Preparation method for amide mineral oil type defoamer

By mixing hydrophobic silica and fatty acid amide in mineral oil and performing heating and cooling treatment, the problem of large particles of fatty acid amide in mineral oil-based defoamer is solved, and the stability and anti-foaming performance of the defoamer are improved. Suitable for a variety of industrial applications.

WO2024221777A1PCT designated stage expired Publication Date: 2024-10-31JIANGSU SIXIN SCI-TECH APPL RES INST CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/126393
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-10-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

During the preparation process of existing mineral oil-based defoaming agents, the phenomenon of large particles of fatty acid amide affects the defoaming and suppressing performance, and the stability is insufficient, making it difficult to show good compatibility and stability in applications such as papermaking and coatings.

Method used

By mixing hydrophobic silica and fatty acid amide in some mineral oil and grinding at high speed, combined with heating and cooling treatment, the particle size of the fatty acid amide is reduced, and the stability and anti-foaming performance of the defoamer are improved to form an amide mineral oil type. Defoaming agent.

Benefits of technology

Significantly improves the stability and anti-foaming performance of the defoaming agent, allowing it to show good compatibility and use effects in applications such as papermaking, coatings, coatings, sewage treatment, and latex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023126393-FTAPPB-I100001
    Figure PCTCN2023126393-FTAPPB-I100001
  • Figure PCTCN2023126393-FTAPPB-I100002
    Figure PCTCN2023126393-FTAPPB-I100002
  • Figure PCTCN2023126393-FTAPPB-I100003
    Figure PCTCN2023126393-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention aims to provide a preparation method for an amide mineral oil type defoamer, the method comprising: first mixing in part of mineral oil hydrophobic white carbon black and fatty acid amide, and grinding same by means of a colloid mill, so as to reduce the phenomenon of large particles of the fatty acid amide in later stages, thus improving the defoaming and foam inhibition performance; heating a dispersion liquid obtained after the grinding to increase the temperature to be 5-10℃ above the melting point of the fatty acid amide; and then adding the dispersion liquid into the mineral oil for rapid cooling, and reducing the temperature to be 5-10℃ above the condensate point of the fatty acid amide, so as to avoid system viscosity rise and stratification which are caused by fatty acid amide gels, thus improving the product stability.
Need to check novelty before this filing date? Find Prior Art

Description

A preparation method of amide mineral oil type defoamer Technical Field

[0001] This patent mainly relates to a preparation process of an amide mineral oil type defoamer. Defoamers are fine chemicals. Therefore, the present invention belongs to the field of fine chemical technology. Background Art

[0002] Defoamers are fine chemicals widely used in various industrial fields. During use, they must not only possess excellent foam reduction and suppression properties and stability, but also demonstrate excellent compatibility with other additives. Defoamers are primarily categorized as silicone defoamers and non-silicone defoamers. Non-silicone defoamers are generally composed of fatty alcohols, fatty acid esters, metal soaps, fatty acid amides, polyethers, and mineral oils. Due to their higher surface tension than silicone oil, they are less likely to spread across the foam film surface, and therefore generally lack the foam reduction and suppression properties of silicone defoamers. However, their compatibility with organic systems is better, leading to their common use in coatings, inks, papermaking, adhesives, and other systems.

[0003] Numerous documents describe amide-based mineral oil defoamers. US4094812 describes a method for preparing a mineral oil defoamer containing an α-hydroxyamine derivative; US3652452 describes a defoamer composed of a rapidly cooling amine and an organic hydrocarbon; CN101445760 describes a defoamer composed of ethylene bisstearamide, an organic hydrocarbon, and hydrophilic silica; CN101003644 describes a defoamer for peritoneal glue composed of an organic hydrocarbon and a fatty acid amide; CN101445760A utilizes inorganic particles and / or fatty acid amide as the primary defoaming agents, and increases product stability by adding hydrophilic inorganic particles to increase system viscosity; CN1762531A utilizes fatty acid amide, silicone resin, and silica as defoaming agents, and adds a specially modified silicone polyether to enhance the defoaming and antifoaming properties, safety, and stability of the defoamer.

[0004] In the process of preparing mineral oil-type defoaming agents, when fatty acid amides are used as hydrophobic particles, larger amide particles will appear in the obtained defoaming agent, affecting the defoaming and antifoaming performance. The inventor of this patent found through a large number of experimental studies that mixing fatty acid amide and hydrophobic silica as defoaming substances and grinding them at high speed can reduce the large particle phenomenon of fatty acid amide. At the same time, the heating and cooling of the mixture of the two are temperature controlled to improve the stability and defoaming and antifoaming performance of the defoaming agent. The defoaming agent finally prepared has good application effects in papermaking black liquor, coatings, coatings, sewage treatment, latex, and cleaning processes.

[0005] Summary of the Invention

[0006] The present invention aims to provide a method for preparing an amide mineral oil-based defoamer. First, hydrophobic silica and fatty acid amide are mixed in part of mineral oil and ground by a colloid mill to reduce the large particle phenomenon of fatty acid amide in the later stage and improve the defoaming and antifoaming performance. The ground dispersion is heated to 5-10°C above the melting point of fatty acid amide, and then the dispersion is added to mineral oil and rapidly cooled to 5-10°C above the condensation point of fatty acid amide, so as to avoid the increase of viscosity of the system and stratification due to gelation of fatty acid amide, thereby improving the stability of the product.

[0007] The amide mineral oil type defoamer of the present invention is composed of the following components:

[0008] A. Mineral oil

[0009] Mineral oil is used as a carrier and is selected from kerosene, diesel, engine oil, white oil, liquid paraffin, and alkylbenzene; these mineral oils are liquid at room temperature and are used in an amount of 60-80% of the total mass of the defoamer; the mineral oil consists of two parts, A1 and A2: mineral oil A1: the amount accounts for 30-50% of the total mass of the mineral oil; mineral oil A2: the amount accounts for 50-70% of the total mass of the mineral oil; mineral oil A1 and mineral oil A2 can be the same or different.

[0010] B. Defoaming substances

[0011] The defoaming substance consists of fatty acid amide and white carbon black.

[0012] B1: fatty acid amide, selected from one or more of ethylene bisstearamide (abbreviated as EBS), ethylene bispalmitamide, ethylene bismyristamide, ethylene bislauric amide, ethylene bisoleic amide, propylene bisstearamide, propylene bispalmitamide, propylene bismyristamide, propylene bislauric amide, propylene bisoleic amide, butylene bisstearamide, butylene bispalmitamide, butylene bismyristamide, butylene bislauric amide, and butylene bisoleic amide; preferably ethylene bisstearamide and ethylene bislauric amide; the amount of fatty acid amide is 3 to 10% of the total mass of the mineral oil defoamer.

[0013] B2: Silica

[0014] The white carbon black is selected from precipitated hydrophobic white carbon black and fumed hydrophobic white carbon black, preferably fumed hydrophobic white carbon black, and has a specific surface area of ​​20 to 500 m 2 / g; the dosage is 0.5-10% of the total mass of the defoaming agent.

[0015] C. Defoaming agent

[0016] The defoaming agent is polyether, and the general structural formula of polyether is as follows: RO(EO) x (PO) y H

[0017] wherein the subscript x is an integer of 1 to 100, and y is an integer of 1 to 200; R is an alkyl group; the alkyl group is a branched or straight-chain alkyl group having 4 to 20 carbon atoms, including butyl, isobutyl, octyl, isooctyl, dodecyl, tetradecyl, hexadecyl, and octadecyl; and the defoaming agent accounts for 1 to 20% of the total mass of the defoaming agent.

[0018] D. Emulsifier

[0019] The emulsifier is a nonionic surfactant, which is selected from fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, polyoxyethylene fatty amine compound, castor oil polyoxyethylene ether, polyoxyethylene sorbitan monolaurate (Tween-20), polyoxyethylene sorbitan monopalmitate (Tween-40), polyoxyethylene sorbitan monostearate (Tween-60), polyoxyethylene sorbitan monooleate (Tween-80), polyoxyethylene sorbitan trioleate (Tween-85), sorbitan monolaurate (Span-20), sorbitan monopalmitate (Span-40), sorbitan monostearate (Span-60), and sorbitan monooleate (Span-80), and is used alone or in combination. The amount of the emulsifier is 3 to 20% of the total mass of the defoamer.

[0020] On the basis of the above substances, an amide mineral oil defoamer is prepared, and the steps are as follows:

[0021] (1) Mineral oil A1, defoaming agent C, defoaming substance B1, and defoaming substance B2 are mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X;

[0022] (2) The mixture X is heated in a sealed container to the melting point B1 of the defoaming substance B1. mp ℃ as the benchmark, raise the temperature to [B1 mp +(5-10)]℃, after stirring for a while, add the heated mixture X into mineral oil A2 and cool it quickly to the condensation point B1 of the defoaming substance B1. fp ℃ as the benchmark, cool down to [B1 fp +(5-10)]℃, forming a mixture Y;

[0023] (3) Continue to add emulsifier to the mixture Y and cool to room temperature while stirring to obtain the mineral oil defoamer. DETAILED DESCRIPTION

[0024] Example 1

[0025] (1) Mix 30g white oil and 10g defoaming agent C 18 H 37 O(EO)20 (PO) 40 H, 10g defoaming substance ethylene bis stearamide, 10g defoaming substance fumed hydrophobic silica (specific surface area of ​​200m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X1;

[0026] (2) The mixture X1 is heated in a sealed container to a temperature of about 100°C to the melting point of the defoaming substance ethylene bisstearamide. mp ℃ as the benchmark, raise the temperature to (B1 mp +5) ℃, after stirring for a while, the heated mixture X1 was added to 30g white oil and quickly cooled to the condensation point B1 of the defoaming substance ethylene bisstearamide. fp ℃ as the benchmark, cool to (B1 fp +8) °C, forming a mixture Y1;

[0027] (3) Add 10 g of emulsifier fatty alcohol polyoxyethylene ether to the mixture Y1, and cool to room temperature while stirring to obtain the mineral oil defoamer.

[0028] Example 2

[0029] (1) Mix 28g kerosene and 20g defoaming agent C 20 H 41 O(EO)5(PO) 20 H, 5g defoaming substance ethylene bislauric acid amide, 2g defoaming substance fumed hydrophobic silica (specific surface area of ​​500m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X2;

[0030] (2) The mixture X2 is heated in a sealed container to a temperature lower than the melting point of the defoaming substance ethylene bislauric acid amide B1. mp ℃ as the benchmark, raise the temperature to (B1 mp +6) ℃, after stirring for a while, the heated mixture X2 was added to 42g kerosene and quickly cooled to the condensation point B1 of the defoaming substance ethylene bislauric acid amide. fp ℃ as the benchmark, cool to (B1 fp +9) °C, forming a mixture Y2;

[0031] (3) Continue to add 3 g of emulsifier fatty acid polyoxyethylene ether and castor oil polyoxyethylene ether mixture to the mixture Y2, and cool to room temperature while stirring to obtain the mineral oil defoamer.

[0032] Example 3

[0033] (1) Mix 24g of engine oil and 1g of defoaming agent C 16 H33 O(EO) 30 (PO) 60 H, 3g of a mixture of ethylene bispalmitamide and ethylene bismyristamide, 0.5g of a precipitated hydrophobic silica (specific surface area 300m2) 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X3;

[0034] (2) The mixture X3 is heated in a sealed container to a temperature of about 100°C ... mp ℃ as the benchmark, raise the temperature to (B1 mp +7) ℃, after stirring for a while, the heated mixture X3 was added to 56g white oil and quickly cooled to the condensation point B1 of the mixture of defoaming substances ethylene bispalmitamide and ethylene bismyristamide. fp ℃ as the benchmark, cool to (B1 fp +10) °C, forming a mixture Y3;

[0035] (3) 15.5 g of a mixture of emulsifiers Tween-20 and Span-20 was added to the mixture Y3, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0036] Example 4

[0037] (1) 20g liquid wax, 3g defoaming agent C 14 H 29 O(EO) 10 (PO) 25 H, 8g of defoaming material ethylene bisoleamide and propylene bisstearamide mixture, 4g of defoaming material precipitated hydrophobic white carbon black (specific surface area 20m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X4;

[0038] (2) The mixture X4 is heated in a sealed container to a temperature of about 100°C to the melting point B1 of the mixture of the defoaming substances ethylenebisoleamide and propylenebisstearamide. mp ℃ as the benchmark, raise the temperature to (B1 mp +8) ℃, after stirring for a while, the heated mixture X4 was added to 45g of alkylbenzene and quickly cooled to the condensation point B1 of the defoaming substance ethylene bisoleamide and propylene bisstearamide mixture. fp ℃ as the benchmark, cool to (B1 fp +7) °C, forming a mixture Y4;

[0039] (3) 20 g of a mixture of emulsifiers Tween-40 and Span-40 were added to the mixture Y4, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0040] Example 5

[0041] (1) 30g alkylbenzene, 8g defoaming agent C 12 H 23 O(EO) 20 (PO) 50 H, 6g of a mixture of propylene bispalmitamide and propylene bismyristamide as a defoaming substance, 8g of a fumed hydrophobic silica (specific surface area 50m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X5;

[0042] (2) The mixture X5 is heated in a sealed container to a temperature of about 100°C to the melting point B1 of the mixture of the defoaming substances propylene bispalmitamide and propylene bismyristamide. mp ℃ as the benchmark, raise the temperature to (B1 mp +9) ℃, after stirring for a while, the heated mixture X5 was added to 40g white oil and cooled quickly to the condensation point B1 of the mixture of defoaming substances propylene bispalmitamide and propylene bismyristamide. fp ℃ as the benchmark, cool to (B1 fp +6) °C, forming a mixture Y5;

[0043] (3) 8 g of a mixture of emulsifiers Tween-60 and Span-60 was added to the mixture Y5, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0044] Example 6

[0045] (1) Mix 35g white oil and 15g defoaming agent C8H 17 O(EO) 15 (PO) 35 H, 4g defoaming material propylene bislauric acid amide and propylene bisoleic acid amide mixture, 1g defoaming material fumed hydrophobic silica (specific surface area of ​​100m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X6;

[0046] (2) The mixture X6 is heated in a sealed container to a temperature of about 100°C to a temperature of about 100°C. The mixture is heated to a temperature of about 100°C to a temperature of about 100°C. mp ℃ as the benchmark, raise the temperature to (B1 mp+10) ℃, after stirring for a while, the heated mixture X6 was added to 40g of liquid wax and quickly cooled to the condensation point B1 of the defoaming substance mixture of propylene bislauric acid amide and propylene bisoleic acid amide. fp ℃ as the benchmark, cool to (B1 fp +5) °C, forming a mixture Y6;

[0047] (3) 5 g of a mixture of emulsifiers Tween-80 and Span-80 was added to the mixture Y6, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0048] Example 7

[0049] (1) 35g liquid wax, 15g defoaming agent C4H9O (EO) 15 (PO) 35 H, 4g of a mixture of butylene bisstearic acid amide and butylene bispalmitic acid amide as a defoaming substance, 1g of a precipitated hydrophobic silica (specific surface area 400m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X7;

[0050] (2) The mixture X7 is heated in a sealed container to a temperature of about 100°C to the melting point B1 of the mixture of the defoaming substances butylene bisstearamide and butylene bispalmitamide. mp ℃ as the benchmark, raise the temperature to (B1 mp +8) ℃, after stirring for a while, the heated mixture X7 was added to 40g of liquid wax and quickly cooled to the condensation point B1 of the mixture of defoaming substances butylene bisstearic acid amide and butylene bispalmitic acid amide. fp ℃ as the benchmark, cool to (B1 fp +6) °C, forming a mixture Y7;

[0051] (3) 5 g of a mixture of emulsifiers Tween-85 and Span-80 was added to the mixture Y7, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0052] Comparative Example 1 - Example 1 comparison - heating temperature is lower than 5 ° C

[0053] (1) Mix 30g white oil and 10g defoaming agent C 18 H 37 O(EO) 20 (PO) 40 H, 10g defoaming substance ethylene bis stearamide, 10g defoaming substance fumed hydrophobic silica (specific surface area of ​​200m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X1;

[0054] (2) The mixture X1 is heated in a sealed container to a temperature of about 100°C to the melting point of the defoaming substance ethylene bisstearamide. mp ℃ as the benchmark, raise the temperature to less than (B1 mp +5) ℃, after stirring for a while, the heated mixture X1 was added to 30g white oil and quickly cooled to the condensation point B1 of the defoaming substance ethylene bisstearamide. fp ℃ as the benchmark, cool to (B1 fp +8) °C, forming a mixture Y8;

[0055] (3) 10 g of emulsifier fatty alcohol polyoxyethylene ether was added to the mixture Y8, and the temperature was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0056] Comparative Example 2 - Example 2 comparison - heating temperature is higher than 10 ° C

[0057] (1) Mix 28g kerosene and 20g defoaming agent C 20 H 41 O(EO)5(PO) 20 H, 5g defoaming substance ethylene bislauric acid amide, 2g defoaming substance fumed hydrophobic silica (specific surface area of ​​500m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X2;

[0058] (2) The mixture X2 is heated in a sealed container to a temperature lower than the melting point of the defoaming substance ethylene bislauric acid amide B1. mp ℃ as the benchmark, raise the temperature to greater than (B1 mp +10) ℃, after stirring for a while, the heated mixture X2 was added to 42g kerosene and quickly cooled to the condensation point B1 of the defoaming substance ethylene bislauric acid amide. fp ℃ as the benchmark, cool to (B1 fp +9) °C, forming a mixture Y9;

[0059] (3) Continue to add 3 g of emulsifier fatty acid polyoxyethylene ether and castor oil polyoxyethylene ether mixture to the mixture Y9, and cool to room temperature while stirring to obtain the mineral oil defoamer.

[0060] Comparative Example 3-Example 4 comparison, cooling to a condensation point less than 5 ° C

[0061] (1) 20g liquid wax, 3g defoaming agent C 14 H 29 O(EO) 10 (PO) 25 H, 8g of defoaming material ethylene bisoleamide and propylene bisstearamide mixture, 4g of defoaming material precipitated hydrophobic white carbon black (specific surface area 20m2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X4;

[0062] (2) The mixture X4 is heated in a sealed container to a temperature of about 100°C to the melting point B1 of the mixture of the defoaming substances ethylenebisoleamide and propylenebisstearamide. mp ℃ as the benchmark, raise the temperature to (B1 mp +8) ℃, after stirring for a while, the heated mixture X4 was added to 45g of alkylbenzene and quickly cooled to the condensation point B1 of the defoaming substance ethylene bisoleamide and propylene bisstearamide mixture. fp ℃ as the benchmark, cool to (B1 fp +4) °C, forming a mixture Y10;

[0063] (3) 20 g of a mixture of emulsifiers Tween-40 and Span-40 were added to the mixture Y10, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0064] Comparative Example 4-Example 5 comparison, cooling to a condensation point greater than 10 ° C

[0065] (1) 30g alkylbenzene, 8g defoaming agent C 12 H 23 O(EO) 20 (PO) 50 H, 6g of a mixture of propylene bispalmitamide and propylene bismyristamide as a defoaming substance, 8g of a fumed hydrophobic silica (specific surface area 50m 2 / g) were mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X5;

[0066] (2) The mixture X5 is heated in a sealed container to a temperature of about 100°C to the melting point B1 of the mixture of the defoaming substances propylene bispalmitamide and propylene bismyristamide. mp ℃ as the benchmark, raise the temperature to (B1 mp +9) ℃, after stirring for a while, the heated mixture X5 was added to 40g white oil and cooled quickly to the condensation point B1 of the mixture of defoaming substances propylene bispalmitamide and propylene bismyristamide. fp ℃ as the benchmark, cool to (B1 fp +11) °C, forming a mixture Y11;

[0067] (3) 8 g of a mixture of emulsifiers Tween-60 and Span-60 was added to the mixture Y11, and the mixture was cooled to room temperature while stirring to obtain the mineral oil defoamer.

[0068] Test Method

[0069] (1) Foam suppression performance test

[0070] Test method: Add 200g of self-prepared water-based paint to a 1000ml stainless steel cup, then add 0.3% defoaming agent, use a laboratory high-speed disperser to disperse at a speed of 1000rpm for 10 minutes, and immediately pour into a 1000ml measuring cylinder after stopping, record the weight and volume of the liquid, and calculate the specific gravity. A larger specific gravity value indicates a smaller air content, indicating that the defoaming agent has good anti-foaming performance.

[0071] (2) Compatibility test

[0072] Test method: After the high-speed dispersed paint is placed for 10 minutes, take out a small amount and place it on a glass plate. Use a 75um wet film preparation device to scrape the paint evenly at a constant speed, observe the state of the coating, and express it with a grade. The higher the grade, the better the compatibility.

[0073] Table 2 Coating grade classification

[0074] (3) The stability of the sample was tested using a Formulaction / Turbiscan Tower / Multiple Light Scattering Stability Analyzer at a test temperature of 40°C and a sample size of 20 g. The smaller the TSI index in the test results, the better the sample stability.

[0075] The test results are as follows:

[0076] (1) Foam suppression performance test results:

[0077] (2) Compatibility test results:

[0078] (3) Stability test results:

Claims

1. A method for preparing an amide mineral oil defoamer, comprising the following components: A. Mineral oil Mineral oil is used as a carrier, selected from kerosene, diesel, engine oil, white oil, liquid wax, alkylbenzene; these mineral oils are liquid at room temperature, and the amount used is 60-80% of the total mass of the defoamer; the mineral oil is composed of two parts, A1 and A2, and the mineral oil A1 and the mineral oil A2 can be the same or different; B. Defoaming substances The defoaming substance is composed of fatty acid amide and white carbon black; B1: fatty acid amide, selected from one or more of ethylene bisstearic acid amide (abbreviated as EBS), ethylene bispalmitic acid amide, ethylene bismyristic acid amide, ethylene bislauric acid amide, ethylene bisoleic acid amide, propylene bisstearic acid amide, propylene bispalmitic acid amide, propylene bismyristic acid amide, propylene bislauric acid amide, propylene bisoleic acid amide, butylene bisstearic acid amide, butylene bispalmitic acid amide, butylene bismyristic acid amide, butylene bislauric acid amide, and butylene bisoleic acid amide; the amount of fatty acid amide is 3-10% of the total mass of the mineral oil type defoamer; B2: White carbon black The white carbon black is selected from the precipitation method hydrophobic white carbon black and the gas phase method hydrophobic white carbon black, and its specific surface area is 20 to 500 m 2 / g; the dosage is 0.5-10% of the total mass of the defoamer; C. Defoaming agent The defoaming agent is polyether, and the general structural formula of polyether is as follows: RO(EO) x (SHELF) y H wherein the subscript x is an integer of 1 to 100, and y is an integer of 1 to 200; R is an alkyl group; the alkyl group is a branched or straight chain alkyl group having 4 to 20 carbon atoms, including butyl, isobutyl, octyl, isooctyl, dodecyl, tetradecyl, hexadecyl, and octadecyl; and the defoaming agent accounts for 1 to 20% of the total mass of the defoaming agent; D. Emulsifier The emulsifier is a nonionic surfactant, which is selected from fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, polyoxyethylene fatty amine compound, castor oil polyoxyethylene ether, polyoxyethylene sorbitan monolaurate (Tween-20), polyoxyethylene sorbitan monopalmitate (Tween-40), polyoxyethylene sorbitan monostearate (Tween-60), polyoxyethylene sorbitan monooleate (Tween-80), polyoxyethylene sorbitan trioleate (Tween-85), sorbitan monolaurate (Span-20), sorbitan monopalmitate (Span-40), sorbitan monostearate (Span-60), sorbitan monooleate (Span-80), and is used alone or in combination; the amount of the emulsifier is 3-20% of the total mass of the defoamer; The preparation method of the amide mineral oil type defoamer is as follows: (1) Mineral oil A1, defoaming agent C, defoaming substance B1 and defoaming substance B2 are mixed and stirred uniformly, and then further dispersed by grinding with a colloid mill to form a mixture X; (2) The mixture X is heated in a sealed container to a temperature of the melting point B1 of the defoaming substance B1. mp ℃ as the benchmark, raise the temperature to [B1 mp +(5-10)]℃, after stirring for a while, the heated mixture X is added to the mineral oil A2 and quickly cooled to the condensation point B1 of the defoaming substance B1. fp ℃ as the benchmark, cooling to [B1 fp +(5-10)]℃, forming a mixture Y; (3) Continue to add emulsifier to mixture Y and cool to room temperature while stirring to obtain The mineral oil defoamer.

2. The method for preparing an amide mineral oil type defoamer according to claim 1, characterized in that: The amount of the mineral oil A1 accounts for 30-50% of the total mass of the mineral oil; the amount of the mineral oil A2 accounts for 50-70% of the total mass of the mineral oil.

3. The method for preparing an amide mineral oil type defoamer according to claim 1, characterized in that: The fatty acid amides are ethylene bisstearic acid amide and ethylene bislauric acid amide.

4. The method for preparing an amide mineral oil type defoamer according to claim 1, characterized in that: The white carbon black is gas phase hydrophobic white carbon black.

Citation Information

Patent Citations

  • Method for improving stability of mineral oil defoaming agent

    CN101445760A

  • Mineral oil defoaming agent and preparation method thereof

    CN101991975A

  • Preparation method of amide mineral oil type defoaming agent

    CN116808636A

  • Biodiesel-based emulsion defoamer and method for making the same

    WO2014179127A1