Ba- and b-doped fischer-tropsch synthesis iron-based catalyst and preparation method therefor

By doping Ba and B elements into the Fischer-Tropsch synthesis iron-based catalyst, the problem of insufficient thermal stability of the catalyst is solved, and the catalyst's high activity and low selectivity are achieved, making it suitable for industrial applications.

WO2024221883A1PCT designated stage expired Publication Date: 2024-10-31CHINA ENERGY INVESTMENT CORP LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/133696
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-11-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing iron-based catalysts for Fischer-Tropsch synthesis have insufficient thermal stability in high-temperature reactions, resulting in reduced catalyst activity and sintering problems. Existing methods such as adding SiO2 and structural additives cannot effectively solve the thermal stability problem.

Method used

By doping Ba and B elements, a Ba and B-doped Fischer-Tropsch synthesis iron-based catalyst is formed. The heat resistance of Ba and the synergistic effect of B are used to improve the thermal and chemical stability of the catalyst and avoid Fe grain sintering. , and control the content and distribution of Ba and B to ensure high activity and low selectivity of the catalyst.

Benefits of technology

It significantly improves the thermal stability and catalytic activity of the catalyst, reduces the selectivity of CO2 and CH4, extends the service life of the catalyst, and simplifies the preparation process, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023133696-FTAPPB-I100001
    Figure PCTCN2023133696-FTAPPB-I100001
  • Figure PCTCN2023133696-FTAPPB-I100002
    Figure PCTCN2023133696-FTAPPB-I100002
  • Figure 00000022_0000
    Figure 00000022_0000
Patent Text Reader

Abstract

The present invention provides a Ba- and B-doped Fischer-Tropsch synthesis iron-based catalyst, which comprises an element Fe, an element Cu, an element K, and SiO2. The Fischer-Tropsch synthesis iron-based catalyst is doped with the element Ba and the element B. In percentage by mass, when the ratio of the element Fe to SiO2 is from 100:10 to 100:(less than 20), the ratio of the element Ba to the element B is from 1:1 to (less than 4):1; and when the ratio of the element Fe to SiO2 is from 100:20 to 100:40, the ratio of the element Ba to the element B is from 4:1 to 6:1. The present invention further provides a preparation method for the Fischer-Tropsch synthesis iron-based catalyst. The Fischer-Tropsch synthesis iron-based catalyst provided by the present invention is doped with the element Ba and the element B which have specific contents; by means of the cooperation of the element Ba and the element B, the catalyst has excellent catalytic activity and thermal stability; the application of the catalyst can significantly improve the production efficiency of the Fischer-Tropsch synthesis process, and reduce the production costs, and therefore, the Fischer-Tropsch synthesis iron-based catalyst has very important economic and social values.
Need to check novelty before this filing date? Find Prior Art

Description

A Ba and B doped Fischer-Tropsch synthesis iron-based catalyst and preparation method thereof Technical Field

[0001] The present invention relates to the field of Fischer-Tropsch synthesis, and in particular to a Ba- and B-doped Fischer-Tropsch synthesis iron-based catalyst and a preparation method thereof. Background Art

[0002] The Fischer-Tropsch synthesis (FTS) reaction, under appropriate temperature, pressure, and catalyst conditions, can synthesize hydrocarbons of varying carbon numbers from CO and H₂. These products can then be processed to produce fuels and chemicals. Therefore, FTS can be used to convert coal, natural gas, biomass, and other energy sources into syngas-to-liquids. FTS technology is divided into high-temperature and low-temperature technologies. High-temperature FTS operates at temperatures above 300°C, typically using a fluidized bed reactor and a molten iron catalyst. The products are primarily olefins and oxygenates. Low-temperature FTS operates at temperatures below 280°C, typically using a fixed bed or slurry bed reactor, using either a precipitated iron catalyst (suitable for reaction temperatures between 250-280°C) or a supported cobalt catalyst (suitable for reaction temperatures between 200-230°C). The products are primarily diesel and wax. Cobalt-based and iron-based catalysts differ in their active phase structures and primary and secondary reaction pathways, resulting in distinct formulations and preparation methods. Iron-based catalysts with iron as the active component are more suitable for large-scale industrial applications due to their low price, strong resistance to poisoning, and high content of linear α-olefins in the product.

[0003] Iron-based catalysts prepared by precipitation methods have small crystals and numerous active sites, but these small crystals are prone to sintering. Furthermore, Fischer-Tropsch synthesis is a highly exothermic reaction, with intense exothermic hot spots at the catalyst's active sites. Therefore, high thermal stability is required for the catalyst. Otherwise, the catalyst is prone to sintering or fragmentation due to the heat of reaction, resulting in a decrease in catalyst performance. Therefore, developing iron-based catalysts with both high activity and high thermal stability is a key research and development direction for slurry-bed Fischer-Tropsch synthesis technology.

[0004] Commonly used methods to improve catalyst stability include: (1) adding binders (such as SiO2) to disperse and bond iron grains, (2) improving the preparation process (such as through heat treatment) to improve particle strength and inhibit breakage; (3) adding structural additives (such as Ti, Zr) to improve particle strength. Among them, adding binders is the most effective method to improve the mechanical strength of catalysts. At present, almost all Fischer-Tropsch synthesis iron-based catalysts contain SiO2 binders. Although the addition of silicon plays a role in separating and bonding the active particles of the catalyst to avoid sintering of the active phase of the catalyst, it is not a good solution to the problem of thermal stability of the catalyst because silicon is a poor thermal conductor and silicon will also aggregate silicon balls under the action of heat and water vapor, which easily leads to a decrease in catalyst strength. Therefore, it cannot effectively solve the problem of thermal stability of the catalyst. Some researchers have also improved the mechanical strength of the catalyst by adding structural additives. For example, Chinese patents CN 1245255C, CN 101293206A and CN 101298046A respectively improve the wear resistance of the catalyst by adding zinc, zirconium and titanium additives. However, the above method of suppressing catalyst breakage by increasing catalyst particle strength cannot improve the catalyst's anti-sintering stability under the action of reaction heat, thereby preventing the decrease in catalyst activity caused by iron grain sintering. Therefore, how to improve the thermal stability of iron-based catalysts during the reaction remains an urgent problem to be solved for precipitated iron-based catalysts in Fischer-Tropsch synthesis.

[0005] Chinese patent CN 107913714B discloses an iron-based catalyst for Fischer-Tropsch synthesis, comprising Fe, Cu, Mn, K, SiO2, a first additive, and a second additive, wherein the first additive is selected from one or more of Ca, Sr, and Ba, and the second additive is one or more of La, Ce, Y, and Nd. The patent states that its technical solution provides a catalyst with high stability and low CO2 and CH4 selectivity, and emphasizes that the catalyst within the composition range of the invention can maintain low carbon dioxide selectivity and methane selectivity at high conversion rates under the synergistic effect of rare earth metals, alkaline earth metals, and other additives, and effectively inhibit catalyst deactivation; if only rare earth metals or alkaline earth metal additives are added alone, the above effects cannot be achieved simultaneously. In addition, from the perspective of its preparation method, when the first additive solution is added by impregnation, the precipitated catalyst slurry needs to be dried and calcined before impregnation. The impregnated catalyst needs to be dried and calcined a second time, which makes the preparation process long and costly.

[0006] Chinese patent CN 105478128B discloses an iron-based catalyst for Fischer-Tropsch synthesis with high wear resistance and high reactivity, and its preparation method. The catalyst's main active component is Fe, along with a structural additive M, anti-sintering additives yttrium, boron, and SiO2, and an electronic additive potassium, where M is selected from at least one of the following: Zn, Cr, Mn, Zr, and Cu. The patent states that the introduction of elements such as sintering-resistant boron and yttrium significantly improves the catalyst's mechanical strength and wear resistance during the reaction, significantly reducing the difficulty of filtering the wax product in the reactor, improving the operational stability of the equipment, and reducing operational difficulty. The patent reports low overall catalyst activity and high methane selectivity. Furthermore, the patent does not address the chemical stability of the prepared catalyst.

[0007] Summary of the Invention

[0008] In order to make up for the deficiencies in the prior art, one object of the present invention is to provide a Ba and B-doped Fischer-Tropsch synthesis iron-based catalyst. By doping with specific amounts of Ba and B elements, the obtained Fischer-Tropsch synthesis iron-based catalyst can have excellent catalytic performance and thermal stability, thereby greatly improving the reaction efficiency and extending the service life of the catalyst.

[0009] Another object of the present invention is to provide a method for preparing the Ba and B doped Fischer-Tropsch synthesis iron-based catalyst.

[0010] The first aspect of the present invention provides a Ba and B doped Fischer-Tropsch synthesis iron-based catalyst, which contains Fe element, Cu element, K element and SiO2, wherein the Fischer-Tropsch synthesis iron-based catalyst is doped with Ba element and B element, and by mass ratio, when Fe element:SiO2=100:10~less than 20, Ba element:B element=1~less than 4:1, and when Fe element:SiO2=100:20~40, Ba element:B element=4~6:1.

[0011] Ba element has good heat resistance and thermal conductivity. By utilizing the characteristics of Ba element, the heat resistance and thermal conductivity of the Fischer-Tropsch synthesis iron-based catalyst can be effectively improved, thereby effectively avoiding Fe grain sintering and eliminating thermal stress, and the alkalinity of Ba element also helps the catalyst to suppress the generation of methane (CH4) by-products, thereby improving the C5+ product selectivity of the catalyst. The B element can interact with each component in the Fischer-Tropsch synthesis iron-based catalyst, and the synergistic effect between the active phase and the auxiliary agent in the catalyst can be promoted by the B element, thereby significantly reducing the carbon deposition deactivation of the catalyst during the Fischer-Tropsch reaction, thereby improving the chemical stability of the catalyst. The present invention uniformly dopes a specific amount of Ba element and B element in the Fischer-Tropsch synthesis iron-based catalyst so that it is highly dispersed in Fe grains and SiO2 particles. By two doping elements, the Fe grains can be effectively protected, and Fe sintering and Fe grains are avoided. The particles are combined to form iron silicate species that are difficult to reduce, thereby enabling the resulting catalyst to obtain excellent catalytic activity and thermal stability.

[0012] In the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention, the Ba additive itself has a certain alkalinity, which helps to suppress the generation of methane by-products in the Fischer-Tropsch synthesis reaction, improve the C5+ product selectivity and olefin selectivity, but also improves the selectivity of CO2. The inventors have found that when Ba and B act synergistically, Ba can more effectively play the role of an alkaline earth metal additive, promote the catalyst to improve the degree of reduction carbonization, and at the same time avoid the problem of increased CO2 selectivity caused by strong alkalinity (such as barium oxide and barium hydroxide), thereby enabling the resulting catalyst to have lower CO2 selectivity and CH4 selectivity at the same time, further improving its catalytic performance.

[0013] In some preferred embodiments, the specific surface area of ​​the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may be 100 to 220 m2 / g. In some more preferred embodiments, the specific surface area of ​​the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may be 100 to 200 m2 / g.

[0014] In some preferred embodiments, the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may contain the following components by mass ratio: the Fischer-Tropsch synthesis iron-based catalyst contains the following components by mass ratio: Fe element: SiO2: Cu element: K element: Ba element: B element = 100:10~40:0.2~5:0.5~8:1~10:0.4~2.5.

[0015] A second aspect of the present invention provides a method for preparing the Ba and B doped Fischer-Tropsch synthesis iron-based catalyst, the preparation method comprising the following steps:

[0016] S1: forming a mixed aqueous solution of a water-soluble salt of Fe and a water-soluble salt of Cu, preparing a precipitant solution, and adding 0 to 100 wt % of a silicon source to the precipitant solution;

[0017] S2: contacting the mixed aqueous solution with the precipitant solution to perform a precipitation reaction, and separating the resulting precipitated product after the reaction is completed;

[0018] S3: mixing the precipitated product with the K promoter precursor aqueous solution and the remaining silicon source to form a mixed slurry and performing a slurry treatment to obtain a catalyst precursor slurry; and

[0019] S4: drying and calcining the catalyst precursor slurry;

[0020] The method of adding the Ba element includes: adding a water-soluble salt of Ba to the mixed aqueous solution of step S1, and making the concentration of Ba lower than 2.0g Ba / 100g water; or

[0021] A water-soluble salt of Ba is prepared into an aqueous solution with a concentration of less than 2.0 g Ba / 100 g water, and then added to the aqueous solution of the K additive precursor and / or the mixed slurry in step S3;

[0022] The method of adding the B element includes: adding a boron source to the mixed aqueous solution and / or precipitant solution in step S1; or

[0023] The boron source is added to the K additive precursor aqueous solution and / or the mixed slurry in step S3.

[0024] In the preparation method provided by the present invention, by controlling the concentration of Ba when added, the Ba element can be uniformly distributed on the catalyst surface at a specific content and form very fine particles. The B element itself is easily dispersed in the preparation system and does not easily crystallize during the calcination process, thus also easily forming fine particles. Therefore, the addition of Ba and B to the iron-based Fischer-Tropsch synthesis catalyst does not substantially change the original catalyst morphology (as shown in Figure 1).

[0025] In the preparation method provided by the present invention, the water-soluble salt of Ba can be one or both of barium nitrate and barium hydroxide.

[0026] In the preparation method provided by the present invention, the boron source can be one or more of boric acid, metaboric acid, boron oxide, and water-soluble borates. In some preferred embodiments, the water-soluble borates can be potassium borate and / or sodium borate. In some more preferred embodiments, the boron source can be boric acid.

[0027] In the preparation method provided by the present invention, the silicon source can be added in whole or in part to the precipitant solution, or in whole or in part to the mixed slurry. For example, the silicon source added to the precipitant solution can be about 0 wt%, about 10 wt%, about 20 wt%, about 30 wt%, about 40 wt%, about 50 wt%, about 60 wt%, about 70 wt%, about 80 wt%, about 90 wt%, about 100 wt%, or any combination of weight ratios of the total mass of the silicon source, and the remaining silicon source is added to the mixed slurry.

[0028] In the preparation method provided by the present invention, the water-soluble salt of Fe may be a common type in the art, including but not limited to nitrate, hydrochloride or hydrate of each of Fe (wherein the number of crystal waters may be a common number in the art), such as Fe(NO3)3·9H2O. In some preferred embodiments, the concentration of Fe in the mixed aqueous solution may be 5 to 100 g / L, for example, about 5 g / L, about 10 g / L, about 20 g / L, about 30 g / L, about 40 g / L, about 50 g / L, about 60 g / L, about 70 g / L, about 80 g / L, about 90 g / L, about 100 g / L or any combination of concentration intervals.

[0029] In the preparation method provided by the present invention, the water-soluble salt of Cu can be a common type in the art, including but not limited to Cu nitrate, hydrochloride or their respective hydrates (wherein the number of crystal waters can be a common number in the art), such as Cu(NO3)2·3H2O.

[0030] In the preparation method provided by the present invention, the precipitant can be any common type in the art, including but not limited to one or more of sodium carbonate, ammonia water, ammonium carbonate, sodium hydroxide, potassium hydroxide, and potassium carbonate. In some preferred embodiments, the precipitant can be selected from one or more of sodium carbonate, ammonia water, and ammonium carbonate. In other preferred embodiments, the concentration of the precipitant in the precipitant solution can be 50 to 150 g / L, for example, about 50 g / L, about 60 g / L, about 70 g / L, about 80 g / L, about 90 g / L, about 100 g / L, about 110 g / L, about 120 g / L, about 130 g / L, about 140 g / L, about 150 g / L, or any combination of concentration intervals.

[0031] In the preparation method provided by the present invention, the silicon source can be any common type in the art, including but not limited to one or more of potassium silicate solution, sodium silicate solution, and silica sol solution, wherein the SiO2 concentration can be 10 to 50 wt%. In some preferred embodiments, the SiO2 concentration in the silicon source can be 10 to 30 wt%.

[0032] In the preparation method provided by the present invention, the K additive precursor can be any common type in the art, including but not limited to one or more of potassium nitrate, potassium carbonate, potassium bicarbonate, potassium silicate, and potassium chloride.

[0033] In the preparation method provided by the present invention, in step S2, the precipitation temperature of the precipitation reaction can be 5 to 95°C (for example, it can be about 5°C, about 20°C, about 40°C, about 60°C, about 80°C, about 95°C, or any combination of temperature intervals), the precipitation time can be 5 to 100 min (for example, it can be about 5 min, about 20 min, about 40 min, about 60 min, about 80 min, about 100 min, or any combination of time intervals), and the pH value during the precipitation process can be controlled at 5 to 10 (for example, it can be about 5, about 6, about 7, about 8, about 9, about 10, or any combination of pH value intervals).

[0034] In the preparation method provided by the present invention, in step S3, when forming a mixed slurry, the mixing temperature of each material can be 20-70°C (for example, it can be about 20°C, about 30°C, about 40°C, about 50°C, about 60°C, about 70°C, or any combination of temperature intervals), and the mixing time can be 1-60 min (for example, it can be about 5 min, about 10 min, about 20 min, about 30 min, about 40 min, about 50 min, about 60 min, or any combination of time intervals).

[0035] In the preparation method provided by the present invention, in the step S3, the slurrying temperature of the slurrying treatment can be 10-80°C (for example, it can be about 10°C, about 20°C, about 30°C, about 40°C, about 50°C, about 60°C, about 70°C, about 80°C, or any combination of temperature intervals), the slurrying time can be 10-80 min (for example, it can be about 10 min, about 20 min, about 30 min, about 40 min, about 50 min, about 60 min, about 70 min, about 80 min, or any combination of time intervals), and the concentration of the slurry during the slurrying treatment can be controlled to be 5-40 wt% (for example, it can be about 5 wt%, about 10 wt%, about 15 wt%, about 20 wt%, about 25 wt%, about 30 wt%, about 35 wt%, about 40 wt%, or any combination of concentration intervals).

[0036] In the preparation method provided by the present invention, in step S4, the drying may include the following process: first, spray drying the catalyst precursor slurry, and drying the resulting powder in an air atmosphere at 110-300°C for 1-12 hours. In some preferred embodiments, the hot air inlet temperature of the spray drying may be 180-400°C, and the exhaust air outlet temperature may be 100-220°C.

[0037] In the preparation method provided by the present invention, in the step S4, the calcination temperature can be 400-600° C., and the calcination time can be 1-15 hours.

[0038] The technical solution provided by the present invention has the following advantages:

[0039] (1) The Ba and B doped Fischer-Tropsch synthesis iron-based catalyst provided by the present invention is doped with a specific content of Ba element and B element. Through the synergistic effect of the two, the obtained catalyst can have very excellent catalytic activity and thermal stability.

[0040] (2) In the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention, the synergistic effect of the Ba element and the B element can also avoid the problems caused by excessive alkalinity, so that the catalyst has lower CO2 selectivity and CH4 selectivity when used in the Fischer-Tropsch synthesis reaction.

[0041] (3) The preparation process of the iron-based catalyst for Fischer-Tropsch synthesis provided by the present invention is simple, requiring only the addition of a small amount of barium salt and boric acid or its salt. The conditions are mild and easy to control, and no secondary roasting is required. The catalyst has strong operability and low cost, and is suitable for large-scale industrial production.

[0042] In summary, the Ba and B doped Fischer-Tropsch synthesis iron-based catalyst provided by the present invention is easy to manufacture, has excellent catalytic performance and good heat resistance, and is not easily deactivated after long-term use. Therefore, its application can significantly improve the production efficiency of the Fischer-Tropsch synthesis process and reduce production costs, and has very important economic and social value. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 is a TEM-EDS spectrum of the catalyst prepared in Example 1, wherein Figure A shows the microscopic morphology of the catalyst, Figure B shows the distribution of B on the catalyst, Figure C shows the distribution of Ba on the catalyst, and Figure D shows the distribution of Fe on the catalyst. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described in detail below with reference to specific embodiments.

[0045] The testing method used in the present invention is as follows:

[0046] (1) Catalyst composition:

[0047] The components were determined by X-ray fluorescence analyzer (XRF).

[0048] (2) Catalyst specific surface area (BET)

[0049] The static low-temperature nitrogen adsorption method was used to measure the N2 adsorption isotherm at 77K, and the BET model equation was used to calculate the BET.

[0050] (3) Pore volume (PV)

[0051] The pore volume corresponds to P / P0=0.98~0.99 on the N2 adsorption isotherm measured at 77K.

[0052] (4) Average pore diameter (PD):

[0053] Calculated based on PD=4*PV / BET.

[0054] Unless otherwise specified, the raw materials or reagents used in the examples and comparative examples of the present invention are commercially available products.

[0055] Unless otherwise specified, the percentages used in the examples and comparative examples of the present invention are all percentages by mass.

[0056] Example 1

[0057] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 260 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 5 kg of ammonium carbonate and 1.84 kg of a 30% silica sol solution to the deionized water to prepare a 40 liter precipitant solution. A mixed solution containing iron, copper, and barium was co-precipitated with the precipitant solution at a temperature of 30°C, a precipitation time of 60 minutes, and a pH of 9.0. After the precipitation reaction was complete, the precipitated slurry was filtered and washed several times to obtain a catalyst precursor filter cake. A K promoter precursor aqueous solution was prepared by dissolving 195 g of potassium carbonate and 178 g of boric acid in 1.5 kg of deionized water. This K promoter precursor aqueous solution was added to the catalyst precursor filter cake and slurried at a concentration of 15% at a temperature of 25°C and a slurry time of 20 minutes to obtain a catalyst precursor slurry. The inlet temperature was controlled at 380°C and the outlet hot air temperature was controlled at 220°C for spray drying. The spray-dried product was collected, dried at 120°C in an air atmosphere for 12 hours, and calcined at 450°C in an air atmosphere for 5 hours to obtain a finished catalyst, which was recorded as Catalyst 1.

[0058] Example 2

[0059] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 46 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4 kg of sodium carbonate and 30 g of a 20% silica sol solution to the deionized water to prepare a 40 liter precipitant solution. The mixed solution containing iron, copper, and barium is co-precipitated with the precipitant solution at 50°C for 50 minutes, with the pH controlled at 8.5. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare an aqueous solution of the K additive precursor by dissolving 12 g of potassium carbonate and 138 g of boric acid in 1.5 kg of deionized water. An aqueous solution of a K-promoter precursor and 660 g of a silica sol solution with a 20% silica concentration were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 30°C, and the slurry time was 30 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature at 350°C and the outlet hot air temperature at 160°C. The spray-dried product was collected and dried at 150°C in air for 10 hours. It was then calcined at 400°C in air for 15 hours to obtain the finished catalyst, designated Catalyst 2.

[0060] Example 3

[0061] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 260 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia and 140 g of a potassium silicate solution with a modulus of 1 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 70°C for 30 minutes, with a pH of 5.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare the K promoter precursor aqueous solution by dissolving 104 g of potassium carbonate and 79 g of boric acid in 0.5 kg of deionized water. Prepare the Ba promoter aqueous solution by dissolving 105 g of Ba(NO₃)₂ in 3.0 kg of deionized water. 2.63 kg of a silica sol solution with a 20% silica mass concentration, a Ba additive aqueous solution, and a K additive precursor aqueous solution were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 50°C, and the slurry time was 40 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 320°C and the outlet hot air temperature at 140°C. The spray-dried product was collected and dried at 180°C in air for 8 hours. It was then calcined at 600°C in air for 6 hours to obtain the finished catalyst, designated Catalyst 3.

[0062] Example 4

[0063] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 10 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 12 kg of 25% ammonia water to the deionized water to prepare a 40 liter precipitant solution. Add the iron- and copper-containing mixed solution to the precipitant solution for precipitation. The precipitation temperature was maintained at 90°C, the precipitation time was 20 minutes, and the endpoint pH was controlled at 6.0. After the precipitation reaction, the precipitate slurry was filtered and washed several times to obtain a catalyst precursor filter cake. The catalyst precursor filter cake was slurried in 1.5 kg of deionized water. A K additive precursor aqueous solution was prepared by dissolving 104 g of potassium carbonate, 178 g of boric acid, and 460 g of a potassium silicate solution with a modulus of 1 and a silica content of 30% in 1.0 kg of deionized water. The K additive precursor aqueous solution was added to the catalyst precursor filter cake slurry, mixed thoroughly, and 5wt% nitric acid solution was added to the slurry, the endpoint pH was controlled to 7.0, and the above slurry was filtered to obtain a filter cake. 260g Ba(NO3)2 was fully dissolved in 7kg deionized water to prepare a Ba additive aqueous solution, and the Ba additive aqueous solution was added to the filter cake for slurry treatment, the mass concentration of the slurry was controlled to be 15%, the slurry temperature was 70°C, and the slurry time was 50min to obtain a catalyst precursor slurry. The inlet temperature was controlled at 290°C and the outlet hot air temperature was controlled at 120°C for spray drying, the spray-dried product was collected, and the resulting product was dried at 200°C in an air atmosphere for 6h, and calcined at 600°C in an air atmosphere for 8h to obtain a finished catalyst, which was recorded as Catalyst 4.

[0064] Example 5

[0065] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 260 g of Cu(NO₃)₂·3H₂O, and 260 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 3.5 kg of sodium carbonate and 1.73 kg of a sodium silicate solution with a modulus of 1 and a silica concentration of 20% by mass to the deionized water to prepare a 40 liter precipitant solution. Add a mixed solution containing iron, copper, and barium to the precipitant solution for precipitation. The precipitation temperature was maintained at 10°C, the precipitation time was 90 minutes, and the endpoint pH was controlled at 7.0. After the precipitation reaction, the precipitate slurry was filtered and washed several times to obtain a catalyst precursor filter cake. Prepare an aqueous solution of the K additive precursor by dissolving 12 g of potassium carbonate and 138 g of boric acid in 1.5 kg of deionized water. An aqueous solution of a K-promoter precursor was added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 10°C, and the slurry time was 60 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature at 260°C and the outlet hot air temperature at 110°C. The spray-dried product was collected and dried at 220°C in air for 4 hours. It was then calcined at 550°C in air for 10 hours to obtain the finished catalyst, designated Catalyst 5.

[0066] Example 6

[0067] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 10 g of Cu(NO₃)₂·3H₂O, and 118 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4.5 kg of ammonium carbonate and 120 g of a sodium silicate solution with a modulus of 3.5 and a silica concentration of 30% by mass to the deionized water to prepare a 40 liter precipitant solution. Add a mixed solution containing iron, copper, and barium to the precipitant solution for precipitation. The precipitation temperature was maintained at 30°C, the precipitation time was 30 minutes, and the endpoint pH was controlled at 8.5. After the precipitation reaction, the precipitate was filtered and washed several times to obtain a catalyst precursor filter cake. Prepare an aqueous solution of the K additive precursor by dissolving 195 g of potassium carbonate and 79 g of boric acid in 1.5 kg of deionized water. An aqueous solution of a K-promoter precursor and 1.04 kg of a silica sol solution with a 30% silica concentration were added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 25°C, and the slurry time was 20 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 230°C and the outlet hot air temperature at 105°C. The spray-dried product was collected and dried at 250°C in air for 3 hours. It was then calcined at 400°C in air for 12 hours to obtain the finished catalyst, designated Catalyst 6.

[0068] Example 7

[0069] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 260 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia and 690 g of a potassium silicate solution with a modulus of 3.5 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. Add the iron- and copper-containing mixed solution to the precipitant solution for precipitation at a temperature of 50°C, a precipitation time of 60 minutes, and an endpoint pH of 5.0. After the precipitation reaction is complete, filter the precipitate slurry and wash several times to obtain a catalyst precursor filter cake. Dissolve 160 g of Ba(NO₃)₂ in 7 kg of deionized water to prepare a Ba additive aqueous solution. Dissolve 195 g of potassium carbonate and 138 g of boric acid in 1.0 kg of deionized water to prepare a K additive precursor aqueous solution. An aqueous solution of Ba and an aqueous solution of a K additive precursor were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 30°C, and the slurry time was 30 minutes to obtain a catalyst precursor slurry. Spray drying was performed with an inlet temperature of 200°C and an outlet hot air temperature of 105°C. The spray-dried product was collected and dried at 280°C in air for 2 hours. It was then calcined at 500°C in air for 8 hours to obtain the finished catalyst, designated Catalyst 7.

[0070] Example 8

[0071] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 10 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 9 kg of 25% ammonia and 2.76 kg of a sodium silicate solution with a modulus of 1 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. Add the precipitant solution to the iron-copper mixed solution for precipitation at a temperature of 70°C, a precipitation time of 40 minutes, and an endpoint pH of 6.0. After the precipitation reaction is complete, filter the precipitate slurry and wash several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 160 g of Ba(NO₃)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 12 g of potassium carbonate and 79 g of boric acid in 1.0 kg of deionized water. An aqueous solution of Ba and an aqueous solution of K additive precursor were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 50°C, and the slurry time was 40 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 180°C and the outlet hot air temperature at 100°C. The spray-dried product was collected and dried at 300°C in air for 1 hour. It was then calcined at 550°C in air for 8 hours to obtain the finished catalyst, designated Catalyst 8.

[0072] Example 9

[0073] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, 79 g of Ba(NO₃)₂, and 40 g of boric acid in deionized water to prepare a 50 liter solution. Add 3 kg of sodium carbonate and 1.73 kg of a sodium silicate solution with a modulus of 3.5 and a silica concentration of 20% by mass to the deionized water to prepare a 40 liter precipitant solution. The mixed solution containing iron, copper, and barium was co-precipitated with the precipitant solution at 30°C for 80 minutes, with a pH of 7.0. After the precipitation reaction was complete, the precipitate was filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 152 g of potassium nitrate in 1.5 kg of deionized water to prepare an aqueous solution of the K promoter precursor. An aqueous solution of a K-promoter precursor was added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 25°C, and the slurry time was 50 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 380°C and the outlet hot air temperature at 220°C. The spray-dried product was collected and dried at 120°C in air for 12 hours. Finally, it was calcined at 600°C in air for 10 hours to obtain the finished catalyst, designated Catalyst 9.

[0074] Example 10

[0075] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 10 g of Cu(NO₃)₂·3H₂O, 131 g of Ba(NO₃)₂, and 178 g of boric acid in deionized water to prepare a 50 liter solution. Add 4.5 kg of ammonium carbonate and 460 g of a sodium silicate solution with a modulus of 1 and a silica concentration of 30% by mass to the deionized water to prepare a 40 liter precipitant solution. This precipitant solution is added to a mixed solution containing iron, copper, and barium for precipitation. The precipitation temperature is maintained at 50°C, the precipitation time is 50 minutes, and the endpoint pH is controlled at 8.5. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 18 g of potassium nitrate in 1.5 kg of deionized water to prepare an aqueous solution of the K additive precursor. An aqueous solution of a K promoter precursor was added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 30°C, and the slurry time was 60 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 350°C and the outlet hot air temperature at 150°C. The spray-dried product was collected and dried in air at 150°C for 10 hours. Finally, it was calcined in air at 400°C for 9 hours to obtain the finished catalyst, designated Catalyst 10.

[0076] Example 11

[0077] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 260 g of Cu(NO₃)₂·3H₂O, and 158 g of boric acid in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia water to the deionized water to prepare a 40 liter precipitant solution. Add the precipitant solution to the iron-copper mixed solution to precipitate. The precipitation temperature is controlled at 90°C, the precipitation time is 20 minutes, and the endpoint pH is controlled at 5.0. After the precipitation reaction is complete, filter the precipitate slurry and wash several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 260 g of Ba(NO₃)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 286 g of potassium nitrate in 0.5 kg of deionized water. An aqueous solution of Ba additive, an aqueous solution of K additive precursor, and 1.84 kg of a silica sol solution with a silica mass concentration of 30% were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 70°C, and the slurry time was 20 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 320°C and the outlet hot air temperature at 130°C. The spray-dried product was collected and dried at 180°C in air for 8 hours. It was then calcined at 600°C in air for 4 hours to obtain the finished catalyst, designated Catalyst 11.

[0078] Example 12

[0079] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 140 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 9 kg of 25% ammonia, 630 g of potassium silicate solution with a modulus of 3.5 and a 30% silica concentration, and 40 g of boric acid to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 90°C for 20 minutes, with a pH of 6.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 79 g of Ba(NO₃)₂ in 2.5 kg of deionized water. An aqueous solution of Ba additive and 530 g of a potassium silicate solution with a modulus of 3.5 and a silica concentration of 30% were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 70°C, and the slurry time was 30 minutes to obtain a catalyst precursor slurry. Spray drying was then performed with an inlet temperature of 290°C and an outlet hot air temperature of 120°C. The spray-dried product was collected and dried at 200°C in air for 6 hours. It was then calcined at 600°C in air for 4 hours to obtain the finished catalyst, designated Catalyst 12.

[0080] Example 13

[0081] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 260 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 3 kg of sodium carbonate, 750 g of a silica sol solution with a 25% silica concentration, and 178 g of boric acid to the deionized water to prepare a 40 liter precipitant solution. This precipitant solution is added to a mixed solution containing iron, copper, and barium for precipitation. The precipitation temperature is controlled at 70°C, the precipitation time is 30 minutes, and the endpoint pH is controlled at 7.0. After the precipitation reaction is complete, the precipitated slurry is filtered and washed several times to obtain a catalyst precursor filter cake. A K additive precursor aqueous solution is prepared by dissolving 630 g of a potassium silicate solution with a modulus of 3.5 and a 25% silica concentration in 1.0 kg of deionized water. An aqueous solution of a K-promoter precursor was added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 50°C, and the slurry time was 40 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature at 260°C and the outlet hot air temperature at 110°C. The spray-dried product was collected and dried at 220°C in air for 4 hours. It was then calcined at 450°C in air for 6 hours to obtain the finished catalyst, designated Catalyst 13.

[0082] Example 14

[0083] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 26 g of Cu(NO₃)₂·3H₂O, and 132 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4.5 kg of ammonium carbonate and 99 g of boric acid to the deionized water to prepare a 40 liter precipitant solution. A mixed solution containing iron, copper, and barium is co-precipitated with the precipitant solution at 30°C for 70 minutes, with a pH of 8.5. After the precipitation reaction is complete, the precipitated slurry is filtered and washed several times to obtain a catalyst precursor filter cake. A K additive precursor aqueous solution is prepared by dissolving 580 g of a potassium silicate solution with a modulus of 3.5 and a silica concentration of 25% in 0.5 kg of deionized water. An aqueous solution of a K-promoter precursor and 1.08 kg of a silica sol solution with a 25% silica concentration were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 25°C, and the slurry time was 50 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 230°C and the outlet hot air temperature at 105°C. The spray-dried product was collected and dried at 250°C in air for 3 hours. It was then calcined at 550°C in air for 6 hours to obtain the finished catalyst, designated Catalyst 14.

[0084] Example 15

[0085] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 68 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia, 770 g of sodium silicate solution with a modulus of 3.5 and a 25% silica concentration, and 40 g of boric acid to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 50°C for 40 minutes, with a pH of 5.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 39 g of Ba(NO₃)₂ in 1.5 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 107 g of potassium nitrate in 0.5 kg of deionized water. An aqueous solution of Ba and an aqueous solution of K additive precursor were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 30°C, and the slurry time was 60 minutes to obtain a catalyst precursor slurry. Spray drying was performed with an inlet temperature of 200°C and an outlet hot air temperature of 100°C. The spray-dried product was collected and dried at 280°C in air for 2 hours. It was then calcined at 550°C in air for 4 hours to obtain the finished catalyst, designated Catalyst 15.

[0086] Example 16

[0087] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 184 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 9 kg of 25% ammonia, 550 g of sodium silicate solution with a modulus of 3.5 and a 25% silica concentration, and 119 g of boric acid to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 10°C for 90 minutes, with a pH of 6.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 210 g of Ba(NO₃)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 214 g of potassium nitrate in 0.5 kg of deionized water. An aqueous solution of Ba additive, an aqueous solution of K additive precursor, and 550 g of a silica sol solution with a silica mass concentration of 25% were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 10°C, and the slurry time was 60 minutes to obtain a catalyst precursor slurry. Spray drying was performed with an inlet temperature of 180°C and an outlet hot air temperature of 100°C. The spray-dried product was collected and dried at 300°C in air for 1 hour. It was then calcined at 600°C in air for 2 hours to obtain the finished catalyst, designated Catalyst 16.

[0088] Comparative Example 1

[0089] Except for not adding Ba(NO3)2, the remaining steps were the same as those in Example 1 to obtain a finished catalyst, which was recorded as comparative agent 1.

[0090] Comparative Example 2

[0091] Except for not adding boric acid, the remaining steps were the same as in Example 2 to obtain a finished catalyst, which was recorded as comparative agent 2.

[0092] Comparative Example 3

[0093] Except that Ba(NO3)2 and boric acid were not added (only 104g potassium carbonate was fully dissolved in 1.0kg deionized water to prepare the K additive precursor aqueous solution), the remaining steps were the same as in Example 3 to obtain a finished catalyst, which was recorded as comparative agent 3.

[0094] Comparative Example 4

[0095] Except for using 815g Ca(NO3)2·4H2O instead of Ba(NO3)2, the remaining steps were the same as those in Example 4 to obtain a finished catalyst, which was recorded as comparative agent 4.

[0096] Comparative Example 5

[0097] Except for using 1458g Mg(NO3)2·6H2O instead of Ba(NO3)2, the remaining steps were the same as those in Example 5 to obtain a finished catalyst, which was recorded as comparative agent 5.

[0098] Comparative Example 6

[0099] Except for using 33g Sr(NO3)2 instead of Ba(NO3)2, the remaining steps are the same as those in Example 6 to obtain a finished catalyst, which is recorded as comparative agent 6.

[0100] Comparative Example 7

[0101] Except for using 96 g of Al(NO 3 ) 3 ·9H 2 O instead of boric acid, the remaining steps were the same as in Example 9 to obtain a finished catalyst, which was recorded as comparative agent 7.

[0102] Comparative Example 8

[0103] Except for using 290g Ba(NO3)2 to fully dissolve in 8kg deionized water to prepare the Ba auxiliary agent aqueous solution, the remaining steps are the same as Example 8 to obtain a finished catalyst, which is recorded as comparative agent 8.

[0104] Comparative Example 9

[0105] Except for replacing the amount of Ba(NO3)2 with 24g, the remaining steps were the same as those in Example 7 to obtain a finished catalyst, which was recorded as comparative agent 9.

[0106] Comparative Example 10

[0107] Except for replacing the amount of boric acid with 206 g, the remaining steps were the same as in Example 10 to obtain a finished catalyst, which was recorded as comparative agent 10.

[0108] Comparative Example 11

[0109] Except for replacing the amount of boric acid with 24 g, the remaining steps were the same as in Example 11 to obtain a finished catalyst, which was recorded as comparative agent 11.

[0110] Comparative Example 12

[0111] Except for replacing the amount of boric acid with 24 g, the amount of Ba(NO3)2 with 290 g and fully dissolving them in 8 kg of deionized water to prepare the Ba auxiliary agent aqueous solution, the remaining steps are the same as Example 12 to obtain the finished catalyst, which is recorded as comparative agent 12.

[0112] Comparative Example 13

[0113] Except for replacing the amount of boric acid with 206 g and the amount of Ba(NO3)2 with 24 g, the remaining steps are the same as those in Example 13 to obtain a finished catalyst, which is recorded as comparative agent 13.

[0114] Comparative Example 14

[0115] Except for replacing the amount of Ba(NO3)2 with 145g and the amount of silica sol with 0.25kg, the remaining steps are the same as those in Example 14 to obtain a finished catalyst, which is recorded as comparative agent 14.

[0116] Comparative Example 15

[0117] Except for replacing the amount of Ba(NO3)2 with 26 g and the amount of silica sol with 0.25 kg, the remaining steps are the same as those in Example 14 to obtain a finished catalyst, which is recorded as comparative agent 15.

[0118] Comparative Example 16

[0119] Except for replacing the amount of Ba(NO3)2 with 208 g and the amount of silica sol with 0.8 kg, the remaining steps are the same as those in Example 14 to obtain a finished catalyst, which is recorded as comparative agent 16.

[0120] Comparative Example 17

[0121] Except for replacing the amount of Ba(NO3)2 with 104 g and the amount of silica sol with 0.8 kg, the remaining steps are the same as those in Example 14 to obtain a finished catalyst, which is recorded as comparative agent 17.

[0122] Test Case

[0123] Test equipment: 1L stirred tank.

[0124] Test conditions: 10g of the catalysts prepared in Examples 1-16 and Comparative Examples 1-17 were mixed with 300mL of liquid paraffin and placed in a 1L stirred tank. After reduction activation, the reaction was switched to Fischer-Tropsch synthesis reaction conditions. The process conditions for reduction activation and Fischer-Tropsch synthesis reaction were as follows:

[0125] (1) Reduction activation: Use synthesis gas with a volume ratio of H2 / CO of 20:1 to reduce the reaction mixture by heating (4 h at 30-200 °C, 10 h at 200-265 °C, and 24 h at a constant temperature of 265 °C). The space velocity of the synthesis gas is 8000 h -1 , the reduction gauge pressure is 3.0MPa.

[0126] (2) Fischer-Tropsch synthesis: After the reduction is completed, the H2 / CO volume ratio of the synthesis gas is adjusted to 3:1 and stabilized for a period of time until the gas phase composition in the reaction tail gas basically does not change with time, which is recorded as the reaction zero point.

[0127] (3) Data calculation: The molar number of CO in the feed was measured and analyzed at the feed port of the stirred tank, and the molar number of CO, CO2, and CH4 in the discharge was measured and analyzed at the discharge port. The CO conversion rate (%), CO2 selectivity (%), and CH4 selectivity (%) were calculated using the following formulas:

[0128] CO conversion rate % = [(CO moles in feed - CO moles in discharge) / CO moles in feed] × 100%;

[0129] CO2 selectivity % = [CO2 moles in the discharge / (CO moles in the feed - CO moles in the discharge)] × 100%;

[0130] CH4 selectivity % = [mole number of CH4 in the discharge / (mole number of CO in the feed × CO conversion rate % × (1-CO2 selectivity %))] × 100%.

[0131] The deactivation rate of the catalyst refers to the rate at which the catalyst activity (carbon monoxide conversion rate) decreases from the reaction plateau to the end of the reaction, and the unit is % / h.

[0132] The composition, properties and reaction performance results of the catalysts prepared in Examples 1-16 are shown in Table 1, and the composition, properties and reaction performance results of the catalysts prepared in Comparative Examples 1-17 are shown in Table 2.

[0133] Table 1

[0134] Table 2

[0135] It can be seen from the results in Table 1 and Table 2 that the Ba and B doped Fischer-Tropsch synthesis iron-based catalyst provided by the present invention has a higher CO conversion rate and lower CO2 selectivity and CH4 selectivity, indicating that it has excellent catalytic activity; the Ba and B doped Fischer-Tropsch synthesis iron-based catalyst provided by the present invention also has a lower deactivation rate, indicating that it has good thermal stability, which is particularly important for highly exothermic Fischer-Tropsch synthesis reactions under high catalytic activity.

[0136] However, for catalysts without added Ba element and / or B element (for example, comparative examples 1-3), catalysts with added other alkaline earth metal elements of the same group as Ba (for example, comparative examples 4-6), catalysts with added Al element of the same group as B (for example, comparative example 7), and catalysts with added Ba element and B element but the added amount is not within the range described in the present invention, none of them can achieve the excellent catalytic activity and good thermal stability comparable to the Fischer-Tropsch synthesis iron-based catalyst of the present invention.

[0137] Unless otherwise defined, the terms used in the present invention have the same meanings as those commonly understood by those skilled in the art.

[0138] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above-mentioned embodiments, but is only limited by the claims.

Claims

1. A Ba and B doped Fischer-Tropsch synthesis iron-based catalyst comprising Fe, Cu, K and SiO2, characterized in that: The Fischer-Tropsch synthesis iron-based catalyst is doped with Ba element and B element. By mass ratio, when Fe element:SiO2=100:10-less than 20, Ba element:B element=1-less than 4:1; when Fe element:SiO2=100:20-40, Ba element:B element=4-6:

1.

2. The Fischer-Tropsch synthesis iron-based catalyst according to claim 1, characterized in that The Fischer-Tropsch synthesis iron-based catalyst comprises the following components in a mass ratio: Fe element: SiO2: Cu element: K element: Ba element: B element = 100: 10-40: 0.2-5: 0.5-8: 1-10: 0.4-2.

5.

3. The method for preparing the Ba and B doped Fischer-Tropsch synthesis iron-based catalyst according to claim 1 or 2, characterized in that: The following steps are involved: S1: forming a mixed aqueous solution of a water-soluble salt of Fe and a water-soluble salt of Cu, preparing a precipitant solution, and adding 0 to 100 wt % of a silicon source to the precipitant solution; S2: contacting the mixed aqueous solution with the precipitant solution to perform a precipitation reaction, and separating the obtained precipitation product after the reaction is completed; S3: mixing the precipitated product with the K additive precursor aqueous solution and the remaining silicon source to form a mixed slurry and performing slurry treatment to obtain a catalyst precursor slurry; as well as S4: drying and calcining the catalyst precursor slurry; The method of adding the Ba element includes: adding a water-soluble salt of Ba to the mixed aqueous solution of step S1, and making the concentration of Ba lower than 2.0 g Ba / 100 g water; or The water-soluble salt of Ba is prepared into an aqueous solution with a concentration of less than 2.0 g Ba / 100 g water, and then added to the aqueous solution of the K additive precursor and / or the mixed slurry in step S3; The method of adding the B element includes: adding a boron source to the mixed aqueous solution and / or the precipitant solution in step S1; or The boron source is added to the aqueous solution and / or the mixed slurry of the K additive precursor in step S3.

4. The preparation method according to claim 3, characterized in that: The water-soluble salt of Ba is one or both of barium nitrate and barium hydroxide; and / or The boron source is one or more of boric acid, metaboric acid, boric oxide, and water-soluble borates; Preferably, the water-soluble borate is potassium borate and / or sodium borate.

5. The preparation method according to claim 3 or 4, characterized in that: The water-soluble salt of Fe is nitrate, hydrochloride or hydrate of Fe, and the water-soluble salt of Cu is nitrate, hydrochloride or hydrate of Cu; preferably, the concentration of Fe in the mixed aqueous solution is 5-100 g / L; and / or The precipitant is selected from one or more of sodium carbonate, ammonia water, ammonium carbonate, sodium hydroxide, potassium hydroxide, and potassium carbonate; preferably, the concentration of the precipitant is 50-150 g / L.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The silicon source is selected from one or more of potassium silicate solution, sodium silicate solution and silica sol solution, wherein the SiO2 concentration is 10-50wt%; and / or The K additive precursor is one or more of potassium nitrate, potassium carbonate, potassium bicarbonate, potassium chloride and potassium silicate.

7. The preparation method according to any one of claims 3 to 6, characterized in that: In the step S2, the precipitation temperature of the precipitation reaction is 5 to 95° C., the precipitation time is 5 to 100 min, and the pH value is controlled at 5 to 10 during the precipitation process.

8. The preparation method according to any one of claims 3 to 7, characterized in that: In the step S3, the slurrying temperature of the slurrying treatment is 10-80° C., the slurrying time is 10-80 min, and the concentration of the slurry is controlled to be 5-40 wt % during the slurrying treatment.

9. The preparation method according to any one of claims 3 to 8, characterized in that: In the step S4, the drying includes the following process: firstly, the catalyst precursor slurry is spray-dried, and the obtained powder is dried in an air atmosphere at 110-300° C. for 1-12 hours; Preferably, the hot air inlet temperature of the spray drying is 180-400°C, and the exhaust air outlet temperature is 100-220°C.

10. The preparation method according to any one of claims 3 to 9, characterized in that: In the step S4, the calcination temperature is 400-600° C. and the calcination time is 1-15 hours.

Citation Information

Patent Citations

  • Iron base catalyst for fischer-tropsch synthesis and preparation method thereof

    CN101293206A

  • Iron catalyst containing titanium deposition for catalyzing Fischer-Tropsch synthesis reaction and method for producing the same

    CN101298046A

  • A Fischer-Tropsch iron-based catalyst with high wear resistance and high reactivity and its preparation method.

    CN105478128B

  • Iron-based catalysts for Fischer-Tropsch synthesis, their preparation methods, and Fischer-Tropsch synthesis methods

    CN107913714B

  • Iron base catalyzer through Fischer-Tropsch synthesis and preparation method

    CN1245255C