Lithium manganate positive electrode material and preparation method therefor
By introducing a fluorine element gradient distribution and an aluminum-fluoride compound protective layer into the lithium manganate cathode material, combined with boron and aluminum doping technology, the problem of manganese dissolution in the lithium manganate cathode material is solved, and the cycle life and stability are improved. Enhanced battery energy density.
Patent Information
- Application Number
- PCT/CN2024/084789
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium manganate cathode materials are prone to manganese dissolution during the cycle, resulting in a reduction in cycle life. Existing technology does not adequately study the penetration depth of fluorine elements and cannot effectively improve the manganese dissolution problem.
Using the technology of gradient distribution of fluorine element in the spherical lithium manganate cathode material, a protective layer is formed by aluminum-fluorine compounds to reduce the dissolution of manganese ions, and the structure and electronic conduction of the material are improved by controlling the sphericity and the doping of boron and aluminum. performance.
It significantly improves the cycle life and stability of the lithium manganate cathode material, reduces the dissolution of manganese ions, enhances the crystal structure and electronic conductivity of the material, and increases the energy density of the battery.
Smart Images

Figure CN2024084789_31102024_PF_FP_ABST
Abstract
Description
A lithium manganate positive electrode material and preparation method thereof Technical Field
[0001] The present invention belongs to the field of lithium-ion battery materials, and in particular relates to a spherical lithium manganate positive electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are highly efficient, environmentally friendly, and renewable energy devices. Due to their high energy density, light weight, and low self-discharge, they have become a primary energy source in traditional consumer electronics, electric vehicles, energy storage, and other fields. Lithium-ion cathode materials are a key component of lithium-ion batteries, and their performance directly determines their performance and lifespan.
[0003] Currently, the most commonly used lithium-ion battery cathode materials on the market are lithium cobalt oxide, ternary materials, and lithium iron phosphate cathode materials. The disadvantages of lithium cobalt oxide are that cobalt resources are scarce and expensive, and thermal runaway reactions can occur during use, posing a safety hazard. In addition, the structural stability of lithium cobalt oxide materials is insufficient and they are prone to decomposition at high temperatures. Ternary materials are mainly based on lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. Although their prices are lower than lithium cobalt oxide cathode materials, they have problems such as temperature sensitivity and capacity degradation. Lithium iron phosphate has a low capacity and is not suitable for large-capacity battery applications. Therefore, the search for a new cathode material with high capacity, long life, and low cost has become a research hotspot in recent years.
[0004] Lithium manganese oxide has the advantages of large capacity, high operating voltage, good safety performance, abundant resources and low price, and has become a new type of positive electrode material that has attracted much attention. However, lithium manganese oxide is prone to manganese dissolution during the cycle, which leads to a reduction in its cycle life and greatly limits the development of lithium manganese oxide positive electrode materials. In order to solve the technical problem of manganese dissolution in lithium manganese oxide, the main solution is to improve it through doping or coating. Using fluorine to modify lithium manganese oxide is an effective technical means. However, the current existing technology does not have sufficient research on the penetration depth of fluorine and is limited to surface coating of fluorine. Therefore, the improvement of manganese dissolution cannot always achieve the best effect.
[0005] Summary of the Invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a lithium manganate positive electrode material and a preparation method thereof.
[0007] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0008] A lithium manganate positive electrode material, whose chemical formula is Li a Al b Mn 2-b-c Bc O 4-d F d , wherein, 0.96≤a≤1.15, 0<b≤0.3, 0<c≤0.03, 0<d≤0.03; the secondary particles of the lithium manganate positive electrode material are spherical, the fluorine element permeates the spherical lithium manganate positive electrode material, and the fluorine element content is distributed in a decreasing gradient from the surface of the spherical lithium manganate positive electrode material particle to the center of the particle.
[0009] The fluorine element is distributed in a decreasing gradient from the surface of the spherical lithium manganese oxide positive electrode material particles to the center of the particles, which can enhance the crystal structure of the lithium manganese oxide positive electrode material to a certain extent, reduce the influence of the Jahn-Taylor effect, and thus reduce the manganese dissolution caused by structural distortion; at the same time, the infiltration of fluorine element can change the electronic energy band structure of the lithium manganese oxide positive electrode material, thereby improving its electronic conductivity and electrochemical reaction activity.
[0010] The above-mentioned lithium manganate positive electrode material preferably has a fluorine content in a spherical region 0.22R≤L≤R from the surface of the spherical lithium manganate positive electrode material particle, which accounts for 20% to 40% of the fluorine content in the entire lithium manganate positive electrode material; in a region L<0.22R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine content accounts for 60% to 80% of the fluorine content in the entire lithium manganate positive electrode material, wherein R is the equivalent radius of the secondary particle of the lithium manganate positive electrode material.
[0011] The above-mentioned lithium manganate positive electrode material, preferably, has a sphericity of 0.8 to 1. The dissolution of lithium manganate mainly occurs on the (111) crystal plane. This is because the structure of the (111) crystal plane of lithium manganate is more easily corroded by ions in the electrolyte than other crystal planes, resulting in the dissolution of manganese ions. Therefore, by reducing the proportion of the (111) crystal plane of lithium manganate, the dissolution of manganese ions can be reduced, thereby improving the cycle life and stability of lithium-ion batteries. Studies have shown that the (111) plane of spherical lithium manganate is smaller than the (111) plane of octahedron, and the dissolution amount of lithium manganate in the electrolyte is about 40% lower than that of the octahedral crystal. Therefore, controlling the sphericity of the lithium manganate positive electrode material to 0.8 to 1, making it close to spherical, can effectively reduce manganese dissolution.
[0012] The above-mentioned lithium manganate positive electrode material preferably has a manganese dissolution amount of 0.01% to 0.1%.
[0013] The above-mentioned lithium manganate positive electrode material preferably has a secondary particle D50 of 10 to 16 μm and a particle size distribution coefficient Span of 0.5 to 0.9.
[0014] As a general inventive concept, the present invention also provides a method for preparing the above-mentioned lithium manganate positive electrode material, comprising the following steps:
[0015] (1) weighing a lithium source, a manganese source, and a boron source according to the stoichiometric ratio of lithium, manganese, and boron in a chemical formula, mixing them, and then sintering them once to obtain a lithium manganate positive electrode material precursor;
[0016] (2) The lithium manganate positive electrode material precursor is mixed with an aluminum source and a fluorine source according to a stoichiometric ratio, and then subjected to secondary sintering. After the sintering is completed, the mixture is sieved to obtain a lithium manganate positive electrode material.
[0017] The above preparation method introduces a boron source in step (1). On the one hand, the boron element can be used to help the reaction to reduce the temperature required, reduce the volatilization of Li caused by high temperature, and reduce energy consumption. On the other hand, the boron element can modify the surface of polycrystalline lithium manganese oxide, so that the primary particles grow uniformly. At the same time, the boron element can also serve as a binder to tightly combine the polycrystalline primary particles together, thereby improving the mechanical strength of the material and maintaining the high sphericity of the precursor.
[0018] The above preparation method simultaneously introduces an aluminum source and a fluorine source in step (2). The aluminum element can form an aluminum-fluorine compound with the fluorine element. This compound has high ionic conductivity and low resistivity, and can promote the penetration and diffusion of the fluorine element in the lithium manganese oxide positive electrode material, thereby forming a gradient distribution of the fluorine element inside the material. The high-gradient fluorine on the surface combines with the aluminum to form a physical coating layer of aluminum-fluorine compound, which can effectively reduce the corrosion of the electrolyte to the inside of the material, stabilize the crystal structure of the lithium manganese oxide positive electrode material, reduce manganese dissolution, and improve the cycle life and energy density of the battery.
[0019] The above preparation method, through the synergistic effect of uniform bulk doping of boron and aluminum, enables the lithium manganese oxide positive electrode material to still inherit the high sphericity of the precursor during the sintering process.
[0020] In the above preparation method, preferably, in step (1), the primary sintering temperature is 700-850° C., and the sintering time is 4-10 h.
[0021] In the above preparation method, preferably, in step (2), the temperature of the secondary sintering is 300-600° C., and the sintering time is 2-8 hours.
[0022] In the above-mentioned preparation method, preferably, in step (1), the manganese source includes at least one of aluminum-doped manganese carbonate, aluminum-doped manganese tetraoxide, aluminum-doped manganese trioxide, aluminum-doped manganese oxyhydroxy and aluminum-doped manganese dioxide; selecting the aluminum-doped manganese source can obtain a precursor with uniform aluminum bulk doping, thereby stabilizing the crystal structure of lithium manganate and inhibiting the generation of oxygen defects in lithium manganate during the synthesis process, so that the material undergoes a single-phase reaction in the entire high and low voltage regions during the charging process, thereby improving the cycle performance.
[0023] In the above preparation method, preferably, in step (1), the lithium source includes at least one of lithium carbonate and lithium hydroxide; and the boron source includes at least one of H3BO3 and B2O3.
[0024] In the above preparation method, preferably, in step (2), the fluorine source includes at least one of lithium fluoride, ammonium fluoride, aluminum fluoride, polyvinylidene fluoride homopolymer, polyvinylidene fluoride copolymer, polyvinylidene fluoride-hexafluoropropylene polymer and polytetrafluoroethylene; the aluminum source includes at least one of aluminum hydroxide, aluminum oxide and aluminum nitrate.
[0025] Compared with the prior art, the advantages of the present invention are:
[0026] (1) The present invention adjusts the gradient distribution of fluorine in the lithium manganese oxide positive electrode material, which not only improves the stability of the internal crystal structure of the lithium manganese oxide positive electrode material and ensures that the internal structure of the material will not collapse during the charge and discharge process, but also forms a layer of aluminum fluoride compound protective layer on the surface of the positive electrode material in the area where the distance L is less than 0.22R from the surface, which can prevent the electrolyte from corroding the interior of the material, thereby reducing the dissolution amount of divalent manganese in the electrolyte and improving the energy density of the battery.
[0027] (2) The present invention controls the sphericity of the lithium manganate positive electrode material to 0.8-1, thereby reducing the proportion of the lithium manganate (111) crystal plane and reducing the dissolution of divalent manganese ions, thereby improving the cycle life and stability of the lithium ion battery.
[0028] (3) In the preparation method of the present invention, an aluminum source and a fluorine source are added simultaneously. The aluminum element can form an aluminum-fluorine compound with the fluorine element having higher ionic conductivity and lower resistivity, thereby promoting the gradient distribution of the fluorine element in the lithium manganese oxide positive electrode material.
[0029] (4) In the preparation method of the present invention, a secondary low-temperature sintering process is adopted, which can achieve a spherical lithium manganate positive electrode material with a fluorine element distributed in a decreasing gradient from the surface of the material particle to the center of the particle by adding a small amount of fluorine element. The process cost is low and it is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] FIG1 is a diagram showing the distribution of fluorine elements in an electron probe cross section of a lithium manganate positive electrode material prepared in Example 1 of the present invention.
[0031] FIG2 is a SEM image of the lithium manganate positive electrode material prepared in Example 3 of the present invention.
[0032] FIG3 is a computer-automatically identified sphericity equivalent diagram of the lithium manganate positive electrode material prepared in Example 3 of the present invention.
[0033] FIG4 is a charge and discharge curve diagram of the lithium manganate positive electrode material prepared in Example 3 of the present invention.
[0034] FIG5 is a graph showing the 7C / 0.2C rate performance of the lithium manganate positive electrode materials prepared in the examples of the present invention and the comparative examples.
[0035] FIG6 is a graph showing the capacity cycle retention rate of the lithium manganate positive electrode materials prepared in the examples of the present invention and the comparative examples. DETAILED DESCRIPTION
[0036] To facilitate understanding of the present invention, the present invention will be described in more comprehensive and detailed form below in conjunction with the accompanying drawings and preferred embodiments. However, the scope of protection of the present invention is not limited to the following specific embodiments.
[0037] Unless otherwise defined, all technical terms used hereinafter have the same meanings as those generally understood by those skilled in the art. The technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0039] Example 1:
[0040] The lithium manganate positive electrode material of this embodiment has the chemical formula Li 1.05 Al 0.2 Mn 1.78 B 0.02 O 3.982 F 0.018 The secondary particles of the lithium manganate positive electrode material are spherical, with a sphericity of 0.894, a secondary particle D50 of 14.5 μm, and a particle size distribution coefficient Span value of 0.8; the fluorine element permeates the spherical lithium manganate positive electrode material, and the fluorine element is distributed in a decreasing gradient from the surface of the spherical lithium manganate positive electrode material particle to the center of the particle. In a spherical region with a distance of 0.22R≤L≤R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine element content accounts for 23% of the fluorine content in the entire lithium manganate positive electrode material; in a region with a distance of L<0.22R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine element content accounts for 77% of the fluorine content in the entire lithium manganate positive electrode material, where R is the equivalent radius of the secondary particle of the lithium manganate positive electrode material.
[0041] The method for preparing the lithium manganate positive electrode material of this embodiment includes the following steps:
[0042] (1) (Mn 0.95 Al 0.05)3O4, lithium carbonate, and boric acid are weighed according to a stoichiometric ratio of 1.78:1.05:0.02, and then placed in a high-speed mixer for mixing. After the mixture is evenly mixed, it is placed in a roller kiln and heated to 760°C at a heating rate of 3°C / min in an air atmosphere and sintered for 4 hours. After sintering, it is cooled and then crushed by a jet mill. The crushed material is passed through a 300-mesh manual sieve to obtain an aluminum- and boron-doped spherical lithium manganese oxide polycrystalline positive electrode material;
[0043] (2) The spherical lithium manganate polycrystalline positive electrode material obtained in step (1) is weighed with aluminum hydroxide and polyvinylidene fluoride in a stoichiometric ratio of 1:0.05:0.018, and the mixture is placed in a high-speed mixer and mixed evenly. The mixture is placed in a roller kiln and heated to 300°C at a heating rate of 2°C / min in an air atmosphere, sintered for 5 hours, cooled after sintering, and passed through a 300-mesh manual sieve to obtain a lithium manganate positive electrode material.
[0044] The distribution of fluorine in the lithium manganate positive electrode material prepared in this embodiment was characterized by electron probe cross-sectional analysis. The results are shown in Figure 1. In the area where L is less than 0.22R from the surface of the spherical lithium manganate positive electrode material particles, the fluorine content accounts for 77% of the fluorine content in the entire lithium manganate positive electrode material. In the spherical area where 0.22R≤L≤R is away from the surface of the spherical lithium manganate positive electrode material particles, the fluorine content accounts for 23% of the fluorine content in the entire lithium manganate positive electrode material.
[0045] By training the computer to automatically identify particles and measure the particle size of the lithium manganese oxide positive electrode material in the tungsten filament electron microscope photo, and calculate its sphericity, the calculation result is: the sphericity is 0.894.
[0046] Electrical performance test: The lithium manganese oxide positive electrode material sample prepared in this embodiment was made into a button battery, and the positive electrode sheet was prepared with an active material: conductive agent: binder = 92%: 5%: 3%. The metal lithium sheet was used as the negative electrode to prepare a 2032-type button battery. The Wuhan Blue Electric electrochemical test cabinet was used for testing. The test operating voltage was 3.0-4.3V, and the charge and discharge test was performed at 1C / 1C. The capacity retention rate was 98.0% after 50 cycles at 60°C. The rate performance test was performed at room temperature using currents of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, and 7C, and the 7C / 0.2C rate retention rate was 89.9%.
[0047] Mn dissolution test: The lithium manganese oxide positive electrode material prepared in this example was prepared according to the same preparation method as described above, and then placed in a 60°C constant temperature chamber. After constant voltage charging for 30 hours at 50% and 100% charge states, the battery was disassembled, and the residual electrolyte on the surface of the negative electrode was cleaned with dimethyl carbonate and then dissolved in hydrochloric acid solution. The Mn content was then tested by ICP. The Mn dissolution amounts in the lithium manganese oxide positive electrode material at 50% and 100% charge states were 0.069 wt% and 0.085 wt%, respectively.
[0048] Example 2:
[0049] The lithium manganate positive electrode material of this embodiment has the chemical formula Li 1.05 Al 0.2 Mn 1.78 B 0.02 O 3.99 F 0.01 The secondary particles of the lithium manganate positive electrode material are spherical, with a sphericity of 0.869, a secondary particle D50 of 15.2 μm, and a particle size distribution coefficient Span value of 0.88; the fluorine element permeates the spherical lithium manganate positive electrode material, and the fluorine element is distributed in a decreasing gradient from the surface of the spherical lithium manganate positive electrode material particle to the center of the particle. In a spherical region with a distance of 0.22R≤L≤R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine element content accounts for 31% of the fluorine content in the entire lithium manganate positive electrode material; in a region with a distance of L<0.22R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine element content accounts for 69% of the fluorine content in the entire lithium manganate positive electrode material, wherein R is the equivalent radius of the secondary particle of the lithium manganate positive electrode material.
[0050] The preparation method of the lithium manganate positive electrode material of this embodiment includes the following steps:
[0051] (1) (Mn 0.95 Al 0.05 )3O4, lithium carbonate, and boric acid were weighed according to a stoichiometric ratio of 1.78:1.05:0.02, and then placed in a high-speed mixer for mixing. After mixing evenly, the mixture was placed in a roller kiln and heated to 760°C at a heating rate of 3°C / min in an air atmosphere and sintered for 4 hours. After sintering, the mixture was cooled and then crushed by a jet mill. The crushed material was passed through a 300-mesh manual sieve to obtain an aluminum- and boron-doped spherical lithium manganese oxide polycrystalline positive electrode material;
[0052] (2) The spherical lithium manganate polycrystalline positive electrode material obtained in step (1) is weighed with aluminum hydroxide and polyvinylidene fluoride in a stoichiometric ratio of 1:0.05:0.01, placed in a high-speed mixer and mixed evenly, and the mixture is placed in a roller kiln, and heated to 450°C at a heating rate of 2°C / min in an air atmosphere, sintered for 5 hours, cooled after sintering, and the cooled material is sieved through a 300-mesh manual sieve to obtain a lithium manganate positive electrode material.
[0053] The distribution of fluorine in the lithium manganate positive electrode material was characterized by electron probe cross-section analysis. The fluorine was distributed in a decreasing gradient from the surface of the spherical lithium manganate positive electrode material particles to the center of the particles. In the spherical region with a distance of 0.22R≤L≤R from the surface of the spherical lithium manganate positive electrode material particles, the fluorine content accounted for 31% of the fluorine content in the entire lithium manganate positive electrode material; in the region with a distance of L<0.22R from the surface of the spherical lithium manganate positive electrode material particles, the fluorine content accounted for 69% of the fluorine content in the entire lithium manganate positive electrode material.
[0054] By training the computer to automatically identify particles and measure the size of lithium manganese oxide positive electrode material particles in tungsten filament electron microscope photos, and calculate their sphericity, the calculation result is: sphericity is 0.869.
[0055] The performance of the lithium manganese oxide positive electrode material prepared in this embodiment was tested according to the electrical performance test and Mn dissolution test methods in Example 1. The results showed that the button battery prepared using the lithium manganese oxide positive electrode material in this embodiment had a capacity retention rate of 98.2% after 50 cycles at 1C and 60°C; at room temperature, the 7C / 0.2C rate retention rate was 91.3%; and the Mn dissolution amounts in the lithium manganese oxide positive electrode material at 50% charge state and 100% charge state were 0.055wt% and 0.071wt%, respectively.
[0056] Example 3:
[0057] The lithium manganate positive electrode material of this embodiment has the chemical formula Li 1.05 Al 0.2 Mn 1.78 B 0.02 O 3.97 F 0.03The secondary particles of the lithium manganate positive electrode material are spherical, with a sphericity of 0.906, a secondary particle D50 of 14.5 μm, and a particle size distribution coefficient Span value of 0.84; the fluorine element permeates the spherical lithium manganate positive electrode material, and the fluorine element is distributed in a decreasing gradient from the surface of the spherical lithium manganate positive electrode material particle to the center of the particle. In a spherical region with a distance of 0.22R≤L≤R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine element content accounts for 38% of the fluorine content in the entire lithium manganate positive electrode material; in a region with a distance of L≤0.22R from the surface of the spherical lithium manganate positive electrode material particle, the fluorine element content accounts for 62% of the fluorine content in the entire lithium manganate positive electrode material, where R is the equivalent radius of the secondary particle of the lithium manganate positive electrode material.
[0058] The preparation method of the lithium manganate positive electrode material of this embodiment includes the following steps:
[0059] (1) (Mn 0.95 Al 0.05 )3O4, lithium carbonate, and boric acid are weighed according to a stoichiometric ratio of 1.78:1.05:0.02, and then placed in a high-speed mixer for mixing. After the mixture is evenly mixed, it is placed in a roller kiln and heated to 760°C at a heating rate of 3°C / min in an air atmosphere and sintered for 4 hours. After sintering, it is cooled and then crushed by a jet mill. The crushed material is passed through a 300-mesh manual sieve to obtain an aluminum- and boron-doped spherical lithium manganese oxide polycrystalline positive electrode material;
[0060] (2) The spherical lithium manganate polycrystalline positive electrode material obtained in step (1) is weighed with aluminum hydroxide and polyvinylidene fluoride in a stoichiometric ratio of 1:0.05:0.03, and the mixture is placed in a high-speed mixer and mixed evenly. The mixture is placed in a roller kiln and heated to 600°C at a heating rate of 2°C / min in an air atmosphere, sintered for 5 hours, and cooled after sintering. The cooled material is sieved through a 300-mesh manual sieve to obtain a lithium manganate positive electrode material, whose SEM image is shown in Figure 2. It can be seen from Figure 2 that the secondary particles of the prepared lithium manganate positive electrode material are spherical.
[0061] The distribution of fluorine in the lithium manganate positive electrode material was characterized by electron probe cross-section analysis. The fluorine was distributed in a gradient from the surface of the spherical lithium manganate positive electrode material particles to the center of the particles. In the spherical region with a distance of 0.22R≤L≤R from the surface of the spherical lithium manganate positive electrode material particles, the fluorine content accounted for 38% of the fluorine content in the entire lithium manganate positive electrode material; in the region with a distance of L<0.22R from the spherical lithium manganate positive electrode material particles, the fluorine content accounted for 62% of the fluorine content in the entire lithium manganate positive electrode material.
[0062] By training the computer to automatically identify particles and measure the particle size of the lithium manganese oxide positive electrode material in the tungsten filament electron microscope photograph, the equivalent diagram of the computer automatically identified particles is shown in Figure 3, and its sphericity is calculated, and the calculated result is a sphericity of 0.906.
[0063] The performance of the lithium manganese oxide positive electrode material prepared in this embodiment was tested according to the electrical performance test and Mn dissolution test method of Example 1. The results showed that the button battery prepared using the lithium manganese oxide positive electrode material in this embodiment had a capacity retention rate of 98.7% after 50 cycles at 1C and 60°C; at room temperature, the 7C / 0.2C rate retention rate was 94.2%. Its charge and discharge curve is shown in Figure 4. At a current density of 0.1C, the first charge capacity was 114.9mAh / g, the first discharge capacity was 112.6mAh / g, and the first charge and discharge efficiency was 98.4%; the Mn dissolution amounts in the lithium manganese oxide positive electrode material at 50% charge state and 100% charge state were 0.035wt% and 0.043wt%, respectively.
[0064] Comparative Example 1:
[0065] The preparation method of the lithium manganate positive electrode material in this comparative example is basically the same as that in Example 1, except that aluminum hydroxide is not added in step (2). Other process parameters are the same as those in Example 1. The chemical formula of the prepared lithium manganate positive electrode material is Li 1.05 Al 0.15 Mn 1.83 B 0.02 O 3.982 F 0.018 The distribution of fluorine element in the lithium manganate positive electrode material prepared in this comparative example was characterized by electron probe cross-section analysis. In the area L<0.22R from the surface of the spherical lithium manganate positive electrode material particles, the fluorine element content accounted for 100% of the fluorine content in the entire spherical area, where R is the equivalent radius of the lithium manganate positive electrode material secondary particle.
[0066] The performance of the lithium manganese oxide positive electrode material prepared in this comparative example was tested according to the electrical performance test and Mn dissolution test methods in Example 1. The results showed that the button battery prepared using the lithium manganese oxide positive electrode material in this comparative example had a capacity retention rate of 97.9% after 50 cycles at 1C and 60°C; at room temperature, the 7C / 0.2C rate retention rate was 87.0%, and the Mn dissolution amounts in the lithium manganese oxide positive electrode material at 50% charge state and 100% charge state were 0.086wt% and 0.109wt%, respectively.
[0067] Comparative Example 2:
[0068] The lithium manganate positive electrode material of this comparative example has the chemical formula Li 1.05 Al 0.2 Mn 1.78 B 0.02 O 3.97 F 0.03The secondary particles of the lithium manganese oxide positive electrode material are spherical with a sphericity of 0.874, a secondary particle D50 of 14.9 μm, a particle size distribution coefficient Span value of 0.81, and fluorine element is evenly distributed inside the lithium manganese oxide positive electrode material.
[0069] The steps of the preparation method of the lithium manganate positive electrode material of this comparative example are as follows:
[0070] (Mn 0.95 Al 0.05 )3O4, lithium carbonate, boric acid, and polyvinylidene fluoride are weighed according to the stoichiometric ratio of 1.78:1.05:0.02:0.03, and then placed in a high-speed mixer for mixing. After mixing evenly, the mixture is placed in a roller kiln and heated to 760°C at a heating rate of 3°C / min in an air atmosphere. The mixture is sintered for 4 hours, cooled after sintering, and crushed by a jet mill. The crushed material is sieved through a 300-mesh manual sieve to obtain a spherical lithium manganese oxide polycrystalline positive electrode material uniformly doped with aluminum, boron, and fluorine.
[0071] The distribution of fluorine in lithium manganese oxide was characterized by electron probe cross-section analysis, and it was found that fluorine was evenly distributed in lithium manganese oxide.
[0072] The performance of the lithium manganese oxide positive electrode material prepared in this comparative example was tested according to the electrical performance test and Mn dissolution test methods in Example 1. The results showed that the button battery prepared using the lithium manganese oxide positive electrode material in this comparative example had a capacity retention rate of 97.4% after 50 cycles at 1C and 60°C; at room temperature, the 7C / 0.2C rate retention rate was 87.4%, and the Mn dissolution amounts in the lithium manganese oxide positive electrode material at 50% charge state and 100% charge state were 0.282wt% and 0.396wt%, respectively.
[0073] The fluorine distribution, Mn dissolution amount and electrochemical performance of the lithium manganate positive electrode materials prepared in the above examples and comparative examples are shown in Table 1 and Figures 5 and 6.
[0074] Table 1: Fluorine distribution, Mn dissolution and electrochemical performance of lithium manganate cathode materials in Examples and Comparative Examples
[0075] From the comparison of Example 1 and Comparative Example 1, it can be seen that during the secondary sintering process, the addition of Al element can promote the penetration of fluorine element into the interior of lithium manganate, forming a gradient distribution of fluorine element; from the comparison of Example 3 and Comparative Example 2, it can be seen that the lithium manganate positive electrode material with a gradient distribution of fluorine element has better manganese dissolution, cycle performance and rate performance than the lithium manganate positive electrode material uniformly doped with fluorine element. This is because the gradient distribution of fluorine element can form a more stable structural layer in different gradient regions inside the material, stabilize the internal structure of the material, and reduce the Jiang-Taylor effect. From the comparison of the above embodiments and comparative examples, it can also be seen that the gradient distribution of fluorine element is not only related to the promoting effect of Al, but the increase in temperature is also conducive to the realization of gradient doping of fluorine. This is mainly because the increase in temperature can accelerate the diffusion rate of fluorine element, making it easier to pass through the lattice structure of lithium manganate, thereby increasing the penetration rate of fluorine element into the interior of lithium manganate; in addition, increasing the temperature can also reduce the lattice energy of lithium manganate, making it easier to be replaced by fluorine element, thereby promoting the gradient doping of fluorine element.
Claims
1. A lithium manganese oxide positive electrode material, It is characterized in that The chemical formula of the lithium manganese oxide positive electrode material is Li a Al b Mn 2-b-c B c O 4-d F d , wherein 0.96≤a≤1.15, 0<b≤0.3, 0<c≤0.03, 0<d≤0.03; the secondary particles of the lithium manganese oxide positive electrode material are spherical, the fluorine element permeates the spherical lithium manganese oxide positive electrode material, and the fluorine element content is distributed in a decreasing gradient from the surface of the spherical lithium manganese oxide positive electrode material particles to the center of the particles.
2. The lithium manganate positive electrode material according to claim 1, It is characterized in that In the spherical region where 0.22R≤L≤R is away from the surface of the spherical lithium manganate positive electrode material particle, the fluorine content accounts for 20% to 40% of the fluorine content in the entire lithium manganate positive electrode material; in the region where L<0.22R is away from the surface of the spherical lithium manganate positive electrode material particle, the fluorine content accounts for 60% to 80% of the fluorine content in the entire lithium manganate positive electrode material, wherein R is the equivalent radius of the secondary particle of the lithium manganate positive electrode material.
3. The lithium manganate positive electrode material according to claim 1, It is characterized in that The sphericity of the lithium manganate positive electrode material is 0.8-1.
4. The lithium manganate positive electrode material according to claim 1, It is characterized in that The unit manganese dissolution amount in the lithium manganate positive electrode material is 0.01% to 0.1%.
5. The lithium manganate positive electrode material according to claim 1, It is characterized in that The secondary particles D50 of the lithium manganate positive electrode material are 10-16 μm, and the particle size distribution coefficient Span is 0.5-0.
9.
6. A method for preparing the lithium manganate positive electrode material according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) mixing a lithium source, a manganese source, and a boron source and sintering them once to obtain a lithium manganate positive electrode material precursor; (2) After mixing the lithium manganate positive electrode material precursor with an aluminum source and a fluorine source, performing secondary sintering, and sieving after sintering to obtain a lithium manganate positive electrode material.
7. The preparation method according to claim 6, It is characterized in that In step (1), the primary sintering temperature is 700-850° C., and the sintering time is 4-10 hours.
8. The preparation method according to claim 6, It is characterized in that In step (2), the secondary sintering temperature is 300-600° C., and the sintering time is 2-8 hours.
9. The preparation method according to claim 6, It is characterized in that In step (1), the manganese source includes at least one of aluminum-doped manganese carbonate, aluminum-doped manganese tetraoxide, aluminum-doped manganese trioxide, aluminum-doped manganese oxyhydroxide and aluminum-doped manganese dioxide; The lithium source includes at least one of lithium carbonate and lithium hydroxide; The boron source includes H 3 BO 3 , B 2 O 3 At least one of .
10. The preparation method according to claim 6, It is characterized in that In step (2), the fluorine source includes at least one of lithium fluoride, ammonium fluoride, aluminum fluoride, polyvinylidene fluoride homopolymer, polyvinylidene fluoride copolymer, polyvinylidene fluoride-hexafluoropropylene polymer and polytetrafluoroethylene; The aluminum source includes at least one of aluminum hydroxide, aluminum oxide and aluminum nitrate.
Citation Information
Patent Citations
Lithium-manganese-aluminum oxygen anode material and preparation method thereof
CN102683667A
High-property lithium manganate gradient anode material and preparation method thereof
CN103700841A
Lithium manganate material and preparation method thereof and lithium ion battery cathode material
CN104425814A
Lithium manganate positive electrode material and preparation method thereof
CN109768268A
Lithium manganate positive electrode material and preparation method thereof