Adhesive suitable for solar cells, and preparation and use thereof
By developing a copolymer adhesive, the problem of insufficient bonding strength and weather resistance of solar cell backsheet adhesives has been solved, achieving high adhesion and durability and suitable for long-term use of solar cell backsheets.
Patent Information
- Application Number
- PCT/CN2024/080563
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-31
AI Technical Summary
Existing adhesives for solar cell backsheets have limited bonding strength and insufficient weather resistance to meet long-term UV exposure and durability requirements.
A copolymer adhesive was developed, which contains fluorinated monomers and vinyl ester monomers and is prepared through polymerization. It is suitable for combining fluoropolymer films with fluorine-free matrix layers to improve bonding strength and weather resistance. .
It achieves high adhesion and bonding strength, significantly improving the weather resistance and durability of the solar cell backsheet, especially its excellent performance under long-term ultraviolet irradiation.
Smart Images

Figure CN2024080563_31102024_PF_FP_ABST
Abstract
Description
Adhesive suitable for solar cells and its preparation and use Technical Field
[0001] The present application relates to the field of solar cells, and more specifically to a copolymeric binder suitable for solar cells, a synthesis method thereof, and uses thereof. Background Art
[0002] As a device that utilizes renewable energy, solar cells have received increasing attention in the past decade and have been industrialized. However, current solar cells still have a large number of technical defects that need further improvement to meet the market's increasingly high requirements for market scalability, low cost and equipment performance.
[0003] Improvements to solar cells focus on their various components. For example, adhesives used to manufacture solar panels, especially adhesives used for their backsheets, are one of the key research targets. The backsheet is a photovoltaic encapsulation material used on the back of a solar cell module and is in direct contact with the external environment over a large area. It needs to have excellent weather resistance, electrical insulation resistance, water vapor barrier properties, and other properties. Currently, the most commonly used solar cell backsheet on the market is a backsheet with a three-layer composite structure. The upper and lower layers are fluorine-containing polymer films, such as polyvinyl fluoride (PVF) or polyvinylidene fluoride (PVDF), and the base layer is mostly a fluorine-free polymer film, such as polyethylene terephthalate (PET). However, due to the low surface energy of the fluorine-containing film, it is difficult to composite it with the high surface energy PET film of the base layer. Therefore, it is necessary to use an adhesive to composite the three layers of materials to produce a solar cell backsheet. The currently commonly used adhesives have limited bonding strength with the fluorine-containing polymer film of the backsheet and are prone to aging, resulting in the fluorine-containing polymer film easily peeling off from the base layer of the fluorine-free material, and the performance cannot meet the 25-year durability requirement.
[0004] To overcome the aforementioned issues of bond strength and weather resistance between fluoropolymer films and adhesives, researchers have conducted numerous experiments, including modifying various material components, using physical and chemical treatments, and surface modifications. However, the results have been quite unsatisfactory, and to date, no adhesive material has truly resolved these issues. Consequently, there is an urgent need to develop an adhesive that exhibits high adhesion and bond strength to fluoropolymer films while also exhibiting excellent weather resistance under long-term, sustained UV exposure outdoors.
[0005] Summary of the Invention
[0006] In response to the above problems, the inventors of the present application conducted in-depth research and successfully developed an adhesive material, thereby effectively solving the long-standing problem in the prior art that urgently needs to be solved.
[0007] The first aspect of the present application provides an adhesive, comprising a copolymer comprising copolymerized structural units derived from the following monomers:
[0008] Monomer A: a fluorinated monomer represented by formula I;
[0009] In Formula I, R1, R2 and R3 are each independently selected from the group consisting of hydrogen, fluorine, chlorine, C1-C12 alkyl, partially fluorinated or perfluorinated C1-C12 alkyl, C3-C12 cycloalkyl, partially fluorinated or perfluorinated C3-C12 cycloalkyl, C6-C12 aryl, partially fluorinated or perfluorinated C6-C12 aryl, C2-C12 alkenyl, partially fluorinated or perfluorinated C2-C12 alkenyl;
[0010] Monomer B: Monomer represented by formula II:
[0011] In Formula II, R4, R5 and R6 are each independently selected from the group consisting of hydrogen, C1-C12 alkyl, C1-C12 alkoxy, C3-C12 cycloalkyl, C3-C12 cycloalkoxy, C2-C12 alkenyl, C6-C12 aryl, C6-C12 aryloxy, C2-C12 alkenyl, C2-C12 alkenyloxy; R7 is selected from the group consisting of hydrogen, fluorine, C1-C18 alkyl; and
[0012] Optional monomer C: a C1-C8 fluorine-free olefin monomer represented by formula III;
[0013] In formula III, R8, R9, R 10 and R 11 Each is independently selected from the group consisting of hydrogen, C1-C12 alkyl, C1-C12 alkoxy, C3-C12 cycloalkyl, C3-C12 cycloalkoxy, C2-C12 alkenyl, C6-C12 aryl, C6-C12 aryloxy, and C2-C12 alkenyl.
[0014] According to one embodiment of the first aspect of the present application, based on the total molar amount of all comonomers in the copolymer, the content of monomer A is 1-40 mol%. According to another embodiment of the first aspect of the present application, based on the total molar amount of all comonomers in the copolymer, the content of monomer B is 60-99 mol%. According to another embodiment of the first aspect of the present application, based on the total molar amount of all comonomers in the copolymer, the content of monomer C is 0-5 mol%.
[0015] According to another embodiment of the first aspect of the present application, the monomer A is selected from at least one of the following: tetrafluoroethylene, hexafluoropropylene, perfluoro-1-butene, perfluoro-2-butene, perfluoroisobutylene, perfluoro-1-n-pentene, perfluoro-2-n-pentene, perfluoroisopentene, perfluoro-1-hexene, perfluoro-2-methyl-2-pentene, and trifluoromonochloroethylene.
[0016] According to another embodiment of the first aspect of the present application, the monomer B is selected from at least one of the following: vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl stearate.
[0017] According to another embodiment of the first aspect of the present application, the monomer C is selected from at least one of the following: ethylene, propylene, n-butene, isobutylene, butadiene, 1-pentene, cyclobutene, 2-pentene, isopentene, isoprene, cyclopentadiene, and styrene.
[0018] According to another embodiment of the first aspect of the present application, the number average molecular weight Mn of the copolymer is 20,000-1,000,000.
[0019] The second aspect of the present application provides a method for synthesizing the adhesive of the present application, which comprises carrying out a polymerization reaction of the monomer A, the monomer B and optionally the monomer C in a polymerization reactor.
[0020] According to one embodiment of the second aspect of the present application, during the polymerization reaction, the polymerization reactor further contains at least one of the following components: water, a dispersant, a stabilizer, and an initiator. According to another embodiment of the second aspect of the present application, the polymerization reaction is carried out at a temperature of 55-100° C. and a pressure of 0.6-2.8 MPa.
[0021] The third aspect of the present application provides a backboard, which includes one or more layers of fluoropolymer film and one or more base layers, the material of the base layer being different from the material of the fluoropolymer film, the one or more base layers being combined with the fluoropolymer film using an adhesive, and the adhesive is the adhesive of the present application.
[0022] The fourth aspect of the present application provides a solar cell, which includes a transparent protective sheet, a cell sheet, a backplane and a frame, wherein the backplane is the backplane described in the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The following paragraphs discuss various embodiments of the present application with reference to the accompanying drawings. However, it should be noted that the embodiments shown in the drawings and described below are merely preferred embodiments of the present application. The scope of protection of the present application is defined by the claims and is not limited to these preferred embodiments. Furthermore, for the purpose of clarity, the reactors and components shown in the drawings are not drawn to scale.
[0024] FIG1 shows a cross-sectional view of a back plate according to one embodiment of the present application;
[0025] FIG2 shows a schematic diagram of a solar cell according to one embodiment of the present application. DETAILED DESCRIPTION
[0026] "Range" disclosed herein is in the form of a lower limit and an upper limit. It can be one or more lower limits, and one or more upper limits, respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e., any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values listed are 1 and 2, and if the maximum range values listed are 3, 4, and 5, then the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5.
[0027] In this application, unless otherwise specified, the numerical range "ab" is an abbreviation for any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is merely an abbreviation for these numerical combinations.
[0028] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0029] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0030] In this application, unless otherwise specified, the term "comprising" as used herein may be open-ended or closed-ended. For example, "comprising" may mean that other components not listed may also be included, or only the listed components may be included.
[0031] In this application, the terms "solar cell", "solar panel", "solar cell module", "photovoltaic panel" and "photovoltaic module" can be used interchangeably to refer to solar cells manufactured using the technology of this application.
[0032] In this application, the term "polymerized structural unit / copolymerized structural unit derived from a monomer" refers to a structural unit formed as part of the copolymer backbone by addition polymerization of the monomer's carbon-carbon double bond. The original composition, substituents, and structure of the monomer are retained within the resulting copolymer structural unit, but may also undergo appropriate changes through chemical reactions. For example, the vinyl ester monomer represented by Formula II may undergo a small amount of hydrolysis during or after polymerization, converting the ester groups pendant to the backbone into hydroxyl groups pendant to the backbone.
[0033] In the present application, monomer C is an optional component. Therefore, the comonomers used in the preparation of the copolymer of the present invention may only include monomer A and monomer B without monomer C; it is also possible that the comonomers used in the preparation of the copolymer of the present invention include monomer A, monomer B and monomer C at the same time.
[0034] According to one embodiment of the present application, the monomer A is a fluorinated monomer having a structure shown in Formula I:
[0035] According to one embodiment of the present application, in Formula I, R1, R2 and R3 are each independently selected from the group consisting of: hydrogen, fluorine, chlorine, C1-C12 alkyl, partially fluorinated or perfluorinated C1-C12 alkyl, C3-C12 cycloalkyl, partially fluorinated or perfluorinated C3-C12 cycloalkyl, C6-C12 aryl, partially fluorinated or perfluorinated C6-C12 aryl, C2-C12 alkenyl, partially fluorinated or perfluorinated C2-C12 alkenyl. According to another embodiment of the present application, in Formula I, R1, R2 and R3 are each independently selected from the group consisting of: hydrogen, fluorine, chlorine, C1-C10 alkyl, partially fluorinated or perfluorinated C1-C10 alkyl, C3-C10 cycloalkyl, partially fluorinated or perfluorinated C3-C10 cycloalkyl, C6-C10 aryl, partially fluorinated or perfluorinated C6-C10 aryl, C2-C10 alkenyl, partially fluorinated or perfluorinated C2-C10 alkenyl. According to another embodiment of the present application, in Formula I, R1, R2 and R3 are each independently selected from the group consisting of: hydrogen, fluorine, chlorine, C1-C8 alkyl, partially fluorinated or perfluorinated C1-C8 alkyl, C3-C8 cycloalkyl, partially fluorinated or perfluorinated C3-C8 cycloalkyl, C6-C8 aryl, partially fluorinated or perfluorinated C6-C8 aryl, C2-C8 alkenyl, partially fluorinated or perfluorinated C2-C8 alkenyl. According to another embodiment of the present application, in Formula I, R1, R2 and R3 are each independently selected from the group consisting of: hydrogen, fluorine, chlorine, C1-C6 alkyl, partially fluorinated or perfluorinated C1-C6 alkyl, C3-C6 cycloalkyl, partially fluorinated or perfluorinated C3-C6 cycloalkyl, C6-C7 aryl, partially fluorinated or perfluorinated C6-C7 aryl, C2-C6 alkenyl, partially fluorinated or perfluorinated C2-C6 alkenyl.
[0036] In this application, when a group or compound is described as "fully fluorinated", "fully fluorinated", "perfluorinated" or "perfluorinated", it means that all hydrogen atoms connected to carbon atoms through C-H bonds in the group or compound have been 100% replaced by fluorine. When a group or compound is described as "partially fluorinated" or "partially fluorinated", it means that a portion of the hydrogen atoms connected to carbon atoms through C-H bonds in the group or compound are replaced by fluorine, for example, the proportion of hydrogen atoms replaced by fluorine atoms can be 2-95%, or 5-90%, or 10-85%, or 15-80%, or 20-75%, or 25-70%, or 30-65%, or 35-60%, or 40-55%, or 45-50%, and the above proportions are calculated relative to the total number of hydrogen atoms connected to carbon atoms through C-H bonds in the group or compound.
[0037] According to a specific embodiment of the present application, the monomer A is selected from at least one of the following: tetrafluoroethylene, hexafluoropropylene, perfluoro-1-butene, perfluoro-2-butene, perfluoroisobutylene, perfluoro-1-n-pentene, perfluoro-2-n-pentene, perfluoroisopentene, perfluoro-1-hexene, perfluoro-2-methyl-2-pentene, and trifluoromonochloroethylene; more specifically, the monomer A can be tetrafluoroethylene.
[0038] According to one embodiment of the present application, based on the total molar amount of all monomers used to prepare the copolymer, the molar content of the monomer A can be 1-40 mol%, for example, 5-38 mol%, or 7-36 mol%, or 8-35 mol%, or 10-32 mol%, or 12-30 mol%, or 15-28 mol%, or 18-26 mol%, or 20-24 mol%, or 22-23 mol, or can be within the numerical range obtained by combining any two of the above end values.
[0039] According to one embodiment of the present application, the monomer B is a vinyl ester monomer having a structure shown in Formula II:
[0040] According to another embodiment of the present application, in Formula II, R4, R5, and R6 are each independently selected from the group consisting of hydrogen, C1-C12 alkyl, C1-C12 alkoxy, C3-C12 cycloalkyl, C3-C12 cycloalkoxy, C2-C12 alkenyl, C6-C12 aryl, C6-C12 aryloxy, C2-C12 alkenyl, and C2-C12 alkenyloxy; and R7 is selected from the group consisting of hydrogen, fluorine, and C1-C18 alkyl. According to another embodiment of the present application, in Formula II, R4, R5, and R6 are each independently selected from the group consisting of hydrogen, C1-C10 alkyl, C1-C10 alkoxy, C3-C10 cycloalkyl, C3-C10 cycloalkoxy, C2-C10 alkenyl, C6-C10 aryl, C6-C10 aryloxy, C2-C10 alkenyl, and C2-C10 alkenyloxy; and R7 is selected from the group consisting of hydrogen, fluorine, and C1-C16 alkyl. According to another embodiment of the present application, in Formula II, R4, R5 and R6 are each independently selected from the group consisting of hydrogen, C1-C8 alkyl, C1-C8 alkoxy, C3-C8 cycloalkyl, C3-C8 cycloalkoxy, C2-C8 alkenyl, C6-C8 aryl, C6-C8 aryloxy, C2-C8 alkenyl, C2-C8 alkenyloxy; and R7 is selected from the group consisting of hydrogen, fluorine, and C1-C12 alkyl. According to another embodiment of the present application, in Formula II, R4, R5 and R6 are each independently selected from the group consisting of hydrogen, C1-C6 alkyl, C1-C6 alkoxy, C3-C6 cycloalkyl, C3-C6 cycloalkoxy, C2-C6 alkenyl, C6-C7 aryl, C6-C7 aryloxy, C2-C6 alkenyl, C2-C6 alkenyloxy; and R7 is selected from the group consisting of hydrogen and C1-C6 alkyl.
[0041] According to a specific embodiment of the present application, the monomer B is selected from at least one of the following: vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl stearate; for example, the monomer B may be vinyl acetate.
[0042] According to one embodiment of the present application, based on the total molar amount of all monomers used to prepare the copolymer, the molar content of the monomer B can be 60-99 mol%, for example, 62-98 mol%, or 65-96 mol%, or 68-95 mol%, or 70-92 mol%, or 72-90 mol%, or 74-86 mol%, or 75-85 mol%, or 78-82 mol%, or 79-80 mol, or can be within the numerical range obtained by combining any two of the above end values.
[0043] According to one embodiment of the present application, when the copolymer further comprises monomer C, monomer C may be a C1-C8 olefin monomer having a structure represented by formula III, in particular a fluorine-free C1-C8 olefin monomer.
[0044] In Formula III, R8, R9, R 10 and R 11 Each is independently selected from the group consisting of: hydrogen, C1-C12 alkyl, C1-C12 alkoxy, C3-C12 cycloalkyl, C3-C12 cycloalkoxy, C2-C12 alkenyl, C6-C12 aryl, C6-C12 aryloxy, C2-C12 alkenyl. According to another embodiment of the present application, in formula III, R8, R9, R 10 and R 11 Each is independently selected from the group consisting of: hydrogen, C1-C10 alkyl, C1-C10 alkoxy, C3-C10 cycloalkyl, C3-C10 cycloalkoxy, C2-C10 alkenyl, C6-C10 aryl, C6-C10 aryloxy, C2-C10 alkenyl. According to another embodiment of the present application, in formula III, R8, R9, R 10 and R 11 Each is independently selected from the group consisting of: hydrogen, C1-C8 alkyl, C1-C8 alkoxy, C3-C8 cycloalkyl, C3-C8 cycloalkoxy, C2-C8 alkenyl, C6-C8 aryl, C6-C8 aryloxy, C2-C8 alkenyl. According to another embodiment of the present application, in formula III, R8, R9, R 10 and R 11 Each is independently selected from the group consisting of: hydrogen, C1-C6 alkyl, C1-C6 alkoxy, C3-C6 cycloalkyl, C3-C6 cycloalkoxy, C2-C6 alkenyl, C6-C7 aryl, C6-C7 aryloxy, and C2-C6 alkenyl.
[0045] According to a specific embodiment of the present application, the monomer C is selected from at least one of the following: ethylene, propylene, n-butene, isobutylene, butadiene, 1-pentene, cyclobutene, 2-pentene, isopentene, isoprene, cyclopentadiene, and styrene; for example, the monomer C may be ethylene.
[0046] According to one embodiment of the present application, based on the total molar amount of all monomers used to prepare the copolymer, the molar content of the monomer C can be 0-5 mol%, for example, 0.5-4.5 mol%, or 1-4 mol%, or 1.5-3.5 mol%, or 2-3 mol%, or 2.2-2.5 mol%, or can be within the numerical range obtained by combining any two of the above end values.
[0047] According to one embodiment of the present application, the molecular weight (in terms of number-average molecular weight Mn) of the copolymer can be 20,000-1,000,000, for example, 30,000-900,000, or 40,000-800,000, or 50,000-700,000, or 60,000-600,000, or 70,000-500,000, or 80,000-400,000, or 90,000-300,000, or 100,000-200,000, or can be within the numerical range obtained by combining any two of the above end values. The number-average molecular weight can be characterized by techniques known in the art, for example, end group analysis, membrane permeation method, etc., and the molecular weight of the copolymer can be detected by the above method using a commercial molecular weight meter, according to the instrument manual or standard method.
[0048] According to another embodiment of the present application, the intrinsic viscosity of the copolymer product prepared by the present invention is 0.6-3.0 dL / g, for example, 0.8-2.8 dL / g, or 1.0-2.5 dL / g, or 1.2-2.3 dL / g, or 1.5-2.0 dL / g, or 1.6-1.8 dL / g, or within the numerical range obtained by combining any two of the above end values. The intrinsic viscosity can be measured using equipment, steps, and formulas known in the art, for example, the intrinsic viscosity of the copolymer can be measured according to standard methods such as GB / T 1548-2016 and STAS 7614-1988.
[0049] The present application also provides a method for preparing the copolymer, which comprises carrying out a polymerization reaction of the monomer A, the monomer B and optionally the monomer C in a polymerization reactor.
[0050] According to an embodiment of the application, in the polyreaction, in addition to the above-mentioned polymerizable monomers, one or more other components, such as water, dispersant, stabilizer, initiator etc. can also be used.The water can be distilled water, deionized water, double distilled water or ultrapure water, preferably deionized water. Taking the gross weight of all monomers for reacting as 100 weight parts, the consumption of the water used can be 50-200 weight part, such as 70-180 weight part, or 80-160 weight part, or 90-140 weight part, or 100-130 weight part, or 110-128 weight part, or 120-125 weight part, or within the numerical range that can be obtained by combining the above-mentioned arbitrary two end values.
[0051] The dispersant is used to improve the dispersibility of the raw materials, intermediate products, and final products in the reaction system to promote uniform reaction throughout the reactor. Exemplary dispersants for the polymerization reaction system of the present invention include perfluorinated carboxylates, particularly perfluorinated carboxylates, such as ammonium perfluorooctanoate. Based on 100 parts by weight of the total weight of all monomers used in the reaction, the amount of the dispersant used can be 0.01-20 parts by weight, for example, 0.05-15 parts by weight, or 0.1-12 parts by weight, or 0.12-10 parts by weight, or 0.15-5 parts by weight, or 0.18-2 parts by weight, or 0.20-1 part by weight, or 0.25-0.6 parts by weight, or 0.30-0.50 parts by weight, or within a numerical range obtained by combining any two of the above values.
[0052] Described stabilizer is used for making in the reactor have stable process operation conditions in the polymerization reaction process, improves the stability of reaction system thus, preferably adopts stable performance, will not cause any negative impact to polymerization reaction, and is easy to separate stabilizer after polymerization reaction is completed.Described stabilizer example includes paraffin, resin microsphere etc.With the gross weight of all monomers for reacting as 100 weight parts, the consumption of the stabilizer used can be 1-50 weight part, for example 2-45 weight part, Or 3-40 weight part, or 4-35 weight part, or 5-30 weight part, or 6-25 weight part, or 7-20 weight part, or 8-15 weight part, or 8.2-10 weight part, or can be within the numerical range that above-mentioned any two end values are combined with each other and obtain.
[0053] The initiator is used to provide free radicals to initiate the free radical polymerization reaction of the monomers of the present invention. The initiator can be various peroxide initiators known in the art, such as peroxysuccinic acid, ammonium persulfate, hydrogen peroxide, tert-butyl hydroperoxide, potassium persulfate, benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, etc. Based on the total weight of all monomers used for the reaction as 100 parts by weight, the amount of the initiator used can be 0.001-1 part by weight, such as 0.005-0.8 part by weight, or 0.01-0.6 part by weight, or 0.012-0.5 part by weight, or 0.015-0.2 part by weight, or 0.018-0.1 part by weight, or 0.019-0.08 part by weight, or 0.020-0.06 part by weight, or 0.021-0.04 part by weight, or can be within the numerical range obtained by combining any two of the above end values.
[0054] According to one embodiment of the present application, the polymerization reaction is carried out under an inert atmosphere, for example, a nitrogen atmosphere or a rare gas atmosphere, for example, a nitrogen atmosphere.
[0055] According to another embodiment of the present application, the reactor is first vacuumed to remove oxygen, and then the monomer feed is allowed to begin polymerization in the reactor. For example, the reactor can be vacuumed before the polymerization reaction begins to remove as much oxygen as possible. Simultaneously with or after the vacuuming and deoxygenation, the monomers for copolymerization are added to the reactor. According to one embodiment of the present application, before the copolymerization reaction begins, the vacuuming and deoxygenation operation is performed to reduce the oxygen content in the gas phase in the reactor to less than 30 ppm, or less than 20 ppm, or less than 10 ppm, where the above ratios are based on the total gas volume in the gas phase in the reactor.
[0056] According to one embodiment of the present application, the polymerization reaction can be carried out at a temperature of 55-100°C, for example, the reaction temperature can be 58-90°C, or 60-80°C, or 60-70°C, or 60-65°C. According to another embodiment of the present application, the polymerization reaction can be carried out at a pressure of 0.6-2.8MPa, for example, the reaction pressure can be 0.8-2.7MPa, or 1-2.5MPa, or 1.2-2.4MPa, or 1.5-2.3MPa, or 1.8-2.2MPa, or 2.0-2.1MPa. According to one embodiment of the present application, the pressure is provided by the gaseous polymerization monomer raw materials participating in the polymerization reaction, for example, it can be provided by one or more of monomer A, monomer B and optional monomer C, and the pressure contributed by other gases (such as oxygen or air) is extremely small and can be ignored. According to one embodiment of the present application, the pressure in the reactor used for the copolymerization reaction is provided by the monomer A, or by monomer A and monomer C, or by monomer A and monomer B, or by monomer A, monomer B and monomer C.
[0057] According to some embodiments of the present application, the copolymer of the present application can be directly used as an adhesive, that is, the adhesive is composed of the copolymer without containing other components. According to another embodiment of the present application, in addition to containing the copolymer of the present application, the adhesive may also contain other additives as needed. For example, examples of additives that can be used in the adhesive of the present application may include one or more of the following: diluents, lubricants, heat stabilizers, UV stabilizers, antioxidants, processing aids, dispersants, compatibilizers, coupling agents, tackifiers, fillers, impact modifiers, flame retardants, antistatic agents, conductive agents, pigments, colorants, plasticizers, processing aid oils, antibacterial agents, etc.
[0058] The adhesive of the present application can exhibit good bonding strength to both fluoropolymer components and non-fluoropolymer components, and can therefore be used to bond components made of the two different materials together, thereby producing a device or apparatus with excellent bonding strength. According to an exemplary embodiment, the adhesive of the present application can be used to manufacture the backplane of a solar cell.
[0059] According to one embodiment of the present application, the backplane of the solar cell includes one or more layers of fluoropolymer film and one or more layers of substrate layer, the material of the substrate layer is different from the material of the fluoropolymer film, and the one or more layers of substrate layer are combined with the fluoropolymer film using the adhesive of the present invention. According to one embodiment of the present application, the fluoropolymer film of the backplane can contain various fluoropolymers as needed, such as polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), etc., and the polymer contained in the substrate layer can be a fluorine-free polymer, such as polyethylene terephthalate (PET), etc. According to one embodiment of the present application, the adhesive of the present invention can be arranged between the fluoropolymer film and the substrate layer in the form of any continuous pattern, discrete pattern or complete layer to combine the two together, preferably applied between the two in the form of a complete adhesive layer. The adhesive layer can be prepared by extruding, casting, pouring, etc. the adhesive of the present invention.
[0060] For example, Figure 1 shows a cross-sectional view of a backplane according to the present application. In the embodiment shown in Figure 1, the backplane includes two fluoropolymer films on both sides and a base layer in the middle, and the two fluoropolymer films are respectively bonded to the two sides of the base layer using the adhesive layer of the present invention.
[0061] The back sheet of the present application can be used in a solar cell module and provides excellent adhesive strength (peel strength) and weather resistance (oxidation resistance, UV degradation resistance, and discoloration resistance).
[0062] Figure 2 shows a schematic diagram of an exemplary solar cell, which includes the following components, in order from top to bottom: a frame, a transparent protective sheet, a first adhesive film, a cell, a second adhesive film, a backsheet, and a junction box. The design of these components, except for the backsheet, is known in the art. For example, the transparent protective sheet can be a glass sheet with high light transmittance. Two adhesive films are used to seal the transparent protective sheet and the backsheet to the cell. A common example of an adhesive film is a film made of ethylene vinyl acetate (EVA) resin. The cell is used to convert sunlight into electrical energy. The generated electrical energy is transmitted to an external energy storage and transmission device via a junction box. According to another embodiment of the present application, one or two of the adhesive films in the solar cell can also be formed using the adhesive of the present application; for example, the second adhesive film between the backsheet and the cell can also be prepared using the adhesive of the present application. The adhesive of the present application can simultaneously exhibit excellent bonding strength to fluoropolymer films (such as the fluoropolymer film located on the outside of the backsheet) and other non-fluorinated materials (such as the cell, more specifically the substrate or current collector of the cell), thereby achieving the desired bonding strength, service life, and weather resistance.
[0063] The present application is described below in the form of specific examples for the purpose of providing a better understanding of the present application. It should be understood that these examples are merely illustrative and non-restrictive. The reagents used in the examples are all commercially available unless otherwise specified. The methods and conditions used in the examples are conventional methods and conditions unless otherwise specified.
[0064] Example
[0065] In the following examples, the copolymers of the present invention were prepared and their performance was compared with conventional polymer binder materials from the prior art. The following examples are merely specific examples cited in this application, but the technical features of this application are not limited thereto. Any simple variations, equivalent substitutions, or other modifications based on this application that solve essentially the same technical problems and achieve essentially the same technical effects are encompassed within the scope of this application.
[0066] The paraffin wax used in the following examples was purchased from Jiangsu Yijiu Company, tetrafluoroethylene was produced by Shanghai Sanaifu New Materials Co., Ltd., vinyl acetate was purchased from Sichuan Wei Company, and other reagents (ammonium perfluorooctanoate, peroxysuccinic acid, and ammonium persulfate) were all analytically pure reagents and used directly without further purification. The water used was deionized water.
[0067] Example 1: Synthesis of tetrafluoroethylene-vinyl acetate copolymer
[0068] A 50L stainless steel reactor was used as a polymerization reactor, with the agitator speed set at 500 rpm. 30kg of deionized water, 12kg of vinyl acetate, and 1kg of paraffin were added to the reactor. The reactor was then sealed and 150g of a 20wt% aqueous solution of ammonium perfluorooctanoate was added. The reactor was evacuated using a vacuum pump. After the gas in the reactor was evacuated, tetrafluoroethylene was injected into the reactor to a pressure of 0.2MPa. The reactor was then evacuated again using a vacuum pump. This process was repeated three times. The oxygen content in the reactor was tested. A value of <20ppm was considered acceptable. If the value was unacceptable, the "evacuation-tetrafluoroethylene injection" cycle was repeated until the oxygen content in the reactor was acceptable. After the oxygen content in the reactor meets the required standards, the reactor is heated to 60°C. Gas-phase tetrafluoroethylene is introduced into the reactor through the gas inlet until the pressure reaches 2.0 MPa. At this point, an aqueous solution containing 5g of peroxysuccinic acid and 0.12g of ammonium persulfate is added to the reactor through the feed port to initiate the polymerization reaction. During the reaction, tetrafluoroethylene gas is introduced into the reactor to maintain the pressure at 2.0 MPa and the temperature at 60°C. Throughout the reaction, 60g of the ammonium perfluorooctanoate solution are continuously added to the reactor through the liquid feed port. When the tetrafluoroethylene feed reaches 12kg, the reaction is terminated, the gas-phase monomer is recovered, the temperature is lowered, and the paraffin wax is separated to obtain a copolymer emulsion. This emulsion is then coagulated in a coagulation drum at room temperature at 450 rpm. The product is washed with water and dried to obtain a copolymer powder. The molar ratio of tetrafluoroethylene to vinyl acetate in the copolymer product was measured to be 25:75 by nuclear magnetic resonance technology, and the Mn of the copolymer was measured to be 212,000 by gel permeation chromatography technology.
[0069] The powder was extruded in an extrusion test machine purchased from Potop Company. The extrusion temperature was controlled at 200° C. The extrudate was subjected to the steps of casting, cooling, slitting and winding to form a film with a thickness of 400 μm.
[0070] Example 2: Synthesis of tetrafluoroethylene-vinyl acetate-ethylene copolymer
[0071] A 50L stainless steel reactor was used as a polymerization reactor, with the agitator speed set at 500 rpm. 30kg of deionized water, 12kg of vinyl acetate, and 1kg of paraffin were added to the reactor. The reactor was then sealed and 150g of a 20wt% aqueous solution of ammonium perfluorooctanoate was added. The reactor was evacuated using a vacuum pump. After the gas in the reactor was evacuated, tetrafluoroethylene was injected into the reactor to a pressure of 0.2MPa. The reactor was then evacuated again using a vacuum pump. This process was repeated three times. The oxygen content in the reactor was tested. A value of <20ppm was considered acceptable. If the value was unacceptable, the "evacuation-tetrafluoroethylene injection" cycle was repeated until the oxygen content in the reactor was acceptable. Using a compression pump, gaseous tetrafluoroethylene and ethylene were mixed at a molar ratio of 10:1 to form a mixed feed gas. After the oxygen content in the reactor reached a satisfactory level, the reactor was heated to 60°C and the mixed feed gas was introduced through the gas inlet until the pressure reached 2.0 MPa. At this point, an aqueous solution containing 5g of peroxysuccinic acid and 0.12g of ammonium persulfate was added to the reactor through the feed port to initiate the polymerization reaction. During the reaction, the mixed feed gas was introduced into the reactor to maintain the pressure at 2.0 MPa and the temperature at 60°C. During the reaction, 60g of the ammonium perfluorooctanoate solution was continuously added to the reactor through the liquid feed port. When the mixed feed gas reached 12kg, the reaction was terminated, the gaseous monomers were recovered, the temperature was lowered, and the paraffin wax was separated to obtain a copolymer emulsion. This emulsion was coagulated in a coagulation drum at room temperature at 450 rpm. The product was washed with water and dried to obtain a copolymer powder.
[0072] The molar ratio of tetrafluoroethylene:vinyl acetate:ethylene in the copolymer product was measured to be 21:76.6:2.4 by nuclear magnetic resonance technology, and the Mn of the copolymer was measured to be 288,000 by gel permeation chromatography technology.
[0073] The powder was extruded in an extrusion test machine purchased from Potop Company. The extrusion temperature was controlled at 200° C. The extrudate was subjected to the steps of casting, cooling, slitting and winding to form a film with a thickness of 400 μm.
[0074] Comparative Example 1:
[0075] In this comparative example 1, a commercial product ethylene-vinyl acetate copolymer (vinyl acetate content 33 mol%) purchased from Yanshan Petrochemical Company was used. The copolymer resin was extruded in the extruder described in Example 1. The extrusion temperature was controlled at 90°C. The extrudate was subjected to the steps of casting, cooling, slitting, and winding to form a film with a thickness of 400 μm.
[0076] Example 3
[0077] In this Example 3, the properties of the materials (polymer films) prepared in Examples 1-2 and Comparative Example 1 were characterized using the following techniques.
[0078] (1) Adhesive strength was tested according to the national standard GB / T2790, "Adhesives - 180° Peel Strength Test Method - Flexible Materials to Rigid Materials." Specifically, a 1 mm thick PVDF film purchased from Shanghai Sanaifu New Materials Co., Ltd. was cut into 100 mm × 100 mm pieces. The polymer films prepared in Examples 1-2 and Comparative Example 1 were each cut into 100 mm × 100 mm pieces and superimposed on the PVDF film. The two films were then laminated in a laminator. The laminated structure was tested on a tensile testing machine at a speed of 100 mm / min, and the tensile strength values were recorded.
[0079] (2) Carry out UV aging resistance test according to GB / T19394-2003 test method.
[0080] Specifically, a 1 mm thick PVDF film purchased from Shanghai San Ai Fu New Materials Co., Ltd. was cut into a size of 100 mm × 100 mm, and the polymer films prepared in Examples 1-2 and Comparative Example 1 were cut into a size of 100 mm × 100 mm, respectively, and superimposed on the PVDF film. The laminated body of the two films was sent to a laminator for lamination. The laminated structure after lamination was sent to a UV irradiation box, and the temperature was 60°C, using light with a wavelength of 280 nm to 400 nm at a rate of 120 kWh / m 2 The irradiation was carried out for 720 hours at an irradiation intensity of 1000 nm.
[0081] The yellowness of the sample was tested before and after irradiation according to the national standard "Plastic Yellowness Index Test Method" GB2409, and the yellowing index was calculated based on the difference between the values before and after irradiation.
[0082] The test results are summarized in Table 1 below:
[0083] Table 1: Characterization results of adhesive films
[0084] The above performance test indicators show that the adhesive film of the present invention has the advantages of high peel strength and good UV aging resistance. In addition, both Examples 1-2 and Comparative Example 1 exhibit excellent adhesion strength (high peel strength) to PET (a non-fluoropolymer material commonly used as the substrate layer of solar cell backsheets). Due to the excellent bonding strength and better radiation aging resistance exhibited by the adhesives of Examples 1-2 of the present invention to both the non-fluoropolymer substrate layer and the PVDF film, they are significantly superior to adhesives in the prior art and are more suitable for use in the manufacture of solar cell module backsheets and packaging.
Claims
1. An adhesive comprising a copolymer comprising copolymerized structural units derived from the following monomers: Monomer A: a fluorinated monomer of formula I; In Formula I, R1, R2 and R3 are each independently selected from: hydrogen, fluorine, chlorine, C1-C12 alkyl, partially fluorinated or perfluorinated C1-C12 alkyl, C3-C12 cycloalkyl, partially fluorinated or perfluorinated C3-C12 cycloalkyl, C6-C12 aryl, partially fluorinated or perfluorinated C6-C12 aryl, C2-C12 alkenyl, partially fluorinated or perfluorinated C2-C12 alkenyl; Monomer B: Monomer represented by formula II: In Formula II, R4, R5 and R6 are each independently selected from the group consisting of hydrogen, C1-C12 alkyl, C1-C12 alkoxy, C3-C12 cycloalkyl, C3-C12 cycloalkoxy, C2-C12 alkenyl, C6-C12 aryl, C6-C12 aryloxy, C2-C12 alkenyl, C2-C12 alkenyloxy; R7 is selected from the group consisting of hydrogen, fluorine, C1-C18 alkyl; and Optional monomer C: a C1-C8 fluorine-free olefin monomer represented by formula III; In Formula III, R8, R9, R 10 and R 11 Each is independently selected from the group consisting of: hydrogen, C1-C12 alkyl, C1-C12 alkoxy, C3-C12 cycloalkyl, C3-C12 cycloalkoxy, C2-C12 alkenyl, C6-C12 aryl, C6-C12 aryloxy, and C2-C12 alkenyl.
2. The adhesive according to claim 1, characterized in that Based on the total molar amount of all comonomers in the copolymer, the content of the monomer A is 1-40 mol %, the content of the monomer B is 60-99 mol %, and the content of the monomer C is 0-5 mol %.
3. The adhesive according to claim 1, characterized in that The monomer A is selected from at least one of the following: tetrafluoroethylene, hexafluoropropylene, perfluoro-1-butene, perfluoro-2-butene, perfluoroisobutylene, perfluoro-1-n-pentene, perfluoro-2-n-pentene, perfluoroisopentene, perfluoro-1-hexene, perfluoro-2-methyl-2-pentene, and trifluoromonochloroethylene.
4. The adhesive according to claim 1, characterized in that The monomer B is selected from at least one of the following: vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl stearate.
5. The adhesive according to claim 1, characterized in that The monomer C is selected from at least one of the following: ethylene, propylene, n-butene, isobutylene, butadiene, 1-pentene, cyclobutene, 2-pentene, isopentene, isoprene, cyclopentadiene, and styrene.
6. The adhesive according to any one of claims 1 to 5, characterized in that The number average molecular weight Mn of the copolymer is 20,000-1,000,000.
7. A method for synthesizing the adhesive according to any one of claims 1 to 6, comprising carrying out a polymerization reaction of the monomer A, the monomer B and optionally the monomer C in a polymerization reactor.
8. The method according to claim 7, characterized in that During the polymerization reaction, the polymerization reactor also contains at least one of the following components: water, a dispersant, a stabilizer, and an initiator; and The polymerization reaction is carried out at a temperature of 55-100° C. and a pressure of 0.6-2.8 MPa.
9. A back sheet, comprising one or more layers of fluoropolymer film and one or more layers of substrate layer, wherein the material of the substrate layer is different from the material of the fluoropolymer film, and the one or more layers of substrate layer are bonded together with the fluoropolymer film using an adhesive, characterized in that: The adhesive is the adhesive according to any one of claims 1 to 6.
10. A solar cell comprising a transparent protective sheet, a cell sheet, a back sheet and a frame, wherein the back sheet is the back sheet according to claim 9.
Citation Information
Patent Citations
Novel high-cohesiveness vinylidene fluoride copolymer
CN104725545A
High-life solar panel
CN109244165A
Self-cleaning solar photovoltaic panel
CN110224040A
Vinylidene fluoride copolymer as well as preparation method and application thereof
CN112542588A
Adhesive suitable for solar cells and preparation and use thereof
CN116814193A