Metal separator and manufacturing method therefor
The metal separator plate, with a specific chromium and iron content and surface modification, achieves both excellent electrical conductivity and corrosion resistance, addressing the corrosion issues in hydrogen fuel cell systems.
Patent Information
- Application Number
- PCT/KR2023/012830
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-08-29
- Publication Date
- 2024-10-24
AI Technical Summary
The metal separator plate in hydrogen fuel cell systems faces challenges in achieving both excellent electrical conductivity and corrosion resistance, particularly in the manifold portion where exposed surfaces can lead to corrosion issues.
A metal separator plate design with a base material comprising 28-33% chromium, 0.01% carbon, 0.2% silicon, 0.3% manganese, and the remainder iron and impurities, featuring a surface modification layer with 20-28% chromium and 15-25% iron, heat-treated between 100°C to 300°C, and optionally laminated with a porous body for enhanced performance.
The solution provides a metal separator plate with improved electrical conductivity and corrosion resistance, as demonstrated by reduced contact resistance and current density, effectively addressing the corrosion concerns in the manifold portion.
Smart Images

Figure KR2023012830_24102024_PF_FP_ABST
Abstract
Description
Metal separator and manufacturing method thereof
[0001] This application relates to a metal separator and a method for manufacturing the same.
[0002] Recently, to combat global warming, powertrains are shifting from internal combustion engines (ICEs) to electric vehicles (EVs) and hydrogen fuel cell vehicles (FCEVs). Fuel cells used in FCEVs not only power industrial, household, and vehicular applications, but also power small electronic devices such as portable devices. Their applications are expanding as a highly efficient, clean energy source, contributing to both energy conservation and environmental protection.
[0003] A fuel cell is a type of power generation device that converts the chemical energy of fuel into electrical energy through an electrochemical reaction within a stack. It generates power by utilizing the energy generated by the combination reaction of hydrogen and oxygen. Specifically, a fuel cell can use hydrogen gas or a substance capable of producing hydrogen as fuel, and the oxidation reaction of the fuel produces hydrogen ions (protons) and electrons. These hydrogen ions and electrons then undergo an electrochemical reaction with oxygen in the air, producing water and generating electrical energy from the electron flow.
[0004] These hydrogen fuel cells are composed of a membrane electrode assembly, a gas diffusion layer (GDL), and a metal separator.
[0005] Among these components, the metal separator must separate hydrogen, oxygen, and coolant, and distribute and supply them evenly across the entire membrane electrode assembly to ensure smooth electrochemical reactions. Therefore, the required properties of the metal separator material include, in addition to low cost, excellent processability, excellent mechanical strength, high electrical conductivity, low gas permeability, thermal conductivity, and chemical stability.
[0006] The shape of the metal separator can be broadly divided into two parts: a reaction part formed in the center and a manifold part formed on each side of the reaction part.
[0007] The manifold section is equipped with inlets and outlets for supplying hydrogen and air, respectively, to enable electrochemical reactions, and also includes inlets and outlets for cooling water to control the stack's operating temperature. At this time, a manifold piercing process is performed to form the manifold section on the metal separator.
[0008] Meanwhile, the metal separator may undergo a manifold piercing process after surface modification to improve corrosion resistance and conductivity. However, this may result in an exposed portion of the manifold of the metal separator, potentially compromising corrosion resistance.
[0009] Therefore, to solve these problems, a metal separator having excellent electrical conductivity as well as corrosion resistance and a method for manufacturing the same are required.
[0010] The object of the present application is to provide a metal separator having excellent electrical conductivity as well as excellent corrosion resistance and a method for manufacturing the same.
[0011] In order to solve the above problem, the metal separator of the present application includes a first base material including a first manifold part, a second manifold part, and a reaction part provided between the first manifold part and the second manifold part, wherein the first manifold part and the second manifold part each have a plurality of openings and a surface part existing between the plurality of openings, and a surface modification layer is formed on the upper surface of the surface part and the inner surface of the openings, respectively.
[0012] The above first base material may contain 28,000 to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, the remainder being iron and other unavoidable impurities.
[0013] In addition, the surface modification layer formed on the upper surface of the surface portion may include 20 at% to 28 at% of chromium in a region from the externally exposed surface to a depth of 1.0 nm, and may include 15 at% to 25 at% of iron in a region from the externally exposed surface to a depth of 1.0 nm.
[0014] In addition, the surface modification layer formed on the upper surface of the surface portion and the inner surface of the opening may be heat-treated at 100°C to 300°C for 10 to 300 seconds.
[0015] In addition, the first parent material has a contact resistance of 14 mΩ·cm under a contact pressure of 1.0 MPa. 2 Below, 0.6 V vs SCE At a potential of , the current density is 4 ㎂ / cm 2 It could be as follows:
[0016] Additionally, the metal separator may further include a porous body laminated on the upper surface of the reaction section.
[0017] Additionally, the fuel cell of the present application includes the metal separator.
[0018] In addition, the method for manufacturing a metal separator of the present application includes a preparation step of preparing a first base material; a manifold piercing step of forming a first manifold part and a second manifold part, respectively, by piercing both side surfaces of one side of the first base material to form a plurality of openings and a surface part existing between the plurality of openings; a surface modification layer forming step of forming a surface modification layer on the exposed surface of the first base material by modifying an externally exposed surface of the first base material on which the first manifold part and the second manifold part are formed; and a heat treatment step of heat treating the first base material on which the surface modification layer is formed, wherein the surface modification layer is formed on the upper surface of the surface part and the inner surface of the opening part provided in each of the first manifold part and the second manifold part.
[0019] Additionally, the first base material may contain 28,000 to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, the remainder being iron and other unavoidable impurities.
[0020] In addition, the surface modification layer forming step may include a first modification step of preparing a solution in which at least one selected from fluorine, hydrochloric acid, and phosphoric acid is added to a sulfuric acid solution, and immersing the surface of the first base material in the solution; and a second modification step of immersing the first base material that has undergone the first modification step in a solution containing hydrogen peroxide and fluorine.
[0021] Additionally, the heat treatment step can be performed at 100°C to 300°C for 10 seconds to 300 seconds.
[0022] In addition, the method for manufacturing the metal separator may further include a porous body piercing step of preparing a second base material in the preparation step and forming a porous body having a plurality of holes by punching the prepared second base material.
[0023] In addition, the method for manufacturing the metal separator may further include a laminate forming step of forming a laminate by laminating and bonding the porous body to the center of the first base material after performing the heat treatment step and the porous body piercing step.
[0024] In addition, the surface modification layer forming step may further include forming a surface modification layer on the exposed surface of the second base material or porous body by modifying the externally exposed surface of the second base material or porous body before or after the porous body piercing step, and the heat treatment step may further include heat treating the second base material or porous body on which the surface modification layer is formed.
[0025] In addition, the method for manufacturing the metal separator may further include a slitting step of slitting the widths of the first and second base materials, respectively, before performing the manifold piercing step and the porous body piercing step.
[0026] According to the metal separator of the present application and its manufacturing method, not only can it have excellent electrical conductivity, but also excellent corrosion resistance.
[0027] FIG. 1 is a top view illustrating an example of a metal separator according to one embodiment of the present application.
[0028] FIG. 2 is a side view showing an example of a manifold formed on a first base material of a metal separator according to one embodiment of the present application, cut in the width direction.
[0029] FIG. 3 is a top view illustrating a metal separator according to another embodiment of the present application.
[0030] Hereinafter, the metal separator of the present application will be described with reference to the attached drawings. The attached drawings are exemplary, and the metal separator of the present application is not limited to the attached drawings.
[0031] FIG. 1 is a top view illustrating a metal separator according to one embodiment of the present application. As illustrated in FIG. 1, the metal separator of the present application includes a first base material (1100). The metal separator of the present application not only exhibits excellent electrical conductivity but also exhibits excellent corrosion resistance.
[0032] The above first parent material (1100) is a material used for a metal separator for a fuel cell, and includes a first manifold part (1110), a second manifold part (1120), and a reaction part (1130) provided between the first manifold part (1110) and the second manifold part (1120).
[0033] FIG. 2 is a side view exemplarily showing a manifold formed on a first base material of a metal separator according to one embodiment of the present application, cut in the width direction. As shown in FIGS. 1 and 2, the first manifold (1110) and the second manifold (1120) are each parts that supply hydrogen and air to the first base material (1100) so that an electrochemical reaction can occur in the separator, and each has a plurality of openings (1101) and a surface portion (1102) existing between the plurality of openings (1101), and a surface modification layer (1103, 1104) is formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) provided in each of the first manifold (1110) and the second manifold (1120). Specifically, the first manifold part (1110) and the second manifold part (1120) may be formed with hydrogen and air inlets and outlets for supplying and discharging hydrogen and air, respectively, and may be formed with cooling water inlets and outlets for controlling the operating temperature, and may be provided with respective surface parts (1102) between each inlet and outlet. In one embodiment, the first manifold part (1110) may be formed at one end with respect to the longitudinal direction of the first base material (1100), and a hydrogen inlet, a cooling water outlet, and an air outlet may be formed along a width direction perpendicular to the longitudinal direction of the first base material (1100), and each surface part (1102) may be present between the hydrogen inlet, the cooling water outlet, and the air outlet. In addition, the second manifold portion (1120) is formed at the other end with respect to the longitudinal direction of the first base material (1100), and an air inlet, a coolant inlet, and a hydrogen outlet may be formed along a width direction perpendicular to the longitudinal direction of the first base material (1100), and a surface portion (1102) may be present between each of the air inlet, coolant inlet, and hydrogen outlet.At this time, since the number of the above-mentioned openings is not particularly limited as long as it is two or more, the upper limit is not particularly limited. In this specification, the term "manifold section" is used to refer to both the first manifold section and the second manifold section. In addition, the longitudinal direction refers to the direction from one end to the other end of the first base material (1100). In addition, the width direction refers to the direction perpendicular to the longitudinal direction.
[0034] In one example, the first base material (1100) may include 28,000 wt% to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, the remainder iron, and other unavoidable impurities. In one embodiment, the first base material (1100) may include about 28,000 wt% to about 33,000 wt% of chromium, about 0.010 wt% or less of carbon, about 0.200 wt% or less of silicon, about 0.300 wt% or less of manganese, about 0.300 wt% or less of titanium, the remainder iron, and other unavoidable impurities. Specifically, the first base material (1100) may have an upper limit of a chromium content of about 32,000 wt% or less or about 31,000 wt% or less, and a lower limit of a chromium content of about 29,000 wt% or more. In addition, the first base material (1100) may have a lower limit of a carbon content of about 0.001 wt% or more, a lower limit of a silicon content of about 0.100 wt% or more, a lower limit of a manganese content of about 0.100 wt% or more, and a lower limit of a titanium content of about 0.100 wt% or more. By including the above-described components, the first base material (1100) may have excellent electrical conductivity as well as excellent corrosion resistance. At this time, since the physical properties of each component included in the first base material (1100) are known in the art, they will be omitted.
[0035] In addition, the first base material (1100) may further include at least one selected from among 0.030 wt% or less of phosphorus, 0.002 wt% or less of sulfur, and 0.300 wt% or less of niobium. The first base material (1100) may further include at least one selected from among about 0.030 wt% or less of phosphorus, about 0.002 wt% or less of sulfur, and about 0.300 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.
[0036] In one example, the surface modification layer (1103) formed on the upper surface of the surface portion (1102) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may contain chromium in an amount of 20 at% to 28 at% in a region from the externally exposed surface to a depth of 1.0 nm, and in one embodiment, may contain about 20 at% to about 28 at%, and specifically, may contain about 22 at% to about 27 at% or about 24 at% to about 26 at%. The surface modification layer (1103) formed on the upper surface of the surface portion (1102) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may contain chromium in the aforementioned amount in a region from the externally exposed surface to a depth of 1.0 nm, thereby not only having excellent electrical conductivity but also having excellent corrosion resistance. At this time, the chromium content of the surface modification layer (1103) can be measured using EDAX equipment.
[0037] In another example, the surface modification layer (1103) formed on the upper surface of the surface portion (1102) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may contain iron in an amount of 15 at% to 25 at% in a region from the externally exposed surface to a depth of 1.0 nm, and in one embodiment, may contain iron in an amount of about 15 at% to about 25 at%, and specifically, may contain iron in an amount of about 17 at% to about 23 at% or about 19 at% to about 21 at%. The surface modification layer (1103) formed on the upper surface of the surface portion (1102) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may have excellent electrical conductivity as well as excellent corrosion resistance by including iron in the aforementioned amount in a region from the externally exposed surface to a depth of 1.0 nm. At this time, the iron content of the surface modification layer (1103) may be measured using an EDAX device.
[0038] The surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may have a thickness of 5 nm or less. Specifically, the thickness of the surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may be about 4 nm or less or about 3 nm or less. In addition, the lower limit of the thickness of the surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may be about 1 nm or more. Since the surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) has the aforementioned thickness, not only can the electrical conductivity be excellent, but also the corrosion resistance can be excellent.
[0039] In addition, the surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may be heat-treated at 100°C to 300°C for 10 to 300 seconds. In one embodiment, the surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may be heat-treated at about 100°C to about 300°C for about 10 to about 300 seconds. Specifically, the surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) provided in each of the first manifold portion (1110) and the second manifold portion (1120) may be heat-treated at about 120°C to about 260°C, about 140°C to about 220°C, or about 160°C to about 180°C for about 30 seconds to about 250 seconds, about 50 seconds to about 200 seconds, about 70 seconds to about 150 seconds, or about 90 seconds to about 100 seconds. The surface modification layer (1103) formed on the upper surface of the surface portion (1102) and the inner surface of the opening portion (1101) of each of the first manifold portion (1110) and the second manifold portion (1120) can have improved corrosion resistance by being heat treated under the conditions described above.
[0040] The above reaction unit (1130) is a unit where an electrochemical reaction occurs by hydrogen and air supplied and discharged through the first manifold unit (1110) and the second manifold unit (1120), respectively.
[0041] For example, a flow path (not shown) may be formed on the upper surface of the reaction unit (1130), and a porous body (not shown) described later may be laminated thereon. The method for forming the flow path on the upper surface of the reaction unit (1130) is not particularly limited, as a method known in the art may be used. In addition, the reaction unit (1130) may have a flat plate shape when a porous body is laminated thereon. By laminating the porous body (1200) on the flat plate-shaped reaction unit (1130), a separate flow path forming process may not be required.
[0042] In one example, the thickness of the first base material (1100) may be from 0.05 mm to 1 mm, and in one embodiment, from about 0.05 mm to about 1 mm. By having a thickness within the aforementioned range, the first base material (110) can achieve excellent mechanical strength and gas permeability.
[0043] In another example, the first parent material (1100) has a contact resistance of 14 mΩ·cm under a contact pressure of 1.0 MPa. 2 It may be as follows. In one embodiment, the first parent material (1100) has a contact resistance of about 14 mΩ·cm under a contact pressure of 1.0 MPa. 2 It may be as follows. The first base material (1100) may have excellent electrical conductivity since the contact resistance measured under the above-mentioned contact pressure has the above-mentioned range. In addition, the lower limit is not particularly limited in terms of the contact resistance of the first base material (1100) measured under the above-mentioned contact pressure being lower, the better the electrical conductivity, but for example, it may be about 1 mΩ·cm. 2 It can be ideal, specifically, about 3 mΩ·cm 2 Above, about 5 mΩ·cm 2 Above, about 10 mΩ·cm 2 Ideal or about 12 mΩ·cm 2 It could be strange.
[0044] Also, in one example, the first parent material (1100) is 0.6 V vs SCE At a potential of , the current density is 4 ㎂ / cm 2 may be less than or equal to 0.6 V. In one embodiment, the first parent material (1100) is 0.6 V. vs SCE At a potential of , the current density is about 4 ㎂ / cm 2 It may be below. The first base material (1100) may have excellent corrosion resistance since the current density measured at the above-mentioned potential has the above-mentioned range. In addition, the lower limit of the current density of the first base material (1100) measured at the above-mentioned potential is not particularly limited in that the lower the current density, the better the electrical conductivity, but, for example, about 1 ㎂ / cm 2 It can be ideal, specifically, about 3 ㎂ / cm 2 It could be strange.
[0045] Fig. 3 is a top view exemplarily showing a metal separator according to another embodiment of the present application. As shown in Fig. 3, the metal separator further includes a porous body (1200) laminated on the upper surface of the first base material (1100), specifically, the upper surface of the reaction unit (1130), and the porous body (1200) may include a plurality of holes (not shown) and a surface portion (not shown) formed between the plurality of holes. In this case, the number of holes is not particularly limited as long as it is two or more, and thus the upper limit is not particularly limited.
[0046] The porous body (1200) above is a channel in which the aforementioned electrochemical reaction occurs and has a microporous structure. At this time, the porous body (1200) may have an area corresponding to the reaction section (1130) of the first base material (1100). In this specification, the term "corresponding area" means the same area. The porous body (1200) may be laminated on the upper surface of the reaction section (1130) of the first base material (1100), thereby enhancing the function of a hydrogen or air channel.
[0047] In one example, a surface modification layer or a passive film may be formed on the upper surface of the surface portion and the inner surface of the hole provided in the porous body (1200), respectively. When a surface modification layer is formed on the upper surface of the surface portion and / or the inner surface of the hole provided in the porous body (1200), excellent corrosion resistance and electrical conductivity of the porous body can be secured. In addition, when a passive film is formed on the upper surface of the surface portion and / or the inner surface of the hole provided in the porous body (1200), oxygen can be blocked from penetrating into the interior of the porous body (1200), thereby preventing rust from occurring.
[0048] The porous body (1200) may include 28,000 wt% to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, the remainder iron, and other unavoidable impurities. In one embodiment, the porous body (1200) may include about 28,000 wt% to about 33,000 wt% of chromium, about 0.010 wt% or less of carbon, about 0.200 wt% or less of silicon, about 0.300 wt% or less of manganese, about 0.300 wt% or less of titanium, the remainder iron, and other unavoidable impurities. Specifically, the porous body (1200) may have an upper limit of a chromium content of about 32,000 wt% or less or about 31,000 wt% or less, and a lower limit of a chromium content of about 29,000 wt% or more. In addition, the porous body (1200) may have a lower limit of a carbon content of about 0.001 wt% or more, a lower limit of a silicon content of about 0.100 wt% or more, a lower limit of a manganese content of about 0.100 wt% or more, and a lower limit of a titanium content of about 0.100 wt% or more. Since the porous body (1200) is made of stainless steel containing chromium having the aforementioned content, when the surface is exposed to the outside, a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm, in one embodiment, about 1 nm to about 5 nm, can be naturally formed on the surface, and when the passive film is modified, a surface modification layer can be formed. At this time, since the physical properties of each component included in the porous body (1200) are known in the art, they will be omitted.
[0049] In one example, the porous body (1200) may further include at least one selected from 0.030 wt% or less of phosphorus, 0.002 wt% or less of sulfur, and 0.300 wt% or less of niobium. The porous body (1200) may further include at least one selected from about 0.030 wt% or less of phosphorus, about 0.002 wt% or less of sulfur, and about 0.300 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.
[0050] The plurality of holes may have a short axis length formed in a direction parallel to the air flow direction and a long axis length formed in a direction perpendicular to the air flow direction. For example, the short axis length may have a length of 0.3 mm to 1.0 mm, and in one embodiment, about 0.3 mm to 1.0 mm. The plurality of holes may enhance the function of a hydrogen or air flow path by each having the aforementioned length.
[0051] The present application also relates to a fuel cell. The fuel cell relates to a fuel cell including the aforementioned metal separator. Since the specific details of the metal separator described below are equally applicable to the description of the metal separator, they will be omitted.
[0052] The fuel cell cell includes the aforementioned metal separator. By including the aforementioned metal separator, the fuel cell can perform a smooth electrochemical reaction of the membrane electrode assembly and can smoothly function as an electrical path.
[0053] The fuel cell may include two of the aforementioned metal separators, and a first gas diffusion layer, a membrane electrode assembly, and a second gas diffusion layer may be provided between the two metal separators. At this time, the first gas diffusion layer, the membrane electrode assembly, and the second gas diffusion layer may be any type known in the art without limitation, and are not particularly limited.
[0054] The present application also relates to a method for manufacturing a metal separator. The method for manufacturing the metal separator relates to a method for manufacturing the aforementioned metal separator. Since the specific details of the metal separator described below are equally applicable to the metal separator described above, they will be omitted.
[0055] The method for manufacturing a metal separator of the present application comprises a preparation step, a manifold piercing step, a surface modification layer formation step, and a heat treatment step. According to the method for manufacturing a metal separator of the present application, a metal separator having excellent electrical conductivity and corrosion resistance can be manufactured.
[0056] The above preparation step is the step of preparing the first parent material.
[0057] For example, the first base material may include 28,000 wt% to 33,000 wt% chromium, 0.010 wt% or less carbon, 0.200 wt% or less silicon, 0.300 wt% or less manganese, 0.300 wt% or less titanium, the remainder iron, and other unavoidable impurities. In one embodiment, the first base material may include about 28,000 wt% to about 33,000 wt% chromium, about 0.010 wt% or less carbon, about 0.200 wt% or less silicon, about 0.300 wt% or less manganese, about 0.300 wt% or less titanium, the remainder iron, and other unavoidable impurities. Specifically, the first base material may have an upper limit of a chromium content of about 32,000 wt% or less or about 31,000 wt% or less, and a lower limit of a chromium content of about 29,000 wt% or more. In addition, the first base material may have a lower limit of a carbon content of about 0.001 wt% or more, a lower limit of a silicon content of about 0.100 wt% or more, a lower limit of a manganese content of about 0.100 wt% or more, and a lower limit of a titanium content of about 0.100 wt% or more. By including the above-described components, a naturally very thin Cr2O3 passive film having a thickness of about 1 nm to about 5 nm, in one embodiment, about 1 nm to about 5 nm, may be formed on the surface.
[0058] In addition, the first base material may further include at least one selected from 0.030 wt% or less of phosphorus, 0.002 wt% or less of sulfur, and 0.300 wt% or less of niobium. In one embodiment, the first base material may further include at least one selected from about 0.030 wt% or less of phosphorus, about 0.002 wt% or less of sulfur, and about 0.300 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.
[0059] In one example, the method for manufacturing the metal separator may further include a cold rolling step. Specifically, the cold rolling step may be a step of forming the first base material prepared in the preparation step and the second base material described below by passing them between two rolls that rotate at a temperature lower than the recrystallization temperature, and may be performed in the preparation step. By further including the cold rolling step, the method for manufacturing the metal separator may improve the dimensional accuracy and mechanical properties of the first base material and the second base material described below. At this time, when performing each step in the method for manufacturing the metal separator, if the first base material and / or the second base material are exposed to the outside, a passive film may be formed on the surface of each of the first base material and / or the second base material by natural oxidation. Specifically, since each of the first and second base materials is made of stainless steel containing chromium having the aforementioned content, a naturally very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm, in one embodiment, about 1 nm to about 5 nm, can be formed.
[0060] The above manifold piercing step is a step of forming a first manifold and a second manifold, each having a plurality of openings in the first base material and a surface portion between the plurality of openings, by piercing both side surfaces of one side of the first base material. At this time, when performing each step in the method for manufacturing the metal separator, if the first base material and / or the second base material are exposed to the outside, a passive film may be formed on the surface of each of the first base material and / or the second base material by natural oxidation.
[0061] The above surface modification layer forming step is a step of forming a surface modification layer on the exposed surface of the first base material that has undergone the manifold piercing step, and is performed by modifying the externally exposed surface of the first base material on which the first manifold part and the second manifold part are formed, specifically, the passive film formed on the surface of the first base material, and a surface modification layer is formed on each of the upper surface of the surface part and the inner surface of the opening.
[0062] The method for manufacturing the above metal separator can manufacture a metal separator having excellent electrical conductivity as well as corrosion resistance by performing the surface modification layer forming step after the manifold piercing step even if the first base material includes the above-described components.
[0063] In one example, the surface modification layer forming step may include a first modification step and a second modification step.
[0064] The first modification step is a step of removing a passive film formed on the surface of the first base material and reconstituting chemical components, and can be performed by preparing a solution in which at least one selected from fluorine, hydrochloric acid, and phosphoric acid is added to a sulfuric acid solution, and immersing the surface of the first base material in the solution. Specifically, the first modification step can be performed by preparing a solution in which at least one selected from 1.0 mol to 5.0 mol of fluorine, 0.3 mol to 1.0 mol of hydrochloric acid, and 0.3 mol to 1.0 mol of phosphoric acid is added to a sulfuric acid solution having a concentration of 350 g / L or more, and immersing the surface of the first base material, specifically, the passive film formed on the surface of the first base material, in the solution at 40°C to 80°C for 10 seconds to 180 seconds. In one embodiment, the first modification step may be performed by preparing a solution in which at least one selected from about 1.0 mol to about 5.0 mol of fluorine, about 0.3 mol to about 1.0 mol of hydrochloric acid, and about 0.3 mol to about 1.0 mol of phosphoric acid is added to a sulfuric acid solution having a concentration of about 350 g / L or more, and immersing the surface of the first base material, specifically, the passive film formed on the surface of the first base material, in the solution at about 40° C. to about 80° C. for about 10 seconds to about 180 seconds. The method for manufacturing a metal separator may include the first modification step, thereby improving the amount of chromium hydroxide produced in the surface modification layer, thereby improving corrosion resistance and electrical conductivity of the metal separator. At this time, the ratio of the components included in the surface modification layer may be adjusted depending on the ratio of the components of the solution used in the first modification step and the immersion conditions.
[0065] The second modification step is a step for removing SMUT, which is a by-product that may be generated through the first modification step, and may be performed continuously after the first modification step, and may be performed by immersing the first base material that has undergone the first modification step in a solution containing hydrogen peroxide and fluorine. Specifically, the second modification step may be performed by immersing the first base material that has undergone the first modification step in a solution containing 1.0 mol to 5.0 mol of hydrogen peroxide and 1.0 mol to 5.0 mol of fluorine at 40°C to 80°C for 10 seconds to 180 seconds. In one embodiment, the second modification step may be performed by immersing the first base material subjected to the first modification step in a solution containing about 1.0 mol to about 5.0 mol of hydrogen peroxide and about 1.0 mol to about 5.0 mol of fluorine at about 40° C. to about 80° C. for about 10 seconds to about 180 seconds. The surface modification layer forming step may include the second modification step, thereby ensuring the cleanliness of the surface of the surface modification layer.
[0066] The above heat treatment step is a step of strengthening the surface modification layer formed on the first base material, and is performed by heat treating the first base material on which the surface modification layer is formed through the surface modification layer forming step. For example, the heat treatment step may be performed at 100°C to 300°C for 10 seconds to 300 seconds. In one embodiment, the heat treatment step may be performed at about 100°C to about 300°C for about 10 seconds to about 300 seconds. The method for manufacturing a metal separator includes the heat treatment step, thereby inducing a dehydration phenomenon to change iron hydroxide included in the surface modification layer into iron oxide, and thereby manufacturing a metal separator with improved corrosion resistance.
[0067] In one example, the method for manufacturing the metal separator may further include preparing a second base material in the preparation step, and may further include a porous body piercing step for the prepared second base material.
[0068] The second base material prepared in the above preparation step may include 28,000 wt% to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, the remainder iron, and other unavoidable impurities. In one embodiment, the second base material may include about 28,000 wt% to about 33,000 wt% of chromium, about 0.010 wt% or less of carbon, about 0.200 wt% or less of silicon, about 0.300 wt% or less of manganese, about 0.300 wt% or less of titanium, the remainder iron, and other unavoidable impurities. Specifically, the second base material may have an upper limit of a chromium content of about 32,000 wt% or less or about 31,000 wt% or less, and a lower limit of a chromium content of about 29,000 wt% or more. In addition, the second base material may have a lower limit of a carbon content of about 0.001 wt% or more, a lower limit of a silicon content of about 0.100 wt% or more, a lower limit of a manganese content of about 0.100 wt% or more, and a lower limit of a titanium content of about 0.100 wt% or more. By including the above-described components, a naturally very thin Cr2O3 passive film having a thickness of about 1 nm to about 5 nm, in one embodiment, about 1 nm to about 5 nm, may be formed on the surface. Additionally, the second base material may further include at least one selected from 0.030 wt% or less of phosphorus, 0.002 wt% or less of sulfur, and 0.300 wt% or less of niobium. In one embodiment, the second base material may further include at least one selected from about 0.030 wt% or less of phosphorus, about 0.002 wt% or less of sulfur, and about 0.300 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.
[0069] The above porous body piercing step is a step of forming a second base material on which the surface modification layer is not formed into a porous body having a plurality of holes before performing the surface modification layer forming step, and can be performed by punching the second base material on which the surface modification layer is not formed. The method for manufacturing the metal separator can improve the function of a hydrogen or air passage by including the porous body piercing step.
[0070] In one example, the method for manufacturing the metal separator may further include a three-dimensional forming step. The three-dimensional forming step is a step for forming an air passage in the porous body, and may be performed by pressing the porous body that has undergone the porous body piercing step. By further including the three-dimensional forming step, the method for manufacturing the metal separator may secure a three-dimensional air passage in the porous body that has undergone the three-dimensional forming step.
[0071] In another example, the method for manufacturing the metal separator may further include a laminate forming step. The laminate forming step is a step of forming a laminate by laminating a porous body on the first base material, and may be performed by, after performing the heat treatment step and the porous body piercing step, laminating the porous body on the center of the first base material including the first and second manifold parts having the surface part and the openings described above, and bonding them. For example, the bonding method may use a bonding method using laser welding or micro spot welding. The method for manufacturing the metal separator may include the laminate forming step, thereby manufacturing a two-layer metal separator in which a porous body is laminated on the first base material including the first and second manifold parts having the surface part and the openings described above.
[0072] In one example, the surface modification layer forming step may further include modifying an externally exposed surface of the second base material or porous body before or after the porous body piercing step to form a surface modification layer on the exposed surface of the second base material or porous body, and the heat treatment step may further include heat treating the second base material or porous body on which the surface modification layer is formed. Specifically, the surface modification layer forming step for the second base material may be performed before the porous body piercing step, and after the surface-modified second base material undergoes the porous body piercing step, a surface modification layer may be formed on an upper surface of a surface portion provided in each, and a passive film may be formed on an inner surface of the hole. In addition, the surface modification layer forming step for the porous body may be performed after the porous body piercing step, and after the porous body undergoes the surface modification layer forming step, a surface modification layer may be formed on an upper surface of a surface portion provided in each, and an inner surface of the hole.
[0073] In another example, the method for manufacturing the metal separator may further include a slitting step. Specifically, the slitting step is a step of slitting each of the first and second base materials, on which no surface modification layer is formed, to a width suitable for application to the metal separator before performing the manifold piercing step and the porous body piercing step. For example, the width of each of the first and second base materials, on which no surface modification layer is formed, may be divided into 1 / 4 through the slitting step.
[0074]
[0075] Hereinafter, the present application will be described in more detail through examples according to the present application and comparative examples not according to the present application, but the scope of the present application is not limited by the examples presented below.
[0076]
[0077] Example 1
[0078] Manufacturing of metal separators
[0079] A first base material having a thickness of 0.1 mm and a second base material having a thickness of 0.08 mm, each composed of 30,000 wt% chromium, 0.006 wt% carbon, 0.144 wt% silicon, 0.200 wt% manganese, 0.016 wt% phosphorus, 0.001 wt% sulfur, 0.200 wt% titanium, 0.200 wt% niobium, the remainder iron, and other unavoidable impurities, were prepared, and cold rolling was performed by passing each of the first base material and the second base material between two rotating rolls. At this time, the surfaces of the first base material and the second base material were naturally formed with a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm by natural oxidation.
[0080] Afterwards, each of the first and second parent materials was slit into 1 / 4 pieces with a width of 500 nm to have a width of 120 mm.
[0081] Thereafter, after piercing the second base material, a porous body was formed by three-dimensional molding using a press, which had a plurality of holes and a surface layer existing between the plurality of holes. At this time, during the three-dimensional molding, the unnecessary outer portion of the porous body was removed.
[0082] Thereafter, the first manifold part and the second manifold part were formed by perforating both sides of one surface of the first base material from the first base material, respectively, to include a plurality of openings and a surface part existing between the plurality of openings.
[0083] Afterwards, a solution containing 3.0 mol of fluorine in a sulfuric acid solution having a concentration of 400 g / L was prepared, and the surfaces of each of the first base material and the porous body were immersed in the solution at a temperature of 60°C for 30 seconds for a first modification treatment, and then a second modification treatment was performed successively to immerse the surfaces of each of the first base material and the porous body in a solution containing 3.5 mol of hydrogen peroxide and 2.5 mol of fluorine at a temperature of 60°C for 60 seconds to form a surface modification layer on the surfaces of each of the first base material and the porous body, thereby forming a surface modification layer of 2 nm thickness on each of the upper surface of the surface portion and the inner surface of the opening or hole.
[0084] Thereafter, each of the first parent material and the porous body on which the surface modification layer was formed was heat-treated at 160°C for 90 seconds.
[0085] Afterwards, the porous body was laminated on the center of the heat-treated first base material, and laser bonding was performed to manufacture a metal separator in which the porous body was laminated on the first base material.
[0086]
[0087] Comparative Example 1
[0088] Manufacturing of metal separators
[0089] A first base material having a thickness of 0.1 mm and a second base material having a thickness of 0.08 mm, each composed of 30,000 wt% chromium, 0.006 wt% carbon, 0.144 wt% silicon, 0.200 wt% manganese, 0.016 wt% phosphorus, 0.001 wt% sulfur, 0.200 wt% titanium, 0.200 wt% niobium, the remainder iron, and other unavoidable impurities, were prepared, and cold rolling was performed by passing each of the first base material and the second base material between two rotating rolls. At this time, the surfaces of each of the first base material and the second base material were naturally formed with a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm by natural oxidation.
[0090] Afterwards, a solution containing 3.0 mol of fluorine in a sulfuric acid solution having a concentration of 400 g / L was prepared, and the surfaces of each of the first and second base materials were immersed in the solution at a temperature of 60°C for 30 seconds for a first modification treatment, and then a second modification treatment was performed successively by immersing the surfaces in a solution containing 3.5 mol of hydrogen peroxide and 2.5 mol of fluorine at a temperature of 60°C for 60 seconds to form a surface modification layer having a thickness of 2 nm on the surfaces of each of the first and second base materials.
[0091] Thereafter, each of the first and second base materials on which the surface modification layer was formed was heat-treated at 160°C for 90 seconds.
[0092] Afterwards, the heat-treated first and second base materials were each slit into 1 / 4 pieces from 500 mm to have a width of 120 mm.
[0093] Afterwards, the heat-treated second base material was pierced and then three-dimensionally molded using a press to form a porous body having multiple holes. At this time, during the three-dimensional molding, the unnecessary outer portion of the porous body was removed.
[0094] Thereafter, in the heat-treated first base material, both sides of one surface of the first base material were perforated to form a first manifold part and a second manifold part, each including a plurality of openings and a surface part formed between the plurality of openings. At this time, a surface modification layer was formed on the upper surface of the surface part formed in each of the first manifold part and the second manifold part, and no surface modification layer was formed on the inner surface of the opening, and a very thin Cr2O3 passivation film with a thickness of 1 nm to 5 nm was naturally formed.
[0095] Thereafter, the porous body was laminated on the center of the first base material, and laser bonding was performed to manufacture a metal separator in which the porous body was laminated on the first base material.
[0096]
[0097] Comparative Example 2
[0098] Manufacturing of metal separators
[0099] A metal separator was manufactured in the same manner as in Example 1, except that the first modification treatment, the second modification treatment, and the heat treatment were not performed. At this time, the manufactured metal separator had a naturally very thin Cr2O3 passivation film of 1 nm to 5 nm thickness formed on the upper surface of the surface portion of the first and second manifold portions and the inner surface of the opening portion, respectively.
[0100]
[0101] Comparative Example 3
[0102] Manufacturing of metal separators
[0103] A metal separator was manufactured in the same manner as in Example 1, except that heat treatment was not performed.
[0104]
[0105] Experimental Example 1. Evaluation of the components of the surface modification layer and passive film.
[0106] Using energy dispersive spectroscopy (EDS), the components in the region from the externally exposed surface of the surface modification layer or passive film formed on the upper surface of the surface of the first base material of the metal separator manufactured in the above examples and comparative examples to a depth of 1.0 nm were analyzed with an EDAX device, and the results are shown in Table 1 below.
[0107]
[0108] Experimental Example 2. Contact Resistance Evaluation
[0109] After inserting the metal separator manufactured in the examples and comparative examples between gas diffusion layers (Carbon paper type, SGL), the contact resistance of the first manifold part of the metal separator manufactured in the examples and comparative examples was measured using a method of measuring current under a contact pressure of 1.0 MPa, and the results are shown in Table 1 below.
[0110]
[0111] Experimental Example 3. Current Density Evaluation
[0112] The current density for the first manifold and the second manifold of the metal separator manufactured in the examples and comparative examples was evaluated using the Tafel Slop of a potentiostat, and the dynamic potential was evaluated in a mixture of 0.1 N sulfuric acid and 2 ppm hydrofluoric acid heated to 80°C, and 0.6 V SCE The voltage was measured when applied, and the results are shown in Table 1 below.
[0113] Analysis of the components of the surface modification layer or passive film formed on the upper surface of the surface part provided in the manifold part. Contact resistance (mΩ·cm) with or without the surface modification layer 2 )Current density (㎂ / cm 2 )Chrome (at%)Iron (at%)The surface of the upper surface of the manifold sectionThe inner surface of the opening section of the manifold section Example 12520OO133Comparative Example 11520OX205Comparative Example 2305XX4806Comparative Example 32520OO1312
[0114] As shown in Table 1 above, the metal separator manufactured in Example 1 had lower contact resistance and current density than the metal separators manufactured in Comparative Examples 1 and 2, and thus it was confirmed that the electrical conductivity and corrosion resistance were excellent.
[0115] In addition, the metal separator manufactured in Example 1 had a similar contact resistance to the metal separator manufactured in Comparative Example 3 and thus had similar electrical conductivity, but had a relatively low current density, so it was confirmed that the corrosion resistance of the manifold part was excellent.
[0116] <Explanation of symbols>
[0117] 1100: First Mother Material
[0118] 1110: 1st manifold section
[0119] 1120: Second manifold section
[0120] 1130: Reaction section
[0121] 1101: Opening
[0122] 1102: Surface
[0123] 1103: Surface modification layer formed on the upper surface of the surface
[0124] 1104: Surface modification layer formed on the inner surface of the opening
[0125] 1200: Porous body
Claims
1. A first base material comprising a first manifold section, a second manifold section, and a reaction section provided between the first manifold section and the second manifold section, The first manifold portion and the second manifold portion each have a plurality of openings and a surface portion existing between the plurality of openings, A metal separator having a surface modification layer formed on the upper surface of the surface portion and the inner surface of the opening portion.
2. In paragraph 1, The above first base material is a metal separator containing 28,000 to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, and the remainder being iron and other unavoidable impurities.
3. In paragraph 1, A metal separator, wherein the surface modification layer formed on the upper surface of the surface layer contains 20 at% to 28 at% of chromium in a region from the externally exposed surface to a depth of 1.0 nm, and contains 15 at% to 25 at% of iron in a region from the externally exposed surface to a depth of 1.0 nm.
4. In paragraph 1, A metal separator, wherein the surface modification layer formed on the upper surface of the surface portion and the inner surface of the opening is heat-treated at 100°C to 300°C for 10 to 300 seconds.
5. In paragraph 1, The above first parent material has a contact resistance of 14 mΩ·cm under a contact pressure of 1.0 MPa. 2 Below, 0.6 V vs SCE At a potential of , the current density is 4 ㎂ / cm 2 Below is the metal separator.
6. In paragraph 1, A metal separator further comprising a porous body laminated on the upper surface of the above reaction section.
7. A fuel cell cell comprising a metal separator according to any one of claims 1 to 6.
8. Preparatory stage for preparing the first parent material; A manifold piercing step of forming a first manifold and a second manifold, each having a plurality of openings and a surface layer existing between the plurality of openings by piercing both sides of one surface of the first base material in the first base material; A surface modification layer forming step of modifying the externally exposed surface of the first base material on which the first manifold portion and the second manifold portion are formed to form a surface modification layer on the exposed surface of the first base material; and It includes a heat treatment step of heat treating the first base material on which the surface modification layer is formed, A method for manufacturing a metal separator, wherein a surface modification layer is formed on the upper surface of the surface portion and the inner surface of the opening portion provided in each of the first manifold portion and the second manifold portion.
9. In paragraph 8, A method for manufacturing a metal separator, wherein the first base material comprises 28,000 to 33,000 wt% of chromium, 0.010 wt% or less of carbon, 0.200 wt% or less of silicon, 0.300 wt% or less of manganese, 0.300 wt% or less of titanium, and the remainder being iron and other unavoidable impurities.
10. In paragraph 8, The above surface modification layer forming step is a first modification step of preparing a solution in which at least one selected from fluorine, hydrochloric acid, and phosphoric acid is added to a sulfuric acid solution, and immersing the surface of the first base material in the solution; and A method for manufacturing a metal separator, comprising a second modification step of immersing a first base material that has undergone the first modification step in a solution containing hydrogen peroxide and fluorine.
11. In paragraph 8, A method for manufacturing a metal separator, wherein the above heat treatment step is performed at 100°C to 300°C for 10 seconds to 300 seconds.
12. In paragraph 8, In the above preparation step, prepare the second parent material, A method for manufacturing a metal separator further comprising a porous body piercing step of forming a porous body having a plurality of holes by punching the second base material prepared above.
13. In paragraph 12, A method for manufacturing a metal separator, further comprising a laminate forming step of forming a laminate by laminating and bonding the porous body to the center of the first base material after performing the heat treatment step and the porous body piercing step.
14. In paragraph 12, The surface modification layer forming step further includes modifying an externally exposed surface of the second base material or porous body before or after the porous body piercing step to form a surface modification layer on the exposed surface of the second base material or porous body. A method for manufacturing a metal separator, wherein the heat treatment step further includes heat treating a second base material or porous body on which the surface modification layer is formed.
15. In paragraph 12, A method for manufacturing a metal separator, further comprising a slitting step of slitting the widths of the first and second base materials, respectively, before performing the manifold piercing step and the porous body piercing step.
Citation Information
Patent Citations
Stainless steel separator for polymer electrolyte fuel cell and polymer electrolyte fuel cell
JP2006302731A
Ferritic stainless steel material, separator, solid polymer fuel cell, and method for producing separator
KR101878115B1
Bipolar plate for direct methanol fuel cell and method of manufacturing the same
KR1020120072824A
Method of manufacturing stainless steel for proton exchange membrane fuel cell separator
KR102102608B1
Paste For Solar Cell's Electrode And Solar Cell using the same