Reflectance adjustment film, multilayer body, and method for producing reflectance adjustment film
The reflectance adjustment film, formed by alternately laminating silicon dioxide and yttrium oxide films with replaced yttrium atoms using a sputtering method, addresses the low hardness and contamination issues of existing films, achieving high hardness and effective light management without a separate hard coat layer.
Patent Information
- Application Number
- PCT/JP2023/043305
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-12-04
- Publication Date
- 2024-10-31
AI Technical Summary
Existing reflectance adjustment films have low hardness, leading to scratch risks and increased complexity when a hard coat layer is added separately, and there is a risk of foreign matter contamination during film formation.
A reflectance adjustment film is created by alternately laminating low refractive index films, such as silicon dioxide and yttrium oxide with replaced yttrium atoms, and high refractive index films, using a sputtering method to enhance hardness and scratch resistance without a separate hard coat layer, while maintaining low refractive index film properties.
The solution provides a reflectance adjustment film with high hardness and improved scratch resistance, reducing the risk of foreign matter contamination and simplifying the manufacturing process, while maintaining effective light reflectance and transmittance adjustment capabilities.
Smart Images

Figure JP2023043305_31102024_PF_FP_ABST
Abstract
Description
Reflectance adjustment film, laminate, and method for manufacturing reflectance adjustment film
[0001] The present disclosure relates to a reflectance adjustment film, a laminate, and a method for manufacturing a reflectance adjustment film.
[0002] A reflectance adjusting film for adjusting the reflectance of light may be laminated on the surface of a glass substrate or the like. For example, Patent Document 1 describes an antireflection film for preventing reflection of light as the reflectance adjusting film. The antireflection film of Patent Document 1 can be formed, for example, by alternately laminating low-refractive index films and high-refractive index films on a glass substrate.
[0003] International Publication No. 2019-151321
[0004] The reflectance adjustment film having the configuration described in Patent Document 1 has low hardness (softness), and therefore may be scratched during use, etc. For this reason, in order to increase the hardness of the reflectance adjustment film and improve scratch resistance, etc., a hard coat layer can be provided on the substrate as a layer separate from the reflectance adjustment film.
[0005] However, providing a hard coat layer as a separate film from the reflectance adjusting film increases the number of steps, and there is a risk of foreign matter being mixed into the reflectance adjusting film when the reflectance adjusting film is formed on the hard coat layer.
[0006] Therefore, an object of the present disclosure is to provide a reflectance adjustment film having high hardness, a laminate including this reflectance adjustment film, and a method for manufacturing the reflectance adjustment film.
[0007] In order to achieve this object, the reflectance adjustment film of the present disclosure is a reflectance adjustment film that adjusts the reflectance of light, and is formed by stacking a plurality of films, the plurality of films including a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, and the low refractive index film is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that the yttrium oxide (Y 2 O 3) is a reflectance adjusting film in which some of the yttrium (Y) atoms are substituted with atoms of a 4A group element, and the refractive index of at least one film among the films adjacent to the high refractive index film is smaller than the refractive index of the high refractive index film.
[0008] The laminate of the present disclosure is a laminate in which the reflectance adjustment film of the present disclosure is formed on at least one surface of a substrate.
[0009] The manufacturing method of the reflectance adjustment film of the present disclosure includes a low refractive index film formation process of forming the low refractive index film and a high refractive index film formation process of forming the high refractive index film, in which the low refractive index film is formed by a sputtering method in the low refractive index film formation process, and the high refractive index film is formed by a sputtering method in the high refractive index film formation process.
[0010] According to the present disclosure, it is possible to provide a reflectance adjustment film having high hardness, a laminate including this reflectance adjustment film, and a method for manufacturing the reflectance adjustment film.
[0011] Fig. 1 is a cross-sectional view showing an example of a reflectance adjusting film and a laminate of the present disclosure, and Fig. 2 is a cross-sectional view showing an example of a laminate having a hard coat layer and a reflectance adjusting film of the present disclosure.
[0012] In the present disclosure, "on" or "on the surface" may refer to a state of being in direct contact with the surface or a state of being interposed between another layer or the like.
[0013] In this disclosure, unless otherwise specified, when "suppressing" any phenomenon, it is not limited to minimizing the occurrence of the phenomenon, but also includes eliminating the occurrence of the phenomenon.
[0014] In this disclosure, unless otherwise specified, the term "reflectance adjusting film" refers to a film-like structure that can adjust the reflectance of incident light by changing the film thickness, refractive index, etc.
[0015] In the present disclosure, unless otherwise specified, the term "film thickness" may refer to either "physical film thickness" or "optical film thickness."
[0016] Specific embodiments of the present disclosure will be described below with reference to drawings, etc. as necessary. For the sake of convenience, each drawing is drawn schematically with appropriate omissions, exaggerations, etc. Furthermore, when mechanisms and principles are mentioned in the following embodiments and examples, the mechanisms and principles described are merely presumptions and are not limited to the described mechanisms and principles.
[0017] [1. Reflectance Adjusting Film and Laminate] First, the reflectance adjusting film and laminate of the present disclosure will be described with reference to examples.
[0018] [1-1. Configuration of Reflectance Adjustment Film and Laminate] The cross-sectional view of Figure 1 schematically shows the configuration of an example of a reflectance adjustment film of the present disclosure and a laminate of the present disclosure using the same. As shown in the figure, a laminate 100 of the present disclosure has a reflectance adjustment film 10 of the present disclosure formed on one surface of a substrate 20. The reflectance adjustment film 10 is a film formed by laminating a plurality of films (low refractive index films 11 and high refractive index films 12 described below) onto which light is incident. The reflectance adjustment film 10 is formed by alternately laminating low refractive index films 11 and high refractive index films 12. In the figure, the film adjacent to the substrate 20 and the film farthest from the substrate 20 are each a low refractive index film 11.
[0019] The stacking order of the low refractive index film 11 and the high refractive index film 12 is not particularly limited, but when the reflectance adjustment film 10 is used as an anti-reflection film, the film farthest from the substrate 20 is the low refractive index film 11 .
[0020] In FIG. 1 , there are three low-refractive-index films 11 and two high-refractive-index films 12. However, in the reflectance adjustment film of the present disclosure, the number of low-refractive-index films and high-refractive-index films is not limited, and at least one of each may be used. In the reflectance adjustment film of the present disclosure, the lower limit of the total number of low-refractive-index films and high-refractive-index films is preferably three or more, more preferably five or more, and the upper limit is not particularly limited, but may be, for example, 30 or less, 20 or less, 15 or less, or 10 or less. A smaller total number of low-refractive-index films and high-refractive-index films (i.e., a smaller total number of low-refractive-index films and high-refractive-index films) is preferable because it can shorten the time required to produce the reflectance adjustment film of the present disclosure or reduce the production costs. Furthermore, a larger total number of low-refractive-index films and high-refractive-index films (i.e., a larger total number of low-refractive-index films and high-refractive-index films) is preferable because it makes it easier to achieve the desired reflectance, etc., of the reflectance adjustment film of the present disclosure.
[0021] The substrate 20 is not particularly limited, but may be, for example, a plate-shaped substrate. The material of the substrate 20 may be glass, resin, or the like. Examples of glass include glass plates and glass lenses. Examples of resin include resin plates and resin lenses. The resin material is not particularly limited, but may be, for example, polyolefin, polyester, PC (polycarbonate), acrylic resin, or the like. Examples of the polyolefin include, for example, PP (polypropylene), PE (polyethylene), and COP (cycloolefin polymer). Examples of the polyester include, for example, PET (polyethylene terephthalate). Examples of the acrylic resin include, for example, PMMA (polymethyl methacrylate). Although the substrate 20 in FIG. 1 is a single layer, this is not limited thereto, and the substrate 20 may be a laminate of multiple layers, in which case the layers may be the same or different. The laminate 100 may be, for example, a lens or window glass having a reflectance control film 10.
[0022] The reflectance adjustment film 10 in FIG. 1 includes only a low-refractive-index film 11 and a high-refractive-index film 12. However, the reflectance adjustment film of the present disclosure is not limited to this and may include layers other than the low-refractive-index film and the high-refractive-index film. Furthermore, the number of low-refractive-index films 11 is three, and the number of high-refractive-index films 12 is two. The reflectance adjustment film 10 in FIG. 1 is stacked such that the low-refractive-index film 11 and the high-refractive-index film 12 are in direct contact with each other. However, the configuration of the present disclosure is not limited to this configuration. For example, the low-refractive-index film 11 and the high-refractive-index film 12 may be stacked via a layer other than the low-refractive-index film and the high-refractive-index film. Furthermore, in FIG. 1, the reflectance adjustment film 10 is stacked on the substrate 20 in direct contact with each other. However, the present disclosure is not limited to this configuration. For example, the reflectance adjustment film 10 may be stacked on the substrate 20 via a layer other than the low-refractive-index film 11 and the high-refractive-index film 12. However, from the viewpoint of preventing foreign matter originating from the other layers from being mixed into the reflectance adjustment film, it is preferable that the reflectance adjustment film and the laminate of the present disclosure do not contain any layers other than the low refractive index film and the high refractive index film.
[0023] 2 shows an example of a laminate having a hard coat layer and a reflectance adjusting film according to the present disclosure. As shown in the figure, in this laminate 100a, a hard coat layer 30 is formed on one surface of a substrate 20, and a reflectance adjusting film 10a is formed on the surface of the hard coat layer 30 opposite the substrate 20. The reflectance adjusting film 10a is formed by alternately stacking low refractive index films 11a and high refractive index films 12a. In FIG. 2, the film adjacent to the hard coat layer 30 (closest to the substrate 20) and the film farthest from the substrate 20 are each a low refractive index film 11a.
[0024] Using a hard coat layer as a separate layer from the reflectance adjustment film, as shown in Figure 2, can increase the hardness of the reflectance adjustment film and improve its scratch resistance, for example. However, as mentioned above, providing the hard coat layer increases the number of steps. Also, when forming the reflectance adjustment film on the hard coat layer, there is a risk of foreign matter being mixed into the reflectance adjustment film. In contrast, the reflectance adjustment film 10 in Figure 1 has high hardness even without a hard coat layer, so it can solve these problems.
[0025] As described above, the reflectance adjusting film of the present disclosure has a low refractive index film made of silicon dioxide (SiO 2) and yttrium oxide (Y 2 O 3 ), provided that yttrium oxide (Y 2 O 3 In the case of yttrium oxide (Y), some of the yttrium (Y) atoms are replaced by atoms of a Group 4A element. 2 O 3 In the case of yttrium oxide (Y), some of the oxygen (O) atoms may be substituted with nitrogen (N) atoms. 2 O 3 By substituting some of the oxygen (O) atoms of the reflectance adjusting film with nitrogen (N) atoms, it is expected that the film will have low adhesion to basic substances and antifouling properties with respect to certain substances. The principle behind the provision of adhesion and antifouling properties is thought to be, for example, that the substitution of some of the oxygen (O) atoms with nitrogen (N) atoms deactivates hydroxyl groups, which are active groups on the surface of the reflectance adjusting film.
[0026] In addition, yttrium oxide (Y 2 O 3 ) is silicon dioxide (SiO 2 ) is harder than yttrium oxide (Y 2 O 3 ) and silicon dioxide (SiO 2 The film formed by the mixture containing silicon dioxide (SiO 2 It is believed that the hardness of the low refractive index film is higher than that of a low refractive index film made of only yttrium oxide (Y 2 O 3 When some of the yttrium (Y) atoms in the low refractive index film are substituted with atoms of a Group 4A element, the bonding of the crystals that make up the low refractive index film becomes stronger. Therefore, when some of the yttrium (Y) atoms in the low refractive index film are substituted with atoms of a Group 4A element, it is thought that the hardness becomes higher than when no substitution is made.
[0027] The hardness of the reflectance adjustment film of the present disclosure is not particularly limited. However, when the substrate is glass, the hardness of the reflectance adjustment film is preferably 6.0 GPa or more, more preferably 6.1 GPa or more. The upper limit is, for example, 11 GPa or less.
[0028] In the present disclosure, the hardness is a numerical value measured by the method described in the examples below. However, in the present disclosure, the hardness may be measured by a method other than the measurement method described below.
[0029] The reflectance adjustment film of the present disclosure may be, but is not limited to, an anti-reflection film. For example, the reflectance adjustment film of the present disclosure may have a light transmittance of approximately 0%. Such a reflectance adjustment film may be, for example, a mirror with a light reflectance of approximately 100%. In the reflectance adjustment film of the present disclosure, the light reflectance, transmittance, etc. can be adjusted, for example, by appropriately setting the number, film thickness, refractive index, stacking order, etc. of the low refractive index films and the high refractive index films. Furthermore, in the reflectance adjustment film of the present disclosure, the light reflectance, transmittance, etc. can also be adjusted to vary depending on the wavelength of light, for example.
[0030] The reflectance of the reflectance adjustment film of the present disclosure is adjusted, for example, by the following method. As described above, the reflectance adjustment film of the present disclosure is configured by stacking multiple films. The refractive indexes of the multiple adjacent films differ from each other. Here, when light is incident from one film to another, if the refractive indexes of the two adjacent films are different, a portion of the incident light is reflected at the boundary between the two adjacent films. The greater the difference in refractive index between the two adjacent layers, the greater the intensity of the reflected light. Furthermore, the film thickness of the multiple stacked films affects the phase of the reflected light that occurs at the boundary between the two adjacent films. In the reflectance adjustment film of the present disclosure, light is reflected at the boundary between each of the multiple stacked films. Therefore, the reflectance of the reflectance adjustment film of the present disclosure can be adjusted by adjusting the refractive index and film thickness of the multiple stacked films.
[0031] When the reflectance adjusting film of the present disclosure is an anti-reflection film, the upper limit of the light reflectance is not particularly limited, but the average reflectance in visible light (380 nm to 780 nm) is preferably 2.5% or less, more preferably 2.0% or less, 1.5% or less, or 1.0% or less. The lower limit of the reflectance is not particularly limited, but is, for example, 0 or a value exceeding 0.
[0032] In the present disclosure, the light reflectance may be measured using an apparatus capable of measuring the light reflectance. An example of an apparatus capable of measuring the light reflectance is a reflection spectroscopic film thickness meter (product name: FE-3000) manufactured by Otsuka Electronics Co., Ltd. The light reflectance can be a numerical value measured from the wavelength of incident light, the film thickness of the low refractive index film and the high refractive index film, the optical constants of these films, and the optical constants of the substrate. However, in the present disclosure, the light reflectance may be measured by a method other than the above-mentioned measurement method. In addition, in the present disclosure, the light reflectance may be an actual measurement value using an apparatus, or may be a simulated value calculated using optical simulation software or the like.
[0033] [1-2. Low Refractive Index Film] Hereinafter, the low refractive index film in the reflectance adjustment film of the present disclosure will be described with reference to an example.
[0034] The refractive index of the low refractive index film is not particularly limited, but for example, the refractive index for light with a wavelength of 500 nm is in the range of 1.47 to 1.58.
[0035] In the present disclosure, the refractive index may be a value measured using, for example, an apparatus capable of measuring the refractive index. An example of an apparatus capable of measuring the refractive index is a reflection spectroscopic film thickness meter (product name: FE-3000) manufactured by Otsuka Electronics Co., Ltd. However, in the present disclosure, the refractive index may be measured using a measurement method other than the following.
[0036] As described above, the low refractive index film in the reflectance adjusting film of the present disclosure is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that yttrium oxide (Y 2 O 3 In the case of yttrium oxide (Y), some of the yttrium (Y) atoms are replaced by atoms of a Group 4A element. 2 O 3In the case of yttrium oxide, some of the oxygen (O) atoms may be substituted with nitrogen (N) atoms. The content of yttrium oxide in the low refractive index film is not particularly limited, but for example, the lower limit is preferably 1.0 mol% or more, and more preferably 1.1 mol% or more, and the upper limit is preferably less than 10 mol%, and more preferably less than 6 mol%, from the viewpoint of improving antireflection performance.
[0037] In the present disclosure, the atomic content in a film may be a value measured, for example, by an X-ray photoelectron spectrometer. An example of an X-ray photoelectron spectrometer is an X-ray photoelectron spectrometer (product name: PHI5000 VersaProbe2) manufactured by ULVAC-PHI, Inc. With an X-ray photoelectron spectrometer, a sample is irradiated with X-rays and the energy of photoelectrons emitted from the sample surface is measured, thereby obtaining information about the surface composition and chemical bonding state, thereby enabling the atomic content in a film to be measured. In the present disclosure, the atomic content in a film may be measured by a method other than the following measurement method.
[0038] The low refractive index film in the reflectance adjusting film of the present disclosure is made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ) may or may not contain other components. Examples of other components include magnesium fluoride (MgF 2 ) etc.
[0039] In the reflectance adjusting film of the present disclosure, yttrium oxide (Y 2 O 3In the case of (I), some of the yttrium (Y) atoms are substituted with atoms of a Group 4A element. The atoms of the Group 4A element are not particularly limited, but may be, for example, at least one selected from the group consisting of titanium (Ti), zirconium (Zr), and hafnium (Hf), preferably at least one of zirconium (Zr) and hafnium (Hf), and particularly preferably zirconium (Zr). These atoms or their forming materials may be used alone, or a combination of two or more of these atoms and their forming materials may be used.
[0040] The reflectance adjusting film of the present disclosure is a low refractive index film containing yttrium oxide (Y 2 O 3 For example, by substituting some of the yttrium (Y) atoms with atoms of a Group 4A element, high hardness (scratch resistance, etc.) can be obtained. The reason for this is that, for example, when some of the yttrium (Y) atoms are substituted with atoms of a Group 4A element (for example, zirconium (Zr)), the hardness of yttrium oxide (Y 2 O 3 This is thought to be because the hardness is higher than that of the sintered body.
[0041] Furthermore, the low refractive index film in the reflectance adjustment film of the present disclosure may be, for example, crystalline. Whether the low refractive index film is crystalline can be confirmed by common crystallinity evaluation methods such as X-ray diffraction, electron beam diffraction, Raman spectroscopy, etc. Furthermore, whether the low refractive index film contains yttrium oxide containing nitrogen and a Group 4A element can be identified by, for example, secondary ion mass spectrometry (SIMS).
[0042] In the low refractive index film, yttrium oxide (Y 2 O 3 The substitution rate of yttrium (Y) atoms in the yttrium (Y)-containing yttrium (Y) alloy with atoms of a Group 4A element (the content of atoms of a Group 4A element) is not particularly limited as long as it exceeds 0, but the upper limit may be, for example, 20 mol % or less, 15 mol % or less, 10 mol % or less, or 5 mol % or less.
[0043] In the low refractive index film, yttrium oxide (Y 2 O 3 ), when some of the oxygen (O) atoms are replaced with nitrogen (N) atoms, yttrium oxide (Y 2 O 3 The substitution rate (nitrogen atom content) of oxygen (O) atoms in the polyimide (A) (A), (B), (C), (D), (E), (F), (G), (H), (I ...
[0044] Furthermore, the low refractive index film does not need to contain metal elements or harmful metals that can cause allergies, such as Hg, Ni, Cr, Co, Cu, Sn, Au, Pt, Pd, Sb, Ag, Fe, or Zn.
[0045] The physical thickness of the low refractive index film is not particularly limited and can be appropriately selected depending on the desired optical properties.
[0046] In the present disclosure, the physical film thickness may be a value measured using a spectroscopic film thickness meter. With a spectroscopic film thickness meter, a sample is irradiated with light, and an optical interference phenomenon caused by a phase shift resulting from the optical path difference between the irradiated light and the reflected light is measured. The film thickness can be measured from the obtained reflection spectrum and refractive index. An example of a spectroscopic film thickness meter is the Reflection Spectroscopic Film Thickness Meter (product name: FE-3000) manufactured by Otsuka Electronics Co., Ltd. However, in the present disclosure, the physical film thickness may also be measured using a method other than the above.
[0047] [1-3. High Refractive Index Film] Hereinafter, the high refractive index film in the reflectance adjustment film of the present disclosure will be described with examples.
[0048] The refractive index of the high-refractive-index film is not particularly limited as long as it is higher than the refractive index of the low-refractive-index film. For example, the refractive index of the high-refractive-index film with respect to light having a wavelength of 500 nm is preferably such that the lower limit is 1.9 or more and the upper limit is 2.75 or less, 2.5 or less, or 2.3 or less.
[0049] In the reflectance adjusting film of the present disclosure, the material for forming the high refractive index film is not particularly limited, but may be, for example, tantalum pentoxide (Ta 2 O 5 ), niobium pentoxide (Nb 2 O 5 ), titanium oxide (TiO 2 ), zirconium oxide (ZrO 2 ), and cerium oxide (CeO 2 ) or may be formed of other materials. From the viewpoint of achieving both hardness and refractive index, the high refractive index film is preferably formed of tantalum pentoxide. Furthermore, when the high refractive index film is formed of tantalum pentoxide, it may or may not contain other materials. These atoms or their forming materials may be used alone, or a combination of two or more of these atoms and their forming materials may be used.
[0050] The physical thickness of the high refractive index film is not particularly limited and can be appropriately selected depending on the desired optical properties.
[0051] [1-4. Other Films] The reflectance adjusting film of the present disclosure may include, for example, other films. Examples of other films include a medium refractive index film. The medium refractive index film is not particularly limited as long as it has a refractive index higher than that of the low refractive index film and lower than that of the high refractive index film. The material for forming the medium refractive index film is not particularly limited, but may be, for example, aluminum oxide (Al 2 O 3 ) or may be formed of other materials.
[0052] [2. Method for manufacturing reflectance adjustment film and laminate] The method for manufacturing the reflectance adjustment film and laminate of the present disclosure is not particularly limited, and for example, the low refractive index film and the high refractive index film may be formed sequentially on the substrate.
[0053] The method for forming the low-refractive-index film and the high-refractive-index film in the reflectance adjustment film of the present disclosure is not particularly limited. For example, it is preferable to use a vacuum deposition method, a sputtering method, an ion plating method, or an ion beam deposition method, which are classified as physical vapor deposition, or an atomic layer deposition method or a plasma CVD method, which are classified as chemical vapor deposition. Vapor deposition methods tend to produce films with a high film formation rate but low hardness (soft). Sputtering methods tend to produce films with a low film formation rate but high hardness (hard). In terms of hardness, it is preferable that the low-refractive-index film and the high-refractive-index film are each formed by a sputtering method in the reflectance adjustment film of the present disclosure. In the manufacturing method for the reflectance adjustment film and the manufacturing method for the laminate of the present disclosure, as described above, in the low-refractive-index film formation step, the low-refractive-index film is formed by a sputtering method, and in the high-refractive-index film formation step, the high-refractive-index film is formed by a sputtering method.
[0054] The low refractive index film is made of yttrium oxide (Y 2 O 3 ), further, in order to replace some of the oxygen (O) atoms with nitrogen (N) atoms, for example, argon (Ar) is replaced with nitrogen (N 2 Alternatively, the film may be formed by a sputtering method (reactive sputtering method) in an atmosphere containing HCl.
[0055] In the low refractive index film formation process and the high refractive index film formation process in the manufacturing method of the reflectance adjustment film of the present disclosure and the manufacturing method of the laminate of the present disclosure, the method of performing sputtering is not particularly limited, and may be, for example, the same as or equivalent to a general sputtering method.
[0056] In the low refractive index film formation process and the high refractive index film formation process, from the viewpoint of manufacturing efficiency, it is preferable that the film formation rate by the sputtering method is not too slow, and from the viewpoint of film hardness, it is preferable that the film formation rate by the sputtering method is not too fast.
[0057] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.
[0058] <Materials used> Silicon dioxide (SiO2 ), yttrium oxide (Y 2 O 3 ), and zirconium oxide (ZrO 2 Tantalum pentoxide (Ta) was used as a target for forming a high refractive index film. 2 O 5 ) was used. Glass was used as the substrate.
[0059] <Production of Laminates with Reflectance Adjusting Films> Laminates with reflectance adjusting films formed thereon were produced by sputtering in Examples 1 to 3 and Comparative Example 1. The sputtering of the low refractive index films and high refractive index films described below was carried out using a nitrogen (N 2 First, the target for forming the low refractive index film was prepared in an atmosphere containing yttrium oxide (Y 2 O 3 A low refractive index film was formed on one surface of the substrate by sputtering the target for forming the high refractive index film onto the surface of the first low refractive index film (second layer, physical thickness 15 nm). Next, a target for forming the low refractive index film was sputtered onto the surface of the first low refractive index film to form a high refractive index film (second layer, physical thickness 15 nm). Next, a target for forming the low refractive index film was sputtered onto the surface of the first low refractive index film by sputtering the target for forming the high refractive index film onto the surface of the first low refractive index film. 2 O 3 A low refractive index film was formed by sputtering the target for forming the high refractive index film onto the surface of the low refractive index film of the third layer so that the composition of yttrium oxide (Y) was as shown in Table 1 below (third layer, physical film thickness 30 nm). Next, a target for forming the high refractive index film was sputtered onto the surface of the low refractive index film of the third layer to form a high refractive index film (fourth layer, physical film thickness 115 nm). Finally, a target for forming the low refractive index film was sputtered onto the surface of the low refractive index film of the third layer so that the composition of yttrium oxide (Y) was as shown in Table 1 below (fourth layer, physical film thickness 115 nm). 2 O 3 A low refractive index film was formed by sputtering on the surface of the fourth high refractive index film so that the composition of yttrium oxide (Y) was as shown in Table 1 below (fifth layer, physical film thickness 86 nm). The laminate thus obtained, in which a reflectance adjustment film was formed on a glass substrate, was evaluated. The low refractive index film formed by the above method was 2 O 3 ) in which some of the yttrium (Y) atoms are replaced by zirconium (Zr) atoms, and yttrium oxide (Y2 O 3 ) in which some of the oxygen (O) atoms have been replaced with nitrogen (N) atoms.
[0060] <Evaluation Method> For the low refractive index films formed as described above, (1) the refractive index was measured according to the following procedure. Furthermore, for the laminates formed with the reflectance adjustment films of Examples 1 to 3 and Comparative Example 1, (2) the hardness and (3) the average reflectance were measured according to the following procedure.
[0061] (1) Refractive Index The refractive index of the low refractive index film at a light wavelength of 500 nm was measured using a reflection spectroscopic film thickness meter (manufactured by Otsuka Electronics Co., Ltd., product name: FE-3000). The results are shown in Table 1 below.
[0062] (2) Hardness The hardness of the reflectance control film in the manufactured laminate was measured using a nanoindenter (manufactured by ELIONIX Co., Ltd., product name: ENT-1100a). A Berkovich indenter was used as the indenter, and the nanoindentation hardness (hardness) was measured when the reflectance control film was pressed with a maximum load of 1.5 mN. Specifically, the indenter was first pressed into the sample at a constant rate until the maximum load was reached. Next, the load was released at a constant rate until the load reached 0, and the indenter was removed from the sample. The displacement of the indenter during loading and unloading was recorded to determine the maximum load. Next, the contact projected area (base area of the cone) of the contact portion when the indenter was pressed was determined. The nanoindentation hardness was calculated by dividing the determined maximum load by the contact projected area. The results are shown in Table 1 below.
[0063] (3) Average Reflectance: Using optical simulation software (manufactured by TOHO TSUSHO INC., product name: ThinFilmView), simulated values of average reflectance in the visible light region (380 nm to 780 nm) were calculated. The results are shown in Table 1 below.
[0064]
[0065] As shown in Table 1, the hardness of Examples 1 to 3 was higher than that of Comparative Example 1. In addition, the hardness of the yttrium oxide (Y 2 O 3Increasing the proportion of yttrium oxide (Y) in the low refractive index film increased the hardness. 2 O 3 The average reflectance was calculated by simulation by changing the ratio of
[0066] The laminates of Examples 1 to 3 all had a total light transmittance of 95% as measured with an ultraviolet-visible-near infrared spectrophotometer (manufactured by Shimadzu Corporation, product name: SolidSpec-3700), which resulted in excellent transparency (not shown in Table 1). Furthermore, the laminates of Examples 1 to 3 all had a pencil hardness (based on the old JIS K5400) of 9H or more, which was high hardness (not shown in Table 1). In addition, the low refractive index film formed by the method of this example contained yttrium oxide (Y 2 O 3 ) in which some of the oxygen (O) atoms have been replaced with nitrogen (N) atoms, but yttrium oxide (Y 2 O 3 Even in a low refractive index film in which oxygen (O) atoms are not substituted with nitrogen (N) atoms, the yttrium oxide (Y 2 O 3 ) the hardness increased (not shown in Table 1).
[0067] Furthermore, the present invention is not limited to the above-described embodiments, and can be arbitrarily and appropriately combined, modified, or selected and adopted as needed within the scope of the spirit of the present invention.
[0068] Some or all of the above-described embodiments may be described as, but are not limited to, the following supplementary notes: (Supplementary Note 1) A reflectance adjustment film for adjusting the reflectance of light, comprising a plurality of films stacked one upon the other, the plurality of films including a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, the low refractive index film being made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that the yttrium oxide (Y 2 O 3Regarding the yttrium oxide (Y), a part of the yttrium (Y) atoms is substituted with atoms of a 4A group element, and the refractive index of at least one film among the films adjacent to the high refractive index film is smaller than the refractive index of the high refractive index film. (Appendix 2) 2 O 3 (Supplementary Note 3) The reflectance adjusting film according to Supplementary Note 1, wherein a part of oxygen (O) atoms is substituted with nitrogen (N) atoms. 2 O 3 ) content of 1.0 mol % or more. (Appendix 4) The reflectance adjustment film according to any one of Appendices 1 to 3, wherein the atoms of the 4A Group element in the low refractive index film are zirconium (Zr) atoms. (Appendix 5) A reflectance adjustment film for adjusting the reflectance of light, the reflectance adjustment film being a stacked film of a plurality of films, the plurality of films including a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, the refractive index of at least one film among the films adjacent to the high refractive index film being lower than that of the high refractive index film, and the hardness of the reflectance adjustment film being 6.0 GPa or more. (Appendix 6) The reflectance adjustment film according to any one of Appendices 1 to 5, wherein the refractive index of the low refractive index film for light with a wavelength of 500 nm is in the range of 1.47 to 1.58. (Appendix 7) The reflectance adjustment film according to any one of Appendices 1 to 6, wherein the number of the plurality of films is three or more. (Appendix 8) The high refractive index film is tantalum pentoxide (Ta 2 O 5 ), niobium pentoxide (Nb 2 O 5 ), titanium oxide (TiO 2 ), zirconium oxide (ZrO 2 ), and cerium oxide (CeO 2). (Appendix 9) The reflectance adjustment film according to any one of Appendices 1 to 8, which is an anti-reflection film that prevents reflection of light. (Appendix 10) A laminate, in which the reflectance adjustment film according to any one of Appendices 1 to 9 is formed on at least one surface of a substrate. (Appendix 11) The laminate according to Appendices 10, in which the film farthest from the substrate among the plurality of films in the reflectance adjustment film is the low refractive index film. (Appendix 12) The laminate according to Appendices 10 or 11, in which the substrate is at least one of glass and resin. (Appendix 13) A method for manufacturing a reflectance adjustment film according to any one of Appendices 1 to 9, comprising a low refractive index film forming step of forming the low refractive index film and a high refractive index film forming step of forming the high refractive index film, in which the low refractive index film is formed by sputtering in the low refractive index film forming step, and the high refractive index film is formed by sputtering in the high refractive index film forming step. (Appendix 14) A method for producing a laminate according to any one of Appendices 10 to 12, comprising the step of producing the reflectance control film on the substrate by the production method according to Appendices 13.
[0069] This application claims priority based on Japanese Patent Application No. 2023-075063, filed on April 28, 2023, the disclosure of which is incorporated herein in its entirety by reference.
[0070] 10, 10a Reflectance adjusting film 11, 11a Low refractive index film 12, 12a High refractive index film 20 Substrate 30 Hard coat layer 100, 100a Laminate
Claims
1. A reflectance adjustment film for adjusting the reflectance of light, comprising a plurality of films laminated together, the plurality of films including a low refractive index film and a high refractive index film having a refractive index higher than that of the low refractive index film, the low refractive index film being made of silicon dioxide (SiO 2 ) and yttrium oxide (Y 2 O 3 ), provided that the yttrium oxide (Y 2 O 3 ) a part of yttrium (Y) atoms is substituted with atoms of a Group 4A element, and a refractive index of at least one film among the high refractive index film and the films adjacent to the high refractive index film is smaller than a refractive index of the high refractive index film.
2. The yttrium oxide (Y 2 O 3 2. The reflectance adjusting film according to claim 1, wherein a part of oxygen (O) atoms is further substituted with nitrogen (N) atoms.
3. The yttrium oxide (Y 2 O 3 3. The reflectance adjusting film according to claim 1, wherein the content of said compound is 1.0 mol % or more.
4. A reflectance adjusting film according to any one of claims 1 to 3, wherein the atoms of the Group 4A element in the low refractive index film are zirconium (Zr) atoms.
5. The reflectance adjusting film according to any one of claims 1 to 4, wherein the refractive index of the low refractive index film for light with a wavelength of 500 nm is in the range of 1.47 to 1.
58.
6. The high refractive index film is tantalum pentoxide (Ta 2 O 5 The reflectance adjusting film according to claim 1 , which is formed of 7. The reflectance adjusting film according to any one of claims 1 to 6, which is an anti-reflection film for preventing reflection of light.
8. A laminate comprising a reflectance control film according to any one of claims 1 to 7 formed on at least one surface of a substrate.
9. The laminate according to claim 8, wherein the film furthest from the substrate among the plurality of films in the reflectance adjustment film is the low refractive index film.
10. A method for manufacturing a reflectance adjusting film described in any one of claims 1 to 7, comprising a low refractive index film formation process for forming the low refractive index film and a high refractive index film formation process for forming the high refractive index film, wherein in the low refractive index film formation process, the low refractive index film is formed by a sputtering method, and in the high refractive index film formation process, the high refractive index film is formed by a sputtering method.
Citation Information
Patent Citations
Method for producing maleimide resin
JP2023075063A
Antireflection film-equipped glass substrate and optical component
WO2019151321A1
Lens with antireflection film
JP1991162943A
Optical member having antireflection film
JP1993011101A
Optical member with antireflection film
JP1993034502A