Temperature control member and electrostatic chuck device

The use of conductive ceramic temperature control members with specific material ratios and an electrostatic chuck device with a stress relaxation layer addresses the thermal expansion issues in metal temperature control members, achieving stable and wide-range temperature control in semiconductor processing.

WO2024219500A1PCT designated stage expired Publication Date: 2024-10-24SUMITOMO OSAKA CEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015641
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Metal temperature control members used in electrostatic chuck devices for semiconductor processing face challenges in controlling temperature over a wide range due to thermal expansion, which can cause strain and damage to the device.

Method used

A temperature control member made of conductive ceramic with a high thermal conductivity material and a conductive material, having a specific volume ratio and thermal expansion coefficient, is used, along with an electrostatic chuck device that includes a bonding layer with a stress relaxation layer to minimize thermal stress.

Benefits of technology

The solution provides effective temperature control with reduced thermal expansion, minimizing strain and damage, and enabling stable operation over a wide temperature range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015641_24102024_PF_FP_ABST
    Figure JP2024015641_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This temperature control member is formed of an electrically conductive ceramic, and has a flow path through which a heating medium flows. The electrically conductive ceramic contains a highly thermally conductive material and an electrically conductive material. The volume ratio of the highly thermally conductive material and the electrically conductive material is 10:90 to 90:10. The coefficient of thermal expansion of the electrically conductive ceramic at 800°C is at most 10×10-6 / K.
Need to check novelty before this filing date? Find Prior Art

Description

Temperature control member and electrostatic chuck device

[0001] This application claims priority to Japanese Patent Application No. 2023-069432, filed April 20, 2023, the contents of which are incorporated herein by reference.

[0002] A temperature control member such as a heat exchanger having a flow path inside can exchange heat with another member in contact with the flow path member by flowing a heat medium through the flow path. This allows the temperature of the other member in contact with the temperature control member to be adjusted. In this specification, the term "heat medium" includes both a heat medium (or heat transfer medium) for heating and a heat medium (or refrigerant) for cooling.

[0003] For example, in a semiconductor manufacturing process for manufacturing semiconductors such as ICs, LSIs, and VLSIs, an electrostatic chuck device is used to electrostatically attract a plate-like sample such as a silicon wafer when performing plasma processing on the plate-like sample. The electrostatic chuck device uses a metal base having a flow path for flowing a heat medium as a temperature control member, and cools an electrostatic chuck member supported by the base by flowing a coolant inside (see, for example, Patent Documents 1 and 2).

[0004] JP 2014-131015 A JP 2023-1603 A

[0005] With the diversification of semiconductor processes, electrostatic chuck devices are required to be able to control the temperature of plate-shaped samples during processing over a wider temperature range than ever before.Similarly, with regard to various devices that use temperature control members, as a result of the diversification of processes in which the devices are used, there is a demand for them to be usable over a wide temperature range, from high to low.

[0006] Metallic temperature control members such as those used in Patent Documents 1 and 2 have good thermal conductivity and allow heat to move easily. However, metallic temperature control members are prone to volumetric changes as the temperature of the member changes, which can easily cause distortion at the interface between the temperature control member and the object (object of temperature control) with which it comes into contact. Because this distortion can cause damage to the device, improvements were needed.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a novel temperature control member that is capable of good temperature control, and a further object of the present invention is to provide an electrostatic chuck device having such a temperature control member.

[0008] In order to solve the above problems, one aspect of the present invention includes the following aspects.

[0009] [1] A temperature control element made of conductive ceramics, having a flow path therein for allowing a heat medium to flow, the conductive ceramics being composed of a highly thermally conductive material and a conductive material, the volume ratio of the highly thermally conductive material to the conductive material being 10:90 to 90:10, and the conductive ceramics having a thermal expansion coefficient of 10×10 at 800°C. -6 / K or less.

[0010] [2] The high thermal conductivity material is AlN, SiC, GaN, SiO 2 , Al 2 O 3 , SmAlO 3 , MgO, SiO 2 , Si 3 N 4 , Al(OH) 3 , MgO, Mg(OH) 2 , BN, ZnO, BeO, B 4 At least one material selected from the group consisting of C, carbon, aluminum, copper, silver, and gold, and the conductive material is SiC, TiO 2 , TiN, TiC, W, WC, Mo, MoC, Mo 2 The temperature control element according to [1], which is at least one selected from the group consisting of C, TaC, TaN, NbC, VC and C.

[0011] [3] The temperature control element according to [2], wherein the highly thermally conductive material is AlN, and the electrically conductive material is either or both of TiN and Mo.

[0012] [4] The temperature control element according to [2], wherein the highly thermally conductive material is AlN and the electrically conductive material is Mo.

[0013] [5] The temperature control element according to [2], wherein the highly thermally conductive material is AlN, and the electrically conductive material is TiN and Mo.

[0014] [6] An electrostatic chuck device comprising: the temperature adjustment member according to any one of [1] to [5]; and an electrostatic chuck member supported by the temperature adjustment member and having a dielectric substrate and an internal electrode.

[0015] The present invention may also be embodied in the following manner: For example, the base of the electrostatic chuck device described in [A1] below may be the temperature control member described in [1] above.

[0016] [A1] An electrostatic chuck device comprising: an electrostatic chuck member having a dielectric substrate and an internal electrode; a base; and a bonding layer made of a metal material that bonds the electrostatic chuck member to the base, wherein the dielectric substrate is made of ceramics, and the base is made of conductive ceramics having a volume ratio of highly thermally conductive material to conductive material of 30:70 to 60:40.

[0017] [A2] The high thermal conductivity material is AlN, SiC, GaN, SiO 2 , Al 2 O 3 , SmAlO 3 , MgO, SiO 2 , Si 3 N 4 , Al(OH) 3 , MgO, Mg(OH) 2 , BN, ZnO, BeO, B 4 At least one material selected from the group consisting of C, carbon, aluminum, copper, silver, and gold, and the conductive material is SiC, TiO 2 , TiN, TiC, W, WC, MoC, Mo 2 The electrostatic chuck device according to [A1], wherein the material is at least one selected from the group consisting of C, TaC, TaN, NbC, VC, and C.

[0018] [A3] The electrostatic chuck device according to [A2], wherein the highly thermally conductive material is AlN and the electrically conductive material is TiN.

[0019] [A4] The electrostatic chuck device according to any one of [A1] to [A3], wherein the bonding layer includes a stress relaxation layer, a first bonding layer that bonds the stress relaxation layer to the electrostatic chuck member, and a second bonding layer that bonds the stress relaxation layer to the base.

[0020] [A5] The electrostatic chuck device according to [A4], wherein the stress relaxation layer is a metal foil made of at least one metal selected from the group consisting of Cu, Al, Ti, Nb, and W, the materials of the first bonding layer and the second bonding layer have a lower melting point than the material forming the stress relaxation layer, and the material of the first bonding layer is an alloy containing 50 volume % or more of Al or Ag and 0.02 volume % to 40 volume % of at least one metal selected from the group consisting of Ti, Zr, and Hf, when the entire first bonding layer is taken as 100 volume %.

[0021] [A6] The electrostatic chuck device according to [A5], wherein the first bonding layer and the second bonding layer are made of the same material.

[0022] [A7] An electrostatic chuck device according to any one of [A1] to [A6], which has a support plate on the opposite side of the base from the electrostatic chuck member, and the support plate is made of a material having a Young's modulus higher than that of the material of the base.

[0023] According to the present invention, it is possible to provide a novel temperature control member capable of excellent temperature control, and also to provide an electrostatic chuck device having such a temperature control member.

[0024] Fig. 1 is a cross-sectional schematic diagram showing a temperature control member and an electrostatic chuck device 1A according to a first embodiment. Fig. 2 is an explanatory diagram of an electrostatic chuck device 1B according to a second embodiment. Fig. 3 is a scanning electron microscope (SEM) image of the conductive ceramic plate used in Example 1. Fig. 4 is a scanning electron microscope (SEM) image of the conductive ceramic plate used in Example 4.

[0025] [First Embodiment] A temperature control member and an electrostatic chuck device according to a first embodiment of the present invention will be described below with reference to Fig. 1. The first embodiment and a second embodiment described later are specifically described to provide a better understanding of the spirit of the invention, and do not limit the present invention unless otherwise specified. For example, unless otherwise specified, conditions such as materials, amounts, types, numbers, sizes, shapes, positions, ratios, and temperatures may be changed, added, or omitted as necessary.

[0026] 1 is a cross-sectional schematic view showing a temperature control member and electrostatic chuck device 1A according to a first embodiment. The electrostatic chuck device 1A includes an electrostatic chuck member 2, a base 3, a bonding layer 4, a support plate 5, an insulator (insertion component) 23, and a power supply terminal 16. The electrostatic chuck member 2 and the base 3 are stacked together with the bonding layer 4 interposed therebetween. The base 3 corresponds to the "temperature control member" in the present invention.

[0027] In this specification, the direction in which the electrostatic chuck member 2 and the base 3 are stacked is referred to as the stacking direction. Furthermore, the side on which the electrostatic chuck member 2 is disposed with respect to the base 3 may be referred to as "one side in the stacking direction," and the opposite side may be referred to as "the other side in the stacking direction." In the following description, each part of the electrostatic chuck device 1A will be described assuming that the vertical direction is the stacking direction. However, the vertical direction here is used merely for the sake of simplicity of description and does not limit the position of the electrostatic chuck device 1A during use. The upper side corresponds to one side in the stacking direction, and the lower side corresponds to the other side in the stacking direction.

[0028] <Electrostatic Chuck Member> The electrostatic chuck member 2 has a dielectric substrate 11 and an attraction electrode (internal electrode) 13 located inside the dielectric substrate 11. A mounting surface 2 a for attracting and holding a wafer W is provided on the upper surface of the electrostatic chuck member 2. A focus ring surrounding the wafer W may be disposed outside the mounting surface 2 a of the electrostatic chuck member 2.

[0029] (Dielectric Substrate) The dielectric substrate 11 is preferably made of ceramics that has sufficient mechanical strength and is resistant to corrosive gases and their plasma.

[0030] The ceramics constituting the dielectric substrate 11 are mainly composed of aluminum oxide (Al 2 O 3 The term "main component" refers to a component that accounts for 50% or more by volume of the entire component. If necessary, aluminum oxide may account for 60% or more by volume, 70% or more by volume, 80% or more by volume, 90% or more by volume, or 98% or more by volume of the entire component. Examples of the ceramic include aluminum oxide (Al 2 O 3 ) sintered body, aluminum oxide (Al 2 O 3 In particular, from the viewpoints of dielectric properties at high temperatures, high corrosion resistance, plasma resistance, and heat resistance, the material constituting the dielectric substrate 11 is preferably Al 2 O 3 A sintered SiC composite is preferred.

[0031] The dielectric substrate 11 has a circular or substantially circular plate shape in a plan view. The dielectric substrate 11 has a mounting surface 2a on which the wafer W is mounted and a back surface 2b facing the opposite side of the mounting surface 2a. The mounting surface 2a may have, for example, a plurality of protrusions (not shown) formed at predetermined intervals. In this case, the mounting surface 2a supports the wafer W at the tips of the plurality of protrusions. In this specification, the term "plan view" refers to a field of view seen from the thickness direction (stacking direction) of the electrostatic chuck member 2.

[0032] (Attraction Electrode) The attraction electrode 13 is disposed inside the dielectric substrate 11. The attraction electrode 13 preferably extends in a plate shape along the mounting surface 2 a of the dielectric substrate 11. When a voltage is applied to the attraction electrode 13, the attraction electrode 13 generates an electrostatic attraction force that holds the wafer W on the mounting surface 2 a of the dielectric substrate 11. A power supply terminal 16 for applying a DC voltage to the attraction electrode 13 is connected to the attraction electrode 13.

[0033] The chucking electrode 13 is preferably made of a composite of an insulating material and a conductive material. The insulating material contained in the chucking electrode 13 is not particularly limited, but may be, for example, aluminum oxide (Al 2 O 3 ), aluminum nitride (AlN), silicon nitride (Si 3 N4 ), yttrium (III) oxide (Y 2 O 3 ), yttrium aluminum garnet (YAG) and SmAlO 3 It is preferable that the polymer is at least one selected from the group consisting of:

[0034] The conductive material contained in the attraction electrode 13 is molybdenum carbide (Mo 2 It is preferable that the material is at least one selected from the group consisting of molybdenum (Mo), tungsten carbide (WC), tungsten (W), tantalum carbide (TaC), tantalum (Ta), silicon carbide (SiC), carbon black, carbon nanotubes, and carbon nanofibers.

[0035] The thickness of the electrostatic chuck member 2 can be selected arbitrarily, but is preferably 0.5 mm or more and 5 mm or less. When the thickness of the electrostatic chuck member 2 is 0.5 mm or more, the withstand voltage of the electrostatic chuck member 2 increases. Furthermore, when the thickness of the electrostatic chuck member 2 is 5 mm or less, the heat capacity of the electrostatic chuck member 2 decreases, making it easier to maintain a uniform temperature of the plate-shaped sample, which is the processing target, during plasma processing.

[0036] <Base> The base 3 is a disc-shaped or approximately disc-shaped member in a plan view, and supports the electrostatic chuck member 2 from below (the other side in the stacking direction). The base 3 is provided with a support surface 3a facing upward (one side in the stacking direction) and a lower surface 3b facing downward. The support surface 3a faces the back surface 2b of the dielectric substrate 11 in the vertical direction (stacking direction) via the bonding layer 4. The base 3 supports the electrostatic chuck member 2 on the support surface 3a. The thickness of the base 3 can be selected arbitrarily as needed. For example, the thickness of the base 3 may be 20 mm to 50 mm.

[0037] A flow path 3f for circulating a heat medium (refrigerant) is provided inside the base 3. The refrigerant flowing through the flow path 3f can be selected arbitrarily, and may be water, He gas, N 2Gas, a fluorine-based inert liquid, liquid nitrogen, oil, alcohol, etc. are used. The flow path 3f extends along the support surface 3a. The coolant in the flow path 3f cools the entire base 3 and also cools the electrostatic chuck member 2 via the support surface 3a. The base 3 is connected to an external high-frequency power source 22 via a matching box (not shown), and may also serve as an internal electrode for generating plasma.

[0038] The base 3 is made of a conductive ceramic (hereinafter sometimes abbreviated as "conductive ceramic") containing a highly thermally conductive material and a conductive material. Specifically, when the entire base 3 is taken as 100% by volume, the material of the base 3 has a volume ratio of the highly thermally conductive material to the conductive material (volume of the highly thermally conductive material:volume of the conductive material) of 10:90 to 90:10, preferably 20:80 to 80:20, more preferably 25:75 to 70:30, and even more preferably 30:70 to 60:40. If necessary, the ratio may be 15:85 to 35:65, 35:55 ​​to 55:45, or 55:45 to 75:25, etc.

[0039] When the heat medium flows through the flow path 3f, it is expected that frictional charging will occur between the heat medium and the base 3. Since the charge generated in this way has adverse effects on the process and the device, it is preferable to quickly remove the charge. In contrast, by using a conductive ceramic material for the base 3, the charge generated by frictional charging can be easily removed.

[0040] The thermal expansion coefficient of the conductive ceramic material of the base 3 at 800°C is 10×10 -6 / K (10 ppm / K) or less, preferably 9 × 10 -6 / K or less, more preferably 8×10 -6 / K or less. By setting the thermal expansion coefficient of the base 3 to such a value, it is possible to suppress a change in the volume of the base 3 that accompanies a change in the temperature of the base 3 when a heat medium is flowed through the base 3. As a result, distortion is less likely to occur at the interface between the base 3 and the structure in contact with it (the bonding layer 4 in the case of the electrostatic chuck device 1A), and damage to the device can be suppressed. Note that the lower limit of the thermal expansion coefficient of the base 3 at 800°C can be selected arbitrarily, but may be set to, for example, 5 × 10 as needed. -6 / K or more, and may be 6×10 -6 / K or more, and may be 6.8 × 10 -6 / K or more.

[0041] The thermal expansion coefficient of the material of the base 3 at 800°C can be determined by the average coefficient of linear expansion (CTE) when the material of the base 3 is subjected to a temperature change from 25°C to 800°C.

[0042] The average linear expansion coefficient when the material (conductive ceramic) of the base 3 is changed in temperature from 25°C to 800°C can be measured using any measuring device, for example, a thermal expansion measuring device (TD5000SA, manufactured by NETZSCH). First, a measurement sample (test piece) made of conductive ceramic is heated from 25°C to 800°C at a temperature increase rate of 5°C / min, and the length (L0) of the measurement sample at 25°C and the length (L1) at 800°C are measured, and the change in length (ΔL) of the measurement sample is measured. The thermal expansion coefficient is calculated by dividing ΔL by the length (L0) of the measurement sample at 25°C, and then the thermal expansion coefficient is calculated by dividing the thermal expansion coefficient by the temperature change width (ΔT = 800°C - 25°C).

[0043] That is, the "coefficient of thermal expansion at 800° C." in this embodiment can be calculated by {(L1−L0) / L0} / ΔT=(ΔL / L0) / ΔT.

[0044] The base 3 is preferably made of a material with a thermal conductivity of 40 W / m·K or more, and more preferably 50 W / m·K to 110 W / m·K. The thermal conductivity may be 45 W / m·K to 100 W / m·K, 60 W / m·K to 90 W / m·K, or 70 W / m·K to 80 W / m·K, as needed. When the thermal conductivity is within the above range, input heat can be effectively dissipated.

[0045] The conductive material can be selected arbitrarily, but SiC, TiO 2 , TiN, TiC, W, WC, Mo, MoC, Mo 2Preferably, the conductive material is at least one selected from the group consisting of C, TaC, TaN, NbC, VC, and C. Among these, TiN is preferred because of its excellent plasma resistance. Mo and W are preferred because of their high thermal conductivity. As the conductive material, TiN and Mo may be used alone or in combination.

[0046] The high thermal conductivity material can be selected arbitrarily, but examples include AlN, SiC, GaN, and SiO 2 , Al 2 O 3 , SmAlO 3 , MgO, SiO 2 , Si 3 N 4 , Al(OH) 3 , MgO, Mg(OH) 2 , BN, ZnO, BeO, B 4 Preferably, the material is at least one selected from the group consisting of C, carbon (C), aluminum, copper, silver, and gold. Among these, AlN is preferred because of its high thermal conductivity and ease of handling.

[0047] When SiC is used as the highly thermally conductive material, a conductive material other than SiC is selected. When SiC is used as the highly thermally conductive material, for example, TiN can be selected as the conductive material. Similarly, when C is used as the highly thermally conductive material, a conductive material other than C is selected.

[0048] Furthermore, when combining the above-mentioned materials with a conductive material and a highly thermally conductive material, the resulting material preferably contains inorganic oxides, inorganic carbides, inorganic nitrides, and / or inorganic carbonitrides, which belong to either the conductive material or the highly thermally conductive material. Among these, it is preferable to contain inorganic oxides and / or inorganic nitrides. By including these, the resulting material can be said to be preferable as a "conductive ceramic."

[0049] Metal matrix composites (MMCs), which are composite materials of metal and ceramic, are also known as electrically conductive ceramic materials. However, MMCs are generally prepared by preparing a porous ceramic substrate and then introducing molten metals such as Mg, Al, and Si into the pores of the ceramic substrate (metal infiltration method, forging method). Therefore, the metals contained within are limited to metals with relatively low melting points. Such metals may melt depending on the conditions of use of the temperature control component.

[0050] On the other hand, in the conductive ceramics described above, high melting point metals (Mo: melting point 2622°C, W: melting point 3407°C) with melting points of 1800°C or higher can be used, compared to Mg (melting point 650°C), Al (melting point 660°C), and Si (melting point 1414°C) used as conductive materials in MMCs. Therefore, the base 3 can be suitably used even at high temperatures.

[0051] The thermal expansion coefficient of the dielectric substrate 11 can be selected arbitrarily. When the main component of the dielectric substrate 11 is aluminum oxide and is combined with silicon carbide, the thermal expansion coefficient of the dielectric substrate 11 is the thermal expansion coefficient of aluminum oxide at 800° C. (7.8×10 -6 / K~8.5 x 10 -6 / K) and the thermal expansion coefficient of silicon carbide at 800°C (4.1 × 10 -6 / K).

[0052] As the highly thermally conductive material contained in the temperature control member, it is advisable to select a material that can reduce the difference in the thermal expansion coefficient between the dielectric substrate 11 and the base 3, taking into consideration the thermal expansion coefficient of the conductive material to be combined. For example, when a material with a thermal expansion coefficient larger than that of aluminum oxide is used as the conductive material contained in the temperature control member, it is preferable that the highly thermally conductive material to be combined is a material with a relatively smaller thermal expansion coefficient than that of aluminum oxide, such as AlN. The thermal expansion coefficient of AlN at 40°C to 800°C is 5.2 x 10 -6 It is thought to be around / K.

[0053] The base 3 is made of AlN and TiN (thermal expansion coefficient at 900°C: 7.75 × 10-6 / K), i.e., an AlN-TiN composite sintered body. It is also preferable that the base 3 be made of conductive ceramics formed from SiC and TiN, i.e., a SiC-TiN composite sintered body.

[0054] The thermal expansion coefficient of the material of the base 3 at 800°C is 6.0 × 10 -6 / K or more 9.0×10 -6 / K or less. When the thermal expansion coefficient of the material of the base 3 is within the above range, it is easy to reduce the difference in thermal expansion with the dielectric substrate 11 containing mainly aluminum oxide, and distortion is less likely to occur at the interface between the electrostatic chuck member 2 and the base 3 when the electrostatic chuck member 2 and the base 3 are joined. Furthermore, even when the electrostatic chuck device 1A is used at high or low temperatures, distortion is less likely to occur at the interface between the electrostatic chuck member 2 and the base 3. The thermal expansion coefficient of the material of the base 3 at 800°C may be set to 6.5 × 10 or less, as needed. -6 / K or more 8.5×10 -6 / K or less, 6.8 x 10 -6 / K or more 8.3×10 -6 / K or less or 7.0 x 10 -6 / K or more 8.0×10 -6 / K or less.

[0055] The base 3 may contain one or more sintering aids as needed, as long as the effects of the present invention are not impaired. The amount and type of sintering aid are not particularly limited as long as they are generally added. 2 O 3 , MgO, SiO 2 , CaO, La 2 O 3 , Ce 2 O 3 , Y.O.F., Y.F. 3 Among these, Y 2 O 3 , MgO, SiO 2 , Y.F. 3 is preferred.

[0056] The volume resistivity of the base 3 can be selected arbitrarily, but is preferably 1.0×10 -3The volume resistivity of the base 3 is preferably in the above range, so that sufficient conductivity can be obtained. The lower the volume resistivity of the base 3, the better. However, the lower limit is, for example, 1.0×10 -10 The volume resistivity of the base 3 may be 1.0×10 Ω·cm or more, if necessary. -8 Ω・cm or more 1.0×10 -4 It may be Ω cm or less, and may be 1.0 × 10 -6 Ω・cm or more 1.0×10 -5 The volume resistivity of the base 3 may be 1.0×10 -6 Ω・cm or more 1.0×10 -5 Ω・cm or less or 1.0×10 -5 Ω・cm or more 1.0×10 -4 Ω・cm or less or 1.0×10 -4 Ω・cm or more 1.0×10 -3 It may be Ω·cm or less.

[0057] The thermal expansion coefficient at 800°C of the material of the base 3 is preferably the same as that of the dielectric substrate 11. The absolute value of the difference between the thermal expansion coefficient at 800°C of the material of the base 3 and the thermal expansion coefficient at 800°C of the material of the dielectric substrate 11 is 2.5×10 -6 / K or less, and preferably 1.5 × 10 -6 / K or less, and more preferably 1.3 × 10 -6 / K or less, and more preferably 1.0 × 10 -6 It is even more preferable that the value is 0.1 / K or less.

[0058] The surface of the base 3 is preferably provided with an alumina sprayed film as required to improve plasma resistance.

[0059] A hole 17 is provided in the base 3. The hole 17 extends in the vertical direction. The hole 17 penetrates the base 3 in the vertical direction and opens to the support surface 3a and the lower surface 3b of the base 3. The hole 17 has, for example, a circular or approximately circular shape in a plan view. An insulator 23, which will be described later, is preferably inserted into the hole 17. Although FIG. 1 shows the hole 17 as penetrating the base 3 in the vertical direction, the hole 17 does not necessarily have to penetrate the base 3 as long as it opens to at least the support surface 3a and an insulator 23 is inserted therein.

[0060] (Method for Manufacturing Conductive Ceramics) The conductive ceramics that are the material of the base 3 can be manufactured by any method. For example, they can be obtained by mixing a high thermal conductivity material and a conductive material in a predetermined range to obtain a raw material powder, and then using the obtained raw material powder to manufacture ceramics by a known method. Specific examples of manufacturing methods include, for example, mixing a high thermal conductivity material and a conductive material in an arbitrarily selected volume ratio, such as 10:90 to 90:10 or 30:70 to 60:40, to obtain a raw material powder, applying pressure to the obtained raw material powder to obtain a molded body, and pressure-sintering the obtained molded body to obtain a conductive ceramic. The obtained conductive ceramics can be manufactured by processing them into the shape of the base 3, thereby obtaining the base 3 of this embodiment.

[0061] The average primary particle size of the highly thermally conductive material is not particularly limited as long as a conductive ceramic is obtained, and for example, a highly thermally conductive material of 0.5 μm to 5 μm can be used. The average primary particle size may be 1.0 μm to 5.0 μm, or 2.0 μm to 4.0 μm. The average primary particle size of the conductive material is not particularly limited as long as a conductive ceramic is obtained, and for example, a conductive material of 0.5 μm to 5 μm can be used. The average primary particle size may be 1.0 μm to 5.0 μm, or 2.0 μm to 4.0 μm.

[0062] In the mixing step, the highly thermally conductive material and the electrically conductive material may be mixed to obtain a raw material powder, and the mixing method is not particularly limited. To prevent the highly thermally conductive material and the electrically conductive material from agglomerating, it is preferable to mix them with a dispersant or solvent as needed, and then mix them using a mixing device such as a disperser. The mixing device is not particularly limited, and general devices such as a ball mill, planetary mill, bead mill, and atomizer can be used.

[0063] A drying step may be performed after the mixing step. The drying method may be natural drying, a dryer, or spray drying to form granules of 30 to 100 μm from the raw material powder.

[0064] After the mixing step or the drying step, the raw material powder may be placed in a non-oxidizing atmosphere. For example, the raw material powder may be heated in a non-oxidizing atmosphere at an arbitrarily selected temperature, for example, 300° C. or higher and 600° C. or lower, to remove impurities contained in the raw material powder, such as moisture, solvent, and dispersant.

[0065] The non-oxidizing atmosphere is preferably an inert gas atmosphere using nitrogen or argon. When the heating is performed under an inert gas atmosphere, it is preferable to perform the heating treatment under a gas flow, in other words, a gas flow, in order to efficiently discharge generated impurities out of the system.

[0066] In the molding step, the obtained raw material powder is subjected to pressure, preferably uniaxial molding (uniaxial press molding), using a molding method that can be arbitrarily selected depending on the shape of the desired conductive ceramic, to obtain a molded body of the desired shape.

[0067] In the pressure sintering step, the compact obtained in the compacting step is pressed under a pressure of 5 MPa or more, preferably in a vacuum or a non-oxidizing atmosphere, while being heated to a temperature of 1600°C or higher. This procedure promotes sintering of the highly thermally conductive material and electrically conductive material contained in the compact, resulting in a dense sintered body with few pores. The temperature can be selected as needed, and may be 1600 to 1900°C or 1650 to 1800°C, for example. The heating time can be selected as needed, and may be, for example, 1 to 5 hours, 3 to 8 hours, or 6 to 12 hours.

[0068] The conductive ceramic can be obtained by the above steps, and the obtained conductive ceramic can be processed to obtain the base 3. The method for processing the obtained conductive ceramic can be selected arbitrarily. For example, the base 3 may be formed by joining a plurality of members having arbitrarily selected shapes.

[0069] <Bonding Layer> The bonding layer 4 bonds the electrostatic chuck member 2 and the base 3. Any material can be selected for the bonding layer 4, and for example, a known material used for bonding the electrostatic chuck member 2 and the base 3 can be used. For example, the material may be a silicone resin, a silicone resin containing a highly thermally conductive filler such as aluminum nitride particles or surface-coated aluminum nitride particles, or an inorganic material such as a metal material. From the viewpoint of controlling the temperature of the electrostatic chuck part 2, the material for the bonding layer 4 is preferably an inorganic material.

[0070] (Bonding Layer Material: Inorganic Material 1) When the inorganic material of the bonding layer 4 is a metal, the material of the bonding layer 4 is preferably an alloy containing 50 vol% to 99.98 vol% of Al or Ag and 0.02 vol% to 40 vol% of at least one metal selected from the group consisting of Ti, Zr, and Hf, when the entire bonding layer 4 is taken as 100 vol%. The proportion of Al or Ag may be, for example, 55 vol% to 95 vol%, 65 vol% to 90 vol%, or 70 vol% to 80 vol%. When the bonding layer 4 contains at least one metal selected from the group consisting of Ti, Zr, and Hf, the molten alloy formed by melting the material of the bonding layer 4 easily wets and spreads over the surface of the ceramic (electrostatic chuck member 2) during bonding between the electrostatic chuck member 2 and the base 3, facilitating bonding. Furthermore, since the bonding layer 4 contains the above metal, the metal and the ceramic (electrostatic chuck member 2) are easily bonded to each other, and the occurrence of voids at the interface can be suppressed, enabling a strong bond.

[0071] The thickness of the bonding layer 4 can be selected arbitrarily, but is preferably 5 μm to 500 μm. The thickness may be 5 μm to 30 μm, 30 μm to 100 μm, or 10 μm to 300 μm.

[0072] When manufacturing the electrostatic chuck device 1A, for example, a metal foil or a metal paste obtained by adding a binder to metal powder may be used as the material for forming the bonding layer 4. These materials are placed between the electrostatic chuck member 2 and the base 3 and heated to a temperature equal to or higher than the melting point of the metal material for forming the bonding layer 4, and the molten metal material spreads between the electrostatic chuck member 2 and the base 3, thereby forming the bonding layer 4.

[0073] By using a conductive ceramic as the material for forming the base 3, it is possible to suppress the occurrence of cracks when the base 3 and the electrostatic chuck member 2 are joined (brazed) with a metal material. The mechanism by which the occurrence of cracks is suppressed when the base 3 is joined by brazing by using a conductive ceramic as the material for forming the base 3 is presumed to be as follows.

[0074] The material forming the base must have excellent thermal conductivity, electrical conductivity, and workability. For this reason, it has traditionally been formed from metals such as aluminum. On the other hand, the dielectric substrate that forms the electrostatic chuck member is made from ceramics. In general, the thermal expansion coefficient of ceramics is significantly smaller than that of metals, so there is a large difference in the thermal expansion coefficient between the conventional base made of metal and the electrostatic chuck member made from ceramics.

[0075] For example, when the base material is aluminum, the melting point of aluminum is about 660°C, so there is no thermal expansion coefficient at 800°C. However, the thermal expansion coefficient of the base material (20°C to 100°C) is about 24×10 -6 On the other hand, when the main component of the material of the dielectric substrate 11 constituting the electrostatic chuck member 2 is aluminum oxide, the thermal expansion coefficient of the material of the dielectric substrate 11 (25°C to 800°C) is 7.8 × 10 -6 / K~8.5 x 10 -6 / K). That is, when the material of the base is aluminum and the material of the dielectric substrate 11 is mainly composed of aluminum oxide, the thermal expansion coefficient of the material of the dielectric substrate 11 is smaller than the thermal expansion coefficient of the material of the base.

[0076] Joining using metal materials (brazing) is performed at high temperatures of 500°C or higher (e.g., 800°C). Therefore, during brazing, the base and the electrostatic chuck member also become hot. If a metal base is used, tensile stress is likely to occur in the joining layer (brazing material layer) joining the metal base and the ceramic dielectric substrate 11 (electrostatic chuck member) due to the difference in thermal expansion coefficients between the two materials. This stress may cause cracks in the electrostatic chuck member.

[0077] On the other hand, the base 3 employed in the electrostatic chuck device 1A of this embodiment is made of a conductive ceramic. Therefore, the difference in thermal expansion coefficient between the material of the base 3 and the ceramic dielectric substrate 11 is smaller than that of a base made of metal. Furthermore, since the base 3 contains a highly thermally conductive material, its thermal conductivity is sufficiently high. Furthermore, since the base 3 contains a conductive material, its electrical conductivity is sufficiently high. Therefore, the tensile stress generated in the bonding layer 4 during brazing bonding of the electrostatic chuck member 2 and the base 3 is reduced, and heat can be effectively dissipated even after bonding. Therefore, in the electrostatic chuck device 1A of this embodiment, cracks are less likely to occur in the electrostatic chuck member 2.

[0078] Furthermore, in the electrostatic chuck device 1A formed in this manner, the bonding layer 4 is preferably formed from a metal material (brazing filler metal), and therefore heat can also be effectively released from the bonding layer 4. Therefore, in the electrostatic chuck device 1A, it is possible to lower the temperatures of the wafer W, the dielectric substrate 11, the bonding layer 4, and the base 3 relative to the plasma heat input, and stable temperature control is possible.

[0079] (Bonding Layer Material: Inorganic Material 2) When the inorganic material forming the bonding layer 4 is nonmetallic, the material contained in the electrostatic chuck member 2 or the base 3 can be used for the bonding layer 4. For example, an insulating material contained in the dielectric substrate 11 constituting the electrostatic chuck member 2, or a highly thermally conductive material or conductive material contained in the base 3 can be used as needed. By forming a bonding layer using the materials contained in the electrostatic chuck member 2 and the base 3, the electrostatic chuck member 2 and the base 3 can be bonded together. The bonding layer 4 may contain a binder component as long as it does not impair the effects of the invention, but it is preferable that it does not contain a binder. For example, the material forming the bonding layer 4 may contain a binder, and the resulting bonding layer 4 may contain no or almost no binder.

[0080] The inorganic material that is the material of the bonding layer 4 may include an insulating material contained in the dielectric substrate 11 that constitutes the electrostatic chuck member 2, and at least one of a highly thermally conductive material and a conductive material contained in the base 3. The bonding layer 4 may include a binder component as long as it does not impair the effects of the invention, but it is preferable that the bonding layer 4 does not include a binder component.

[0081] In this case, the bonding layer 4 can be formed using a bonding material (described later) containing the insulating material and at least one of the high thermal conductivity material and the conductive material. When the bonding layer 4 is to be insulating, the bonding material should contain a high thermal conductivity material but not a conductive material. When the bonding layer 4 is to be conductive, the bonding material should contain a conductive material.

[0082] As the binder component, for example, a resin material can be used. Resin materials that are less likely to undergo cohesive failure due to thermal stress are preferred, including silicone resins, acrylic resins, epoxy resins, phenolic resins, polyurethane resins, and unsaturated polyester resins. Among these, silicone resins are preferred because they have high elasticity and are less likely to undergo cohesive failure due to changes in thermal stress. It is preferred to use a volatile binder component so that no binder remains after the layers are bonded.

[0083] The ratio of the insulating material to at least one of the highly thermally conductive material and the electrically conductive material in the bonding layer 4 is not particularly limited as long as it bonds the electrostatic chuck member 2 and the base 3. Hereinafter, "at least one of the highly thermally conductive material and the electrically conductive material" may be abbreviated as "highly thermally conductive material, etc."

[0084] In the manufactured electrostatic chuck device 1A, if the interface between the bonding layer 4 and the electrostatic chuck member 2 is prone to peeling, it is advisable to increase the proportion of the insulating material in the bonding layer 4. Furthermore, in the electrostatic chuck device 1A, if the interface between the bonding layer 4 and the base 3 is prone to peeling, it is advisable to increase the content of the highly thermally conductive material or the like in the bonding layer 4.

[0085] In the bonding layer 4, the volume ratio of the insulating material to the highly thermally conductive material or the like can be selected arbitrarily, and may be, for example, 2:1 to 1:2, or 1:1 to 2:1.

[0086] The content of the binder component in the bonding layer 4 is not particularly limited as long as it bonds the electrostatic chuck member 2 and the base 3. In order to facilitate heat transfer in the bonding layer 4, it is preferable that the bonding layer 4 does not contain a binder component. The bonding layer 4 may contain the binder component in an amount of, for example, 1% by mass to 50% by mass, 10% by mass to 45% by mass, or 20% by mass to 40% by mass.

[0087] The thickness of the bonding layer 4 can be selected arbitrarily, and is preferably 1 μm to 50 μm, more preferably 5 μm to 30 μm, and even more preferably 10 μm to 20 μm.

[0088] The material (bonding material) of the bonding layer 4 may be, for example, a paste-like composition obtained by mixing an insulating material contained in the electrostatic chuck member 2 with a highly thermally conductive material contained in the base 3. The bonding layer 4 is formed between the electrostatic chuck member 2 and the base 3 by stacking the electrostatic chuck member 2 and the base 3 with a coating of the bonding material interposed therebetween, and then heating them under pressure (pressure heating) in a vacuum or in a non-oxidizing atmosphere.

[0089] The resulting bonding layer 4 contains the insulating material that is the material of the electrostatic chuck member 2. Therefore, the bonding layer 4 and the electrostatic chuck member 2 are preferably bonded together by applying pressure and heat.

[0090] Similarly, the resulting bonding layer 4 contains the highly thermally conductive material that is the material of the base 3. Therefore, the base 3 and the bonding layer 4 are preferably bonded together by applying pressure and heat.

[0091] As a result, the electrostatic chuck member 2 and the base 3 are bonded together via the bonding layer 4 .

[0092] The coating film of the bonding material can be formed by any method and under any conditions selected. For example, the coating film may be formed by applying the bonding material to at least one of the electrostatic chuck member 2 and the base 3 in a dry film thickness of 1 μm or more and 50 μm or less.

[0093] The conditions for the pressure and heat treatment may be any conditions that allow the electrostatic chuck member 2 and the base 3 to be joined together, and it is preferable to perform the heat treatment at a pressure of 5 MPa or more and at 1600° C. to 1800° C. for several hours.

[0094] By using an inorganic material for the bonding layer 4, in addition to the effect of the present invention, the base 3 can be more effectively heat-removed.

[0095] It was confirmed by simulation that the base 3 having the above-described configuration can transfer heat input to the dielectric substrate 11 and dissipate it effectively.

[0096] In the simulation, the dielectric substrate 11 is Al 2 O 3 The heat transfer effect of the base 3 was confirmed for electrostatic chuck device A, which used an AlN-TiN composite sintered body and an aluminum base 3, and electrostatic chuck device B, which used an AlN-TiN composite sintered body for the base 3. The simulation was performed using a silicone adhesive as the material for the bonding layer 4 in electrostatic chuck device A, and a metal brazing material (Ag) in electrostatic chuck device B.

[0097] In the simulation, the thermal conductivity per unit thickness of each layer was calculated from the thickness and thermal conductivity of the material of each layer.Then, the wafer temperature and the temperature of each layer were calculated assuming that a certain amount of heat is input to the wafer and a refrigerant at -70°C is flowing through the flow path.

[0098] As a result, when the temperature of the bonding layer 4 in the electrostatic chuck device A was T° C., the temperature of the bonding layer 4 in the electrostatic chuck device B was T−50° C. Furthermore, the temperatures of the dielectric substrate 11, the wafer W, and the contact portion between the wafer W and the dielectric substrate 11 were also 50° C. lower in the electrostatic chuck device B than in the electrostatic chuck device A. In other words, it was confirmed that by changing the material forming the base 3 from the conventional metal to a conductive ceramic, it is possible to effectively release (remove) plasma heat.

[0099] Furthermore, by checking the temperature of each layer in detail, it was confirmed that in the electrostatic chuck device A, heat transfer was inhibited in the bonding layer.

[0100] Considering only heat removal performance, electrostatic chuck device B, which uses a base made of conductive ceramics, may be considered to be at a disadvantage compared to electrostatic chuck device A, which uses a base made of a metal material. However, a base made of conductive ceramics can suitably employ a bonding layer made of an inorganic material with high thermal conductivity. Therefore, electrostatic chuck device B is considered to be able to transfer heat input to dielectric substrate 11 more comprehensively and dissipate it more effectively than electrostatic chuck device A. Furthermore, electrostatic chuck device B is considered to have the advantage of being less susceptible to distortion.

[0101] <Other Configurations> (Support Plate) The support plate 5 preferably supports the base 3 from the lower surface 3b of the base 3. The support plate 5 is preferably made of a material having a higher Young's modulus than the material of the base 3. For example, any of metal, MMC, and ceramics can be used as the material of the support plate 5. Among these, the support plate 5 is preferably made of Al, which has a higher Young's modulus than the material of the base 3. 2 O 3 It is preferable to use a ceramic plate such as the above.

[0102] The ceramic material used for the support plate 5 is preferably the same as the material used for the electrostatic chuck member 2. Specific examples of the ceramic material include aluminum oxide, aluminum nitride, and Al. 2 O 3 By using the same material for the support plate 5 and the electrostatic chuck member 2, the difference in thermal expansion coefficient between the materials of the support plate 5 and the electrostatic chuck member 2 can be reduced, and warping of the electrostatic chuck device 1A can be suppressed.

[0103] (Insulator) The insulator 23 is inserted into the hole 17 and assembled to the base 3. That is, the insulator 23 functions as an insertion part that is inserted into the hole 17. The insulator 23 has a cylindrical shape that extends in the vertical direction. The power supply terminal 16 is disposed inside the insulator 23. The outer circumferential surface of the insulator 23 is joined to the inner surface of the hole 17 using a joining means such as adhesive. The insulator 23 insulates the metal base 3 from the power supply terminal 16.

[0104] The insulator 23 is made of, for example, ceramics. That is, the insulator 23 is preferably made of an insulating material. This makes it possible for the insulator 23 to prevent the gas introduction hole from becoming a starting point for abnormal discharge. The insulator 23 has durability against plasma. Examples of ceramics that make up the insulator 23 include AlN, Al 2 O 3 , Si 3 N 4 , zirconium oxide (ZrO 2 ), sialon, boron nitride (BN), and SiC.

[0105] An upper end surface of the insulator 23 (hereinafter referred to as an upper end surface 23a) is in contact with the electrostatic chuck member 2 or is disposed between the insulator 2 and the electrostatic chuck member 2 via an insulating adhesive.

[0106] (Power Supply Terminal) The power supply terminal 16 extends downward from the chucking electrode 13. The power supply terminal 16 is connected to an external power supply 21. The power supply 21 applies a voltage to the chucking electrode 13. The number, shape, etc. of the power supply terminals 16 are determined depending on the type of the chucking electrode 13, i.e., whether it is a monopolar type or a bipolar type.

[0107] The power supply terminal 16 passes through a first hole 17a in the dielectric substrate 11, a second hole 17b in the bonding layer 4, and a third hole 17c in the support plate 5. The first hole 17a is provided in a portion of the dielectric substrate 11 below the chucking electrode 13.

[0108] The first hole 17a, the second hole 17b, and the third hole 17c are each circular or approximately circular when viewed in the stacking direction. The first hole 17a, the second hole 17b, and the third hole 17c are in communication with the hole 17 of the base 3.

[0109] The inner circumferential surfaces of the first hole 17a, the second hole 17b, and the third hole 17c are continuous with the inner circumferential surface of the insulator 23 when viewed from the stacking direction. The inner diameters of the first hole 17a, the second hole 17b, and the third hole 17c are approximately equal to the inner diameter of the insulator 23 and slightly larger than the outer diameter of the power supply terminal 16.

[0110] According to the base 3 (temperature control member) described above, it is possible to provide a novel temperature control member that is less susceptible to distortion and breakage, and that allows for good temperature control.

[0111] According to the electrostatic chuck device having the above-described configuration, by having such a temperature control member, it is possible to provide a novel electrostatic chuck device that is suppressed from being damaged and enables good temperature control.

[0112] Although the electrostatic chuck device 1A has a bonding layer 4, the electrostatic chuck member 2 and the base 3 may be directly bonded to each other without the bonding layer 4 by diffusion bonding the electrostatic chuck member 2 and the base 3.

[0113] In the above embodiment, the temperature control member is used as a base of an electrostatic chuck device, but the present invention is not limited to this. For example, the temperature control member may be used as a heat transfer medium for a heat exchanger, a heater unit, a battery module, or a nuclear reactor.

[0114] 2 is an explanatory diagram of an electrostatic chuck device 1B according to a second embodiment of the present invention. The electrostatic chuck device 1B of this embodiment has some components in common with the electrostatic chuck device 1A of the first embodiment. Therefore, the same components as those of the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.

[0115] The electrostatic chuck device 1B includes an electrostatic chuck member 2, a base 3, a bonding layer 6, a support plate 5, an insulator (insertion component) 23, and a power supply terminal 16. The electrostatic chuck member 2 and the base 3 are stacked on top of each other with the bonding layer 6 interposed therebetween.

[0116] (Bonding Layer) The bonding layer 6 has a stress relaxation layer 61, a first bonding layer 62 that bonds the stress relaxation layer 61 to the electrostatic chuck member 2, and a second bonding layer 63 that bonds the stress relaxation layer 61 to the base 3. The bonding layer 6 has a higher thermal conductivity than the base 3. It is preferable that the first bonding layer 62, the stress relaxation layer 61, and the second bonding layer 63 be in direct contact with each other, but this is not limited to this example.

[0117] The stress relaxation layer 61 is made of a material that is easily plastically deformed, and relieves thermal stress caused by the difference in thermal expansion coefficient between the electrostatic chuck member 2 and the base 3. The stress relaxation layer 61 is preferably made of a metal foil made of at least one metal selected from the group consisting of Cu, Al, and Ti.

[0118] Alternatively, the stress relaxation layer 61 may be made of Al, which is a material constituting the electrostatic chuck member 2. 2 O 3 Materials with a small difference in thermal expansion coefficient from Al can also be used. 2 O 3 The thermal expansion coefficient (7.8 x 10 -6 / K~8.5 x 10 -6 / K) and is used as a material for the stress relaxation layer. -6 / K), Nb (7.1 × 10 -6 / K), W (4.6 × 10 -6 The small difference in thermal expansion coefficient means, for example, that the difference is 4.0 × 10 -6 / K ~ 0.5 × 10 -6 / K. When comparing the thermal expansion coefficient of the material of the stress relaxation layer 61 with the thermal expansion coefficient of the material constituting the electrostatic chuck member 2, it is advisable to use the thermal expansion coefficients at the same measurement temperature.

[0119] The thickness of the stress relaxation layer 61 can be selected arbitrarily, but is preferably 0.1 mm to 1 cm, and more preferably 1 mm to 1 cm. If necessary, the thickness may be 0.5 mm to 8 mm, or 2 mm to 5 mm. When the thickness of the stress relaxation layer 61 is within this range, thermal stress can be sufficiently relaxed, and peeling between the electrostatic chuck member 2 and the base 3 can be suppressed.

[0120] The material of the first bonding layer 62 and the second bonding layer 63 preferably has a lower melting point than the material of the stress relaxation layer 61. The first bonding layer 62 and the second bonding layer 63 may be made of the same material.

[0121] The material of first bonding layer 62 can preferably be the same as that of bonding layer 4 of the first embodiment and can be made under the same conditions. That is, the material of first bonding layer 62 is preferably an alloy containing 50% by volume or more of Al or Ag and 0.02% by volume or more and 40% by volume or less of at least one metal selected from the group consisting of Ti, Zr, and Hf, when the entire first bonding layer 62 is taken as 100% by volume. The same material can also be used for second bonding layer 63.

[0122] The thickness of the first bonding layer 62 and the second bonding layer 63 can be selected arbitrarily, and is preferably, for example, 0.005 mm or more and 0.5 mm or less.

[0123] By providing the bonding layer 6 with the stress relaxation layer 61, the stress occurring at the interface between the base 3 and the electrostatic chuck member 2 is further relaxed, and peeling of the bonding layer 6 can be suppressed.

[0124] Even with the electrostatic chuck device 1B having the above-described configuration, it is possible to provide a novel electrostatic chuck device that is suppressed from being damaged and allows for good temperature control.

[0125] While the preferred embodiments of the present invention have been described above with reference to the accompanying drawings, the present invention is not limited to these examples. The shapes and combinations of the components shown in the above examples are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention.

[0126] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0127] The following test pieces were prepared and used in Example 1 and Comparative Example 1 described below. 2 O 3 :SiC=95:5 (mass ratio), thickness 2 mm) Conductive ceramic substrate (AlN:TiN=50:50, thickness 1 mm) Aluminum substrate (thickness 1 mm)

[0128] The conductive ceramic substrate was prepared by the following method.

[0129] (Preparation of Conductive Ceramic Substrate) A mixture of AlN particles having an average primary particle size of 1 μm, TiN particles having an average primary particle size of 1 μm, a dispersant, and ethanol was mixed for 12 hours using a ball mill using aluminum oxide media having a diameter of 1 mm to 5 mm. The AlN particles and TiN particles were weighed to have a volume ratio of 50:50.

[0130] The resulting mixture was then air-dried to obtain a raw material powder for the conductive ceramics, which was then heated at 500° C. in a nitrogen atmosphere for 12 hours.

[0131] The heated raw material powder was uniaxially press-molded at a pressure of 8 MPa using a die molding method to obtain a molded body, which was then set in a graphite mold and pressure-sintered at 1700°C for 2 hours under a nitrogen atmosphere at a pressure of 20 MPa to obtain a conductive ceramic substrate.

[0132] The obtained conductive ceramic substrate was processed to a thickness of 1 mm to obtain a test piece of the conductive ceramic substrate.

[0133] Fig. 3 is a scanning electron microscope (SEM) image of the conductive ceramic plate produced by the above method. More specifically, Fig. 3 is an image of the conductive ceramic plate observed with a field emission scanning electron microscope (FE-SEM) (manufactured by Zeiss, product name: Merlin). In Fig. 3, the areas that appear relatively dark are areas occupied by AlN, and the areas that appear relatively light are areas occupied by TiN. From Fig. 3, it was confirmed that a conductive ceramic in which AlN and TiN were mixed approximately uniformly was obtained.

[0134] [Example 1] A dielectric substrate and a conductive ceramic substrate were bonded using a metal brazing filler metal (TKC-661, manufactured by Tanaka Kikinzoku Kogyo K.K.) at 860°C under a pressure of 13 Pa. As a result, no cracks were found in either the dielectric substrate or the conductive substrate, and it was confirmed that bonding could be performed without any problems.

[0135] Comparative Example 1 A dielectric substrate and an aluminum substrate were bonded using a metal brazing filler metal (TKC-661, manufactured by Tanaka Kikinzoku Kogyo K.K.) at 550° C. under a pressure of 13 Pa. As a result, although the dielectric substrate and the aluminum substrate could be bonded, cracks occurred in the dielectric substrate, and it was confirmed that this bonded body was unsuitable for use in an electrostatic chuck device.

[0136] Although the results of Example 1 and Comparative Example 1 described above were obtained using test pieces, it is believed that similar behavior also occurs at the interface between the electrostatic chuck member 2 made of a dielectric substrate and the base 3 made of a conductive ceramic. In other words, when an electrostatic chuck member made of a dielectric substrate and a base made of a conductive ceramic as defined in the present invention are brazed together, it is expected that no cracks will occur in either the dielectric substrate or the conductive substrate, and a favorable joining will be possible.

[0137] [Examples 2 to 7] Conductive ceramic substrates having the compositions shown in Table 1 below were prepared, and their thermal expansion coefficients and volume resistivities were measured. The conductive ceramic substrates were produced by the method described above in (Preparation of conductive ceramic substrate).

[0138] That is, the conductive ceramic plate of Example 2 was produced in the same manner as Example 1, except that the AlN particles and TiN particles were weighed out so as to have a volume ratio of 40:60.

[0139] The conductive ceramic plate of Example 3 was produced in the same manner as in Example 1, except that the AlN particles and TiN particles were weighed out so as to have a volume ratio of 65:35.

[0140] The conductive ceramic plate of Example 4 was produced in the same manner as in Example 1, except that Mo particles having an average primary particle diameter of 1.5 μm were used instead of the TiN particles having an average primary particle diameter of 1 μm, and the AlN particles and Mo particles were weighed out to have a volume ratio of 35:65.

[0141] The conductive ceramic plate of Example 5 was produced in the same manner as in Example 4, except that the AlN particles and Mo particles were weighed out so as to have a volume ratio of 65:35.

[0142] A backscattered electron image of the conductive ceramic plate of Example 5 observed with a field emission scanning electron microscope (FE-SEM) (manufactured by Zeiss, product name: Merlin) is shown in Figure 4. In Figure 4, the areas that appear relatively dark are areas occupied by AlN, and the areas that appear relatively light are areas occupied by Mo. It was confirmed from Figure 4 that a conductive ceramic in which AlN and Mo were mixed approximately uniformly was obtained.

[0143] The conductive ceramic plate of Example 6 was produced in the same manner as Example 1, except that in addition to the AlN particles and TiN particles, Mo particles having an average primary particle size of 1.5 μm were used, and the AlN particles, TiN particles, and Mo particles were weighed in a ratio of 29:36:35.

[0144] The conductive ceramic plate of Example 7 was produced in the same manner as in Example 6, except that the AlN particles, TiN particles, and Mo particles were weighed out in a ratio of 36:29:35.

[0145] The thermal expansion coefficient and volume resistivity were measured by the following method. (Thermal Expansion Coefficient) A test piece measuring 3 mm x 3 mm x 15 mm was obtained from the obtained conductive ceramic plate. Using this test piece, the change in diameter length when the temperature was changed from 25 ° C to 800 ° C at a heating rate of 5 ° C / min was measured using a thermal expansion measuring device (TD5000SA, manufactured by NETZSCH), and the thermal expansion coefficient from 25 ° C to 800 ° C was calculated. Furthermore, the calculated thermal expansion coefficient was divided by the temperature change range (ΔT = 800 ° C - 25 ° C = 775 ° C) to measure the thermal expansion coefficient ( / K) at 800 ° C.

[0146] (Measurement of Volume Resistivity) A test piece of 3 mm x 4 mm x 40 mm was obtained from the obtained conductive ceramic substrate, and the volume resistivity (Ω cm) was measured using an electrical resistance measuring device (TER-2000RH model, manufactured by Advance Riko Co., Ltd.) by the four-terminal method in accordance with "JIS C 2525". The measurement conditions were as follows: Measurement temperature: room temperature (22°C) Measurement current: 2.0 A Distance between voltage terminals: 31 mm

[0147] The measurement results are shown in Table 1. In Table 1, "A:B" and "B1:B2" both indicate volume ratios.

[0148] Aluminum (Al), which is commonly used as a material for temperature control members, has a thermal expansion coefficient of 24 ppm / K and a volume resistivity of 2.7 × 10 -6 It was confirmed that all of the conductive ceramics of Examples 1 to 7 had a thermal expansion coefficient smaller than that of Al, and also had sufficient conductivity compared to Al.

[0149] From the above results, it was confirmed that the present invention is useful.

[0150] DESCRIPTION OF SYMBOLS 1A, 1B...Electrostatic chuck device 2...Electrostatic chuck member 2a...Placement surface 2b...Back surface 3...Base 3a...Support surface 3b...Lower surface 3f...Flow path 4, 6...Joint layer 5...Support plate 11...Dielectric substrate 13...Attraction electrode 16...Power supply terminal 17...Hole portion of base 17a...First hole 17b...Second hole 17c...Third hole 22...High frequency power supply 23...Insulator 23a...Upper end surface 61...Stress relaxation layer 62...First bonding layer 63...Second bonding layer

Claims

1. A temperature control component made of conductive ceramics, the component having a flow path for a heat transfer medium therein, the conductive ceramics being composed of a highly thermally conductive material and a conductive material, the volume ratio of the highly thermally conductive material to the conductive material being 10:90 to 90:10, and the conductive ceramics having a thermal expansion coefficient of 10×10 at 800°C. -6 / K or less.

2. The highly thermally conductive material is AlN, SiC, GaN, SiO 2 , Al 2 O 3 , SmAlO 3 , MgO, SiO 2 , Si 3 N 4 , Al(OH) 3 , MgO, Mg(OH) 2 , BN, ZnO, BeO, B 4 At least one selected from the group consisting of C, carbon, aluminum, copper, silver, and gold, and the conductive material is SiC, TiO 2 , TiN, TiC, W, WC, Mo, MoC, Mo 2 The temperature control member according to claim 1, which is at least one selected from the group consisting of C, TaC, TaN, NbC, VC and C.

3. The temperature control member according to claim 2, wherein said highly thermally conductive material is AlN and said electrically conductive material is TiN.

4. The temperature control member according to claim 2, wherein the highly thermally conductive material is AlN and the electrically conductive material is Mo.

5. The temperature control member of claim 2, wherein said highly thermally conductive material is AlN and said electrically conductive materials are TiN and Mo.

6. An electrostatic chuck device comprising: a temperature adjustment member according to any one of claims 1 to 5; and an electrostatic chuck member supported by the temperature adjustment member and having a dielectric substrate and an internal electrode.

Citation Information

Patent Citations

  • Electroconductive ceramics and their manufacturing method and member for semiconductor manufacturing device

    JP2007112705A

  • Ceramic sintered body, flow-channel member using the same, and semiconductor inspection device and semiconductor manufacturing apparatus

    JP2014131015A

  • Electrostatic chuck device

    JP2020053576A

  • Cooling plate, its manufacturing method, and components for semiconductor manufacturing equipment

    JP5666749B1

  • Electrostatic chuck device and method for manufacturing same

    WO2019189141A1