Barrier film, layered body, packaging container, and packaging product

The barrier film with a contact layer of lower softening temperature and a specific laminate configuration addresses adhesion issues after heat sterilization, ensuring strong lamination and barrier properties for packaging integrity.

WO2024219469A1PCT designated stage expired Publication Date: 2024-10-24TOPPAN HOLDINGS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015459
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing barrier films used in packaging for foods and medical drugs face issues with adhesion after heat sterilization, leading to shrinkage and distortion, which compromises the integrity of the packaging.

Method used

A barrier film structure comprising a base layer with a contact layer that has a lower softening temperature than the anchor coat layer, allowing for stress relief and maintaining adhesion even after heat sterilization, along with a laminate configuration that includes a second base layer with enhanced interlayer adhesion properties.

Benefits of technology

The proposed solution ensures excellent lamination strength and interlayer adhesion after heat sterilization, preventing delamination and maintaining the integrity of the packaging, while also improving oxygen and water vapor barrier properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015459_24102024_PF_FP_ABST
    Figure JP2024015459_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This barrier film comprises, in order: a substrate layer containing a polypropylene resin; an anchor coating layer; and an inorganic oxide layer. The substrate layer has a contact layer which is in contact with the anchor coating layer. When the softening temperatures of the anchor coating layer and the contact layer are measured by local thermal analysis, the softening temperature T1 of the contact layer is lower than the softening temperature T2 of the anchor coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Barrier films, laminates, packaging containers and packaging products

[0001] The present disclosure relates to barrier films, laminates, packaging containers and packaging products.

[0002] Barrier films are widely used as packaging materials for foods and medical drugs that are subjected to heat sterilization treatments such as boiling and retort treatments. Barrier films used in such packaging materials include those that include a substrate layer, an anchor coat layer, and an inorganic oxide layer, and the substrate layer may contain a polypropylene resin from the viewpoints of transparency, mechanical strength, and heat resistance.

[0003] Patent Document 1 listed below discloses a transparent laminate in which a transparent primer layer made of a mixture of an acrylic resin and an isocyanate resin and a thin film layer made of an inorganic compound are sequentially laminated on a substrate made of a stretched polypropylene film. Patent Document 1 also discloses a heat-sealable laminate obtained by laminating a gas barrier coating and a heat-sealable resin layer (sealant layer) on the thin film layer made of an inorganic compound of the transparent laminate.

[0004] Japanese Patent Application Publication No. 10-264292

[0005] However, the transparent laminate described in Patent Document 1 has room for improvement in terms of adhesion to the sealant layer after heat sterilization treatment.

[0006] Therefore, an object of the present disclosure is to provide a barrier film, a laminate, a packaging container, and a packaging product that have excellent lamination strength with another film even after heat sterilization treatment.

[0007] The inventors of the present disclosure conducted studies to solve the above-mentioned problems. When a barrier film including a base layer containing a polypropylene resin, an anchor coat layer, and an inorganic oxide layer is subjected to a heat sterilization treatment after a separate film such as a sealant layer is attached, shrinkage or the like occurs in the base layer. The inventors suspected that in this case, shrinkage stress generated in the base layer is transmitted to the inorganic oxide layer via the anchor coat layer, causing distortion between this inorganic oxide layer and the separate film. Therefore, the inventors conducted further intensive studies focusing on the above points, and as a result, they found that the above-mentioned problems can be solved by the present disclosure below.

[0008] That is, one aspect of the present disclosure provides a barrier film comprising a base material layer containing a polypropylene resin, an anchor coat layer, and an inorganic oxide layer in this order, wherein the base material layer has a contact layer in contact with the anchor coat layer, and when the softening temperatures of the anchor coat layer and the contact layer are measured by local thermal analysis, the softening temperature T1 of the contact layer is lower than the softening temperature T2 of the anchor coat layer.

[0009] The barrier film has excellent lamination strength with another film even after heat sterilization treatment.

[0010] The inventors of the present disclosure speculate that the reason why the above effects are obtained is as follows.

[0011] That is, when a barrier film including a polypropylene resin-containing substrate layer, an anchor coat layer, and an inorganic oxide layer is subjected to a heat sterilization treatment with another film such as a sealant layer attached thereto, shrinkage or the like occurs in the substrate layer, and the shrinkage stress generated in the substrate layer is transmitted to the inorganic oxide layer via the anchor coat layer. According to the barrier film of the present disclosure, the substrate layer includes a contact layer that has a softening temperature T1 lower than the softening temperature T2 of the anchor coat layer and is more flexible than the anchor coat layer, so that the shrinkage stress applied from the substrate layer to the anchor coat layer is alleviated by the contact layer. Therefore, distortion is less likely to occur between the inorganic oxide layer and the other film, and a decrease in adhesion between the other film and the barrier film is suppressed. The inventors of the present disclosure speculate that, as a result, the barrier film will have excellent lamination strength with the other film even after heat sterilization treatment.

[0012] In the barrier film, the softening temperature T2 of the anchor coat layer is preferably in the range of 140°C or higher and 195°C or lower.

[0013] When the softening temperature T2 is 140°C or higher, the heat resistance of the anchor coat layer can be increased, deformation of the anchor coat layer is reduced even at high temperatures during heat sterilization treatment such as retort treatment, and damage to the inorganic oxide layer can be reduced. Therefore, the barrier film can have an improved oxygen permeability even after heat sterilization treatment. Furthermore, when the softening temperature T2 of the anchor coat layer is 195°C or lower, the anchor coat layer does not become too hard, making it easier to obtain durability against deformation of the barrier film during heat sterilization treatment such as retort treatment, and making the inorganic oxide layer less likely to be destroyed.

[0014] In the above barrier film, the base material layer may further have a core layer on the opposite side of the contact layer from the anchor coat layer, the contact layer being a skin layer, and the softening temperature T1 of the contact layer may be lower than the softening temperature T3 of the core layer.

[0015] In the barrier film, T2-T1 is preferably 70° C. or less.

[0016] When T2-T1 is 70° C. or less, the difference in flexibility between the contact layer and the anchor coat layer is unlikely to become large, and the adhesion between the contact layer and the anchor coat layer is unlikely to decrease.

[0017] In the above barrier film, the contact layer may contain a copolymer of propylene and an α-olefin.

[0018] In this case, it becomes easier to increase the difference between the softening temperature T1 of the skin layer and the softening temperature T2 of the anchor coat layer.

[0019] In the barrier film, the anchor coat layer may contain a polyurethane resin.

[0020] When the anchor coat layer contains a polyurethane resin, the barrier film can have high heat resistance and high durability against heat sterilization treatment.

[0021] In the barrier film, the anchor coat layer may have a thickness of 0.05 to 2 μm.

[0022] In this case, it is possible to further suppress the deterioration of the water vapor barrier property when the barrier film is subjected to external force such as stretching, and it is also possible to further improve the flexibility of the barrier film and the oxygen gas barrier property of the barrier film after abuse.

[0023] Another aspect of the present disclosure provides a laminate comprising the above-described barrier film and a sealant layer.

[0024] According to the laminate, the barrier film has excellent lamination strength with the sealant layer as a separate film even after heat sterilization, so that delamination can be suppressed even after heat sterilization. That is, the laminate can have excellent interlayer adhesion even after heat sterilization.

[0025] The laminate may further include a second substrate layer on the surface of the barrier film opposite to the sealant layer, and the second substrate layer may contain a polyolefin resin.

[0026] The laminate includes the second base material layer, the barrier film, and the sealant layer in this order, the base material layer of the barrier film is a first base material layer, and the second base material layer, the first base material layer, and the sealant layer all contain polypropylene films, and an intensity I of a (040) plane peak in an X-ray diffraction pattern obtained by X-ray diffraction measurement of the second base material layer is 040 Intensity of the (110) plane peak I 110 The peak intensity ratio A may be 0.75 or more.

[0027] This laminate has excellent recyclability and can maintain excellent interlayer adhesion even after heat sterilization treatment such as retort treatment.

[0028] Among the above effects, the reason why the excellent interlayer adhesion is maintained even after heat sterilization is not clear, but it is thought to be as follows.

[0029] That is, by setting the peak intensity ratio A of the second substrate layer to 0.75 or more, the crystallinity of the second substrate layer is reduced, and sufficient flexibility is imparted to the second substrate layer. Therefore, even if the laminate is significantly deformed by heat sterilization treatment and the first substrate layer is also significantly deformed as a result, the second substrate layer can easily follow the deformation of the first substrate layer due to its sufficient flexibility. Therefore, it is possible to reduce the shear stress between the second substrate layer and the first substrate layer. Furthermore, by reducing the shear stress between the second substrate layer and the first substrate layer, the distortion occurring in the first substrate layer is reduced, and it is also possible to reduce the shear stress between the first substrate layer and the sealant layer. As a result, it is thought that the laminate can have excellent interlayer adhesion even after heat sterilization treatment of the laminate.

[0030] In the laminate, the second base material layer may be an unstretched film, and the first base material layer may be a stretched film.

[0031] The laminate may further include the inorganic oxide layer and the gas barrier layer at least either between the first base material layer and the second base material layer or between the first base material layer and the sealant layer.

[0032] In this case, the gas barrier properties of the gas barrier laminate can be further improved.

[0033] The laminate may further include the inorganic oxide layer and the gas barrier layer between the first base material layer and the second base material layer.

[0034] In this case, the laminate can have better interlayer adhesion even after heat sterilization treatment, compared to when an inorganic oxide layer and a gas barrier layer are provided between the first base layer and the sealant layer.

[0035] In the laminate, the inorganic oxide layer may be a vapor-deposited layer, and the vapor-deposited layer may contain at least one of aluminum oxide and silicon oxide.

[0036] In this case, the laminate can improve resistance to various types of sterilization.

[0037] In the laminate, the gas barrier layer may be a layer formed from a coating liquid containing a silicon compound and a water-soluble polymer, the silicon compound may include at least one of a first silicon compound and a second silicon compound, the first silicon compound may include at least one of a silicon alkoxide represented by the following general formula (1) and a hydrolyzate thereof, and the second silicon compound may include at least one of a silane coupling agent represented by the following general formula (2) and a hydrolyzate thereof: Si(OR 1 ) 4 ...(1) (In the general formula (1), OR 1 represents a hydrolyzable group. 2 Si(OR 3 ) 3 ) n ...(2) (In the general formula (2), OR 3 represents a hydrolyzable group, R 2 represents a monovalent organic group, and n is an integer of 1 or more.

[0038] In this case, the interlayer adhesion of the laminate can be further improved.

[0039] The laminate has an oxygen permeability of 200 cc / m at 30°C and 70% RH. 2 ・day・atm or less.

[0040] This laminate has an oxygen permeability of 200 cc / m at 30°C and 70% RH. 2 Compared to the case where the temperature exceeds 100 / day·atm, when a packaging container is made using the laminate 100 and contents are placed in the packaging container to make a packaged product, deterioration of the contents due to oxygen can be effectively suppressed.

[0041] In the above laminate, the anchor coat layer contains an organic polymer, and the organic polymer may contain at least one of a polyacrylic resin, a polyol resin, a polyurethane resin, a polyamide resin, and a reaction product of these resins.

[0042] The anchor coat layer may have a thickness of 0.01 to 1 μm.

[0043] In this case, compared to when the thickness of the anchor coat layer is less than 0.01 μm, it is possible to further improve the smoothness of the surface of the anchor coat layer relative to the surface of the first substrate layer, making it possible to make the thickness of the vapor deposition layer more uniform and further improving the oxygen barrier property. Therefore, the oxygen barrier property of the laminate can be further improved. Furthermore, compared to when the thickness of the anchor coat layer is more than 1 μm, the flexibility of the laminate can be further improved, and the oxygen gas barrier property of the laminate after abuse can be further improved.

[0044] Yet another aspect of the present disclosure provides a packaging container formed using the above-described laminate.

[0045] According to the above-mentioned packaging container, the barrier film has excellent lamination strength with the sealant layer, which is a separate film, even after heat sterilization treatment, and the laminate can have excellent interlayer adhesion even after heat sterilization treatment, so that it is possible to suppress interlayer delamination even after heat sterilization treatment.

[0046] In addition, when a packaging container is obtained using the above-mentioned laminate, the laminate comprises a second base material layer, a barrier film, and a sealant layer in this order, the base material layer of the barrier film is the first base material layer, the second base material layer, the first base material layer, and the sealant layer all comprise polypropylene films, and the peak intensity ratio A is 0.75 or more, the laminate has excellent recyclability and can have better interlayer adhesion even after heat sterilization treatment. Therefore, even after a packaged product containing contents in a packaging container is heat sterilized, delamination in the laminate can be further suppressed. Furthermore, after the contents are discharged from the packaged product, the packaging container has excellent recyclability.

[0047] Yet another aspect of the present disclosure provides a packaged product comprising a packaging container and a content to be contained in the packaging container, wherein the packaging container is the packaging container described above.

[0048] According to the packaged product, the barrier film has excellent lamination strength with the sealant layer as a separate film even after heat sterilization treatment, so that delamination can be prevented even after heat sterilization treatment.

[0049]

[0013] In addition, when a packaged product includes a packaging container obtained using the above-described laminate, the laminate includes a second base material layer, a barrier film, and a sealant layer in this order, the base material layer of the barrier film is the first base material layer, the second base material layer, the first base material layer, and the sealant layer all comprise polypropylene films, and the peak intensity ratio A is 0.75 or more, the laminate has excellent recyclability and can have better interlayer adhesion even after heat sterilization treatment. Therefore, delamination in the gas barrier laminate can be suppressed even after heat sterilization treatment. Furthermore, the packaging container remaining after the contents are discharged from the packaged product has excellent recyclability.

[0050] According to the present disclosure, it is possible to provide a barrier film, a laminate, a packaging container, and a packaged product that have excellent lamination strength with another film even after heat sterilization treatment.

[0051] Fig. 1 is a schematic cross-sectional view showing one embodiment of a barrier film of the present disclosure; Fig. 2 is a schematic cross-sectional view showing a first embodiment of a laminate of the present disclosure; Fig. 3 is a schematic cross-sectional view showing a second embodiment of a laminate of the present disclosure; Fig. 4 is a schematic cross-sectional view showing a first embodiment of a packaging product of the present disclosure; Fig. 5 is a schematic cross-sectional view showing a third embodiment of a laminate of the present disclosure; Fig. 6 is a schematic cross-sectional view showing a fourth embodiment of a laminate of the present disclosure; Fig. 7 is a schematic cross-sectional view showing a second embodiment of a packaging product of the present disclosure.

[0052] Hereinafter, embodiments of the present disclosure will be described in detail, with reference to the drawings as needed. However, the present disclosure is not limited to the following embodiments.

[0053] <Barrier Film> First, one embodiment of the barrier film of the present disclosure will be described with reference to FIG. 1. FIG. 1 is a schematic cross-sectional view showing one embodiment of a barrier film according to one aspect of the present disclosure. As shown in FIG. 1, a barrier film 10 according to this embodiment includes, in this order, a substrate layer 1 containing a polypropylene resin, an anchor coat layer 2, an inorganic oxide layer 3, and a gas barrier layer 4. The substrate layer 1 may be configured as a multilayer film including a skin layer 11 and a core layer 12 as shown in FIG. 1, or may be configured only with the skin layer 11. The skin layer 11 is a contact layer that contacts the anchor coat layer 2. In the barrier film 10, when the softening temperatures of the anchor coat layer 2 and the skin layer 11 are measured by local thermal analysis (LTA), the softening temperature T1 of the skin layer 11 is lower than the softening temperature T2 of the anchor coat layer 2.

[0054] The barrier film 10 maintains excellent lamination strength between itself and another film, such as a sealant layer, even after the other film is attached to the gas barrier layer 4 and subjected to heat sterilization treatment.

[0055] The substrate layer 1, anchor coat layer 2, inorganic oxide layer 3 and gas barrier layer 4 will be described in detail below.

[0056] [Substrate Layer] The substrate layer 1 is a film (base film) that serves as a support, and includes a skin layer 11 and a core layer 12 .

[0057] (Core Layer) The core layer 12 contains a polypropylene resin. Examples of the polypropylene resin include a homopolypropylene resin, which is a homopolymer of propylene, a random copolymer of propylene and an α-olefin, and a mixture thereof. From the viewpoint of improving heat resistance, a homopolypropylene resin, which is a homopolymer of propylene, is preferred.

[0058] The polypropylene resin used in the core layer 12 may be a resin polymerized from fossil fuel, a recycled resin, or a resin obtained by polymerizing raw materials derived from biomass such as plants. These resins may be used alone, or a mixture of a resin polymerized from fossil fuel and a recycled resin or a resin obtained by polymerizing raw materials derived from biomass such as plants may be used. The polypropylene resin may be an amorphous polypropylene resin or a crystalline polypropylene resin.

[0059] The content of the polypropylene resin may be 90% by mass or more, 95% by mass or more, or 99% by mass or more, based on the total mass of the core layer 12. The content of the polypropylene resin may be substantially 100% by mass, based on the total mass of the core layer 12. That is, the core layer 12 may be a layer consisting essentially of polypropylene resin only.

[0060] The core layer 12 may contain, as needed, organic additives such as antioxidants, stabilizers, lubricants, and antistatic agents, or inorganic additives such as silica, zeolite, hydrotalcite, silicon particles, and siloid.

[0061] The thickness (total thickness) of the core layer 12 is not particularly limited, and may be, for example, 3 μm to 200 μm, 6 μm to 50 μm, or 10 μm to 30 μm. When the thickness of the core layer 12 is 3 μm or more, wrinkles are less likely to occur during production of the barrier film 10 and when the barrier film 10 is used as a packaging film, making handling easier. When the thickness of the core layer 12 is 200 μm or less, transportability during roll-to-roll processing is further improved.

[0062] (Skin Layer) The skin layer 11 included in the substrate layer 1 is a contact layer that contacts the anchor coat layer 2 and is provided between the core layer 12 and the anchor coat layer 2. The skin layer 11 contains a polypropylene resin. As the polypropylene resin, a copolymer of propylene and another monomer can be used. As the other monomer used in the copolymer, for example, an α-olefin such as ethylene, 1-butene, or 1-hexene may be used. When the other monomer is an α-olefin, the skin layer 11 contains a copolymer of propylene and an α-olefin. In this case, it becomes easier to increase the difference between the softening temperature T1 of the skin layer 11 and the softening temperature T2 of the anchor coat layer 2. The copolymer may be a random copolymer.

[0063] The copolymer used in the skin layer 11 may be a resin polymerized from fossil fuel, a recycled resin, or a resin obtained by polymerizing a raw material derived from biomass such as plants. These resins may be used alone, or a mixture of a resin polymerized from fossil fuel and a recycled resin or a resin obtained by polymerizing a raw material derived from biomass such as plants may be used.

[0064] The content of propylene units in the copolymer may be 80 mol% or more, 90 mol% or more, 95 mol% or more, or 96 mol% or more, and may be 99.7 mol% or less, 99.5 mol% or less, 99 mol% or less, or 98 mol% or less, based on the total amount of monomer units.

[0065] The content of the polypropylene resin may be 90% by mass or more, 95% by mass or more, or 99% by mass or more, based on the total mass of the skin layer 11. The content of the polypropylene resin may be substantially 100% by mass, based on the total mass of the skin layer 11. That is, the skin layer 11 may be a layer consisting essentially of polypropylene resin only.

[0066] The skin layer 11 may contain, as needed, organic additives such as antioxidants, stabilizers, lubricants, and antistatic agents, or inorganic additives such as silica, zeolite, hydrotalcite, silicon particles, and siloid.

[0067] The softening temperature T1 of the skin layer 11 is lower than the softening temperature T2 of the anchor coat layer 2. By providing the base material layer 1 with the skin layer 11, the barrier film 10 has excellent lamination strength with another film even after heat sterilization treatment.

[0068] In the barrier film 10, T2-T1 is not particularly limited as long as it is greater than 0°C, but is preferably 70°C or less. When T2-T1 is 70°C or less, the difference in flexibility between the skin layer 11 and the anchor coat layer 2 is unlikely to increase, and the adhesion between the skin layer 11 and the anchor coat layer 2 is unlikely to decrease. T2-T1 is preferably 68°C or less, more preferably 60°C or less. Furthermore, T2-T1 is preferably 1°C or more, more preferably 2°C or more. When T2-T1 is 3°C or more, the effect of imparting flexibility to the skin layer 11 is enhanced, and the stress applied to the anchor coat layer 2 due to shrinkage of the substrate layer 1 after heat sterilization treatment can be alleviated, and the stress applied to the inorganic oxide layer 3 can be alleviated. In other words, the difference in strain between the substrate layer 1 and the anchor coat layer 2 can be effectively compensated for. This makes it possible to suppress damage to the inorganic oxide layer 3 and to prevent deterioration of the barrier properties of the inorganic oxide layer 3.

[0069] The softening temperature T1 of the skin layer 11 is not particularly limited as long as it is lower than the softening temperature T2 of the anchor coat layer 2, but is preferably between 115° C. and 170° C. When the softening temperature T1 is 115° C. or higher, the heat resistance of the skin layer 11 does not decrease too much, and the skin layer 11 is less likely to soften during heat sterilization treatment, making it less likely that a decrease in adhesion to the anchor coat layer 2 or core layer 12 or deterioration of barrier properties will occur. Furthermore, when the softening temperature T1 is 170° C. or lower, a decrease in the flexibility of the skin layer 11 can be suppressed, and the adhesion strength between the skin layer 11 and the core layer 12 can be further increased.

[0070] The softening temperature T1 may be 120°C or higher, 125°C or higher, or 130°C or higher from the viewpoint of imparting heat resistance to the skin layer 11, and may be 165°C or lower or 160°C or lower from the viewpoint of imparting flexibility to the skin layer 11.

[0071] The skin layer 11 may have only the softening temperature T1, or may have one or more softening temperatures higher than the softening temperature T1. When the skin layer 11 has multiple softening temperatures, the lowest softening temperature among them is the softening temperature T1.

[0072] The softening temperature T1 of the skin layer 11 may be lower than the softening temperature T3 of the core layer 12, or may be equal to or higher than the softening temperature T3 of the core layer 12. If the softening temperature T1 of the skin layer 11 is lower than the softening temperature T3 of the core layer 12, the stress transmitted from the core layer 12 to the anchor coat layer 2 is likely to be large, and therefore it is particularly useful to set the softening temperature T1 of the skin layer 11 lower than the softening temperature T2 of the anchor coat layer 2. In this case, T3 - T1 may be 20°C or higher, or may be 25°C or higher. T3 - T1 may be 80°C or lower, or may be 75°C or lower.

[0073] The thickness (total thickness) of the skin layer 11 is not particularly limited, but may be, for example, 0.1 μm or more and 5 μm or less, 0.2 μm or more and 3 μm or less, or 0.3 μm or more and 2 μm or less.

[0074] The base layer 1 can be formed, for example, by co-extrusion of the resin forming the core layer 12 and the resin forming the skin layer 11 into a sheet, and then stretching the sheet as necessary to orient it uniaxially or biaxially. The skin layer 11 may be formed on only one side of the core layer 12, or on both sides.

[0075] [Anchor Coat Layer] The anchor coat layer 2 is a layer for further improving the adhesion between the substrate layer 1 and the inorganic oxide layer 3, and is provided between the substrate layer 1 and the inorganic oxide layer 3.

[0076] The material constituting the anchor coat layer 2 is not particularly limited as long as it can improve the adhesion between the substrate layer 1 and the inorganic oxide layer 3, and for example, a material containing a reaction product of a polyol compound containing a (meth)acrylic resin and an isocyanate compound can be used. In the following description, "(meth)acrylic resin" means at least one of "acrylic resin" and the corresponding "methacrylic resin."

[0077] Examples of (meth)acrylic resins include (meth)acrylic polymers obtained by polymerizing polymerizable monomers containing (meth)acrylic monomers. The (meth)acrylic polymer may be a homopolymer of a (meth)acrylic monomer, or a copolymer of a (meth)acrylic monomer and a polymerizable monomer other than a (meth)acrylic monomer. The (meth)acrylic resin may be a resin capable of thermal crosslinking, such as urethane curing or epoxy curing. In view of reactivity with an isocyanate compound used as a curing agent, which will be described later, the (meth)acrylic resin may be a polyol having two or more hydroxyl groups in one molecule, and in particular, may be a (meth)acrylic polyol.

[0078] The (meth)acrylic polyol may be a (meth)acrylic copolymer obtained by copolymerizing a hydrocarbon (meth)acrylate with a hydroxyl group-containing monomer, or a (meth)acrylic copolymer obtained by copolymerizing a hydrocarbon (meth)acrylate, a hydroxyl group-containing monomer, and a monomer component other than these (other monomer components). By copolymerizing the above-mentioned hydroxyl group-containing monomer with at least one of the hydrocarbon (meth)acrylate and the other monomer component, a (meth)acrylic polyol containing multiple hydroxyl groups can be obtained.

[0079] The anchor coat layer 2 may contain a curing agent. The curing agent may be an isocyanate-based compound having two or more NCO groups in the molecule, from the viewpoint of excellent reactivity with the (meth)acrylic resin.

[0080] The isocyanate compound may be a monomeric isocyanate. Examples of the monomeric isocyanate include aromatic or araliphatic isocyanates such as tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), xylene diisocyanate (XDI), and tetramethylxylylene diisocyanate (TMXDI); and aliphatic isocyanates such as hexamethylene diisocyanate (HDI), bisisocyanate methylcyclohexane (H6XDI), isophorone diisocyanate (IPDI), and dicyclohexylmethane diisocyanate (H12MDI).

[0081] The isocyanate compound may be a polymer or derivative of the above-mentioned monomeric isocyanate. The isocyanate compound may be, for example, an isocyanate having a structure such as a trimer nurate type, an adduct type obtained by reacting with 1,1,1-trimethylolpropane, or a biuret type obtained by reacting with biuret. The isocyanate compound may be an isocyanate having an aromatic ring, from the viewpoint of excellent reactivity with the (meth)acrylic resin.

[0082] When the (meth)acrylic resin is a (meth)acrylic polyol, the content of the isocyanate compound may be an amount such that the number of OH groups in the acrylic polyol is equal to the number of NCO groups in the isocyanate compound.

[0083] The anchor coat layer 2 may further contain a silane coupling agent from the viewpoint of further improving adhesion to the inorganic oxide layer 3. Examples of the silane coupling agent include epoxy-based silane coupling agents having an epoxy group such as 3-glycidoxypropyltrimethoxysilane; amino-based silane coupling agents having an amino group such as 3-aminopropyltrimethoxysilane; mercapto-based silane coupling agents having a mercapto group such as 3-mercaptopropyltrimethoxysilane; and isocyanate-based silane coupling agents having an NCO group such as 3-isocyanatepropyltriethoxysilane. These silane coupling agents can be used alone or in combination of two or more.

[0084] Additionally, the material constituting the anchor coat layer 2 may contain a polyurethane resin. When the material constituting the anchor coat layer 2 contains a polyurethane resin, the barrier film 10 can have high heat resistance and high durability against heat sterilization treatment. The polyurethane resin can be formed, for example, from an acid group-containing polyurethane and a polyamine. The polyurethane resin is obtained by bonding the acid groups of the acid group-containing polyurethane with the amino groups of a polyamine serving as a crosslinking agent. In other words, the polyurethane resin can be said to be a reaction product of the acid group-containing polyurethane and the polyamine, or to be formed by crosslinking the acid group-containing polyurethane with the polyamine. The bond between the acid groups of the acid group-containing polyurethane and the amino groups of the polyamine may be an ionic bond (e.g., an ionic bond between a carboxyl group and a tertiary amino group) or a covalent bond (e.g., an amide bond).

[0085] A silane coupling agent or a carbodiimide compound may be added to the polyurethane resin. By adding the silane coupling agent or the carbodiimide compound, a crosslinked structure is formed with the polyurethane resin, thereby further improving the adhesion between the substrate layer 1 and the inorganic oxide layer 3. As the silane coupling agent, a commonly used agent can be used, and examples thereof include compounds in which an alkoxy group and an organic reactive group are bonded to a silicon atom.

[0086] The thickness of the anchor coat layer 2 is not particularly limited as long as it is a thickness that can improve the adhesion between the base layer 1 and the inorganic oxide layer 3, but is preferably 30 nm or more. In this case, compared to when the thickness of the anchor coat layer 2 is less than 30 nm, it is possible to further improve the surface smoothness of the anchor coat layer 2, making it possible to make the thickness of the inorganic oxide layer 3 more uniform, and also to further improve the oxygen barrier property. Therefore, the oxygen barrier property of the barrier film 10 can be further improved. The thickness of the anchor coat layer 2 is more preferably 40 nm or more, and even more preferably 50 nm or more. By increasing the thickness of the anchor coat layer 2, it is possible to further suppress the deterioration of the water vapor barrier property when an external force such as stretching is applied.

[0087] The thickness of the anchor coat layer 2 is preferably 2000 nm (2 μm) or less. In this case, the flexibility of the barrier film 10 is further improved compared to when the thickness of the anchor coat layer 2 exceeds 2000 nm, and the oxygen gas barrier properties of the barrier film 10 after abuse can be further improved. The thickness of the anchor coat layer 2 is more preferably 1500 nm (1.5 μm) or less.

[0088] The thickness of the anchor coat layer 2 is preferably 50 nm (0.05 μm) or more and 2000 nm (2 μm) or less. This can further suppress the deterioration of the water vapor barrier property when an external force such as stretching is applied to the barrier film 10. In addition, the flexibility of the barrier film 10 is further improved, and the oxygen gas barrier property of the barrier film 10 after abuse can be further improved.

[0089] The anchor coat layer 2 can be formed, for example, by applying an anchor coat solution onto the skin layer 11 of the base layer 1 by a method such as gravure coating, roll coating, or bar coating, and then drying it.

[0090] The softening temperature T2 of the anchor coat layer 2 may be higher than the softening temperature T1 of the skin layer 11, but is preferably in the range of 140°C or higher and 195°C or lower. A softening temperature T2 of 140°C or higher can improve the heat resistance of the anchor coat layer 2, reducing deformation of the anchor coat layer 2 even at high temperatures during heat sterilization treatment such as retort, and reducing damage to the inorganic oxide layer 3. Therefore, the barrier film 10 can have an improved oxygen permeability even after heat sterilization treatment. The softening temperature T2 is preferably 142°C or higher, more preferably 145°C or higher, and particularly preferably 150°C or higher.

[0091] Furthermore, by setting the softening temperature T2 of the anchor coat layer 2 to 195°C or lower, the anchor coat layer 2 does not become too hard, and the barrier film 10 is more likely to have durability against deformation during heat sterilization treatment such as retort, and the inorganic oxide layer 3 is less likely to be destroyed. The softening temperature T2 of the anchor coat layer 2 is more preferably 192°C or lower, and even more preferably 190°C or lower.

[0092] In the anchor coat layer 2, only the softening temperature T2 may exist, or one or more softening temperatures higher than the softening temperature T2 may also exist. When the anchor coat layer 2 has multiple softening temperatures, the lowest softening temperature among them becomes the softening temperature T2.

[0093] The softening temperature T2 of the anchor coat layer 2 can be adjusted by changing the compounding ratio of the components in the anchor coat layer forming composition or by adjusting the coating conditions (drying temperature, etc.) when applying the anchor coat layer forming composition.

[0094] [Inorganic Oxide Layer] The inorganic oxide layer 3 contains an inorganic oxide. The inorganic oxide layer 3 may or may not be formed directly on the anchor coat layer 2, but from the viewpoint of improving gas barrier properties against water vapor, oxygen, etc., it is preferable that the inorganic oxide layer 3 be formed directly on the anchor coat layer 2. The inorganic oxide layer 3 may or may not be transparent.

[0095] Examples of inorganic oxides that can be used include aluminum oxide, silicon oxide, tin oxide, magnesium oxide, and mixtures thereof. From the viewpoint of excellent sterilization resistance, the inorganic oxide may be at least one selected from aluminum oxide and silicon oxide.

[0096] The thickness of the inorganic oxide layer 3 may be 5 nm or more, 10 nm or more, or 15 nm or more from the viewpoint of achieving a uniform film thickness and excellent gas barrier properties, and may be 300 nm or less, 150 nm or less, or 100 nm or less from the viewpoint of making it difficult for cracks to occur in the inorganic oxide layer 3 even when an external force is applied after film formation. From these viewpoints, the thickness of the inorganic oxide layer 3 may be 5 to 300 nm, 10 to 150 nm, or 15 to 100 nm.

[0097] The inorganic oxide layer 3 can be formed by, for example, a vacuum deposition method, a plasma-assisted method, an ion-beam-assisted method, a sputtering method, a reactive deposition method, etc. The inorganic oxide layer 3 may be formed by a vacuum deposition method from the viewpoint of excellent productivity, or may be formed by a plasma-assisted method or an ion-beam-assisted method from the viewpoint of excellent adhesion between the inorganic oxide layer 3 and the anchor coat layer 2 and improving the density of the inorganic oxide layer 3, or may be formed by a reactive deposition method in which various gases such as oxygen are blown in from the viewpoint of excellent transparency of the inorganic oxide layer 3.

[0098] Examples of the heating method for the vacuum deposition method include an electron beam heating method, a resistance heating method, an induction heating method, etc. The heating method for the vacuum deposition method may be an electron beam heating method, from the viewpoint of an excellent range of selectivity for evaporation materials.

[0099] [Gas Barrier Layer] The gas barrier layer 4 is provided on the inorganic oxide layer 3 on the opposite side to the anchor coat layer 2. Providing the gas barrier layer 4 in the barrier film 10 can protect the inorganic oxide layer 3 and further improve the gas barrier properties of the barrier film 10. The barrier film 10 does not necessarily have to include the gas barrier layer 4.

[0100] The gas barrier layer 4 may contain a silicon compound or a hydrolyzate thereof, and a water-soluble polymer having a hydroxyl group.

[0101] Examples of silicon compounds include Si(OR 1 ) 4 and R 2 Si(OR 3 ) 3 It may be at least one selected from: OR 1 and OR 3 are each independently a hydrolyzable group, and R 2 is an organic functional group. 2 Examples of the alkyl group include a vinyl group, an epoxy group, a methacryloxy group, a ureido group, and an isocyanate group. 1 ) 4 is relatively stable in aqueous solvents after hydrolysis, so tetraethoxysilane (Si(OC 2 H 5 ) 4 ) may also be used.

[0102] Examples of water-soluble polymers having hydroxyl groups include polyvinyl alcohol, polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, sodium alginate, etc. The water-soluble polymer having hydroxyl groups may be polyvinyl alcohol from the viewpoint of excellent gas barrier properties.

[0103] The gas barrier layer 4 may further contain additives such as an isocyanate compound, a silane coupling agent, a dispersant, a stabilizer, a viscosity adjuster, and a colorant, as needed.

[0104] The thickness of the gas barrier layer 4 may be 0.1 μm or more or 0.3 μm or more, and may be 5 μm or less or 1 μm or less. The thickness of the gas barrier layer 4 may be 0.1 to 5 μm or 0.3 to 1 μm. When the thickness of the gas barrier layer 4 is 0.1 μm or more, the barrier properties after retort treatment are less likely to decrease. When the thickness of the gas barrier layer 4 is 5 μm or less, the gas barrier layer 4 is less likely to deteriorate due to insufficient drying during coating, and therefore good barrier properties are more likely to be exhibited. When the thickness of the gas barrier layer 4 is 1 μm or less, the gas barrier layer 4 is less likely to deteriorate due to insufficient drying during coating, and therefore good barrier properties are more likely to be exhibited.

[0105] The gas barrier layer 4 can be formed, for example, by dissolving a water-soluble polymer in water or a water / alcohol mixed solvent, mixing in a silicon compound or a hydrolyzate thereof, applying the mixed solution onto the inorganic oxide layer 3 by a method such as gravure coating, roll coating, or bar coating, and drying the solution.

[0106] When the water-soluble polymer is polyvinyl alcohol, the content of polyvinyl alcohol in the mixed solution may be 20% by mass or more or 25% by mass or more, based on the total solid content of the mixed solution, from the viewpoint of facilitating the formation of the gas barrier layer 4, and may be 50% by mass or less or 40% by mass or less, from the viewpoint of excellent gas barrier property. The content of polyvinyl alcohol in the mixed solution may be 20 to 50% by mass or 25 to 40% by mass, based on the total solid content of the mixed solution.

[0107] [Softening Temperature] The softening temperature is measured from the cross section of each layer of the barrier film 10. (Measurement Sample) First, the barrier film 10 is prepared. At this time, the barrier film 10 itself may be prepared, or a laminate obtained by attaching another film such as a sealant layer to the barrier film 10 may be prepared.

[0108] Next, the barrier film 10 is cut with a razor into strips or wedges, and the resulting cut pieces are embedded in an embedding resin to obtain block pieces. A photocurable resin is used as the embedding resin. For example, D-800 (product name) manufactured by Toa Gosei Co., Ltd. can be used as the photocurable resin. Note that, in order to prevent peeling between the embedding resin and the barrier film 10 after embedding, corona treatment may be performed as a surface treatment on the front and back surfaces of the barrier film 10 or the laminate before cutting the barrier film 10 or the laminate.

[0109] Next, the embedding resin is hardened by irradiating the block piece with light to form an embedding resin.

[0110] Next, the cured block piece is fixed with an insert for an AFM sample holder, and the embedding resin is trimmed with a glass knife at room temperature (25°C), and the cross-section of the barrier film 10 is cut using a cross-section cutting device. Thereafter, using the cross-section cutting device, the cross-section is cut with a diamond knife at a low temperature (-40°C) until a mirror finish is obtained, and a measurement sample with a cross-section of the barrier film 10 is obtained.

[0111] The cross-section cutting with a diamond knife can be performed, for example, at a cutting speed of 1.0 mm / s and a cutting film thickness of 100 nm. The measurement sample is used for measuring the softening temperature in a state where it is fixed in an insert for an AFM sample holder.

[0112] The cross-section cutting device may be, for example, an Ultramicrotome EM UC7 (trade name) or a Cryosystem EM FC7 (trade name) manufactured by Leica Corp. The cutting direction is parallel to the interface between the adjacent layers.

[0113] (Softening Temperature Measurement Method) The softening temperature is the temperature at which a material such as a resin exhibits softening behavior. In this embodiment, the softening temperature is measured by performing local thermal analysis (LTA) on a measurement sample using an atomic force microscope (AFM). To measure the softening temperature, the measurement sample is heated by applying a voltage to a cantilever equipped with a heater. In local thermal analysis (LTA), the cross-sectional shape of the measurement sample is measured, and then a constant force (contact pressure) is applied to a predetermined location on the cross-section of the measurement sample with the cantilever. The sample is heated while maintaining the contact pressure constant. The softening temperature is calculated as the temperature at which the height position (Z displacement) of the cantilever changes due to a change in the hardness of the sample surface before and after heating. In this case, the position where the cantilever applies contact pressure is the center of the thickness direction of the skin layer 11, anchor coat layer 2, and core layer 12. The change in the cantilever height refers to the change caused by the rise in the vertical position of the cantilever due to thermal expansion of the sample surface, and the fall in the vertical position of the cantilever due to softening of the sample surface. By converting the voltage applied to the cantilever heater when such a change in the cantilever height occurs into a softening temperature, the softening temperature can be determined locally in the nanoscale region and near the surface.

[0114] The softening temperature was measured using an atomic force microscope (AFM) MFP-3D-SA (trade name) manufactured by Oxford Instruments, and a local thermal analysis option, the Ztherm system (trade name). AC mode (tapping mode) was used for surface shape measurement, and contact mode was used for softening temperature measurement.

[0115] The cantilever used is an AN2-200 (trade name) manufactured by Anasys Instruments, with a spring constant of 0.5 to 3.5 N / m.

[0116] In measuring the softening temperature, the voltage application rate (temperature increase rate) of the cantilever is set to 0.5 V / sec.

[0117] The Ztherm system controls the contact pressure of the cantilever to a constant value. Contact pressure represents the force equivalent to the change in the cantilever's deflection (deflection) before and after contact between the cantilever and the sample. Deflection is obtained as a unit of voltage by detecting the reflected light of a laser irradiated on the back of the cantilever using a laser displacement meter (hereinafter also referred to as "deflection voltage"). Since the deflection voltage changes depending on the applied voltage during heating even without contact with the sample, it is necessary to control the contact pressure after subtracting the change in deflection voltage due to the applied voltage. The Ztherm system has a detrend correction function that acquires the change in deflection voltage with respect to the applied voltage. The Ztherm system applies the voltage used for measurement to the cantilever without the cantilever contacting the sample surface, increasing it from 0 V to the maximum applied voltage, and then performs detrend correction on the applied voltage. In this embodiment, the surface shape is measured, and before measuring the softening temperature, detrend correction is performed on the applied voltage used for measurement at a voltage application rate (heating rate) of 0.5 V / sec, and then the measurement is performed. When setting the contact pressure, the amount of change in deflection voltage is set to, for example, 0.2 V when measuring the softening temperature T1 of the skin layer 11 of the substrate layer 1, 0.2 V when measuring the softening temperature T3 of the core layer 12 of the substrate layer 1, and 1.5 V when measuring the softening temperature T2 of the anchor coat layer 2.

[0118] The set value for the downward displacement of the cantilever to stop the measurement is 10 nm.

[0119] The softening point is determined as the point where the vertical height (Z displacement) of the cantilever is maximum, and the applied voltage at this point is read.

[0120] To convert the voltage applied to the cantilever heater into a softening temperature, a calibration curve of applied voltage and temperature is created. Four polymeric materials with melting points differing by at least 50°C are used as calibration samples. These polymeric materials include materials with melting points above the softening temperature of the measurement sample and materials with melting points below the softening temperature. The melting points (melting peak temperatures) of the calibration samples are measured in advance using a differential scanning calorimeter (DSC), and the melting points are used as the softening temperatures of the calibration samples. Local thermal analysis is performed on each calibration sample at different measurement positions, and a calibration curve is created by approximating the average applied voltage at the obtained softening points and the softening temperatures of the calibration samples (melting points measured by DSC) with a cubic function using the least squares method. This is the calibration curve. The calibration samples were polycaprolactone pellets (melting point: 60°C), low-density polyethylene pellets (melting point: 112°C), polypropylene pellets (melting point: 166°C), and biaxially stretched polyethylene terephthalate film (melting point: 255°C), with cross-sectional specimens prepared in an environment below their glass transition temperature. An ultramicrotome and cryosystem were used to prepare the cross-sectional specimens, with cross-sections cut in an environment of -80°C for polycaprolactone, -140°C for low-density polyethylene, -40°C for polypropylene, and room temperature 25°C for polyethylene terephthalate.

[0121] Using this calibration curve of applied voltage and temperature, the temperature corresponding to the applied voltage at the softening point is determined, and this temperature is taken as the softening temperature.

[0122] <Laminate> Next, a laminate according to another aspect of the present disclosure will be described with reference to Fig. 2 or Fig. 3. Fig. 2 is a schematic cross-sectional view showing a first embodiment of a laminate according to another aspect of the present disclosure, and Fig. 3 is a schematic cross-sectional view showing a second embodiment of a laminate according to another aspect of the present disclosure. In Fig. 2 and Fig. 3, components that are the same as or equivalent to those in Fig. 1 are denoted by the same reference numerals.

[0123] The laminate of the present disclosure includes the above-described barrier film 10 and a separate film, a sealant layer 5, as in the laminate 20 shown in Fig. 2. The laminate of the present disclosure may also include the above-described barrier film 10, a sealant layer 5, and a second substrate layer 31 on the surface of the barrier film 10 opposite to the sealant layer 5, as in the laminate 30 shown in Fig. 3. The second substrate layer 31 may contain, for example, a polyolefin resin.

[0124] According to the laminate 20 or 30, the barrier film 10 has excellent adhesion to the sealant layer 5 even after heat sterilization treatment, so that delamination can be prevented from occurring even after heat sterilization treatment.

[0125] The sealant layer 5 may contain any resin having heat-sealing properties. Examples of such resins include polyolefin resins and polyester resins. Examples of polyolefin resins include polyethylene resins and polypropylene resins. Among these, from the viewpoint of improving recyclability, it is preferable to use polypropylene resin as the polyolefin resin. As the polypropylene resin, a polypropylene resin similar to the polypropylene resin contained in the core layer 12 can be used. The sealant layer 5 may be a stretched film or an unstretched film, but from the viewpoint of imparting a melting point lower than that of the base layer 1, it is preferable to use an unstretched film.

[0126] The thickness of the sealant layer 5 may be 10 μm or more, or 20 μm or more, and may be 200 μm or less, or 100 μm or less. The thickness of the sealant layer 5 may be 10 to 200 μm, or 20 to 100 μm. When the thickness of the sealant layer 5 is 10 μm or more, packaging containers such as packaging bags become less likely to tear. When the thickness of the sealant layer 5 is 200 μm or less, the sealant layer 5 maintains its heat sealability, and the possibility of sealing defects is reduced.

[0127] The laminate 20 may have an adhesive layer (not shown) between the barrier film 10 and the sealant layer 5. The adhesive layer may be formed of a polyurethane resin in which a bifunctional or higher functional isocyanate compound is allowed to react with, for example, polyester polyol, polyether polyol, acrylic polyol, carbonate polyol, or the like.

[0128] In order to improve adhesiveness, the adhesive layer may contain, in addition to the polyurethane resin, a carbodiimide compound, an oxazoline compound, an epoxy compound, a phosphorus compound, a silane coupling agent, or the like.

[0129] When the second base layer 31 contains a polyolefin resin, examples of the polyolefin resin include polyethylene resin and polypropylene resin. From the viewpoint of increasing the rigidity of the laminate 30, the polyolefin resin is preferably polypropylene resin. As the polypropylene resin, the same polypropylene resin as the polypropylene resin contained in the core layer 12 can be used.

[0130] In the X-ray diffraction pattern obtained by X-ray diffraction measurement of the second base layer 31, the intensity I of the (040) plane peak 040 Intensity of the (110) plane peak I 110 The peak intensity ratio A, which is the ratio of the peak intensity ratios of the laminate 20 and the peak intensity ratios of the laminate 20, is 0.75 or more. This laminate 20 has excellent recyclability and can maintain excellent interlayer adhesion even after heat sterilization treatment such as retort treatment. The peak intensity ratio A is preferably 0.80 or more, and more preferably 0.90 or more. The peak intensity ratio A may be 2 or less, 1.5 or less, 1.3 or less, or 1.1 or less.

[0131] <Packaging Product> Next, a packaging product according to yet another aspect of the present disclosure will be described with reference to Fig. 4. Fig. 4 is a schematic cross-sectional view showing an embodiment of a packaging product according to yet another aspect of the present disclosure. Note that components that are the same as or equivalent to those in Fig. 1 or 2 are denoted by the same reference numerals. The packaging product 100 shown in Fig. 4 includes a packaging bag 40 as a packaging container and contents C contained in the packaging bag 40. The packaging bag 40 is formed using two laminates 20.

[0132] According to the packaged product 100, the barrier film 10 has excellent adhesion to the sealant layer 5 even after heat sterilization treatment, so that delamination can be prevented from occurring even after heat sterilization treatment.

[0133] There are no particular limitations on the contents C, and examples of the contents C include food, liquid, medicine, and electronic parts.

[0134] In Fig. 4, the packaging product 100 can be formed by overlapping two laminates 20 with the sealant layers 5 facing each other, heat-sealing a portion of the peripheral edge to form a packaging bag 40, placing the contents C in the remaining portion of the packaging bag 40 that has not been heat-sealed, and then heat-sealing the remaining portion of the peripheral edge that has not been heat-sealed. Note that the packaging product 100 may be formed using a single laminate 20. In this case, the packaging product 100 can also be formed by folding one laminate 20 in half, heat-sealing a portion of the peripheral edge other than the folded portion to form a packaging bag, placing the contents C in the remaining portion of the packaging bag that has not been heat-sealed, and then heat-sealing the remaining portion of the peripheral edge that has not been heat-sealed.

[0135] The packaged product 100 may further include a stopper on the packaging bag 40. The stopper may be fixed by sandwiching it between the two laminates 20 or two laminates 30 that form the packaging bag 40, or may be fixed to the spout by drilling a hole in one surface of the packaging bag 40 and adhering the spout. The stopper may be located either above or diagonally above the packaging bag 40. When the packaging bag 40 has a top surface, a bottom surface, and a side surface connecting the top and bottom surfaces, the surface to which the spout is adhered may be any one of the top surface, side surface, or bottom surface of the packaging bag 40.

[0136] When the content C is liquid or gel-like, the stopper may be a spout so that the content C can be directly poured into the mouth and sucked out. In this case, the packaged product 100 may further include, in addition to the spout, a straw that extends from the spout and reaches the bottom inside the packaging bag 40.

[0137] When the content C in the packaging bag 40 is a liquid such as a soft drink or an alcoholic drink, the packaged product may be a bag-in-box that further includes a carton (outer box) that houses a bag (inner bag) serving as the packaging bag. In this case, the packaged product may further include a spout (tube) for pouring that is provided on the outside of the carton and connects to the bag by passing through the carton.

[0138] From the viewpoint of improving recyclability, the plug may be formed from the same resin as the base layer 1 of the barrier film 10 .

[0139] <Laminate> First, a third embodiment of the laminate of the present disclosure will be described with reference to Fig. 5. Fig. 5 is a schematic cross-sectional view showing the third embodiment of the laminate of the present disclosure.

[0140] The laminate 100A shown in FIG. 5 includes, in this order, a second base layer 10A, a first structure (hereinafter also referred to as a "barrier film") 25 including a first base layer 20A, and a sealant layer 30A.

[0141] The second base layer 10A, the first base layer 20A, and the sealant layer 30A all contain polypropylene films. In addition, in an X-ray diffraction pattern obtained by X-ray diffraction (XRD) measurement of the second base layer 10A, the intensity I of the (040) plane peak is 040 Intensity of the (110) plane peak I 110 The peak intensity ratio A (= I 110 / I 040 ) is 0.75 or more.

[0142] The second base layer 10A and the barrier film 25 may be bonded together by an adhesive layer 40A, and the sealant layer 30A and the barrier film 25 may be bonded together by an adhesive layer 40A. The barrier film 25 includes, between the first base layer 20A and the second base layer 10A, an anchor coat layer 21 and a vapor deposition layer 22 as an inorganic oxide layer, in this order from the first base layer 20A side. The barrier film 25 may further include a gas barrier layer 23 on the vapor deposition layer 22. When the softening temperatures of the anchor coat layer 21 and the first base layer 20A in the barrier film 25 are measured by local thermal analysis (LTA), the softening temperature T1 of the first base layer 20A is lower than the softening temperature T2 of the anchor coat layer 21.

[0143] According to the laminate 100A, the barrier film 25 maintains excellent lamination strength with the sealant layer 30A, which is a separate film, even after the sealant layer 30A is attached to the gas barrier layer 23 and subjected to heat sterilization treatment.

[0144] Furthermore, the laminate 100A has excellent recyclability and can maintain excellent interlayer adhesion even after heat sterilization treatment such as retort treatment. In particular, the laminate 100A can improve the interlayer adhesion between the second base material layer 10A and the first base material layer 20A after heat sterilization treatment. When a packaging container is manufactured using the laminate 100A, the second base material layer 10A is the outermost layer and is also the layer that is easily subjected to external forces. Therefore, the laminate 100A, which can improve the interlayer adhesion between the second base material layer 10A and the first base material layer 20A after heat sterilization treatment, is useful as a laminate for constituting a packaging container.

[0145] The second base layer 10A, the barrier film 25, the sealant layer 30A, and the adhesive layer 40A will be described in detail below.

[0146] [Second Base Layer] The second base layer 10A contains a polypropylene film. The polypropylene film contains a polypropylene resin. Examples of polypropylene resins include homopolypropylene, which is a homopolymer of propylene, and propylene-α-olefin copolymer, which is a copolymer of propylene and an α-olefin. These can be used alone or in combination of two or more. The second base layer 10A may further have a layer containing a propylene-α-olefin copolymer or a mixture of a propylene-α-olefin copolymer and homopolypropylene on the surface of the polypropylene film for the purpose of improving adhesion with a layer in contact with the second base layer 10A.

[0147] The polypropylene resin contained in the polypropylene film may be any of a fossil fuel-derived polypropylene resin obtained by homopolymerizing or copolymerizing with other monomers propylene derived from ordinary fossil fuels, a recycled polypropylene resin, and a biomass-derived polypropylene resin obtained by homopolymerizing or copolymerizing with other monomers propylene derived from biomass such as plants. These polypropylene resins may be used alone or in combination of two or more.

[0148] The second base layer 10A may further contain additives as needed, such as antioxidants, stabilizers, lubricants such as calcium stearate, fatty acid amides, and erucic acid amide, organic additives such as antistatic agents, and particulate lubricants such as silica, zeolite, syloid, hydrotalcite, and silicon particles.

[0149] The polypropylene film contained in the second base layer 10A may be a stretched film or an unstretched film. A stretched film can be obtained by forming the polypropylene resin into a sheet and stretching the sheet by a conventional means. The stretched film may be a uniaxially oriented film or a biaxially oriented film. The polypropylene film is preferably an unstretched film. In this case, the laminate 100A can have better interlayer adhesion even after heat sterilization treatment.

[0150] The thickness of the second base layer 10A is not particularly limited and may be, for example, 5 μm or more, 10 μm or more, or 15 μm or more. The thickness of the first base layer 20A may be 100 μm or less, 80 μm or less, 60 μm or less, or 40 μm or less.

[0151] The thickness of the second base layer 10A may be greater than the thickness of the first base layer 20A, or may be equal to or less than the thickness of the first base layer 20A.

[0152] Intensity I of the (040) plane peak in the X-ray diffraction pattern obtained by X-ray diffraction measurement of the second base layer 10A 040 Intensity of the (110) plane peak I 110 The peak intensity ratio A is 0.75 or more. The peak intensity ratio A is preferably 0.80 or more, and more preferably 0.90 or more. The peak intensity ratio A may be 2 or less, 1.5 or less, 1.3 or less, or 1.1 or less.

[0153] [Barrier Film] The barrier film 25 includes an anchor coat layer 21, a vapor deposition layer 22, and a gas barrier layer 23 between the first base layer 20A and the second base layer 10A. When the vapor deposition layer 22 and the gas barrier layer 23 are provided between the second base layer 10A and the first base layer 20A in this way, the laminate 100A can have better interlayer adhesion even after heat sterilization treatment, compared to when the vapor deposition layer 22 and the gas barrier layer 23 are provided between the first base layer 20A and the sealant layer 30A.

[0154] (1) Anchor Coat Layer The anchor coat layer 21 is a layer for further improving the adhesion between the first substrate layer 20A and the vapor deposition layer 22, and is provided between the first substrate layer 20A and the vapor deposition layer 22.

[0155] The material constituting the anchor coat layer 21 includes an organic polymer. The organic polymer may be at least one of a polyacrylic resin, a polyol resin, a polyurethane resin, a polyamide resin, or a reaction product of these resins.

[0156] The polyurethane resin may contain a reaction product of a polyol compound and an isocyanate compound. From the viewpoint of transparency, the polyol compound is preferably an acrylic polyol. The isocyanate compound mainly functions as a crosslinking agent or a curing agent.

[0157] The proportion of the organic polymer in the material constituting the anchor coat layer 21 may be 50% by mass or more, or may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. When the proportion of the organic polymer is 50% by mass or more, the heat resistance, water resistance, and flexibility of the barrier film 25 can be further improved.

[0158] The softening temperature T2 of the anchor coat layer 21 may be higher than the softening temperature T1 of the first base layer 20A, but is preferably in the range of 140°C or higher and 195°C or lower. A softening temperature T2 of 140°C or higher can improve the heat resistance of the anchor coat layer 21, reducing deformation of the anchor coat layer 21 even at high temperatures during heat sterilization treatment such as retort, thereby reducing damage to the vapor deposition layer 22. Therefore, the barrier film 25 can further improve the oxygen permeability even after heat sterilization treatment. The softening temperature T2 is preferably 142°C or higher, more preferably 145°C or higher, and particularly preferably 150°C or higher.

[0159] Furthermore, by setting the softening temperature T2 of the anchor coat layer 21 to 195°C or lower, the anchor coat layer 21 does not become too hard, and the barrier film 25 is more likely to have durability against deformation during heat sterilization treatment such as retort, and the vapor deposition layer 22 is less likely to be destroyed. The softening temperature T2 of the anchor coat layer 21 is more preferably 192°C or lower, and even more preferably 190°C or lower.

[0160] The anchor coat layer 21 may have only the softening temperature T2, or may have one or more softening temperatures higher than the softening temperature T2. When the anchor coat layer 21 has multiple softening temperatures, the lowest softening temperature among them is the softening temperature T2.

[0161] The softening temperature T2 of the anchor coat layer 21 can be adjusted by changing the compounding ratio of the components in the anchor coat layer forming composition or by adjusting the coating conditions (such as the drying temperature) when applying the anchor coat layer forming composition.

[0162] The thickness of the anchor coat layer 21 is not particularly limited as long as it is capable of improving the adhesion between the first substrate layer 20A and the vapor deposition layer 22, and may be 0.01 μm or more. In this case, compared to when the thickness of the anchor coat layer 21 is less than 0.01 μm, it is possible to further improve the smoothness of the surface of the anchor coat layer 21 relative to the surface of the first substrate layer 20A, making it possible to make the thickness of the vapor deposition layer 22 more uniform and further improving the oxygen barrier property. Therefore, the oxygen barrier property of the laminate 100A can be further improved. The thickness of the anchor coat layer 21 may be 0.03 μm or more, 0.04 μm or more, or 0.05 μm or more. By increasing the thickness of the anchor coat layer 21, it is possible to further suppress the deterioration of the water vapor barrier property when an external force such as stretching is applied. The thickness of the anchor coat layer 21 may be 1 μm or less. In this case, the flexibility of the laminate 100A is improved and the oxygen gas barrier properties of the laminate 100A after abuse can be further improved compared to when the thickness of the anchor coat layer 21 exceeds 1 μm. The thickness of the anchor coat layer 21 may be 0.3 μm or less or 0.2 μm or less. Note that the anchor coat layer 2 may be replaced with the anchor coat layer 2.

[0163] (2) Vapor Deposition Layer The vapor deposition layer 22 is a layer obtained by vapor deposition, and can further improve the gas barrier properties of the laminate 100 A. The vapor deposition layer 22 may or may not be transparent.

[0164] The deposition layer 22 is an inorganic oxide layer and is made of an inorganic oxide. Examples of inorganic oxides include oxides of metals. Examples of metals include at least one selected from the group consisting of Si, Al, Mg, Sn, Ti, and In. Examples of such metal oxides include aluminum oxide (AlO x ), silicon oxide (SiOx ), tin oxide, and magnesium oxide. These can be used alone or in combination of two or more. Among them, aluminum oxide or silicon oxide is preferred from the viewpoint of various sterilization resistance. Silicon oxide is particularly preferred as the inorganic oxide. In this case, the laminate 100A can have better water vapor barrier properties. The vapor deposition layer 22 may be composed of a single layer or multiple layers.

[0165] The thickness of the vapor-deposited layer 22 varies depending on the type of material used, but is generally preferably 5 to 300 nm, and the value is appropriately selected from this range. If the thickness of the vapor-deposited layer 22 is 5 nm or more, the vapor-deposited layer 22 is likely to become a uniform film and is likely to fully fulfill its gas barrier function. Furthermore, if the thickness of the vapor-deposited layer 22 is 300 nm or less, the vapor-deposited layer 22 is likely to retain flexibility, and the generation of cracks in the vapor-deposited layer 22 due to external factors such as bending or pulling the laminate 100A is more likely to be suppressed. The thickness of the vapor-deposited layer 22 is more preferably 10 to 150 nm. Note that an inorganic oxide layer 3 may be used instead of the vapor-deposited layer 22.

[0166] (3) Gas Barrier Layer The gas barrier layer 23 is a layer having gas barrier properties, and is obtained using a composition for forming a gas barrier layer. The composition for forming a gas barrier layer contains a water-soluble polymer and a silicon compound. The silicon compound contains at least one of a first silicon compound and a second silicon compound. The first silicon compound contains at least one of a silicon alkoxide represented by the following general formula (1) and a hydrolyzate thereof. The second silicon compound contains at least one of a silane coupling agent represented by the following general formula (2) and a hydrolyzate thereof. Si(OR 1 ) 4 ...(1) (In the above general formula (1), OR 1 represents a hydrolyzable group. 2 Si(OR 3 ) 3 ) n ...(2) (In the above general formula (2), OR 3 represents a hydrolyzable group, R 2 represents a monovalent organic group, and n is an integer of 1 or more.

[0167] The water-soluble polymer has a hydroxyl group. Examples of water-soluble polymers include polyvinyl alcohol resin, modified products thereof, and polyacrylic acid. These may be used alone or in combination of two or more. Among these, polyvinyl alcohol resin or modified products thereof is preferred as the water-soluble polymer. In this case, the gas barrier layer-forming composition can impart superior gas barrier properties to the laminate 100A upon curing. Furthermore, even after curing, the gas barrier layer-forming composition can impart superior flexibility to the laminate 100A, and can suppress the occurrence of cracks in the gas barrier layer 23 during processes such as lamination.

[0168] When the water-soluble polymer is composed of a polyvinyl alcohol resin or a modified product thereof, the degree of saponification of the water-soluble polymer is not particularly limited, but from the viewpoint of improving the gas barrier property of the laminate 100A, it is preferably 95% or more, and may be 100%. When the degree of saponification of the water-soluble polymer is 95% or more, the water resistance of the gas barrier layer 23 is increased, and deterioration of the gas barrier property of the laminate 100A can be suppressed even during heat sterilization treatment such as retort treatment.

[0169] The degree of polymerization of the water-soluble polymer is not particularly limited, but from the viewpoint of improving the gas barrier properties of the laminate 100A, it is preferably 300 or more. The degree of polymerization of the water-soluble polymer is preferably 450 to 2400. When the degree of polymerization of the water-soluble polymer is 2400 or less, the viscosity of the coating liquid (gas barrier layer-forming composition) is not too high, making it easier to form the gas barrier layer 23 with a uniform thickness.

[0170] The content of the water-soluble polymer is not particularly limited, but is preferably 25% by mass or more, based on the total mass of the water-soluble polymer and the silicon compound (100% by mass). In this case, curing can further improve the gas barrier properties and interlayer adhesion of the laminate 100A even after heat sterilization treatment. The content of the water-soluble polymer is preferably 26% by mass or more, more preferably 27% by mass or more, and particularly preferably 40% by mass or more, based on the total mass of the water-soluble polymer and the silicon compound.

[0171] The content of the water-soluble polymer is not particularly limited, but is preferably 60% by mass or less, more preferably 58% by mass or less, and particularly preferably 55% by mass or less, based on the total mass of the water-soluble polymer and the silicon compound (100% by mass). When the content of the water-soluble polymer is 60% by mass or less, the water resistance of the gas barrier layer 23 is improved, and the gas barrier properties and interlayer adhesion of the laminate 100A can be further improved even after heat sterilization treatment.

[0172] The first silicon compound is at least one of a silicon alkoxide and a hydrolyzate thereof. The silicon alkoxide is represented by the general formula (1) above. In this case, not only can the gas barrier properties of the laminate 100A be improved, but also the adhesion between the gas barrier layer 23 and the vapor deposition layer 22 can be improved, thereby suppressing intralayer delamination in the laminate 100A. In the general formula (1) above, OR 1 represents a hydrolyzable group. 1 Examples of the group include alkyl groups and -C 2 H 4 OCH 3 Examples of the alkyl group include a methyl group and an ethyl group. Of these, an ethyl group is preferred. In this case, the silicon alkoxide becomes tetraethoxysilane (TEOS), which becomes relatively stable in an aqueous solvent after hydrolysis.

[0173] The content of the first silicon compound is not particularly limited, but is preferably 40% by mass or more, more preferably 42% by mass or more, and particularly preferably 45% by mass or more, based on the total mass of the water-soluble polymer and the silicon compound (100% by mass). In this case, the gas barrier property and interlayer adhesion of the laminate 100A can be further improved even after heat sterilization treatment, compared to when the content of the first silicon compound is less than 40% by mass.

[0174] The content of the first silicon compound is preferably 75% by mass or less, more preferably 74% by mass or less, and particularly preferably 73% by mass or less, based on the total mass of the water-soluble polymer and the silicon compound (100% by mass). When the content of the first silicon compound is 75% by mass or less, the cured gas barrier layer 23 does not become too hard, cracks in the gas barrier layer 23 are less likely to occur, and the gas barrier properties are less likely to deteriorate. Furthermore, the gas barrier properties and interlayer adhesion of the laminate 100A can be further improved even after heat sterilization treatment. Furthermore, the amount of hydrochloric acid required for hydrolysis can be reduced, and the amount of chlorine in the laminate 100A is less likely to become excessive, which improves the recyclability of the laminate 100A.

[0175] The second silicon compound is at least one of a silane coupling agent and a hydrolyzate thereof. The silane coupling agent is represented by the above general formula (2). In this case, it is possible to improve the adhesion between the gas barrier layer 23 and the vapor deposition layer 22, and the interlayer adhesion of the laminate 100A can be further improved. In the above general formula (2), R 2 represents a monovalent organic group, and OR 3 represents a hydrolyzable group, and n represents an integer of 1 or more.

[0176] R 2 Examples of the monovalent organic group represented by the formula (I) include a monovalent organic group containing a vinyl group, an epoxy group, a mercapto group, an amino group, or an isocyanate group. Among these, a monovalent organic group containing an isocyanate group is preferred. In this case, the gas barrier layer-forming composition can have better hot water resistance upon curing, and can impart stronger laminate strength to the laminate 100A even after heat sterilization treatment.

[0177] R 3 Examples of the alkyl group include alkyl groups and -C 2 H 4 OCH 3Examples of the alkyl group include a methyl group and an ethyl group. Among them, a methyl group is preferable. In this case, the hydrolysis of the silane coupling agent is carried out quickly. 3 is R 2 When n is an integer of 2 or more, R 3 They may be the same or different from each other.

[0178] n represents an integer of 1 or greater. When n is 1, the silane coupling agent represents a monomer, whereas when n is 2 or greater, the silane coupling agent represents a polymer. n is preferably 3. In this case, the hot water resistance of the gas barrier layer 23 can be further improved, and it is possible to impart greater laminate strength to the laminate 100A even after heat sterilization treatment.

[0179] Examples of silane coupling agents include silane coupling agents having a vinyl group such as vinyltrimethoxysilane and vinyltriethoxysilane; silane coupling agents having an epoxy group such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropylethyldiethoxysilane; silane coupling agents having a mercapto group such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropylmethyldimethoxysilane; silane coupling agents having an amino group such as 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane; and silane coupling agents having an isocyanate group such as 3-isocyanatepropyltriethoxysilane and 1,3,5-tris(3-methoxysilylpropyl)isocyanurate. These silane coupling agents may be used alone or in combination of two or more.

[0180] Among the above silane coupling agents, those of the general formula (NCO-R 4 Si(OR 3 ) 3 ) 3 (In the formula, R 4 Ha-(CH 2 ) nMost preferred is 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate represented by the formula (I), where n is 1 or greater. This 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate is hydrophobic due to the polarity of the nurate moiety, and can therefore impart high water resistance to the gas barrier layer 23.

[0181] The content of the second silicon compound is not particularly limited, but is preferably 3% by mass or more, more preferably 5% by mass or more, and particularly preferably 7% by mass or more, based on the total mass of the water-soluble polymer and the silicon compound (100% by mass). In this case, the curing can impart greater laminate strength to the laminate 100A even after heat sterilization treatment, compared to when the content of the second silicon compound is less than 3% by mass.

[0182] The content of the second silicon compound is preferably 20% by mass or less, more preferably 15% by mass or less, and particularly preferably 12% by mass or less, based on the total mass of the water-soluble polymer and the silicon compound (100% by mass). In this case, the contents of the water-soluble polymer and the first silicon compound in the gas barrier layer 23 are relatively higher than when the content of the second silicon compound exceeds 20% by mass, and therefore good gas barrier properties can be maintained.

[0183] When calculating the content of the water-soluble polymer, the first silicon compound, and the second silicon compound, the calculation of each content is carried out by dividing the mass of the first silicon compound by the mass of SiO 2 The mass of the second silicon compound is converted to the mass of R 2 Si(OH) 3 This is done by converting it into mass.

[0184] The composition for forming a gas barrier layer may contain known additives such as an isocyanate compound, a dispersant, a stabilizer, a viscosity modifier, a colorant, etc., as needed, to the extent that the gas barrier properties are not impaired.

[0185] The thickness of the gas barrier layer 23 is not particularly limited, but is preferably 0.1 μm or more. In this case, the gas barrier properties of the laminate 100A can be further improved even after heat sterilization treatment, compared to when the thickness of the gas barrier layer 23 is less than 0.1 μm. From the viewpoint of improving the gas barrier properties of the laminate 100A, the thickness of the gas barrier layer 23 is more preferably 0.15 μm or more, and particularly preferably 0.17 μm or more.

[0186] On the other hand, the thickness of the gas barrier layer 23 is preferably 1.0 μm or less. Compared to when the thickness of the gas barrier layer 23 exceeds 1.0 μm, the laminate 100A is less likely to curl, making it easier to use as a laminate for forming a packaging container. From the viewpoint of further improving the flexibility of the laminate 100A, the thickness of the gas barrier layer 23 is more preferably 0.7 μm or less, and particularly preferably 0.5 μm or less. Note that the gas barrier layer 4 may be used instead of the gas barrier layer 23.

[0187] [First Base Material Layer] The first base material layer 20A is a contact layer that comes into contact with the anchor coat layer 21 and contains a polypropylene film. The polypropylene film contains a polypropylene-based resin (hereinafter also referred to as "polypropylene resin"). Examples of polypropylene resins include homopolypropylene and propylene-α-olefin copolymer. These can be used alone or in combination of two or more. The first base material layer 20A may further have a layer containing a propylene-α-olefin copolymer or a mixture of a propylene-α-olefin copolymer and homopolypropylene on the surface of the polypropylene film for the purpose of improving adhesion between the first base material layer 20A and a layer that comes into contact with the first base material layer 20A.

[0188] The polypropylene resin contained in the polypropylene film may be any of a fossil fuel-derived polypropylene resin, a recycled polypropylene resin, and a biomass-derived polypropylene resin. These polypropylene resins may be used alone or in combination of two or more.

[0189] The first base layer 20A may further contain additives as needed, such as antioxidants, stabilizers, lubricants such as calcium stearate, fatty acid amides, and erucic acid amide, organic additives such as antistatic agents, and particulate lubricants such as silica, zeolite, syloid, hydrotalcite, and silicon particles.

[0190] The polypropylene film contained in the first base layer 20A may be a stretched film or an unstretched film. A stretched film can be obtained by forming the polypropylene resin into a sheet and stretching the sheet by a conventional means. The stretched film may be a uniaxially oriented film or a biaxially oriented film. From the viewpoint of imparting rigidity to the laminate 100A, the first base layer 20A is preferably a stretched film.

[0191] The surface of the first base material layer 20A may be subjected to a surface treatment such as plasma treatment or corona treatment in order to strengthen the adhesion between the first base material layer 20A and the anchor coat layer 21.

[0192] The first substrate layer 20A may be the same as or different from the second substrate layer 10A.

[0193] The intensity I of the (040) plane peak in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measurement of the first base layer 20A 040 Intensity of the (110) plane peak I 110 The peak intensity ratio A (= I 110 / I 040 ) is not particularly limited, and the peak intensity ratio A may be 0.75 or more or less than 0.75. When the peak intensity ratio A is less than 0.75, the peak intensity ratio A may be 0.6 or less, 0.55 or less, or 0.5 or less. The peak intensity ratio A may also be 0.2 or more, 0.3 or more, or 0.4 or more.

[0194] In the barrier film 25, T2-T1 is not particularly limited as long as it is greater than 0°C, but is preferably 70°C or less. When T2-T1 is 70°C or less, the difference in flexibility between the first substrate layer 20A and the anchor coat layer 21 is unlikely to increase, and the adhesion between the first substrate layer 20A and the anchor coat layer 21 is unlikely to decrease. T2-T1 is preferably 68°C or less, more preferably 60°C or less. Furthermore, T2-T1 is preferably 1°C or more, more preferably 2°C or more. When T2-T1 is 3°C or more, the effect of imparting flexibility to the first substrate layer 20A is enhanced, and the stress applied to the anchor coat layer 21 due to shrinkage of the first substrate layer 20A after heat sterilization treatment can be alleviated, thereby alleviating the stress applied to the vapor deposition layer 22. In other words, the difference in strain between the first substrate layer 20A and the anchor coat layer 21 can be effectively compensated for. This prevents damage to the vapor deposition layer 22 and suppresses deterioration of the barrier properties of the vapor deposition layer 22.

[0195] The softening temperature T1 of the first substrate layer 20A is not particularly limited as long as it is lower than the softening temperature T2 of the anchor coat layer 21, but is preferably between 115° C. and 170° C. When the softening temperature T1 is 115° C. or higher, the heat resistance of the first substrate layer 20A is not too low, and the first substrate layer 20A is less likely to soften during heat sterilization treatment, making it less likely that the adhesion to the anchor coat layer 21 will decrease or that the barrier properties will deteriorate. Furthermore, when the softening temperature T1 is 170° C. or lower, the flexibility of the first substrate layer 20A can be prevented from decreasing, and the adhesion strength between the first substrate layer 20A and the core layer 12 can be further increased.

[0196] The softening temperature T1 may be 120°C or higher, 125°C or higher, or 130°C or higher from the viewpoint of imparting heat resistance to the first base layer 20A, and may be 165°C or lower or 160°C or lower from the viewpoint of imparting flexibility to the first base layer 20A.

[0197] The first base material layer 20A may have only the softening temperature T1, or may have one or more softening temperatures higher than the softening temperature T1. When the first base material layer 20A has multiple softening temperatures, the lowest softening temperature among them is the softening temperature T1.

[0198] The thickness of the first substrate layer 20A is not particularly limited and may be, for example, 5 μm or more, 10 μm or more, or 15 μm or more. The thickness of the first substrate layer 20A may also be 100 μm or less, 80 μm or less, 60 μm or less, or 40 μm or less. When the thickness of the first substrate layer 20A is 5 μm or more and 100 μm or less, wrinkles and sagging are suppressed in the first substrate layer 20A during formation of the gas barrier layer 23, and the first substrate layer 20A has excellent processability, such as transportability. The substrate layer 1 may be used instead of the first substrate layer 20A.

[0199] [Adhesive Layer] The adhesive layer 40A is a layer that bonds the barrier film 25 to the sealant layer 30A or the second base layer 10A. Examples of adhesives that form the adhesive layer 40A include polyurethane resins obtained using an adhesive containing a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol and a bifunctional or higher isocyanate compound. Various polyols may be used alone or in combination. From the perspective of heat resistance during thermal sterilization (thermal sterilization resistance), two-component curing urethane adhesives are preferred. The adhesives may contain carbodiimide compounds, oxazoline compounds, epoxy compounds, phosphorus compounds, silane coupling agents, etc. to promote adhesion. From an environmental perspective, adhesives whose polymer components are derived from biomass or biodegradable may be used as adhesives used to form the adhesive layer 40A. The adhesive may also have barrier properties.

[0200] The amount of adhesive to be applied is, for example, 0.5 to 10 g / m from the viewpoint of obtaining the desired adhesive strength, followability, processability, etc. 2 The amount of adhesive after removing the solvent by heating and drying etc. may be 0.1 to 10 g / m 2The amount of adhesive after solvent removal may be 0.1 g / m 2 When the amount of adhesive after solvent removal is 10 g / m or more, the adhesive can be uniformly applied, and sufficient lamination strength is likely to be obtained in the laminate 100A. 2 If the thickness is less than this, peeling is unlikely to occur inside the adhesive, and the laminate strength of the laminate 100A is unlikely to decrease.

[0201] [Sealant Layer] The sealant layer 30A contains a polypropylene film. The polypropylene film contains a polypropylene resin. Examples of the polypropylene resin include homopolypropylene and propylene-α-olefin copolymer. These can be used alone or in combination of two or more.

[0202] The polypropylene resin contained in the polypropylene film may be any of fossil fuel-derived polypropylene resin, recycled polypropylene resin, and biomass-derived polypropylene resin. These polypropylene resins may be used alone or in combination. The sealant layer 30A may further contain additives as needed. Examples of additives include antioxidants, stabilizers, lubricants such as calcium stearate, fatty acid amides, and erucic acid amide, organic additives such as antistatic agents, and particulate lubricants such as silica, zeolite, syloid, hydrotalcite, and silicon particles.

[0203] The polypropylene film contained in the sealant layer 30A may be a stretched film or an unstretched film, but an unstretched film is preferred from the viewpoint of lowering the melting point and facilitating heat sealing.

[0204] The thickness of the sealant layer 30A is not particularly limited and may be, for example, 5 μm or more, 10 μm or more, 15 μm or more, 30 μm or more, or 50 μm or more. The thickness of the first base material layer 20A may be 150 μm or less, 125 μm or less, 100 μm or less, or 80 μm or less. When the thickness of the sealant layer 30A is 5 μm or more, packaging containers such as packaging bags are less likely to tear. When the thickness of the sealant layer 30A is 150 μm or less, the sealant layer 30A maintains its heat sealability, reducing the possibility of sealing defects. Note that a sealant layer 5 may be used instead of the sealant layer 30A.

[0205] (Laminate) The oxygen permeability of the laminate 100A at 30°C and 70% RH is not particularly limited, but is preferably 200 cc / m 2 In this case, the oxygen permeability at 30°C and 70% RH is preferably 200 cc / m 2 Compared to when the temperature exceeds 100°C / day·atm, when a packaging container is made using the laminate 100A and contents are placed in the packaging container to make a packaged product, deterioration of the contents due to oxygen can be effectively suppressed.

[0206] The oxygen permeability of the laminate 100A at 30°C and 70% RH is more preferably 100 cc / m 2 ·day·atm or less, and particularly preferably 50 cc / m 2 ・day・atm or less.

[0207] In the laminate 100A, the proportion of polypropylene resin in the entire laminate 100A is not particularly limited, but is preferably 90% by mass or more. By making the proportion of polypropylene resin in the entire laminate 100A 90% by mass or more, the laminate 100A can have higher recyclability. The proportion of polypropylene resin in the entire laminate 100A is more preferably 92% by mass or more, and particularly preferably 94% by mass or more.

[0208] The thickness of the laminate 100A is not particularly limited, but is preferably 200 μm or less. When the thickness of the laminate 100A is 200 μm or less, the heat sealability is less likely to decrease when producing a packaging container, and the laminate 100A is less likely to bend, making it easier to use as a packaging container. The thickness of the laminate 100A may be 40 μm or more, 80 μm or more, or 100 μm or more. When the thickness of the laminate 100A is 40 μm or more, the laminate 100A is less likely to buckle, making it easier to make bags using the laminate 100A, and the bags are more likely to stand upright after production.

[0209] <Method for Producing Laminate> Next, a method for producing the laminate 100A will be described. First, a second base material layer 10A is prepared. The second base material layer 10A is a layer having a peak intensity ratio A (=I) in an X-ray diffraction pattern obtained by X-ray diffraction measurement. 110 / I 040 The peak intensity ratio A can be adjusted, for example, by adjusting the amount of a nucleating agent blended into the raw material of the polypropylene film or by adjusting the stretching conditions of the polypropylene film before stretching.

[0210] On the other hand, a barrier film 25 is prepared. To do this, first a first base material layer 20A is prepared. Next, an anchor coat layer 21 is formed on the first base material layer 20A. The anchor coat layer 21 can be obtained by applying an anchor coat layer-forming composition onto the surface of the first base material layer 20A and drying it.

[0211] Next, a vapor deposition layer 22 is formed as an inorganic oxide layer on the anchor coat layer 21. The vapor deposition layer 22 can be formed using vacuum deposition, sputtering, ion plating, plasma vapor deposition (CVD), or the like. However, considering productivity, vacuum deposition is most preferred. The heating method used in vacuum deposition is preferably one of electron beam heating, resistance heating, and induction heating. However, considering the wide range of vapor deposition material options, electron beam heating is more preferred. Furthermore, vapor deposition can also be performed using a plasma-assisted method or an ion beam-assisted method to improve the adhesion between the vapor deposition layer 22 and the first substrate layer 20A and the density of the vapor deposition layer 22. Furthermore, reactive vapor deposition, in which various gases such as oxygen are blown into the vapor deposition film to increase the transparency of the vapor deposition film, may also be used. When forming the anchor coat layer 21 and the first substrate layer 20A, the anchor coat layer 21 and the first substrate layer 20A are formed so that when the softening temperatures of the anchor coat layer 21 and the first substrate layer 20A are measured by local thermal analysis (LTA), the softening temperature T1 of the first substrate layer 20A is lower than the softening temperature T2 of the anchor coat layer 21.

[0212] Next, a gas barrier layer 23 is formed on the vapor deposition layer 22. In this way, a barrier film 25 is obtained. The gas barrier layer 23 can be obtained by applying a composition for forming a gas barrier layer onto the vapor deposition layer 22 and drying it.

[0213] Examples of the coating method include wet film-forming methods such as gravure coating, dip coating, reverse coating, wire bar coating, and die coating.

[0214] Next, the second base layer 10A is formed via the adhesive layer 40A on the gas barrier layer 23 of the barrier film 25. Meanwhile, the sealant layer 30A is formed via the adhesive layer 40A on the first base layer 20A of the barrier film 25. In this manner, the laminate 100A is obtained.

[0215] <Packaging Product> Next, a second embodiment of the packaging product of the present disclosure will be described with reference to FIG. 6 . Note that FIG. 6 is a side view showing the second embodiment of the packaging product of the present disclosure. In FIG. 6 , the same components as those in FIG. 5 are designated by the same reference numerals, and redundant description will be omitted. As shown in FIG. 6 , the packaging product 400 includes a packaging container 300 and a content C to be contained in the packaging container 300. The packaging product 400 is obtained by using a pair of laminates 100A, heat-sealing a portion of the periphery of the laminates 100A with the sealant layers 30A facing each other, containing the content C, and then heat-sealing the remaining portion of the periphery of the laminates 100A. At this time, the packaging container 300 is also obtained at the same time.

[0216] This packaged product 400 has excellent lamination strength between the barrier film 25 and the sealant layer 30A, which is a separate film, even after heat sterilization. This allows the laminate to maintain excellent interlayer adhesion even after heat sterilization, thereby preventing delamination. The packaged product 400 also includes a packaging container 300 obtained using the laminate 100A. The laminate 100A includes a second base layer 10A, a barrier film 25, and a sealant layer 30A, in this order. The base layer of the barrier film 25 is the first base layer 20A, and the second base layer 10A, the first base layer 20A, and the sealant layer 30A all comprise polypropylene films. Since the peak intensity ratio A is 0.75 or higher, the laminate 100A has excellent recyclability and excellent interlayer adhesion even after heat sterilization. This also prevents delamination in the laminate 100A even after heat sterilization. Furthermore, the packaging container 300 remaining after the contents C are discharged from the packaged product 400 has excellent recyclability.

[0217] The packaged product 400 can also be obtained by folding one laminate 100A, heat-sealing a portion of the three peripheral edges of the laminate 100A with the sealant layers 30A facing each other, placing the contents C inside, and then heat-sealing the remaining peripheral edges of the laminate 100A. At this time, the packaged container 300 is also obtained at the same time.

[0218] Examples of the packaging container 300 include a packaging bag, a laminated tube container, and a liquid paper container.

[0219] The laminate of the present disclosure is not limited to the above-described embodiments. For example, in the third embodiment, the vapor deposition layer 22 and the gas barrier layer 23 are provided between the second substrate layer 10A and the first substrate layer 20A in the barrier film 25. However, as in a laminate 200 of a fourth embodiment shown in Fig. 7, the vapor deposition layer 22 and the gas barrier layer 23 may be provided between the sealant layer 30A and the first substrate layer 20A, instead of between the second substrate layer 10A and the first substrate layer 20A. This laminate 200 also has excellent recyclability and can maintain excellent interlayer adhesion even after heat sterilization treatment.

[0220] The vapor deposition layer 22 and the gas barrier layer 23 may be provided between the second base layer 10A and the first base layer 20A, and between the sealant layer 30A and the first base layer 20A. In the barrier film 25, the vapor deposition layer 22 and the gas barrier layer 23 are arranged in this order from the first base layer 20A side, but the gas barrier layer 23 and the vapor deposition layer 22 may also be arranged in this order from the first base layer 20A side.

[0221] The present disclosure is outlined as follows. [1] A barrier film comprising, in this order, a substrate layer containing a polypropylene resin, an anchor coat layer, and an inorganic oxide layer, the substrate layer having a contact layer in contact with the anchor coat layer, wherein, when the softening temperatures of the anchor coat layer and the contact layer are measured by local thermal analysis, the softening temperature T1 of the contact layer is lower than the softening temperature T2 of the anchor coat layer. [2] The barrier film according to [1], wherein the softening temperature T2 of the anchor coat layer is in the range of 140°C or higher and 195°C or lower. [3] The barrier film according to [1] or [2], wherein the substrate layer further comprises a core layer on the opposite side of the contact layer from the anchor coat layer, the contact layer being a skin layer, and the softening temperature T1 of the contact layer is lower than the softening temperature T3 of the core layer. [4] The barrier film according to any of [1] to [3], wherein T2 - T1 is 70°C or lower. [5] The barrier film according to any one of [1] to [4], wherein the contact layer comprises a copolymer of propylene and an α-olefin. [6] The barrier film according to any one of [1] to [5], wherein the anchor coat layer comprises a polyurethane resin. [7] The barrier film according to any one of [1] to [6], wherein the anchor coat layer has a thickness of 0.05 to 2 μm. [8] A laminate comprising the barrier film according to any one of [1] to [7] and a sealant layer, wherein the sealant layer comprises a polyolefin. [9] The laminate according to [8], further comprising a second substrate layer on the surface of the barrier film opposite to the sealant layer, wherein the second substrate layer comprises a polyolefin resin.

[10] The laminate according to

[10] , comprising the second substrate layer, the barrier film, and the sealant layer in this order, wherein the substrate layer of the barrier film is a first substrate layer, wherein the second substrate layer, the first substrate layer, and the sealant layer all comprise polypropylene films, wherein the intensity I of the (040) plane peak in an X-ray diffraction pattern obtained by X-ray diffraction measurement of the second substrate layer 040 Intensity of the (110) plane peak I 110The laminate according to [9], wherein a peak intensity ratio A, which is the ratio of the above, is 0.75 or more.

[11] The laminate according to [9] or

[10] , wherein the second substrate layer is an unstretched film and the first substrate layer is a stretched film.

[12] The laminate according to

[10] or

[11] , further comprising the inorganic oxide layer and a gas barrier layer at least one between the first substrate layer and the second substrate layer and between the first substrate layer and the sealant layer.

[13] The laminate according to

[12] , further comprising the inorganic oxide layer and the gas barrier layer between the first substrate layer and the second substrate layer.

[14] The laminate according to

[12] or

[13] , wherein the inorganic oxide layer is a vapor-deposited layer, and the vapor-deposited layer contains at least one of aluminum oxide and silicon oxide.

[15] The laminate according to any one of

[12] to

[14] , wherein the gas barrier layer is a layer formed from a coating liquid containing a silicon compound and a water-soluble polymer, the silicon compound contains at least one of a first silicon compound and a second silicon compound, the first silicon compound contains at least one of a silicon alkoxide represented by the following general formula (1) and a hydrolyzate thereof, and the second silicon compound contains at least one of a silane coupling agent represented by the following general formula (2) and a hydrolyzate thereof. Si(OR 1 ) 4 ...(1) (In the general formula (1), OR 1 represents a hydrolyzable group. 2 Si(OR 3 ) 3 ) n ...(2) (In the general formula (2), OR 3 represents a hydrolyzable group, R 2 represents a monovalent organic group. n is an integer of 1 or more.)

[16] Oxygen transmission rate at 30°C and 70% RH is 200 cc / m 2

[17] The laminate according to any one of

[10] to

[15] , wherein the viscosity is 1 / 3 day·atm or less.

[17] The laminate according to any one of

[10] to

[16] , wherein the anchor coat layer contains an organic polymer, and the organic polymer contains at least one of a polyacrylic resin, a polyol resin, a polyurethane resin, a polyamide resin, and a reaction product of these resins.

[18] The laminate according to any one of

[10] to

[17] , wherein the anchor coat layer has a thickness of 0.01 to 1 μm.

[19] A packaging container formed using the laminate according to any one of [8] to

[18] .

[20] A packaged product comprising a packaging container and contents to be accommodated in the packaging container, wherein the packaging container is the packaging container according to

[19] .

[0222] The present disclosure will be explained in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to these examples.

[0223] <Preparation of Anchor Coat Layer-Forming Compositions> Anchor coat layer-forming compositions AC1, AC2, and AC3 were prepared as follows. (AC1) Acrylic polyol and tolylene diisocyanate were mixed such that the number of NCO groups in tolylene diisocyanate was equal to the number of OH groups in the acrylic polyol, and the mixture was diluted with ethyl acetate to a solids content (total amount of acrylic polyol and tolylene diisocyanate) of 5% by mass. β-(3,4-epoxycyclohexyl)trimethoxysilane was further added to the diluted mixture in an amount of 5 parts by mass per 100 parts by mass of the total amount of acrylic polyol and tolylene diisocyanate, and the mixture was mixed to prepare anchor coat layer-forming composition AC1. (AC2) Takelac WPB-341 (manufactured by Mitsui Chemicals, Inc.) and isocyanate silane KBE-403 (manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed in a solids ratio of 9:1 to prepare anchor coat layer-forming composition AC2. (AC3) Acryl polyol Acrydic CL-1000 (manufactured by DIC Corporation) and tolylene diisocyanate (TDI) type curing agent Coronate 2030 (manufactured by Tosoh Corporation) were blended as an isocyanate compound in a solid content mass ratio of 6:4, and ethyl acetate was used as a dilution solvent to prepare anchor coat layer forming composition AC3 (solid content: 2% by mass).

[0224] <Preparation of Coating Liquid> Coating liquids used as compositions for forming gas barrier layers in the Examples and Comparative Examples were prepared as follows. (Coating Liquid 1) A solution was prepared by mixing the following liquids A, B, and C in a blending ratio (mass ratio) of 70 / 20 / 10. Liquid A: A hydrolyzed solution (solid content 5 mass % (SiO 2Solution B: A water / methanol solution containing 5% by mass of polyvinyl alcohol (water / methanol weight ratio = 95 / 5). Solution C: A hydrolyzed solution (solid content 5% by mass (R 1 ) obtained by gradually adding hydrochloric acid (1N) to a mixed solution of β-(3,4-epoxycyclohexyl)trimethoxysilane and isopropyl alcohol (IPA solution), stirring for 30 minutes, and hydrolyzing with a water / IPA solution (water / IPA weight ratio = 1 / 1). 2 Si(OH) 3 conversion), R 2 represents a 3,4-epoxycyclohexyl group).

[0225] (Coating Liquid 2) A solution prepared by mixing the following liquids A, B, and C in a blending ratio (mass ratio) of 45 / 45 / 10. Liquid A: Tetraethoxysilane (trade name: KBE04, solid content: 100%, manufactured by Shin-Etsu Chemical Co., Ltd., hereinafter also referred to as "TEOS"), methanol (manufactured by Kanto Chemical Co., Ltd.), and 0.1N hydrochloric acid (manufactured by Kanto Chemical Co., Ltd.) were mixed in a ratio of 17 / 10 / 73 (mass ratio), and the solution obtained by hydrolyzing TEOS (5 mass% of TEOS (SiO 2 (R conversion) hydrolysis solution). Solution B: 5 mass % aqueous solution of polyvinyl alcohol (trade name: Kuraray Poval 60-98, manufactured by Kuraray Co., Ltd., hereinafter also referred to as "PVA") Solution C: 1,3,5-tris(3-methoxysilylpropyl) isocyanurate (trade name: X-12-965P, manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent was dissolved in a mixed solvent of water / IPA = 1 / 1 (mass ratio) until the solid content was 5 mass % (R conversion). 2 Si(OH) 3 The hydrolysis solution is diluted to obtain a solution of 1000 ppm (equivalent to 1000 ppm).

[0226] [Preparation of Barrier Film] Example 1 An ethylene-1-butene-propylene random copolymer resin (ethylene content: 2.5 mol %, 1-butene content: 3.5 mol %, propylene content: 94.0 mol %) was used as the material for the skin layer, and a homopolypropylene resin was used as the material for the core layer. These resins were co-extruded and then biaxially stretched to prepare a rectangular substrate film (substrate layer) with a total thickness of 20 μm.

[0227] Subsequently, the anchor coat layer forming composition AC1 was applied onto the skin layer of the base material layer by gravure coating and dried in an oven at 100° C. for 10 seconds to form an anchor coat layer with a thickness of 0.12 μm.

[0228] Next, silicon oxide was vapor-deposited on the anchor coat layer by reactive vapor deposition using high-frequency excited ion plating in an oxygen atmosphere under reduced pressure, thereby forming a vapor-deposited layer of inorganic oxide having a thickness of 30 nm.

[0229] Next, the above-mentioned coating liquid 1 was applied onto the vapor deposition layer by gravure coating and dried under conditions of 80°C for 20 seconds to form a gas barrier layer with a thickness of 0.3 µm, thereby producing a barrier film.

[0230] Example 2 A barrier film was produced in the same manner as in Example 1, except that a 1-butene-propylene random copolymer resin (1-butene content: 4.5 mol %, propylene content: 95.5 mol %) was used as the material for the skin layer.

[0231] Example 3 A barrier film was produced in the same manner as in Example 1, except that the anchor coat layer-forming composition AC2 was applied onto the skin layer of the base material layer by gravure coating, and then dried in an oven at 100°C for 10 seconds to form an anchor coat layer with a thickness of 1.5 µm.

[0232] Example 4 A barrier film was produced in the same manner as in Example 1, except that the anchor coat layer-forming composition AC1 was applied onto the skin layer of the base material layer by gravure coating and dried in an oven at 40°C for 30 seconds to form an anchor coat layer.

[0233] Comparative Example 1 A barrier film was produced in the same manner as in Example 1, except that an ethylene-propylene block copolymer resin (ethylene content: 1 mol %, propylene content: 99 mol %) was used as the material for the skin layer.

[0234] Example 5 A barrier film was produced in the same manner as in Example 1, except that an ethylene-propylene random copolymer resin (ethylene content: 2.5 mol %, propylene content: 97.5 mol %) was used as the material for the skin layer.

[0235] Example 6 A barrier film was produced in the same manner as in Example 1, except that an ethylene-propylene random copolymer resin (ethylene content: 10 mol %, propylene content: 90 mol %) was used as the material for the skin layer.

[0236] Example 7 A barrier film was produced in the same manner as in Example 1, except that when forming the anchor coat layer on the skin layer of the base material layer, the composition for forming the anchor coat layer was dried in an oven at 120°C.

[0237] Example 8 A barrier film was produced in the same manner as in Example 1, except that the anchor coat layer-forming composition AC2 was applied onto the skin layer of the base material layer by gravure coating, and dried in an oven at 120°C for 10 seconds to form an anchor coat layer with a thickness of 1.5 µm.

[0238] <Comparative Example 2> A barrier film was produced in the same manner as in Example 1, except that the anchor coat layer-forming composition AC2 was applied onto the skin layer of the base material layer by gravure coating, and dried in an oven at 40°C for 30 seconds to form an anchor coat layer with a thickness of 1.5 µm.

[0239] [Preparation of Laminate] A 60 μm thick unstretched polypropylene film was attached to the gas barrier layer side of each of the barrier films prepared in Examples 1 to 8 and Comparative Examples 1 and 2 using a two-component curing urethane adhesive by dry lamination to prepare a rectangular laminate.

[0240] [Retort Treatment] Two sheets of each of the laminates prepared in Examples 1 to 8 and Comparative Examples 1 and 2 were prepared, the two laminates were stacked with the sealant layers facing each other, and three of the four sides were heat-sealed to prepare a packaging bag. Water was filled into the remaining side as the content, and finally the remaining side was heat-sealed to obtain a packaged product. Thereafter, this packaged product was subjected to a retort sterilization treatment at 130°C for 60 minutes.

[0241] [Evaluation] <Softening Temperature Measurement> The softening temperatures of the skin layer and anchor coat layer of the base material layer were measured using the method described below. The above packaged product was retorted, and after draining the water, a laminate was cut out from the packaging bag. Corona treatment was performed on both the front and back surfaces of this laminate at 0.20 kW. A corona treater (product name: CT-0212) manufactured by Kasuga Electric Co., Ltd. was used for the corona treatment.

[0242] After corona treatment of the front and back surfaces of the laminate, the laminate was cut into strips with a razor blade, measuring 1.0 mm in base and 5.0 mm in height, to obtain cut pieces. The cut pieces were embedded in a photocurable resin, and the photocurable resin was cured using a halogen lamp (Kenko Tokina, product name: KTX-100R) to obtain block pieces. The photocurable resin used was D-800 (product name) manufactured by Toa Gosei Co., Ltd. The photocured block pieces were fixed in an insert for an AFM sample holder, and the cross-section of the sample was cut with a glass knife at room temperature (25°C) using a cross-section cutting device. Then, at a low temperature (-40°C), final cross-section cutting was performed with a diamond knife using the cross-section cutting device at a cutting speed of 1.0 mm / s and a cutting film thickness of 100 nm. Cutting was terminated when a mirror surface was obtained, and the cross-section of the laminate was exposed to obtain a measurement sample. The cross-section cutting devices used were an ultramicrotome (Leica, product name: EM UC7) and a cryosystem (Leica, product name: EM FC7). The cutting direction of the knife was parallel to the interface between the adjacent layers and perpendicular to the long sides of the strip-shaped cut pieces. The measurement sample was fixed in an insert for the AFM sample holder and used for softening temperature measurement.

[0243] The atomic force microscope (AFM) was an MFP-3D-SA (trade name) manufactured by Oxford Instruments, the local thermal analysis option was a Ztherm system (trade name), and the cantilever was an AN2-200 (trade name) manufactured by Anasys Instruments with a spring constant of 0.5 to 3.5 N / m, and softening temperature and cross-sectional shape measurements were performed on the measurement sample. The softening temperature measurements were performed at the center of the thickness direction of the skin layer and anchor coat layer of the substrate layer.

[0244] At this time, when setting the contact pressure of the cantilever (change in cantilever deflection (deflection)), the change in deflection voltage was set to 0.2 V for the skin layer and core layer of the base material layer and 1.5 V for the anchor coat layer, the voltage application rate (heating rate) was 0.5 V / sec, and the maximum applied voltage was 5.5 V. When the sample surface was heated after detrend correction, the sample surface expanded and the cantilever position rose. Further heating of the sample surface softened the sample surface and the cantilever position fell. The measurement was terminated when the cantilever fell 10 nm. If the Z displacement reached the maximum applied voltage without falling 10 nm from the change point, the maximum applied voltage during detrend correction and measurement was increased by 0.5 V, and the measurement was performed again.

[0245] The voltage applied at the point where the vertical height (Z displacement) of the cantilever was maximum was taken as the voltage applied at the softening point, and the voltage value was read.

[0246] To calculate the softening temperature of the samples, calibration curves were created for the measurement conditions of the skin layer and anchor coat layer of the substrate layer. The calibration samples were the following four polymeric materials, whose melting points (peak melting temperatures) had been measured in advance using a differential scanning calorimeter (DSC). Cross-sectional specimens were prepared in an environment below their glass transition temperatures: Polycaprolactone pellets (melting point: 60°C), low-density polyethylene pellets (melting point: 112°C), polypropylene pellets (melting point: 166°C), and biaxially oriented polyethylene terephthalate film (melting point: 255°C). Cross-sectional specimens were prepared using an ultramicrotome and cryosystem. Polycaprolactone was cut at -80°C, low-density polyethylene at -140°C, polypropylene at -40°C, and polyethylene terephthalate at room temperature (25°C). The measurement conditions were a voltage application rate (heating rate) of 0.5 V / sec, and a maximum applied voltage of 3.5 V for polycaprolactone, 5 V for low-density polyethylene, 6 V for polypropylene, and 7.8 V for polyethylene terephthalate. When setting the cantilever contact pressure (change in cantilever deflection (deflection)), the change in deflection voltage was set to 0.2 V for the calibration curves of the skin layer and core layer of the substrate layer, and 1.5 V for the calibration curve of the anchor coat layer. After detrend correction, the sample surface was heated and the applied voltage at the softening point was measured. The measurement position of the calibration sample was changed and the applied voltage at the softening point was measured 10 times. A calibration curve was created by approximating the average value of the applied voltage at the softening point and the melting point (melting peak temperature) measured by DSC with a cubic function using the least squares method.

[0247] Using a calibration curve of applied voltage and temperature, the temperatures corresponding to the applied voltage at the softening points of the skin layer and anchor coat layer of the substrate layer were determined, and these temperatures were designated as softening temperatures T1 and T2. The value of T2 - T1 was also calculated. The results are shown in Table 1 or Table 2. The results are shown in Table 1 or Table 2.

[0248] <Gas barrier property> The gas barrier property was evaluated based on oxygen permeability. The oxygen permeability was measured for a laminate cut out from a packaging bag obtained after removing water from a packaged product after retort treatment. The measurement was carried out using an oxygen permeability measuring device (OXTRAN 2 / 20, manufactured by Modern Control) under conditions of a temperature of 30°C and a relative humidity of 70%. The measurement method complies with JIS K-7126, Method B (constant pressure method), and ASTM D3985-81, and the measurement value is expressed in units of cm 3 (STP) / m 2 The oxygen permeability was expressed in units of 1 / day / atm. The results of the oxygen permeability are shown in Table 1 or Table 2.

[0249] <Lamination Strength> A laminate measuring 1.5 cm x 10 cm was cut out from the packaging bag obtained after draining the water from the packaged product after retort treatment, and the laminate strength between the barrier film and the sealant layer of the laminate was evaluated. The laminate strength was measured in accordance with JIS K6854, with a test width of 15 mm, a peel speed of 300 mm / min, and a T-type peel angle. The measured value was expressed in units of [N / 15 mm]. A laminate strength of 2 N / 15 mm or more was determined to have excellent laminate strength between the barrier film and the sealant layer. The results of the laminate strength are shown in Table 1 or Table 2.

[0250]

[0251]

[0252] Example 9 First, a rectangular unstretched polypropylene (PP) film 1 having a thickness of 50 μm was prepared as the second base layer, as shown in Table 3. When this PP film 1 was subjected to the X-ray diffraction measurement described later, a peak intensity I 040 The peak intensity ratio A (=I 110 / I 040 ) was 1.03 as shown in Table 3. PP film 1 had a three-layer structure, and all layers were made of polypropylene copolymer resin.

[0253] On the other hand, a 20 μm-thick biaxially oriented polypropylene film (product name "ME-1", OPP, manufactured by Mitsui Chemicals Tohcello, Inc.; hereinafter also referred to as "PP Film 5") was prepared as a first substrate layer. Next, the anchor coat layer-forming composition AC3 prepared as described above was applied to one side of the first substrate layer by gravure coating to form a coating film. The coating film was then passed through a 100°C oven for 10 seconds to dry, thereby forming an anchor coat layer with a thickness of 0.1 μm. Subsequently, a silicon oxide vapor-deposited layer was formed on the anchor coat layer to a thickness of 25 nm. The silicon oxide vapor-deposited layer was formed by evaporating silicon oxide using an electron beam vacuum deposition method using an electron beam heating system. Next, the coating liquid 2, which served as a gas barrier layer-forming composition prepared as described above, was applied to the silicon oxide vapor-deposited layer by gravure coating to form a coating film. The coating was then dried in an oven at 60°C for 60 seconds to form a gas barrier layer having a thickness of 0.3 µm, thus obtaining a barrier film (first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer).

[0254] The second substrate layer and the barrier film were then laminated by dry lamination, with the gas barrier layer of the barrier film facing the second substrate layer. A two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) was used in the dry lamination, and the adhesive layer was cured to form an adhesive layer. This resulted in a second structure (first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer / adhesive layer / second substrate layer).

[0255] Next, the second structure was laminated with a 60 μm-thick unstretched polypropylene film (product name "Torayfan ZK207" manufactured by Toray Industries, Inc.) as a sealant layer by dry lamination, with the first substrate layer of the second structure facing the sealant layer. A two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) was used in the dry lamination process, and the adhesive layer was cured to form a square-shaped laminate (sealant layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor deposition layer / gas barrier layer / adhesive layer / second substrate layer). The proportion of polypropylene resin in the entire laminate was 91% by mass.

[0256] Example 10 A laminate (sealant layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer / adhesive layer / second substrate layer) was produced in the same manner as in Example 9, except that a 30 μm-thick unstretched polypropylene (PP) film 2 was used as the second substrate layer, as shown in Table 3. When the PP film 2 was subjected to the X-ray diffraction measurement described below, the peak intensity ratio A was 0.81, as shown in Table 3. The PP film 2 had a three-layer structure, and all layers were composed of polypropylene copolymer resins. The proportion of polypropylene resin in the entire laminate thus obtained was 92% by mass.

[0257] Example 11 As shown in Table 3, a 30 μm-thick unstretched polypropylene (PP) film 2 (I 110 / I 040 = 0.81) was prepared. Then, this second substrate layer and a barrier film prepared in the same manner as in Example 9 were laminated by dry lamination, with the first substrate layer of the barrier film facing the second substrate layer. In the dry lamination method, a two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes Inc.) was used, and cured to form an adhesive layer. In this way, a third structure (second substrate layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer) was obtained.

[0258] Next, the third structure was laminated with a 60 μm-thick unstretched polypropylene film (product name "Torayfan ZK207" manufactured by Toray Industries, Inc.) as a sealant layer by dry lamination, with the gas barrier layer of the third structure facing the sealant layer. A two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) was used in the dry lamination process, and the adhesive layer was cured to form a laminate. This resulted in a laminate (second substrate layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer / adhesive layer / sealant layer). The proportion of polypropylene resin in the entire laminate was 91% by mass.

[0259] Example 12 A laminate (sealant layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer / adhesive layer / second substrate layer) was produced in the same manner as in Example 9, except that a 25 μm-thick stretched polypropylene (PP) film 3 was prepared as the second substrate layer, as shown in Table 3. When the PP film 3 was subjected to the X-ray diffraction measurement described below, the peak intensity ratio A was 0.72, as shown in Table 3. The PP film 3 had a three-layer structure, with the middle layer being composed of a homopolypropylene resin and the outer and inner layers being composed of a polypropylene copolymer resin. The inner layer was the layer on the adhesive layer side that bonded the gas barrier layer and the second substrate layer. The proportion of polypropylene resin in the entire laminate thus obtained was 92% by mass.

[0260] Example 13 A laminate (sealant layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor deposition layer / gas barrier layer / adhesive layer / second substrate layer) was produced in the same manner as in Example 9, except that a 25 μm-thick stretched polypropylene (PP) film 4 was prepared as the second substrate layer, as shown in Table 3. When the PP film 4 was subjected to the X-ray diffraction measurement described below, the peak intensity ratio A was 0.48, as shown in Table 3. The PP film 4 had a three-layer structure, with the outer and middle layers composed of homopolypropylene resin, and the inner layer composed of polypropylene copolymer resin. The proportion of polypropylene resin in the entire laminate thus obtained was 91% by mass.

[0261] Example 14 As shown in Table 3, a 30 μm-thick unstretched polypropylene (PP) film 2 (I 110 / I 040 = 0.81) was prepared.

[0262] On the other hand, a 20 μm-thick biaxially oriented polypropylene film (hereinafter also referred to as "PP film 6") was prepared as the first substrate layer. This biaxially oriented polypropylene film was composed of a core layer made of homopolypropylene and a skin layer made of an ethylene-1-butene-propylene random copolymer resin (ethylene content: 2.5 mol%, 1-butene content: 3.5 mol%, propylene content: 94.0 mol%). Next, the anchor coat layer-forming composition AC1 prepared as described above was applied to one side of the skin layer of the first substrate layer by gravure coating to form a coating film. The coating film was then passed through an oven at 100°C for 10 seconds to dry, thereby forming an anchor coat layer with a thickness of 0.12 μm. Subsequently, a silicon oxide vapor-deposited layer was formed on the anchor coat layer to a thickness of 30 nm. The silicon oxide vapor-deposited layer was formed by evaporating silicon oxide using an electron beam vacuum deposition method using an electron beam heating system. Next, the coating liquid 1 prepared as described above as a gas barrier layer-forming composition was applied onto the silicon oxide vapor-deposited layer by gravure coating to form a coating film. The coating film was then passed through an oven at 80°C for 20 seconds to dry, thereby forming a gas barrier layer with a thickness of 0.3 µm. In this way, a barrier film (first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer) was obtained.

[0263] The second substrate layer and the barrier film were then laminated by dry lamination, with the first substrate layer of the barrier film facing the second substrate layer. A two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) was used in the dry lamination, and the adhesive was cured to form an adhesive layer. This resulted in a third structure (second substrate layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer).

[0264] Next, the third structure was laminated by dry lamination to a 60 μm-thick unstretched polypropylene film (product name "Torayfan ZK207" manufactured by Toray Industries, Inc.) as a sealant layer, with the gas barrier layer of the third structure facing the sealant layer. In the dry lamination method, a two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) was used and cured to form an adhesive layer. In this way, a laminate (second substrate layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor deposition layer / gas barrier layer / adhesive layer / sealant layer) was obtained.

[0265] Example 15 As shown in Table 3, a 30 μm-thick unstretched polypropylene (PP) film 2 (I 110 / I 040 = 0.81) was prepared.

[0266] On the other hand, a 20 μm-thick biaxially oriented polypropylene film (hereinafter also referred to as "PP Film 7") was prepared as the first substrate layer. This biaxially oriented polypropylene film was constructed so that a core layer made of homopolypropylene was sandwiched between two skin layers made of ethylene-1-butene-propylene random copolymer resin (ethylene content: 2.5 mol%, 1-butene content: 3.5 mol%, propylene content: 94.0 mol%). Next, the anchor coat layer-forming composition AC1 prepared as described above was applied to one surface of the skin layer of the first substrate layer by gravure coating to form a coating film. The coating film was then passed through an oven at 100°C for 10 seconds to dry, thereby forming an anchor coat layer with a thickness of 0.12 μm. Subsequently, a silicon oxide vapor-deposited layer was formed on the anchor coat layer to a thickness of 30 nm. The silicon oxide vapor-deposited layer was formed by evaporating silicon oxide using an electron beam vacuum deposition method using an electron beam heating system. Next, the coating liquid 1 prepared as described above as a gas barrier layer-forming composition was applied onto the silicon oxide vapor-deposited layer by gravure coating to form a coating film. The coating film was then passed through an oven at 80°C for 20 seconds to dry, thereby forming a gas barrier layer with a thickness of 0.3 µm. In this way, a barrier film (first substrate layer / anchor coat layer / silicon oxide vapor-deposited layer / gas barrier layer) was obtained.

[0267] The second substrate layer and the barrier film were then laminated by dry lamination, with the gas barrier layer of the barrier film facing the second substrate layer. A two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) was used in the dry lamination, and the adhesive layer was cured to form an adhesive layer. This resulted in a second structure (second substrate layer / adhesive layer / gas barrier layer / silicon oxide vapor-deposited layer / anchor coat layer / first substrate layer).

[0268] Next, the second structure and a 60 μm-thick unstretched polypropylene film (product name "Torayfan ZK207" manufactured by Toray Industries, Inc.) serving as a sealant layer were laminated by dry lamination, with the first substrate layer of the second structure facing the sealant layer. In the dry lamination method, a two-component curing adhesive ("A525 / A52" manufactured by Mitsui Chemicals SKC Polyurethanes Co., Ltd.) was used and cured to form an adhesive layer. In this way, a laminate (second substrate layer / adhesive layer / gas barrier layer / silicon oxide vapor deposition layer / anchor coat layer / first substrate layer / adhesive layer / sealant layer) was obtained. In this way, a laminate (sealant layer / adhesive layer / first substrate layer / anchor coat layer / silicon oxide vapor deposition layer / gas barrier layer / adhesive layer / second substrate layer) was produced.

[0269] Example 16 A laminate (sealant layer / adhesive layer / gas barrier layer / silicon oxide vapor-deposited layer / anchor coat layer / first substrate layer / adhesive layer / second substrate layer) was produced in the same manner as in Example 14, except that a solvent-free adhesive was used as the adhesive bonding the second substrate layer and the first substrate layer, and as the adhesive bonding the gas barrier layer and the sealant layer. When PP film 2 was subjected to the X-ray diffraction measurement described below, the peak intensity ratio A was 0.48, as shown in Table 3.

[0270] [Peak Intensity Ratio A] The peak intensity ratio A for the PP films 1 to 4, which were the second substrate layers used in Examples 9 to 16, was determined by X-ray diffraction measurement. Specifically, the peak intensity ratio A was determined as follows. First, the X-ray diffraction pattern of the second substrate layer was obtained using a wide-angle X-ray diffractometer (ATX_G type, manufactured by Rigaku Corporation) by out-of-plane measurement, with the X-ray incident angle fixed at 0.5° and 2θ / θ scanning over a diffraction angle range of 10° to 30°. Characteristic X-rays, CuKα, were used as the X-rays, and the optical system was a slit collimation optical system. The X-rays were incident on the surface of the second substrate layer through an entrance slit with an opening of 0.1 mm x 10 mm, and the diffracted X-rays were detected by a detector through a solar slit as a receiving slit. From the obtained X-ray diffraction pattern, the peak intensity of the (110) plane at 2θ=14° and the peak intensity of the (040) plane at 2θ=17° were determined, and the peak intensity ratio A was calculated from these peak intensity values.

[0271] [Retort Treatment] Two sheets of each of the laminates prepared in Examples 9 to 16 were prepared, and the two laminates were stacked with the sealant layers facing each other, and three of the four sides were heat-sealed to prepare a packaging bag. Water was filled into the remaining side as the content, and finally the remaining side was heat-sealed to obtain a packaged product. Thereafter, this packaged product was subjected to a retort treatment at 120°C for 30 minutes.

[0272] [Evaluation] <Softening Temperature Measurement> The softening temperature T1 of the first substrate layer and the softening temperature T2 of the anchor coat layer were measured in the same manner as in Example 1. The value of T2 - T1 was also calculated. The results are shown in Table 3. <Interlayer Adhesion of Laminate> A laminate measuring 1.5 cm x 10 cm was cut out from the packaging bag obtained after removing water from the packaged product after retort treatment. The laminate was evaluated for the laminate strength between the second substrate layer and the first substrate layer and the laminate strength between the first substrate layer and the sealant layer, i.e., the interlayer adhesion of the laminate. The laminate strength was measured in accordance with JIS K6854, using a test width of 15 mm, a peel rate of 300 mm / min, and a T-type peel angle. The measured values ​​were expressed in units of [N / 15 mm]. A laminate strength of 2 N / 15 mm or more was considered to indicate excellent laminate strength between the barrier film and the sealant layer or the second substrate layer, and to indicate excellent interlayer adhesion of the laminate. The results of interlayer adhesion are shown in Table 4.

[0273]

[0274]

[0275] The results shown in Tables 1 to 3 indicate that the packaged products of Examples 1 to 16 had greater laminate strength after retort treatment than the packaged products of Examples 12 and 13. Furthermore, the laminates of Examples 9 to 13 had a high proportion of polypropylene resin, at 90% by mass or more, throughout the entire laminate. From the above, it was confirmed that the barrier film of the present disclosure exhibits excellent laminate strength with another film even after heat sterilization. Furthermore, it was confirmed that the laminate of the present disclosure exhibits excellent recyclability and excellent interlayer adhesion even after heat sterilization.

[0276] The barrier film according to the present disclosure has excellent lamination strength with other films such as sealant layers even when subjected to heat sterilization treatments such as boiling and retort treatment, and is therefore useful for laminates in packaging containers.

[0277] 1...substrate layer (first substrate layer), 2...anchor coat layer, 3...inorganic oxide layer, 4...gas barrier layer, 5...sealant layer (separate film), 10...barrier film, 11...skin layer (contact layer), 12...core layer, 20, 30...laminate, 31...second substrate layer, 40...packaging bag (packaging container), 100...packaged product, 10A...second substrate layer, 20A...first substrate layer, 21...anchor coat layer, 22...vapor deposition layer, 23...gas barrier layer, 25...first structure (barrier film), 30A...sealant layer, 40A...adhesive layer, 100A, 200...laminate, 300...packaging container, 400...packaged product, C...contents.

Claims

1. A barrier film comprising a base layer containing a polypropylene resin, an anchor coat layer, and an inorganic oxide layer in this order, the base layer having a contact layer in contact with the anchor coat layer, wherein, when the softening temperatures of the anchor coat layer and the contact layer are measured by local thermal analysis, the softening temperature T1 of the contact layer is lower than the softening temperature T2 of the anchor coat layer.

2. The barrier film according to claim 1, wherein the softening temperature T2 of the anchor coat layer is in the range of 140°C or higher and 195°C or lower.

3. The barrier film according to claim 1, wherein the base layer further has a core layer on the opposite side of the contact layer to the anchor coat layer, the contact layer being a skin layer, and the softening temperature T1 of the contact layer is lower than the softening temperature T3 of the core layer.

4. The barrier film according to claim 1 or 2, wherein T2-T1 is 70° C. or less.

5. The barrier film of claim 1 or 2, wherein the contact layer comprises a copolymer of propylene and an α-olefin.

6. The barrier film according to claim 1 or 2, wherein the anchor coat layer contains a polyurethane resin.

7. The barrier film according to claim 1 or 2, wherein the thickness of the anchor coat layer is 0.05 to 2 μm.

8. A laminate comprising the barrier film according to claim 1 or 2 and a sealant layer.

9. The laminate according to claim 8, further comprising a second substrate layer on a surface of said barrier film opposite said sealant layer, said second substrate layer comprising a polyolefin resin.

10. A laminate comprising the second base layer, the barrier film, and the sealant layer in this order, the base layer of the barrier film being a first base layer, the second base layer, the first base layer, and the sealant layer all containing polypropylene films, and an intensity I of a (040) plane peak in an X-ray diffraction pattern obtained by X-ray diffraction measurement of the second base layer 040 Intensity of the (110) plane peak I 110The laminate according to claim 9, wherein a peak intensity ratio A is 0.75 or more.

11. The laminate according to claim 10, wherein the second substrate layer is an unstretched film and the first substrate layer is a stretched film.

12. The laminate according to claim 10, further comprising the inorganic oxide layer and a gas barrier layer at least one between the first substrate layer and the second substrate layer and between the first substrate layer and the sealant layer.

13. The laminate according to claim 12, further comprising the inorganic oxide layer and the gas barrier layer between the first substrate layer and the second substrate layer.

14. The laminate according to claim 13, wherein the inorganic oxide layer is a vapor-deposited layer, the vapor-deposited layer comprising at least one of aluminum oxide and silicon oxide.

15. The laminate according to claim 12, wherein the gas barrier layer is a layer formed from a coating liquid containing a silicon compound and a water-soluble polymer, the silicon compound contains at least one of a first silicon compound and a second silicon compound, the first silicon compound contains at least one of a silicon alkoxide represented by the following general formula (1) and a hydrolyzate thereof, and the second silicon compound contains at least one of a silane coupling agent represented by the following general formula (2) and a hydrolyzate thereof. Si(OR 1 ) 4 ...(1) (In the general formula (1), OR 1 represents a hydrolyzable group. 2 Si(OR 3 ) 3 ) n ...(2) (In the general formula (2), OR 3 represents a hydrolyzable group, R 2 represents a monovalent organic group; and n is an integer of 1 or more.

16. Oxygen permeability at 30℃ and 70RH% is 200cc / m 2 The laminate according to claim 15, wherein the thermal expansion coefficient is 0.05-0.05 day-atm or less.

17. The laminate according to claim 10, wherein the anchor coat layer comprises an organic polymer, the organic polymer comprising at least one of a polyacrylic resin, a polyol resin, a polyurethane resin, a polyamide resin, and a reaction product of these resins.

18. The laminate according to claim 17, wherein the thickness of the anchor coat layer is 0.01 to 1 μm.

19. A packaging container formed using the laminate according to claim 8.

20. A packaging product comprising: a packaging container; and a content to be contained in the packaging container, the packaging container being the packaging container described in claim 19.

Citation Information

Patent Citations

  • Multilayer base material, multilayer film provided with the multilayer base material, multilayer body provided with the multilayer film, and packaging material provided with the multilayer body

    JP2021024266A

  • Adhesive film for metal terminals and batteries

    JP2022095833A

  • Gas barrier film

    WO2021220935A1

  • Packaging material, packaging bag and package

    WO2022196211A1