Steel plate for stamping and preparation method therefor, and stamping part and preparation method therefor
By increasing the Mn content and hot-dip galvanizing annealing treatment in the stamping steel plate, combined with pre-cooling treatment, the problem of liquid metal embrittlement in hot stamping is solved, the strength and plasticity of the stamping parts are improved, and the corrosion resistance of the coating is extended.
Patent Information
- Application Number
- PCT/CN2023/131307
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2023-11-13
- Publication Date
- 2024-10-31
AI Technical Summary
High-strength steel is prone to liquid metal embrittlement during the hot stamping process, leading to strength reduction and cracking problems. Traditional coatings liquefy at high temperatures, causing zinc-based coatings to fail.
By designing the chemical composition of the stamping steel plate, increasing the Mn content to expand the austenitization temperature range, combined with hot-dip galvanizing annealing and pre-cooling treatment, a multi-phase structure is formed to reduce the risk of liquid metal embrittlement and improve tensile strength and plasticity.
Achieve high tensile strength and plasticity at lower stamping temperatures, reduce the risk of cracking, extend the corrosion resistance of the coating, and improve the overall performance of the stamped parts.
Smart Images

Figure CN2023131307_31102024_PF_FP_ABST
Abstract
Description
A stamping steel plate and its preparation method, a stamping part and its preparation method
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to the Chinese patent application filed on April 27, 2023, with application number 202310473279.4 and entitled “A steel plate for stamping and its preparation method, a stamping part and its preparation method”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure belongs to the technical field of metallurgical materials, and in particular relates to a steel plate for stamping and a preparation method thereof, a stamping part and a preparation method thereof. Background Art
[0004] The use of high-strength and ultra-high-strength steel has a positive and effective effect on lightweighting automobile bodies. However, as the strength of automobile body steel continues to increase, its plasticity and formability have significantly decreased. This makes it prone to cracking and springback during the forming process, seriously affecting the shape and dimensional accuracy of parts. Hot stamping technology utilizes the properties of easy forming without springback at high temperatures and quenching and cooling the mold to produce ultra-high-strength parts exceeding 1300MPa, effectively solving the problems of cracking and severe springback caused by cold forming.
[0005] Traditional uncoated hot-stamped parts produce a large amount of surface oxide scale during the heating process, reducing the life of the mold. The need for regular mold cleaning also reduces production efficiency. To prevent oxide scale and decarburization on the surface of hot-stamped steel sheets and improve corrosion resistance, the main coatings currently suitable for hot-stamped steel include Al-Si coatings, GI coatings, GA coatings, and Zn-Ni coatings. Hot-stamped steel sheets with zinc-based coatings not only prevent surface oxidation and decarburization during heating, eliminating the need for subsequent shot peening, but also provide sacrificial anode protection, improving corrosion resistance after painting. However, a problem with hot-stamped steel sheets with zinc-based coatings is that the liquefied zinc at high temperatures of 900°C causes the steel sheet to become embrittled, a phenomenon known as LME (Liquid Metal Embrittlement). Surface cracks are prone to forming during hot stamping at temperatures above approximately 700°C and can propagate into the substrate, leading to reduced strength and other problems.
[0006] Summary of the Invention
[0007] By utilizing one or more embodiments of the present disclosure, the technical problem of reduced strength of stamping steel sheets due to embrittlement of liquid metal is solved.
[0008] An embodiment of the present disclosure provides a steel plate for stamping, wherein the chemical composition of the steel in the stamping steel plate includes the following components in mass percentage: C and Si: ≤0.5%, Al: ≤0.06%, Cr: 0.1%-0.7%, Mo: ≤0.7%, B: 0.001%-0.005%, P: ≤0.01%, S: ≤0.005%, N: ≤0.01%, O: ≤0.003%; wherein, when 0.17%≤C<0.23%, Mn is 2.0%-3.0%; when 0.23%≤C<0.29%, Mn is 1.8%-2.5%; when 0.29%≤C<0.33%, Mn is 1.6%-2.0%; when 0.33%≤C<0.40%, Mn is 1.2%-1.8%.
[0009] Based on the same inventive concept, the embodiment of the present disclosure also provides a method for preparing a steel plate for stamping as described above, comprising the following steps: obtaining a steel billet having the chemical composition described above through smelting and casting; subjecting the steel billet to a first heating, hot rolling, pickling and cold rolling to obtain a steel strip; and subjecting the steel strip to hot-dip galvanizing annealing, skin pass and straightening to obtain the steel plate for stamping; wherein the end temperature of the first heating is 1100°C-1280°C; the final rolling temperature of the hot rolling is 750°C-920°C; the coiling temperature of the hot rolling is 500°C-700°C; the total reduction rate of the cold rolling is 30%-80%; the temperature of the hot-dip galvanizing annealing is 400°C-600°C; the thickness of the coating formed by the hot-dip galvanizing annealing is 20g / m 2 -300g / m 2 .
[0010] Based on the same inventive concept, the embodiment of the present disclosure also provides a stamping part, which is made of any of the above-mentioned stamping steel plates.
[0011] Based on the same inventive concept, the embodiments of the present disclosure also provide a method for preparing any of the above-mentioned stamping parts, comprising the following steps: blanking the stamping steel plate to obtain a sheet; subjecting the sheet to a second heating and heat preservation to obtain a preheated sheet; and precooling, hot stamping and quenching the preheated sheet to obtain the stamping part.
[0012] The above description is only an overview of the technical solution of the present disclosure. In order to more clearly understand the technical means of the present disclosure, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present disclosure more obvious and easy to understand, the specific implementation methods of the present disclosure are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, a brief introduction will be given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0014] FIG1 shows a flow chart of a method for preparing a stamping steel plate according to some embodiments of the present disclosure;
[0015] FIG2 shows a metallographic structure diagram of a stamping steel plate according to some embodiments of the present disclosure;
[0016] FIG. 3 shows a SEM image of a plating layer of a stamped part according to some embodiments of the present disclosure. DETAILED DESCRIPTION
[0017] The present disclosure will be described in detail below in conjunction with specific embodiments and examples, and the advantages and various effects of the present disclosure will be more clearly presented. It should be understood by those skilled in the art that these specific embodiments and examples are used to illustrate the present disclosure, rather than to limit the present disclosure.
[0018] Throughout the specification, unless otherwise specified, the terms used herein should be understood as having the meaning commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as generally understood by those skilled in the art to which the present disclosure belongs. In the event of a conflict, the present specification takes precedence. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present disclosure. For example, room temperature may refer to a temperature in the range of 10°C to 35°C.
[0019] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present disclosure can be purchased from the market or prepared by existing methods.
[0020] The technical solution of the embodiments of the present disclosure is to solve the above technical problems, and the overall idea is as follows:
[0021] According to a typical embodiment of the present disclosure, a stamping steel plate is provided, wherein the chemical composition of the steel in the stamping steel plate comprises, in percentage by mass:
[0022] C and Si: ≤0.5%, Al: ≤0.06%, Cr: 0.1%-0.7%, Mo: ≤0.7%, B: 0.001%-0.005%, P: ≤0.01%, S: ≤0.005%, N: ≤0.01%, O: ≤0.003%;
[0023] Among them, when 0.17%≤C<0.23%, Mn is 2.0%-3.0%; when 0.23%≤C<0.29%, Mn is 1.8%-2.5%; when 0.29%≤C<0.33%, Mn is 1.6%-2.0%; when 0.33%≤C<0.40%, Mn is 1.2%-1.8%.
[0024] The stamping steel plate provided in the embodiment of the present disclosure is designed with a specific chemical composition and increases the Mn content to expand the austenitizing temperature range, which can effectively reduce the hot stamping deformation temperature, thereby alleviating the problem of liquid metal embrittlement, improving strength, and reducing the risk of cracking.
[0025] According to a typical embodiment of the present disclosure, a stamping steel plate is provided, wherein the chemical composition of the steel in the stamping steel plate comprises, in percentage by mass:
[0026] C, Mn and Si: ≤0.5%, Al: ≤0.06%, Cr: 0.1%-0.7%, Mo: ≤0.7%, B: 0.001%-0.005%, P: ≤0.01%, S: ≤0.005%, N: ≤0.01%, O: ≤0.003%;
[0027] Among them, when 0.17%≤C<0.23%, Mn is 2.0%-3.0%; when 0.23%≤C<0.29%, Mn is 1.8%-2.5%; when 0.29%≤C<0.33%, Mn is 1.6%-2.0%; when 0.33%≤C<0.40%, Mn is 1.2%-1.8%.
[0028] The stamping steel plate provided in the embodiment of the present disclosure is designed with a specific chemical composition and increases the Mn content to expand the austenitizing temperature range, which can effectively reduce the hot stamping deformation temperature, thereby alleviating the problem of liquid metal embrittlement, improving strength, and reducing the risk of cracking.
[0029] The stamping steel plate of the embodiment of the present disclosure can obtain fine martensite, and may also contain a small amount of bainite and ferrite. Its tensile strength is at least greater than 1300MPa, and can even reach 2000MPa; the elongation at break is greater than or equal to 4%, so that the hot stamping steel plate has good strength and plasticity.
[0030] Compared with the traditional method of hot stamping steel plates, which requires two hot stamping processes to reduce the embrittlement of liquid metal, the process of obtaining a complex phase structure of the stamping steel plate disclosed in the present invention is simple and does not require changing the existing hot stamping treatment process. Stamping parts can be obtained through a single hot stamping at a relatively low stamping temperature, which has broad prospects for practical industrial applications.
[0031] The functions and limited ranges of the above main alloying elements are detailed as follows:
[0032] C: In the present disclosure, C is the most effective and cheapest solid solution strengthening element, which can effectively ensure the strength level of the stamping steel plate; at the same time, C is an austenite stabilizing element and can most effectively stabilize austenite.
[0033] Mn: Mn is used to increase the austenite region, reduce the austenitizing temperature, improve hardenability, and reduce the stamping temperature.
[0034] Si: Si is a ferrite-forming element. When the stamping steel sheet is heated to the austenite (γ) zone and held at this temperature, Si atoms dissolve in the ferrite. The dissolution of Si in ferrite increases the activity of carbon atoms, promoting outward diffusion of carbon atoms from the ferrite, and increasing the carbon content in the surrounding austenite. As the carbon content in austenite increases, its stability also increases. During the cooling process, Si inhibits the precipitation of carbides, ensuring a certain amount of retained austenite in the structure. Therefore, the Si content is controlled to ≤0.5%.
[0035] Cr: Cr can significantly increase hardenability and reduce severe oxidation on the surface at high temperatures, but it promotes the formation of bainite and should not be too high. Therefore, the Cr content is controlled at 0.1%-0.7%.
[0036] Mo: Mo can refine the grain size of steel and improve hardenability. Considering the cost of Mo, the Mo content is controlled to ≤0.7%.
[0037] B: A small amount of B ensures sufficiently good hardenability, so the B content is controlled at 0.001%-0.005%.
[0038] P: P is easy to form micro segregation during the solidification of molten steel, and then segregates to the grain boundaries when heated to the post-austenite temperature, which significantly increases the brittleness of the steel and thus increases the sensitivity to hydrogen-induced delayed fracture. Therefore, the P content should be controlled below 0.01%.
[0039] S: S is an unavoidable impurity. The formation of MnS inclusions and segregation at grain boundaries will deteriorate the toughness of steel, thereby reducing the toughness and ductility of steel and increasing the sensitivity to hydrogen-induced delayed fracture. Therefore, the S content should be controlled below 0.005%.
[0040] N: N combines with Al, Ti, Nb, V, etc. to form compounds, thereby refining grains and reducing hydrogen-induced delayed fracture sensitivity. However, it also segregates at grain boundaries, reducing grain boundary strength. Therefore, the N content should be controlled at ≤0.01%.
[0041] Oxygen is a harmful gas that affects hydrogen-induced delayed fracture sensitivity and may form coarse alumina inclusions with aluminum, deteriorating the toughness of the steel. The O content should be controlled below 0.003% through various means.
[0042] It should be noted that the reason for controlling the relative ratio of C content to Mn content is to control the temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling to below 700°C so that a fully martensitic structure can be obtained when stamping at below 700°C.
[0043] As an optional embodiment, the temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is ≤650°C, and the critical cooling rate (Vc) of martensite of the stamping steel plate is ≤20°C / s.
[0044] In some embodiments, by controlling the temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling to ≤650°C, it can be ensured that a fully martensitic structure can be obtained when stamping at a temperature below 700°C. The hot stamping temperature of the stamping steel plate with a martensitic structure is further reduced, which can alleviate or avoid the occurrence of liquid metal embrittlement problems to a certain extent, thereby achieving the purpose of improving the strength of the stamping steel plate and reducing the risk of cracking.
[0045] In some embodiments, the empirical calculation formula for the temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of a stamping steel sheet is as follows:
[0046] Ar3=833.6-190C-102Mn, where the element symbol represents the mass percentage of the corresponding element.
[0047] In some embodiments, the critical cooling rate of martensite (Vc) is the minimum cooling rate for obtaining a complete martensite structure. Through specific chemical composition design, the critical cooling rate of martensite (Vc) of the stamping steel plate can be made ≤20°C / s. Furthermore, when the stamping steel plate is pre-cooled before hot stamping, the pre-cooling cooling rate can be controlled to obtain a more ideal martensite content and microstructure of the stamping steel plate, thereby improving the hardness, strength and wear resistance of the stamping steel plate.
[0048] As an optional embodiment, the chemical composition of the steel further includes, by mass percentage, any one or more combinations of: Ti: 0.02%-0.15%, Nb: 0.02%-0.15%, and V: 0.02%-0.15%, with the remainder being Fe and unavoidable impurities.
[0049] The functions and limited ranges of the above main alloying elements are detailed as follows:
[0050] Nb, Ti, V combine with C and N to form precipitates, which are mainly used to refine austenite grains.
[0051] As an optional embodiment, the metallographic structure of the stamping steel plate includes ferrite, pearlite, bainite and martensite.
[0052] In some embodiments, by controlling the metallographic structure of the stamping steel sheet to include ferrite, pearlite, bainite, and martensite, a complex phase structure can be formed before stamping, which is beneficial for uncoiling, leveling, and blanking.
[0053] According to another typical embodiment of the present disclosure, a method for preparing the above-mentioned stamping steel plate is provided, comprising the following steps:
[0054] S1. After smelting and casting, a steel billet with chemical composition is obtained;
[0055] S2, subjecting the steel billet to a first heating, hot rolling, pickling and cold rolling to obtain a steel strip; and
[0056] S3. The steel strip is subjected to hot-dip galvanizing annealing, skin-passing, and tensioning to obtain a stamping steel sheet. The first heating end temperature is 1100°C-1280°C; the hot rolling finish temperature is 750°C-920°C; the hot rolling coiling temperature is 500°C-700°C; the total cold rolling reduction is 30%-80%; the hot-dip galvanizing annealing temperature is 400°C-600°C; the coating thickness formed by the hot-dip galvanizing annealing is 20g / m 2 -300g / m 2 .
[0057] According to another typical embodiment of the present disclosure, a stamping part is provided, which is made of any of the above-mentioned stamping steel plates.
[0058] In some embodiments, stamping parts made from the above-mentioned stamping steel plate can simultaneously meet the requirements of high corrosion resistance and high resistance to state metal (zinc) induced brittle cracking (LME) performance.
[0059] As an optional embodiment, the metallographic structure of the stamping part includes, by volume percentage, ferrite 0-5%, austenite 0-10%, bainite 0-10%, and the remainder martensite.
[0060] As an optional embodiment, the metallographic structure of the stamping part includes, by volume percentage, 0-5% ferrite, 0-5% austenite, 0-5% bainite, and the remainder martensite.
[0061] According to another typical embodiment of the present disclosure, a method for preparing the above-mentioned stamping part is provided, comprising the following steps:
[0062] S4, blanking the stamping steel plate to obtain a blank;
[0063] S5, subjecting the sheet to a second heating and heat preservation step to obtain a preheated sheet; and
[0064] S6. Precooling, hot stamping and quenching the preheated sheet to obtain a stamped part.
[0065] In order to ensure the high strength of the stamping parts disclosed in the present invention, the matrix structure of the stamping parts is mainly a fine lath martensite structure containing high-thickness dislocations, supplemented by a bainite structure and a residual austenite structure. The original austenite grain size is controlled by hot rolling in the austenite region and adding Nb, Ti, V, etc., and the martensite size and lath spacing are refined by refining the original austenite grain size. Secondly, the residual austenite between the martensite laths is obtained by controlling the mold opening temperature after hot forming, increasing the C partitioning time, and adding Si and Al elements. Finally, a multiphase composite structure of fine dislocation martensite, a small amount of bainite and ferrite is obtained. Its high strength is due to the fine grain strengthening and dislocation strengthening of martensite and multiphase structure, and its plasticity improvement comes from the small amount of bainite and ferrite present in the structure. At the same time, grain refinement and coordinated deformation of multiple phases also help to improve plasticity.
[0066] In some embodiments, unlike the traditional hot stamping process, the sheet needs to be pre-cooled before hot stamping, that is, before entering the press, to ensure that the sheet's mold entry temperature is low during hot stamping, so as to avoid liquid metal embrittlement defects caused by excessively high hot stamping temperatures and reduce the risk of brittle cracking of stamped parts.
[0067] In some embodiments, the blank may be temperature-tested before hot stamping to ensure that the blank has a low die entry temperature during hot stamping.
[0068] As an optional implementation manner, the second heating temperature is 800° C.-1000° C., and the insulation time is 3 min-10 min.
[0069] In some embodiments, by controlling the second heating temperature to 800°C-1000°C, on the one hand, it is possible to avoid the risk of incomplete austenitization due to slow heating speed at temperatures below 800°C; on the other hand, it is possible to avoid the risk of reduced corrosion resistance due to excessive Fe content in the galvanized layer caused by rapid evaporation of the Zn layer at temperatures above 1000°C.
[0070] As an optional implementation manner, the cooling rate of the precooling is greater than 10°C / s, and the terminal temperature of the precooling is ≤700°C.
[0071] In some embodiments, the sheet needs to be pre-cooled before hot stamping, that is, before entering the press, so that the end temperature of the pre-cooling is ≤700°C, so as to ensure that the entering mold temperature of the sheet during hot stamping is lower than 700°C, thereby avoiding liquid metal embrittlement defects caused by excessively high hot stamping temperatures, and thereby reducing the risk of brittle cracking of stamped parts.
[0072] In some embodiments, the cooling rate of the pre-cooling is controlled to be higher than 10° C. / s to avoid ferrite transformation that may cause low strength when the cooling rate is lower than 10° C. / s.
[0073] As an optional embodiment, the cooling rate of the pre-cooling is greater than 15° C. / s. Alternatively, the cooling rate of the pre-cooling is greater than 20° C. / s.
[0074] In some embodiments, by controlling the cooling rate of pre-cooling to be higher than 15°C / s or even higher than 20°C / s, it is possible to ensure that the cooling rate of pre-cooling is higher than the critical cooling rate of martensite (Vc), so that the stamping steel plate can obtain a more ideal martensite content and microstructure, thereby improving the hardness, strength and wear resistance of the stamping steel plate.
[0075] In some embodiments, to ensure that the initial temperature of the sheet during hot stamping is below 700°C and to ensure the speed of pre-cooling before hot stamping, a gaseous cooling medium and / or a liquid cooling medium may be used during pre-cooling. When the cooling medium is a gas, pre-cooling may be performed by jetting; when the cooling medium is a liquid, pre-cooling may be performed by spraying.
[0076] As an optional embodiment, the pre-cooling cooling medium is an alkaline aqueous solution.
[0077] In some embodiments, the alkaline aqueous solution can increase the boiling point of the cooling medium to a certain extent.
[0078] In some embodiments, the amount of cooling medium is calculated as follows: m V m (T i -T f )=C s V s (T si -T sf )
[0079] Among them, C m is the specific heat capacity of the cooling medium, V m is the volume of cooling medium, T i is the end temperature of the cooling medium, T f is the initial temperature of the cooling medium; C s is the specific heat capacity of the sheet, V s is the volume of the sheet, T si is the initial temperature of the sheet precooling, T sf is the average temperature of the sheet after pre-cooling, and the unit of temperature mentioned in the formula is ℃.
[0080] In some embodiments, the amount of cooling medium is calculated as follows: m V m (T i -T f )=C s V s (782-Tsf )
[0081] In this embodiment, the initial temperature of the web pre-cooling is 782 degrees Celsius.
[0082] As an optional embodiment, the end temperature of the pre-cooling is 560°C-680°C.
[0083] In some embodiments, by controlling the end temperature of pre-cooling to 560°C-680°C, it is possible to ensure that the mold entry temperature of the sheet during hot stamping is low to avoid liquid metal embrittlement defects, and to avoid defects during hot stamping of the sheet due to the mold entry temperature being too low, which is not conducive to forming, thereby reducing the risk of cracking caused by forming defects.
[0084] The present disclosure will be described in detail below with reference to examples, comparative examples and experimental data.
[0085] Example 1
[0086] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate comprises, by mass percentage, C: 0.20%, Mn: 2.1%, Si: 0.3%, Al: 0.049%, Cr: 0.2%, Mo: 0.002%, B: 0.003%, P: 0.01%, S: 0.003%, N: 0.004%, Ti: 0.035%, Nb: 0.03%, V: 0%, and the balance is Fe and unavoidable impurities.
[0087] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=581°C, the critical cooling rate (Vc) of martensite is 20°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0088] The method for preparing the stamping steel plate comprises the following steps:
[0089] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0090] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1230°C; the hot rolling finish temperature is 900°C; the hot rolling coiling temperature is 570°C; and the total cold rolling reduction is 60%.
[0091] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 430℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0092] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0093] The metallographic structure of the stamping parts includes, by volume percentage, 3% ferrite, 2% bainite, and the remainder martensite.
[0094] The method for preparing the stamping part comprises the following steps:
[0095] S4. Blanking the stamping steel plate to obtain a blank.
[0096] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0097] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 680°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 700°C.
[0098] Example 2
[0099] A stamping steel plate, wherein the chemical composition of the steel in the stamping steel plate comprises, by mass percentage:
[0100] C: 0.22%, Mn: 2.2%, Si: 0.3%, Al: 0.049%, Cr: 0.18%, Mo: 0.002%, B: 0.003%, P: 0.01%, S: 0.003%, N: 0.004%, Ti: 0.03%, Nb: 0.04%, V: 0.02%, and the balance is Fe and inevitable impurities.
[0101] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=567.4°C, the critical cooling rate (Vc) of martensite is 15°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0102] The method for preparing the stamping steel plate comprises the following steps:
[0103] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0104] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1250°C; the hot rolling finish temperature is 900°C; the hot rolling coiling temperature is 560°C; and the total cold rolling reduction is 65%.
[0105] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 430℃; the hot-dip galvanizing coating thickness is 120g / m 2 .
[0106] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0107] The metallographic structure of the stamping parts includes, by volume percentage, ferrite 2%, bainite 1%, and the balance martensite.
[0108] The method for preparing the stamping part comprises the following steps:
[0109] S4. Blanking the stamping steel plate to obtain a blank.
[0110] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0111] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 660°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 680°C.
[0112] Example 3
[0113] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate comprises, by mass percentage, C: 0.26%, Mn: 1.9%, Si: 0.2%, Al: 0.049%, Cr: 0.22%, Mo: 0.002%, B: 0.003%, P: 0.01%, S: 0.003%, N: 0.0041%, Ti: 0.03%, Nb: 0.03%, V: 0.03%, and the balance is Fe and unavoidable impurities.
[0114] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=590.4°C, the critical cooling rate (Vc) of martensite is 15°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0115] The method for preparing the stamping steel plate comprises the following steps:
[0116] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0117] S2. The steel billet is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 570°C; and the total cold rolling reduction is 60%.
[0118] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 430℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0119] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0120] The metallographic structure of the stamping parts includes, by volume percentage, ferrite 2%, bainite 3%, and the balance martensite.
[0121] The method for preparing the stamping part comprises the following steps:
[0122] S4. Blanking the stamping steel plate to obtain a blank.
[0123] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0124] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 680°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 700°C.
[0125] Example 4
[0126] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate comprises, by mass percentage, C: 0.30%, Mn: 1.7%, Si: 0.2%, Al: 0.049%, Cr: 0.18%, Mo: 0.002%, B: 0.0027%, P: 0.01%, S: 0.003%, N: 0.0041%, Ti: 0.03%, Nb: 0.03%, V: 0.03%, and the balance is Fe and unavoidable impurities.
[0127] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=603.2°C, the critical cooling rate (Vc) of martensite is 10°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0128] The method for preparing the stamping steel plate comprises the following steps:
[0129] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0130] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1210°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 550°C; and the total cold rolling reduction is 40%.
[0131] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain a stamping steel sheet. The hot-dip galvanizing annealing temperature is 430°C; the hot-dip galvanizing coating thickness is 100g / m 2 .
[0132] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0133] The metallographic structure of the stamping parts includes, by volume percentage, 2% austenite, 3% bainite, and the remainder martensite.
[0134] The method for preparing the stamping part comprises the following steps:
[0135] S4. Blanking the stamping steel plate to obtain a blank.
[0136] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0137] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 650°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 660°C.
[0138] Example 5
[0139] A steel plate for stamping, the chemical composition of the steel plate for stamping including, by mass percentage, C: 0.33%, Mn: 1.6%, Si: 0.2%, Al: 0.03%, Cr: 0.18%, Mo: 0.10%, B: 0.0022%, P: 0.01%, S: 0.003%, N: 0.0041%, Ti: 0.03%, Nb: 0.02%, V: 0.10%, and the balance being Fe and unavoidable impurities.
[0140] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=607.7°C, the critical cooling rate (Vc) of martensite is 10°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0141] The method for preparing the stamping steel plate comprises the following steps:
[0142] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0143] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1250°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 600°C; and the total cold rolling reduction is 50%.
[0144] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 450℃; the hot-dip galvanizing coating thickness is 160g / m 2 .
[0145] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0146] The metallographic structure of the stamping parts includes, by volume percentage, 2% austenite, 2% bainite, and the remainder martensite.
[0147] The method for preparing the stamping part comprises the following steps:
[0148] S4. Blanking the stamping steel plate to obtain a blank.
[0149] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0150] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 680°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 700°C.
[0151] Example 6
[0152] A steel plate for stamping, the chemical composition of the steel plate for stamping including, by mass percentage, C: 0.33%, Mn: 1.6%, Si: 0.2%, Al: 0.03%, Cr: 0.18%, Mo: 0.10%, B: 0.0022%, P: 0.01%, S: 0.003%, N: 0.0041%, Ti: 0.03%, Nb: 0.02%, V: 0.10%, and the balance being Fe and unavoidable impurities.
[0153] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=607.7°C, the critical cooling rate (Vc) of martensite is 10°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0154] The method for preparing the stamping steel plate comprises the following steps:
[0155] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0156] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1250°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 600°C; and the total cold rolling reduction is 50%.
[0157] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 450℃; the hot-dip galvanizing coating thickness is 160g / m 2 .
[0158] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0159] The metallographic structure of the stamping parts includes, by volume percentage, 1% austenite, 4% bainite, and the remainder martensite.
[0160] The method for preparing the stamping part comprises the following steps:
[0161] S4. Blanking the stamping steel plate to obtain a blank.
[0162] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0163] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 680°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 700°C.
[0164] Example 7
[0165] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate comprises, by mass percentage, C: 0.35%, Mn: 1.4%, Si: 0.22%, Al: 0.03%, Cr: 0.18%, Mo: 0.12%, B: 0.0023%, P: 0.009%, S: 0.002%, N: 0.004%, Ti: 0.03%, Nb: 0.04%, V: 0.11%, and the balance is Fe and unavoidable impurities.
[0166] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=624.3°C, the critical cooling rate (Vc) of martensite is 10°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0167] The method for preparing the stamping steel plate comprises the following steps:
[0168] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0169] S2. The steel billet is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 620°C; and the total cold rolling reduction is 50%.
[0170] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 445℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0171] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0172] The metallographic structure of the stamping parts includes, by volume percentage, 2% austenite, 2% bainite, and the remainder martensite.
[0173] The method for preparing the stamping part comprises the following steps:
[0174] S4. Blanking the stamping steel plate to obtain a blank.
[0175] S5, subjecting the sheet to a second heating and heat preservation process to obtain a preheated sheet, wherein the second heating temperature is 900° C. and the heat preservation time is 5 minutes.
[0176] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping forming temperature is 640°C, the pre-cooling rate is 20°C / s, and the end temperature of the pre-cooling is 650°C.
[0177] Comparative Example 1
[0178] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate includes, by mass percentage, C: 0.23%, Mn: 1.23%, Si: 0.22%, Al: 0.043%, Cr: 0.18%, Mo: 0%, B: 0.003%, P: 0.009%, S: 0.002%, N: 0.004%, Ti: 0.03%, and the balance is Fe and unavoidable impurities.
[0179] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel sheet is 833.6-190C-102Mn=664.4°C, the critical cooling rate (Vc) of martensite is 25°C / s, and its metallographic structure includes bainite and martensite.
[0180] The method for preparing the stamping steel plate comprises the following steps:
[0181] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0182] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 620°C; and the total cold rolling reduction is 60%.
[0183] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 435℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0184] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0185] The metallographic structure of the stamping part includes, by volume percentage, 2% bainite and the remainder martensite.
[0186] The method for preparing the stamping part comprises the following steps:
[0187] S4. Blanking the stamping steel plate to obtain a blank.
[0188] S5, subjecting the sheet to a second heating and heat preservation step to obtain a preheated sheet, wherein the second heating temperature is 930° C. and the heat preservation time is 5 minutes.
[0189] S6. Precooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping temperature is 720° C. without precooling.
[0190] Comparative Example 2
[0191] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate comprises, by mass percentage, C: 0.23%, Mn: 1.23%, Si: 0.22%, Al: 0.043%, Cr: 0.18%, Mo: 0%, B: 0.003%, P: 0.009%, S: 0.002%, N: 0.004%, Ti: 0.03%, and the balance is Fe and unavoidable impurities.
[0192] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel sheet is 833.6-190C-102Mn=664.4°C, the critical cooling rate (Vc) of martensite is 25°C / s, and its metallographic structure includes bainite and martensite.
[0193] The method for preparing the stamping steel plate comprises the following steps:
[0194] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0195] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 620°C; and the total cold rolling reduction is 60%.
[0196] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 435℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0197] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0198] The metallographic structure of the stamping part includes, by volume percentage, 2% bainite and the remainder martensite.
[0199] The method for preparing the stamping part comprises the following steps:
[0200] S4. Blanking the stamping steel plate to obtain a blank.
[0201] S5, subjecting the sheet to a second heating and heat preservation step to obtain a preheated sheet, wherein the second heating temperature is 930° C. and the heat preservation time is 5 minutes.
[0202] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping temperature is 780° C. without pre-cooling.
[0203] Comparative Example 3
[0204] A steel plate for stamping, wherein the chemical composition of the steel in the steel plate comprises, by mass percentage, C: 0.23%, Mn: 1.23%, Si: 0.22%, Al: 0.043%, Cr: 0.18%, Mo: 0%, B: 0.003%, P: 0.009%, S: 0.002%, N: 0.004%, Ti: 0.03%, and the balance is Fe and unavoidable impurities.
[0205] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel plate is 833.6-190C-102Mn=664.4°C, the critical cooling rate (Vc) of martensite is 25°C / s, and its metallographic structure includes ferrite, bainite and martensite.
[0206] The method for preparing the stamping steel plate comprises the following steps:
[0207] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0208] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 620°C; and the total cold rolling reduction is 60%.
[0209] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 435℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0210] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0211] The metallographic structure of the stamping parts includes, by volume percentage, ferrite 7%, bainite 6%, and the balance martensite.
[0212] The method for preparing the stamping part comprises the following steps:
[0213] S4. Blanking the stamping steel plate to obtain a blank.
[0214] S5, subjecting the sheet to a second heating and heat preservation step to obtain a preheated sheet, wherein the second heating temperature is 930° C. and the heat preservation time is 5 minutes.
[0215] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping temperature is 630° C. without pre-cooling.
[0216] Comparative Example 4
[0217] A stamping steel plate, the chemical composition of the steel including, by mass percentage:
[0218] C: 0.32%, Mn: 1.33%, Si: 0.22%, Al: 0.043%, Cr: 0.18%, Mo: 0%, B: 0.0028%, P: 0.009%, S: 0.002%, N: 0.004%, Ti: 0.03%, Nb: 0.03%, and the balance is Fe and inevitable impurities.
[0219] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel sheet is 833.6-190C-102Mn=650.4°C, the critical cooling rate (Vc) of martensite is 15°C / s, and its metallographic structure includes bainite and martensite.
[0220] The method for preparing the stamping steel plate comprises the following steps:
[0221] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0222] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 620°C; and the total cold rolling reduction is 60%.
[0223] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 439℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0224] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0225] The metallographic structure of the stamping part includes, by volume percentage, 2% bainite and the remainder martensite.
[0226] The method for preparing the stamping part comprises the following steps:
[0227] S4. Blanking the stamping steel plate to obtain a blank.
[0228] S5, subjecting the sheet to a second heating and heat preservation step to obtain a preheated sheet, wherein the second heating temperature is 930° C. and the heat preservation time is 5 minutes.
[0229] S6. Precooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping temperature is 720° C. without precooling.
[0230] Comparative Example 5
[0231] A stamping steel plate, the chemical composition of the steel including, by mass percentage:
[0232] C: 0.32%, Mn: 1.2%, Si: 0.22%, Al: 0.043%, Cr: 0.18%, Mo: 0%, B: 0.0028%, P: 0.009%, S: 0.002%, N: 0.004%, Ti: 0.03%, Nb: 0.03%, and the balance is Fe and inevitable impurities.
[0233] The temperature (Ar3) at which austenite begins to precipitate free ferrite during cooling of the stamping steel sheet is 833.6-190C-102Mn=650.4°C, the critical cooling rate (Vc) of martensite is 15°C / s, and its metallographic structure includes bainite and martensite.
[0234] The method for preparing the stamping steel plate comprises the following steps:
[0235] S1. After smelting and casting, a steel billet with chemical composition is obtained.
[0236] S2. The steel slab is subjected to a first heating, hot rolling, pickling, and cold rolling to obtain a steel strip. The first heating end temperature is 1220°C; the hot rolling finish temperature is 910°C; the hot rolling coiling temperature is 620°C; and the total cold rolling reduction is 60%.
[0237] S3, the steel strip is subjected to hot-dip galvanizing annealing, skin-passing and straightening to obtain stamping steel sheet. The hot-dip galvanizing annealing temperature is 439℃; the hot-dip galvanizing coating thickness is 140g / m 2 .
[0238] A stamping part is prepared by using the above-mentioned stamping steel plate.
[0239] The metallographic structure of the stamping part includes, by volume percentage, 2% bainite and the remainder martensite.
[0240] The method for preparing the stamping part comprises the following steps:
[0241] S4. Blanking the stamping steel plate to obtain a blank.
[0242] S5, subjecting the sheet to a second heating and heat preservation step to obtain a preheated sheet, wherein the second heating temperature is 930° C. and the heat preservation time is 5 minutes.
[0243] S6. Pre-cooling, hot stamping, and quenching the preheated blank to obtain a stamped part, wherein the hot stamping temperature is 780° C. without pre-cooling.
[0244] The performance of the stamping steel plates provided in Examples 1-6 and Comparative Examples 1-5 was tested, and the performance test results are shown in Table 1.
[0245] Table 1
[0246] It can be seen from the above table:
[0247] The mechanical properties of the stamping steel provided in Examples 1-5 and 7 are significantly better than those in Comparative Examples 1, 2 and 4, and the crack depth is significantly reduced. Therefore, the stamping steel provided in the present disclosure can effectively solve the technical problem in the prior art of reduced strength of stamping steel plates due to embrittlement of liquid metal.
[0248] Explanation of the accompanying drawings:
[0249] FIG2 is a metallographic structure diagram of a stamping steel plate provided in an embodiment of the present disclosure. As can be seen from FIG2 , the matrix martensite content reaches more than 95%.
[0250] FIG3 is an SEM image of the coating of the stamping part provided in the embodiment of the present disclosure. As can be seen from FIG3 , the crack depth is well controlled.
[0251] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements, but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0252] Although some embodiments of the present disclosure have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the above embodiments and all changes and modifications that fall within the scope of the present disclosure.
[0253] Obviously, those skilled in the art may make various changes and modifications to the present disclosure without departing from the spirit and scope of the present disclosure. Thus, if these modifications and variations of the present disclosure fall within the scope of the claims of the present disclosure and their equivalents, the present disclosure is intended to include these modifications and variations.
Claims
1. A stamping steel sheet, wherein the chemical composition of the steel in the stamping steel sheet comprises the following components by mass percentage: C and Si: ≤0.5%, Al: ≤0.06%, Cr: 0.1%-0.7%, Mo: ≤0.7%, B: 0.001%-0.005%, P: ≤0.01%, S: ≤0.005%, N: ≤0.01%, O: ≤0.003%; in: When 0.17%≤C<0.23%, Mn is 2.0%-3.0%; When 0.23%≤C<0.29%, Mn is 1.8%-2.5%; When 0.29%≤C<0.33%, Mn is 1.6%-2.0%; When 0.33%≤C<0.40%, Mn is 1.2%-1.8%.
2. The stamping steel sheet according to claim 1, wherein: The chemical composition of the steel in the stamping steel plate includes the following components by mass percentage: C, Mn and Si: ≤0.5%, Al: ≤0.06%, Cr: 0.1%-0.7%, Mo: ≤0.7%, B: 0.001%-0.005%, P: ≤0.01%, S: ≤0.005%, N: ≤0.01%, O: ≤0.003%; in: When 0.17%≤C<0.23%, Mn is 2.0%-3.0%; When 0.23%≤C<0.29%, Mn is 1.8%-2.5%; When 0.29%≤C<0.33%, Mn is 1.6%-2.0%; When 0.33%≤C<0.40%, Mn is 1.2%-1.8%.
3. The stamping steel sheet according to claim 1, wherein: When the stamping steel sheet is cooled, the temperature (Ar3) at which austenite starts to precipitate free ferrite is ≤650°C, and the critical cooling rate (Vc) of martensite of the stamping steel sheet is ≤20°C / s.
4. [Corrected 18.12.2023 according to Rule 91] A steel sheet for stamping according to claim 1, wherein: The chemical composition of the steel further comprises, by mass percentage, any one or more combinations of Ti: 0.02%-0.15%, Nb: 0.02%-0.15% and V: 0.02%-0.15%, with the remainder being Fe and unavoidable impurities.
5. The stamping steel sheet according to any one of claims 1 to 4, wherein: The metallographic structure of the stamping steel plate includes ferrite, pearlite, bainite and martensite.
6. A method for preparing a stamping steel plate according to any one of claims 1 to 5, comprising the following steps: After smelting and casting, a steel billet having the chemical composition is obtained; The steel billet is first heated, hot rolled, pickled and cold rolled to obtain a steel strip; The steel strip is subjected to hot-dip galvanizing annealing, skin-passing and tensioning to obtain the stamping steel plate; in: The end temperature of the first heating is 1100°C-1280°C; The final rolling temperature of the hot rolling is 750°C-920°C; The hot rolling coiling temperature is 500°C-700°C; The total reduction rate of the cold rolling is 30%-80%; The temperature of the hot-dip galvanizing annealing is 400°C-600°C; The coating thickness formed by hot-dip galvanizing annealing is 20 g / m 2 -300g / m 2 .
7. A stamping part made from the stamping steel plate according to any one of claims 1 to 5.
8. The stamping part according to claim 7, wherein: The metallographic structure of the stamping part includes, by volume percentage, ferrite 0-5%, austenite 0-10%, bainite 0-10%, and the remainder martensite.
9. The stamping part according to claim 8, wherein: The metallographic structure of the stamping part includes, by volume percentage, 0-5% ferrite, 0-5% austenite, 0-5% bainite, and the remainder is martensite.
10. A method for preparing a stamping part according to any one of claims 7 to 9, comprising the following steps: Blanking the stamping steel plate to obtain a blank; The sheet is subjected to a second heating and heat preservation to obtain a preheated sheet; The preheated sheet is precooled, hot stamped and quenched to obtain the stamped part.
11. The method for preparing a stamping part according to claim 10, wherein: The second heating temperature is 800° C.-1000° C., and the insulation time is 3 min-10 min.
12. The method for preparing a stamping part according to claim 10, wherein: The cooling rate of the precooling is greater than 10°C / s, and the terminal temperature of the precooling is less than or equal to 700°C.
13. The method for preparing a stamping part according to claim 12, wherein: The cooling rate of the precooling is >20°C / s.
14. The method for preparing a stamping part according to claim 12, wherein: The precooling cooling medium is an alkaline aqueous solution.
15. The method for preparing a stamping part according to claim 12, wherein: The end point temperature of the precooling is 560°C-680°C.
Citation Information
Patent Citations
Hot stamping steel coated with zinc-base clad layer and preparing method of steel
CN111020124A
Galvanized sheet hot forming method capable of reducing cost and improving production efficiency
CN114260350A
Hot press molded body
CN115298344A
Preparation method of zinc-based alloy coating hot stamping forming steel
CN115958059A
Steel plate for stamping, preparation method of steel plate, stamping part and preparation method of stamping part
CN116623100A