Method for recycling manganese from laterite-nickel ore hydrometallurgy raffinate
By using oxalate, carbonate or carbon gas precipitants in the laterite nickel ore hydrosmelting residual liquid to precipitate manganese element in a divalent form, the problem of manganese element not being recovered is solved, and efficient utilization of resources and cost reduction are achieved. , and provides directly available manganese raw materials for the battery industry.
Patent Information
- Application Number
- PCT/CN2023/116259
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-31
AI Technical Summary
Manganese element cannot be effectively recovered during the hydrosmelting process of laterite nickel ore, resulting in waste of resources and increased costs.
By adding a precipitant containing oxalate, carbonate or carbon gas to the laterite nickel ore hydrosmelting residual liquid, the manganese element is precipitated in a divalent form, and solid-liquid separation is performed to recover the manganese element. The pH value and temperature are controlled to Optimize the precipitation reaction.
It improves the recovery rate and resource utilization rate of manganese, reduces wastewater treatment costs, and provides economic benefits. The divalent manganese precipitation can be directly used in the battery industry, reducing downstream treatment costs.
Smart Images

Figure CN2023116259_31102024_PF_FP_ABST
Abstract
Description
Method for recovering manganese from residual liquid of laterite nickel ore hydrometallurgy
[0001] This application claims priority to a Chinese patent application filed on April 25, 2023, with application number 202310467247.3, entitled “Method for recovering manganese from residual liquid from wet smelting of laterite nickel ore”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The present application relates to the technical field of hydrometallurgical wastewater treatment, and in particular to a method for recovering manganese from residual liquid in the hydrometallurgical process of laterite nickel ore. Background Art
[0003] Laterite nickel ore is a key mineral for nickel and cobalt extraction. During atmospheric or high-pressure acid leaching, other valuable associated metals are partially leached into the leachate. Manganese typically accounts for 0.1% to 2% of manganese content in laterite nickel ore. Because manganese is relatively low in value compared to nickel and cobalt, it is typically not recovered during laterite nickel ore hydrometallurgy. After nickel and cobalt precipitation, manganese remains in the residual smelting solution and is discharged with it. This results in manganese waste and hinders cost reduction. Technical issues
[0004] In view of this, the present application provides a method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy, which can better recover the manganese element to reduce costs. Technical Solutions
[0005] The present application provides a method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy, the method comprising:
[0006] S1: adding a precipitant to the residual solution of laterite nickel ore hydrometallurgy to precipitate manganese in the residual solution, wherein the precipitant precipitates the manganese in the form of divalent ions;
[0007] S2: performing solid-liquid separation on the smelting residual liquid of the precipitate containing manganese element.
[0008] Furthermore, the precipitant is an oxalate-containing substance, a carbonate-containing substance or a carbon-containing gas.
[0009] Furthermore, the oxalate-containing substance includes one or more of potassium oxalate, sodium oxalate, ammonium oxalate, calcium oxalate and magnesium oxalate, and the molar ratio of manganese element in the laterite nickel ore wet smelting residual liquid to oxalate in the added precipitant is 1:0.5-1:5.
[0010] Furthermore, the carbonate-containing substance includes one or more of potassium carbonate, sodium carbonate, ammonium carbonate, calcium carbonate, magnesium carbonate and magnesium bicarbonate, and the molar ratio of manganese element in the laterite nickel ore wet smelting residual liquid to carbonate in the added precipitant is 1:0.5-1:5.
[0011] Furthermore, the carbon-containing gas includes one or more of carbon monoxide, carbon dioxide, methane and acetylene, and the molar ratio of manganese element in the laterite nickel ore wet smelting residual liquid to carbon in the carbon-containing gas in the added precipitant is 1:0.5-1:10.
[0012] Furthermore, in step S1, the method further comprises adjusting the pH of the laterite nickel ore hydrometallurgical residual solution after the addition of the precipitant, wherein the pH is controlled in the range of 6-12.
[0013] Furthermore, when adjusting the pH, the method includes adding an alkaline neutralizer to the laterite nickel ore wet smelting residual solution, and the alkaline neutralizer includes one or more of NaOH, Na2CO3, CaO, Ca(OH)2, MgO and Mg(OH)2.
[0014] Furthermore, in step S1, when the precipitation reaction of manganese element is carried out, this step also includes controlling the temperature and reaction time of the smelting residual liquid, wherein the temperature is 25-99° C. and the reaction time is 10 min-10 h.
[0015] Furthermore, when performing step S1, the method further comprises adding a precipitate containing manganese elements to the residual liquid of the laterite nickel ore wet smelting in step S1.
[0016] Furthermore, the molar ratio of the precipitate containing manganese added to the residual solution of laterite nickel ore wet smelting to the manganese in the residual solution of laterite nickel ore wet smelting is 1:0.1-1:20. Beneficial effects
[0017] In summary, in the present application, by adding a precipitant such as a carbonate-containing substance, an oxalate-containing substance or a carbon-containing gas to the residual solution of laterite nickel ore wet smelting to precipitate manganese in the form of divalent ions, the manganese in the smelting residual solution can be directly precipitated in the form of divalent manganese, which can directly recover manganese, improve resource utilization, and reduce wastewater treatment costs. The recovered divalent manganese precipitate can be used as a raw material for the manganese smelting industry, providing additional economic benefits for laterite nickel ore smelters; further, since manganese is precipitated as a divalent precipitate, in the battery industry, manganese is generally also utilized in a divalent form, which means that the manganese recovered by this method can be directly utilized in the downstream battery industry without the need for reduction treatment of the manganese precipitate product, and the divalent manganese precipitate has good acid solubility, which greatly reduces the cost of manganese utilization in the downstream industry and increases the enthusiasm of the entire industry for manganese recovery.
[0018] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] FIG1 is a schematic flow chart showing the steps of a method for recovering manganese from residual liquid from laterite nickel ore hydrometallurgy provided in an embodiment of the present application. Modes for Carrying Out the Invention
[0020] In order to further illustrate the technical means and effects adopted by this application to achieve the predetermined invention objectives, the following is a detailed description with reference to the accompanying drawings and preferred embodiments.
[0021] The present application provides a method for recovering manganese from the residual liquid of laterite nickel ore wet smelting, which can effectively recover the manganese element and reduce costs.
[0022] FIG1 is a flow diagram of the steps of the method for recovering manganese from the residual solution of laterite nickel ore hydrometallurgy provided in an embodiment of the present application. As shown in FIG1 , the method for recovering manganese from the residual solution of laterite nickel ore hydrometallurgy provided in an embodiment of the present application comprises the following steps:
[0023] S1: adding a precipitant to the residual solution of laterite nickel ore hydrometallurgy to precipitate manganese in the residual solution, wherein the precipitant precipitates the manganese in the form of divalent ions;
[0024] In the present application, the residual liquid of laterite nickel ore wet smelting refers to the residual liquid after nickel and cobalt are precipitated from laterite nickel ore through a wet smelting process. The residual liquid contains manganese, and the mass concentration of manganese is generally greater than 0.2 g / L.
[0025] Furthermore, in this step, the residual liquid from the wet smelting of laterite nickel ore is generally placed in a reaction tank first, and then a precipitant is added to the reaction tank.
[0026] In this embodiment, the precipitant is a substance containing oxalate, a substance containing carbonate, or a carbon-containing gas.
[0027] In the present embodiment, the precipitation agent containing the material of oxalate is one or more of materials such as potassium oxalate, sodium oxalate, ammonium oxalate, calcium oxalate and magnesium oxalate, to obtain manganese oxalate precipitation. In the residual solution of laterite nickel ore hydrometallurgy, the mol ratio of manganese element and the precipitation agent added is 1:0.5-1:5, such as 1:0.5, 1:0.7, 1:0.9, 1:1.1, 1:1.3, 1:1.5, 1:2, 1:3, 1:4, 1:5 etc. Within the scope, the manganese recovery rate is high, and the oxalic acid substance consumption is few. If the oxalate ratio is too high, it causes more waste of oxalic acid. If too low, the recovery rate of manganese can be low. Before carrying out the recovery of manganese, the content of manganese element in the residual solution of laterite nickel ore hydrometallurgy can be measured first, to determine the amount of the precipitation agent added.
[0028] In the present embodiment, the precipitation agent containing carbonate radical material is one or more in materials such as salt of wormwood, sodium carbonate, volatile salt, calcium carbonate, magnesium carbonate and magnesium bicarbonate, to obtain manganese carbonate precipitation.In the residual solution of laterite nickel ore hydrometallurgy, the mol ratio of carbonate radical in manganese element and the precipitation agent added is 1:0.5-1:5, such as 1:0.5, 1:0.7, 1:0.9, 1:1.1, 1:1.3, 1:1.5, 1:2, 1:3, 1:4, 1:5 etc.Within the scope of this, the manganese recovery rate is high, and the carbonate radical material consumption is few. If the carbonate radical ratio is too high, it causes the more waste of carbonate radical. If too low, the recovery rate of manganese can be low.
[0029] In this embodiment, the carbon-containing gas precipitant is one or more gases selected from carbon monoxide, carbon dioxide, methane, and acetylene to produce manganese carbonate precipitate. The molar ratio of manganese in the residual solution from laterite nickel ore hydrometallurgy to carbon in the added precipitant is 1:0.5-1:10, such as 1:0.5, 1:0.7, 1:0.9, 1:1.0, 1:2, 1:3, 1:4, 1:5, 1:7, 1:9, etc. Within this range, the manganese recovery rate is high and the amount of gas precipitant used is low. If the ratio is too high, the gas precipitant is wasted significantly, while if it is too low, the manganese recovery rate is low.
[0030] Furthermore, in this step, the pH of the residual solution of laterite nickel ore wet smelting after adding the precipitant may be adjusted to facilitate precipitation, and the control range of the pH is 6-12. If the pH value is too high, the proportion of tetravalent manganese in the precipitated manganese is too high, which is not conducive to the subsequent utilization of manganese. If the pH value is too low, manganese cannot be precipitated. The method for adjusting the pH can be to add an alkaline neutralizer to the residual solution of laterite nickel ore wet smelting after adding the precipitant, and the alkaline neutralizer is one or more of NaOH, Na2CO3, CaO, Ca(OH)2, MgO and Mg(OH)2. It is understandable that whether to adjust the pH needs to be determined based on the pH of the solution after adding the precipitant.
[0031] Furthermore, during the manganese precipitation reaction, the temperature and reaction time of the smelting residual solution must be controlled, with the controlled temperature being 25-99°C and the reaction time being 10 minutes to 10 hours. This temperature and time range is conducive to the precipitation of manganese as a divalent ion and a high manganese recovery rate.
[0032] After adding an oxalate-containing substance, a carbonate-containing substance, or a carbon-containing gas and neutralizing the smelting residual solution, the carbonate or oxalate in the solution can directly react with the divalent manganese element to form a precipitate of manganese carbonate or manganese oxalate. During the formation of this precipitate, the valence state of the manganese element does not need to change, and the precipitation is still in a divalent form. At the same time, manganese carbonate or manganese oxalate has good acid solubility and a low impurity content, making it suitable as a high-quality manganese ore raw material for the manganese smelting industry, helping to reduce downstream usage costs.
[0033] S2: performing solid-liquid separation on the smelting residual liquid of the precipitate containing manganese element to complete the recovery of manganese element.
[0034] In this embodiment, it can be first settled, such as by static settling or thickener settling, and then solid-liquid separation can be performed by positive pressure filtration or negative pressure filtration.
[0035] After solid-liquid separation, the obtained solid matter can also be washed.
[0036] Furthermore, in this embodiment, a manganese-containing precipitate may be added to the residual solution from the laterite nickel ore hydrometallurgy process in step S1. The addition of this substance is equivalent to adding seed crystals to the residual solution from the laterite nickel ore hydrometallurgy process, which accelerates the reaction rate of manganese precipitation and facilitates the formation of the precipitate in step S1. The manganese-containing precipitate may be the underflow of the manganese-containing precipitate obtained in step S1 after sedimentation, or it may be the solid material obtained after solid-liquid separation in step S2.
[0037] Furthermore, in the present embodiment, the molar ratio of the manganese-containing precipitate added to the residual solution of laterite nickel ore hydrometallurgy to the manganese element in the original residual solution of laterite nickel ore hydrometallurgy is 1:0.1-1:20, such as 1:1.01, 1:3, 1:5, 1:7, 1:9, 1:11, 1:13, 1:15, 1:17, 1:19, 1:20, etc. Preferably, the ratio of the two is 1:0.5-1:5. Within this range, the amount of seed crystal added can significantly increase the reaction speed of manganese precipitation. If the amount of seed crystal added is too high, the increase in reaction speed will no longer increase, but the circulation amount will be too large, resulting in unnecessary energy waste. If the amount of seed crystal added is too low, the reaction speed increase is not obvious.
[0038] The following is a specific embodiment to illustrate the method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy provided by the present application:
[0039] Example 1
[0040] The raw solution, derived from the residual liquid from the laterite nickel ore hydrometallurgy process, was determined to contain 1.15 g / L Mn and 11.50 g / L Mg. Na₂C₂O₄ was added under stirring, with the molar ratio of oxalate in the Na₂C₂O₄ to manganese in the residual liquid from the laterite nickel ore hydrometallurgy process being 4:1. The reaction temperature was 80°C, a neutralizer was added to control the pH to 7.6, and the reaction time was 6 hours. After the reaction, the slurry was allowed to settle, filtered, and washed to produce a precipitate containing manganese oxalate. Analysis of the manganese grade in the solid sample revealed that manganese accounted for 35.65% of the total mass of the precipitate.
[0041] Example 2
[0042] The raw solution, derived from the residual liquid from the laterite nickel ore hydrometallurgy process, was determined to contain 1.80 g / L Mn and 12.50 g / L Mg. MgCO₃ was added while stirring, with a molar ratio of 3:1 between the carbonate and the manganese in the residual liquid. The reaction temperature was 70°C, a neutralizer was added to control the pH to 7.0, and the reaction time was 7 hours. After the reaction, the slurry was allowed to settle, filtered, and washed to obtain a precipitate containing manganese carbonate. Analysis of the manganese grade in the solid sample revealed that manganese accounted for 42.55% of the total mass of the precipitate.
[0043] Example 3
[0044] The raw liquid, derived from the residual liquid from the laterite nickel ore hydrometallurgy process, was measured to contain 2.10 g / L of Mn and 15.50 g / L of Mg. CO2 gas was introduced while stirring, with a molar ratio of 10:1 between CO2 and manganese in the residual liquid from the laterite nickel ore hydrometallurgy process. The reaction temperature was 80°C, and the neutralizer Ca(OH)2 was added to control the pH to 7.5. The reaction time was 8 hours. After the reaction, the slurry was allowed to settle, filtered, and washed to obtain a precipitate containing manganese carbonate. Analysis of the manganese grade in the solid sample revealed that manganese accounted for 18.05% of the total mass of the precipitate.
[0045] Example 4
[0046] The parameters of the present embodiment and Example 3 are substantially the same, except that the manganese-containing precipitate generated in Example 3 is added to the stirred reactor before the precipitation reaction in an amount of about 3 times the theoretical production solids of the present embodiment. Under stirring, CO gas is introduced, the molar ratio of CO to the manganese element in the residual liquid of laterite nickel ore hydrometallurgy is 5:1, the reaction temperature is 60°C, and a neutralizing agent Ca(OH) is added to control the reaction pH value to 7.0, and the reaction time is 4h. After the reaction, the ore pulp is settled, filtered, and washed to obtain the manganese carbonate-containing precipitate. The mass of manganese accounts for 18.55% of the total mass of the precipitate after measurement. In the present embodiment, after adding the manganese-containing precipitate, the reaction of precipitating manganese is easier to carry out and the reaction speed is faster. From the comparative data, the manganese content in the obtained final product is also slightly higher than that in Example 3.
[0047] In summary, in the present application, by adding a precipitant such as a carbonate-containing substance, an oxalate-containing substance or a carbon-containing gas to the residual solution of laterite nickel ore wet smelting to precipitate manganese in the form of divalent ions, the manganese in the smelting residual solution can be directly precipitated in the form of divalent manganese, which can directly recover manganese, improve resource utilization, and reduce wastewater treatment costs. The recovered divalent manganese precipitate can be used as a raw material for the manganese smelting industry, providing additional economic benefits for laterite nickel ore smelters; further, since manganese is precipitated as a divalent precipitate, in the battery industry, manganese is generally also utilized in a divalent form, which means that the manganese recovered by this method can be directly utilized in the downstream battery industry without the need for reduction treatment of the manganese precipitate product, and the divalent manganese precipitate has good acid solubility, which greatly reduces the cost of manganese utilization in the downstream industry and increases the enthusiasm of the entire industry for manganese recovery.
[0048] The above description is merely a preferred embodiment of the present application and does not constitute any form of limitation to the present application. Although the present application has been disclosed as a preferred embodiment, it is not intended to limit the present application. Any technician familiar with this profession can make slight changes or modifications to equivalent embodiments of the technical contents disclosed above without departing from the scope of the technical solution of the present application. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application are still within the scope of the technical solution of the present application.
Claims
1. A method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy, characterized in that: The method includes: S1: adding a precipitant to the residual solution of laterite nickel ore hydrometallurgy to precipitate the manganese element in the residual solution, wherein the precipitant precipitates the manganese element in the form of divalent ions; S2: solid-liquid separation of the smelting residual liquid of the precipitate containing manganese element.
2. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 1, characterized in that: The precipitant is an oxalate-containing substance, a carbonate-containing substance or a carbon-containing gas.
3. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 2, characterized in that: The oxalate-containing substance includes one or more of potassium oxalate, sodium oxalate, ammonium oxalate, calcium oxalate and magnesium oxalate. The molar ratio of manganese element in the laterite nickel ore wet smelting residual liquid to oxalate in the added precipitant is 1:0.5-1:
5.
4. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 2, characterized in that: The carbonate-containing substance includes one or more of potassium carbonate, sodium carbonate, ammonium carbonate, calcium carbonate, magnesium carbonate and magnesium bicarbonate. The molar ratio of manganese element in the laterite nickel ore hydrometallurgical residual liquid to carbonate in the added precipitant is 1:0.5-1:
5.
5. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 2, characterized in that: The carbon-containing gas includes one or more of carbon monoxide, carbon dioxide, methane and acetylene, and the molar ratio of manganese element in the laterite nickel ore wet smelting residual liquid to carbon in the carbon-containing gas in the added precipitant is 1:0.5-1:
10.
6. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 1, characterized in that: In step S1, the method further comprises adjusting the pH of the laterite nickel ore hydrometallurgical residual solution after the precipitant is added, and the pH control range is 6-12.
7. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 6, characterized in that: When adjusting the pH, the method includes adding an alkaline neutralizer to the laterite nickel ore wet smelting residual solution, and the alkaline neutralizer includes one or more of NaOH, Na2CO3, CaO, Ca(OH)2, MgO and Mg(OH)2.
8. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 1, characterized in that: In step S1, when the precipitation reaction of manganese element is carried out, this step also includes controlling the temperature of the smelting residual liquid and the reaction time. The temperature of the smelting residual liquid is 25-99° C., and the reaction time is 10 min-10 h.
9. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 1, characterized in that: When performing step S1, the method further comprises adding a precipitate containing manganese elements to the residual liquid of the laterite nickel ore wet smelting in step S1.
10. The method for recovering manganese from the residual liquid of laterite nickel ore hydrometallurgy according to claim 9, characterized in that: The molar ratio of the precipitate containing manganese added to the residual solution of laterite nickel ore hydrometallurgy to the manganese in the residual solution of laterite nickel ore hydrometallurgy is 1:0.1-1:20.
Citation Information
Patent Citations
Method for recycling manganese from P204 manganese back extraction solution in nickel laterite hydrometallurgical process
CN102560156A
Method for recycling manganese from electrolyzed manganese ore residues
CN105417584A
Method for recovering manganese from laterite-nickel ore hydrometallurgy raffinate
CN116497219A
Process for producing low-phosphorus manganese phosphide concentrate for making high-grade manganese alloys
RU2010880C1
Method for homogeneous precipitation separation of nickel, cobalt and manganese from laterite nickel ore acid leaching solution
WO2020019918A1
Cited By
MHP precipitation method based on compound alkali precipitant and application of MHP precipitation method
CN119491101A
Precipitation method of heavy metal solution
CN119571061A