Broadband yellow light emission microcrystal composite glass optical fiber and preparation method therefor

Through the preparation of NaLa(WO4)2:Dy3+ glass-ceramic fiber, the shortcomings of Dy3+-doped fluoride glass fiber in yellow laser output performance are solved, and broadband yellow light emission and low loss are achieved, which is suitable for tunable or ultrasonic applications. Fast yellow laser.

WO2024221994A1PCT designated stage expired Publication Date: 2024-10-31SOUTH CHINA UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/141135
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-12-22
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing Dy3+-doped fluoride glass fiber has problems with poor chemical stability, low laser damage threshold and low fluorescence branch in yellow laser output performance, which limits the tunability and pulse output performance of yellow laser.

Method used

Using NaLa(WO4)2:Dy3+ceramic glass optical fiber, drawn by core fusion method and heat-treated, a microcrystalline composite glass optical fiber with broadband yellow light emission and low transmission loss is prepared, taking advantage of its non-uniform broadening spectral characteristics and flexibility property, as the gain medium of Dy3+ doped yellow fiber laser.

Benefits of technology

It achieves broadband and intense yellow light emission, improves the output performance of yellow laser, and is especially suitable for tunable or ultrafast yellow lasers with low transmission loss and good compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023141135_31102024_PF_FP_ABST
    Figure CN2023141135_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A broadband yellow light emission microcrystal composite glass optical fiber and a preparation method therefor. A cladding layer of the microcrystalline composite glass optical fiber is quartz glass, and a fiber core is Dy3+-doped NaLa(WO4 2 microcrystalline glass. The preparation method is as follows: firstly, pickling and drying a quartz glass tube, and then sealing one end of the quartz glass tube by means of tapering; placing a fiber core ceramic rod in the quartz glass tube to prepare an optical fiber preform; wiredrawing the optical fiber preform at a high temperature of 1950-2010ºC to obtain an optical fiber precursor; and then subjecting the optical fiber precursor to a heat treatment for 3-6 hours at a temperature of 900-1000ºC to obtain a broadband yellow light emission microcrystal composite glass optical fiber. The prepared microcrystalline composite glass optical fiber has broadband and stronger yellow light emission, keeps relatively low transmission loss, can provide a broadband light-emitting and stable gain medium for a Dy3+-doped yellow light optical fiber laser, and is expected to achieve tuning or ultrafast yellow light laser direct output.
Need to check novelty before this filing date? Find Prior Art

Description

A microcrystalline composite glass optical fiber with broadband yellow light emission and its preparation method Technical Field

[0001] The invention belongs to the field of optical fibers, and in particular relates to a microcrystalline composite glass optical fiber emitting broadband yellow light and a preparation method thereof. Background Art

[0002] Visible yellow lasers with a wavelength range of approximately 565-590 nm are widely used in laser medicine, laser radar, astronomical observation, etc. For example, in the biomedical field, hemoglobin has a high absorption rate for yellow lasers with a wavelength of 577 nm, so there is an urgent need for yellow lasers in the treatment of skin diseases, vascular diseases and ophthalmic diseases. However, the output of yellow lasers is relatively difficult, and is currently mainly based on dye lasers and nonlinear frequency conversion, including sum frequency, frequency doubling and Raman shift. Dye lasers have high maintenance costs and low safety in use; and systems using nonlinear crystals and self-space alignment are complex, non-compact in structure, not conducive to integration, and have low pumping efficiency. In contrast, the use of laser diodes (LDs) to pump rare earth-doped optical fiber materials can directly realize yellow light transport, and yellow lasers can be output after resonant cavity mode selection and amplification. This direct emission method can eliminate complex nonlinear optical processes and has the advantages of simple system, low loss and high reliability. Based on trivalent Dy 3+ correspond 4 F 9 / 2 → 6 H 13 / 2 The transition of Dy has the strongest yellow emission near 570 nm. The fluorescence branch of yellow light is relatively large, and there are multiple shorter wavelengths in the range from ultraviolet band to blue light band that can be used to directly excite ground state particles. 3+ It is considered to be the best rare earth ion for direct emission of yellow lasers. 3+ The 4f transition in the visible light range is spin-forbidden (resulting in relatively small blue light absorption cross section and yellow light emission cross section), and Dy 3+ The energy level structure is complex and cross relaxation is prone to occur, resulting in a low quenching threshold.

[0003] Traditional yellow laser crystals, such as Dy:YAG and Dy:ZnWO4, have good thermal conductivity and high mechanical strength, but their narrow yellow light emission spectrum (FWHM < 7 nm) limits their application in pulsed lasers. 3+The mainstream gain fiber used in doped fiber lasers is still fluoride glass fiber (Limpert.J, Zellmer H, Riedel P, et al. Laser oscillation in yellow and blue spectral range in Dy 3+ :ZBLAN[J]. Electronics Lettres, 2000, 36(16): 1386-1387; Fujimoto Y, Ishii O, Yamazaki M. 575 nm laser oscillation in Dy 3+ -doped waterproof fluoro-aluminate glass fiber pumped by violet GaN laser diodes[J]. Solid State Lasers XX: Technology and Devices, 2011, 7912: 79120J;Wang HJ, Zou JH, Dong CC, et al. High-efficiency, yellow-light Dy 3+ -doped fiber laser with tuning from 568.7 to 581.9 nm[J]. Optics Letters, 2019, 44(17): 4423-4426; Luo SY, Gu H, Tang X, et al. High-power yellow DSR pulses generated from a wavelength-locked Dy:ZBLAN fiber laser[J]. Optics Letters, 2022, 47(5): 1157-1160.). Although the above reports confirmed that Dy 3+ The application of fluoride-doped glass fiber in continuous, tunable and pulsed yellow lasers, but fluoride glass fiber still has many shortcomings. On the one hand, fluoride glass has relatively poor chemical stability and low laser damage threshold, which greatly limits the application of Dy 3+ On the other hand, the fluoride ion radius in fluoride glass is small, the polarizability is low, and the covalency to the surrounding local field is small, which leads to the increase of the output power of Dy 3+The Ω2 value is small, and the fluorescence branching in the yellow light band is relatively low, which leads to a low emission cross section of yellow light emission and poor theoretical gain performance. In addition, there are a few studies on Dy 3+ Doping other gain fibers to emit yellow light (Tian SH, Lun YP, Sun YS, et al. Silicate-clad Dy 3+ doped multi-component phosphate glass core glass fiber for yellow laser applications[J]. Journal of Non-Crystalline Solids, 2022, 577, 121313.) and yellow laser output (Majewski MR, Jackson S D. Diode pumped silicate fiber for yellow laser emission[J]. OSA Continuum, 2021, 4(11), 2845-2851.), but there has been no breakthrough in Dy 3+ Progress in yellow laser output performance of fluoride-doped glass fibers.

[0004] Therefore, to further improve the output performance of tunable or pulsed yellow laser, the key is not only to improve the Dy 3+ In order to solve the inherent yellow light emission problem, we need to develop a gain medium with broadband emission, stable chemical properties and high damage threshold. NaLa(WO4)2 crystal is composed of layered [WO4] tetrahedrons, and Na and La are randomly distributed at the corresponding lattice positions in a 1:1 ratio between layers, resulting in a disordered structure of the crystal and non-uniform broadening of the spectrum. In addition, NaLa(WO4)2:Dy 3+ The crystal has excellent yellow light gain performance (Wei YP, Tu CY, Wang HY, et al. Optical spectroscopy of NaLa(WO4)2:Dy 3+ single crystal[J]. Journal of Alloys and Compounds, 2007, 438(1-2): 310-316.), which has great potential in realizing tunable or pulsed yellow laser output.

[0005] Summary of the Invention

[0006] In order to solve the above technical problems, the present invention provides a broadband yellow light emitting microcrystalline composite glass optical fiber and its preparation method. 3+ The characteristics of the crystal's non-uniform spectrum broadening and the advantages of the optical fiber's good flexibility and low laser threshold are used to prepare a microcrystalline composite glass optical fiber with broadband yellow light emission. The present invention uses the core melting method to draw the composite optical fiber, and then heat treats it to obtain NaLa(WO4)2:Dy with a controllable degree of crystallization. 3+ Microcrystalline glass composite optical fiber. This method has wide applicability and combines the advantages of NaLa(WO4)2 microcrystals inhomogeneously broadening the spectrum to produce microcrystalline composite glass optical fiber with broadband and strong yellow light emission while maintaining low transmission loss. 3+ Doped yellow fiber lasers provide broadband luminescence and stable gain medium, which is expected to achieve tunable or ultrafast yellow laser direct output.

[0007] The optical fiber of the present invention has an emission peak half-width at 575 nm of up to 18-22 nm.

[0008] In order to achieve the above object, the technical solution of the present invention is:

[0009] A microcrystalline composite glass optical fiber with broadband yellow light emission, its cladding is quartz glass and its core is Dy 3+ Doped NaLa(WO4)2 glass-ceramics.

[0010] Preferably, the Dy 3+ The chemical formula of doped NaLa(WO4)2 glass-ceramics is NaLa ( 1-x ) (WO4)2:xDy 3+ , x=0.03~0.07;

[0011] Further preferably, x=0.03, 0.04, 0.05, 0.06, 0.07.

[0012] Preferably, the core diameter of the microcrystalline composite glass optical fiber is 5-20 μm, and the outer diameter of the cladding is 120-130 μm.

[0013] Preferably, the microcrystalline composite glass optical fiber obtains 18-22 nm broadband yellow light emission under the pumping of a blue semiconductor laser.

[0014] Preferably, the precursor of the fiber core is a fiber core ceramic rod; and the method for preparing the fiber core ceramic rod comprises the following steps:

[0015] (a) mixing sodium carbonate powder, tungsten oxide powder, lanthanum oxide powder and dysprosium oxide powder, grinding and sintering;

[0016] (b) Grinding the powder sintered in step (a), adding a binder to form a compact, sintering, and grinding it into a cylinder to obtain a fiber core ceramic rod.

[0017] Further preferably, in step (a), the purity of the sodium carbonate powder is ≥99.9%, the purity of the tungsten oxide powder is ≥99.99%, the purity of the lanthanum oxide powder is ≥99.99%, and the purity of the dysprosium oxide powder is ≥99.99%;

[0018] Further preferably, the molar ratio of the sodium carbonate powder, tungsten oxide powder, lanthanum oxide powder, and dysprosium oxide powder in step (a) is 1:4:0.93-0.97:0.03-0.07.

[0019] Further preferably, the sintering temperature in step (a) is 1000-1200°C and the sintering time is 6-10 h; and the sintering is carried out in a muffle furnace.

[0020] Further preferably, the binder in step (b) is a PVA binder, and its mass percentage is 0.1-1.5% of the sintered powder; the sintering temperature is 1000-1200°C, and the time is 6-10 h; and the sintering is carried out in a muffle furnace.

[0021] More preferably, the mass percentage of the binder is 0.5% of the sintered powder.

[0022] The method for preparing the above-mentioned microcrystalline composite glass optical fiber with broadband yellow light emission comprises the following steps:

[0023] (1) First, pickle and dry the quartz glass tube, and then seal one end of the tube by taper.

[0024] (2) Placing the fiber core ceramic rod in a quartz glass tube to produce an optical fiber preform;

[0025] (3) Drawing the optical fiber preform at a high temperature of 1950-2010°C to obtain an optical fiber precursor;

[0026] (4) The optical fiber precursor is heat-treated at a temperature of 900-1000°C for 3-6 hours to obtain a microcrystalline composite glass optical fiber with broadband yellow light emission.

[0027] Preferably, the wire drawing in step (3) is carried out in a high-temperature graphite furnace of Rasta;

[0028] Preferably, the heat treatment in step (4) is carried out in a muffle furnace.

[0029] Due to the adoption of the above technical solution, the present invention has the following positive effects and outstanding features compared with the prior art:

[0030] (1) The present invention is a broadband yellow light emitting microcrystalline composite glass optical fiber, which fully combines NaLa(WO4)2:Dy 3+ The characteristics of non-uniform spectrum broadening of microcrystalline glass and the good flexibility and low laser threshold of optical fiber make the microcrystalline composite glass optical fiber have broadband and strong yellow light emission. By controlling the degree of crystallization and size of microcrystals, its broadband luminescence performance is outstanding, which is comparable to the common Dy 3+ The comparison of doped crystals is as follows:

[0031] Material half maximum width FWHM (nm) @~575 nm References Y3Al5O12: Dy3+<7Bowman SR, Connor SO, Condon N J. Diode pumped yellow dysprosium lasers[J]. Optics Express, 2012, 20(12): 12906-12911.ZnWO4: Dy3+6.50Xia ZC, Yang FG, Qiao L, et al. End pumped yellow laser performance of Dy3+:ZnWO4[J]. Optics Communications, 2017, 387: 357-360.CaYAlO4: Dy3+8~12Chen H, Loiseau P, Aka G. Optical properties of Dy3+-doped CaYAlO4 crystal[J]. Journal of Luminescence, 2018, 199: 509-515.NaLa(WO4)2: Dy3+10~13Wei YP, Tu CY, Wang HY, et al. Optical spectroscopy of NaLa(WO4)2:Dy3+ single crystal[J]. Journal of Alloys and Compounds, 2007, 438(1-2): 310-316.NaLa(WO4)2:Dy3+ microcrystalline composite glass fiber 18~22

[0032] (2) The present invention provides a microcrystalline composite glass optical fiber with broadband yellow light emission. Through material design, the cladding is made of quartz glass and has good compatibility with existing optical fiber systems.

[0033] (3) The present invention provides a method for preparing a microcrystalline composite glass optical fiber with broadband yellow light emission. The preform rod preparation process has wide applicability and low cost. The core ceramic rod components can be adjusted according to application requirements. The drawing process is mature and can be drawn using a commercial drawing tower.

[0034] (4) The present invention provides a method for preparing a microcrystalline composite glass optical fiber with broadband yellow light emission. The composite optical fiber precursor is prepared based on the core melt drawing method, and then subjected to heat treatment to obtain a microcrystalline glass composite optical fiber with a controllable degree of crystallization, and the optical fiber maintains a low transmission loss.

[0035] (5) The broadband yellow light emitting microcrystalline composite glass optical fiber of the present invention can be used in yellow light fiber lasers, especially in tunable or ultrafast yellow light fiber lasers. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] FIG1 is an excitation spectrum diagram of a microcrystalline composite glass optical fiber with broadband yellow light emission prepared in Example 1 of the present invention.

[0037] FIG2 is a graph showing the visible emission spectrum of the broadband yellow light emitting microcrystalline composite glass optical fiber prepared in Example 3 of the present invention under the excitation of a blue semiconductor laser.

[0038] FIG3 is a transmission electron microscope image of a microcrystalline composite glass optical fiber with broadband yellow light emission prepared in Example 4 of the present invention.

[0039] DETAILED DESCRIPTION

[0040] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, which does not limit the scope of protection thereof.

[0041] The quartz glass tube used in the embodiment was processed as follows: first, it was pickled and dried, and then one end was sealed by taper.

[0042] Example 1

[0043] Sodium carbonate powder (purity ≥ 99.9%), tungsten oxide powder (purity ≥ 99.99%), lanthanum oxide powder (purity ≥ 99.99%), and dysprosium oxide powder (purity ≥ 99.99%) were ground into powder in a mortar with a stoichiometric ratio of 1, 0.93, and 0.07, respectively. The mixed powders were then sintered in a muffle furnace at 1100°C for 8 h. The pure NaLa(WO4)2:Dy 3+ The sample was reground and added with 0.5% by mass (relative to pure phase NaLa(WO4)2:Dy 3+The sample was placed in a mold and pressed into a strip-shaped block. The pressed sample was sintered in a muffle furnace at 1150 ºC for 6 h. The sintered strip ceramic rod was then ground into a cylinder with a diameter of 3.8 mm and a length of 6 cm. The core ceramic rod was placed in a quartz glass tube with an inner diameter of 4 mm, an outer diameter of 25 mm and a length of 15 cm to obtain an optical fiber preform. The preform was then placed in a vacuum high-temperature graphite furnace and drawn into an optical fiber at a high temperature of 1980 ºC, which is higher than the melting temperature of the core material. The core diameter of the optical fiber was 10 μm and the outer diameter of the cladding was 125 μm. Finally, the NaLa(WO4)2:Dy prepared above was 3+ The crystal derived fiber was heat treated in a muffle furnace at 900 ºC for 4 h to obtain NaLa(WO4)2:Dy 3+ Microcrystalline composite glass optical fiber.

[0044] The excitation spectrum of the microcrystalline composite glass fiber was measured using an Edinburgh spectrometer FLS920. The emission spectrum of the microcrystalline composite glass fiber was measured using an Ocean Maya2000 Pro fiber spectrometer, with a 450 nm semiconductor laser as the excitation source. The microstructure of the nanocrystals in the microcrystalline composite glass fiber was observed using a FEI Talos F200x transmission electron microscope.

[0045] The excitation spectrum of the broadband yellow light-emitting microcrystalline composite glass fiber prepared in Example 1 is shown in Figure 1. As can be seen from Figure 1, the half-width at half-maximum of the excitation peak of the fiber in the blue light band can reach 7 nm. This shows that the fiber of the present invention can be well matched with a commercial 450 nm pump source and is conducive to improving the pump absorption efficiency, thereby facilitating the realization of tunable or ultrafast yellow laser direct output.

[0046] Example 2

[0047] Sodium carbonate powder (purity ≥ 99.9%), tungsten oxide powder (purity ≥ 99.99%), lanthanum oxide powder (purity ≥ 99.99%), and dysprosium oxide powder (purity ≥ 99.99%) were ground thoroughly in a mortar with a stoichiometric ratio of 1, 0.94, and 0.06, respectively. The mixed powders were then sintered in a muffle furnace at 1100°C for 10 h. The pure NaLa(WO4)2:Dy 3+ The sample was reground and added with 0.5% by mass (relative to pure phase NaLa(WO4)2:Dy 3+The sample was placed in a mold and pressed into a strip-shaped block. The pressed sample was sintered in a muffle furnace at 1050 ºC for 8 h. The sintered strip ceramic rod was then ground into a cylinder with a diameter of 3.8 mm and a length of 6 cm. The core ceramic rod was placed in a quartz glass tube with an inner diameter of 4 mm, an outer diameter of 25 mm and a length of 15 cm to prepare an optical fiber preform. The preform was then placed in a vacuum high-temperature graphite furnace and drawn into an optical fiber at a high temperature of 2000 ºC, which is higher than the melting temperature of the core material. The core diameter of the optical fiber was 15 μm and the outer diameter of the cladding was 130 μm. Finally, the NaLa(WO4)2:Dy prepared above was 3+ The crystal derived fiber was heat treated in a muffle furnace at 950 ºC for 3 h to obtain NaLa(WO4)2:Dy 3+ Microcrystalline composite glass optical fiber.

[0048] The excitation spectrum of the microcrystalline composite glass fiber was measured using an Edinburgh spectrometer FLS920. The emission spectrum of the microcrystalline composite glass fiber was measured using an Ocean Maya2000 Pro fiber spectrometer, with a 450 nm semiconductor laser as the excitation source. The microstructure of the nanocrystals in the microcrystalline composite glass fiber was observed using a FEI Talos F200x transmission electron microscope.

[0049] Example 3

[0050] Sodium carbonate powder (purity ≥ 99.9%), tungsten oxide powder (purity ≥ 99.99%), lanthanum oxide powder (purity ≥ 99.99%), and dysprosium oxide powder (purity ≥ 99.99%) were ground into powder in a mortar with a stoichiometric ratio of 1, 0.95, and 0.05, respectively. The mixed powders were then sintered in a muffle furnace at 1100°C for 7 h. The pure NaLa(WO4)2:Dy 3+ The sample was reground and added with 0.5% by mass (relative to pure phase NaLa(WO4)2:Dy 3+ The sample was placed in a mold and pressed into a strip-shaped block. The pressed sample was sintered in a muffle furnace at 1100 ºC for 9 h. The sintered strip ceramic rod was then ground into a cylinder with a diameter of 3.8 mm and a length of 8 cm. The core ceramic rod was placed in a quartz glass tube with an inner diameter of 4 mm, an outer diameter of 25 mm and a length of 15 cm to prepare an optical fiber preform. The preform was then placed in a vacuum high-temperature graphite furnace and drawn into an optical fiber at a high temperature of 2010 ºC, which is higher than the melting temperature of the core material. The core diameter of the optical fiber was 8 μm and the outer diameter of the cladding was 125 μm. Finally, the NaLa(WO4)2:Dy prepared above was 3+The crystal-derived fiber was heat-treated in a muffle furnace at 980 °C for 4 h to obtain NaLa(WO4)2:Dy 3+ Microcrystalline composite glass optical fiber.

[0051] The excitation spectrum of the microcrystalline composite glass fiber was measured using an Edinburgh spectrometer FLS920. The emission spectrum of the microcrystalline composite glass fiber was measured using an Ocean Maya2000 Pro fiber spectrometer, with a 450 nm semiconductor laser as the excitation source. The microstructure of the nanocrystals in the microcrystalline composite glass fiber was observed using a FEI Talos F200x transmission electron microscope.

[0052] The visible emission spectrum of the broadband yellow light emitting microcrystalline composite glass fiber prepared in Example 3 under the excitation of a blue light semiconductor laser is shown in FIG2 . As can be seen from FIG2 , the half-maximum width of the emission peak of the fiber at 575 nm can reach 20 nm, which is relatively common in Dy 3+ The broadband luminescence performance of the doped crystal is outstanding, which is conducive to the direct output of tunable or ultrafast yellow laser.

[0053] Example 4

[0054] Sodium carbonate powder (purity ≥ 99.9%), tungsten oxide powder (purity ≥ 99.99%), lanthanum oxide powder (purity ≥ 99.99%), and dysprosium oxide powder (purity ≥ 99.99%) were ground thoroughly in a mortar with a stoichiometric ratio of 1, 0.96, and 0.04, respectively. The mixed powders were then sintered in a muffle furnace at 1200°C for 6 h. The pure NaLa(WO4)2:Dy 3+ The sample was reground and added with 0.5% by mass (relative to pure phase NaLa(WO4)2:Dy 3+ The sample was placed in a mold and pressed into a strip-shaped block. The pressed sample was sintered in a muffle furnace at 1000 ºC for 10 h. The sintered strip ceramic rod was then ground into a cylinder with a diameter of 3.8 mm and a length of 6 cm. The core ceramic rod was placed in a quartz glass tube with an inner diameter of 4 mm, an outer diameter of 25 mm and a length of 15 cm to obtain an optical fiber preform. The preform was then placed in a vacuum high-temperature graphite furnace and drawn into an optical fiber at a high temperature of 1990 ºC, which is higher than the melting temperature of the core material. The core diameter of the optical fiber was 5 μm and the outer diameter of the cladding was 120 μm. Finally, the NaLa(WO4)2:Dy prepared above was 3+ The crystal derived fiber was heat treated in a muffle furnace at 960 ºC for 6 h to obtain NaLa(WO4)2:Dy 3+ Microcrystalline composite glass optical fiber.

[0055] The excitation spectrum of the microcrystalline composite glass fiber was measured using an Edinburgh spectrometer FLS920. The emission spectrum of the microcrystalline composite glass fiber was measured using an Ocean Maya2000 Pro fiber spectrometer, with a 450 nm semiconductor laser as the excitation source. The microstructure of the nanocrystals in the microcrystalline composite glass fiber was observed using a FEI Talos F200x transmission electron microscope.

[0056] The transmission electron microscope image of the broadband yellow light emitting microcrystalline composite glass fiber prepared in Example 4 is shown in FIG3 . FIG3 a shows that the crystals precipitated in the microcrystalline glass fiber are nanocrystals with a diameter of 4 to 6 nm. FIG3 b shows a high-resolution lattice fringe image, which shows that the NaLa(WO4)2:Dy 3+ Nanocrystals will not cause significant scattering losses, allowing the optical fiber to maintain low transmission loss, which is conducive to the direct output of tunable or ultrafast yellow lasers.

[0057] Example 5

[0058] Sodium carbonate powder (purity ≥ 99.9%), tungsten oxide powder (purity ≥ 99.99%), lanthanum oxide powder (purity ≥ 99.99%), and dysprosium oxide powder (purity ≥ 99.99%) were ground into powder in a mortar with a stoichiometric ratio of 1, 0.97, and 0.03, respectively. The mixed powders were then sintered in a muffle furnace at 1000°C for 9 h. The pure NaLa(WO4)2:Dy 3+ The sample was reground and added with 0.5% by mass (relative to pure phase NaLa(WO4)2:Dy 3+ The sample was placed in a mold and pressed into a strip-shaped block. The pressed sample was sintered in a muffle furnace at 1200 ºC for 9 h. The sintered strip ceramic rod was then ground into a cylinder with a diameter of 3.8 mm and a length of 8 cm. The core ceramic rod was placed in a quartz glass tube with an inner diameter of 4 mm, an outer diameter of 25 mm and a length of 15 cm to obtain an optical fiber preform. The preform was then placed in a vacuum high-temperature graphite furnace and drawn into an optical fiber at a high temperature of 2000 ºC, which is higher than the melting temperature of the core material. The core diameter of the optical fiber was 13 μm and the outer diameter of the cladding was 127 μm. Finally, the NaLa(WO4)2:Dy prepared above was 3+ The crystal derived fiber was heat treated in a muffle furnace at 1000 ºC for 3 h to obtain NaLa(WO4)2:Dy 3+ Microcrystalline composite glass optical fiber.

[0059] The excitation spectrum of the microcrystalline composite glass fiber was measured using an Edinburgh spectrometer FLS920. The emission spectrum of the microcrystalline composite glass fiber was measured using an Ocean Maya2000 Pro fiber spectrometer, with a 450 nm semiconductor laser as the excitation source. The microstructure of the nanocrystals in the microcrystalline composite glass fiber was observed using a FEI Talos F200x transmission electron microscope.

[0060] The above embodiments are preferred implementation methods of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A microcrystalline composite glass optical fiber with broadband yellow light emission, characterized in that: Its cladding is quartz glass and its core is Dy 3+ Doped NaLa(WO4)2 glass-ceramics.

2. The microcrystalline composite glass optical fiber with broadband yellow light emission according to claim 1, characterized in that: The Dy 3+ The chemical formula of doped NaLa(WO4)2 glass-ceramics is NaLa ( 1-x ) (WO4)2:xDy 3+ , x=0.03~0.

07.

3. The broadband yellow light emitting microcrystalline composite glass optical fiber according to claim 1, characterized in that: The core diameter of the microcrystalline composite glass optical fiber is 5-20 μm, and the outer diameter of the cladding is 120-130 μm.

4. The microcrystalline composite glass optical fiber with broadband yellow light emission according to claim 1, characterized in that: The microcrystalline composite glass optical fiber obtains 18-22 nm broadband yellow light emission under the pumping of a blue light semiconductor laser.

5. The broadband yellow light emitting microcrystalline composite glass optical fiber according to claim 1, characterized in that: The precursor of the fiber core is a fiber core ceramic rod; the preparation method of the fiber core ceramic rod comprises the following steps: (a) Sodium carbonate powder, tungsten oxide powder, lanthanum oxide powder and dysprosium oxide powder are mixed, ground and sintered; (b) The powder sintered in step (a) is ground, a binder is added, pressed into a shape, sintered and ground into a cylinder to obtain a core ceramic rod.

6. The microcrystalline composite glass optical fiber with broadband yellow light emission according to claim 5, characterized in that: In step (a), the purity of the sodium carbonate powder is ≥99.9%, the purity of the tungsten oxide powder is ≥99.99%, the purity of the lanthanum oxide powder is ≥99.99%, and the purity of the dysprosium oxide powder is ≥99.99%; The amount ratio of the sodium carbonate powder, tungsten oxide powder, lanthanum oxide powder and dysprosium oxide powder is 1:4:0.93-0.97:0.03-0.

07.

7. The microcrystalline composite glass optical fiber with broadband yellow light emission according to claim 5, characterized in that: The sintering temperature in step (a) is 1000-1200°C for 6-10 h; the sintering is carried out in a muffle furnace.

8. The microcrystalline composite glass optical fiber with broadband yellow light emission according to claim 5, characterized in that: The binder in step (b) is a PVA binder, and its mass percentage is 0.1-1.5% of the sintered powder; the sintering temperature is 1000-1200 ºC, and the time is 6-10 h; and the sintering is carried out in a muffle furnace.

9. The method for preparing a microcrystalline composite glass optical fiber with broadband yellow light emission according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) First, pickle and dry the quartz glass tube, and then seal one end by taper; (2) Placing the fiber core ceramic rod in a quartz glass tube to obtain an optical fiber preform; (3) Drawing the optical fiber preform at a high temperature of 1950-2010°C to obtain an optical fiber precursor; (4) The optical fiber precursor is heat treated at 900-1000°C for 3-6 hours to obtain a microcrystalline composite glass optical fiber with broadband yellow light emission.

10. The preparation method according to claim 9, characterized in that: The wire drawing in step (3) is carried out in a high temperature graphite furnace of Rasta; The heat treatment in step (4) is carried out in a muffle furnace.

Citation Information

Patent Citations

  • Low-loss high-strength all-glass optical fiber in 2 to 5 micron wave band and preparation method thereof

    CN109574509A

  • Dy&lt;3+&gt;-doped phosphate glass for outputting yellow laser, optical fiber and preparation method of Dy&lt;3+&gt;-doped phosphate glass

    CN113087388A

  • Microcrystal composite glass optical fiber capable of emitting broadband yellow light and preparation method of microcrystal composite glass optical fiber

    CN116589196A

  • High power low-loss fiber waveguide

    CN1726414A

  • Device for growing single crystals of refractory oxides

    SU1629361A1