Pigment preparation with metal effect pigment
The pigment preparation with metal effect pigments, water-soluble binders, and surface-active additives addresses safety and stability issues, offering high hiding power and durability without phosphorus compounds, ensuring safe and effective use in aqueous systems.
Patent Information
- Application Number
- PCT/EP2024/060505
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-31
AI Technical Summary
Metallic effect pigments pose safety risks due to dust explosion hazards, require environmentally harmful additives, and have adhesion issues in aqueous systems, limiting their use and storage stability.
A pigment preparation comprising 60-98% metal effect pigments with metal oxide layers, 1-30% water-soluble binder, and 1-30% surface-active additive, with less than 3% residual moisture and phosphorus content, allowing for dust-free handling and improved storage stability without organic phosphates or solvents.
The solution provides high hiding power, improved dimensional stability, and enhanced interlayer adhesion, preventing pigment detachment and ensuring durability and longevity of coated surfaces, while eliminating dust formation and environmental hazards.
Smart Images

Figure IMGF000016_0001 
Figure IMGF000019_0001 
Figure IMGF000021_0001
Abstract
Description
[0001] Pigment preparation with metallic effect pigment
[0002] The invention relates to a pigment preparation comprising metallic effect pigments, a process for producing the pigment preparation and its use.
[0003] Metallic effect pigments are frequently used in coatings, paints, printing inks, cosmetics, or plastics to add color and create a metallic effect. However, metallic effect pigments, such as aluminum effect pigments, can pose safety risks and handling problems. For example, dry metallic effect pigments can generate dust that is potentially explosive and toxic if inhaled, as well as causing handling problems. Furthermore, the use of metallic effect pigments in water-borne coatings requires stabilization of the pigments to prevent loss of optical properties. Metallic effect pigments can be stabilized with metal oxide layers, such as silicon dioxide layers; however, dry pigment compositions containing metallic effect pigments are undesirable due to the risk of dust explosions.
[0004] To offer such metallic effect pigment preparations in a dust-free manner, they are made into a paste with organic solvents. However, this results in increased volatile organic solvent (VOC) exposure and introduces larger quantities of undesirable solvents into aqueous coating formulations. Alternatively, the pigment preparations can be made into a paste with water, but this addition also limits formulation freedom, and there remains a risk of metals such as aluminum reacting with water, which is why these products cannot be shipped by air freight. Furthermore, pastes often exhibit problems with aggregation during storage, which negatively impacts the optical properties.
[0005] To overcome these problems, metallic effect pigments are often stabilized with organophosphorus compounds, such as organophosphates. However, this has the disadvantage that phosphorus stabilization leads to impaired adhesion and flexibility in the application, and cracking and flaking can occur. In particular, organic phosphorus compounds often impair overprintability. Furthermore, many organophosphorus compounds are hazardous to water, which raises concerns and restricts their use for environmental and health protection reasons.
[0006] US 10,385,230 B2 describes a metallic effect pigment preparation comprising an effect pigment, a dispersing additive, and a passivating agent. The preparation is in dry form, with the pigment accounting for about 84% or more of the mass of the preparation, the dispersing additive accounting for up to 15% of the mass, and the number of theoretical layers of the passivating agent being between about 2 and about 12. This preparation is non-dusting and can be easily stirred into liquid coating formulations based on water, solvent, or UV-curing. However, a phosphorus compound is required, which can lead to, for example, adhesion problems and shifting between layers.
[0007] US 2007 / 0199478 A1 describes aluminum pigments that are at least partially coated with fatty acids. The pigments have a water coverage of between 40,000 and 130,000 cm³. 2 / g. The production and use of these pigments are also described. Phosphorus compounds are also required.
[0008] The present invention is based on the object of providing a pigment preparation with metallic effect pigments that can be used in aqueous systems, does not require environmentally harmful additives such as organophosphorus compounds or organic solvents, is in a compacted formulation, and can be dosed dust-free. This improves handling, storage stability, and occupational safety. This object is achieved by a pigment preparation with metallic effect pigments according to claim 1, a process for the preparation according to claim 13, and the uses according to claim 15. Further features, embodiments, and advantages emerge from the subclaims, the description, and the figures.
[0009] One aspect of the invention relates to a pigment preparation with metallic effect pigments, wherein the pigment preparation comprises the following components: a) 60 - 98 wt.%, based on the total weight of the pigment preparation, of at least one metallic effect pigment having one or more metal oxide and / or metal hydroxide and / or metal oxide hydrate layers on a metallic core, b) 1 - 30 wt.%, based on the total weight of the pigment preparation, of at least one water-soluble binder, c) 1 - 30 wt.%, based on the total weight of the pigment preparation, of a surface-active additive, and d) less than 3 wt.%, based on the total weight of the pigment preparation, of residual moisture, wherein the residual moisture comprises water and organic solvents, wherein the pigment preparation has less than 500 ppm phosphorus.
[0010] Components a) to d) amount to 100 wt.%.
[0011] A further aspect of the invention relates to a process for producing the pigment preparation according to the invention, which comprises the following steps: a) mixing a metallic effect pigment having one or more metal oxide and / or metal hydroxide and / or metal oxide hydrate layers on a metallic core with at least one water-soluble binder and a surface-active additive, b) compacting the mixture obtained in step a), c) optionally drying the compacted mixture. A further aspect of the invention relates to the use of the pigment preparation according to the invention in paints, varnishes, powder coatings, masterbatches, printing inks, plastics, cosmetic preparations, in security printing or security printing.
[0012] Surprisingly, despite the absence of organic phosphates and phosphonates (which results in a phosphorus content of less than 500 ppm, in particular less than 20 ppm), the pigment preparation according to the invention exhibits high hiding power in application media, with improved dimensional stability and significantly improved storage stability. Furthermore, pigment aggregation can be avoided, and the optical properties of the metallic pigments are not adversely affected. The pigment preparation according to the invention is easily dispersible in aqueous application systems and exhibits high interlayer adhesion during application, thus preventing detachment of the pigments from the substrate medium. This results in improved durability and longevity of the coated surface. Due to the binder and the water-soluble additive it contains, the pigment preparation according to the invention exhibits no significant dust formation despite low residual moisture.
[0013] The terms "metallic effect pigment" and "metallic pigment" are used synonymously within the scope of the present invention. A metallic effect pigment is understood to be a pigment having a metallic core, which is preferably platelet-shaped and has at least one metal oxide and / or metal hydroxide and / or metal oxide hydrate layer. The average diameter of the metallic core is typically 1-250 pm, preferably 2-150 pm, in particular 5-100 pm. The thickness of the platelets is usually in the range of about 4 nm - 2 pm, preferably 15 - 200 nm, in particular 30 to 140 nm or 60 to 120 nm. The ratio of diameter to thickness is generally 1500:1 - 20:1, preferably 1000:1 - 100:1, in particular 500:1 - 200:1. This ratio of diameter to thickness is referred to as the form factor. The metallic effect pigments can be obtained by grinding (so-called cornflake or silver dollar, orVery thin, ground metallic effect pigments) or by VMP / PVD processes. A pigment preparation is understood to be a pigment composition. A water-soluble binder is understood here to mean that at least 10 g of the binder dissolves in 1 L of demineralized water at 20 °C and 1 bar pressure.
[0014] A surface-active additive is a substance that has the ability to reduce the surface tension of water. A non-ionic surface-active additive is a substance that does not contain any ionic functional groups, while an ionic additive contains one or more ionic functional groups. A surface-active additive can also be referred to as a surfactant.
[0015] The pigment preparation according to the invention comprises 60-98 wt.% of at least one metallic effect pigment, based on the total weight of the pigment preparation. In a preferred embodiment, the pigment preparation according to the invention contains 70-95 wt.%, more preferably 75-93 wt.%, in particular 80 to 91 wt.% of at least one metallic effect pigment, based on the total weight of the pigment preparation.
[0016] The pigment preparation according to the invention further comprises 1-30% by weight, based on the total weight of the pigment preparation, of at least one water-soluble binder, preferably 3-25% by weight, more preferably 4-15% by weight, in particular 5-10% by weight of at least one water-soluble binder.
[0017] As a further component, the pigment preparation of the present invention comprises 1-30 wt.% of a surface-active additive, based on the total weight of the pigment preparation, preferably 1.5-20 wt.%, in particular 2-15 wt.%, in particular 2.5-10 wt.%.
[0018] The pigment preparation according to the invention contains less than 500 ppm of phosphorus, based on the total weight of the pigment preparation. In the prior art, pigment preparations often contain larger amounts of phosphorus due to the use of organic phosphates, phosphonates, or phosphites, which are not used in the present invention. This has the advantage that environmentally hazardous phosphorus compounds, such as in particular organic phosphates and phosphonates, can be dispensed with and, moreover, improved adhesion is achieved in the application. In a preferred embodiment, the pigment preparation according to the invention comprises less than 300 ppm, in particular less than 200 ppm or less than 100 ppm or less than 20 ppm of phosphorus. The phosphorus is measured by optical emission spectrometry (OES).According to one embodiment, the pigment preparation according to the invention further comprises less than 300 ppm, in particular less than 200 ppm or less than 100 ppm or less than 30 ppm of sulfur (unless an ionic surface-active additive based on organic sulfates or sulfonates is used).
[0019] A further advantage of the pigment preparation according to the invention is the low residual moisture content and thus its presence in compacted form. According to the invention, the pigment preparation contains less than 3% by weight, based on the total weight of the pigment preparation, of residual moisture, wherein the residual moisture comprises water and organic solvents. The pigment preparation according to the invention preferably contains less than 2.5% by weight of residual moisture, in particular less than 2% by weight of residual moisture. In one embodiment, the pigment preparation according to the invention contains a residual moisture content of 1.0 to less than 3% by weight, preferably of 1.0 to 2.5% by weight, particularly preferably of 1.0 to 2.0% by weight. The metallic effect pigment preparation according to the invention is in compacted form (and not in powder form).
[0020] The metallic effect pigment of the invention is preferably an aluminum or iron effect pigment, more preferably an aluminum effect pigment.
[0021] It is further preferred that in the pigment preparation of the present invention, the at least one metal oxide and / or metal hydroxide and / or metal oxide hydrate layer is selected from the group consisting of oxides, hydroxides or oxide hydrates of the elements silicon, vanadium, molybdenum, chromium, titanium, iron, aluminum, tin and mixtures thereof. In a preferred embodiment, the one or more layer(s) is / are a metal oxide layer, in particular a metal oxide layer or two or three metal oxide layers made of different metal oxides. In a preferred embodiment, the layer is an SiO2 layer. In a preferred embodiment, the metallic effect pigment is an aluminum effect pigment in which the metallic oxide, metallic hydroxide and / or metallic oxide hydrate layer comprises an SiO2 layer. In another preferred embodiment, the metallic core has an SiO2 layer and an iron oxide layer thereon.According to the invention, the layer thickness of the metal oxide, metal hydroxide, and / or metal oxide hydrate layer is 2-270 nm (total layer(s) thickness). In one embodiment, the layer thickness is preferably 7 to 270 nm, particularly preferably 7-100 nm, and most preferably 10 to 50 nm. In another embodiment, the layer thickness is preferably 150-270 nm, particularly preferably 260 nm. The at least one metal oxide and / or metal hydroxide and / or metal oxide hydrate layer can be modified with surface modifiers such as optionally functionalized silanes, for example alkyl-, alkoxy-, primary amino-, secondary amino-, epoxy-, isocyano-, mercapto-, azido-, (meth)acryl-, vinyl-, or hydroxyl-functionalized silanes.Furthermore, the metal oxide and / or metal hydroxide and / or metal oxide hydrate layer can be coated with a polymer layer for stabilization, for example based on polyacrylates or polymethacrylates, polyurethanes, polyesters, epoxides or polyolefins, optionally modified with silanes.
[0022] The water-soluble binder is preferably nonionic, more preferably a cellulose derivative. Preference is given to hydroxypropyl methylcellulose (e.g., Methocel (DuPont), VIVAPHARM HPMC (JRS)), hydroxypropyl cellulose (e.g., Klucel H (Ashland), Klucel E (Ashland)), hydroxyethyl cellulose (e.g., Tylose HEC (SE Tylose GmbH)), methylhydroxyethyl cellulose (e.g., Tylose MHEC (SE Tylose GmbH)). Further preference is given to polyvinylpyrrolidone (e.g., Sokalan K (BASF)) or acrylic acids (e.g., Carbopol (Lubrizol)). The surface-active additive is preferably a nonionic surface-active additive. Preferred non-ionic additives include polyglycol, polyvinyl butyral (PVB) and / or polyvinylpyrrolidone (PVP) or polysiloxanes (e.g. Getren (Evonik)), particularly preferred is a polyglycol.The polyglycol is preferably a polyethylene glycol or polypropylene glycol, in particular a polyethylene glycol with an average molar mass of 200-600 g / mol, preferably 300-500 g / mol, more preferably 380-420 g / mol. A particularly preferred polyethylene glycol ether is PEG 400 (PCC Chemax Inc.).
[0023] Ionic surface-active additives can also be used according to the invention. Preferred ionic additives include alkyl sulfates (e.g., Chemsulf (PCC Chemax Inc.), Rewopol (Evonik), ROSULfan E (PCC Chemax Inc.)), alkyl sulfosuccinates (e.g., PLANTAPON SUS (BASF), TEXAPON SB 3 KC (BASF), Genapol SBE (Clariant), Rewopol SB (Evonik)), alkylbenzene and paraffin sulfonates (e.g., Marlon A (Sasol Chemicals), Marlopon AT (Sasol Chemicals)), and secondary alkanesulfonates (e.g., MERSOLAT H (Lanxess)). Further preferred are alkyl ether sulfates (e.g. SUL- FOROKanol (PCC Chemax Inc.), ROSULfan OD (PCC Chemax Inc.), EXOsoft MG (PCC Chemax Inc.)), alkyl carboxylates (e.g. Tween 20 (Croda)), benzalkonium chloride (e.g. BTC 1218-50 (ADBAC)), taurides (e.g. Igepon TK (Nantong Tailida Chemical Industry)), or amine oxides (e.g. Tegotens (Evonik)).
[0024] The binder in the pigment preparation according to the invention has the particular function of enabling the pigment preparation to be directly dispersed into an application medium, for example, a varnish or paint, without prior slurrying. The metallic effect pigments are then present in the application medium in a non-agglomerated form.
[0025] In a preferred embodiment, the pigment preparation according to the invention comprises 88-92% by weight, preferably 90% by weight, of an SiO2-coated aluminum effect pigment, as well as 5-8% by weight, preferably 6% by weight, of a hydroxypropyl methylcellulose, and 2-4% by weight, preferably 3% by weight, of a nonionic wetting agent based on polyethylene glycol, with a phosphorus content of less than 50 ppm and a residual moisture content of 1-2% by weight. This pigment preparation is preferably in compacted form, particularly preferably in granular form.
[0026] In another preferred embodiment, the pigment preparation according to the invention comprises 78-82% by weight, preferably 80% by weight, of an SiO2-coated aluminum effect pigment, as well as 8-12% by weight, preferably 10% by weight, of a hydroxypropyl methylcellulose, and 8-12% by weight, preferably 9% by weight, of a nonionic wetting agent based on polyethylene glycol, with a phosphorus content of less than 50 ppm and a residual moisture content of 1-2% by weight. This pigment preparation is preferably in compacted form, particularly preferably in granular form.
[0027] The invention further relates to a process for producing the pigment preparation according to the invention, comprising the steps of a) mixing a metallic effect pigment having one or more metal oxide and / or metal hydroxide and / or metal oxide hydrate layers on a metallic core with at least one water-soluble binder and a surface-active additive, b) compacting the mixture obtained in step a), c) optionally drying the compacted mixture.
[0028] The mixture is preferably compacted by pressing, tabletting, briquetting, pelletizing, granulating, or extruding, or a combination of these processes. The resulting compacted product is preferably in granular form. The granules are preferably cylindrical (with diameters of about 0.5 mm to about 5 mm and lengths of about 0.1 cm to about 8 cm). The granules in cylindrical form of the metallic effect pigment preparation usable according to the invention preferably have a diameter of 1 to 3 mm and a length of 0.5 to 7 cm, more preferably a diameter of 1.5 to 2.5 mm and a length of 1 to 5 cm.Such granules can be produced by conventional processes such as extrusion, perforation pressing (a press with a ram and perforated plate), or extrusion, especially low-pressure extrusion using a basket extruder, optionally with subsequent drying (at approximately 20°C to 150°C) and comminution using, for example, a rotating knife. Spherical granules with diameters of approximately 0.05 to approximately 5 mm, in particular 1 to 3 mm, can also be used; these can be produced using spray and fluidized-bed granulation or with a granulating disc.
[0029] Drying is preferably carried out at elevated temperature, for example above 40 °C, preferably between 55 and 65 °C.
[0030] The present invention also relates to the use of the pigment preparation according to the invention, in particular in paints, varnishes, powder coatings, masterbatches, printing inks, plastics, cosmetic preparations and the use in security printing or security printing.
[0031] It is understood that the features mentioned above and those to be explained below can be used not only in the specified combinations, but also in other combinations or alone, without departing from the scope of the present invention. The advantages of features or combinations of several features mentioned are merely exemplary and can be used alternatively or cumulatively.
[0032] The following examples and comparative examples further explain the invention and show advantages of the invention.
[0033] Examples according to the invention:
[0034] Example 1 : Granule production
[0035] 30 g of Methocel E5 Premium LV binder (hydroxypropyl methylcellulose (methoxyl content: 28.0-30.0%; hydroxypropoxyl content: 7.0-12.0%; viscosity 2% in water at 20°C: 4.0-6.0 cP), Dupont) were dissolved in 100 mL of cold water. Of this solution, 16.3 g were homogenized together with 2.1 g of PEG 400 (polyethylene glycol, average molar mass: 380-420 g / mol) and 120.68 g of filter cake (Aquamet ST-IL 10600 / 50 silver dollar coated with SiO2 in isopropanol (sales product of Schlenk)). The homogenized mixture thus contained 63 g of the SiO2-coated aluminum pigment. It was pressed into granules with a diameter of approximately 2 mm and a length of approximately 1-5 cm using a press with a punch and perforated plate. The granules were then dried in a drying cabinet at 60°C for 5 hours. The resulting granules comprised 89.6% by weight of aluminum pigment, 6.5% by weight of a water-soluble binder, 2.6% by weight of the binder.-% of a surface-active additive and 1.3 wt.% residual moisture.
[0036] Example 2: Granule production
[0037] 5 g of binder Methocel E10 M Premium CR (hydroxypropyl methylcellulose (methoxyl content: 28.0 - 30.0%; hydroxypropoxyl content: 7.0 - 12.0%; viscosity 2% in water at 20°C: 7500 - 15000 cP) Dupont) were dissolved in 100 mL of cold water. 70 g of this solution were homogenized together with 3.5 g of PEG 400 (polyethylene glycol, average molar mass: 380 - 420 g / mol) and 116.02 g of filter cake (Aquamet ST-IL 10600 / 50 silver dollar coated with SiO2 in isopropanol (Schlenk)). The homogenized mixture thus contained 63 g of the SiO2-coated aluminum pigment. It was pressed into granules with a diameter of approximately 2 mm and a length of approximately 1-5 cm using a press with a stamp and perforated plate. The granules were then dried in a drying cabinet at 60°C for 5 hours. The resulting granules comprised 89.5% by weight of aluminum pigment, 6.4% by weight of a water-soluble binder, 2.5% by weight of a surface-active additive, and 1.6% by weight of a binder.-% residual moisture.
[0038] Examples not inventive:
[0039] Comparative example 3: Granule production
[0040] 30 g of Methocel E5 Premium LV binder (hydroxypropyl methylcellulose (methoxyl content: 28.0-30.0%; hydroxypropoxyl content: 7.0-12.0%; viscosity 2% in water at 20°C: 4.0-6.0 cP) Dupont) were dissolved in 100 mL of cold water. 18.7 g of this solution were mixed with 2.4 g of PEG 400 (polyethylene glycol, average molar mass: 380-420 g / mol) and 122.61 g of filter cake (Aquamet ST-IL 10600 / 50 silver dollar coated with SiO2 in isopropanol (sales product of Schlenk)). A mixture of 2.4 g of Phosphetal 218 (from Zschimmer & Schwarz), 1.08 g of triethanolamine, 0.98 g of Pluriol E4000 (from BASF), 0.49 g of MCT oil, and 3 g of ethanol was added, and the mixture was then homogenized. The homogenized mixture thus contained 64 g of the SiO 2 - coated aluminum pigment. It was pressed into granules with a diameter of approximately 2 mm and a length of approximately 1-5 cm using a press equipped with a die and perforated plate.The granules were then dried in a drying cabinet at 60 °C for 12 hours.
[0041] Comparative example 4: Granules Grandal W 10600 (sales product of Schlenk)
[0042] Comparative example 5: Granules Aquavex® Plus Ultra 011 (sales product of Silberline)
[0043] Comparative example 6: Granules Aquavex® Plus Premier 011 (sales product of Silberline)
[0044] Characterization of the pigment preparations
[0045] Test for dust-freeness and dimensional stability of the granules:
[0046] To test the dust-free nature of the pigment preparation, a defined amount of granules (3 g) is filled into a plastic container and shaken on a shaker (GFL 3006) for 0.5 h at a shaking frequency of 300 mm 1shaken. The granules are then removed from the plastic container, and the remaining abrasion is weighed using an analytical balance. The percentage abrasion is thus determined.
[0047] Determination of the Al content of the granules:
[0048] The aluminum content of the granules is determined using thermogravimetric analysis. For this purpose, 10 mg of the pigment preparation is weighed into an aluminum oxide crucible. This is then placed in the Netzsch STA 449 F5 Jupiter apparatus. The TGA chamber is closed, and a constant flow of nitrogen is introduced into the sample chamber. The crucible is heated to 1500°C at a starting temperature of 30°C and a heating rate of 10°K / min, and the weight loss or weight gain of the crucible is measured. The percentage of aluminum in the sample can be determined from the weight gain from approximately 600°C to approximately 850°C. This is due to the nitration reaction of aluminum, whereby metallic aluminum reacts directly with the incoming nitrogen to form aluminum nitride.
[0049] Determination of the phosphorus content of the granules:
[0050] To determine the phosphorus content of the pigment preparation, optical emission spectrometry (OES) is performed using the Spectro Genesis and Spectroblue FMX36 instruments. These operate with inductively coupled plasma excitation and semiconductor-based CCD detector systems. Liquid samples are used for this, which is why the pigment preparation must be digested before measurement. A distinction must be made between SiO2-coated and uncoated samples. The uncoated samples are weighed (500 mg) in an Erlenmeyer flask and mixed with 10 mL of water and 10 mL of HCl (diluted 1 / 1). Then, 5 mL of a 30% H2O2 solution are added. The mixture is heated briefly, and excess H2O2 is boiled off after the digestion reaction. The solution is cooled to room temperature and diluted to the desired dilution with deionized water.The coated samples are weighed (500 mg) into a Teflon crucible and dissolved in 15 mL HNO3 (37%). After the reaction is complete, the samples are mixed with 15 mL HCl (diluted 1 / 1) and cooled to room temperature. 3 mL of hydrofluoric acid (40%) are then added, and the sample is left to stand, covered, for 3 hours. The sample is then diluted to the desired dilution with deionized water. To measure the phosphorus content, the liquid sample is atomized and introduced into the plasma as an aerosol, where it is evaporated. The emitted radiation is fed into the system via the transfer optics and optically resolved into its spectral components, the intensity of which is recorded by the CCD detector. To determine the element concentrations, element-specific calibration curves are measured in advance, and calibration functions are created from them.
[0051] Determination of the residual solvent content of the granules:
[0052] To determine the residual solvent content of the pigment preparation, a weighing boat made of thin aluminum foil is placed on the Sartorius Ultramat MA35. The weight of the weighing boat is tared, and 2 g of the pigment preparation is added to it. The lid of the Ultramat is then closed, and the pigment preparation is heated to 120°C. During this time, the weight of the pigment preparation is continuously determined. When no further weight loss can be registered, the solids content of the pigment preparation is determined in percent from the initial weight and the remaining weight of the pigment preparation. The residual moisture content of the pigment preparation corresponds to the value resulting from subtracting the solids from 100%.
[0053] Determination of the stability of the granules using GFM measurement:
[0054] The resistance change in the heating wire of the bypass tube in the gas mass flow meter (ENZ) is measured. For a constant gas type in the bypass tube, the resistance change is proportional to the gas mass flow. Due to the measuring principle, value correction is not necessary for a wider temperature and air pressure range. For the measurement, 9.0 g of calcium hydroxide and 350 mL of deionized water are placed in a three-necked flask equipped with the gas mass flow meter and a KPG stirrer. The mixture is stirred for 5 minutes at 500 rpm. Ensure that the gas mass flow meter and the KPG stirrer are connected to the flask in a gas-tight manner. The three-necked flask is immersed in a water bath maintained at 25 + / - 0.5 °C for the entire measurement period, up to the middle of the necks. Depending on the metal content, enough of the granulate is weighed to obtain a calculated amount of 600 mg of aluminum.The granules are weighed into a preformed cap made of weighing paper, in which they are predispersed with 4 mL of soap solution and a rounded glass rod. The measurement program is then started, measuring the gas mass flow every 10 seconds for 16 minutes. The measurement program is equipped with a countdown that counts down from 5 before the measurement is started. This allows the cap to be pushed into the flask with the help of the glass rod, and the flask can be sealed gas-tight with a rubber stopper 1 second before the measurement starts. The integral over the measurement curve gives the total value of the hydrogen produced during the decomposition of the aluminum. The lower this value, the more stable the pigment in an aqueous alkaline environment. The values for the individual pigments are listed in Table 1. It is noticeable that inventive examples 1 and 2, as well as examples 3 and 4, are exceptionally stable, in contrast to example 5.
[0055] Data of the pigment preparations
[0056] Table 1: Assessment of dust-free properties, stability and environmental impact of the granules.
[0057] The measured values in Table 1 clearly show that no phosphorus-containing compounds are present in inventive examples 1 and 2, whereas at least 5000 ppm of phosphorus can be detected in comparative examples 3-6. Furthermore, the increased dimensional stability of inventive examples 1 and 2 is also evident, as they exhibit hardly any abrasion after prolonged mechanical stress. A further advantage of inventive examples 1 and 2 is the increased metal content compared to examples 3-6. This leads to a lower incorporation of binder into the coating formulation and to a lower consumption of pigment preparation. In addition, the environmental compatibility of inventive examples 1 and 2 is also significantly improved.This is evident from the lack of a water hazard class, in contrast to Comparative Examples 3 and 4, which must be classified in Water Hazard Class 1, and Comparative Examples 5 and 6, which must be classified in Water Hazard Class 2. Furthermore, the very good stability of inventive Examples 1 and 2 in aqueous systems should also be noted. Especially in comparison to Comparative Examples 5 and 6, a significant improvement in stability can be observed in the aqueous-alkaline environment, which normally prevails in aqueous coating formulations.
[0058] Testing of pigment preparations in a printing ink:
[0059] Testing for interlayer adhesion:
[0060] To test intercoat adhesion, a print of the pigment preparation was produced. For this purpose, the pigment preparation (10% metal content) was dispersed in an aqueous varnish (69.9%) together with the defoamer Tego Foamex 800 (1.0%; Evonic) and a film former dipropylene glycol (2.0%). The viscosity was adjusted to approximately 60 s using water. This viscosity was determined using a flow cup according to DIN EN ISO 2431 by measuring the time required for the formulation to flow out of the standardized cup. The aqueous varnish consists of 75% NeoCryl® BT-21 (Covestro), 0.2% Tego Foamex 800 (Evonic), 19% water, and 5.8% DMAMP-80 (Angus). The printing ink was then applied to glossy coated paper (120g / m 2 ) was printed. For this purpose, a printing roller with a capacity of 14.65 cm 3 / m 2and a printing speed of 30 m / min is used.
[0061] The Tesa test to determine interlayer adhesion according to DIN EN ISO 10683 was then carried out three times: immediately, one hour, and 24 hours after printing. A Tesa brand adhesive tape was firmly adhered to the surface printed with the pigment preparation, smoothed 10 times with the finger, then peeled off and stuck onto a transparent glass pane. Figure 1 shows the result of the Tesa test 2 weeks after printing. With good interlayer adhesion, there are hardly any pigment residues on the adhesive tape, whereas with poor interlayer adhesion, the pigment adheres to the adhesive tape and leaves clear contours of the Tesa film on the printed image. Due to the loss of transparency of the adhesive tape, a qualitative statement about the interlayer adhesion of the print can be made by measuring the T_den value. The T_den value describes the transparency of a material.The lower the T_den value, the more transparent the material being measured. The T_den value of the Tesa film was measured using a transparency and haze meter from BYK. This uses a light source with a nearly parallel beam path. The light beam hits the clamped sample, which is located directly at the entrance to an integrating sphere, at a right angle. The light is partially reflected and absorbed by the sample, and the remaining portion is transmitted into the integrating sphere. The sphere's surface allows for diffuse scattering, allowing the built-in sensor to detect the total transmittance. The percentage difference between the intensity of the incident light beam and the measured total transmittance gives the T_den value. Before the Tesa film, which has been removed from the print, is measured, a background measurement is carried out using an unused Tesa film to prevent its influence on the measurement.In addition, a T_den measurement is taken on the proof to demonstrate the opacity of the pigment preparation, as well as after the Tesa test to demonstrate the influence of interlayer adhesion on the opacity of the print. The lower the T_den value, the better the interlayer adhesion. Measurement of optical properties:
[0062] The BYK-mac i 23 mm measuring device from BYK is used to measure the brightness (L15) of the printed images. The BYK micro-gloss 60° device is used to measure gloss.
[0063] Table 2: Measurement values of a printing ink produced with inventive examples 1 and 2 and comparative examples 3-4
[0064] The measured values in Table 2 show that inventive examples 1 and 2 exhibit significantly better interlayer adhesion than comparative examples 3 and 4, since the Tesa film does not pull any pigment from the proof (see Figure 1), even immediately after printing. The brightness (L15) and gloss of inventive examples 1 and 2 are equivalent to those of comparative examples 3 and 4, despite the lack of organophosphorus compounds.
[0065] Application of pigment preparation in powder coating
[0066] For the application of the pigment preparation in powder coating, it must be bonded. For this purpose, inventive example 1 (pigment preparation in granular form) is compared with its starting material, Aquamet ST-IL 10600 / 50 (a commercial product from Schlenk). This is first dried in an oven at 120°C for 5 hours to obtain a powder from the isopropanol paste. The corresponding powder is referred to below as Comparative Example 7. Bonding procedure:
[0067] In the bonding process, the pigment preparation or pigment powder is mixed with the corresponding powder coating (transparent in PES-PRIMID or PES-PRIMID black high-gloss). The material mixture is then brought to the glass transition temperature of the powder coating and heated 2°C above the DSC end set point. This takes place with a constant mixing movement to ensure complete dispersion of the powder coating-pigment mixture. The pigment content of the pigment preparation in the powder coating is 3% for the transparent PES-PRIMID system and 1% for the black high-gloss PES-PRIMID system. After reaching a specified temperature above the DSC end set point, the mixture is cooled as quickly as possible to prevent a curing reaction. Before the powder is applied, a protective sieve is also carried out using a sieve with a mesh size of 100 μm to remove any agglomerates.
[0068] Powder coating application:
[0069] A powder gun from Gema is used to apply the bonded powder coating. The bonded transparent PES-PRIMID powder coating is applied with the following gun parameters (20% powder cloud, 2.5 Nm / cm A 3, 60 mA, 90 kV) is applied to a sheet metal panel and then baked at 180 °C for 20 minutes. The bonded black high-gloss PES-PRIMID powder coating is applied with the following gun parameters (20% powder cloud, 2.5 Nm / cm A 3, 60 mA, 90 kV) was also applied to a sheet metal panel and then baked at 180 °C for 20 minutes.
[0070] Optical inspection of the coating:
[0071] The optical properties were measured in the same way as the printed images. Table 3: Measurement values of the powder coating application, bonded in the transparent PES-PRIMID system
[0072] Table 4: Measurement values of powder coating application, bonded in the black high gloss PES-PRIMID system
[0073] It can be seen here that Inventive Example 1 exhibits a higher gloss than Comparative Example 7, particularly in the application with the transparent PES-PRIMID system, the gloss is significantly increased. Furthermore, the flop index of the application with the transparent PES-PRIMID system is also increased with Inventive Example 1 compared to Comparative Example 7.
[0074] In addition, the dust-free dosing of the granulate form of Example 1 according to the invention significantly reduces dust exposure during the bonding process, in contrast to Comparative Example 7. Handling, storage stability, and occupational safety are significantly improved by using the metallic effect preparation according to the invention.
Claims
Claims 1. Pigment preparation with metallic effect pigments, characterized in that the pigment preparation comprises the following components: a) 60–98 wt.%, based on the total weight of the pigment preparation, of at least one metallic effect pigment having one or more metal oxide and / or metal hydroxide and / or metal oxide hydrate layers on a metallic core; b) 1–30 wt.%, based on the total weight of the pigment preparation, of at least one water-soluble binder; c) 1–30 wt.%, based on the total weight of the pigment preparation, of a surfactant additive; and d) less than 3 wt.%, based on the total weight of the pigment preparation, residual moisture, wherein the residual moisture comprises water and organic solvents, and wherein the pigment preparation contains less than 500 ppm phosphorus.
2. Pigment preparation according to claim 1, characterized in that the metal oxide and / or metal hydroxide and / or metal oxide hydrate layer is selected from the group consisting of oxides, hydroxides or oxide hydrates of the elements silicon, vanadium, molybdenum, chromium, titanium, iron, aluminum, tin and mixtures thereof.
3. Pigment preparation according to one of the preceding claims, characterized in that the metal effect pigment is an aluminum effect pigment, preferably an aluminum effect pigment in which the metal oxide, metal hydroxide and / or metal oxide hydrate layer comprises a SiO2 layer.
4. Pigment preparation according to one of the preceding claims, characterized in that the layer thickness of the metal oxide, metal hydroxide and / or metal oxide hydrate layer is 2 - 270 nm, preferably 7 - 270 nm.
5. Pigment preparation according to one of the preceding claims, characterized in that the water-soluble binder is non-ionic.
6. Pigment preparation according to one of the preceding claims, characterized in that the water-soluble binder is a cellulose derivative, preferably hydroxypropyl methylcellulose.
7. Pigment preparation according to one of the preceding claims, characterized in that the surfactant additive is an ionic surfactant additive.
8. Pigment preparation according to any one of claims 1 to 6, characterized in that the surfactant additive is a non-ionic surfactant additive, preferably a polyglycol, polyvinyl butyral (PVB) and / or polyvinylpyrrolidone (PVP).
9. Pigment preparation according to claim 8, characterized in that the polyglycol is a polyethylene glycol or polypropylene glycol.
10. Pigment preparation according to claim 9, characterized in that the polyethylene glycol has a mean molar mass of 200 - 600 g / mol, preferably 380 - 420 g / mol.
11. Pigment preparation according to one of the preceding claims, characterized in that the pigment preparation has less than 200 ppm phosphorus.
12. Pigment preparation according to one of the preceding claims, characterized in that the pigment preparation is in granular form.
13. A method for producing a pigment preparation according to one of the preceding claims, characterized in that it comprises the following steps: a) Mixing a metallic effect pigment having one or more metal oxide and / or metal hydroxide and / or metal oxide hydrate layers on a metallic core with at least one water-soluble binder and a surfactant additive, b) Compacting the mixture obtained in step a), c) Optionally drying the compacted mixture.
14. The method according to claim 13, wherein the produced pigment preparation is in granular form.
15. Use of a pigment preparation according to any one of claims 1-12 in paints, varnishes, powder coatings, masterbatches, printing inks, plastics, cosmetic preparations, in security printing or security printing.
Citation Information
Patent Citations
Effect pigment preparation
US10385230B2
Solid type pigment composition and preparation method thereof
CN105602295A
pigment preparation in granular form
DE10046152A1
Pigment preparation
EP0964895B1
Thin Covering Aluminum Pigments, Process For The Production Thereof, And Use Of Said Aluminum Pigments
US20070199478A1