Cellulose porous body, and transparent insulating material

By integrating fish-derived antifreeze proteins and nanofibers with controlled freeze-drying, the cellulose porous material achieves high transparency and heat insulation, addressing the transparency and agglomeration issues in existing cellulose porous materials for advanced applications.

WO2024219357A1PCT designated stage expired Publication Date: 2024-10-24FUJIFILM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014979
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing cellulose porous materials produced by freeze-drying methods lack sufficient transparency due to agglomeration and ice crystal growth, limiting their applications in transparent heat insulation.

Method used

Incorporating antifreeze proteins derived from fish with a thermal hysteresis of 0.4°C or higher and cellulose nanofibers with a fiber diameter of 40 nm or less, along with a controlled freeze-drying process, to suppress ice crystal growth and enhance transparency.

Benefits of technology

The resulting cellulose porous material achieves high transparency and effective heat insulation, suitable for applications such as transparent windows and laminated glass, with transmittance exceeding 70% and improved thermal hysteresis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a cellulose porous body having high transparency. A cellulose porous body according to the present invention contains cellulose nanofibers and an antifreeze agent, and has a fiber diameter of 40 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Porous cellulose, transparent insulation material

[0001] The present invention relates to a porous cellulose body. The present invention also relates to a transparent heat insulating agent containing the porous cellulose body.

[0002] Cellulose nanofibers (hereinafter also referred to as "CNF") are fibers produced from pulp and other cellulose-based raw materials through pulp milling and chemical processing. CNF is lightweight and strong, and is therefore expected to be used in a variety of applications. CNF is also a natural material derived from plants or living organisms, and is attracting attention for its low environmental impact upon disposal. Porous materials have also been used in a variety of applications due to their structure, specific surface area, and other factors. Here, porous cellulose materials containing CNF are expected to have the lightweight and high strength properties of CNF.

[0003] In the production of porous cellulose materials containing CNF, a freeze-drying process is sometimes applied to prevent aggregation of CNF. For example, Patent Document 1 discloses a method for producing a porous cellulose material, in which a mixed solvent of water and an organic solvent, in which the concentration of the organic solvent in the mixed solvent is 2 to 40 mass %, is used as a dispersion medium for CNF, and the CNF dispersion is freeze-dried.

[0004] Patent No. 5827178

[0005] Depending on the application of a CNF-containing porous cellulose material, transparency may be required. The present inventors have studied a porous cellulose material produced by the method described in Patent Document 1 and found that the transparency is insufficient and further improvement is necessary.

[0006] Therefore, an object of the present invention is to provide a highly transparent porous cellulose body. Another object of the present invention is to provide a transparent heat insulating material.

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, they have found that the above problems can be solved by the following configuration.

[0008] [1] A porous cellulose body comprising cellulose nanofibers and an antifreeze agent, the fiber diameter being 40 nm or less. [2] The porous cellulose body according to [1], wherein the antifreeze agent is an antifreeze protein. [3] The porous cellulose body according to [2], wherein the antifreeze protein is derived from fish. [4] The porous cellulose body according to any one of [1] to [3], wherein the thermal hysteresis of the antifreeze agent is 0.4°C or more. [5] The porous cellulose body according to any one of [1] to [4], wherein the fiber diameter is 4 to 30 nm. [6] The porous cellulose body according to any one of [1] to [5], wherein the content of the antifreeze agent is 10 to 30 mass% relative to the total mass of the porous cellulose body. [7] A transparent heat insulating material comprising the porous cellulose body according to any one of [1] to [6].

[0009] According to the present invention, a highly transparent porous cellulose body can be provided, and a transparent heat insulating material can be provided.

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0011] The meaning of each description in this specification is as follows: In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] <Porous cellulose body> The porous cellulose body of the present invention contains cellulose nanofibers (CNFs) and an antifreeze agent, and has a fiber diameter of 40 nm or less. Since the porous cellulose body of the present invention has a fiber diameter of 40 nm or less, it is thought that the porous cellulose body of the present invention is likely to have little light scattering and excellent transparency.

[0013] In this specification, the fiber diameter of the porous cellulose body is measured by small angle X-ray scattering (SAXS). Specifically, X-rays are first incident on the porous cellulose body to obtain a pre-treatment scattering curve. The scattering intensity in this pre-treatment scattering curve is normalized based on the intensity of the incident X-rays transmitted through the beam stopper to obtain a normalized scattering curve for the porous cellulose body. A blank measurement is also performed, and a normalized scattering curve for the medium (air) is obtained in the same manner. The scattering curve I(q) for the fibers constituting the porous cellulose body is obtained by subtracting the normalized scattering curve for the medium from the normalized scattering curve for the porous cellulose body. Here, q is a scattering vector calculated from the following equation using the scattering angle 2θ. q = 4 * π * (sin(θ)) / λ (π: pi, 2θ: scattering angle [rad], λ: wavelength of X-rays [nm]) When the scattering curve I(q) of the obtained porous cellulose material is plotted on a double logarithmic graph, a region where the slope is linear appears. For this region, a Guinier plot for the cross section is created, and the scattering intensity average fiber diameter Dc is calculated using the following formula: q * I(q) ∝ exp(-(Dc 2 * q 2 ) / 16) The scattering intensity average fiber diameter Dc obtained by the above formula is the fiber diameter of the porous cellulose material.

[0014] As described above, in the present invention, the fiber diameter of the porous cellulose body is 40 nm or less, and is preferably 4 to 30 nm, more preferably 10 to 25 nm, in order to obtain a porous cellulose body with superior transparency. The fiber diameter of the porous cellulose body can be adjusted, for example, by the fiber diameter and type of CNF used, the type of antifreeze agent contained therein, the method for forming the porous cellulose body, etc.

[0015] The CNF and antifreeze agent contained in the porous cellulose material, as well as other components that may be contained therein, will be described below.

[0016] [Cellulose Nanofibers] The cellulose nanofibers (CNFs) contained in the porous cellulose material of the present invention are not particularly limited, and known CNFs can be used. CNFs refer to cellulose molecular chains formed into bundles of two or more. The term "cellulose molecular chains formed into bundles of two or more" refers to a state in which two or more cellulose molecular chains are aggregated to form an aggregate called a microfibril. CNFs are generally obtained by processing plant-derived fibers. The raw material for CNF is not particularly limited, and examples include plant-derived fibers contained in wood, bamboo, hemp, jute, kenaf, cotton, beet pulp, potato pulp, agricultural waste, cloth, and paper. These raw materials may be used alone or in combination of two or more.

[0017] CNF may be chemically modified, and chemically modified CNF is preferred because it is easier to increase the permeability of the porous cellulose body. In chemically modified CNF, some or all of the groups in the cellulose molecular chain are modified by chemical treatment. For example, the cellulose molecular chain in chemically modified CNF may be oxidized to aldehyde groups, carboxyl groups, or the like, or oxidized to aldehyde groups, carboxyl groups, or the like, or hydroxyl groups other than the C6 position, or esterified CNF such as nitrate esters, acetate esters, or phosphate esters, or etherified CNF such as methyl ethers, hydroxypropyl ethers, or carboxymethyl ethers, or substituted with other functional groups. More specifically, examples of groups that can be introduced by chemical modification include a carboxyl group, an acetyl group, a sulfate group, a sulfonate group, an acryloyl group, a methacryloyl group, a propionyl group, a propioloyl group, a butyryl group, a 2-butyryl group, a pentanoyl group, a hexanoyl group, a heptanoyl group, an octanoyl group, a nonanoyl group, a decanoyl group, an undecanoyl group, a dodecanoyl group, a myristoyl group, a palmitoyl group, a stearoyl group, a pivaloyl group, a benzoyl group, a naphthoyl group, a nicotinoyl group, an isopropyl ... Examples of such groups include acyl groups such as sonicotinoyl, furoyl, and cinnamoyl groups, isocyanate groups such as 2-methacryloyloxyethylisocyanoyl groups, alkyl groups such as methyl, ethyl, propyl, 2-propyl, butyl, 2-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, myristyl, palmityl, and stearyl groups, oxirane, oxetane, thiirane, and thietane groups. Of these, the group introduced by chemical modification preferably contains at least a carboxy group.

[0018] Chemical modification of CNF can be carried out using conventional methods. That is, cellulose can be chemically modified by reacting it with a chemical modifying agent. If necessary, solvents, catalysts, heating, reduced pressure, etc. may be used. Chemical modifying agents include acids, acid anhydrides, alcohols, halogenating agents, and cyclic ethers such as alcohols, isocyanates, alkoxysilanes, and oxiranes (epoxies). These may be used alone or in combination. Examples of acids include acetic acid, acrylic acid, methacrylic acid, propanoic acid, butanoic acid, 2-butanoic acid, and pentanoic acid. After chemical modification, it is preferable to thoroughly wash the cellulose with water to terminate the reaction. After thorough washing with water, it is also preferable to further replace the cellulose with an organic solvent such as alcohol. In this case, the cellulose is replaced by immersing it in an organic solvent such as alcohol.

[0019] The average fiber diameter of the CNF is not particularly limited, but is preferably 1 to 100 nm, more preferably 2 to 50 nm, and even more preferably 2 to 10 nm. Using CNF with an average fiber diameter of 1 to 100 nm makes it easier to obtain a porous cellulose body with a large specific surface area. When the average fiber diameter is 1 nm or more, the single fiber strength of the nanofiber increases, making it easier to maintain the structure of the porous cellulose body. Here, the average fiber diameter is calculated as follows: An electron microscope image of the CNF is obtained using a transmission electron microscope (TEM) or a scanning electron microscope (SEM). Two random axes are drawn vertically and horizontally on the obtained image, and the fiber diameters of the fibers intersecting the axes are visually read. This is done at a magnification of 5,000x, 10,000x, or 50,000x, depending on the size of the constituent fibers. The sample or magnification must be such that 20 or more fibers intersect the axis. At least three images of non-overlapping surface areas are then taken with an electron microscope, and the fiber diameter values ​​of the fibers intersecting each of the two axes are read. Therefore, a minimum of 20 x 2 x 3 = 120 pieces of fiber information are obtained. The number-average fiber diameter is calculated from the fiber diameter data thus obtained, and is used as the average fiber diameter of the CNF. For branched fibers, if the length of the branched portion is 50 nm or more, it is counted as a single fiber in the fiber diameter calculation.

[0020] The average fiber length of the CNF is not particularly limited, but is preferably 0.01 to 20 μm, and more preferably 0.05 to 10 μm. The average fiber length is calculated by casting a thin layer of CNF dispersion on a substrate, freeze-drying the resulting sample, and observing it with an SEM. From the obtained observation image, 10 independent fibers are randomly selected per image, and their fiber lengths are visually read. This is done at a magnification of either 5,000x or 10,000x, depending on the length of the constituent fibers. The sample or magnification is selected so that the starting and ending points of the fibers are within the same image. In this way, at least 12 non-overlapping surface portions are observed with the SEM, and the fiber lengths are read. Therefore, information on a minimum of 10 fibers x 12 images = 120 fibers is obtained. The number-average fiber length is calculated from the fiber diameter data obtained in this way, and is used as the average fiber length of the CNF. For branched fibers, the length of the longest part of the fiber is used as the fiber length.

[0021] The method for adjusting the average fiber diameter of CNF is not particularly limited, but for example, in the mechanical crushing method, it can be adjusted by the processing time and number of times of the ultra-high pressure homogenizer or grinder used. In addition, in the chemical crushing method, it can be adjusted by the type of oxidizing agent (e.g., sodium hypochlorite), the concentration of the catalyst (e.g., TEMPO (2,2,6,6-tetramethyl-1-piperidinyloxy) catalyst), the reaction time, etc.

[0022] The method for preparing CNF is not particularly limited, and a mechanical or chemical disintegration method is preferred. Examples of the mechanical disintegration method include a method in which an aqueous suspension or slurry of a cellulose fiber-containing material is mechanically ground or beaten using a refiner, a high-pressure homogenizer, a grinder, a single- or multi-screw kneader, a bead mill, or the like to disintegrate the material. Examples of mechanical processing methods include Japanese Patent No. 5500842, Japanese Patent No. 5283050, Japanese Patent No. 5207246, Japanese Patent No. 5170193, Japanese Patent No. 5170153, Japanese Patent No. 5099618, Japanese Patent No. 4845129, Japanese Patent No. 4766484, Japanese Patent No. 4724814, Japanese Patent No. 4721186, Japanese Patent No. 4428521, International Publication No. 11 / 068023, Japanese Patent No. 5477265, and Japanese Patent Laid-Open No. 2014-84434. On the other hand, examples of chemical disintegration methods include oxidizing a cellulosic raw material using an oxidizing agent in the presence of an N-oxyl compound and a bromide and / or iodide, and then subjecting the oxidized cellulose to wet atomization for defibration into nanofibers. Examples of chemical treatment methods include those described in Japanese Patent Nos. 5,381,338, 4,981,735, 5,404,131, 5,329,279, 5,285,197, 5,179,616, 5,178,931, 5,330,882, and 5,397,910.

[0023] In the porous cellulose material, the CNF content is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the total mass of the porous cellulose material.

[0024] [Antifreeze Agent] The antifreeze agent contained in the porous cellulose body of the present invention is not particularly limited as long as it has the function of inhibiting the freezing of water, and known antifreeze agents can be used. Examples of antifreeze agents include water-soluble polymers, sugars, and antifreeze proteins, and among these, antifreeze proteins are preferred. Antifreeze agents have the effect of inhibiting the growth of ice crystals and can inhibit the coarsening of ice crystals. If the porous cellulose body contains an antifreeze agent, for example, when the porous cellulose body is formed through a freeze-drying process, the ice crystals are not coarsened, and the fiber diameter of the resulting porous cellulose body becomes smaller.

[0025] Examples of water-soluble polymers that can be used as antifreeze agents include polyvinyl alcohol, polyvinylpyrrolidone, and polyethylene glycol.

[0026] Examples of sugars that can be used as antifreeze agents include glucose, maltose, sucrose, lactose, trehalose, raffinose, etc. Polysaccharides extracted from fungi (e.g., Flammulina velutipes) are also preferred.

[0027] Examples of antifreeze proteins include antifreeze glycoproteins and antifreeze proteins. Antifreeze proteins may be any proteins that have the effect of inhibiting ice crystal growth, and may be extracted and purified from natural resources such as fish, plants, insects, and fungi, or may be produced using bacterial culture and genetic engineering techniques, or produced by chemical synthesis. Among these, antifreeze proteins derived from fish are preferred because they provide superior transparency for the porous cellulose body.

[0028] Antifreeze proteins vary widely in amino acid composition and higher-order structure. For example, fish-derived antifreeze proteins include type I antifreeze proteins with molecular weights of approximately 3,000 to 5,000, which are composed of an α-helical structure primarily containing Ala (alanine), type II antifreeze proteins with molecular weights of approximately 14,000 to 24,000, which are composed of a C-type lectin-like structural motif, type III antifreeze proteins with molecular weights of approximately 7,000, which are composed of a globular structure containing multiple β structures, type IV antifreeze proteins with molecular weights of approximately 12,000, which are composed of a bundle of α-helices, and antifreeze glycoproteins (AFGPs) with molecular weights of approximately 3,000 to 24,000, which are composed of a repeating triplet of -Ala-Thr (threonine)-Ala-, in which the side chain of the Thr residue is glycosylated. Other preferred antifreeze proteins include insect-derived antifreeze proteins having a β-helix structure and a molecular weight of about 7,000 to 12,000, and antifreeze proteins derived from radish sprouts.

[0029] The antifreeze preferably exhibits thermal hysteresis. Thermal hysteresis is defined as the value (°C) obtained by subtracting the freezing temperature (°C) from the equilibrium melting point (°C) shown below, and exhibiting thermal hysteresis means that this value is 0.05°C or higher. The greater the thermal hysteresis, the lower the temperature at which ice crystal growth can be suppressed, indicating greater antifreeze ability. The freezing temperature refers to the temperature at which ice crystal growth begins in an aqueous solution containing the antifreeze when the temperature is lower than the freezing point of water. The equilibrium melting point refers to the temperature at which melting begins when the temperature of a completely frozen aqueous solution containing the antifreeze is raised. The freezing temperature and equilibrium melting point are measured according to the method described in the Examples below. The antifreeze exhibits thermal hysteresis, and the value is preferably 0.1°C or higher, more preferably 0.4°C or higher, even more preferably 0.5°C or higher, particularly preferably 0.9°C or higher, and most preferably 1.0°C or higher. There is no particular upper limit to the thermal hysteresis value, but it can be, for example, 10°C. When the thermal hysteresis value of the antifreeze agent is within the above preferred range, the transparency of the porous cellulose material is superior.

[0030] In the porous cellulose body, the content of the antifreeze agent is preferably 1 to 40% by mass, more preferably 10 to 30% by mass, relative to the total mass of the porous cellulose body. One type of antifreeze agent may be used alone, or two or more types may be used simultaneously. When two or more types of antifreeze agents are used simultaneously, it is preferable that the total content is within the above-mentioned preferred range. The content of the antifreeze agent may be calculated from the content of the antifreeze agent added during production of the porous cellulose body, or the content may be measured by extracting the antifreeze agent from the porous cellulose body. When extracting the antifreeze agent from the porous cellulose body and measuring the content of the antifreeze agent, the antifreeze agent may be immersed in a solvent capable of extracting the antifreeze agent (e.g., water), and the content of the antifreeze agent in the solvent containing the antifreeze agent may be measured using a known method.

[0031] [Additives] The porous cellulose body may contain additives other than CNF and antifreeze agents. Examples of additives include strength modifiers. Examples of strength modifiers include various latex emulsions such as acrylic latex, NBR latex, vinyl acetate latex, and olefin latex, as well as water-soluble polymers such as polyacrylamide, polyamide epichlorohydrin, polyvinyl alcohol, and starch. The content of the additive is preferably 5% by mass or less, more preferably 1% by mass or less, based on the total mass of the porous cellulose body. The porous cellulose body may not contain additives.

[0032] [Method for producing porous cellulose body] The method for producing a porous cellulose body is not particularly limited, but it is preferable to adopt the first method for producing a porous cellulose body described below, since it is easy to obtain a porous cellulose body with excellent transparency. Furthermore, by adopting the first method for producing a porous cellulose body, it is possible to obtain a porous cellulose body with a large area.

[0033] (First method for producing a porous cellulose body) The first method for producing a porous cellulose body includes, in this order, a step of preparing a CNF dispersion containing an antifreeze agent in which CNFs are dispersed, a step of gelling the CNF dispersion to obtain a CNF wet gel, a step of substituting the solvent component in the CNF wet gel, and a step of freeze-drying the CNF wet gel to obtain a CNF aerogel. Each step is described below.

[0034] First, a CNF dispersion containing an antifreeze agent and dispersed CNF is prepared. The CNF dispersion containing an antifreeze agent and dispersed CNF can be obtained, for example, by preparing a CNF dispersion using the method described above for preparing CNF and then adding an antifreeze agent to the dispersion. The dispersion medium in the CNF dispersion preferably contains water, and the dispersion medium preferably contains 70% by mass or more of water, more preferably 90% by mass or more, and even more preferably 99% by mass or more, based on the total mass of the dispersion medium. The dispersion medium in the CNF dispersion may also be water. The CNF content in the CNF dispersion is preferably 0.001 to 5% by mass, more preferably 0.01 to 2% by mass, and even more preferably 0.1 to 1% by mass, based on the total mass of the CNF dispersion. The content of the antifreeze agent in the CNF dispersion can be adjusted to the preferred content described above, based on the total mass of the porous cellulose body to be formed. That is, the content of the antifreeze agent is preferably adjusted to 1 to 40 mass%, and more preferably adjusted to 10 to 30 mass%, relative to the total mass of the components other than the dispersion medium in the CNF dispersion. Specifically, for example, the content of the antifreeze agent in the CNF dispersion is preferably 0.0001 to 0.8 mass%, and more preferably 0.001 to 0.4 mass%, relative to the total mass of the CNF dispersion. The CNF dispersion may contain the above-mentioned additives.

[0035] Next, the CNF dispersion is gelled to obtain a CNF wet gel. The method for gelling the CNF dispersion is not particularly limited, but examples include adding an acidic or alkaline component, with the addition of an acidic component being preferred. The addition of the above component weakens the electrostatic repulsion that contributes to the dispersion of CNFs in the CNF dispersion, forming a CNF network and thus obtaining a CNF wet gel. The acidic component to be added is not particularly limited, but examples include inorganic acids (e.g., hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid), organic acids (e.g., methanesulfonic acid, tosylic acid), and metal halides (e.g., aluminum chloride). The acidic component is preferably added to the CNF dispersion in the form of a solution. The amount of the acidic component added can be adjusted as appropriate, but it is preferable to add it so that the total volume of the CNF dispersion after the addition of the acidic component is 0.01 to 5 mol / L. It is also preferable to add the acidic component without forcible stirring and then allow it to stand.

[0036] Next, the solvent components in the CNF wet gel are replaced. The solvent components in the CNF wet gel are preferably replaced with a solvent that will precipitate fine crystals in the subsequent freeze-drying process. Examples of solvents that will precipitate fine crystals include mixed solvents, with a mixed solvent of water and alcohol being particularly preferred. The mixed solvent is preferably prepared in a ratio that will cause the components contained in the mixed solvent to precipitate as a eutectic when the temperature is lowered. Examples of alcohols include alcohols that are miscible with water at any ratio, with t-butyl alcohol being preferred. Mixed solvents of water and t-butyl alcohol preferably contain 3 to 20% by mass of water, more preferably 5 to 15% by mass, based on the total mass of the mixed solvent. In the mixed solvent, the component other than water is preferably t-butyl alcohol. The solvent components in the CNF wet gel can be replaced by known methods, for example, by immersing the CNF wet gel in the mixed solvent. Shaking may be performed to promote the replacement.

[0037] Next, the CNF wet gel with the solvent components replaced is freeze-dried to obtain a CNF aerogel. Freezing can be performed using known methods, but rapid cooling is preferred to reduce the size of crystals precipitated from the solvent contained in the CNF wet gel and obtain a more transparent porous cellulose body. Rapid cooling methods include contacting the CNF wet gel with a member cooled with liquid nitrogen. Because the CNF wet gel contains an antifreeze, ice crystals are less likely to grow during freezing, and the CNF wet gel is frozen while maintaining the dispersion state of the CNF in the CNF wet gel. After freezing the CNF wet gel, the solvent components in the frozen CNF wet gel are sublimated. The solvent components can be sublimated by placing the frozen CNF wet gel in an environment below the freezing point of the solvent components. During the sublimation of the solvent components, the sublimation rate can be increased by reducing the pressure.

[0038] Through the above steps, the porous cellulose material of the present invention can be obtained.

[0039] In another embodiment of the method for producing a porous cellulose body, the freeze-drying performed in the first method for producing a porous cellulose body may be replaced with a process in which the solvent component in the CNF wet gel is replaced with a supercritical fluid and then dried.

[0040] <Transparent heat insulating material> The transparent heat insulating material of the present invention comprises the porous cellulose material described above. The porous cellulose material has a fiber diameter of 3 to 40 nm, which is thought to tend to reduce light scattering and provide excellent transparency.

[0041] It is also preferable that the maximum length of the transparent insulating material be 1000 mm or more, as this expands the range of applications for the transparent insulating material. The maximum length refers to the maximum length of the continuously formed porous cellulose body. For example, if the transparent insulating material is plate-shaped and has a rectangular shape when viewed perpendicular to one surface of the plate, the maximum length of the transparent insulating material corresponds to the length of the long side of the rectangle. Furthermore, if the transparent insulating material is plate-shaped and has a circular shape when viewed perpendicular to one surface of the plate, the maximum length of the transparent insulating material corresponds to the diameter of the circle. The method for obtaining a transparent insulating material (porous cellulose body) having a maximum length of 1000 mm or more is as described above. The porous cellulose body obtained by the above-mentioned method may be used as the transparent insulating material, or the porous cellulose body may be processed into a desired shape to form the transparent insulating material.

[0042] The transmittance of the transparent heat insulating material is preferably more than 70%, more preferably 75% or more, and even more preferably 78% or more. The transmittance of the transparent heat insulating material is usually less than 100%. The transmittance of the transparent heat insulating material can be increased by reducing the fiber diameter of the cellulose porous body. The method for measuring the transmittance of the transparent heat insulating material follows the method described in the examples. In other words, it is preferable that the transmittance is within the above range when the thickness of the transparent heat insulating material is 5 mm.

[0043] <Applications> The porous cellulose body (transparent heat insulating material) of the present invention has high transparency and can be applied to a variety of applications. For example, it can be suitably applied to applications where it is necessary to transmit light while exerting a heat insulating effect. Specifically, the porous cellulose body (transparent heat insulating material) of the present invention can be suitably applied to windows or components thereof. Specific examples of the application of the porous cellulose body (transparent heat insulating material) of the present invention to windows are described below, but the porous cellulose body (transparent heat insulating material) of the present invention is not limited to the specific examples below.

[0044] [Laminated Glass] The porous cellulose body (transparent heat insulating material) of the present invention can be used as an interlayer film for laminated glass. The configuration of the laminated glass is not particularly limited, and known configurations can be used. For example, the number of glass plates used in the laminated glass may be two or more, or may be three or more, or may be four or more. When the porous cellulose body (transparent heat insulating material) of the present invention is used as an interlayer film for laminated glass, it is disposed between two or more glass plates used in the laminated glass. When the number of glass plates is three or more, the porous cellulose body (transparent heat insulating material) of the present invention may be disposed between each glass plate, or the porous cellulose body (transparent heat insulating material) of the present invention may be disposed only between one pair of glass plates.

[0045] When the porous cellulose body (transparent heat insulating material) of the present invention is used as an interlayer in laminated glass, a structure (another layer) other than the porous cellulose body (transparent heat insulating material) of the present invention may be present between a pair of glass plates. That is, the porous cellulose body (transparent heat insulating material) of the present invention provided between the glass plates may be in direct contact with the glass plates or may be in contact with the glass plates via another layer. Preferred examples of the other layer include one or more resin layers selected from the group consisting of polyvinyl butyral, polycarbonate, ethylene-vinyl acetate copolymer, polyethylene terephthalate, and the like. Preferred examples of the other layer include an adhesive layer or a pressure-sensitive adhesive layer. Furthermore, the other layers described below in connection with double-glazing may be applied to the laminated glass.

[0046] The glass plates used in the laminated glass can be any known glass depending on the purpose, and examples thereof include transparent glass plates, patterned glass plates, wired glass plates, lined glass plates, tempered glass plates, heat-reflecting glass plates, heat-absorbing glass plates, Low-E glass plates, and various other glass plates. Furthermore, one or more of the glass plates used in the laminated glass may be made of a glass-substitute resin such as polycarbonate. The thickness of the glass plates can be appropriately selected depending on the purpose. The shape of the glass plates is not particularly limited and can be appropriately adjusted depending on the application. Furthermore, the glass plates may have curved surfaces.

[0047] The laminated glass may have a known sealing structure, for example, a structure in which the outer edge of the laminated glass is sealed with a sealing material such as a resin.

[0048] [Double Glazing] The porous cellulose body (transparent heat insulating material) of the present invention can be used in double glazing. Double glazing refers to glass containing a gas layer between two or more glass panes. The gas layer is a layer made of gas, and the gas contained in the gas layer may be air or an inert gas such as nitrogen gas or argon gas. The gas layer may be at a pressure lower than atmospheric pressure. The number of glass panes contained in the double glazing may be two or more, three or more, or four or more. When the porous cellulose body (transparent heat insulating material) of the present invention is used in double glazing, the porous cellulose body (transparent heat insulating material) of the present invention is disposed between a pair of glass panes. When the number of glass panes is three or more, the porous cellulose body (transparent heat insulating material) of the present invention may be disposed between each glass pane, or the porous cellulose body (transparent heat insulating material) of the present invention may be disposed only between a pair of glass panes.

[0049] When the porous cellulose body (transparent heat insulating material) of the present invention is applied to double-glazing, it may have one or more configurations (other layers) other than the porous cellulose body (transparent heat insulating material) of the present invention. Examples of other layers include the other layers described above, as well as a light-shielding layer and a heat-shielding layer. The light-shielding layer may be a layer with low transmittance for at least a portion of visible light, or may be a layer with low transmittance for at least a portion of ultraviolet light. Examples of light-shielding layers include metal vapor deposition films and colored layers such as a dye layer containing a dye. Examples of heat-shielding layers include layers that reflect or absorb infrared rays, such as metal vapor deposition films, polymer layers containing metal particles or metal oxide particles, and dielectric multilayer films. Examples of other layers include flame-retardant layers. Examples of the flame-retardant layer include layers containing a flame retardant, and known flame retardants can be used as the flame retardant. Examples of flame retardants include aromatic phosphate esters, phosphorus compounds such as red phosphorus, halogen compounds such as chlorinated paraffins containing at least one of chlorine and bromine, antimony compounds such as antimony trioxide, metal hydroxides such as aluminum hydroxide and magnesium hydroxide, and nitrogen compounds such as melamine cyanurate.

[0050] The glass plate may be the glass plate used in the above-described laminated glass. The glass plate included in the double-glazing glass may be laminated glass. The laminated glass may include the porous cellulose material (transparent heat insulating material) of the present invention.

[0051] The double-glazed glass may have a known sealing structure. For example, the sealing structure may include a spacer disposed on the outer edge of a pair of glass sheets and a sealing material disposed between the spacer and the opposing glass sheet. The sealing structure allows the space formed by the pair of glass sheets and the spacer to become the gas layer. The spacer may contain a desiccant for the purpose of absorbing moisture from the gas layer. The glass sheets may be sealed with another sealing material further toward the outer edge than the spacer. Examples of other sealing materials include curable resins such as polysulfide resins and silicone resins. The sealing structure may also be formed by a frame that holds the double-glazed glass.

[0052] When the porous cellulose body (transparent heat insulating material) of the present invention is applied to the above-mentioned laminated glass and double glazing, an integrally molded porous cellulose body (transparent heat insulating material) may be applied, or a plurality of porous cellulose bodies (transparent heat insulating materials) may be applied by arranging them in the planar direction of the glass plates. Also, a plurality of porous cellulose bodies (transparent heat insulating materials) may be applied by stacking them in the lamination direction of the glass plates. Note that when the porous cellulose body (transparent heat insulating material) of the present invention is applied to the above-mentioned laminated glass and double glazing, the above-mentioned flame retardant may be added to the porous cellulose body (transparent heat insulating material).

[0053] The above-described laminated glass and double-glazed glass can be suitably used, for example, as windows for houses and windows for vehicles such as passenger cars. Furthermore, the above-described laminated glass and double-glazed glass can transmit radio waves because the porous cellulose body (transparent heat insulating material) of the present invention is not electrically conductive. When radio wave transmission is desired, it is preferable to select a layer that is not electrically conductive as the other layer.

[0054] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.

[0055] Example 1 Preparation of Cellulose Nanofiber Aqueous Dispersion 2.00 g (dry mass equivalent) of NBKP (kraft pulp obtained by bleaching softwood raw materials, mainly consisting of fibers with a fiber diameter exceeding 1000 nm), 0.025 g of TEMPO (2,2,6,6-tetramethylpiperidine-1-oxy radical), and 0.25 g of sodium bromide were dispersed in 150 ml of water, and then a 13% aqueous solution of sodium hypochlorite was added to 1.00 g of NBKP so that the amount of sodium hypochlorite was 5.00 mmol. The reaction was initiated by adding sodium hypochlorite. During the reaction, a 0.50 mol / L aqueous solution of sodium hydroxide was added dropwise to maintain the pH at 10. After the reaction for 2 hours, the reaction product was filtered and thoroughly washed with water to obtain an oxidized cellulose slurry. A 0.15% by mass oxidized cellulose slurry was defibrated for 5 minutes at 15,000 rpm using a biomixer (BM-2, manufactured by Nippon Seiki Seisakusho Co., Ltd.), and then further defibrated for 20 minutes using an ultrasonic disperser (model US-300E, manufactured by Nippon Seiki Seisakusho Co., Ltd.). Subsequently, coarse fibers were removed by centrifugation to obtain a transparent aqueous dispersion of cellulose nanofibers. The obtained aqueous dispersion of cellulose nanofibers was concentrated using a rotary evaporator to a solids concentration of 0.40% and used in subsequent steps. Hereinafter, the aqueous dispersion of cellulose nanofibers with a solids concentration of 0.40% will also be referred to as "aqueous dispersion of cellulose nanofibers A."

[0056] Highly purified fish-derived type I antifreeze protein (manufactured by Nichirei, equivalent to an antifreeze agent) was added to the above cellulose nanofiber aqueous dispersion A at a concentration of 0.08% relative to the total mass of cellulose nanofiber aqueous dispersion A, and the mixture was stirred with a magnetic stirrer.

[0057] [Gelling step] 500 g of cellulose nanofiber aqueous dispersion A containing the antifreeze protein was poured into a 100 cm square Petri dish, and 100 g of 1.0 M hydrochloric acid was gently poured down the side of the dish, followed by standing for 1 hour. The dispersion physically gelled to a thickness of 5 mm.

[0058] [Solvent substitution step] Solvent substitution was carried out using a mixed solvent in which the mixing ratio of t-butyl alcohol and water was 90:10 by mass. The solvent substitution was carried out by immersing the physical gel in a sufficient amount of the substitution solvent and shaking it slowly. Each substitution step was carried out over 4 hours, and substitution was carried out four or more times.

[0059] The physical gel obtained in the solvent substitution step was frozen by sandwiching it between iron plates sufficiently cooled with liquid nitrogen (-196°C). The frozen gel was then dried in a vacuum dryer (manufactured by Tokyo Rikakikai Co., Ltd.) to sublimate the solvent component and obtain an aerogel (porous cellulose).

[0060] Example 2 A porous cellulose material was obtained in the same manner as in Example 1, except that highly purified fish-derived antifreeze glycoprotein (AFGP) (manufactured by Nichirei) was used as the antifreeze agent.

[0061] Example 3 A porous cellulose material was obtained in the same manner as in Example 1, except that a highly purified fish-derived type II antifreeze protein (AFGP) (manufactured by Nichirei) was used as the antifreeze agent.

[0062] Example 4 A porous cellulose material was obtained in the same manner as in Example 1, except that a highly purified fish-derived type III antifreeze protein (manufactured by Nichirei) was used as the antifreeze agent.

[0063] Example 5 A porous cellulose material was obtained in the same manner as in Example 1, except that crudely purified fish-derived type I antifreeze protein (manufactured by Nichirei) was used as the antifreeze agent.

[0064] Example 6 A porous cellulose material was obtained in the same manner as in Example 1, except that crudely purified fish-derived antifreeze glycoprotein (AFGP) (manufactured by Nichirei) was used as the antifreeze agent.

[0065] Example 7 A porous cellulose material was obtained in the same manner as in Example 1, except that a highly purified fish-derived type II antifreeze protein (AFGP) (manufactured by Nichirei) was used as the antifreeze agent.

[0066] Example 8 A porous cellulose material was obtained in the same manner as in Example 1, except that a highly purified fish-derived type III antifreeze protein (manufactured by Nichirei) was used as the antifreeze agent.

[0067] Example 9 A porous cellulose material was obtained in the same manner as in Example 1, except that an antifreeze protein derived from radish sprouts (manufactured by Kaneka) was used as the antifreeze agent.

[0068] Example 10 A porous cellulose material was obtained in the same manner as in Example 1, except that D(+) glucose (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the antifreeze agent.

[0069] Comparative Example 1 A porous cellulose material was obtained in the same manner as in Example 1, except that no antifreeze agent was added.

[0070] <Measurement and Evaluation> [Measurement of Fiber Diameter] The fiber diameters of the porous cellulose bodies of the Examples and Comparative Examples were measured by the method described above.

[0071] [Measurement of Thermal Hysteresis of Antifreeze] The thermal hysteresis value of the antifreeze used in each example was measured as follows. First, antifreeze powder was dissolved in ultrapure water so that the amount was 5 parts by mass relative to the total mass of the solution, and 4 μL of the solution (specimen) was sandwiched between two cover glasses. This was placed on the cooling stage of a cooled temperature range microscope system consisting of a temperature controller (Linkam LNP94 / 2, TMS94), a specimen cooling stage (Linkam THMSG 600), and a microscope (Nikon ECLIPSE E600). While observing the specimen under the microscope, the cooling stage was cooled until the entire specimen was frozen, and the temperature at which the entire specimen began to solidify was taken as the freezing temperature. Next, the completely frozen specimen was heated, and the temperature at which melting began was taken as the equilibrium melting point. The difference between the equilibrium melting point and the freezing temperature was taken as the thermal hysteresis.

[0072] [Transmittance evaluation] The transmittance of the porous cellulose bodies of the Examples and Comparative Examples was measured using an ultraviolet-visible-near-infrared spectrophotometer V-660 equipped with an automatic absolute reflectance measurement unit ARMN-735 manufactured by JASCO Corporation. During the measurement, the sample was placed close to an integrating sphere to measure the total light transmittance, and the transmittance was evaluated as the transmittance at 550 nm. The thickness of the porous cellulose bodies of the Examples and Comparative Examples was 5 mm.

[0073] <Results> Table 1 shows the types of antifreeze agents used in the preparation of the porous cellulose bodies of the Examples and Comparative Examples, as well as the thermal hysteresis, fiber diameter, and transmittance of the antifreeze agents.

[0074]

[0075] From the results shown in Table 1, the porous cellulose body of Comparative Example 1, which did not contain an antifreeze agent, had lower transparency than the other Examples. Comparison of Examples 9 and 10 with other Examples confirmed that when the antifreeze agent was an antifreeze protein and the antifreeze protein was derived from fish, the transparency of the porous cellulose body was superior. Comparison of Examples 9 and 10 with other Examples confirmed that when the thermal hysteresis of the antifreeze agent was 0.4°C or higher (preferably 0.5°C or higher, more preferably 0.9°C or higher, and even more preferably 1.0°C or higher), the transparency of the porous cellulose body was superior. Comparison of Examples 9 and 10 with other Examples confirmed that when the fiber diameter of the porous cellulose body was 4 to 30 nm, the transparency of the porous cellulose body was superior.

Claims

1. A cellulose porous body comprising cellulose nanofibers and an antifreeze agent, the fiber diameter being 40 nm or less.

2. The porous cellulose material according to claim 1, wherein the antifreeze agent is an antifreeze protein.

3. The cellulose porous body according to claim 2, wherein the antifreeze proteins are derived from fish.

4. The cellulose porous body according to any one of claims 1 to 3, wherein the thermal hysteresis of the antifreeze agent is 0.4°C or more.

5. A cellulose porous body according to any one of claims 1 to 3, wherein the fiber diameter is 4 to 30 nm.

6. The cellulose porous body according to any one of claims 1 to 3, wherein the content of the antifreeze agent is 10 to 30 mass % based on the total mass of the cellulose porous body.

7. A transparent heat insulating material comprising the cellulose porous body according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Cellulose porous body and manufacturing method therefor

    JP2015105366A

  • Cellulose porous body and manufacturing method therefor

    JP2015105453A

  • Method for producing cellulose porous body

    JP2023115733A