monofilaments can be obtained by known production methods using copolymerized polyamide resins or polyamide resin compositions. Examples of methods for producing monofilaments include melting copolymerized polyamide resin pellets in an extruder or the like, extruding them through a spinning nozzle, and cooling them in a refrigerant bath containing water, trichloroethylene, or the like to produce undrawn yarns. In this case, the distance between the filament outlet of the spinning nozzle and the refrigerant liquid level is preferably maintained at approximately 10 to 300 mm.
[0052] The undrawn yarn may be further drawn and heat-set. Here, two-stage drawing, in which drawing is performed in two stages, is preferred. In the first stage of the two-stage drawing, the undrawn yarn is preferably drawn 2 to 5 times, more preferably 3 to 4 times, in steam or hot water. If the draw ratio is within this range, the knot strength tends to be further improved.
[0053] When stretching is performed in water vapor, the temperature range is preferably 95 to 120° C., more preferably 100 to 110° C. When the temperature of the water vapor is within this temperature range, the knot strength and transparency of the obtained monofilament tend to be further improved.
[0054] When stretching is performed in hot water, the temperature of the hot water is preferably 50 to 95° C., more preferably 60 to 90° C. When the temperature of the hot water is within this range, the knot strength and transparency of the obtained monofilament tend to be further improved.
[0055] In the second-stage drawing, the monofilament is preferably drawn 1.1 to 2.5 times, more preferably 1.2 to 2.5 times, in a gas atmosphere. The gas is not particularly limited, and examples thereof include inert gases such as helium, nitrogen, and argon, and air. The temperature of the gas atmosphere in the second-stage drawing is preferably 120 to 300°C, more preferably 180 to 250°C. When the second-stage drawing is performed within the above-mentioned temperature range and draw ratio, the knot strength and transparency of the resulting monofilament tend to be further improved.
[0056] The two-stage drawn monofilament is preferably heat-set. The two-stage drawn monofilament can be heat-set in a gas atmosphere at preferably 160 to 350°C, more preferably 160 to 320°C, while being subjected to a 0 to 10% relaxation treatment. When the temperature is within this range, the knot strength tends to be further improved.
[0057] In the above two-stage drawing and heat treatment, the total draw ratio is preferably in the range of 4.0 to 7.0 times, more preferably 4.5 to 6.5 times, and even more preferably 5.5 to 6.0 times.
[0058] [Uses of Monofilaments] Monofilaments have low water absorption and excellent abrasion resistance, and therefore can be used as filaments, multifilaments, nets, and other structures for applications in fishing, industry, clothing, medicine, etc. Furthermore, monofilaments can be used in a variety of applications, including electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, and sporting goods, which are examples of applications for molded products.
[0059] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0060] The various physical properties of the copolymerized polyamide resins or polyamide resins, and mixtures thereof, in the Examples and Comparative Examples were measured by the following methods: (1) Melting point (Tm): Using a DSC7020 model manufactured by Hitachi High-Tech Science Corporation, the polyamide resins of the Examples and Comparative Examples were heated to 300°C at a heating rate of 10°C / min under a nitrogen gas atmosphere, held at that temperature for 1 minute, cooled to 30°C at a rate of 10°C / min, and immediately thereafter heated again to 300°C at 10°C / min. The heating temperature at which the endothermic peak obtained during the reheating process was reached was taken as the melting point (Tm). (2) Crystallization temperature (Tc): Using a Hitachi High-Tech Science DSC7020 model, the polyamide resins of the Examples and Comparative Examples were heated to 300°C at a heating rate of 10°C / min under a nitrogen gas atmosphere, held at that temperature for 1 minute, and then cooled to 30°C at a rate of 10°C / min. The cooling temperature at which the exothermic peak obtained during the cooling process was reached was taken as the crystallization temperature (Tc). (3) Heat of fusion (ΔH): DSC measurement was performed using the same method as for the melting point, and the area value of the endothermic peak portion of the DSC chart obtained during the reheating process was taken as the heat of fusion ΔH (unit: J / g). If ΔH was 40 J / g or less, the molded article was judged to have low crystallinity and excellent transparency. (4) Equilibrium Water Absorption: Using polyamide resin pellets from the Examples and Comparative Examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used. The pellets were preheated at a temperature of melting point + 30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cooled and pressed at 30°C and 5 MPa for 3 minutes to produce unstretched polyamide sheets measuring 20 mm x 80 mm x 2 mm. The resulting sheets were vacuum-dried at 80°C for 48 hours, and their masses were measured. The sheets were then immersed in water at 23°C for 800 hours, and the surface moisture of the removed sheets was lightly absorbed with a cloth, after which their masses were measured. The equilibrium water absorption was calculated from the masses of the sheets before and after immersion in water using the following formula: Equilibrium Water Absorption = [(Sheet Mass After Immersion in Water - Sheet Mass Before Immersion in Water) / Sheet Mass Before Immersion in Water] x 100. An equilibrium water absorption of 15.0% or less was considered to be low absorbency and excellent water resistance.(5) Abrasion volume: Using polyamide resin pellets from the examples and comparative examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used. The pellets were preheated at a temperature of melting point +30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cooled and pressed at 30°C and 5 MPa for 3 minutes to produce two 45 mm x 45 mm x 1 mm unstretched polyamide sheets. The resulting sheets were vacuum-dried at 80°C for 48 hours and sealed in an aluminum bag. One of the two sheets was used as a sample for the abrasion test, and the other was used as a sample for measuring water absorption to correct the water absorption of the sample (dried sheet) during the abrasion test. First, the aluminum bag was opened, and the masses of the two samples were measured. G (garnet)-50 abrasive paper cut to a length of 157 mm and a width of 12 mm was attached to the abrasion wheel of a reciprocating flat abrasion tester manufactured by Suga Test Instruments Co., Ltd., and an abrasion test was performed on the dried sheets under conditions of a load of 3000 g, a stroke of 30 mm, and 120 reciprocations. After the test, resin powder generated on the sheet due to abrasion was brushed off, and the mass of the sample was measured. At almost the same time, the mass of the sample for measuring water absorption was measured. The mass obtained by adding the mass increase (apparent water absorption) of the sample for measuring water absorption to the difference in mass of the sample for abrasion test before and after the abrasion test was taken as the abrasion amount. An abrasion amount of 11.8 mg or less was determined to be excellent in abrasion resistance.
[0061] (Synthesis of Nylon 56 Salt) 32.42 kg of adipic acid and 273 kg of 2-propanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the adipic acid, after which 22.67 kg of 1,5-pentamethylenediamine was slowly added over 71 minutes. Heat of neutralization and heat of crystallization were generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,5-pentamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 56 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 54.8 kg of nylon 56 salt.
[0062] (Synthesis of Nylon 510 Salt) 24.27 kg of sebacic acid and 184 kg of 2-propanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the sebacic acid. 12.27 kg of 1,5-pentamethylenediamine was then slowly added over 65 minutes. Heat of neutralization and heat of crystallization were generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,5-pentamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 510 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 36.3 kg of nylon 510 salt.
[0063] (Synthesis of Nylon 610 Salt) 141.5 g of sebacic acid and 1,000 g of 2-propanol were placed in a 5 L reaction vessel and heated to 40°C to dissolve the sebacic acid. 81.3 g of 1,6-hexamethylenediamine was then slowly added over 30 minutes. Heat of neutralization and crystallization was generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,6-hexamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 610 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 220 g of nylon 610 salt.
[0064] (Synthesis of Nylon 106 Salt) 102.3 g of adipic acid and 1,000 g of 2-propanol were placed in a 5 L reaction vessel and heated to 40°C to dissolve the adipic acid. 120.6 g of 1,10-decamethylenediamine was then slowly added over 30 minutes. Heat of neutralization and crystallization was generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,10-decamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 106 salt was collected as a cake and then dried under reduced pressure at 60°C for 48 hours to obtain 218 g of nylon 106 salt.
[0065] (Synthesis of Nylon 1010 Salt) 18.78 kg of sebacic acid and 175 kg of methanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the sebacic acid. Then, 16.00 kg of 1,10-decanediamine was slowly added over 63 minutes. Heat of neutralization and heat of crystallization were generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,10-decanediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 1010 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 33.9 kg of nylon 1010 salt.
[0066] (Production of Copolymer Polyamide Resin) (Example 1) A 1 L polymerization vessel was charged with 150 g of nylon 56 salt, 100 g of nylon 1010 salt, and 50 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The temperature inside the polymerization vessel was raised to 250°C, and the pressure was released to atmospheric pressure over 40 minutes. After pressure release, polymerization was carried out for 2 hours under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1 MPa. After pressurization, the vessel was extracted as a strand and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain a copolymer polyamide resin. The composition (feed ratio) and physical properties of the copolymer polyamide resin of Example 1 are shown in Table 1. The randomness of the copolymer polyamide resin of Example 1 was also measured. 13 When confirmed by C-NMR measurement, it was a random copolymer.
[0067] A 1-L polymerization vessel was charged with 225 g of nylon 510 salt, 25 g of nylon 1010 salt, and 50 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 1 to obtain a copolyamide resin of Example 2. The composition (feed ratio) and physical properties of the copolyamide resin of Example 2 are shown in Table 1.
[0068] A 1-L polymerization vessel was charged with 175 g of nylon 510 salt, 75 g of nylon 1010 salt, and 50 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 1 to obtain a copolyamide resin of Example 3. The composition (feed ratio) and physical properties of the copolyamide resin of Example 3 are shown in Table 1.
[0069] Example 4 A 1-L polymerization vessel was charged with 225 g of nylon 56 salt, 25 g of nylon 1010 salt, and 50 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while the temperature inside the polymerization vessel was raised to 280°C. After pressure release, polymerization was carried out for 3 hours under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1 MPa. After pressurization, the vessel was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain a copolymerized polyamide resin. The composition (feed ratio) and physical properties of the copolymerized polyamide resin of Example 4 are shown in Table 1.
[0070] Example 5 A 1-L polymerization vessel was charged with 175 g of nylon 106 salt, 75 g of nylon 1010 salt, and 50 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while the temperature inside the polymerization vessel was raised to 280°C. After pressure release, polymerization was carried out for 3 hours under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1 MPa. After pressurization, the vessel was extracted as a strand and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain a copolymer polyamide resin. The composition (feed ratio) and physical properties of the copolymer polyamide resin of Example 5 are shown in Table 1.
[0071] Comparative Example 1 A 1-L polymerization vessel was charged with 205 g of 6-aminocaproic acid and 93.75 g of a nylon 66 salt aqueous solution (48% by mass aqueous solution), and polymerization was carried out in the same manner as in Example 1 to obtain a copolymerized polyamide resin of Comparative Example 1. The composition (charge ratio) and physical properties of the copolymerized polyamide resin of Comparative Example 1 are shown in Table 1.
[0072] (Comparative Example 5) A 1 L polymerization vessel was charged with 175 g of nylon 56 salt and 156.25 g of an aqueous nylon 66 salt solution (48 mass % aqueous solution), and polymerization was carried out in the same manner as in Example 4 to obtain a copolyamide resin of Comparative Example 5. The composition (feed ratio) and physical properties of the copolyamide resin of Comparative Example 5 are shown in Table 1.
[0073] (Production of homopolyamide resin) (Comparative Example 2) A 1 L polymerization vessel was charged with 250 g of nylon 56 salt and 50 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 4 to obtain a homopolyamide resin. The composition (charge ratio) and physical properties of the homopolyamide resin of Comparative Example 2 are shown in Table 1.
[0074] (Comparative Example 3) A 1 L polymerization vessel was charged with 250 g of nylon 510 salt and 50 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 1 to obtain a homopolyamide resin of Comparative Example 3. The composition (charge ratio) and physical properties of the homopolyamide resin of Comparative Example 3 are shown in Table 1.
[0075] Comparative Example 4 A 1-L polymerization vessel was charged with 250 g of nylon 1010 salt and 50 g of degassed ion-exchanged water. The atmosphere inside the vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while the temperature inside the polymerization vessel was raised to 250°C. After pressure release, polymerization was carried out for 3 hours under a nitrogen stream of 200 mL / min. The stirrer was then stopped, and nitrogen was introduced to pressurize the vessel to 1 MPa. After pressurization, the vessel was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain a homopolyamide resin of Comparative Example 4. The composition (feed ratio) and physical properties of the homopolyamide resin of Comparative Example 4 are shown in Table 1.
[0076] Comparative Example 6 A 1-L polymerization vessel was charged with 175 g of nylon 510 salt, 75 g of nylon 610 salt, and 50 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The temperature inside the polymerization vessel was raised to 250°C, and the pressure was released to atmospheric pressure over 40 minutes. After pressure release, polymerization was carried out for 3 hours under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1 MPa. After pressurization, the vessel was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain a copolymerized polyamide resin of Comparative Example 6. The composition (feed ratio) and physical properties of the copolymerized polyamide resin of Comparative Example 6 are shown in Table 1.
[0077] (Preparation of Polyamide Blend) (Comparative Example 7) Comparative Examples 7 to 10 were prepared as a blend of two types of homopolyamides, rather than as a polyamide copolymer. PA56 prepared under the same conditions as in Comparative Example 2 and PA1010 prepared under the same conditions as in Comparative Example 4 were blended in a weight ratio of 60 / 40 to obtain the polyamide blend of Comparative Example 7. The composition and physical properties of the polyamide blend of Comparative Example 7 are shown in Table 1.
[0078] (Comparative Example 8) A polyamide mixture of Comparative Example 8 was obtained in the same manner as in Comparative Example 7, except that the mixing ratio of PA56 and PA1010 was changed to 30 / 70 (weight ratio). The composition and physical properties of the polyamide mixture of Comparative Example 8 are shown in Table 1.
[0079] (Comparative Example 9) PA510 prepared under the same conditions as in Comparative Example 3 and PA1010 prepared under the same conditions as in Comparative Example 4 were mixed in a weight ratio of 70 / 30 to obtain a polyamide mixture of Comparative Example 9. The composition and physical properties of the polyamide mixture of Comparative Example 9 are shown in Table 1.
[0080] (Comparative Example 10) A polyamide mixture of Comparative Example 10 was obtained in the same manner as in Comparative Example 9, except that the mixing ratio of PA510 and PA1010 was changed to 30 / 70 (weight ratio). The composition and physical properties of the polyamide mixture of Comparative Example 10 are shown in Table 1.
[0081] The equilibrium water absorption and abrasion measured for the polyamides of the Examples and Comparative Examples are shown in Table 1.
[0082]
[0083] As shown in Table 1, the copolyamide resin of the present invention exhibited high water resistance and abrasion resistance while retaining thermal properties equivalent to those of conventional polyamide resins containing components not derived from biomass feedstocks, such as PA6, PA66, and PA610. In particular, the copolyamide resin of the present invention had a more pronounced effect in abrasion resistance than simple mixtures or copolymers of a single composition.
[0084] The copolyamide resin of the present invention is highly environmentally friendly due to its high biomass content and has properties equivalent to or even superior to those of conventional polyamide resins, and can therefore be used as a substitute for conventional polyamide resins in electronic components, electrical components, household goods, office supplies, automotive and vehicle-related parts, building materials, sporting goods, and other applications, as well as in films for packaging and other uses.
Claims
1. A copolymer polyamide resin (excluding polyamide 56 / 510) having at least two types of structural units derived from equimolar amounts of a reaction product of at least one selected from pentamethylenediamine or decamethylenediamine with a dicarboxylic acid having 6 to 13 carbon atoms.
2. The copolymer polyamide resin according to claim 1, comprising at least one selected from the group consisting of structural units derived from an equimolar reactant of pentamethylenediamine and adipic acid, structural units derived from an equimolar reactant of pentamethylenediamine and sebacic acid, structural units derived from an equimolar reactant of decamethylenediamine and adipic acid, structural units derived from an equimolar reactant of decamethylenediamine and sebacic acid, and structural units derived from an equimolar reactant of a mixture of pentamethylenediamine and decamethylenediamine with sebacic acid.
3. The copolymer polyamide resin according to claim 1, having as the structural unit [A] a structural unit derived from an equimolar reaction product of pentamethylenediamine and adipic acid, or a structural unit derived from an equimolar reaction product of pentamethylenediamine and sebacic acid.
4. The copolymer polyamide resin according to claim 3, wherein the structural unit [A] is contained in an amount of 50% by mass to 95% by mass based on the entire copolymer polyamide resin.
5. The copolyamide resin according to claim 1, wherein the melting point of the copolyamide resin as measured by DSC is 145 to 250°C.
6. The copolyamide resin according to claim 1, wherein the crystallization temperature of the copolyamide resin as measured by DSC is 90 to 195°C.
7. A polyamide resin composition comprising the copolymer polyamide resin according to any one of claims 1 to 6.
8. A molded article comprising the copolymer polyamide resin according to any one of claims 1 to 6.
9. A film comprising the copolymer polyamide resin according to any one of claims 1 to 6.
10. A monofilament comprising the copolymer polyamide resin according to any one of claims 1 to 6.
Citation Information
Patent Citations
Polyamide and production method and application thereof
CN104163917A
Polyamide hot melt adhesive and preparation method thereof
CN113214474A
Preparation method of low-melting-point nylon fiber
CN114108122A
Polyamide material for industrial yarn, preparation method of polyamide material and fiber
CN114989422A
High-temperature-resistant semi-aromatic copolyamide as well as preparation method, composition and molded product thereof
CN115612095A