Glass member and method for manufacturing same

The glass member, with its unique composition and manufacturing process, addresses the issue of frequent replacements in semiconductor equipment by enhancing plasma resistance and durability, thereby improving production efficiency and maintaining optical properties.

WO2024219405A1PCT designated stage expired Publication Date: 2024-10-24AGC INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015197
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Semiconductor manufacturing equipment components, particularly glass members, face frequent replacement due to harsh plasma environments, leading to decreased production efficiency as they wear out quickly, necessitating improved plasma resistance.

Method used

A glass member with specific composition and manufacturing process, characterized by low hydrogen content, controlled refractive index, and inclusion of yttrium and silicon, along with other elements, providing enhanced plasma resistance and durability.

Benefits of technology

The glass member exhibits improved plasma resistance, reducing the frequency of replacements and maintaining production efficiency by minimizing plasma-induced deterioration and maintaining optical transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention relates to a glass member used in a semiconductor manufacturing device, the glass member having a hydrogen content of 200 mass ppm or less. The present invention also relates to a method for manufacturing the glass member, the method for melting a glass raw material by heating the same at a melting temperature of 1500 to 1800°C, and cooling the obtained molten glass to a cooling stop temperature of 700 to 900°C at a cooling rate of 100 to 1500°C / min.
Need to check novelty before this filing date? Find Prior Art

Description

Glass member and method of manufacturing the same

[0001] The present invention relates to a glass member and a method for manufacturing the same.

[0002] Components used in semiconductor manufacturing equipment are often exposed to plasma during operation and gradually wear out. Components that have worn out are replaced with new ones. In recent years, as products manufactured using semiconductor manufacturing equipment have become taller and more complex, the plasma environment to which components are exposed has become increasingly harsh, resulting in the frequent need to replace components. However, the semiconductor manufacturing equipment cannot be operated while components are being replaced. Therefore, increasing the frequency of component replacement reduces product production efficiency.

[0003] Therefore, the members used in semiconductor manufacturing equipment are required to have a longer life, i.e., good plasma resistance.

[0004] An example of a semiconductor manufacturing device is a plasma etching device. The plasma etching device uses various components such as a top plate (conductor type), a microwave introduction tube, lift pins, and various nozzles. These components have traditionally been made of materials such as cordierite sintered bodies (see Patent Document 1).

[0005] Japanese Patent Application Publication No. 9-295863

[0006] Glass members are often used in semiconductor manufacturing equipment, and in such cases, the glass members are also required to have good plasma resistance.

[0007] The present invention has been made in view of the above points, and an object of the present invention is to provide a glass member for use in semiconductor manufacturing equipment, which has excellent plasma resistance.

[0008] As a result of extensive research, the present inventors have found that the above object can be achieved by employing the following configuration, and have completed the present invention.

[0009] That is, the present invention provides the following [1] to

[15] . [1] A glass member for use in semiconductor manufacturing equipment, the glass member having a hydrogen content of 200 mass ppm or less. [2] The glass member according to the above [1], having an average refractive index of 1.5 or more at a wavelength of 365 nm, with the difference between the upper and lower limits being 0.2 or less. [3] 10 cm 2 [4] The glass member according to any one of [1] to [3] above, which is ring-shaped with an outer diameter of 300 to 600 mm, an inner diameter of 200 to 450 mm, and a thickness of 2 to 30 mm, is chamfered to C1.0 or less, has a surface roughness Ra of 1 μm or less, and has a flatness of 0.5 mm or less. [5] The glass member according to any one of [1] to [4] above, which contains yttrium and silicon, and has a molar ratio Y / Si of the yttrium content to the silicon content of 0.2 to 1.5. [6] SiO 2 The content of Y is 40 to 70 mol %. 2 O 3 The content of Al is 5 to 40 mol %. 2 O 3 [7] The glass member according to any one of [1] to [5] above, wherein the content of at least one element a selected from the group consisting of tantalum, boron, magnesium, calcium, strontium, and barium is 10 mol % or less, calculated as an oxide. [8] The glass member according to [6] or [7] above, wherein the content of at least one element b selected from the group consisting of alkali metal elements, iron, and titanium is 3,000 mass ppm or less, calculated as an oxide. [9] The glass member according to any one of [1] to [8] above, wherein the Young's modulus is 100 GPa or more and the average thermal expansion coefficient at 50 to 350°C is 4 to 7 ppm / K.

[10] The glass member according to any one of [1] to [9] above, wherein the transmittance at a wavelength of 800 nm is 92% or less.

[11] A glass member according to any one of [1] to [9] above, wherein the content of at least one element a selected from the group consisting of tantalum, boron, magnesium, calcium, strontium, and barium is 10 mol % or less, calculated as an oxide. 2 0.1 mm in 10 areas 2

[12] The glass member according to any one of [1] to

[10] above, wherein the total number of bubbles is 40 or less. 2 0.1 mm in 10 areas 2

[13] The glass member according to any one of [1] to

[12] above, which is used as a focus ring, shower plate, electrostatic chuck, susceptor, injector, observation window, top plate, or side wall of the semiconductor manufacturing apparatus.

[14] Flow rate: CF4 of 100 sccm 4 The glass member according to any one of the above [1] to

[13] , wherein the etching rate when etched with a gas is 0.1 or less relative to quartz.

[15] A method for producing the glass member according to any one of the above [1] to

[14] , comprising heating a glass raw material to a melting temperature of 1500 to 1800°C to melt the glass, and cooling the obtained molten glass to a cooling stop temperature of 700 to 900°C at a cooling rate of 100 to 1500°C / min.

[0010] According to the present invention, a glass member having excellent plasma resistance can be provided.

[0011] A numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] [Glass Member] The glass member of this embodiment is a glass member used in a semiconductor manufacturing apparatus, and has a hydrogen content of 200 mass ppm or less.

[0013] Hereinafter, the glass member will also be referred to simply as "glass," and the glass member of this embodiment will also be referred to as "the present glass member" or "the present glass."

[0014] The present glass member has excellent plasma resistance. The reason for this is presumed to be as follows. First, the hydrogen contained in the glass member is believed to be derived from water molecules. The small amount of hydrogen makes the structure of the glass member denser, and as a result, the rate of deterioration due to plasma exposure is slower. Furthermore, if the plasma (or the gas used to generate the plasma) contains fluorine, the hydrogen contained in the glass member is likely to react with this fluorine. However, the small amount of hydrogen relatively reduces the reaction with fluorine, and damage to the glass member is suppressed.

[0015] <Hydrogen Content (H Content)> In the present glass member, the hydrogen content (also referred to as "H content") is 200 ppm by mass or less, as described above. In order to achieve better plasma resistance, the H content is preferably 150 ppm by mass or less, more preferably 100 ppm by mass or less, even more preferably 50 ppm by mass or less, even more preferably 40 ppm by mass or less, particularly preferably 30 ppm by mass or less, very preferably 20 ppm by mass or less, and most preferably 10 ppm by mass or less.

[0016] On the other hand, the H content is a realistic value that is easy to control when considering mass productivity, and is, for example, 1 mass ppm or more, preferably 2 mass ppm or more, and more preferably 3 mass ppm or more.

[0017] The H content of the glass member is determined by secondary ion mass spectrometry (SIMS). More specifically, a secondary ion mass spectrometer (model IMS-6f, manufactured by Ametec Co., Ltd.) is used to measure the primary ion species Cs + The measurement is performed under the conditions of a primary acceleration voltage of 15.0 kV, a detection area of ​​φ30 μm, and a measurement depth of 1 μm.

[0018] <Refractive Index> <Average> In the present glass member, the average refractive index (also simply referred to as "refractive index") at a wavelength of 365 nm is preferably 1.5 or more, more preferably 1.57 or more, even more preferably 1.63 or more, particularly preferably 1.68 or more, and most preferably 1.7 or more. This gives the present glass member better plasma resistance. This is presumably because elements such as yttrium (Y) have good plasma resistance, and the refractive index of the glass member increases when such elements are present in large amounts.

[0019] On the other hand, the average refractive index is preferably 1.8 or less, more preferably 1.76 or less, and even more preferably 1.73 or less. When the average refractive index is within this range, crystallization during the production of the glass member is suppressed, and the surface reflectance of the glass member is reduced, so that light from a sensor or the like can easily transmit through.

[0020] <<Difference (Variation) Between Upper and Lower Limits>> In the present glass member, the difference between the upper and lower limit values ​​of the refractive index (also referred to as "variation") is preferably 0.2 or less, more preferably 0.05 or less, even more preferably 0.01 or less, even more preferably 0.005 or less, particularly preferably 0.001 or less, very preferably 0.0005 or less, and most preferably 0.0003 or less. This results in the present glass member having better plasma resistance. This is presumably because, when the refractive index is uniformly high without bias, phenomena such as partial damage due to plasma irradiation are less likely to occur, resulting in overall good plasma resistance. Note that, when a glass member is enlarged, its strength, composition, etc. may vary depending on the region, so it is beneficial to have such uniform, overall good plasma resistance.

[0021] <<Measurement Method>> The refractive index of a glass member is measured at any 10 points using a Kalnew Precision Refractometer KPR-3000 (accuracy: ±0.00002 (23°C)). The average of the 10 measured values ​​is calculated as the average refractive index. The difference between the upper and lower limit values ​​of the 10 measured values ​​is calculated as the refractive index variation (difference between the upper and lower limit values).

[0022] <Glass Composition> Next, the composition (glass composition) of the present glass member will be described, that is, the contents of elements that the present glass member may contain will be described.

[0023] <Si, Y, and Al> The present glass member may contain silicon (Si) and yttrium (Y), and may further contain aluminum (Al).

[0024] (Molar ratio Y / Si) The molar ratio (Y / Si) of the content of yttrium (Y) and the content of silicon (Si) is preferably 0.2 or more, more preferably 0.4 or more, and even more preferably 0.5 or more. This makes the Y content of the glass member relatively large, and the plasma resistance is more excellent. On the other hand, because crystallization is suppressed when manufacturing the glass member, the molar ratio (Y / Si) is preferably 1.5 or less, more preferably 1.0 or less, and even more preferably 0.8 or less.

[0025] (SiO 2 Content of SiO 2 The content of is preferably 40 mol % or more, more preferably 45 mol % or more, and even more preferably 50 mol % or more. 2 The content is, for example, 80 mol % or less, preferably 70 mol % or less, more preferably 65 mol % or less, and even more preferably 60 mol % or less.

[0026] (Y 2 O 3 Content of Y 2 O 3 The content of Y is preferably 5 mol % or more, more preferably 10 mol % or more, even more preferably 15 mol % or more, and particularly preferably 20 mol % or more. This increases the refractive index of the glass member and improves plasma resistance. 2 O 3 The content of is preferably 40 mol % or less, more preferably 35 mol % or less, even more preferably 30 mol % or less, and particularly preferably 25 mol % or less, because crystallization during the production of the glass member is suppressed.

[0027] (Al 2 O 3Content of Al 2 O 3 From the viewpoint of improving the strength and heat resistance of the glass member, the content of Al is preferably 10 mol % or more, more preferably 15 mol % or more, and even more preferably 18 mol % or more. 2 O 3 From the viewpoint of obtaining better plasma resistance, the content is preferably 30 mol % or less, more preferably 28 mol % or less, and even more preferably 25 mol % or less.

[0028] <Element a: Ta, B, Mg, Ca, Sr, and Ba> The glass member may contain at least one element a selected from the group consisting of tantalum (Ta), boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba). However, the content of element a, calculated as an oxide, is preferably 10 mol% or less, more preferably 8 mol% or less, even more preferably 5 mol% or less, even more preferably 3 mol% or less, particularly preferably 1 mol% or less, and most preferably 0 mol%. Note that when the glass member contains multiple elements as element a, the "content of element a, calculated as an oxide" refers to the sum of the contents of each of the multiple elements, calculated as an oxide.

[0029] The Ta content calculated as an oxide is specifically Ta 2 O 5 The content of B converted into oxide specifically means the content of B 2 O 3 The Mg content calculated as an oxide specifically means the MgO content. The Ca content calculated as an oxide specifically means the CaO content. The Sr content calculated as an oxide specifically means the SrO content. The Ba content calculated as an oxide specifically means the BaO content.

[0030] <Element b: Alkali Metal Element, Fe, and Ti> The glass member may contain at least one element b selected from the group consisting of alkali metal elements, iron (Fe), and titanium (Ti). Examples of alkali metal elements include lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr). Of these, lithium (Li), sodium (Na), and potassium (K) are substantially preferred. However, element b is an impurity element for glass members used in semiconductor manufacturing equipment, and therefore a lower content is preferable. Specifically, the content of element b, calculated as an oxide, is preferably 3000 ppm by mass or less, more preferably 1000 ppm by mass or less, even more preferably 300 ppm by mass or less, particularly preferably 100 ppm by mass or less, and most preferably 50 ppm by mass or less. When the glass member contains a plurality of elements as element b, the "content of element b in terms of oxide" refers to the total content of each of the plurality of elements in terms of oxide.

[0031] The content of alkali metal element (R) converted into oxide is specifically R 2 The oxide-equivalent Fe content means the content of Fe 2 O 3 The content of Ti calculated as an oxide specifically means the content of TiO 2 means the content of

[0032] <<Measurement Method>> The content (expressed as mole percentage or mass percentage based on oxide) of each of the above-mentioned elements (excluding Si) in the glass member is measured using an X-ray fluorescence analyzer (XRF) (ZSX100e, manufactured by Rigaku Corporation). That is, the X-ray intensity of each element on the surface of the glass member is measured and quantitatively analyzed to determine the content of each element.

[0033] SiO in glass members 2The oxygen content is determined as follows. First, a powder sample is collected from the center of the glass member by polishing, and the total oxygen content Z1 in the glass member is determined by infrared absorption method using an oxygen / hydrogen analyzer (ROH-600 manufactured by LECO Corporation). The oxygen content Z3 is calculated by subtracting the oxygen content Z2 that is stoichiometrically bonded to elements (excluding Si) contained in the glass member from the total oxygen content Z1 in the glass member (oxygen content Z3 = total oxygen content Z1 - oxygen content Z2). Assuming that the entire oxygen content Z3 is used for bonding with silicon atoms, the oxygen content Z3 is calculated by subtracting the oxygen content Z2 from the SiO 2 The SiO thus obtained is converted into an amount. 2 The amount of SiO in the glass member 2 The content is as follows:

[0034] <Young's modulus> The Young's modulus of the present glass member is preferably 60 GPa or more, more preferably 80 GPa or more, even more preferably 100 GPa or more, and particularly preferably 110 GPa or more. Such a present glass member has good dimensional accuracy, little deflection, and excellent thermal shock resistance. On the other hand, the upper limit of the Young's modulus of the present glass member is not particularly limited, and is, for example, 200 GPa, preferably 180 GPa, and more preferably 160 GPa. The Young's modulus of the glass member is measured at 25°C by an ultrasonic pulse method.

[0035] <Expansion Coefficient> In semiconductor manufacturing equipment, glass members may be used in combination with other members (also referred to as "peripheral members"), and examples of materials for the peripheral members include SiC and AlN. The expansion coefficient of the present glass member is preferably close to the expansion coefficient of the material of the peripheral members. This ensures that the expansion and contraction behavior of the present glass member is similar to that of the peripheral members, preventing detachment from the peripheral members. Specifically, the average thermal expansion coefficient (also simply referred to as "expansion coefficient") of the present glass member at 50 to 350°C is preferably 4 ppm / K or more, more preferably 4.1 ppm / K or more, even more preferably 4.2 ppm / K or more, and particularly preferably 4.5 ppm / K or more. On the other hand, the expansion coefficient of the present glass member is preferably 7 ppm / K or less, more preferably 6.5 ppm / K or less, and even more preferably 6 ppm / K or less. The expansion coefficient is measured using a differential thermal dilatometer in accordance with the method described in JIS R 3102-1995.

[0036] <Transmittance> The lower the transmittance of a glass member, the better its thermal insulation properties. Therefore, from the viewpoint of obtaining good thermal insulation, the transmittance of the present glass member at a wavelength of 800 nm (also simply referred to as "transmittance") is preferably 92% or less, more preferably 91% or less, even more preferably 90% or less, even more preferably 89% or less, and particularly preferably 88% or less. However, depending on the application in semiconductor manufacturing equipment, a certain degree of transparency may also be required for the glass member. Therefore, from the viewpoint of ensuring good transparency, the transmittance of the present glass member is preferably 80% or more, more preferably 83% or more, and even more preferably 85% or more. The transmittance is measured for a glass member having a thickness of 2 mm by a method conforming to JIS R 3106 (1998). That is, the transmittance is the transmittance converted into a thickness of 2 mm.

[0037] <Number of Bubbles> The glass member may contain bubbles (air bubbles). However, it is preferable that the number of large bubbles is small, because this results in an excellent appearance and superior plasma resistance. Specifically, the number of large bubbles is small, for example, within any 100 mm 2 0.1 mm in 10 areas 2The total number of bubbles (also simply referred to as "bubble count") is preferably 40 or less, more preferably 30 or less, even more preferably 20 or less, particularly preferably 10 or less, and most preferably 5 or less. More specifically, a plate-shaped glass member (thickness: 2 mm) is prepared, and an arbitrary region (area: 100 mm ) on the main surface of this glass member is measured. 2 ) was photographed using an optical microscope, and the area of ​​the sample was determined to be 0.1 mm 2 The number of bubbles that meet the above criteria is counted, and the total number of bubbles in any 10 areas is calculated.

[0038] <Crystalline Ratio> A glass member may contain crystals (crystalline phases), but from the viewpoint of ensuring good transparency, it is preferable that the number of large crystals is small. Also, from the viewpoint of reducing dust generation when the glass member is exposed to plasma, it is preferable that the number of large crystals is small. Specifically, in any 100 mm 2 0.1 mm in 10 areas 2 The area ratio of the above crystals (also referred to as "crystal ratio" for convenience) is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less on average. More specifically, a plate-shaped glass member (thickness: 2 mm) is prepared, and an arbitrary region (area: 100 mm 2 ) on the main surface of this glass member is selected. 2 ) was photographed using an optical microscope, and the area of ​​the sample was determined to be 0.1 mm 2 The area ratio (unit: %) of crystals that are equal to or greater than this is measured, and the average of the area ratios of crystals in 10 randomly selected regions is calculated.

[0039] <Etching rate> For this glass member, a flow rate of 100 sccm of CF 4When using a gas, the etching rate of the glass member relative to quartz is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.04 or less, even more preferably 0.03 or less, and most preferably 0.02 or less. The smaller the etching rate, the better the plasma resistance of the glass member. This extends the life of the glass member, reducing the frequency of replacement and improving the tact time of the manufacturing equipment. The lower limit of the etching rate is not particularly limited, but from the viewpoint of ease of glass production, a value of 0.01 or more is preferred. The conditions for calculating the etching rate in this specification are as follows:

[0040] (Conditions for calculating the etching rate) A test piece measuring 20 mm x 20 mm x 2 mm is cut out from a glass member, and the 20 mm x 20 mm surface is mirror-finished. Kapton tape is applied to a portion of the mirror-finished surface to mask it, and the surface is etched with plasma gas under the following conditions: Apparatus: CCP-RIE Gas type: CF 4 (100 sccm) Output: 350 W Pressure: 10 Pa Time: 130 minutes Temperature: 20°C Then, a stylus surface profiler (Dectak 150, manufactured by ULVAC) is used to measure the step between the etched and non-etched areas to determine the amount of etching (amount of wear). Furthermore, the amount of etching for the quartz glass is determined in the same manner. The ratio of the amount of etching for the glass member to the amount of etching for the quartz glass is determined as the etching rate.

[0041] The glass member is used, for example, as part or all of various components of semiconductor manufacturing equipment (including semiconductor inspection equipment), such as a focus ring, shower plate, electrostatic chuck, susceptor, injector (injector nozzle), observation window (a component for observing the inside of the semiconductor manufacturing equipment from the outside), top plate, or side wall (inner wall).

[0042] <Shape and Size> The shape of the present glass member may be plate-like (for example, disk-like, flat), spherical (true sphere, spheroid), ring-like, etc., and may be appropriately selected depending on the application.

[0043] The size of the glass member is appropriately selected depending on the application. Depending on the application, the glass member may be large, for example, 10 cm. 2 From the viewpoint of versatility, the cross-sectional area of ​​the glass member may be 100 cm or more (for example, the area of ​​a cross section parallel to the main surface when the glass member is plate-shaped). 2 More than 300 cm is preferable. 2 More preferably, 500 cm or more 2 More preferably, the upper limit of the cross-sectional area is 5000 cm. However, from the viewpoint of versatility, the upper limit of the cross-sectional area is not particularly limited. 2 Preferably, 1000 cm or less 2 The following is more preferred:

[0044] When the glass member is used as a focus ring, susceptor, or the like, its shape is ring-shaped. Because it is suitable for applications such as focus rings, the outer diameter of the ring-shaped glass member is preferably 300 to 600 mm, more preferably 350 to 450 mm. For similar reasons, the inner diameter is preferably 200 to 450 mm, more preferably 250 to 350 mm. For similar reasons, the thickness is preferably 2 to 30 mm, more preferably 3 to 7 mm. In this case, the ring-shaped glass member is preferably chamfered to a C of 1.0 or less. Furthermore, from the viewpoints of suppressing dust generation upon plasma irradiation and reducing the influence of thermal stress, the surface roughness (arithmetic mean roughness Ra) of the ring-shaped glass member is preferably 1 μm or less, more preferably 0.1 μm or less, and even more preferably 0.03 μm or less. Ra is measured in accordance with JIS B 0601:2001. Furthermore, for reasons of good dimensional accuracy, the flatness of the ring-shaped glass member is preferably 0.5 mm or less, more preferably 0.1 mm or less, and even more preferably 0.03 mm or less. The flatness can be measured using a non-contact three-dimensional shape measuring device (NH-5Ns, manufactured by Mitaka Optical Co., Ltd.).

[0045] [Method for manufacturing glass member] Next, a method for manufacturing the present glass member (hereinafter also referred to as the present manufacturing method) will be described. In the present manufacturing method, generally, glass raw materials are heated to melt (dissolve), and the resulting molten glass is cooled.

[0046] <Glass Raw Materials> It is preferable to weigh and mix various glass raw materials so that the composition of the resulting glass member will be the glass composition described above.

[0047] <<Use of Oxide>> It is preferable to use an oxide as the glass raw material, rather than a hydroxide. This reduces the OH content (H content) of the glass raw material, and therefore the H content of the resulting glass member is likely to be reduced.

[0048] However, a sulfur compound may be added to the glass raw material for the purpose of reducing the number of bubbles contained in the resulting glass member. As the sulfur compound, for example, aluminum sulfate is preferred from the viewpoint of reducing the amount of impurities contained in the resulting glass member.

[0049] <<Water Content>> The water content contained in the glass raw materials is preferably 200 mass ppm or less, more preferably 150 mass ppm or less, even more preferably 100 mass ppm or less, even more preferably 50 mass ppm or less, particularly preferably 30 mass ppm or less, very preferably 25 mass ppm or less, and most preferably 20 mass ppm or less, because this makes it easier to reduce the H content of the resulting glass member. The water content of the glass raw materials can be adjusted by drying the glass raw materials, etc. The water content of the glass raw materials is determined by thermogravimetric analysis (TGA). Confirmed.

[0050] <Mixing Conditions> When mixing the glass raw materials, it is preferable to use a stirrer to stir the raw materials for 10 minutes or more at 10 to 100 rpm. This allows the glass raw materials to be thoroughly mixed, which makes it easier to reduce the variation in the refractive index of the resulting glass member. The glass raw materials may also be mixed by being placed in a bag and shaken. In this case, it is preferable to shake the bag 100 times or more. This allows the glass raw materials to be thoroughly mixed, which makes it easier to reduce the variation in the refractive index of the resulting glass member.

[0051] <Melting> Next, the mixed glass raw materials are heated and melted. At this time, the melt may be subjected to degassing, homogenization, etc. by a known method, where appropriate. In this way, molten glass is obtained.

[0052] <<Types of Atmospheric Gases>> The atmosphere in which the glass raw materials are melted (also referred to as "melting atmosphere") is, for example, the air (atmospheric atmosphere). A gas (also referred to as "atmospheric gas") may be introduced into the melting atmosphere. As the atmospheric gas, nitrogen gas (N 2 ), oxygen gas (O 2 ), compressed air, water vapor (H 2 O), and the like, which may be used alone or in combination of two or more. 2 and O 2 When using both, the volume ratio of the two (N 2 / O 2 ) is, for example, 8 / 2. Of these, N is preferred because it is easy to reduce the H content in the resulting glass member. 2 , O 2 and compressed air. The atmospheric gas may be bubbled through the glass raw material (molten glass), or may simply be caused to flow over the surface of a container (such as a crucible) containing the glass raw material.

[0053] <<Flow Rate of Atmospheric Gas>> The flow rate SLM (flow rate per minute at 1 atm and 0°C) of the atmospheric gas is, for example, 0.1 L / min or more, preferably 1 L / min or more, more preferably 3 L / min or more, even more preferably 5 L / min or more, even more preferably 10 L / min or more, particularly preferably 15 L / min or more, very preferably 20 L / min or more, and most preferably 25 L / min or more. On the other hand, the flow rate of the atmospheric gas is preferably 60 L / min or less, more preferably 55 L / min or less, even more preferably 50 L / min or less, particularly preferably 45 L / min or less, and most preferably 40 L / min or less.

[0054] <<Temperature of Atmospheric Gas>> From the viewpoint of maintaining a constant glass melting temperature, the temperature of the atmospheric gas is preferably 30° C. or higher, more preferably 35° C. or higher, and even more preferably 40° C. or higher. On the other hand, from the viewpoint of reducing production costs, the temperature of the atmospheric gas is preferably 100° C. or lower, more preferably 80° C. or lower, and even more preferably 60° C. or lower.

[0055] <<Melting Temperature>> The temperature (melting temperature) when heating and melting the glass raw materials is preferably 1500°C or higher, more preferably 1550°C or higher, and even more preferably 1600°C or higher. This allows the glass raw materials to be sufficiently melted, and the variation in refractive index of the resulting glass member is likely to be reduced. On the other hand, from the viewpoint of production costs, etc., the melting temperature is preferably 1800°C or lower, more preferably 1750°C or lower, and even more preferably 1700°C or lower.

[0056] <<Melting Time>> The time for heating and melting the glass raw materials (melting time) is preferably 2 hours or more, more preferably 2.5 hours or more, and even more preferably 3 hours or more. This allows the glass raw materials to be sufficiently melted, making it easy to reduce the variation in the refractive index of the resulting glass member. In addition, since the molten glass can be sufficiently refined, it is easy to reduce the number of bubbles contained in the resulting glass member. On the other hand, for reasons of excellent production cost, the melting time is preferably 24 hours or less, more preferably 12 hours or less, even more preferably 10 hours or less, even more preferably 8 hours or less, particularly preferably 6 hours or less, and most preferably 4 hours or less.

[0057] <<Stirring>> When the glass raw materials are heated and melted, they are preferably stirred using a stirrer at 20 to 60 rpm for 1 hour or more. This ensures that the glass raw materials are sufficiently melted, and tends to reduce the variation in the refractive index of the resulting glass member.

[0058] <<Grinding and Remelting>> The obtained molten glass may be subjected to water granulation one or more times, and then the granulated glass may be remelted. This makes it easier to reduce the variation in the refractive index of the obtained glass member.

[0059] <Cooling> The obtained molten glass is then cooled. At this time, it is preferable to cool (rapidly cool) the molten glass from the melting temperature described above to a cooling stop temperature described later. Thereafter, the molten glass is appropriately cooled to room temperature (for example, 25°C).

[0060] <<Cooling Stop Temperature>> The cooling stop temperature is, for example, 700 to 900°C, and preferably 750 to 850°C.

[0061] <<Cooling Rate>> From the viewpoint of reducing the amount of crystals contained in the resulting glass member, the cooling rate from the melting temperature to the cooling stop temperature is preferably 100°C / min or more, more preferably 200°C / min or more. On the other hand, from the viewpoint of suppressing the variation in the glass composition in the resulting glass member and from the viewpoint of ease of control during production of the glass member, this cooling rate is preferably 1500°C / min or less, more preferably 1000°C / min or less, even more preferably 800°C / min or less, and particularly preferably 500°C / min or less. Note that, if the cooling rate is within the above range, the variation in the glass composition caused by thermal convection during pouring is suppressed, and the variation in the refractive index of the resulting glass member is easily reduced.

[0062] <<Shaping>> The molten glass is preferably formed into a desired shape and then cooled. The forming method is not particularly limited, and examples thereof include a float method, a press method, a fusion method, and a down-draw method. The obtained molten glass may be formed into a provisional shape, cooled, and the resulting provisionally shaped body may be subjected to processing such as cutting.

[0063] <<Slow Cooling>> The formed glass may be slowly cooled to remove strain within the glass. In this case, for example, the glass is held at a given temperature for a certain period of time and then cooled to room temperature (e.g., 25°C). The temperature at which the glass is held (holding temperature) is preferably a temperature near the glass transition point, for example, because strain can be efficiently removed. Specifically, for example, 700 to 1100°C is preferred, and 850 to 950°C is more preferred. The time for which the glass is held at the holding temperature (holding time) is, for example, 1 to 10 hours, and preferably 2 to 5 hours. The holding time is preferably longer the larger and more complex the shape of the glass. The cooling rate from the holding temperature to room temperature is, for example, 0.1 to 5°C / min, and preferably 0.5 to 1°C / min.

[0064] In this way, a glass member having a desired shape is obtained. The obtained glass member may be subjected to treatments such as grinding and polishing, if necessary.

[0065] <<Log η During Pouring>> The viscosity log η of the molten glass during pouring for cooling or the like is preferably 0.5 Pa s or more. This is because variations in the glass composition caused by thermal convection during pouring are suppressed, and variations in the refractive index of the resulting glass member are reduced.

[0066] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the examples described below.

[0067] [Test A: Examples A1 to A11] Below, Examples A1 to A10 are working examples, and Example A11 is a comparative example. 2 : 59 mol%, Y 2 O 3 :22mol%, Al 2 O 3The glass raw materials were weighed and mixed so that the water content of the glass raw materials was 19 mol %. The water content of the glass raw materials is shown in Table 1 below. The mixed glass raw materials were placed in a platinum crucible, and then charged into an electric furnace, and melted by heating at a melting temperature of 1600°C (melting time: 3 hours), to obtain molten glass. An atmospheric gas was introduced into the melting atmosphere under the conditions shown in Table 1 below. However, when the melting was carried out in the air atmosphere without introducing the atmospheric gas, this is recorded as "air" in Table 1 below. Nitrogen gas (N 2 ) and oxygen gas (O 2 ) in a volume ratio of 8 / 2 (N 2 / O 2 ) in combination, the following table 1 shows "N 2 +O 2 The obtained molten glass was cooled from the melting temperature to a cooling stop temperature of 800°C at a cooling rate of 250°C / min, and then further cooled to room temperature (25°C) to obtain a glass member (dimensions: 100 mm x 100 mm x 15 mm). The H content and the contents of element b (Na, Fe, and Ti) in the obtained glass member are shown in Table 1 below.

[0068] <Etching rate> A test piece measuring 20 mm x 20 mm x 2 mm was cut out from a glass member, and the 20 mm x 20 mm surface was mirror-finished. Kapton tape was applied to a portion of the mirror-finished surface to mask it, and etching was performed with plasma gas under the following conditions: Apparatus: CCP-RIE Gas type: CF 4 (100 sccm) Output: 350 W Pressure: 10 Pa Time: 130 minutes Temperature: 20°C Then, a stylus surface profiler (Dectak 150, manufactured by ULVAC) was used to measure the step between the etched and non-etched areas to determine the amount of etching (amount of wear). Furthermore, the amount of etching was determined in the same manner for quartz glass. The ratio of the amount of etching of the glass member to the amount of etching of the quartz glass was determined as the etching rate. The results are shown in Table 1 below. The smaller the etching rate, the better the plasma resistance can be evaluated.

[0069]

[0070] <Summary of Evaluation Results> As shown in Table 1 above, the glass members of Examples A1 to A10, each having an H content of 200 ppm by mass or less, had smaller etching rates and better plasma resistance than the glass member of Example A11, which had an H content of more than 200 ppm by mass.

[0071] [Test B: Examples B1 to B11] The following Examples B1 to B11 are examples. Glass members were obtained in the same manner as in Example A3 of Test A, except that the glass raw materials were weighed so as to obtain the compositions shown in Table 2 below. However, the cooling rate from the melting temperature to the cooling stop temperature was set to the rate shown in Table 2 below. The H content, average refractive index, refractive index variation, Young's modulus, expansion coefficient, transmittance, number of bubbles, crystal ratio, and etching rate of the obtained glass members are shown in Table 2 below.

[0072]

[0073] <Summary of Evaluation Results> As shown in Table 2 above, the glass members of Examples B1 to B11, which had an H content of 200 mass ppm or less, had good plasma resistance.

[0074] [Test C: Examples C1 to C20] Hereinafter, Examples C1 to C20 are examples. Glass members having the dimensions shown in Table 3 were obtained in the same manner as in Example A3 of Test A, except that the glass raw materials were weighed to obtain the compositions shown in Table 3 below. The surfaces of the obtained glass members were processed so that the surface roughness (Ra) and flatness would be the values ​​shown in Table 3 below. However, the melting time was set to the temperature shown in Table 3 below. The cooling rate from the melting temperature to the cooling stop temperature was set to the rate shown in Table 3 below. The H content, average refractive index, refractive index variation, Young's modulus, expansion coefficient, transmittance, number of bubbles, crystal ratio, and etching rate of the obtained glass members are shown in Table 3 below.

[0075]

[0076] <Summary of Evaluation Results> As shown in Table 3 above, the glass members of Examples C1 to C20, which had an H content of 200 mass ppm or less, had good plasma resistance.

[0077] Although various embodiments have been described above, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the claims, and it is understood that these also naturally fall within the technical scope of the present invention. Furthermore, the components of the above embodiments may be combined in any manner as long as they do not deviate from the spirit of the invention.

[0078] This application is based on a Japanese patent application (Patent Application No. 2023-068600) filed on April 19, 2023, the contents of which are incorporated herein by reference.

Claims

1. A glass component used in semiconductor manufacturing equipment, the glass component having a hydrogen content of 200 ppm by mass or less.

2. The glass member according to claim 1, wherein the average refractive index at a wavelength of 365 nm is 1.5 or more, and the difference between the upper and lower limits is 0.2 or less.

3. 10 cm 2 The glass member of claim 1 having a cross-sectional area of ​​at least 100 mm.

4. The glass member according to claim 1, which is ring-shaped with an outer diameter of 300 to 600 mm, an inner diameter of 200 to 450 mm, and a thickness of 2 to 30 mm, which is chamfered to C1.0 or less, has a surface roughness Ra of 1 μm or less, and a flatness of 0.5 mm or less.

5. The glass member according to claim 1, which contains yttrium and silicon, and has a molar ratio Y / Si of the content of yttrium to the content of silicon of 0.2 to 1.

5.

6. SiO 2 The content of Y is 40 to 70 mol %. 2 O 3 The content of Al is 5 to 40 mol %. 2 O 3 2. The glass member according to claim 1, wherein the content of 7. The glass member according to claim 6, wherein the content of at least one element a selected from the group consisting of tantalum, boron, magnesium, calcium, strontium and barium is 10 mol % or less in terms of oxide.

8. The glass member according to claim 6, wherein the content of at least one element b selected from the group consisting of alkali metal elements, iron and titanium is 3,000 ppm by mass or less in terms of oxide.

9. The glass member according to claim 1, which has a Young's modulus of 100 GPa or more and an average thermal expansion coefficient at 50 to 350° C. of 4 to 7 ppm / K.

10. The glass member according to claim 1, which has a transmittance of 92% or less at a wavelength of 800 nm.

11. Any 100 mm 2 0.1 mm in 10 areas 2 2. The glass member according to claim 1, wherein the total number of bubbles is 40 or less.

12. Any 100 mm 2 0.1 mm in 10 areas 2 2. The glass member according to claim 1, wherein the area ratio of the above crystals is 5% or less on average.

13. The glass member according to claim 1, which is used as a focus ring, a shower plate, an electrostatic chuck, a susceptor, an injector, an observation window, a top plate, or a side wall of the semiconductor manufacturing equipment.

14. Flow rate: 100 sccm CF 4 2. The glass member according to claim 1, wherein the etching rate when etched with a gas is 0.1 or less with respect to quartz.

15. A method for producing a glass member according to any one of claims 1 to 14, comprising heating a glass raw material to a melting temperature of 1500 to 1800°C to melt it, and cooling the resulting molten glass to a cooling stop temperature of 700 to 900°C at a cooling rate of 100 to 1500°C / min.

Citation Information

Patent Citations

  • Production of high purity transparent silica glass

    JP1999209132A

  • Plasma corrosion resisting silica glass, manufacturing method therefor and apparatus using the same

    JP2003292337A

  • Synthetic silica glass member for optical use and its manufacturing process

    JP2004123420A

  • Optical component made from synthetic quartz glass with enhanced irradiation resistance, and method for manufacturing the optical component.

    JP2010519751A