Negative photosensitive resin composition, method for producing cured relief pattern using same, and cured film

The negative photosensitive resin composition, featuring a polyimide resin and nitrogen-containing heterocyclic compounds, addresses curing shrinkage and adhesion issues, enhancing the reliability and flatness of semiconductor packages by improving cure residual film rate and copper adhesion.

WO2024219463A1PCT designated stage expired Publication Date: 2024-10-24ASAHI KASEI KOGYO KABUSHIKI KAISHA

Patent Information

Application Number
PCT/JP2024/015413
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional negative photosensitive resin compositions used in semiconductor manufacturing face challenges with curing shrinkage, copper adhesion, and elongation of the cured film, which affect the flatness and reliability of semiconductor packages, particularly in flip-chip mounting and fan-out wafer level packaging processes.

Method used

A negative photosensitive resin composition comprising a polyimide resin, a nitrogen-containing heterocyclic compound, and a photopolymerization initiator, with optional additives such as radically polymerizable compounds, thermal crosslinking agents, and silane coupling agents, is developed to enhance cure residual film rate, copper adhesion, and elongation of the cured film.

Benefits of technology

The composition effectively suppresses curing shrinkage, improves copper adhesion, and increases the elongation of the cured film, leading to improved flatness and reliability of semiconductor packages, particularly in high-speed and high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a negative photosensitive resin composition containing (A) 100 parts by mass of a polyimide resin, (B) 0.01 to 10 parts by mass of a nitrogen-containing heterocyclic compound, and (C) 1 to 30 parts by mass of a photopolymerization initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Negative-type photosensitive resin composition, method for producing cured relief pattern using the same, and cured film

[0001] The present disclosure relates to a negative-type photosensitive resin composition, a method for producing a cured relief pattern using the same, and a cured film.

[0002] Conventionally, polyimide resins, polybenzoxazole resins, phenolic resins, and the like, which have excellent heat resistance and electrical and mechanical properties, have been used as insulating materials for electronic components, and passivation films, surface protective films, interlayer insulating films, and the like for semiconductor devices. Among these resins, those provided in the form of a photosensitive resin composition can easily form a heat-resistant relief pattern film by coating, exposing, developing, and curing the composition to a ring closure treatment (imidization, benzoxazole formation) or thermal crosslinking, and therefore have the advantage of enabling a significant reduction in the process compared to conventional non-photosensitive materials, and are therefore used in the production of semiconductor devices.

[0003] Semiconductor devices (hereinafter also referred to as "elements") are mounted on printed circuit boards by various methods depending on the purpose. Conventional elements have generally been fabricated using wire bonding, which connects the external terminals (pads) of the element to the lead frame with thin wires. However, as elements have become faster and their operating frequencies have reached the GHz range, differences in the wiring length of each terminal during mounting have come to affect the operation of the element. Therefore, when mounting elements for high-end applications, it has become necessary to accurately control the length of the mounting wiring, and wire bonding has become difficult to meet this requirement.

[0004] To address this issue, flip-chip packaging has been proposed, in which a redistribution layer is formed on the surface of a semiconductor chip, bumps (electrodes) are formed on the redistribution layer, and the chip is then flipped over and directly mounted on a printed circuit board. Because flip-chip packaging allows for precise control of wiring distance, it has been adopted for high-end applications that handle high-speed signals, and for mobile phones and other devices due to its small packaging size, resulting in rapidly expanding demand. More recently, a semiconductor chip packaging technology called fan-out wafer-level packaging (FOWLP) has been proposed, in which individual chips are manufactured by dicing a pre-processed wafer, the individual chips are reassembled on a support, encapsulated with molding resin, and a redistribution layer is formed after the support is peeled off. In FOWLP, the redistribution layer is formed with a thin film thickness, which allows for a thinner package, as well as the advantages of high-speed transmission and low cost.

[0005] On the other hand, in FOWLP, the redistribution layer is multilayered, and therefore, in the photolithography process using photoresist, if the flatness of the photosensitive resin composition is poor, deviations in focus depth occur, resulting in a significant deterioration in resolution. Therefore, high flatness of the photosensitive resin composition is required. Furthermore, because the copper wiring and the redistribution layer are in contact due to the package structure, the photosensitive resin composition must also have good adhesion to copper. Furthermore, film properties (especially elongation) are also important because if the redistribution layer breaks, insulation properties cannot be maintained, leading to package damage.

[0006] To flatten the rewiring layer, it is important to achieve in-plane uniformity during spin coating of the photosensitive resin composition and to suppress cure shrinkage during heat curing. The flatness of the rewiring layer (i.e., flatness after curing) is determined by the sum of the in-plane uniformity during spin coating and the amount of cure shrinkage during heating. Known methods for improving in-plane uniformity during spin coating include using a highly soluble polyimide precursor or a low-molecular-weight polymer.

[0007] For example, Patent Document 1 discloses a technique for improving in-plane uniformity during spin coating by using a low-molecular-weight polyimide precursor. Also, for example, Patent Document 2 discloses a negative-type photosensitive resin composition that has excellent mechanical strength and suppresses cure shrinkage by using a polyfunctional (meth)acrylate in a polyimide resin.

[0008] Furthermore, for example, Patent Documents 3 and 4 disclose methods of adding purine derivatives or compounds having a heterocycle and an amino group to improve copper adhesion.

[0009] International Publication No. 2018 / 037997 Japanese Patent Application Laid-Open No. 2021-152634 Japanese Patent Application Laid-Open No. 2012-194520 International Publication No. 2021 / 157571

[0010] When the polyimide precursor described in Patent Document 1 is used, curing shrinkage due to ring closure is large, leaving room for improvement. Large curing shrinkage reduces the remaining film rate (also referred to as the cured remaining film rate in the present disclosure) and reduces flatness. Furthermore, in Patent Document 2, the addition of a polyfunctional (meth)acrylate suppresses the interaction between the polymer and the copper interface, so improvements in adhesion to copper and elongation of the cured film are required.

[0011] Furthermore, the compositions described in Patent Documents 3 and 4 have the problem that the film properties such as cure shrinkage and elongation of the cured film are insufficient.

[0012] The present disclosure aims to provide a negative-tone photosensitive resin composition capable of forming a cured relief pattern having a high cure residual film rate, high copper adhesion, and high elongation of the cured film, as well as a method for producing a cured relief pattern using the same, and a cured film.

[0013] That is, the present invention is as follows.

[0014] [1] A negative-tone photosensitive resin composition comprising: (A) 100 parts by mass of a polyimide resin; (B) 0.01 to 10 parts by mass of a nitrogen-containing heterocyclic compound; and (C) 1 to 30 parts by mass of a photopolymerization initiator. [2] The negative-tone photosensitive resin composition according to [1], wherein the polyimide resin (A) does not have a radical polymerizable group, a hydroxyl group, and / or a carboxyl group in its side chain. [3] The negative-tone photosensitive resin composition according to [1] or [2], wherein the polyimide resin (A) has a reactive group at its terminal. [4] The negative-tone photosensitive resin composition according to any one of [1] to [3], wherein the polyimide resin (A) has an alicyclic structure in an amount of 20 mol % to 70 mol %. [5] The negative-tone photosensitive resin composition according to any one of [1] to [4], wherein the nitrogen-containing heterocyclic compound (B) is an azole compound or a purine compound. [6] The negative-tone photosensitive resin composition according to [5], wherein the azole compound is 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 1H-tetrazole-5-carboxylic acid, 1H-tetrazole-5-ethyl carboxylate, 1H-tetrazole-5-acetic acid, or 1H-tetrazole-5-ethyl acetate. [7] The negative-tone photosensitive resin composition according to [5] or [6], wherein the purine compound is 8-azaadenine or 8-azaguanine, adenine, N,N-dimethyladenine, or hypoxanthine. [8] The negative-tone photosensitive resin composition according to any one of [5] to [7], wherein the purine compound is 8-azaadenine or 8-azaguanine. [9] The negative-tone photosensitive resin composition according to any one of [1] to [8], further comprising (D) a radically polymerizable compound.

[10] The negative photosensitive resin composition according to any one of [1] to [9], further comprising (E) a thermal crosslinking agent.

[11] The negative photosensitive resin composition according to any one of [1] to

[10] , further comprising (F) a silane coupling agent.

[12] The negative photosensitive resin composition according to any one of [1] to

[11] , further comprising (G) an organotitanium compound.

[13] The negative photosensitive resin composition according to any one of [1] to

[12] , further comprising (H) a thermal polymerization inhibitor.

[14] The negative-type photosensitive resin composition according to any one of [1] to

[13] , further comprising (I) a solvent.

[15] The negative-type photosensitive resin composition according to any one of [1] to

[14] , wherein the weight-average molecular weight of the (A) polyimide resin is 5,000 to 100,000.

[16] The negative-type photosensitive resin composition according to any one of [1] to

[15] , wherein the (A) polyimide resin comprises a structure represented by the following general formula (1): {In formula (1), X 1 is a tetravalent organic group, and Y 1 is a divalent organic group, and n is an integer of 1 to 150.}

[17] X in the general formula (1) 1 The negative photosensitive resin composition according to

[16] , wherein:

[18] X in the general formula (1) 1

[19] The negative photosensitive resin composition according to

[17] , wherein Y in the general formula (1) is any one of the structures represented by the general formulas (7) to (9). 1 The negative photosensitive resin composition according to any one of

[16] to

[18] , wherein the compound is a compound represented by any one of the following general formulas (11) to (19):

[20] Y in the general formula (1) 1

[21] The negative photosensitive resin composition according to

[19] , wherein X in the general formula (1) is any one of the structures represented by the general formulas (13) to (16). 1 is any one of the structures represented by the general formulas (7) to (9), and Y 1

[22] The negative photosensitive resin composition according to any one of

[16] to

[21] , wherein a terminal of the polyimide resin (A) contains an acid anhydride group, a carboxyl group, an amino group, or any structure represented by the following general formulas (20) to (22): (In the formula, R 1 , and R 2 are each independently selected from a hydrogen atom and a monovalent organic group having 1 to 3 carbon atoms; R 3 is an organic group having 1 to 20 carbon atoms which may contain a heteroatom, and k is an integer of 1 or 2. 4 represents a hydrogen atom or an organic group having 1 to 4 carbon atoms, and * represents the bonding site with the end of the polyimide resin (A). (In the formula, R 5 , and R 6 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms. * indicates the bonding site with the terminal of the (A) polyimide resin. (In the formula, R 7 , R 8 , and R 9 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and j is an integer of 2 to 10. Also, * represents a bonding site with an end of the (A) polyimide resin.)

[23] A method for producing a cured relief pattern, comprising the following steps: (1) applying the negative photosensitive resin composition according to any one of [1] to

[22] onto a substrate to form a photosensitive resin layer on the substrate, (2) exposing the photosensitive resin layer to light, (3) developing the exposed photosensitive resin layer to form a relief pattern, and (4) heat-treating the relief pattern to form a cured relief pattern.

[24] A cured film comprising a cured product of the negative photosensitive resin composition according to any one of [1] to

[22] .

[0015] According to the present disclosure, it is possible to provide a negative-type photosensitive resin composition capable of forming a cured relief pattern that exhibits reduced cure shrinkage, high copper adhesion, and high elongation in the cured film, as well as a method for producing a cured relief pattern using the same, and a cured film.

[0016] Hereinafter, embodiments of the present disclosure will be described in detail. Throughout this specification, when a structure represented by the same symbol in a general formula is present in a molecule, it is independently selected and may be the same or different from each other unless otherwise specified. Furthermore, structures represented by a common symbol in different general formulas are also independently selected and may be the same or different from each other unless otherwise specified.

[0017] In the following description, the upper or lower limit of a numerical range described in stages may be replaced with the upper or lower limit of another numerical range described in stages. Also, in the following description, the upper or lower limit of a certain numerical range may be replaced with a value described in an example. Furthermore, with regard to the term "step" in the following description, not only an independent step but also a step that cannot be clearly distinguished from other steps may be included in this term as long as the function of that "step" is achieved.

[0018] <Negative Photosensitive Resin Composition> The negative photosensitive resin composition of the present disclosure (hereinafter referred to as "photosensitive resin composition") contains (A) a polyimide resin, (B) a nitrogen-containing heterocyclic compound, and (C) a photopolymerization initiator. If desired, the negative photosensitive resin composition of the present disclosure may further contain, in addition to the above components, (D) a radical polymerizable compound, (E) a thermal crosslinking agent, (F) a silane coupling agent, (G) an organotitanium compound, (H) a thermal polymerization inhibitor, (I) a solvent, and other components.

[0019] (A) Polyimide Resin The negative photosensitive resin composition of the present disclosure contains (A) a polyimide resin.

[0020] The polyimide resin (A) does not generate any resin-derived elimination components, and therefore can suppress the cure shrinkage of the negative-tone photosensitive resin composition, resulting in a high cure residual film rate and improved post-cure flatness compared to commonly used polyimide precursors. Furthermore, the use of the polyimide resin (A) can also suppress deterioration in the storage stability of the negative-tone photosensitive resin composition due to the inclusion of the basic nitrogen-containing heterocyclic compound (B).

[0021] In one embodiment, the polyimide resin (A) may have a polymerizable group in a side chain, but preferably does not have a polymerizable group in a side chain from the viewpoint of the elongation and storage stability of the cured film. In one embodiment, examples of the polymerizable group include a radical polymerizable group, a hydroxyl group, and / or a carboxyl group. Furthermore, the polyimide resin (A) preferably has an alicyclic structure in an amount of 20 mol% to 70 mol% inclusive, since the negative-type photosensitive resin composition of this embodiment has excellent coating film uniformity and cured film elongation. The alicyclic structure is more preferably 22 mol% or more, more preferably 55 mol% or less, even more preferably 35 mol% or less, and particularly preferably 30 mol% or less.

[0022] In this specification, an alicyclic structure refers to a structure in which three or more carbon atoms are bonded in a ring, and is not aromatic. The alicyclic structure of the present disclosure is a structure in which three or more carbon atoms, preferably four to twenty carbon atoms, and more preferably six to ten carbon atoms, are bonded in a ring. The alicyclic structure is a structure derived from a tetracarboxylic dianhydride or a diamine. Specific examples of the alicyclic structure include, but are not limited to, cycloalkane structures such as cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, and cyclooctane, chair structures such as bicyclooctane and bicyclooctene, and structures represented by the following formulas (34) to (36). From the viewpoint of the physical properties of the cured film, the alicyclic structure contained in the polyimide (A) is preferably a cycloalkane structure or a chair structure, and the chair structure is preferably bicyclooctane or bicyclooctene.

[0023] The content of the alicyclic structure in the polyimide resin (A) can be calculated by dividing the number of moles of the tetracarboxylic dianhydride and diamine having an alicyclic structure, among the tetracarboxylic anhydrides and diamines used as raw materials for the polyimide resin (A), by the total amount of the tetracarboxylic anhydride and diamine, and multiplying the result by 100. That is, the content (mol %) of the alicyclic structure in the polyimide resin (A) is expressed by the following formula (i):

[0024] The polyimide resin of the present disclosure preferably does not substantially contain a polyamic acid or polyamic acid ester structure. In the present disclosure, "substantially does not contain" means, for example, that the imidization rate of the polyimide resin is 90% or more, preferably 95% or more. The imidization rate of the polyimide resin can be measured by a known method, but can also be easily calculated, for example, by the following method. First, the infrared absorption spectrum of the polyimide resin is measured, and the absorption peak of the imide structure (1780 cm -1 Near 1377 cm -1 Next, the polyimide resin is heat-treated at 350°C for 1 hour, and the infrared absorption spectrum of the heat-treated polyimide is measured. -1 The imidization rate of the polyimide resin is calculated by comparing the peak intensity in the vicinity with the peak intensity of the polyimide before heat treatment.

[0025] The polyimide resin (A) used in the present disclosure is synthesized from a tetracarboxylic dianhydride and a diamine.

[0026] The polyimide resin (A) preferably contains a structure represented by general formula (1) from the viewpoint of solubility in a solvent and flatness during coating. This structure is also suitable for a solvent-developable negative-tone photosensitive resin composition. {In formula (1), X 1 is a tetravalent organic group, and Y 1 is a divalent organic group, and n is an integer from 1 to 150.

[0027] X 1is a tetravalent organic group, and is not particularly limited as long as it has a structure derived from a known tetracarboxylic dianhydride. From the viewpoint of excellent effects of the present embodiment and solubility in the solvent (I) described later, X 1 Preferably, X has at least one structure represented by the following formulas (2) to (10), and from the viewpoint of the elongation of the cured film, 1 More preferably, the compound contains two or more structures represented by the following formulas (2) to (10).

[0028] Also, X 1 Preferably, X has at least one structure represented by formulas (2) to (9) from the viewpoint of the elongation and chemical resistance of the cured film obtained from the negative photosensitive resin composition of the present disclosure. 1 From the viewpoint of the heat resistance of the cured film obtained from the negative photosensitive resin composition of the present disclosure, it is more preferable that X has at least one structure represented by formulas (2) to (4) and formulas (6) to (9). 1 Since the negative photosensitive resin composition of the present disclosure has particularly excellent coating film uniformity and cured film elongation, it preferably has at least one structure represented by formula (2) and formulas (7) to (9), and particularly preferably has any one of the structures represented by formulas (7) to (9).

[0029] Y in formula (1) 1 is a divalent organic group, and is not particularly limited as long as it has a structure derived from a known diamine. 1 From the viewpoint of excellent effects of this embodiment and (I) solubility in solvents, it is preferable that the compound has at least one structure represented by the following formulas (11) to (19).

[0030] Also, Y 1 From the viewpoint of the elongation and chemical resistance of the cured film obtained from the negative photosensitive resin composition of the present disclosure, it is preferable that Y has at least one structure represented by formulas (11) to (17). 1 From the viewpoint of the mechanical properties of the cured film obtained from the negative photosensitive resin composition of the present disclosure, it is more preferable that Y has at least one structure represented by formulas (11) to (16). 1 It is particularly preferred that the negative photosensitive resin composition of the present disclosure have at least one structure represented by formulas (13) to (16) because the coating film uniformity and cured film elongation of the composition are particularly excellent. The excellent solubility of the structures represented by formulas (13) to (16) in solvents is due to the fact that these structures have a pendant phenyl structure.

[0031] In formula (1), n ​​is an integer of 1 to 150, which satisfies the weight average molecular weight of the polyimide resin (A) described below.

[0032] From the viewpoints of solubility in (I) solvents (described below) and the elongation of cured films obtained from the negative-tone photosensitive resin composition of the present disclosure, it is preferable for the (A) polyimide resin to have a reactive group at its terminal, preferably at its main chain terminal. The reactive group of the present disclosure may be any group reactive with compounds contained in the negative-tone photosensitive resin composition of the present disclosure, such as radically polymerizable compounds and (B) nitrogen-containing heterocyclic compounds. Specific examples of the reactive group include groups having a polymerizable double bond, acid anhydride groups, carboxyl groups, and amino groups. In one embodiment, it is preferable for the terminal of the (A) polyimide resin to contain an acid anhydride group, a carboxyl group, an amino group, or any of the structures represented by the following general formulas (20) to (22).

[0033] The group having a polymerizable double bond preferably has any of the structures represented by the following general formulas (20) to (22). (In the formula, R 1 , and R 2 are each independently selected from a hydrogen atom and a monovalent organic group having 1 to 3 carbon atoms; R 3is an organic group having 1 to 20 carbon atoms which may contain a heteroatom, and k is an integer of 1 or 2. 4 represents a hydrogen atom or an organic group having 1 to 4 carbon atoms, and * represents the bonding site with the end of the polyimide resin (A). (In the formula, R 5 , and R 6 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms. * indicates the bonding site with the end of the (A) polyimide resin. (In the formula, R 7 , R 8 , and R 9 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and j is an integer of 2 to 10. * indicates the bonding site with the end of the (A) polyimide resin.

[0034] The acid anhydride group is derived from the raw material tetracarboxylic acid anhydride, the carboxyl group is formed by ring-opening of the aforementioned acid anhydride group, and the amino group is derived from the raw material diamine. More specific examples of the (A) polyimide resin having a terminal structure represented by general formula (20) include those represented by the following formulas (23) to (26). (In the formula, * indicates the bonding site with the end of the polyimide resin (A).) More specific examples of the general formula (21) include those represented by the following formulas (27) and (28). (In the formula, * indicates the bonding site with the terminal of the polyimide resin (A).)

[0035] More specific examples of the compound represented by general formula (22) include those represented by the following formulae (29) to (32). (In the formula, * indicates the bonding site with the terminal of the polyimide resin (A).)

[0036] In view of the elongation, chemical resistance and solubility in solvents of the cured film, X in general formula (1) 1is any one of the structures represented by general formulas (2) to (10), and Y 1 is preferably any one of the structures represented by general formulas (11) to (19), and X in general formula (1) 1 is any one of the structures represented by general formulas (7) to (9), and Y 1 is more preferably any of the structures represented by general formulas (13) to (16).

[0037] The weight-average molecular weight (Mw) of the (A) polyimide resin is not particularly limited as long as it is within the range in which it can be dissolved in the (I) solvent. From the viewpoint of the film properties and copper adhesion of the cured film obtained from the negative photosensitive resin composition of the present disclosure, the weight-average molecular weight of the (A) polyimide resin is preferably 5,000 or more and 100,000 or less. From the viewpoint of mechanical properties, the lower limit of the weight-average molecular weight of the (A) polyimide resin is more preferably 6,000 or more, and even more preferably 8,000 or more. Furthermore, from the viewpoint of solubility in the (I) solvent and flatness during coating, the upper limit of the weight-average molecular weight of the (A) polyimide resin is more preferably 50,000 or less, and particularly preferably 30,000 or less. The weight-average molecular weight (Mw) of each resin, such as the (A) polyimide resin, is measured by the method described in the Examples.

[0038] The molecular weight distribution (Mw / Mn) of the (A) polyimide resin is preferably 1.0 or more and 2.0 or less. From the viewpoint of production efficiency, the lower limit of the molecular weight distribution of the (A) polyimide resin is more preferably 1.15 or more, and even more preferably 1.25 or more. From the viewpoint of resolution, the upper limit of the molecular weight distribution of the (A) polyimide resin is more preferably 1.8 or less, and even more preferably 1.6 or less.

[0039] The polyimide resin (A) is obtained by reacting a tetracarboxylic dianhydride with a diamine to obtain a polyamic acid, and then imidizing the polyamic acid by dehydration and ring closure.

[0040] The method for dehydrating and cyclizing the polyamic acid is not limited as long as it is a known method, and examples thereof include a thermal imidization method in which the polyamic acid is heated at a high temperature to dehydrate and cyclize, and a chemical imidization method in which the polyamic acid is dehydrated and cyclized by adding acetic anhydride and a tertiary amine, which are dehydrating and reducing agents.

[0041] The temperature in the thermal imidization method is not particularly limited, but since the ring-closing reaction may not be completed at a low temperature, the lower limit is preferably 150° C. or higher, more preferably 160° C. or higher. On the other hand, since a side reaction may proceed at a high temperature, the upper limit is preferably 200° C. or lower, more preferably 180° C.

[0042] The tetracarboxylic dianhydride is not particularly limited, but specific examples include pyromellitic anhydride (PMDA), 4,4'-oxydiphthalic anhydride (ODPA), 3,4'-oxydiphthalic anhydride, 4,4'-biphthalic dianhydride (BPDA), 3,4'-biphthalic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BP AF), norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride (CpODA), bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (BCD), 1,2,3,4-cyclobutanetetracarboxylic anhydride (CBDA), and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA).

[0043] The diamine is not particularly limited, but specific examples include 4,4'-diaminodiphenyl ether (DADPE), 3,4'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 2-phenoxybenzene-1,4-diamine (PND), 9,9-bis(4-aminophenyl)fluorene (BAFL), 6-(4-aminophenoxy)biphenyl-3-amine (PDPE), 3,3'- ... and 2,2-bis[3-phenyl-4-(4-aminophenoxy)phenyl]propane (DAOPPA), 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine (TFMB), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP), and 2-(methacryloyloxy)ethyl-3,5-diaminobenzoate (MAEDAB).

[0044] When the terminals of the (A) polyimide resin are an acid anhydride group, a carboxyl group, and an amino group, the (A) polyimide resin is a polyimide obtained by imidizing a polyamic acid obtained by reacting a tetracarboxylic dianhydride with a diamine, followed by dehydration and ring closure of the polyamic acid.

[0045] The terminals of the polyimide resin (A) may be converted to structures represented by general formulas (20) to (22) by reacting the acid anhydride group, carboxyl group, and amino group at the terminals of the polyimide resin (A) with a predetermined compound.

[0046] The polyimide resin (A) whose terminal has a structure represented by the general formula (20) can be obtained, for example, by reacting the amino group at the polyimide terminal with an isocyanate compound.

[0047] Specific examples of the isocyanate compound include 2-methacryloyloxyethyl isocyanate (2-isocyanatoethyl methacrylate: MOI), 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate.

[0048] The method for reacting the isocyanate compound is not particularly limited, but the compound can be reacted with the amino groups of the dehydrated ring-closed polyimide by stirring at room temperature.

[0049] The polyimide resin (A) whose terminal has a structure represented by the general formula (21) can be obtained, for example, by reacting the amino group at the polyimide terminal with a chloride compound.

[0050] Examples of the chloride compounds include acryloyl chloride and methacryloyl chloride.

[0051] The method for reacting the chloride compound is not particularly limited, but the dehydrated, ring-closed polyimide solution can be cooled with ice, and the chloride compound can be added dropwise to react with the amino groups of the dehydrated, ring-closed polyimide.

[0052] The polyimide resin (A) whose terminals have a structure represented by general formula (22) can be obtained, for example, by reacting the acid anhydride group and carboxyl group at the polyimide terminals with an alcohol compound.

[0053] Examples of alcohol compounds include 2-hydroxyethyl methacrylate (2-hydroxyethyl methacrylate: HEMA), 2-hydroxyethyl acrylate, 4-hydroxyethyl methacrylate, and 4-hydroxyethyl acrylate.

[0054] The method for reacting the alcohol-based compound is not particularly limited, but it can be reacted with the acid anhydride group and carboxyl group of the dehydration-ring-closed polyimide using a condensing agent such as N,N'-dicyclohexylcarbodiimide (DCC) or an esterification catalyst such as p-toluenesulfonic acid.

[0055] (A) In the production of polyimide resin, a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the tetracarboxylic dianhydride, diamine, and compound having a terminal polymerizable functional group. Examples of reaction solvents include γ-butyrolactone (GBL), dimethyl sulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.

[0056] When a thermal imidization method is used in the production of (A) polyimide resin, an azeotropic solvent may be used to promote the imidization reaction. The azeotropic solvent is not particularly limited as long as it is a solvent that forms an azeotrope with water, and examples thereof include toluene, ethyl acetate, N-dicyclohexylpyrrolidone, orthodichlorobenzene, xylene, and benzene.

[0057] The polyimide resin (A) may be purified by a known method such as that described in JP 2012-194520 A. Examples of the purification method include a method in which a solution of the polyimide resin (A) is dropped into water to remove unreacted materials by reprecipitation, a method in which a condensing agent insoluble in the reaction solvent is removed by filtration, and a method in which the catalyst is removed using an ion exchange resin. After such purification, the polyimide resin (A) may be dried by a known method and isolated in a powder state.

[0058] The (A) polyimide resin is contained in an amount of preferably 20 to 70% by mass, more preferably 25 to 65% by mass, based on the negative photosensitive resin composition of the present disclosure.

[0059] (B) Nitrogen-Containing Heterocyclic Compound The negative-type photosensitive resin composition of the present disclosure contains (B) a nitrogen-containing heterocyclic compound. By including (B), the negative-type photosensitive resin composition of the present disclosure can achieve high cure film retention, copper adhesion, and elongation of the cured film.

[0060] While (B) nitrogen-containing heterocyclic compounds are known to improve adhesion to copper, the present inventors have discovered that the use of (A) polyimide resin and (B) nitrogen-containing heterocyclic compound exhibits a unique effect of improving film properties (in one embodiment, the elongation of the cured film). While the mechanism is unclear, it is presumed that, since (A) polyimide resin already has a closed-ring structure (imide group) in the negative-tone photosensitive resin composition of the present disclosure, the imide group and (B) nitrogen-containing heterocyclic compound form an intermolecular network, such as a hydrogen bond, during application of the photosensitive resin composition, thereby improving the elongation of the cured film. On the other hand, the polyimide precursor does not have a closed-ring structure during application of the photosensitive resin composition, and the fluidity of the photosensitive resin composition is impaired during the heat treatment step in which imidization of the polyimide precursor progresses, so it is presumed that the formation of the aforementioned intermolecular network is difficult.

[0061] The nitrogen-containing heterocyclic compound (B) is not particularly limited, and examples thereof include an azole compound, a purine compound, etc. That is, the nitrogen-containing heterocyclic compound (B) is preferably at least one compound selected from the group consisting of an azole compound and a purine compound, and more preferably an azole compound or a purine compound.

[0062] Examples of the azole compounds include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, ... diphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 1-aminobenzotriazole, 2-aminobenzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 3-mercapto-1,2,4- triazole, 3-amino-5-mercapto-1,2,4-triazole, 3-amino-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, 5-amino-1,2,4-triazole-3-carboxylic acid, 3,5-diphenyl-1,2,4-triazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, 1H-tetrazole-5-carboxylic acid, α,Examples of such compounds include α-difluoro-2H-tetrazole-5-acetic acid, α-hydroxy-2H-tetrazole-5-acetic acid, α-amino-2H-tetrazole-5-acetic acid, methyl 1H-tetrazole-5-carboxylate, ethyl 1H-tetrazole-5-carboxylate, 1H-tetrazole-5-acetic acid, methyl 1H-tetrazole-5-acetate, ethyl 1H-tetrazole-5-acetate, propyl 1H-tetrazole-5-acetate, and azole compounds having a polymerizable group.

[0063] The azole compound having a polymerizable group is not particularly limited as long as it is an azole compound having a radical polymerizable group as the polymerizable group, and examples thereof include compounds represented by the following formula:

[0064] From the viewpoint of copper adhesion, the azole compound is particularly preferably at least one selected from the group consisting of 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 1H-tetrazole-5-carboxylic acid, ethyl 1H-tetrazole-5-carboxylate, 1H-tetrazole-5-acetic acid, and ethyl 1H-tetrazole-5-acetate. These azole compounds may be used alone or in a mixture of two or more. Typically, the azole compound is 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 1H-tetrazole-5-carboxylic acid, ethyl 1H-tetrazole-5-carboxylate, 1H-tetrazole-5-acetic acid, or ethyl 1H-tetrazole-5-acetate.

[0065] Specific examples of purine compounds include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminoadenine, 9-methyladenine, 2-hydroxy ...8-aminoadenine, 9-(2-hydroxyethyl)adenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoadenine, 9-aminoa aminoadenine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, 8-azahypoxanthine, and derivatives thereof.

[0066] Among these, from the viewpoint of copper adhesion, the purine compound is more preferably purine, adenine, guanine, 2,6-diaminopurine, 2-hydroxyadenine, 2-methyladenine, 2-fluoroadenine, 8-azaadenine, 8-azaguanine, or 8-azapurine, even more preferably 8-azaadenine, 8-azaguanine, adenine, N,N-dimethyladenine, or hypoxanthine, and most preferably 8-azaadenine or 8-azaguanine.

[0067] In the negative-type photosensitive resin composition of the present disclosure, the content of the (B) nitrogen-containing heterocyclic compound is 0.01 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. The lower limit of the (B) nitrogen-containing heterocyclic compound is preferably 0.05 parts by mass or more, more preferably 0.5 parts by mass or more, from the viewpoints of copper adhesion and the elongation of the cured film. The upper limit of the (B) nitrogen-containing heterocyclic compound is more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, from the viewpoints of photosensitivity and the elongation of the cured film. By containing the (B) nitrogen-containing heterocyclic compound within the range of this embodiment, the effects of this embodiment can be exhibited, but if the upper limit is exceeded, the (B) nitrogen-containing heterocyclic compound will precipitate, tending to reduce the elongation of the cured film.

[0068] (C) Photopolymerization initiator (C) is a compound that generates radicals when exposed to actinic rays and can polymerize an ethylenically unsaturated group-containing compound, etc. Examples of initiators that generate radicals when exposed to actinic rays include compounds containing structures such as benzophenone, N-alkylaminoacetophenone, oxime ester, acridine, phosphine oxide, and lophine. Specific examples include aromatic ketones such as benzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N,N',N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, acrylated benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide; benzoin ether compounds such as benzoin methyl ether, benzoin ethyl ether, and benzoin phenyl ether; benzoin compounds such as benzoin, methylbenzoin, and ethylbenzoin;1,2-Octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (manufactured by BASF Japan Ltd., Irgacure Oxe02), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(o-benzoyloxime) (manufactured by Changzhou New Power Electronic Materials Co., Ltd., PBG305), 1-(6-O-methylbenzoyl-9-ethylcarbazol-3-yl)-(3-cyclopentylacetone)-1-oxime acetate (manufactured by Changzhou New Power Electronic Materials Co., Ltd., TR-PBG-304), trade name: TR-PBG-3057 (Changzhou New Power Electronic Materials Co., Ltd.) Oxime ester compounds such as 1,2-propanedione,3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-,2-(O-acetyloxime) (manufactured by Nikko Chemtech Co., Ltd., product name: TR-PBG-326), trade name: NCI-730 (manufactured by ADEKA Corporation), trade name: NCI-831 (manufactured by ADEKA Corporation), and trade name: NCI-930 (manufactured by ADEKA Corporation); Examples of the photopolymerization initiator (C) include, but are not limited to, benzyl derivatives such as benzyl dimethyl ketal; acridine derivatives such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; N-phenylglycine derivatives such as N-phenylglycine; coumarin compounds; oxazole compounds; phosphine oxide compounds such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide; and lophine compounds such as 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole. The photopolymerization initiator (C) described above can be used alone or in combination of two or more. Among the above photopolymerization initiators, oxime ester compounds are more preferred, particularly from the viewpoint of resolution.

[0069] The content of the (C) photopolymerization initiator is 1 part by mass or more and 30 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. The lower limit of the photopolymerization initiator is preferably 2 parts by mass or more, from the viewpoints of photocurability and the elongation of the cured film. The upper limit of the photopolymerization initiator is preferably 20 parts by mass or less, from the viewpoints of curing the bottom of the relief pattern and the elongation of the cured film. By including the (C) photopolymerization initiator within the range of this embodiment, the effects of this embodiment are exhibited, but if the upper limit is exceeded, the (C) photopolymerization initiator becomes a foreign matter, and the elongation of the cured film tends to decrease.

[0070] (D) Radical Polymerizable Compound In order to improve the resolution of the cured relief pattern and suppress cure shrinkage during thermal curing, the photosensitive resin composition of the present disclosure may optionally contain (D) a radical polymerizable compound. As the (D) radical polymerizable compound, a (meth)acrylic compound that undergoes a radical polymerization reaction in the presence of (C) a photopolymerization initiator is preferred. In this specification, (meth)acrylic means methacrylic or acrylic, and (meth)acrylate means methacrylate or acrylate.

[0071] The radical polymerizable compound is not particularly limited, and examples thereof include monofunctional monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexyl (meth)acrylate, butoxydiethylene glycol methacrylate, isobornyl (meth)acrylate, m-phenoxybenzyl acrylate, o-phenylphenoxyethyl acrylate, 4-methacryloyloxybenzophenone, EO (ethylene oxide)-modified paracumylphenol acrylate, nonylphenoxyethyl acrylate, 6-acrylamidohexanoic acid, and tris-(2-acryloxyethyl)isocyanurate; Di(meth)acrylates of ethylene glycol or polyethylene glycol, including diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, di(meth)acrylates of propylene glycol or polypropylene glycol, di(meth)acrylate or tri(meth)acrylate of glycerol, cyclohexane di(meth)acrylate, di(meth)acrylate of 1,4-butanediol, di(meth)acrylate of 1,6-hexanediol, di(meth)acrylate of 1,9-nonanediol,di(meth)acrylate of 10-decanediol, di(meth)acrylate of neopentyl glycol, di(meth)acrylate of bisphenol A, (meth)acrylamide, derivatives thereof, trimethylolpropane tri(meth)acrylate, di(meth)acrylate or tri(meth)acrylate of glycerol, di(meth)acrylate, tri(meth)acrylate or tetra(meth)acrylate of pentaerythritol, dipentaerythritol poly(meth)acrylate, ethylene oxide (for example, 4-hydroxybutyl acrylate glycidyl ether) or propylene oxide adducts of these compounds, Examples of suitable urethane acrylates include trade names: KRM7735 (manufactured by Daicel-Allnex Corporation), EBECRYL230 (manufactured by Daicel-Allnex Corporation), EBECRYL4491 (manufactured by Daicel-Allnex Corporation), EBECRYL8413 (manufactured by Daicel-Allnex Corporation), EBECRYL8411 (manufactured by Daicel-Allnex Corporation), EBECRYL8402 (manufactured by Daicel-Allnex Corporation), EBECRYL8465 (manufactured by Daicel-Allnex Corporation), EBECRYL8667 (manufactured by Daicel-Allnex Corporation), EBECRYL4740 (manufactured by Daicel-Allnex Corporation), and KRM9276 (manufactured by Daicel-Allnex Corporation), and polyfunctional monomers such as tris-(2-hydroxyethyl)isocyanurate acrylate. Among these radical polymerizable compounds, it is preferable to include a compound having three or more radical polymerizable functional groups from the viewpoint of suppressing cure shrinkage.

[0072] The content of the radical polymerizable compound (D) in the photosensitive resin composition of the present disclosure is preferably 0.5 parts by mass to 100 parts by mass relative to 100 parts by mass of the polyimide resin (A). From the viewpoint of photocurability, the lower limit of the radical polymerizable compound is more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and particularly preferably 20 parts by mass or more. From the viewpoint of copper adhesion and bottom curing of the pattern, the upper limit of the radical polymerizable compound is more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less.

[0073] (E) Thermal Crosslinking Agent In order to suppress cure shrinkage of the cured polyimide film, the negative photosensitive resin composition of the present disclosure may optionally contain a thermal crosslinking agent.

[0074] The (E) thermal crosslinking agent refers to a compound that undergoes an addition reaction or a condensation polymerization reaction by heat. These reactions occur between the (A) polyimide resin and the (E) thermal crosslinking agent, between the (E) thermal crosslinking agents, and between the (E) thermal crosslinking agent and other components described below, and the reaction temperature is preferably 150°C or higher.

[0075] Examples of the (E) thermal crosslinking agent include an alkoxymethyl compound, an epoxy compound, an oxetane compound, a bismaleimide compound, an allyl compound, and a blocked isocyanate compound. From the viewpoint of suppressing cure shrinkage, the (E) thermal crosslinking agent preferably contains a nitrogen atom.

[0076] Examples of alkoxymethyl compounds include, but are not limited to, compounds of the following formula:

[0077] Examples of epoxy compounds include 4-hydroxybutyl acrylate glycidyl ether, epoxy compounds containing bisphenol A groups, and hydrogenated bisphenol A diglycidyl ether (for example, Epolight 4000 manufactured by Kyoeisha Chemical Co., Ltd.).

[0078] Examples of oxetane compounds include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, bis[1-ethyl(3-oxetanyl)]methyl ether, 4,4'-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl, 4,4'-bis(3-ethyl-3-oxetanylmethoxy)biphenyl, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, diethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, and bis(3-ethyl-3-oxetanylmethyl). Examples of suitable oxetane derivatives include diphenoate, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl)ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, poly[[3-[(3-ethyl-3-oxetanyl)methoxy]propyl]silasesquioxane] derivatives, oxetanyl silicate, phenol novolac-type oxetane, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, trade name: OXT121 (manufactured by Toagosei Co., Ltd.), and trade name: OXT221 (manufactured by Toagosei Co., Ltd.).

[0079] Examples of the bismaleimide compound include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,3-phenylenebis(maleimide), N,N'-1,4-phenylenebis(maleimide), 3-methyl-N,N'-1,4-phenylenebis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane.

[0080] Examples of the allyl compound include allyl alcohol, allyl anisole, allyl benzoate, allyl cinnamate, N-allyloxyphthalimide, allylphenol, allylphenylsulfone, allyl urea, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl maleate, diallyl isocyanurate, triallylamine, triallyl isocyanurate, triallyl cyanurate, triallylamine, triallyl 1,3,5-benzenetricarboxylate, triallyl trimellitate, triallyl phosphate, triallyl phosphite, and triallyl citrate.

[0081] Examples of the blocked isocyanate compound include hexamethylene diisocyanate-based blocked isocyanates (for example, manufactured by Asahi Kasei Corporation under the trade names Duranate SBN-70D, SBB-70P, SBF-70E, TPA-B80E, 17B-60P, MF-B60B, E402-B80B, MF-K60B, and WM44-L70G), manufactured by Mitsui Chemicals, Inc. under the trade name Takenate B-882N, manufactured by Baxenden (hereinafter under the trade names 7960, 7961, 7982, 7991, and 7992, etc.), tolylene diisocyanate-based blocked isocyanates (for example, manufactured by Mitsui Chemicals, Inc. under the trade name Takenate B-830, etc.), Examples of such blocked isocyanates include 4,4'-diphenylmethane diisocyanate-based blocked isocyanates (for example, manufactured by Mitsui Chemicals, Inc. under the trade name of Takenate B-815N, manufactured by Daiei Sangyo Co., Ltd. under the trade names of Bronate PMD-OA01 and PMD-MA01), 1,3-bis(isocyanatomethyl)cyclohexane-based blocked isocyanates (for example, manufactured by Mitsui Chemicals, Inc. under the trade name of Takenate B-846N), manufactured by Tosoh Corporation (hereinafter referred to as Coronate BI-301, 2507, and 2554), and isophorone diisocyanate-based blocked isocyanates (for example, manufactured by Baxenden under the trade names of 7950, 7951, and 7990).

[0082] Among these, blocked isocyanate compounds and bismaleimide compounds are preferred from the viewpoint of storage stability. (E) The thermal crosslinking agent may be used alone or in combination of two or more kinds.

[0083] The content of the (E) thermal crosslinking agent in the photosensitive resin composition of the present disclosure is preferably 0.2 parts by mass to 40 parts by mass relative to 100 parts by mass of the (A) polyimide resin. From the viewpoint of chemical resistance, the lower limit of the thermal crosslinking agent is more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more. From the viewpoint of storage stability of the photosensitive resin composition of the present disclosure, the upper limit of the thermal crosslinking agent is more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less.

[0084] (F) Silane Coupling Agent In order to improve the copper adhesion of the cured relief pattern, the photosensitive resin composition of the present disclosure may optionally contain (F) a silane coupling agent. (F) The silane coupling agent preferably has a structure represented by the following general formula (33): In the formula, R 10 is at least one selected from the group consisting of substituents containing an epoxy group, a phenylamino group, a ureido group, an isocyanate group, and an isocyanuric group, and R 11 are each independently an alkyl group having 1 to 4 carbon atoms, and R 12 is a hydroxyl group or an alkyl group having 1 to 4 carbon atoms, a is an integer of 1 to 3, and i is an integer of 1 to 6.

[0085] In general formula (33), a is not limited as long as it is an integer of 1 to 3, but from the viewpoint of adhesion to the metal redistribution layer, it is preferably 2 or 3, and more preferably 3. i is not limited as long as it is an integer of 1 to 6, but from the viewpoint of adhesion to the metal redistribution layer, it is preferably 1 or more and 4 or less. From the viewpoint of resolution, it is preferably 2 or more and 5 or less.

[0086] R 10 is not limited as long as it is a substituent containing any one of the structures of the group consisting of an epoxy group, a phenylamino group, a ureido group, an isocyanate group, and an isocyanuric group. Among these, from the viewpoint of resolution and copper adhesion, it is preferable that it is at least one selected from the group consisting of a substituent containing a phenylamino group and a substituent containing a ureido group, and a substituent containing a phenylamino group is more preferable. 11is not limited as long as it is an alkyl group having 1 to 4 carbon atoms. Examples of R include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, and a t-butyl group. 12 is not limited as long as it is a hydroxyl group or an alkyl group having 1 to 4 carbon atoms. Examples of alkyl groups having 1 to 4 carbon atoms include R 11 The alkyl groups are the same as those shown above.

[0087] Examples of silane coupling agents containing an epoxy group include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0088] An example of a silane coupling agent containing a phenylamino group is N-phenyl-3-aminopropyltrimethoxysilane. An example of a silane coupling agent containing a ureido group is 3-ureidopropyltrialkoxysilane. An example of a silane coupling agent containing an isocyanate group is 3-isocyanatepropyltriethoxysilane.

[0089] The content of the silane coupling agent (F) in the photosensitive resin composition of the present disclosure is preferably 0.2 to 10 parts by mass relative to 100 parts by mass of the polyimide resin (A), and from the viewpoint of copper adhesion, the lower limit is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. From the viewpoint of suppressing the generation of foreign matter due to precipitation, the upper limit is more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less.

[0090] (G) Organotitanium Compound In order to improve the chemical resistance and elongation of the cured film, the photosensitive resin composition of the present disclosure may optionally contain (G) an organotitanium compound.

[0091] Organotitanium compounds that can be used in this embodiment include those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of organotitanium compounds are shown below in I) to VII): I) Titanium chelate compounds: Specific examples include titanium(IV) oxide acetylacetonate, titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), etc.

[0092] II) Tetraalkoxytitanium compounds: for example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], etc.

[0093] III) Titanocene compounds: for example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like.

[0094] IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc.

[0095] V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, etc.

[0096] VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate.

[0097] VII) Titanate coupling agents: for example, isopropyl tridodecylbenzenesulfonyl titanate.

[0098] Among them, the organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, titanium(IV) oxide acetylacetonate is preferred.

[0099] When the negative-type photosensitive resin composition of the present disclosure contains the (G) organotitanium compound, the content thereof is preferably 0.05 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. From the viewpoint of the heat resistance and chemical resistance of the obtained cured film, the lower limit of the content of the organotitanium compound is more preferably 0.5 parts by mass or more. From the viewpoint of the storage stability of the negative-type photosensitive resin composition, the upper limit of the content of the organotitanium compound is more preferably 2 parts by mass or less.

[0100] (H) Thermal Polymerization Inhibitor The photosensitive resin composition of the present disclosure may optionally contain a thermal polymerization inhibitor (H) to improve the stability of viscosity and photosensitivity, particularly when stored in the form of a solution containing a solvent. Examples of thermal polymerization inhibitors that can be used include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.

[0101] The content of the thermal polymerization inhibitor when blended in the photosensitive resin composition of the present disclosure is preferably in the range of 0.005 to 12 parts by mass per 100 parts by mass of the polyimide resin (A).

[0102] (I) Solvent The negative-type photosensitive resin composition of the present disclosure may optionally contain (I) a solvent. The (I) solvent is not limited as long as it can uniformly dissolve or suspend (A) the polyimide resin, (B) the nitrogen-containing heterocyclic compound, and (C) the photopolymerization initiator. Examples of such solvents include γ-butyrolactone (GBL), dimethyl sulfoxide, tetrahydrofurfuryl alcohol, ethyl acetoacetate, ethyl lactate, N,N-dimethylacetoacetamide, ε-caprolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide. These solvents may be used alone or in combination of two or more. From the viewpoint of the solubility of the nitrogen-containing heterocyclic compound (B), the solvent (I) is preferably GBL, dimethyl sulfoxide, N-methyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, or 3-butoxy-N,N-dimethylpropanamide.

[0103] The (I) solvent can be used depending on the desired coating film thickness and viscosity of the photosensitive resin composition of the present disclosure. The (I) solvent can be used, for example, preferably in the range of 30 to 1,000 parts by mass, more preferably in the range of 140 to 1,000 parts by mass, per 100 parts by mass of the (A) polyimide resin.

[0104] When the (I) solvent contains an alcohol having no olefinic double bond, the content of the alcohol having no olefinic double bond in the total solvent is preferably 5 to 50 mass%. The upper limit is more preferably 10 mass% or more from the viewpoint of the storage stability of the photosensitive resin composition of the present disclosure. The lower limit is more preferably 30 mass% or less from the viewpoint of the solubility of the (A) polyimide resin.

[0105] The negative-type photosensitive resin composition of the present disclosure may further contain other components in addition to the above components (A) to (I). Examples of other components in addition to the components (A) to (I) include, but are not limited to, a thermal polymerization initiator, a plasticizer, a hindered phenol compound, an adhesion aid, a sensitizer, etc.

[0106] The thermal polymerization initiator may be a compound that generates radicals by heat, and examples thereof include organic peroxides such as dialkyl peroxides, diacyl peroxides, peroxy esters, and peroxy ketals, and azo-based polymerization initiators such as azonitriles, azo esters, and azo amides. Among these, dialkyl peroxides and diacyl peroxides (e.g., dicumyl peroxide) are preferred from the viewpoint of chemical resistance.

[0107] When the photosensitive resin composition of the present disclosure contains a thermal polymerization initiator, the content thereof is preferably 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. From the viewpoint of chemical resistance, the lower limit of the content of the thermal polymerization initiator is more preferably 0.5 parts by mass or more. From the viewpoint of storage stability of the photosensitive resin composition of the present disclosure, the upper limit of the content of the thermal polymerization initiator is more preferably 5 parts by mass or less.

[0108] Examples of the plasticizer include phthalate ester compounds represented by bis(2-ethylhexyl) phthalate, dicyclohexyl phthalate, and diphenyl phthalate; isophthalate ester compounds represented by bis(2-ethylhexyl) isophthalate, dicyclohexyl isophthalate, and diphenyl isophthalate; terephthalate ester compounds represented by bis(2-ethylhexyl) terephthalate, dicyclohexyl terephthalate, and diphenyl terephthalate; trimellitate ester compounds represented by tris(2-ethylhexyl) trimellitate, tricyclohexyl trimellitate, and triphenyl trimellitate; pyrrolimellitate ester compounds represented by tetrakis(2-ethylhexyl) pyromellitate, tetracyclohexyl pyromellitate, and tetraphenyl pyromellitate; malonate ester compounds represented by bis(2-ethylhexyl) malonate, dicyclohexyl malonate, and diphenyl malonate; succinate compounds typified by bis(2-ethylhexyl) succinate, dicyclohexyl succinate, and diphenyl succinate; glutaric acid ester compounds typified by bis(2-ethylhexyl) glutarate, dicyclohexyl glutarate, and diphenyl glutarate; adipic acid ester compounds typified by bis(2-ethylhexyl) adipate, dicyclohexyl adipate, and diphenyl adipate; pimelic acid ester compounds typified by bis(2-ethylhexyl) pimelic acid, dicyclohexyl pimelic acid, and diphenyl pimelic acid; suberic acid ester compounds typified by bis(2-ethylhexyl) suberate, dicyclohexyl suberate, and diphenyl suberate; azelaic acid ester compounds typified by bis(2-ethylhexyl) azelaate, dicyclohexyl azelaate, and diphenyl azelaate; Sebacic acid ester compounds such as bis(2-ethylhexyl) sebacate, dicyclohexyl sebacate, and diphenyl sebacate; and aliphatic acid tetrahydrofurfuryl compounds such as tetrahydrofurfuryl propionate, tetrahydrofurfuryl butyrate, and tetrahydrofurfuryl isobutyrate.Examples of suitable acrylic polymers include those represented by the product name Disparlon 230 (manufactured by Kusunoki Chemical Co., Ltd.) and the product name Disparlon L-1983N (manufactured by Kusunoki Chemical Co., Ltd.), those represented by the product name Disparlon 1711EF (manufactured by Kusunoki Chemical Co., Ltd.), and those represented by the product name Disparlon U-158 (manufactured by Kusunoki Chemical Co., Ltd.) and those represented by the product name Disparlon U-160 (manufactured by Kusunoki Chemical Co., Ltd.). Among these, phthalate ester compounds, isophthalate ester compounds, terephthalate ester compounds, pyrrolimetic acid ester compounds, trimellitic acid ester compounds, malonic acid ester compounds, succinic acid ester compounds, glutaric acid ester compounds, adipic acid ester compounds, pimelic acid ester compounds, suberic acid ester compounds, azelaic acid ester compounds, sebacic acid ester compounds, and aliphatic acid tetrahydrofurfuryl compounds are preferred from the viewpoint of compatibility with the (A) polyimide resin.

[0109] When the negative-type photosensitive resin composition of the present disclosure contains a plasticizer, the content thereof is preferably 0.5 parts by mass or more and 40 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. From the viewpoint of flatness during coating, the lower limit of the plasticizer content is more preferably 1 part by mass or more. From the viewpoint of flatness during curing, the upper limit of the plasticizer content is more preferably 30 parts by mass or less.

[0110] Examples of hindered phenol compounds include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenol), triethylenediamine, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butylphenol), triethylenediamine, 2,5-di-t-butyl-4-methylphenol ...4-methylphenol, 2,5-di-t-butyl-4-methylphenol, 2 ethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 2,2'-methylene-bis(4- Ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4- t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione )-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6- Examples of the hydroxybenzoates include, but are not limited to, (1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is particularly preferred.

[0111] When the negative-type photosensitive resin composition of the present disclosure contains a hindered phenol compound, the content thereof is preferably 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. The lower limit of the content of the hindered phenol compound is more preferably 0.5 parts by mass or more, since discoloration and corrosion of copper or a copper alloy are prevented when the photosensitive resin composition of the present disclosure is formed on copper or a copper alloy. The upper limit of the content of the hindered phenol compound is more preferably 10 parts by mass or less, from the viewpoint of photosensitivity.

[0112] In order to improve the adhesion between a cured film formed using the negative photosensitive resin composition of the present disclosure and a substrate, the photosensitive resin composition of the present disclosure may optionally contain an adhesion promoter other than a silane coupling agent. As the adhesion promoter, an aluminum-based adhesion promoter or the like can be used.

[0113] Examples of aluminum-based adhesion promoters include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.

[0114] When the negative-type photosensitive resin composition of the present disclosure contains an adhesive aid, the content of the adhesive aid is preferably 0.01 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin. From the viewpoint of adhesiveness, the lower limit of the content of the adhesive aid is more preferably 0.5 parts by mass or more. From the viewpoint of storage stability of the negative-type photosensitive resin composition of the present disclosure, the upper limit of the content of the adhesive aid is more preferably 20 parts by mass or less.

[0115] Examples of sensitizers include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, and p-dimethylaminocinnamylideneindano. p-dimethylaminobenzylidene indanone, 2-(p-dimethylaminophenylbiphenylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl

[0039] Examples of the methylaminobenzoate include methylaminobenzoate, ... These may be used alone or in combination of two to five kinds, for example.

[0116] When the negative-type photosensitive resin composition of the present disclosure contains a sensitizer for improving photosensitivity, the content thereof is preferably 0.1 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the (A) polyimide resin.

[0117] <Method for Producing Cured Relief Pattern> The method for producing a cured relief pattern of the present disclosure includes: (1) a step of applying the above-described negative photosensitive resin composition of the present disclosure onto a substrate to form a photosensitive resin layer on the substrate (resin layer forming step); (2) a step of exposing the photosensitive resin layer to light (exposure step); (3) a step of developing the exposed photosensitive resin layer to form a relief pattern (relief pattern forming step); and (4) a step of heat-treating the relief pattern to form a cured relief pattern (cured relief pattern forming step).

[0118] (1) Resin Layer Formation Step In this step, the negative photosensitive resin composition of the present disclosure is applied to a substrate, and then dried as necessary to form a photosensitive resin layer (in one embodiment, a coating film containing the photosensitive resin composition). As the application method, methods conventionally used for applying negative photosensitive resin compositions, such as application using a spin coater, bar coater, blade coater, curtain coater, screen printing machine, etc., or spray application using a spray coater, can be used.

[0119] If necessary, a coating film containing the negative photosensitive resin composition of the present disclosure can be dried. Drying methods include air drying, heat drying using an oven or a hot plate, and vacuum drying. Specifically, in the case of air drying or heat drying, drying can be carried out at a temperature of 20°C to 150°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on a substrate.

[0120] (2) Exposure Step In this step, the photosensitive resin layer formed above is exposed to an ultraviolet light source or the like using an exposure device such as a contact aligner, mirror projection, or stepper, either directly or through a patterned photomask or reticle. This exposure causes the polymerizable functional groups of the polyimide resin (A) contained in the negative photosensitive resin composition of the present disclosure to crosslink due to the action of the photopolymerization initiator (C). This crosslinking makes the exposed portion insoluble in the developer described below, enabling the formation of a relief pattern.

[0121] Thereafter, for the purpose of improving photosensitivity, etc., post-exposure baking (PEB) or pre-development baking, or both, may be performed at any combination of temperature and time, as necessary. The baking conditions are preferably a temperature of 40°C to 120°C and a time of 10 seconds to 240 seconds, but are not limited to these ranges as long as the properties of the negative-type photosensitive resin composition of the present disclosure are not impaired.

[0122] (3) Relief Pattern Forming Step In this step, the unexposed portions of the exposed photosensitive resin layer are developed and removed to form a relief pattern. As a development method for developing the exposed (irradiated) photosensitive resin layer, any method can be selected from conventionally known photoresist development methods, such as a rotary spray method, a paddle method, and an immersion method accompanied by ultrasonic treatment. After development, post-development baking may be performed at any combination of temperature and time, as necessary, for the purpose of adjusting the shape of the relief pattern, etc.

[0123] The developer used for development is preferably, for example, a good solvent for the negative-tone photosensitive resin composition, or a combination of a good solvent and a poor solvent. Examples of good solvents include N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, and α-acetyl-γ-butyrolactone. Examples of poor solvents include toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, and water. When a mixture of a good solvent and a poor solvent is used, it is preferable to adjust the ratio of the poor solvent to the good solvent depending on the solubility of the polymer in the negative-tone photosensitive resin composition. Two or more solvents, for example, a combination of several solvents, can also be used.

[0124] (4) Cured Relief Pattern Formation Step In this step, the relief pattern obtained by development is heat-treated to dissolve the photosensitive component, thereby forming a cured relief pattern made of polyimide. Heat treatment can be performed using a variety of methods, including a hot plate, an oven, or a temperature-programmable heating oven. Heat treatment can be performed, for example, at 160°C to 350°C for 30 minutes to 5 hours. The heat treatment temperature is preferably 300°C or lower, more preferably 250°C or lower. Air may be used as the atmospheric gas during heat curing, or an inert gas such as nitrogen or argon may also be used.

[0125] <Polyimide Cured Film> The present disclosure also provides a cured film formed from the negative photosensitive resin composition of the present disclosure. The cured film formed from the negative photosensitive resin composition of the present disclosure contains (A) a polyimide resin. The cured film of the present disclosure also contains a cured product of the negative photosensitive resin composition of the present disclosure. The cured film of the present disclosure can be produced based on the above-described method for producing a cured relief pattern.

[0126] <Semiconductor Device> The present disclosure also provides a semiconductor device having a cured relief pattern obtained from the above-described negative photosensitive resin composition. Specifically, the present disclosure provides a semiconductor device having a substrate that is a semiconductor element and a cured relief pattern. The cured relief pattern may be produced by the above-described method for producing a cured relief pattern using the above-described negative photosensitive resin composition.

[0127] The present disclosure also provides a method for manufacturing a semiconductor device, which uses a semiconductor element as a substrate and includes, as part of its steps, the method for manufacturing a cured relief pattern according to the present embodiment. In this case, the cured relief pattern formed by the method for manufacturing a cured relief pattern according to the present disclosure can be formed as a surface protective film for a semiconductor device, an interlayer insulating film, an insulating film for redistribution wiring, a protective film for a flip-chip device, or a protective film for a semiconductor device having a bump structure, and can be manufactured by combining the formed cured relief pattern with a known method for manufacturing a semiconductor device.

[0128] <Display Device> The present disclosure also provides a display device including a display element and a cured film provided on the display element, the cured film having the cured relief pattern described above. The cured relief pattern may be laminated in direct contact with the display element, or may be laminated via another layer. The cured film may be applied to, for example, surface protection films, insulating films, planarizing films, etc. of TFT liquid crystal display elements and color filter elements; protrusions for MVA-type liquid crystal display devices; and partition walls for cathodes of organic EL elements.

[0129] The negative photosensitive resin composition of the present disclosure is useful not only for application to the semiconductor devices described above, but also for applications such as interlayer insulation in multilayer circuits, cover coats for flexible copper-clad boards, solder resist films, and liquid crystal alignment films.

[0130] <Method for producing negative-type photosensitive resin composition> The negative-type photosensitive resin composition of the present disclosure can be obtained by mixing 100 parts by mass of (A) polyimide resin, (B) 0.01 to 10 parts by mass of nitrogen-containing heterocyclic compound based on 100 parts by mass of the (A) polyimide resin, and (C) 1 to 30 parts by mass of photopolymerization initiator based on 100 parts by mass of the (A) polyimide resin. Optionally, the composition may further contain (D) a radical polymerizable compound, (E) a thermal crosslinking agent, (F) a silane coupling agent, (G) an organotitanium compound, (H) a thermal polymerization inhibitor, (I) a solvent, and other components.

[0131] The present embodiment will be described in detail below with reference to examples, but the present embodiment is not limited thereto. In the examples, comparative examples, production examples, and synthesis examples, the physical properties of the polyimide, polyimide precursor, or negative-type photosensitive resin composition were measured and evaluated according to the following methods.

[0132] <Measurement and Evaluation Methods> (1) Measurement of Weight-Average Molecular Weight (Mw) The weight-average molecular weight (Mw) of each resin was measured by gel permeation chromatography (GPC) under the following conditions: A calibration curve for calculating the weight-average molecular weight was prepared using standard polystyrene (Easy Type PS-1, manufactured by Agilent Technologies).

[0133] Apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Eluent: N-methyl-2-pyrrolidone, lithium bromide monohydrate 30 mmol / L, phosphoric acid 50 mmol / L Column: Tsk gel Super HM-H (2 columns) / Tsk gel Super H-RC (manufactured by Tosoh Corporation) Flow rate: 0.5 mL / min Column temperature: 40°C Detector: UV-8320

[0134] (2) Calculation of the content of alicyclic structure in (A) polyimide resin The content of alicyclic structure in (A) polyimide resin was calculated by dividing the number of moles of tetracarboxylic dianhydride and diamine having an alicyclic structure among the tetracarboxylic anhydride and diamine used as raw materials for (A) polyimide resin by the total amount of tetracarboxylic anhydride and diamine, and multiplying the result by 100. That is, the content of alicyclic structure in (A) polyimide resin was calculated by applying the following formula (i):

[0135] (3) Cure Residual Film Ratio To evaluate cure shrinkage, the cure residual film ratio shown below was evaluated. A 200 nm thick Ti film and a 400 nm thick Cu film were sputtered in this order onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated onto this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Corporation), and prebaked on a hot plate at 110°C for 180 seconds to form a coating film of the photosensitive resin composition on the Cu. The thickness (T1) of this coating film was measured using a step gauge (P-17, manufactured by ULVAC, Inc.). Subsequently, this coating film was irradiated with 1000 mJ / cm 2 using Prisma GHI (manufactured by Ultratech Co., Ltd.) without using a test pattern mask. 2 The photosensitive resin composition was then irradiated with an energy of 1000 W. Subsequently, the photosensitive resin composition was subjected to a heating treatment at 230°C for 2 hours in a nitrogen atmosphere using a temperature-programmed curing oven (VF-2000 model, manufactured by Koyo Lindberg Co., Ltd.), thereby obtaining a cured film of the photosensitive resin composition on the Cu. The thickness (T4) of the obtained cured film was measured in the same manner as in T1.

[0136] The cured film remaining rate was calculated based on the following formula: Cured film remaining rate (%) = (T4 / T1) x 100 The cured film remaining rate was evaluated according to the following criteria: "Acceptable": 90% or more "Unacceptable": Less than 90%

[0137] (4) Copper Adhesion Evaluation On a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm), a 200 nm thick Ti film and a 400 nm thick Cu film were sputtered in this order using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated on this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Co., Ltd.), and prebaked on a hot plate at 110°C for 180 seconds to form a coating film of the photosensitive resin composition on the Cu. This coating film was then subjected to 1000 mJ / cm irradiation using Prisma GHI (manufactured by Ultratech Co., Ltd.) without using a test pattern mask. 2 Next, a temperature-programmed curing oven (VF-2000 model, manufactured by Koyo Lindberg) was used to perform a heat treatment in a nitrogen atmosphere at 230°C for 2 hours, thereby obtaining a cured film of the photosensitive resin composition having a thickness of approximately 6 μm on the Cu.

[0138] The heat-treated film was evaluated for adhesion properties between the copper substrate and the cured film according to the cross-cut method of JIS K 5600-5-6, based on the following criteria: "Excellent": The lattice number of the cured film adhered to the substrate is more than 100; "Good": The lattice number of the cured film adhered to the substrate is 80 to 100; "Fair": The lattice number of the cured film adhered to the substrate is 50 to less than 80; "Poor": The lattice number of the cured film adhered to the substrate is less than 50

[0139] (5) Evaluation of elongation of cured film: Breaking elongation measurement A photosensitive resin composition prepared by the method described below was spin-coated onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a coater developer (D-Spin 60A model, manufactured by SOKUDO Corporation). The wafer was then pre-baked on a hot plate at 110°C for 180 seconds to form a coating film of the photosensitive resin composition with a thickness of approximately 10.0 μm. This coating film was then subjected to 1000 mJ / cm irradiation using a Prisma GHI (manufactured by Ultratech Corporation). 2 The entire surface was exposed to an exposure dose of 100 ppm. The exposed film was then heat-treated in a temperature-programmed curing oven (VF-2000, manufactured by Koyo Lindberg) under a nitrogen atmosphere at 230°C for 2 hours to obtain a cured film (polyimide film). The cured film was cut into 3 mm wide strips using a dicing saw (DAD3350, manufactured by DISCO Corporation) and then peeled from the silicon wafer using 46% hydrofluoric acid to obtain a polyimide tape. The polyimide tape was then left to stand for 24 hours or more in an atmosphere of 23°C and 50% humidity. The elongation of the left polyimide tape was measured using a tensile tester (UTM-II-20, manufactured by Orientec Co., Ltd.) at a test speed of 40 mm / min and an initial load of 0.5 fs, and evaluated based on the following criteria. The elongation of the cured film was calculated using the following formula: Elongation of cured film (%) = (length of polyimide tape after breakage in tensile test - length of polyimide tape before tensile test) ÷ length of polyimide tape before tensile test × 100

[0140] "Excellent": Elongation of the cured film is 30% or more. "Good": Elongation of the cured film is 20% or more but less than 30%. "Fair": Elongation of the cured film is 10% or more but less than 20%. "Poor": Elongation of the cured film is less than 10%.

[0141] Production Example 1 ((A) Synthesis of Polyimide Resin A-1: ​​Acid Anhydride-Terminated BCD-PDPE) 200 g of γ-butyrolactone (hereinafter GBL) and 24.3 g (0.088 mol) of 6-(4-aminophenoxy)biphenyl-3-amine (hereinafter PDPE) were dissolved in a nitrogen-purged three-neck flask equipped with a Dean-Stark extractor. To this solution, 24.8 g (0.1 mol) of bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (hereinafter BCD) and 50.0 g of toluene were added and heated to 180°C. After confirming that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor, heating was stopped and the mixture was cooled to room temperature. The resulting reaction solution was added dropwise to 2000 g of ion-exchanged water to precipitate a polymer, which was then filtered and vacuum-dried at 40°C to obtain a powdered polymer (Polyimide Resin A-1). The weight average molecular weight of Polyimide Resin A-1 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be 30,000.

[0142] <Production Example 2> (A) Synthesis of Polyimide Resin A-2: Acid Anhydride-Terminated BCD-PDPE) Polyimide Resin A-2 was obtained in the same manner as in Production Example 1, except that the amount of PDPE in Production Example 1 was changed to 13.8 g (0.05 mol). The weight-average molecular weight of Polyimide Resin A-2 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 5,700.

[0143] <Production Example 3> (A) Synthesis of Polyimide Resin A-3: Acid Anhydride-Terminated BCD-PDPE) Polyimide Resin A-3 was obtained in the same manner as in Production Example 1, except that the amount of PDPE in Production Example 1 was changed to 23.0 g (0.083 mol). The weight-average molecular weight of Polyimide Resin A-3 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 14,200.

[0144] <Production Example 4> (A) Synthesis of Polyimide Resin A-4: Acid Anhydride-Terminated BCD-PDPE) Polyimide Resin A-4 was obtained in the same manner as in Production Example 1, except that the amount of PDPE in Production Example 1 was changed to 26.5 g (0.096 mol). The weight-average molecular weight of Polyimide Resin A-4 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 52,000.

[0145] <Production Example 5> (Synthesis of (A) Polyimide Resin A-5: Amine-Terminated BCD-PDPE) Polyimide Resin A-5 was obtained in the same manner as in Production Example 1, except that the amount of PDPE in Production Example 1 was changed to 33.1 g (0.12 mol) and the amount of GBL was changed to 200 g of N-methyl-2-pyrrolidone (hereinafter referred to as NMP). The weight-average molecular weight of Polyimide Resin A-5 was measured by gel permeation chromatography (standard polystyrene equivalent) and was found to have an Mw of 14,300.

[0146] Production Example 6 (Synthesis of (A) Polyimide Resin A-6: HEMA-Modified BCD-PDPE) 200 g of GBL and 24.3 g (0.088 mol) of PDPE were added to a nitrogen-purged three-neck flask equipped with a Dean-Stark extractor and dissolved therein, to which 24.8 g (0.1 mol) of BCD and 50.0 g of toluene were added and heated to 180° C. After confirming that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor, heating was stopped and the mixture was cooled to room temperature.

[0147] Next, under ice cooling, a solution of 5.45 g (0.026 mol) of dicyclohexylcarbodiimide (DCC) dissolved in 10 g of GBL was added to the reaction mixture with stirring, followed by the addition of 3.4 g (0.026 mol) of 2-hydroxyethyl methacrylate (HEMA). 2.0 g of 4-dimethylaminopyridine was then added, and the mixture was stirred at room temperature for 4 hours. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction solution. The resulting reaction solution was added to 500 g of ethyl alcohol to produce a precipitate consisting of a crude polymer. The produced crude polymer was filtered off and dissolved in 300 g of GBL to obtain a crude polymer solution. The obtained crude polymer solution was passed through an ion exchange resin (product name: Amberlite 15JWET, manufactured by DuPont) and then added dropwise to 3 kg of water to precipitate the polymer. The resulting precipitate was filtered off and then vacuum dried to obtain a powdered polymer (Polyimide Resin A-6). The weight average molecular weight of Polyimide Resin A-6 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be 15,000.

[0148] Production Example 7 (Synthesis of (A) Polyimide Resin A-7: MOI-Modified BCD-PDPE) 200 g of GBL and 33.1 g (0.12 mol) of PDPE were added to a nitrogen-purged three-neck flask equipped with a Dean-Stark extractor and dissolved therein, to which 24.8 g (0.1 mol) of BCD and 50.0 g of toluene were added and heated to 180° C. After confirming that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor, heating was stopped and the mixture was cooled to room temperature.

[0149] Next, 6.2 g of 2-isocyanatoethyl methacrylate (hereinafter referred to as MOI) was added at room temperature, and the mixture was allowed to react at room temperature for 12 hours. The resulting reaction solution was added dropwise to 2,000 g of ion-exchanged water to precipitate a polymer, which was then filtered and vacuum-dried at 40°C to obtain a powdery polymer (Polyimide Resin A-7). The weight-average molecular weight of Polyimide Resin A-7 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 15,200.

[0150] <Production Example 8> (A) Synthesis of Polyimide Resin A-8: MOI-Modified BCD / PMDA-PDPE) Polyimide Resin A-8 was obtained in the same manner as in Production Example 7, except that the BCD in Production Example 7 was changed to 12.4 g (0.05 mol) of BCD and 10.8 g (0.05 mol) of pyromellitic anhydride (hereinafter, PMDA). The weight-average molecular weight of Polyimide Resin A-8 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw of 19,200.

[0151] <Production Example 9> (A) Synthesis of Polyimide Resin A-9: MOI-Modified BCD / PMDA-PDPE) Polyimide Resin A-9 was obtained in the same manner as in Production Example 7, except that the BCD in Production Example 7 was changed to 16.1 g (0.065 mol) of BCD and 7.6 g (0.035 mol) of PMDA. The weight average molecular weight of Polyimide Resin A-9 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 17,500.

[0152] Production Example 10 (Synthesis of (A) Polyimide Resin A-10: Acryloyl Chloride-Modified BCD-PDPE) 200 g of GBL and 33.1 g (0.12 mol) of PDPE were added to a nitrogen-purged three-neck flask equipped with a Dean-Stark extractor and dissolved therein, to which 24.8 g (0.1 mol) of BCD and 50.0 g of toluene were added and heated to 180° C. After confirming that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor, heating was stopped and the mixture was cooled to room temperature.

[0153] Next, 3.6 g of acryloyl chloride was added under ice cooling, and the mixture was allowed to react for 2 hours. The resulting reaction solution was added dropwise to 2,000 g of ion-exchanged water to precipitate a polymer, which was then filtered and vacuum-dried at 40°C to obtain a powdery polymer (polyimide resin A-10). The weight-average molecular weight of polyimide resin A-10 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 15,500.

[0154] <Production Example 11> (A) Synthesis of Polyimide Resin A-11: Acid Anhydride-Terminated CBDA-PDPE) Polyimide resin A-11 was obtained in the same manner as in Production Example 3, except that the BCD in Production Example 3 was changed to 19.6 g (0.1 mol) of 1,2,3,4-cyclobutanetetracarboxylic anhydride (hereinafter referred to as CBDA). The weight average molecular weight of polyimide resin A-11 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 13,500.

[0155] <Production Example 12> (A) Synthesis of Polyimide Resin A-12: Acid Anhydride-Terminated 6FDA-PDPE) Polyimide resin A-12 was obtained in the same manner as in Production Example 3, except that BCD in Production Example 3 was changed to 44.4 g (0.1 mol) of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (hereinafter referred to as 6FDA). The weight average molecular weight of polyimide resin A-12 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 14,000.

[0156] <Production Example 13> (A) Synthesis of Polyimide Resin A-13: Acid Anhydride Terminated BCD-BAFL) Polyimide resin A-13 was obtained in the same manner as in Production Example 1, except that the PDPE in Production Example 1 was changed to 30.1 g (0.088 mol) of 9,9'-bis(4-aminophenyl)fluorene (hereinafter referred to as BAFL). The weight average molecular weight of polyimide resin A-13 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 29,000.

[0157] <Production Example 14> (A) Synthesis of Polyimide Resin A-14: Acid Anhydride Terminated BCD-TFMB) Polyimide resin A-14 was obtained in the same manner as in Production Example 1, except that the PDPE in Production Example 1 was changed to 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine (hereinafter referred to as TFMB) (28.2 g, 0.088 mol). The weight average molecular weight of polyimide resin A-14 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 28,000.

[0158] <Production Example 15> (A) Synthesis of Polyimide Resin A-15: Acid Anhydride-Terminated ODPA-TFMB) Polyimide resin A-15 was obtained in the same manner as in Production Example 1, except that the PDPE in Production Example 1 was changed to 30.4 g (0.095 mol) of TFMB and the BCD was changed to 31.0 g (0.1 mol) of 4,4'-oxydiphthalic anhydride (hereinafter referred to as ODPA). The weight average molecular weight of polyimide resin A-15 was measured by gel permeation chromatography (standard polystyrene equivalent) and was found to have an Mw of 50,000.

[0159] <Production Example 16> (A) Synthesis of Polyimide Resin A-16: Acid Anhydride-Terminated ODPA-PDPE) Polyimide resin A-16 was obtained in the same manner as in Production Example 1, except that the PDPE in Production Example 1 was changed to 26.2 g (0.095 mol) and the BCD was changed to 31.0 g (0.1 mol) of ODPA. The weight-average molecular weight of polyimide resin A-16 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 48,600.

[0160] <Production Example 17> (A) Synthesis of Polyimide Resin A-17: Side Chain Acid Anhydride Terminated BCD-PND) Polyimide Resin A-17 was obtained in the same manner as in Production Example 1, except that the PDPE in Production Example 1 was changed to 17.6 g (0.088 mol) of PND (2-phenoxybenzene-1,4-diamine). The weight average molecular weight of Polyimide Resin A-17 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be Mw 30,200.

[0161] <Production Example 18> (A) Polyimide Resin A-18: Synthesis of Side Chain Polymerizable Group 6FDA-MAEDAB) 44.4 g (0.1 mol) of 6FDA was dissolved in 200 g of NMP in a nitrogen-purged three-necked flask equipped with a Dean-Stark extractor. Next, 23.8 g of 2-(methacryloyloxy)ethyl-3,5-diaminobenzoate (MAEDAB) represented by the following formula was added and stirred at room temperature for 3 hours, followed by stirring at 45°C for an additional 3 hours. Further, 31.6 g (0.4 mol) of pyridine and 25.6 g (0.25 mol) of acetic anhydride were added and stirred at 80°C for 3 hours, after which heating was stopped and the mixture was cooled to room temperature. The resulting reaction solution was added dropwise to 2000 g of ion-exchanged water to precipitate a polymer, which was then filtered and vacuum-dried at 40°C to obtain a powdered polymer (Polyimide Resin A-18). The weight average molecular weight of Polyimide Resin A-18 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to be 20,000.

[0162] <Production Example 19> (A) Synthesis of Polyimide Resin A-19: Side Chain Polymerizable Group 6FDA-MAEDAB) Polyimide resin A-19 was obtained in the same manner as in Production Example 18, except that the amount of MAEDAB in Production Example 18 was changed to 25.4 g. The molecular weight of polyimide resin A-19 was measured by gel permeation chromatography (in terms of standard polystyrene) and was found to have an Mw of 50,000.

[0163] <Production Example 20> (Synthesis of Polyimide Precursor A'-1: Polyimide Precursor BCD-PDPE) 12.4 g (0.05 mol) of BCD was placed in a 1 L separable flask and 40 g of GBL was added. Next, 13.0 g of HEMA was added, and 7.9 g of pyridine was added with stirring, and then the mixture was stirred at 40°C for 5 hours using an oil bath to obtain a reaction mixture. After completion of the reaction, the mixture was allowed to cool to room temperature and left to stand for 16 hours.

[0164] Next, while stirring the resulting reaction mixture under ice cooling, a solution of 20.2 g of DCC in 25 g of γ-butyrolactone was added over 40 minutes, followed by the addition of a suspension of 12.1 g (0.044 mol) of PDPE in 75 g of GBL over 60 minutes. After stirring at room temperature for 2 hours, 180 g of ethyl alcohol was added and the mixture was stirred for an additional hour, after which 140 g of γ-butyrolactone was added. The reaction mixture was filtered to remove any precipitate that had formed in the reaction system, yielding a reaction liquid.

[0165] The resulting reaction solution was added to 0.3 kg of ethyl alcohol to precipitate a crude polymer. The precipitated crude polymer was collected by filtration and dissolved in 150 g of γ-butyrolactone to obtain a crude polymer solution. The resulting crude polymer solution was added dropwise to 1.8 kg of water to reprecipitate the polymer. The resulting reprecipitate was collected by filtration and then vacuum dried to obtain a powdery polymer (polyimide precursor A'-1). The weight-average molecular weight of A'-1 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 30,000.

[0166] Example 1 (Synthesis of Negative-Type Photosensitive Resin Composition) A negative-type photosensitive resin composition was prepared by the following method, and the prepared composition was evaluated. (A) 100 g of polyimide resin A-1, (B) 0.01 g of 8-azaadenine B-1 as a nitrogen-containing heterocyclic compound, and (C) 10 g of TR-PBG-3057 (trade name, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) (C-1) as a photopolymerization initiator were dissolved in (I) a mixed solvent of 112 g of γ-butyrolactone (GBL) (I-1) and 28 g of dimethyl sulfoxide (I-2) as a solvent. The viscosity of the resulting solution was adjusted to approximately 40 poise by further adding a small amount of GBL, and this composition was used as the negative-type photosensitive resin composition of Example 1. The composition was evaluated according to the method described above. The results are shown in Table 1. Unless otherwise specified, the units of values ​​in the table are parts by mass.

[0167] Examples 2 to 55, Comparative Examples 1 to 8 Negative photosensitive resin compositions similar to those in Example 1 were prepared and evaluated in the same manner as in Example 1, except that (A) to (I) shown in Table 1 were used. The results are shown in Table 1.

[0168]

[0169]

[0170]

[0171]

[0172]

[0173] A-1: Acid anhydride-terminated BCD-PDPE, Mw=30,000 A-2: Acid anhydride-terminated BCD-PDPE, Mw=5,700 A-3: Acid anhydride-terminated BCD-PDPE, Mw=14,200 A-4: Acid anhydride-terminated BCD-PDPE, Mw=52,000 A-5: Amine-terminated BCD-PDPE, Mw=14,300 A-6: HEMA-modified BCD-PDPE, Mw=15,000 A-7: MOI-modified BCD-PDPE, Mw=15,200 A-8: MOI-modified BCD / PMDA-PDPE=19,200 A-9: MOI-modified BCD / PMDA-PDPE=17,500 A-10: Acryloyl chloride-modified BCD-PDPE, Mw=15,500 A-11: Acid anhydride-terminated CBDA-PDPE, Mw=13,500 A-12: Acid anhydride-terminated 6FDA-PDPE, Mw=14,000 A-13: Acid anhydride-terminated BCD-BAFL, Mw=29,000 A-14: Acid anhydride-terminated BCD-TFMB, Mw=28,000 A-15: Acid anhydride-terminated ODPA-TFMB, Mw=50,000 A-16: Acid anhydride-terminated ODPA-PDPE, Mw=48,600 A-17: Side chain acid anhydride-terminated BCD-PND, Mw=30,200 A-18: Side chain polymerizable group 6FDA-MAEDAB, Mw=20,000 A-19: Side chain polymerizable group 6FDA-MAEDAB, Mw = 50,000 A'-1: Polyimide precursor BCD-PDPE, Mw = 30,000 B-1: 8-azaadenine B-2: 5-amino-1H-tetrazole B-3: 5-methyl-1H-benzotriazole B-4: 4-methyl-1H-benzotriazole B-5: 5-benzotriazolecarboxylic acid (5-carboxy-1H-benzotriazole) B-6: 1H-tetrazole-5-acetic acid B-7: 1H-tetrazole-5-ethyl acetate B-8: tolyltriazole B-9: Compound of the following structure B-10: Compound of the following structure C-1: Product name TR-PBG-3057 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) C-2: Diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide C-3: Product name NCI-730 (manufactured by ADEKA Corporation) D-1: 2-hydroxyethyl methacrylate D-2: Tris-(2-hydroxyethyl) isocyanurate acrylate D-3: Tris-(2-acryloxyethyl) isocyanurate D-4: Tetraethylene glycol dimethacrylate D-5: 4-hydroxybutyl acrylate glycidyl ether D-6: Dipentaerythritol polyacrylate E-1: 1,3,4,6-tetrakis (methoxymethyl) glycoluril F-1: N-phenyl-3-aminopropyltrimethoxysilane F-2: 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane G-1: Diisopropoxytitanium bis(ethyl acetate) G-2: Titanium tetra(n-butoxide) H-1: Hydroquinone H-2: 1-Nitroso-2-naphthol I-1: γ-butyrolactone I-2: Dimethyl sulfoxide I-3: N-methyl-2-pyrrolidone I-4: 3-Methoxy-N,N-dimethylpropanamide I-5: Ethyl lactate

[0174] From the evaluation results in the table, it is clear that Comparative Examples 1 to 8 are unable to achieve good performance in a balanced manner in terms of cure film remaining rate, copper adhesion, and cured film elongation. On the other hand, Examples 1 to 55 show excellent performance in terms of cure film remaining rate, copper adhesion, and cured film elongation. In the present disclosure, excellent performance means a rating of "fair" or higher in each evaluation item.

[0175] The negative-tone photosensitive resin composition according to the present invention can be used to form a cured relief pattern that exhibits reduced cure shrinkage and has film properties such as high copper adhesion and high elongation of the cured film, as well as a method for producing a cured relief pattern using the same and a polyimide cured film. The present invention can be suitably used in the field of photosensitive materials that are useful for producing electrical and electronic materials such as semiconductor devices and multilayer wiring boards.

Claims

1. A negative photosensitive resin composition comprising: (A) 100 parts by mass of a polyimide resin; (B) 0.01 to 10 parts by mass of a nitrogen-containing heterocyclic compound; and (C) 1 to 30 parts by mass of a photopolymerization initiator.

2. The negative photosensitive resin composition according to claim 1, wherein the polyimide resin (A) does not have a radical polymerizable group, a hydroxyl group and / or a carboxyl group in a side chain.

3. The negative photosensitive resin composition according to claim 1 or 2, wherein the polyimide resin (A) has a reactive group at its terminal.

4. The negative photosensitive resin composition according to claim 1 or 2, wherein the polyimide resin (A) has an alicyclic structure in an amount of 20 mol % or more and 70 mol % or less.

5. The negative photosensitive resin composition according to claim 1 or 2, wherein the nitrogen-containing heterocyclic compound (B) is an azole compound or a purine compound.

6. The negative photosensitive resin composition according to claim 5, wherein the azole compound is 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 1H-tetrazole-5-carboxylic acid, 1H-tetrazole-5-ethyl carboxylate, 1H-tetrazole-5-acetic acid, or 1H-tetrazole-5-ethyl acetate.

7. The negative type photosensitive resin composition according to claim 5, wherein the purine compound is 8-azaadenine, 8-azaguanine, adenine, N,N-dimethyladenine, or hypoxanthine.

8. The negative type photosensitive resin composition according to claim 5, wherein the purine compound is 8-azaadenine or 8-azaguanine.

9. The negative photosensitive resin composition according to claim 1 or 2, further comprising (D) a radically polymerizable compound.

10. The negative photosensitive resin composition according to claim 1 or 2, further comprising (E) a thermal crosslinking agent.

11. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (F) a silane coupling agent.

12. The negative photosensitive resin composition according to claim 1 or 2, further comprising (G) an organotitanium compound.

13. The negative photosensitive resin composition according to claim 1 or 2, further comprising (H) a thermal polymerization inhibitor.

14. The negative photosensitive resin composition according to claim 1 or 2, further comprising (I) a solvent.

15. The negative photosensitive resin composition according to claim 1 or 2, wherein the weight average molecular weight of the polyimide resin (A) is 5,000 to 100,000.

16. The negative type photosensitive resin composition according to claim 1, wherein the polyimide resin (A) contains a structure represented by the following general formula (1): {In formula (1), X 1 is a tetravalent organic group, Y 1 is a divalent organic group, and n is an integer from 1 to 150.

17. X in the general formula (1) 1 The negative type photosensitive resin composition according to claim 16, wherein:

18. X in the general formula (1) 1 The negative type photosensitive resin composition according to claim 17, wherein the structure is any one of the structures represented by the general formulas (7) to (9).

19. Y in the above general formula (1) 1 The negative type photosensitive resin composition according to claim 16, wherein:

20. Y in the above general formula (1) 1 The negative type photosensitive resin composition according to claim 19, wherein the structure is any one of the structures represented by the general formulas (13) to (16).

21. X in the general formula (1) 1 is any one of the structures represented by the general formulas (7) to (9), and Y 1 The negative type photosensitive resin composition according to claim 17 or 19, wherein the structure is any one of the structures represented by the general formulas (13) to (16).

22. The negative type photosensitive resin composition according to claim 16, wherein the terminal of the polyimide resin (A) contains an acid anhydride group, a carboxyl group, an amino group, or any of the structures represented by the following general formulas (20) to (22): (In the formula, R 1 , and R 2 are each independently selected from a hydrogen atom and a monovalent organic group having 1 to 3 carbon atoms; R 3 is an organic group having 1 to 20 carbon atoms which may contain a heteroatom, and k is an integer of 1 or 2. 4 is a hydrogen atom or an organic group having 1 to 4 carbon atoms, and * indicates the bonding site with the end of the polyimide resin (A). (In the formula, R 5 , and R 6 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms. Also, * indicates the bonding site with the end of the (A) polyimide resin. (In the formula, R 7 , R 8 , and R 9 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and j is an integer of 2 to 10. In addition, * indicates a bonding site with an end of the (A) polyimide resin.

23. A method for producing a cured relief pattern, comprising the following steps: (1) applying the negative photosensitive resin composition according to claim 1 or 2 onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; and (4) heat-treating the relief pattern to form a cured relief pattern.

24. A cured film comprising a cured product of the negative photosensitive resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Photosensitive resin composition, method for manufacturing cured relief pattern, and semiconductor device

    JP2012194520A

  • Curable resin composition, cured film, laminate, method for producing cured film, semiconductor device, and polyimide or polyimide precursor

    WO2020255859A1

  • Curable resin composition, cured film, layered product, method for producing cured film, and semiconductor device

    WO2021132578A1

Cited By

  • Polymer, negative photosensitive resin composition, patterning process, method for forming cured film, interlayer insulating film, surface protective film, and electronic component

    EP4636011A1

  • Photosensitive resin composition, cured product, transfer film, laminate, method for producing cured product, method for producing semiconductor device, and semiconductor device

    WO2026204976A1

  • Negative photosensitive resin composition and method for producing cured relief pattern using same

    WO2026205344A1

  • Photosensitive resin laminate

    WO2026211895A1