Poly-arm-type resin having polyamide structure or heterocyclic structure, lithography film-forming composition containing same, and production method
A multibranched polyamide resin with a branched structure addresses the poor solubility and film-forming issues of PBO resin, offering enhanced solubility and heat resistance for advanced lithography and optical applications.
Patent Information
- Application Number
- PCT/JP2023/029632
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-08-16
- Publication Date
- 2024-10-31
AI Technical Summary
Polybenzoxazole (PBO) resin exhibits excellent heat resistance, chemical resistance, and mechanical properties but has poor solubility and film-forming properties due to its rigid structure, limiting its applications.
A multibranched resin with a polyamide structure is developed by condensing a diamino compound and a tricarboxylic acid compound, incorporating a branched alkylene or fluorinated alkylene group, which enhances solubility and film-forming properties, and can be further converted into a heterocyclic structure for improved performance.
The resulting resin demonstrates excellent film-forming properties, high refractive index, and extreme heat resistance, making it suitable for lithography and optical applications with improved solubility and processing stability.
Smart Images

Figure JP2023029632_31102024_PF_FP_ABST
Abstract
Description
Hyperbranched resin having polyamide structure or heterocyclic structure, lithography film-forming composition containing the same, and production method
[0001] The present invention relates to a hyperbranched resin having a polyamide structure or a heterocyclic structure, a lithography film-forming composition containing the same, and a production method.
[0002] Polybenzoxazole (PBO) resins have excellent heat resistance, chemical resistance, and mechanical properties, making them promising for a variety of applications. However, due to their rigid structure, they are poor in solubility and film-forming properties. Therefore, branched PBOs have been proposed (see, for example, Non-Patent Document 1).
[0003] Hiroto Kudo et. al., Journal of Polymer Science Part A Polymer Chemistry 44(11):3640 - 3649 (2006).
[0004] The resin described in Non-Patent Document 1 is amorphous and soluble in a solvent. However, there is room for improvement in terms of film-forming properties. In view of the above circumstances, an object of the present invention is to provide a resin with excellent film-forming properties.
[0005] The inventors have found that a resin into which a group of a specific structure has been introduced solves the above-mentioned problems. Aspect 1: A hyperbranched resin having a polyamide structure, produced by a method comprising: (I) preparing a diamino compound represented by formula (A) described below and a tricarboxylic acid compound represented by formula (B) described below; and (II) subjecting these compounds to a condensation reaction to form a polyamide structure. Aspect 2: The resin according to Aspect 1, in which Y in the formula is a branched alkylene group. Aspect 3: The resin according to Aspect 1 or 2, in which Y in the formula is a fluorinated alkylene group. Aspect 4: A hyperbranched resin having a heterocyclic structure, produced by a method comprising: (i) preparing a hyperbranched resin having a polyamide structure according to any one of Aspects 1 to 3; and (ii) subjecting the resin to intramolecular condensation to form a heterocyclic structure. Aspect 5: The resin according to Aspect 4, wherein a unit in which Y is an alkylene group and a unit in which Y is a fluorinated alkylene group are present, and the molar ratio of the alkylene group to the fluorinated alkylene group is 1:(1.5 to 10). Aspect 6: A lithographic film-forming composition comprising the resin according to any one of Aspects 1 to 5. Aspect 7: A lithographic underlayer film-forming composition comprising the resin according to Aspect 3. Aspect 8: The composition according to Aspect 6 or 7, comprising a solvent. Aspect 9: The composition according to any one of Aspects 6 to 8, comprising a component selected from the group consisting of a solvent, an acid generator, an acid crosslinker, and combinations thereof. Aspect 10: A lithographic underlayer film formed using the composition according to Aspect 7. Aspect 11: A lithographic underlayer film comprising the resin according to Aspect 4 or 5. A method for forming a resist pattern, comprising the steps of: forming an underlayer film on a substrate using the composition according to Aspect 7, and heating the precursor to 300°C or higher to form an underlayer film containing a hyperbranched resin having a heterocyclic structure; forming at least one photoresist layer on the underlayer film; and irradiating predetermined regions of the photoresist layer with radiation and developing. Aspect 13: A hyperbranched resin having a polyamide structure, represented by formula (1) described below. Aspect 14: A hyperbranched resin having a heterocyclic structure, represented by formula (2) described below.Aspect 15: The resin according to aspect 13 or 14, wherein X in the formula is represented by any one of formulas (X1) to (X4) described below.
[0006] A resin with excellent film-forming properties can be provided.
[0007] Tricarboxylic acid intermediate 1 H-NMR and 13 C-NMR spectrum of tricarboxylic acid intermediates FT-IR spectrum of tricarboxylic acid compounds 1 H-NMR spectrum of hyperbranched PA resin 1 H-NMR spectrum GPC chart of hyperbranched PA resin Tricarboxylic acid compound 1 H-NMR and 13 C-NMR spectrum of hyperbranched PA resin 1 H-NMR spectrumGPC chart of hyperbranched PA resinTGA (thermogravimetry) chart of hyperbranched PA resinGPC chart of hyperbranched PA resinGPC chart of hyperbranched PA resinFT-IR spectrum of hyperbranched PA resinFT-IR spectrum of hyperbranched PBO resinTGA (thermogravimetry) chart of hyperbranched PBO resin
[0008] 1. Hyperbranched Resin Having a Polyamide Structure In one embodiment, a hyperbranched resin having a polyamide structure is obtained by reacting a diamino compound represented by formula (A) with a tricarboxylic acid compound represented by formula (B). A hyperbranched resin is a resin having branched chains attached to the main chain, where the branched chains are not long enough to form a gel. In this disclosure, "X to Y" include the end values.
[0009] (1) (A) Diamino Compound The diamino compound represented by formula (A) (hereinafter also referred to as "Compound A") is a compound essentially containing two amino groups. The amino groups are preferably primary amino groups. In addition to the two amino groups, Compound A has a group Z. Group Z is selected from the group consisting of -OH, -SH, -NH 2 and combinations thereof.
[0010]
[0011] Y is an alkylene group which may contain fluorine. Examples of Y include alkylene groups having 1 to 6 carbon atoms and fluorinated alkylene groups having 1 to 6 carbon atoms. The number of carbon atoms in these groups is more preferably 1 to 3. Y is preferably a branched alkylene group or a branched fluorinated alkylene group. From the viewpoint of availability, Y is preferably -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -CH(CF 3 )-, and -C(CF 3 ) 2 --etc.
[0012] Z is independently —OH, —SH, or —NH 2 Among these, from the viewpoints of solubility in a solvent or ease of availability of a multi-branched resin having a polyamide structure, Z is preferably —OH.
[0013] Each R is independently a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group, or a hydroxyl group. The aryl group, aralkyl group, alkenyl group, alkynyl group, and arylalkenyl group may contain an ether bond, a ketone bond, an ester bond, or a urethane bond. However, in consideration of heat resistance and the like, R is preferably a hydrogen atom.
[0014] When R is a group other than hydrogen, m represents the number of such groups and is an integer of 1 to 3. When R is a group other than hydrogen, m is preferably 1 in consideration of heat resistance and the like. Preferred embodiments of Compound A are exemplified below.
[0015]
[0016] (2) (B) Tricarboxylic Acid Compound The tricarboxylic acid compound represented by formula (B) (hereinafter also referred to as "compound B") is a compound having three carboxyl groups or derivative groups thereof.
[0017]
[0018] Ar is a group having an aromatic group. Ar is not limited to, but may be an aryltriyl group obtained by removing three hydrogen atoms from an aromatic compound, or a group obtained by removing three hydrogen atoms from the aromatic ring of a triarylalkane.
[0019] E is -COOH, -COHal, -O-R b —COOH or —O—R b -COHal. Hal is a halogen atom, preferably a chlorine atom. R b is an alkylene group having 1 to 6 carbon atoms, preferably an alkylene group having 1 to 3 carbon atoms. More preferably, R b is a methylene group or an ethylene group. Preferred examples of Compound B are shown below.
[0020]
[0021] (3) Structure The resin (hereinafter, for convenience, also referred to as "hyperbranched PA resin") is obtained by a condensation reaction between compound A and compound B. This reaction generates an amide bond, resulting in a polymer having a polyamide structure. The structure of the hyperbranched PA resin is represented as follows:
[0022]
[0023] In the formula, Y, Z, R, and m are defined as above. n is the number of repeats in the main chain, and r is the number of repeats in the branched chain, with n>r. n is not limited, but is preferably 1 to 100, more preferably 2 to 30. If r is too large, gelation occurs, and if r is too small, solubility in solvents decreases. r is selected so that the hyperbranched PA resin does not gel and exhibits solubility. In one embodiment, r can be approximately 10 to 60% of n.
[0024] (4) Properties The hyperbranched PA resin has flexibility due to the presence of Y, and a moderately low density due to the branched chains. Therefore, it has good solubility in solvents and good film-forming properties. Furthermore, if part or all of Y is a fluorinated alkylene group, the density of the resin is moderately reduced and solubility is further increased, which is preferable. Furthermore, if part or all of Y is a fluorinated alkylene group, deterioration of the resin can be avoided when the hyperbranched PA resin is subjected to intramolecular condensation. When a unit in which Y is an alkylene group and a unit in which Y is a fluorinated alkylene group are present, the molar ratio of the alkylene group to the fluorinated alkylene group is preferably 1:(1.5 to 10), and more preferably 1:(2 to 6).
[0025] The resin is useful as a lithography material. Furthermore, because the resin has a high refractive index, it is also useful as an optical component. Furthermore, because the amino group reacts with Z to form a ring, the hyperbranched PA resin can be converted into a resin having a heterocyclic structure. Resins having a heterocyclic structure have extremely high heat resistance and are useful as lithography films, particularly as lithography underlayer films.
[0026] 2. Method for Producing Hyperbranched PA Resin Hyperbranched PA resin is obtained by condensing compound A and compound B. The charge ratio is selected so as to obtain the desired molecular weight and branched chains. The charge ratio of the two can be determined as the ratio of functional group equivalents forming an amide bond. The functional group equivalent ratio (functional group equivalent of compound A: functional group equivalent of compound B) is preferably (1 to 2):1, more preferably (1.1 to 1.6):1. The reaction temperature is selected so as not to form a gel, and in one embodiment, it is 20 to 40°C. The reaction time is also not limited and can be, for example, about 20 to 72 hours.
[0027] If the amount of solvent is small, gelation is likely to occur, while if it is large, production efficiency decreases. In one embodiment, the amount of solvent is 8 to 10 parts by weight per 1 part by weight of the total amount of compounds A and B. The solvent is preferably an aprotic solvent such as NMP (N-methylpyrrolidone) or DMF (dimethylformamide). The reaction is preferably carried out under an inert atmosphere. Also, known condensing agents can be used for the condensation reaction.
[0028] 3. Hyperbranched Resin Having a Heterocyclic Structure This resin (hereinafter, for convenience, also referred to as "hyperbranched heterocyclic resin") is obtained by subjecting a hyperbranched PA resin to an intramolecular condensation reaction. Through this reaction, the amino group and Z form a heterocyclic structure. As mentioned above, it is preferable that some or all of Y are fluorinated alkylene groups. When there are units in which Y is an alkylene group and units in which Y is a fluorinated alkylene group, the molar ratio of the alkylene group to the fluorinated alkylene group is preferably 1:(1.5 to 10), and more preferably 1:(2 to 6). The structure of this resin is preferably represented as follows:
[0029]
[0030] Y 1 and Y 2 is derived from Y of the hyperbranched PA resin. 1 is a fluorinated alkylene group, Y 2 is an alkylene group. The alkylene group is as explained in the description of the hyperbranched PA resin.
[0031] Z' is derived from Z in the hyperbranched PA resin. Z' is independently -O-, -S-, or -NH-. From the viewpoint of ease of synthesis, Z' is preferably -O-. In this case, the heterocycle is a benzoxazole ring, and therefore the resin in this case is also called a "hyperbranched PBO resin."
[0032] X is a group having an aromatic group derived from Ar of the hyperbranched PA resin. X is preferably a group represented by the following formula:
[0033]
[0034] Ar is an aromatic group, as explained in the multi-branched PA resin. b is an alkylene group having 1 to 6 carbon atoms, and the preferred embodiments thereof are as explained for the hyperbranched PA resin.
[0035] R and m are as described for the hyperbranched PA resin.
[0036] n 1 and n 2is the number of repeats in the main chain. 1 and r 2 is the number of repeats in the branched chain. 1 >r 1 And n 2 >r 2 It is. 1 and n 2 The sum of these corresponds to n of the hyperbranched PA resin, and r 1 and r 2 The sum of these corresponds to the r of the hyperbranched PA resin. 1 :n 2 and r 1 :r 2 The ratio of Y 1 :Y 2 For example, when the hyperbranched PA resin does not contain a fluorinated alkylene group as Y, the ratio of n 1 and r 1 is 0. In one embodiment, r 1 and 2 The sum of 1 and 2 It can be about 10 to 60% of the total.
[0037] 4. Method for Producing a Hyperbranched Heterocyclic Resin The resin is produced by a method comprising the steps of (i) preparing a hyperbranched PA resin, and (ii) intramolecularly condensing the resin to form a heterocyclic structure. Step (i) is as described above. Step (ii) can be carried out by heating the hyperbranched PA resin to 250°C or higher. The temperature is preferably 300 to 320°C. This step is preferably carried out in an inert atmosphere.
[0038] The hyperbranched heterocyclic resin has extremely high chemical resistance, and therefore it is preferable to cast the precursor hyperbranched PA resin into a desired shape (such as a membrane) and then carry out this step in that state.
[0039] 5. Composition [Composition] The hyperbranched resin is suitable for lithography applications or optical article applications, and is therefore useful in compositions for such applications.
[0040] [Lithography Film-Forming Composition] The lithography film-forming composition is a composition containing the above-mentioned hyperbranched resin as an essential component, and preferably contains a solvent. The composition is capable of reducing film defects (thin film formation), has good storage stability, high sensitivity, a high refractive index in a specific wavelength region, heat resistance, and chemical resistance, and can impart a good resist pattern shape. From the viewpoint of solubility in solvents, the hyperbranched resin is preferably a hyperbranched PA resin.
[0041] (Physical Properties of Lithography Film-Forming Composition) The composition can be used to form an amorphous film by a known method such as spin coating. Depending on the type of developer used, either a positive resist pattern or a negative resist pattern can be formed. The following describes the use of the composition as a resist composition.
[0042] When the lithography film-forming composition is used to form a positive resist pattern, the dissolution rate of the amorphous film formed by spin coating in a developer at 23°C is preferably 5 Å / sec or less, more preferably 0.0005 to 5 Å / sec, and even more preferably 0.05 to 5 Å / sec. A dissolution rate of 5 Å / sec or less can result in a resist that is insoluble in the developer. Furthermore, a dissolution rate of 0.0005 Å / sec or more can improve resolution. This is presumably because the change in solubility of the resin before and after exposure increases the contrast at the interface between the exposed portion that dissolves in the developer and the unexposed portion that does not dissolve in the developer. Furthermore, the composition is effective in reducing line edge roughness and defects.
[0043] When the lithography film-forming composition is used to form a negative resist pattern, the dissolution rate of the amorphous film formed by spin coating in a developer at 23°C is preferably 10 Å / sec or higher. A dissolution rate of 10 Å / sec or higher means that the film is easily soluble in the developer, making it more suitable for use as a resist. A dissolution rate of 10 Å / sec or higher may also improve resolution. This is presumably because the microscopic surface regions of the resin dissolve, reducing line edge roughness. It also has the effect of reducing defects. The dissolution rate can be determined by immersing an amorphous film in a developer at 23°C for a predetermined time and measuring the film thickness before and after immersion by a known method such as visual observation, an ellipsometer, or a QCM method.
[0044] In the case of a positive resist pattern, the dissolution rate in a developer at 23°C of the portion of the amorphous film formed by spin coating that has been exposed to radiation such as a KrF excimer laser, extreme ultraviolet light, electron beam, or X-ray is preferably 10 Å / sec or higher. A dissolution rate of 10 Å / sec or higher means that the film is easily soluble in a developer and is more suitable for use as a resist. Furthermore, a dissolution rate of 10 Å / sec or higher may improve resolution. This is presumably because the micro-surface portion of the resin dissolves, reducing line edge roughness. It also has the effect of reducing defects.
[0045] In the case of a negative resist pattern, the dissolution rate in a developer at 23°C of the portion of an amorphous film formed by spin coating that has been exposed to radiation such as a KrF excimer laser, extreme ultraviolet light, electron beam, or X-ray is preferably 5 Å / sec or less, more preferably 0.0005 to 5 Å / sec, and even more preferably 0.05 to 5 Å / sec. A dissolution rate of 5 Å / sec or less can result in a resist that is insoluble in a developer. Furthermore, a dissolution rate of 0.0005 Å / sec or more can improve resolution. This is presumably because the change in solubility of the resin before and after exposure increases the contrast at the interface between the unexposed portion that dissolves in a developer and the exposed portion that does not dissolve in a developer. Furthermore, this also has the effect of reducing line edge roughness and defects.
[0046] (Other Components) The solvent used in the lithography film-forming composition is not particularly limited, and those disclosed in WO 2020 / 226150 can be used. The solvent is preferably a safe solvent, more preferably at least one selected from PGMEA (propylene glycol monomethyl ether acetate), PGME (propylene glycol monomethyl ether), CHN (cyclohexanone), CPN (cyclopentanone), 2-heptanone, anisole, butyl acetate, ethyl propionate, and ethyl lactate, and even more preferably at least one selected from PGMEA, PGME, and CHN. A mixed solvent of these solvents may also be used.
[0047] In the composition, the relationship between the amount of solid component and the amount of solvent is not particularly limited, but may be as follows, with the total weight of solid component and solvent being 100% by weight: 1-80% by weight solid component: 20-99% by weight solvent 1-50% by weight solid component: 50-99% by weight solvent 2-40% by weight solid component: 60-98% by weight solvent 2-10% by weight solid component: 90-98% by weight solvent
[0048] The composition may contain, as other solid components, at least one selected from the group consisting of an acid generator (C), an acid crosslinker (G), an acid diffusion controller (E), and other components (F).
[0049] In the composition, the content of the hyperbranched resin is not particularly limited, but is preferably 50 to 99.4 wt %, more preferably 55 to 90 wt %, even more preferably 60 to 80 wt %, and particularly preferably 60 to 70 wt % of the total weight of solid components (the sum of optionally used solid components such as the resin, acid generator (C), crosslinking agent (G), acid diffusion controller (E), and other components (F); the same applies hereinafter). With this content, the resolution is further improved and line edge roughness (LER) is further reduced.
[0050] (Acid Generator (C)) The composition preferably contains one or more acid generators (C) that generate an acid directly or indirectly upon irradiation with any radiation selected from visible light, ultraviolet light, excimer laser, electron beam, extreme ultraviolet light (EUV), X-rays, and ion beams.
[0051] In this case, the content of the acid generator (C) in the composition is preferably 0.001 to 49 wt %, more preferably 1 to 40 wt %, still more preferably 3 to 30 wt %, and particularly preferably 10 to 25 wt %, of the total weight of the solid components. By using the acid generator (C) within this content range, a pattern profile with higher sensitivity and lower edge roughness can be obtained.
[0052] In the composition, the method for generating the acid is not limited as long as the acid is generated in the system. If an excimer laser is used instead of ultraviolet rays such as g-rays or i-rays, finer processing is possible, and if high-energy rays such as electron beams, extreme ultraviolet rays, X-rays, or ion beams are used, even finer processing is possible.
[0053] The acid generator (C) is not particularly limited, and examples thereof include the compounds disclosed in WO 2017 / 033943. As the acid generator (C), an acid generator having an aromatic ring is preferred, an acid generator having a sulfonate ion with an aryl group is more preferred, and diphenyltrimethylphenylsulfonium p-toluenesulfonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium trifluoromethanesulfonate, and triphenylsulfonium nonafluorobutanesulfonate are particularly preferred. By using such an acid generator, line edge roughness can be reduced.
[0054] It is preferable that the composition further contains a diazonaphthoquinone photoactive compound described in WO 2020 / 226150 as an acid generator. Among these, from the viewpoint of low roughness and solubility, a non-polymeric diazonaphthoquinone photoactive compound is preferred, more preferably a low-molecular-weight compound having a molecular weight of 1,500 or less, even more preferably a molecular weight of 1,200 or less, and particularly preferably a molecular weight of 1,000 or less. A preferred specific example of such a non-polymeric diazonaphthoquinone photoactive compound is the non-polymeric diazonaphthoquinone photoactive compound disclosed in WO 2016 / 158881. The acid generator (C) can be used alone or in combination with two or more different compounds.
[0055] (Crosslinking Agent (G)) When used as a negative resist material or as an additive to increase pattern strength in a positive resist material, it is preferable to contain one or more crosslinking agents (G). The crosslinking agent is preferably an acid crosslinking agent. The acid crosslinking agent (G) is a compound that can intramolecularly or intermolecularly crosslink the resin in the presence of an acid generated from the acid generator (C). Such an acid crosslinking agent (G) is not particularly limited, but examples thereof include compounds having one or more groups (hereinafter referred to as "crosslinkable groups") that can crosslink the resin.
[0056] Specific examples of such crosslinkable groups include, but are not limited to, those described in International Publication No. 2020 / 226150. As the crosslinkable group of the acid crosslinker (G), a hydroxyalkyl group, an alkoxyalkyl group, or the like is preferred, and an alkoxymethyl group is particularly preferred.
[0057] The acid crosslinking agent (G) having a crosslinkable group is not particularly limited, but examples thereof include those described in WO 2020 / 226150.
[0058] Further examples of the acid crosslinking agent (G) include compounds having a phenolic hydroxyl group as described in WO 2020 / 226150, and compounds and resins in which the crosslinkable group has been introduced into an acidic functional group in an alkali-soluble resin to impart crosslinkability.
[0059] In the composition, the acid crosslinker (G) is preferably an alkoxyalkylated urea compound or a resin thereof, or an alkoxyalkylated glycoluril compound or a resin thereof (acid crosslinker (G1)), a phenol derivative having 1 to 6 benzene rings in the molecule and having two or more hydroxyalkyl groups or alkoxyalkyl groups throughout the molecule, with the hydroxyalkyl groups or alkoxyalkyl groups bonded to any of the benzene rings (acid crosslinker (G2)), or a compound having at least one α-hydroxyisopropyl group (acid crosslinker (G3)). Examples include the compounds disclosed in WO 2017 / 033943.
[0060] In the composition, the content of the acid crosslinker (G) is preferably 0.5 to 49 wt % of the total weight of the solid components, more preferably 0.5 to 40 wt %, even more preferably 1 to 30 wt %, and particularly preferably 2 to 20 wt %. A content of the acid crosslinker (G) of 0.5 wt % or more is preferable because it improves the effect of suppressing the solubility of the resist film in an alkaline developer and can suppress a decrease in the residual film rate and the occurrence of swelling or meandering of the pattern, while a content of 49 wt % or less is preferable because it can suppress a decrease in the heat resistance of the resist.
[0061] Furthermore, the content of at least one compound selected from the acid crosslinkers (G1), (G2), and (G3) in the acid crosslinker (G) is not particularly limited, and can be set to various ranges depending on factors such as the type of substrate used when forming a resist pattern.
[0062] (Acid Diffusion Controller (E)) The composition may contain an acid diffusion controller (E) that has the effect of controlling the diffusion of the acid generated from the acid generator upon irradiation in the resist film, thereby preventing undesirable chemical reactions in unexposed areas. The use of such an acid diffusion controller (E) improves the storage stability of the composition. In addition, the resolution is further improved, and changes in the line width of the resist pattern due to variations in the exposure time before and after radiation exposure can be suppressed, resulting in extremely excellent process stability.
[0063] The acid diffusion controller (E) is not particularly limited, and examples thereof include radiolytic basic compounds such as nitrogen atom-containing basic compounds, basic sulfonium compounds, and basic iodonium compounds. Examples of the acid diffusion controller (E) include the compounds disclosed in WO 2017 / 033943. The acid diffusion controller (E) may be used alone or in combination of two or more.
[0064] The content of the acid diffusion controller (E) is preferably 0.001 to 49 wt %, more preferably 0.01 to 10 wt %, even more preferably 0.01 to 5 wt %, and particularly preferably 0.01 to 3 wt %, based on the total weight of the solid components. When the content of the acid diffusion controller (E) is within the above range, degradation of resolution, pattern shape, dimensional fidelity, and the like can be further suppressed. Furthermore, even if the exposure time between electron beam irradiation and post-exposure heating is long, the shape of the upper layer of the pattern does not deteriorate. Furthermore, when the content of the acid diffusion controller (E) is 10 wt % or less, degradation of sensitivity, developability of unexposed areas, and the like can be prevented. Furthermore, the use of such an acid diffusion controller improves the storage stability and resolution of the composition, and also suppresses changes in the line width of the resist pattern due to variations in the exposure time before and after radiation exposure, resulting in extremely excellent process stability.
[0065] (Other Components (F)) If necessary, one or more of various additives such as a dissolution promoter, a dissolution controller, a sensitizer, a surfactant, and an organic carboxylic acid, a phosphorus oxoacid, or a derivative thereof may be added to the composition as other components (F) within a range that does not impair the object of this embodiment. Examples of other components (F) include the compounds disclosed in WO 2017 / 033943.
[0066] The total content of the other components (F) is preferably 0 to 49% by weight, more preferably 0 to 5% by weight, even more preferably 0 to 1% by weight, and particularly preferably 0% by weight, based on the total weight of the solid components.
[0067] In the composition, the content of the resin, acid generator (C), acid diffusion controller (E), and other component (F) (resin / acid generator (C) / acid diffusion controller (E) / other component (F)) is preferably 50 to 99.4 / 0.001 to 49 / 0.001 to 49 / 0 to 49, more preferably 55 to 90 / 1 to 40 / 0.01 to 10 / 0 to 5, even more preferably 60 to 80 / 3 to 30 / 0.01 to 5 / 0 to 1, and particularly preferably 60 to 70 / 10 to 25 / 0.01 to 3 / 0, in weight percent on a solids basis. The content ratio of each component is selected from each range so that the total sum adds up to 100% by weight. The above content ratios provide even better performance, such as sensitivity, resolution, and developability.
[0068] The method for preparing the composition is not particularly limited, and examples thereof include a method in which, at the time of use, each component is dissolved in a solvent to form a homogeneous solution, and then, if necessary, filtered through a filter having a pore size of about 0.2 μm.
[0069] The composition may contain other resins to the extent that the effect is not impaired. Examples of such other resins include, but are not limited to, novolac resins, polyvinylphenols, polyacrylic acid, polyvinyl alcohol, styrene-maleic anhydride resins, and polymers containing acrylic acid, vinyl alcohol, or vinylphenol as monomer units, or derivatives thereof. The content of such other resins is not particularly limited and is adjusted appropriately depending on the type. The content of such other resins is preferably 30 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and particularly preferably 0 parts by weight, per 100 parts by weight of the hyperbranched resin.
[0070] [Pattern Forming Method] The pattern forming method may include a method comprising a film forming step of applying the lithography film forming composition onto a substrate to form a film (resist film), an exposure step of exposing the formed film (resist film), and a development step of developing the film (resist film) exposed in the exposure step to form a pattern (resist pattern). The resist pattern can also be used as an upper layer resist in a multilayer process.
[0071] (Film Formation Process) For example, this process can be carried out as follows. First, a resist film is formed by applying the resist composition to a conventionally known substrate by a coating method such as spin coating, casting coating, or roll coating. The conventionally known substrate is not particularly limited, and examples thereof include substrates for electronic components and those having a predetermined wiring pattern formed thereon. More specifically, although not particularly limited, examples include silicon wafers, metal substrates such as copper, chromium, iron, and aluminum, and glass substrates. Materials for the wiring pattern are not particularly limited, and examples include copper, aluminum, nickel, and gold. If necessary, an inorganic or organic film may be provided on the substrate. Examples of inorganic films include, but are not limited to, inorganic anti-reflective coatings (inorganic BARCs). Examples of organic films include, but are not limited to, organic anti-reflective coatings (organic BARCs). Surface treatment with hexamethylenedisilazane or the like may be performed. Next, if necessary, the coated substrate is heated. The heating conditions vary depending on the composition of the composition, etc., but are preferably 20 to 250° C., more preferably 20 to 150° C. Heating is preferred because it can improve the adhesion of the resist to the substrate.
[0072] (Exposure Step) For example, this step can be carried out as follows. The resist film is exposed to any radiation selected from the group consisting of visible light, ultraviolet light, excimer laser, electron beam, extreme ultraviolet (EUV), X-ray, and ion beam in a desired pattern. The exposure conditions are appropriately selected depending on the composition of the composition. In the method for forming a resist pattern, heating is preferably performed after irradiation with radiation in order to stably form a highly accurate fine pattern during exposure. The heating conditions vary depending on the composition of the composition, but are preferably 20 to 250°C, more preferably 20 to 150°C.
[0073] (Development step) For example, this step can be carried out as follows. The exposed resist film is developed with a developer to form a predetermined resist pattern. As the developer, it is preferable to select a solvent having a solubility parameter (SP value) close to that of the resin. Suitable solvents include those disclosed in WO 2020 / 226150.
[0074] An appropriate amount of surfactant can be added to the developer as needed. The surfactant is not particularly limited, but for example, an ionic or nonionic fluorine-based or silicon-based surfactant can be used. Examples of these surfactants include those disclosed in International Publication No. 2020 / 226150. It is more preferable to use a fluorine-based surfactant or a silicon-based surfactant as the nonionic surfactant.
[0075] The amount of the surfactant used is usually 0.001 to 5% by weight, preferably 0.005 to 2% by weight, and more preferably 0.01 to 0.5% by weight, based on the total amount of the developer.
[0076] Examples of development methods that can be applied include a method in which a substrate is immersed in a tank filled with a developer for a certain period of time (dip method), a method in which a developer is piled up on the surface of the substrate by surface tension and left standing for a certain period of time (puddle method), a method in which a developer is sprayed onto the surface of the substrate (spray method), and a method in which a developer is continuously dispensed onto a substrate rotating at a constant speed while a developer dispensing nozzle is scanned at a constant speed (dynamic dispense method). There are no particular restrictions on the time for developing the pattern, but it is preferably 10 to 90 seconds. Furthermore, after the development step, a step of stopping development by replacing the solvent with another solvent may be carried out.
[0077] (Other steps) After development, it is preferable to include a step of washing with a rinse solution containing an organic solvent. Examples of rinse solutions and rinse methods used in the rinse step after development include those disclosed in WO 2020 / 226150.
[0078] After forming the resist pattern, a patterned wiring substrate can be obtained by etching, which can be performed by known methods such as dry etching using plasma gas and wet etching using an alkaline solution, cupric chloride solution, ferric chloride solution, etc.
[0079] After forming the resist pattern, plating may be carried out. The plating method is not particularly limited, but examples thereof include copper plating, solder plating, nickel plating, and gold plating.
[0080] The remaining resist pattern after etching can be stripped using an organic solvent. Examples of the organic solvent and stripping method include those disclosed in WO 2020 / 226150.
[0081] The wiring board can also be formed by a method in which a resist pattern is formed, a metal is evaporated in a vacuum, and then the resist pattern is dissolved in a solution, that is, by a lift-off method.
[0082] [Lithography Underlayer Film-Forming Composition, Lithography Underlayer Film, and Pattern Forming Method] (First Embodiment) <Lithography Underlayer Film-Forming Composition> The lithography underlayer film-forming composition according to this embodiment (hereinafter also referred to as "underlayer film-forming composition") contains the multi-branched resin and a silicon-containing compound (e.g., a hydrolyzable organosilane, its hydrolysate, or its hydrolyzed condensate). The underlayer film-forming composition has a relatively high carbon concentration, a relatively low oxygen concentration, high heat resistance, and high solvent solubility. Therefore, the pattern has excellent rectangularity. Furthermore, it is possible to reduce film defects (thin film formation), has good storage stability, high sensitivity, a high refractive index and transparency in a specific wavelength range, and can impart a good resist pattern shape.
[0083] The underlayer film-forming composition can be suitably used, for example, in a multilayer resist method in which a resist underlayer film is further provided between an upper-layer resist (e.g., photoresist) and a hard mask or organic underlayer film. In such a multilayer resist method, for example, a resist underlayer film is formed on an organic underlayer film or hard mask on a substrate by a coating method or the like, and an upper-layer resist (e.g., photoresist, electron beam resist, EUV resist) is formed on the resist underlayer film. A resist pattern is then formed by exposure and development, and the resist underlayer film is dry-etched using the resist pattern to transfer the pattern. The organic underlayer film is then etched to transfer the pattern, and the substrate is processed using the organic underlayer film.
[0084] That is, a lithography underlayer film (resist underlayer film) formed using the underlayer film-forming composition is less likely to intermix with an upper-layer resist and has heat resistance. For example, the etching rate of the underlayer film with a halogen-based (fluorine-based) etching gas is higher than that of the patterned upper-layer resist used as a mask, thereby enabling the formation of a good rectangular pattern. Furthermore, the resist underlayer film has high resistance to oxygen-based etching gases, and therefore can function as a good mask when patterning a layer provided on a substrate, such as a hard mask. The underlayer film-forming composition can also be used in an embodiment in which multiple resist underlayer films are stacked. In this case, the position of the resist underlayer film (the layer number on which it is stacked) is not particularly limited. It may be directly below the upper-layer resist, the layer closest to the substrate, or sandwiched between resist underlayer films. In the present disclosure, the terms lithography underlayer film and resist underlayer film are used interchangeably.
[0085] When forming fine patterns, the resist film thickness tends to be thin to prevent pattern collapse. Due to the thinning of the resist, dry etching for transferring a pattern to a film existing below it requires a higher etching rate than the film above it, making pattern transfer impossible. In this embodiment, an organic underlayer film is placed on a substrate, which is then coated with the resist underlayer film (containing a silicon-based compound) of this embodiment, and this is then coated with a resist film (organic resist film). The dry etching rates of organic and inorganic component films vary significantly depending on the etching gas selected; organic component films are dry-etched at a higher rate with oxygen-based gases, while inorganic component films are dry-etched at a higher rate with halogen-containing gases. For example, a pattern-transferred resist underlayer film can be used to dry-etch the underlying organic underlayer film with oxygen-based gases to transfer the pattern to the organic underlayer film, and then the pattern-transferred organic underlayer film can be used to process the substrate using a halogen-containing gas.
[0086] Furthermore, when the resist underlayer film contains the hyperbranched resin and a silicon-containing compound (e.g., a hydrolyzable organosilane, its hydrolysate, or its hydrolyzed condensate), the sensitivity of the upper resist layer is improved, intermixing with the upper resist layer is prevented, and the resist underlayer film formed after exposure and development has a rectangular pattern, thereby enabling substrate processing with fine patterns.
[0087] In particular, it is preferable that the resist underlayer film is composed of a multi-branched heterocyclic resin (for example, a multi-branched PBO resin), since this has extremely high heat resistance and is extremely unlikely to cause intermixing with the upper resist layer.
[0088] Furthermore, the resist underlayer film has high heat resistance and can be used even under high-temperature baking conditions. Furthermore, because of its relatively low molecular weight and low viscosity, it can be easily and uniformly filled into every corner of a substrate having steps (especially fine spaces or hole patterns, etc.), and as a result, the planarization and filling properties tend to be relatively advantageously improved.
[0089] In addition to the hyperbranched resin and the silicon-containing compound, the underlayer film-forming composition may further contain a solvent, an acid, an acid crosslinker, etc. Optional components may also include an organic polymer compound, an acid generator, a surfactant, and other components such as water, an alcohol, and a curing catalyst. From the viewpoints of coatability and quality stability, the content of the hyperbranched resin in the lithography underlayer film is preferably 0.1 to 70 wt %, more preferably 0.5 to 50 wt %, and particularly preferably 3.0 to 40 wt %.
[0090] As the solvent, any known solvent can be used as long as it dissolves the multi-branched resin. The type and amount of the solvent can be as disclosed in WO 2020 / 226150.
[0091] The underlayer film-forming composition may contain an acid from the viewpoint of promoting curing. The type and amount of the acid may be as disclosed in WO 2020 / 226150.
[0092] The underlayer film-forming composition can contain one or more acid crosslinkers when used as a negative resist material or as an additive to increase the pattern strength of a positive resist material. The acid crosslinker is a compound that can intramolecularly or intermolecularly crosslink the resin in the presence of the acid. The type and amount of the acid crosslinker can be as disclosed in WO 2020 / 226150.
[0093] The underlayer film-forming composition comprises a silicon-containing compound.The silicon-containing compound may be either an organic silicon-containing compound or an inorganic silicon-containing compound, but is preferably an organic silicon-containing compound.The type and amount of the silicon-containing compound can be as disclosed in WO 2020 / 226150.
[0094] In addition to the above components, the underlayer film-forming composition may optionally contain an organic polymer compound, a crosslinking agent, a photoacid generator, a surfactant, etc. The types and amounts of these components may be as disclosed in WO 2020 / 226150.
[0095] <Lithography Underlayer Film and Pattern Forming Method> The lithography underlayer film of this embodiment can be suitably used as an underlayer (resist underlayer film) of a photoresist (upper layer) used in a multilayer resist method.
[0096] In the present embodiment, for example, a resist underlayer film is formed using the underlayer film-forming composition, at least one photoresist layer is formed on the resist underlayer film, and then a predetermined region of the photoresist layer is irradiated with radiation and developed to form a pattern. The resist underlayer film is preferably formed by forming an underlayer film precursor from a multi-branched PA resin, heating the precursor at 300°C or higher, and converting the multi-branched PA resin into a multi-branched PBO resin.
[0097] Furthermore, one aspect of the pattern formation method according to the first embodiment can include a method comprising the following steps: forming an organic underlayer film on a substrate using a coating-type organic underlayer film material; forming a resist underlayer film on the organic underlayer film using the underlayer film-forming composition of the first embodiment; forming an upper-layer resist film on the resist underlayer film using an upper-layer resist film composition; forming an upper-layer resist pattern on the upper-layer resist film and transferring the pattern to the resist underlayer film by etching using the upper-layer resist pattern as a mask; transferring the pattern to the organic underlayer film by etching using the resist underlayer film to which the pattern has been transferred as a mask; and transferring the pattern to the substrate (workpiece) by etching using the organic underlayer film to which the pattern has been transferred as a mask.
[0098] Another aspect can include a method comprising the following steps: forming an organic hard mask containing carbon as a main component on a substrate by a CVD method; forming a resist underlayer film on the organic hard mask using the underlayer film-forming composition of the first embodiment; forming an upper-layer resist film on the resist underlayer film using an upper-layer resist film composition; forming an upper-layer resist pattern on the upper-layer resist film and transferring the pattern to the resist underlayer film by etching using the upper-layer resist pattern as a mask; transferring the pattern to the organic hard mask by etching using the resist underlayer film to which the pattern has been transferred as a mask; and transferring the pattern to the base material (workpiece) by etching using the organic hard mask to which the pattern has been transferred as a mask.
[0099] The substrate may be, for example, a semiconductor substrate. As the semiconductor substrate, a silicon substrate can generally be used, but is not particularly limited thereto, and may be Si, amorphous silicon (α-Si), p-Si, SiO 2 , SiN, SiON, W, TiN, Al, etc., which are different from the material of the workpiece layer, can be used. In addition, as the metal constituting the base material (workpiece; including the semiconductor substrate), those disclosed in International Publication No. 2020 / 226150 can be used.
[0100] In the pattern formation method of this embodiment, an organic underlayer film or an organic hard mask can be formed on a substrate. The organic underlayer film can be formed from a coating-type organic underlayer film material using a spin coating method, etc., while the organic hard mask can be formed from a carbon-based organic hard mask material using a CVD method. While the types of such organic underlayer film and organic hard mask are not particularly limited, when the top resist film is patterned by exposure, it is preferable for them to exhibit sufficient anti-reflective coating function. By forming such an organic underlayer film or organic hard mask, the pattern formed in the top resist film can be transferred to the substrate (workpiece) without causing size conversion differences. A "carbon-based" hard mask refers to a hard mask in which 50% or more by weight of the solid content is composed of a carbon-based material, such as amorphous hydrogenated carbon, also known as amorphous carbon and denoted as a-C:H. While a-C:H films can be deposited by various techniques, plasma-enhanced chemical vapor deposition (PECVD) is widely used due to its cost-effectiveness and film quality control capabilities. As an example of the hard mask, for example, reference can be made to the one described in JP-A-2013-526783.
[0101] The resist underlayer film used in the pattern formation method of this embodiment can be formed by spin coating or the like on a workpiece provided with an organic underlayer film or the like. When forming the resist underlayer film by spin coating, it is desirable to evaporate the solvent after spin coating and bake the resulting film to promote a crosslinking reaction and prevent mixing with the upper resist film. The bake temperature is preferably within a range of 50 to 500°C. In this case, although it depends on the structure of the device to be manufactured, a bake temperature of 400°C or less is particularly preferred to minimize thermal damage to the device. A bake time within a range of 10 to 300 seconds is preferably used.
[0102] In the pattern formation method of this embodiment, the method of forming a pattern on the upper resist film can be suitably selected from the following: lithography using light having a wavelength of 300 nm or less or EUV light, electron beam direct writing, and directed self-assembly. By using such a method, a fine pattern can be formed on the upper resist film.
[0103] The upper layer resist film composition can be appropriately selected depending on the method for forming a pattern on the above-mentioned upper layer resist film.For example, when performing lithography using light of 300 nm or less or EUV light, a chemically amplified photoresist film material can be used as the upper layer resist film composition.Examples of such photoresist film materials include those that form a positive pattern by forming a photoresist film and exposing it, and then dissolving the exposed portion using an alkaline developer, and those that form a negative pattern by dissolving the unexposed portion using a developer made of an organic solvent.
[0104] The resist underlayer film formed in this embodiment may absorb light depending on the wavelength of the light used in the lithography process, and in such cases, it can function as an anti-reflection film that has the effect of preventing light from being reflected from the substrate.
[0105] Furthermore, the resist underlayer film formed in this embodiment can be used as an EUV resist underlayer film, not only functioning as a hard mask but also as an EUV resist underlayer antireflection film. Furthermore, a film formed from the underlayer film-forming composition has excellent EUV absorption ability, and is therefore capable of exerting a sensitizing effect on the upper layer resist composition, contributing to improved sensitivity. When the resist underlayer film formed in this embodiment is used as an EUV resist underlayer film, the process can be carried out in the same manner as for a photoresist underlayer film.
[0106] Second Embodiment <Resist Underlayer Film-Forming Composition> A resist underlayer film-forming composition according to a second embodiment (hereinafter also referred to as an "underlayer film-forming composition") contains the multi-branched resin, but may not contain a silicon-containing compound.
[0107] The underlayer film-forming composition of this embodiment is applicable to a wet process and is useful for forming a photoresist underlayer film that has excellent heat resistance, step-filling properties, and flatness. Furthermore, since this underlayer film-forming composition uses a compound having a specific structure with a relatively high carbon concentration, a relatively low oxygen concentration, and high solvent solubility, film deterioration during baking is suppressed, and an underlayer film that has excellent etching resistance to fluorine gas-based plasma etching and the like can be formed. Furthermore, since the underlayer film-forming composition of this embodiment has excellent adhesion to the resist layer, an excellent resist pattern can be formed. Because the underlayer film-forming composition of this embodiment has particularly excellent heat resistance, step-filling properties, and flatness, it can be used, for example, to form a resist underlayer film that is provided as the bottom layer of multiple resist layers. However, the resist underlayer film formed in this embodiment may further include another resist underlayer between the substrate and the underlayer film.
[0108] The underlayer film-forming composition according to this embodiment may further contain a solvent, an acid generator, an acid crosslinker, etc. Optional components may also include a basic compound, water, an alcohol, a curing catalyst, etc. From the viewpoints of coatability and quality stability, the content of the resin in the underlayer film-forming composition is preferably 0.1 to 70 wt %, more preferably 0.5 to 50 wt %, and particularly preferably 3.0 to 40 wt %.
[0109] As the solvent used in this embodiment, any known solvent can be used as long as it can at least dissolve the resin. The type and amount of the solvent can be as disclosed in WO 2020 / 226150.
[0110] The underlayer film-forming composition of this embodiment may contain an acid crosslinker as needed from the viewpoint of suppressing intermixing, etc. The type and amount of the acid crosslinker may be as disclosed in WO 2020 / 226150.
[0111] The underlayer film-forming composition of this embodiment may contain an acid generator as needed, from the viewpoint of further promoting the thermal crosslinking reaction, etc. The type and amount of the acid generator may be as disclosed in WO 2020 / 226150.
[0112] Furthermore, the underlayer film-forming composition of this embodiment may contain a basic compound from the viewpoint of improving storage stability, etc. The type and amount of the basic compound may be as disclosed in WO 2020 / 226150.
[0113] The underlayer film-forming composition of the present embodiment may contain other resins or compounds for the purpose of imparting thermosetting properties or controlling absorbance. Examples of such other resins or compounds include those disclosed in WO 2020 / 226150.
[0114] <Resist Underlayer Film for Lithography and Pattern Forming Method> The pattern formed in this embodiment can be used as, for example, a resist pattern or a circuit pattern. The method for producing the resist underlayer film in this embodiment is the same as that described in the first embodiment.
[0115] Furthermore, the pattern formation method according to the second embodiment includes the steps of forming a resist underlayer film on a substrate using the underlayer film-forming composition of the second embodiment (step A-1), forming at least one photoresist layer on the resist underlayer film (step A-2), and, after the at least one photoresist layer has been formed in step A-2, irradiating a predetermined region of the photoresist layer with radiation and developing it (step A-3). The photoresist layer refers to the outermost layer of the resist layer, i.e., the layer provided on the front side (the side opposite to the substrate) of the resist layer.
[0116] Furthermore, another pattern formation method of the second embodiment includes the steps of: forming a resist underlayer film on a substrate using the underlayer film-forming composition of the second embodiment (step B-1); forming a resist intermediate layer film on the underlayer film using a resist intermediate layer film material (for example, a silicon-containing resist layer) (step B-2); forming at least one photoresist layer on the resist intermediate layer film (step B-3); after forming at least one photoresist layer in step B-3, irradiating predetermined regions of the photoresist layer with radiation and developing the photoresist layer to form a resist pattern (step B-4); and after forming the resist pattern in step B-4, etching the resist intermediate layer film using the resist pattern as a mask, etching the underlayer film using the obtained intermediate layer film pattern as an etching mask, and etching the substrate using the obtained underlayer film pattern as an etching mask, thereby forming a pattern on the substrate (step B-5).
[0117] When forming the resist underlayer film, it is preferable to perform a baking treatment to suppress the occurrence of mixing with the upper resist (e.g., a photoresist layer or a resist intermediate layer film) and to promote the crosslinking reaction. The conditions can be as disclosed in WO 2020 / 226150.
[0118] After forming a resist underlayer film on the substrate, a resist intermediate layer film can be provided between the photoresist layer and the resist underlayer film. For example, in the case of a two-layer process, a silicon-containing resist layer or a monolayer resist made of a normal hydrocarbon can be provided on the resist underlayer film as a resist intermediate layer film. Furthermore, for example, in the case of a three-layer process, it is preferable to form a silicon-containing intermediate layer between the resist intermediate layer film and the photoresist layer, and further a silicon-free monolayer resist layer on top of that. Known photoresist materials can be used to form these photoresist layers, resist intermediate layer films, and resist layers provided between these layers. As silicon-containing resist materials, those disclosed in WO 2020 / 226150 can be used. In addition, a resist intermediate layer formed by a chemical vapor deposition (CVD) method can also be used.
[0119] Furthermore, the resist underlayer film of this embodiment can also be used as an anti-reflective film for a normal single-layer resist or as an underlayer material for suppressing pattern collapse. Because the resist underlayer film of this embodiment has excellent etching resistance for underlayer processing, it can also be expected to function as a hard mask for underlayer processing.
[0120] When forming a resist layer using the above-mentioned known photoresist materials, wet processes such as spin coating and screen printing are preferably used, as in the case of forming the resist underlayer film. After applying the resist material by spin coating or the like, pre-baking is typically performed, preferably at a baking temperature of 80 to 180°C and for a baking time of 10 to 300 seconds. Subsequently, exposure, post-exposure baking (PEB), and development are performed according to conventional methods to obtain a resist pattern. The thickness of each resist film is not particularly limited, but is generally preferably 30 to 500 nm, more preferably 50 to 400 nm.
[0121] The exposure light may be appropriately selected depending on the photoresist material used, and generally includes high-energy rays with a wavelength of 300 nm or less, specifically excimer lasers with wavelengths of 248 nm, 193 nm, and 157 nm, soft X-rays with wavelengths of 3 to 20 nm, electron beams, X-rays, and the like.
[0122] The resist pattern formed by the above-described method is prevented from collapsing due to the resist underlayer film of this embodiment. Therefore, by using the resist underlayer film of this embodiment, a finer pattern can be obtained, and the exposure dose required to obtain the resist pattern can be reduced.
[0123] Next, etching is performed using the obtained resist pattern as a mask. Gas etching is preferably used for etching the resist underlayer film in the two-layer process. As the gas etching, etching using oxygen gas is suitable. In addition to oxygen gas, inert gases such as He and Ar, CO, CO 2 , N.H. 3 , S.O. 2 , N 2 , NO 2 , H 2 It is also possible to add gases such as CO, CO2, etc. without using oxygen gas. 2 , N.H. 3 , S.O. 2 , N 2 , NO 2 , H 2 Gas etching can also be performed using only the gas, and the latter gas is particularly preferably used to protect the sidewalls of the pattern to prevent undercutting of the sidewalls.
[0124] On the other hand, gas etching is also preferably used for etching the intermediate layer (the layer located between the photoresist layer and the resist underlayer film) in the three-layer process. The same gas etching as that described in the two-layer process can be applied. In particular, processing of the intermediate layer in the three-layer process is preferably performed using a fluorocarbon-based gas with the resist pattern as a mask. Then, as described above, the resist underlayer film can be processed by, for example, performing oxygen gas etching with the intermediate layer pattern as a mask.
[0125] Here, when an inorganic hard mask intermediate layer film is formed as the intermediate layer, a silicon oxide film, a silicon nitride film, or a silicon oxynitride film (SiON film) is formed by a CVD method, an ALD method, or the like. The nitride film formation method is not limited to the following, but for example, the methods described in Japanese Patent Laid-Open No. 2002-334869 and International Publication No. 2004 / 066377 can be used. A photoresist film can be formed directly on such an intermediate layer film, or an organic antireflective coating (BARC) can be formed on the intermediate layer film by spin coating, and then a photoresist film can be formed on top of that.
[0126] A polysilsesquioxane-based intermediate layer is also preferably used as the intermediate layer. By providing the resist intermediate film with the effect of an anti-reflection film, reflection tends to be effectively suppressed. Specific materials for the polysilsesquioxane-based intermediate layer are not limited to the following, but for example, those described in JP-A-2007-226170 and JP-A-2007-226204 can be used.
[0127] The substrate can also be etched by a conventional method. For example, if the substrate is SiO 2For SiN, etching can be performed using primarily fluorocarbon-based gases, while for p-Si, Al, and W, etching can be performed using primarily chlorine- or bromine-based gases. When etching a substrate with fluorocarbon-based gases, the silicon-containing resist of a two-layer resist process and the silicon-containing intermediate layer of a three-layer process are stripped simultaneously with substrate processing. On the other hand, when etching a substrate with chlorine- or bromine-based gases, the silicon-containing resist layer or silicon-containing intermediate layer is stripped separately, and generally, dry etching stripping using fluorocarbon-based gases is performed after substrate processing.
[0128] The resist underlayer film of this embodiment has excellent etching resistance for these substrates. The substrate can be appropriately selected from known substrates, and is not particularly limited, but includes Si, α-Si, p-Si, SiO 2 , SiN, SiON, W, TiN, Al, etc. The substrate may also be a laminate having a film to be processed (substrate to be processed) on a base material (support). Examples of such a film to be processed include Si, SiO 2 Examples of low-k films include various low-k films and stopper films thereof, such as SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, and Al-Si, and these films are usually made of a material different from that of the substrate (support). The thickness of the substrate or film to be processed is not particularly limited, but is usually preferably about 50 nm to 10,000 nm, and more preferably 75 nm to 5,000 nm.
[0129] The resist underlayer film of this embodiment has excellent embedding and flatness in a substrate having steps. A known method for evaluating the embedding and flatness can be appropriately selected and used, and is not particularly limited. For example, a solution of each compound adjusted to a predetermined concentration is applied by spin coating onto a silicon substrate having steps, followed by drying to remove the solvent at 110°C for 90 seconds to form an underlayer film having a predetermined thickness, and then the underlayer film is baked for a predetermined time at a temperature of about 240 to 300°C. The difference in the underlayer film thickness (ΔT) between the line and space region and the pattern-free open region is measured using an ellipsometer, whereby the embedding and flatness in a substrate having steps can be evaluated.
[0130] [Optical Article-Forming Composition and Cured Product Thereof] The hyperbranched resin is useful for optical materials. An optical component-forming composition containing the resin can provide optical components with a high refractive index, and is expected to have excellent storage stability, structure-forming ability (film-forming ability), and heat resistance. From the viewpoint of miniaturizing optical components and improving light collection efficiency, the refractive index of the optical article is preferably 1.60 or more, more preferably 1.65 or more, even more preferably 1.70 or more, and even more preferably 1.75 or more. From the viewpoint of improving light collection efficiency, the transparency of the optical article is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. The method for measuring the refractive index is not particularly limited, and known methods can be used. Examples include spectroscopic ellipsometry, minimum deviation method, critical angle method (Abbe method, Pulfrich method), V-block method, prism coupler method, and immersion method (Becke line method). The method for measuring transparency is not particularly limited, and known methods can be used. Examples include spectrophotometers and spectroscopic ellipsometry.
[0131] Furthermore, the cured product obtained by curing the optical component-forming composition can be a three-dimensional crosslinked product, and coloring can be suppressed by heat treatment over a wide range from low to high temperatures, and it can be expected to have a high refractive index and high transparency.
[0132] The optical part-forming composition of the present embodiment may further contain a solvent in addition to the resin. The solvent may be the same as the solvent used in the above-mentioned lithography film-forming composition.
[0133] In the optical component-forming composition of this embodiment, the relationship between the amount of solid components and the amount of solvent is not particularly limited, but is preferably 1 to 80 wt % solid components and 20 to 99 wt % solvent, more preferably 1 to 50 wt % solid components and 50 to 99 wt % solvent, even more preferably 2 to 40 wt % solid components and 60 to 98 wt % solvent, and particularly preferably 2 to 10 wt % solid components and 90 to 98 wt % solvent, relative to 100 wt % total of solid components and solvent. The optical component-forming composition of this embodiment may not contain a solvent.
[0134] The optical component-forming composition of the present embodiment may contain, as other solid components, at least one selected from the group consisting of an acid generator (C), an acid crosslinking agent (G), an acid diffusion controller (E), and other components (F).
[0135] In the optical component-forming composition of the present embodiment, the content of the hyperbranched resin is not particularly limited, but is preferably 50 to 99.4 wt % of the total weight of the solid components, more preferably 55 to 90 wt %, even more preferably 60 to 80 wt %, and particularly preferably 60 to 70 wt %.
[0136] The acid generator (C), acid crosslinker (G), acid diffusion controller (E), and other components (F) contained in the optical component-forming composition of this embodiment may be the same as those that may be contained in the above-mentioned lithography film-forming composition.
[0137] In the optical component-forming composition of this embodiment, the content ratio of the resin, acid generator (C), acid diffusion controller (E), and other component (F) (resin / acid generator (C) / acid diffusion controller (E) / other component (F)) is, in weight percent (wt. %) on a solids basis, preferably 50 to 99.4 / 0.001 to 49 / 0.001 to 49 / 0 to 49, more preferably 55 to 90 / 1 to 40 / 0.01 to 10 / 0 to 5, even more preferably 60 to 80 / 3 to 30 / 0.01 to 5 / 0 to 1, and particularly preferably 60 to 70 / 10 to 25 / 0.01 to 3 / 0. The content ratios of the respective components are selected from respective ranges so that the total sum adds up to 100 wt. The above content ratios provide even better performance, such as sensitivity, resolution, and developability.
[0138] The method for preparing the optical part-forming composition of the present embodiment is not particularly limited, and examples thereof include a method in which, at the time of use, each component is dissolved in a solvent to form a homogeneous solution, and then, if necessary, the solution is filtered through a filter with a pore size of about 0.2 μm, for example.
[0139] The optical component-forming composition of this embodiment may contain other resins to the extent that the intended purpose is not impaired. The types and amounts of the other resins may be as disclosed in WO 2020 / 226150.
[0140] Furthermore, the cured product of this embodiment can be obtained by curing the optical component-forming composition and can be used as various resins. These cured products can be used in a variety of applications as highly versatile materials that impart various properties such as a high melting point, a high refractive index, and high transparency. The cured product can be obtained by subjecting the composition to known methods corresponding to each composition, such as light irradiation or heating.
[0141] These cured products can be used as various synthetic resins such as epoxy resins, polycarbonate resins, and acrylic resins, and further, by taking advantage of their functionality, can be used as optical components such as lenses and optical sheets.
[0142] 6. Purification Method The hyperbranched resin is preferably purified. The purification method is not particularly limited, but the methods described in International Publication No. 2015 / 080240 and International Publication No. 2018 / 159707 can be used. Specifically, the purification method includes dissolving the resin in an organic solvent that is immiscible with water to obtain an organic phase, contacting the organic phase with an acidic aqueous solution to perform an extraction process, thereby transferring metals contained in the organic phase containing the resin and the organic solvent to the aqueous phase, and then separating the organic phase from the aqueous phase. The organic solvent that is immiscible with water is typically an organic solvent classified as a water-insoluble solvent. The organic solvent is not particularly limited, but is preferably an organic solvent that can be safely used in semiconductor manufacturing processes. The amount of organic solvent used is typically about 1 to 100 times the weight of the compound used.
[0143] Specific examples of the organic solvent to be used include those described in WO 2015 / 080240. Among these, toluene, 2-heptanone, cyclohexanone, cyclopentanone, methyl isobutyl ketone, propylene glycol monomethyl ether acetate, ethyl acetate, etc. are preferred, with cyclohexanone and propylene glycol monomethyl ether acetate being particularly preferred.
[0144] The acidic aqueous solution can be appropriately selected from aqueous solutions prepared by dissolving commonly known organic or inorganic compounds in water. Examples include those described in International Publication No. 2015 / 080240. These acidic aqueous solutions can be used alone or in combination of two or more. Examples of acidic aqueous solutions include mineral acid aqueous solutions and organic acid aqueous solutions. Examples of mineral acid aqueous solutions include aqueous solutions containing one or more acids selected from the group consisting of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid. Examples of organic acid aqueous solutions include aqueous solutions containing one or more acids selected from the group consisting of acetic acid, propionic acid, oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, tartaric acid, citric acid, methanesulfonic acid, phenolsulfonic acid, p-toluenesulfonic acid, and trifluoroacetic acid. The pH range of the acidic aqueous solution is approximately 0 to 5, and more preferably approximately 0 to 3.
[0145] Example 1 Hyperbranched Resin 1 Having Polyamide Structure (1) Synthesis of Tricarboxylic Acid Compound Intermediate The reaction shown in the following scheme was carried out.
[0146]
[0147] The following was placed in a 100 mL recovery flask: 4,4',4"-trihydroxytriphenylmethane (MTP) 10.0 mmol, 2.92 g K 2 CO 3 The contents were stirred for 60 minutes at 80° C. Then, 35 mmol and 3.87 mL of ethyl bromoacetate (EBA) were added to the flask, and the mixture was further stirred at 80° C. for 24 hours to carry out the reaction.
[0148] The reaction mixture was poured into a 0.01N aqueous solution of hydrochloric acid to cause reprecipitation. The precipitate was collected and subjected to extraction with chloroform. This extraction was performed twice in total. Next, a saturated sodium bicarbonate solution was added to the organic phase for separation and washing. Furthermore, a saturated saline solution was added to the organic phase for separation and washing.
[0149] Anhydrous magnesium sulfate was added to the organic phase obtained after the washing step and dried. The dried organic phase was concentrated using an evaporator to obtain a dark yellow liquid. The dark yellow liquid was subjected to column separation using ethyl acetate / hexane = 1:1 as the mobile phase to separate the residue. The liquid obtained by this column separation was further concentrated using an evaporator to obtain a light yellow viscous liquid. Analysis of the light yellow viscous liquid confirmed that the desired intermediate was produced (Figures 1A and 1B). The yield was 99%.
[0150] (2) Synthesis of tricarboxylic acid compounds The following reaction was carried out.
[0151]
[0152] The following was placed in a 300 mL flask: 10 mmol of the intermediate obtained in the previous step, 5.5 g, 90 mmol of KOH, 5.05 g, and 150 mL of a mixed solvent of tetrahydrofuran (THF):water=1:1. The contents were stirred at 50° C. for 72 hours, and the aqueous phase was recovered.
[0153] The aqueous phase was made weakly acidic and subjected to extraction with ethyl acetate. The ethyl acetate phase was washed with saturated saline and anhydrous magnesium sulfate. The washed ethyl acetate phase was concentrated using an evaporator and washed with hexane. The ethyl acetate phase was filtered using a Kiriyama funnel and dried under reduced pressure at room temperature. In this way, the target tricarboxylic acid compound (orange solid, molecular weight: 466.43) was obtained. The analytical results are shown in Figure 2.
[0154] (3) Synthesis of hyperbranched resin having polyamide structure The following reaction was carried out.
[0155]
[0156] The following was placed in a test tube: 0.23 g of the tricarboxylic acid compound synthesized in (2) above, 3.0 mL of N-methylpyrrolidone (NMP), 0.085 g of 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP), and 0.25 mL of diisopropylcarbodiimide (DIC). The contents were stirred at 25°C for 24 hours to carry out the reaction. The reaction mixture was reprecipitated using dichloromethane, and the precipitate was filtered using a Kiriyama funnel to obtain the target resin. 1 The results of H-NMR and GPC analysis are shown in Figures 3A and 3B. Yield: 97% Mn = 7400, Mn / Mn = 2.40
[0157] The synthesis reaction of this resin was carried out using the same method as above, except for changing the amount of solvent as shown in the table below. However, if the amount of solvent was too small, gelation occurred and the desired resin could not be obtained.
[0158]
[0159] Example 2 Hyperbranched Resin Having Polyamide Structure (1) Synthesis of Tricarboxylic Acid Chloride The reaction shown in the following scheme was carried out.
[0160]
[0161] The following was placed in a 200 mL recovery flask: 2.33 g, 7.76 mmol of the tricarboxylic acid obtained in Example 1, 30 mL of chloroform, 60 mmol of thionyl chloride, 7.14 g, 4.36 mL of dimethylformamide (DMF), one drop of dimethylformamide (DMF).
[0162] The contents were stirred at 70°C for 18 hours. The reaction mixture was concentrated using an evaporator and washed with hexane. An orange viscous solid was obtained as the target product. The yield was 98%. The analytical results are shown in Figure 4.
[0163] (2) Synthesis of hyperbranched resin having polyamide structure The following reaction was carried out.
[0164]
[0165] The following was placed in a test tube: 0.26 g of the compound obtained in (1) (tricarboxylic acid chloride (MBOAC)), 0.5 mmol; 0.19 g of 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP), 0.75 mmol; 0.3 mL of dimethylformamide (DMF); and 0.19 g of 4-dimethylaminopyridine (DMAP).
[0166] The contents were stirred at 25°C for 20 hours to carry out the reaction. The reaction mixture was reprecipitated using diethyl ether. The precipitate was collected and washed with a 1N aqueous solution of hydrochloric acid. The mixture was dried under reduced pressure to obtain the target hyperbranched resin having a polyamide structure. 1 The results of the H-NMR and GPC analyses are shown in FIGS. 5A and 5B.
[0167] Resins were produced in the same manner by changing the charging ratio of 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP) (Table 2 (B)) and tricarboxylic acid chloride (Table 2 (A)). The charging ratio was set to a ratio that would achieve the functional group equivalent ratio shown in the table below. The results are shown in the table.
[0168]
[0169] (3) Physical Properties 1) Heat Resistance The thermal decomposition temperature of the obtained hyperbranched resin was measured by TGA (thermogravimetry). The results are shown in Figure 5C. The resin had excellent heat resistance.
[0170] 2) Solubility The solubility of the hyperbranched resin in various solvents was evaluated. When 2 mg of the resin dissolved in 2 g of solvent at 20°C, it was evaluated as "completely soluble (+)", and when it did not dissolve, it was evaluated as "insoluble (-)". The results are shown in the table below. It is clear that the resin has good solubility in major solvents.
[0171]
[0172] THF: Tetrahydrofuran, DMF: Dimethylformamide, DMSO: Dimethyl sulfoxide, PGMEA: Propylene glycol monomethyl ether acetate, NMP: N-methylpyrrolidone, DMAc: N,N-dimethylacetamide, MEK: Methyl ethyl ketone, PGME: Propylene glycol monomethyl ether
[0173] 3) Film Formability The hyperbranched resin was dissolved in dimethylformamide (DMF) to obtain a composition with a concentration of 3% by weight. The solution was spin-coated onto a silicon wafer under the following conditions, and post-baked to obtain a film. Film formability was good. Rotation speed: 2500 rpm Drying: 10 minutes at 200°C Film thickness: 32.4 nm However, when dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAc), or N-methylpyrrolidone (NMP) was used as the solvent, film formation was not possible.
[0174] Example 3 A hyperbranched resin having a polyamide structure was synthesized by carrying out the following reaction.
[0175]
[0176] The following was placed in a test tube: 0.75 mmol, 0.275 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoromethylpropane (BAHFP), 0.5 mmol, 0.132 g of 1,3,5-benzenetricarbonyl trichloride (BCC), 1.5 mL of dimethylformamide (DMF), and 1.5 mmol, 0.183 g of 4-dimethylaminopyridine (DMAP).
[0177] The contents were stirred at 25°C for 20 hours to carry out the reaction. The reaction mixture was reprecipitated using water. The precipitate was collected and washed with diethyl ether. The precipitate was then filtered using a Kiriyama funnel and dried under reduced pressure at room temperature to obtain the target resin. The analysis results by GPC are shown in Figure 6.
[0178] Resins were produced in the same manner, but the charging ratio of tricarboxylic acid chloride (BCC) and 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoromethylpropane (BAHFP) and the amount of solvent used were changed as shown in Table 4. The charging ratios were as shown in the table below. The results are shown in the table. The results of the GPC analysis are shown in Figure 6.
[0179]
[0180] [Example 4] A resin was produced in the same manner as in Example 3, except that the reaction temperature was changed. The results are shown in Table 5. The analytical results by GPC and FT-IR are shown in Figures 7A and 7B.
[0181]
[0182] The solubility and film-forming properties of the resin in Run 3 in Table 4 were evaluated by the methods described above. The results are shown in Tables 6 and 7, respectively.
[0183]
[0184]
[0185] The refractive index was measured by the following procedure: The resin was dissolved in DMF, and the solution was spin-coated onto a silicon wafer to prepare a thin film. The refractive index of the thin film at 620 nm was measured using a film thickness and refractive index distribution measuring device SE-101 manufactured by Photonic Lattice Co., Ltd.
[0186] Example 5 Synthesis of Hyperbranched Polybenzoxazole A 70 nm thick film (corresponding to the 70 nm film thickness in Table 7) produced from the hyperbranched PA resin obtained in Run 3 of Table 4 was heated at 300°C for 60 minutes in an inert atmosphere. As a result, intramolecular cyclization occurred, producing a hyperbranched polybenzoxazole (PBO) film. The analytical results are shown in Figures 8A and 8B.
[0187] Furthermore, a film of BCA[4]-DBH was formed on the hyperbranched polybenzoxazole film according to a standard method. BCA[4]-DBH is a main chain decomposition type cyclic molecular resist material synthesized from calixarene (see WO 2021 / 230185 or Journal of Photopolymer Science and Technology Volume 33, Number 1 (2020) 45-51). This material has the following structure and is a highly sensitive resist material for extreme ultraviolet radiation with excellent solubility and film-forming properties.
[0188]
[0189]
[0190] Example 6: Investigation of Fluorine Incorporation Rate A hyperbranched PA resin was synthesized in the same manner as in Example 3. However, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoromethylpropane (BAHFP) and 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP) were used as the diamino compounds, and 1,3,5-benzenetricarboxylic acid chloride (BCC) was used as the tricarboxylic acid compound, and the amounts charged were changed as shown in Table 9. Furthermore, the reaction conditions were changed to 25°C and 24 hours. Next, the hyperbranched PA resin was heated in the same manner as in Example 5 to attempt the production of a hyperbranched polybenzoxazole (PBO) resin film. The results are shown in Table 9.
[0191]
[0192] In Run 1, BAHP was used as the fluorine-free diamino compound. From Run 2 onward, BAHP was replaced with fluorine-containing BAHFP to increase the fluorine introduction rate. It became clear that as the fluorine introduction rate increased, intramolecular cyclization became more likely, making it possible to form a hyperbranched PBO resin film. When fluorine atoms were introduced, the fluorine atoms repelled each other, reducing the polymer density. This is thought to improve solubility and film-forming properties.
Claims
1. (I) preparing a diamino compound represented by formula (A) and a tricarboxylic acid compound represented by formula (B); (In the formula, Y is an alkylene group which may contain fluorine, and Z is independently -OH, -SH, or -NH 2 wherein each R is independently a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group or a hydroxyl group, and the aryl group, aralkyl group, alkenyl group, alkynyl group and arylalkenyl group may contain an ether bond, a ketone bond, an ester bond or a urethane bond, m is the number of groups other than hydrogen when R is an integer of 1 to 3, Ar is a group having an aromatic group, E is -COOH, -COHal, -O-R b -COOH or -O-R b -COHal, Hal is a halogen atom, R b is an alkylene group having 1 to 6 carbon atoms.) (II) A step of forming a polyamide structure by subjecting these compounds to a condensation reaction, 2. The resin according to claim 1, wherein Y is a branched alkylene group.
3. The resin according to claim 1 or 2, wherein Y is a fluorinated alkylene group.
4. A hyperbranched resin having a heterocyclic structure, produced by a process comprising: (i) a step of preparing a hyperbranched resin having a polyamide structure according to any one of claims 1 to 3; and (ii) a step of intramolecularly condensing the resin to form a heterocyclic structure.
5. The resin according to claim 4, wherein there are units in which Y is an alkylene group and units in which Y is a fluorinated alkylene group, and the molar ratio of said alkylene group:fluorinated alkylene group is 1:(1.5 to 10).
6. A lithographic film-forming composition comprising the resin according to any one of claims 1 to 5.
7. A lithography underlayer film forming composition comprising the resin according to claim 3.
8. The composition according to claim 6 or 7, which contains a solvent.
9. The composition of any one of claims 6 to 8, comprising a component selected from the group consisting of a solvent, an acid generator, an acid crosslinker, and combinations thereof.
10. A lithographic underlayer film formed using the composition of claim 7.
11. A lithographic underlayer film comprising the resin of claim 4 or 5.
12. A method for forming a resist pattern, comprising the steps of: forming an underlayer film on a substrate using the composition according to claim 7, and heating the precursor to 300°C or higher to form an underlayer film containing a hyperbranched resin having a heterocyclic structure; forming at least one photoresist layer on the underlayer film; and irradiating a predetermined area of the photoresist layer with radiation and carrying out development.
13. Represented by the following formula (1): (In the formula, Y is an alkylene group which may contain fluorine, X is a group having an aromatic group, and Z is -OH, -SH, or -NH. 2 wherein each R is independently a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group or a hydroxyl group, wherein the aryl group, the aralkyl group, the alkenyl group, the alkynyl group or the arylalkenyl group may contain an ether bond, a ketone bond, an ester bond or a urethane bond, m is the number of groups other than hydrogen when R is an integer of 1 to 3, n is the number of repetitions in the main chain, r is the number of repetitions in the branched chain, and n>r. A multi-branched resin having a polyamide structure.
14. Represented by the following formula (2): (In the formula, Y 1 is a fluorinated alkylene group, Y 2 is an alkylene group, Z' is independently -O-, -S- or -NH-, X is a group having an aromatic group, each R is independently a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group or a hydroxyl group, and the aryl group, aralkyl group, alkenyl group, alkynyl group or arylalkenyl group may contain an ether bond, a ketone bond, an ester bond or a urethane bond, m is the number of groups other than hydrogen when R is an integer of 1 to 3, 1 and n 2 is the number of repeats in the main chain, and r 1 and r 2 is the number of repeats in the branched chain, and n 1 >r 1 And n 2 >r 2 ) A hyperbranched resin having a heterocyclic structure.
15. The X is represented by any one of the following formulas: (Ar is an aromatic group, R b is an alkylene group having 1 to 6 carbon atoms.
Citation Information
Patent Citations
Organic insulation film and organic insulation film material
JP2001163977A
Material for insulating film, coating varnish for insulating film, and insulating film and semiconductor unit therewith
JP2003277508A
Positive photosensitive resin composition and semiconductor device or display component using the same
JP2005249847A
Positive photosensitive resin composition, method for forming pattern and electronic component
JP2011158921A
Positive photosensitive resin composition, dry film, cured product, and electronic component
JP2020144222A