Fluoroolefin production method

The use of a catalyst with high α-alumina content and specific Lewis acid site amounts in the production of fluoroolefins enhances conversion rates and maintains efficiency over long-term production, addressing the limitations of conventional methods.

WO2024224947A1PCT designated stage expired Publication Date: 2024-10-31AGC INC

Patent Information

Application Number
PCT/JP2024/013506
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-01
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional methods for producing fluoroolefins face challenges with low conversion rates and significant decreases in conversion rates over time, particularly when using γ-alumina or α-alumina catalysts, which results in inefficient production and catalyst deactivation.

Method used

A method involving a catalyst with 65% by mass or more of α-alumina and a Lewis acid site amount of 0.005 to 0.10 mmol/g, measured by ammonia temperature program desorption, is used to contact fluorocarbons, maintaining a high conversion rate and suppressing catalyst deactivation during long-term production.

Benefits of technology

The method achieves a higher conversion rate and maintains a 69% or more conversion rate retention after 50 hours compared to conventional methods, effectively addressing the issue of catalyst deactivation and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This fluoroolefin production method includes a step in which a fluorocarbon represented by formula (1): CX1X2F-CX3X4H is brought into contact with a catalyst to produce a fluoroolefin represented by formula (2): CX1X2=CX3X4, wherein (I) or (II) is satisfied. (I) The catalyst includes α-alumina in an amount of 65 mass% or larger and has an amount of Lewis acid sites, as determined by an ammonia temperature-programmed desorption method, of 0.005-0.10 mmol / g. (II) The conversion at 10 hours after the contacting of the fluorocarbon with the catalyst is 7.0-13.0%, and the retention of conversion, which is the proportion of the conversion after the lapse of 50 hours to the conversion after the lapse of 10 hours, is 69% or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Fluoroolefin production method

[0001] The present disclosure relates to a process for producing fluoroolefins.

[0002] In recent years, fluoroolefins have been attracting attention as compounds with low global warming potential.

[0003] For example, Patent Document 1 describes a method for producing a fluoroolefin, which includes a dehydrofluorination step of contacting a fluorocarbon with a metal catalyst to dehydrofluorinate the fluorocarbon, and which is carried out in a gas phase in the presence of water, with the water concentration being 500 ppm relative to the fluorocarbon, and γ-alumina is used as the catalyst. Furthermore, Non-Patent Document 1 describes a method for obtaining trifluoroethylene using α-alumina, γ-alumina, θ-alumina, or the like in the dehydrofluorination reaction of 1,1,1,2-tetrafluoroethane.

[0004] Japanese Patent Application Laid-Open No. 2019-196347

[0005] Catalysis Letters 2015, Vol. 145, p654-661

[0006] However, as described in Patent Document 1, when γ-alumina was used as a catalyst, the conversion rate tended to decrease over long-term production. Also, as described in Non-Patent Document 1, when γ-alumina, θ-alumina, or a combination thereof was used as a catalyst, the initial conversion rate was high, but the conversion rate decreased over long-term production. Also, when α-alumina was used as a catalyst, the conversion rate was very low at 1.2%.

[0007] An object of one embodiment of the present invention is to provide a method for producing a fluoroolefin that has a higher conversion rate than conventional methods and that is capable of suppressing a decrease in conversion rate during long-term production.

[0008] The present disclosure includes the following aspects: <1> A method for producing a fluoroolefin, comprising the step of bringing a fluorocarbon represented by the following formula (1) into contact with a catalyst to produce a fluoroolefin represented by the following formula (2), wherein the catalyst contains 65 mass % or more of α-alumina and has an amount of Lewis acid sites of 0.005 to 0.10 mmol / g as measured by ammonia temperature programmed desorption CX: 1 X 2 F-CX 3 X 4 H...(1) CX 1 X 2 =CX 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 <2> The method for producing a fluoroolefin according to <1>, wherein the amount of Lewis acid sites is 0.005 to 0.05 mmol / g. <3> The method for producing a fluoroolefin according to <1> or <2>, wherein the amount of Lewis acid sites is 0.008 to 0.05 mmol / g. <4> The method for producing a fluoroolefin according to <1> or <2>, wherein the amount of fluorocarbons supplied to the catalyst is 350 kg / hr / m 3The method for producing a fluoroolefin according to any one of <1> to <3>, wherein the fluorocarbon is at least one selected from the group consisting of 1,1,1-trifluoroethane, 1,1,2-trifluoroethane, 1,1,2,2-tetrafluoroethane, and 1,1,1,2-tetrafluoroethane. <6> The method for producing a fluoroolefin according to any one of <1> to <5>, wherein the fluoroolefin is at least one selected from the group consisting of 1,2-difluoroethylene, 1,1-difluoroethylene, and trifluoroethylene. <7> The method for producing a fluoroolefin according to any one of <1> to <6>, wherein the fluorocarbon is 1,1,1,2-tetrafluoroethane and the fluoroolefin is trifluoroethylene. <8> The method for producing a fluoroolefin according to any one of <1> to <7>, wherein the fluorocarbon and the catalyst are contacted at a temperature of 300 to 800°C. <9> The method for producing a fluoroolefin according to any one of <1> to <8>, wherein the fluorocarbon and the catalyst are contacted in the presence of an inert gas, and the inert gas is at least one selected from the group consisting of nitrogen, helium, argon, octafluorocyclobutane, and carbon dioxide. <10> The method for producing a fluoroolefin according to any one of <1> to <9>, further comprising a step of drying the catalyst before contacting the fluorocarbon with the catalyst. <11> The method for producing a fluoroolefin according to any one of <1> to <10>, wherein the fluorocarbon and the catalyst are contacted in a gas phase in the presence of water, and the concentration of the water is less than 500 ppm based on the total amount of the feed gas containing the fluorocarbon. <12> A method for producing a fluoroolefin, comprising a step of contacting a fluorocarbon represented by the following formula (1) with a catalyst to produce a fluoroolefin represented by the following formula (2), wherein the conversion rate is 7 to 13% 10 hours after contacting the fluorocarbon with the catalyst, and the conversion maintenance rate, which is the ratio of the conversion rate after 50 hours to the conversion rate after 10 hours, is 69% or more. 1X 2 F-CX 3 X 4 H...(1) CX 1 X 2 =CX 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.

[0009] According to the present disclosure, there is provided a method for producing a fluoroolefin that has a higher conversion rate than conventional methods and that suppresses a decrease in conversion rate over a long production period.

[0010] 1 is a diffraction pattern obtained by XRD measurement of the catalyst of Example 6.

[0011] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the Examples. In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. In the present disclosure, when multiple substances corresponding to each component are present, the amount of each component means the total amount of multiple substances unless otherwise specified. In the present disclosure, long-term production refers to production for 50 hours by contacting a fluorocarbon with a catalyst, and may be production for 50 hours or more.

[0012] [Method for Producing Fluoroolefin] A method for producing a fluoroolefin in a first embodiment of the present disclosure includes a step of contacting a fluorocarbon represented by the following formula (1) with a catalyst to produce a fluoroolefin represented by the following formula (2), wherein the catalyst contains 65% by mass or more of α-alumina and has an amount of Lewis acid sites of 0.005 to 0.10 mmol / g as measured by ammonia thermal desorption spectrometry. A method for producing a fluoroolefin in a second embodiment of the present disclosure includes a step of contacting a fluorocarbon represented by the following formula (1) with a catalyst to produce a fluoroolefin represented by the following formula (2), wherein the conversion rate 10 hours after contacting the fluorocarbon with the catalyst is 7.0 to 13.0%, and the conversion retention rate, which is the ratio of the conversion rate after 50 hours to the conversion rate after 10 hours, is 69% or more. CX 1 X 2 F-CX 3 X 4 H...(1) CX 1 X 2 =CX 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.

[0013] The fluoroolefin production method of the first embodiment and the fluoroolefin production method of the second embodiment are also collectively referred to as the fluoroolefin production method of the present disclosure.

[0014] According to the method for producing a fluoroolefin of the present disclosure, the conversion rate is higher than that of conventional methods, and a decrease in the conversion rate is suppressed during long-term production. The reason for this is unclear, but is presumed to be as follows.

[0015] In the reaction to obtain a fluoroolefin represented by formula (2) from a fluorocarbon represented by formula (1), hydrogen fluoride is generated. The generated hydrogen fluoride reacts with the fluoroolefin represented by formula (2) to return to the fluorofluorocarbon represented by formula (1). Because this reaction proceeds, the conversion rate of the fluorocarbon represented by formula (1) has traditionally been very low. In response to this, the present inventors have discovered that the use of a catalyst containing 65% by mass or more of α-alumina and having an amount of Lewis acid sites measured by ammonia temperature-programmed desorption spectroscopy of 0.005 mmol / g or more improves the conversion rate. This is believed to be due to the presence of an effective amount of active sites that activate C—F bonds in the catalyst, thereby enabling the dehydrofluorination reaction activity to be expressed. Furthermore, they have discovered that the use of a catalyst containing 65% by mass or more of α-alumina and having an amount of Lewis acid sites measured by ammonia temperature-programmed desorption spectroscopy of 0.10 mmol / g or less prevents the decline in catalytic activity over long periods of production. This is believed to be due to the moderate suppression of fluorination of the catalyst by hydrogen fluoride generated by the reaction. It is also believed that this is because the phenomenon of coking, in which carbon produced by decomposition of the raw material accumulates on the catalyst, is moderately suppressed.

[0016] On the other hand, Patent Document 1 describes a method for producing fluoroolefins using γ-alumina. However, because the crystal structure of γ-alumina changes significantly in a high-temperature environment, when γ-alumina is used as a catalyst, the conversion rate tends to decrease over long production times.

[0017] In addition, Non-Patent Document 1 discloses an Al containing 100 mass % of α-alumina. 2 O 3 A method for producing trifluoroethylene using Al-1200 is described. 2 O 3 -1200 is ammonia temperature programmed desorption (NH 3 It is reported that the Al has no Bronsted acid sites but has a Lewis acid site amount of 0.004 mmol / g, as determined by analysis of the IR spectrum of the Al (Al-TPD) or adsorbed pyridine (Py-IR). 2 O 3It is reported that when Al-1200 is used, the conversion rate is about 1.2%. 2 O 3 In the case of -1200, the amount of Lewis acid sites is less than 0.005 mmol / g, and therefore it is presumed that the conversion rate is low due to the small number of active sites of the catalyst.

[0018] Furthermore, Non-Patent Document 1 discloses an Al α-alumina composite containing 64.3 mass % of α-alumina and having an acid site content of 0.006 mmol / g. 2 O 3 This Al-1150 is used for the production of trifluoroethylene. 2 O 3 It is also stated that when -1150 is used, the conversion rate is about 1.2%.

[0019] In addition, Non-Patent Document 1 calculates the amount of fluorocarbon to be fed to the catalyst as 307 kg / h / m 3 Since the raw material supply rate is set low, this is a condition that allows for a high conversion rate. However, if the raw material supply rate is low, industrial productivity decreases, so it is necessary to increase the raw material supply rate. In Non-Patent Document 1, if the raw material supply rate is increased, the conversion rate will be lower than the above value.

[0020] Furthermore, Non-Patent Document 1 describes a method for producing trifluoroethylene using an alumina catalyst having an acid site content of 0.065 to 0.362 mmol / g. These alumina catalysts are composed of γ-alumina, θ-alumina, or the like, and do not contain α-alumina. When these alumina catalysts are used, the initial conversion rate is high, but the conversion rate drops significantly after 15 hours have passed. This is presumably because, as mentioned above, γ-alumina, θ-alumina, or the like, whose crystal structure is susceptible to change in a high-temperature environment, is used.

[0021] In Non-Patent Document 1, the fluoroolefins were produced under high conversion conditions, with an initial conversion of approximately 28% or more and a conversion of 20% or more after 10 hours. In this case, the conversion rate significantly decreased after 15 hours. This is thought to be because an excessively high initial conversion rate increases the amount of hydrogen fluoride generated, thereby promoting fluorination, one of the causes of catalyst deactivation. As catalyst fluorination progresses, catalyst coking is more likely to occur, resulting in catalyst deactivation. It is expected that if the production time in Non-Patent Document 1 is further extended to 50 hours, catalyst deactivation will progress and the conversion rate will further decrease. Therefore, by limiting the conversion rate after 10 hours from contacting the fluorocarbon with the catalyst to 7 to 13%, as in the fluoroolefin production method of the second embodiment, the conversion rate after 50 hours is maintained at 69% or more. A preferred method for effectively achieving a conversion rate of 7 to 13% after 10 hours is to use the catalyst according to the first embodiment.

[0022] (Fluorocarbon Represented by Formula (1)) In the method for producing a fluoroolefin according to the present disclosure, a fluorocarbon represented by the following formula (1) is used as a raw material: CX 1 X 2 F-CX 3 X 4 H...(1) In formula (1), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.

[0023] Examples of the fluorocarbon represented by formula (1) include the following compounds: CHF 2 CH 3 : 1,1-difluoroethane (HFC-152a) CH 2 FCH 2 F: 1,2-difluoroethane (HFC-152) CF 3 CH 3: 1,1,1-trifluoroethane (HFC-143a) CHF 2 CH 2 F: 1,1,2-trifluoroethane (HFC-143) CF 3 CH 2 F: 1,1,1,2-tetrafluoroethane (HFC-134a) CHF 2 CHF 2 : 1,1,2,2-tetrafluoroethane (HFC-134) CF 3 CHF 2 : 1,1,1,2,2-pentafluoroethane (HFC-125)

[0024] Among these, the fluorocarbon represented by formula (1) is preferably at least one selected from the group consisting of HFC-143a, HFC-143, HFC-134a, and HFC-134, from the viewpoint of minimizing side reactions and suppressing the production of by-products. Furthermore, the fluorocarbon represented by formula (1) is preferably HFC-134a, since one type of fluoroolefin can be obtained with high selectivity.

[0025] (Fluoroolefin represented by formula (2)) In the method for producing a fluoroolefin according to the present disclosure, a fluoroolefin represented by the following formula (2) is obtained as a reaction product: CX 1 X 2 =CX 3 X 4 ...(2) In formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.

[0026] Examples of the fluoroolefin represented by formula (2) include the following compounds: CHF=CH 2 : Fluoroethylene CF 2 =CH 2: 1,1-difluoroethylene (HFO-1132a) CHF=CHF: 1,2-difluoroethylene (HFO-1132(E), HFO-1132(Z)) CHF=CF 2 : Trifluoroethylene (HFO-1123) CF 2 =CF 2 : Tetrafluoroethylene

[0027] Among these, the fluoroolefin represented by formula (2) is preferably at least one selected from the group consisting of HFO-1132, HFO-1132a, and HFO-1123, from the viewpoint of usefulness as a refrigerant composition.

[0028] In particular, in the fluoroolefin production method of the present disclosure, from the viewpoint of allowing the reaction to proceed more selectively, it is preferable that the fluorocarbon is HFC-134a and the fluoroolefin is HFO-1123.

[0029] It should be noted that olefins other than the fluoroolefin of formula (2) may be produced together with the fluoroolefin of formula (2), and the olefins other than the fluoroolefin of formula (2) may include ethylene.

[0030] (Catalyst) In the method for producing a fluoroolefin of the present disclosure, a fluorocarbon represented by formula (1) is brought into contact with a catalyst. The catalyst to be brought into contact with the fluorocarbon contains 65% by mass or more of α-alumina and is produced by ammonia temperature programmed desorption (NH 3 The amount of Lewis acid sites measured by PTFE-TPD is 0.005 to 0.10 mmol / g.

[0031] Alumina is a dehydrated product of aluminum hydroxide, and its properties differ depending on the degree of dehydration and the degree of crystallinity. There are various types of alumina, such as γ-alumina, θ-alumina, and α-alumina, depending on their crystalline structure. γ-alumina and θ-alumina are called activated alumina, and have a higher free energy of formation than α-alumina, making them thermodynamically unstable. α-alumina is a high-temperature stable phase with a high degree of crystallinity, and although it has a small specific surface area, it is thermally stable and has high thermal conductivity. The catalyst used in the method for producing fluoroolefins of the present disclosure contains α-alumina. Compared with other alumina structures, α-alumina has a higher barrier for the conversion of Al—O to Al—F in the presence of hydrogen fluoride, and by using a catalyst containing α-alumina, it is possible to convert AlF 3 It is possible to suppress the generation of AlF 3 The formation of is thought to lead to the deactivation of the catalyst, a decrease in selectivity, etc.

[0032] The presence of α-alumina in the catalyst can be confirmed by the diffraction pattern obtained by X-ray diffraction, in other words, XRD (X-ray diffractometer). A commercially available device can be used for XRD, for example, the "SmartLab" manufactured by Rigaku Corporation. If peaks at d = 26.62, 35.21, 37.85, 43.43, 52.65, and 57.61 Å are present in the diffraction pattern, it can be determined that α-alumina is present. Note that this analysis is performed on the catalyst immediately before contact with fluorocarbon or on a catalyst that has been subjected to the same conditions as the catalyst immediately before contact with fluorocarbon.

[0033] Furthermore, by containing 65% by mass or more of α-alumina in the catalyst, the catalyst has high durability and a decrease in conversion rate is suppressed even during long-term production. The fact that the catalyst contains 65% by mass or more of α-alumina can be confirmed by performing Rietveld analysis on the crystal structure of XRD. Specifically, the peaks obtained by XRD measurement of the catalyst are compared with known peak models derived from each alumina structure, and Rietveld analysis is performed to calculate the mass proportion of each crystal structure.

[0034] The catalyst contains α-alumina in an amount of 65% by mass or more, preferably 70% by mass or more, more preferably 75% by mass or more, even more preferably 80% by mass or more, particularly preferably 85% by mass or more, and may even contain 100% by mass.

[0035] The catalyst may contain a compound other than α-alumina. Examples of compounds other than α-alumina include alumina having a crystal structure different from that of α-alumina and oxides other than alumina. Examples of alumina having a crystal structure different from that of α-alumina include β-alumina, γ-alumina, θ-alumina, η-alumina, boehmite, and gibbsite. Examples of oxides other than alumina include chromium oxide, copper oxide, iron oxide, nickel oxide, magnesium oxide, zinc oxide, and zirconium oxide.

[0036] The catalyst may also contain compounds other than α-alumina, such as aluminum oxide fluoride and aluminum fluoride, which are fluorinated forms of α-alumina.

[0037] α-Alumina may function not only as a catalyst but also as a support while functioning as a catalyst. Furthermore, α-alumina may be supported on a support other than α-alumina. Examples of the support include carbon, β-alumina, γ-alumina, zirconia, silica, and titania.

[0038] The catalyst has an amount of Lewis acid sites measured by an ammonia temperature programmed desorption method of 0.005 to 0.10 mmol / g, preferably 0.005 to 0.05 mmol / g, and more preferably 0.008 to 0.05 mmol / g from the viewpoint of further suppressing a decrease in conversion rate after 100 hours has elapsed.

[0039] The catalyst may be one that has undergone a drying treatment, one that has undergone an activation treatment, one that has undergone both treatments, or one that has not undergone both treatments. The state of the catalyst in the present disclosure is assumed to be the state of the catalyst at the start of the reaction (immediately before the start of the reaction), and when various treatments are performed, the catalyst after the treatment is the subject of measurement of the Lewis acid points. Note that, if the number of acid points does not substantially change even after various treatments are performed, the Lewis acid points may be measured on the catalyst before the treatment.

[0040] The ammonia temperature-programmed desorption method is a method in which ammonia (NH 3 After the ammonia is adsorbed, the temperature is continuously increased at a constant rate, and the amount of ammonia desorbed and the desorption temperature are measured. 3 The amount of acid in the sample can be measured from the amount of NH adsorbed on weak acid sites. 3 is desorbed at low temperatures, and NH adsorbed on the strong acid site 3 Since ammonia is desorbed at high temperatures, the acid strength of the object to be measured can also be measured. Therefore, in the present disclosure, the peak intensity of the amount of ammonia desorbed at temperatures below 200°C is taken as the amount of Brønsted acid sites, and the peak intensity of the amount of ammonia desorbed at temperatures above 200°C is taken as the amount of Lewis acid sites, and a distinction is made between Brønsted acid sites and Lewis acid sites. Note that a Lewis acid site is an acid site that accepts an electron pair from a partner molecule, and a Brønsted acid site is an acid site that donates a proton to a partner molecule.

[0041] Ammonia temperature-programmed desorption (NH 3 The measurement of TPD is carried out using a catalyst analyzer (for example, "BELCAT II" manufactured by MicrotracBEL). In the measurement, the temperature is raised to 810°C at a rate of 10°C / min and held for 10 minutes. Helium is used as the carrier gas at a flow rate of 50 mL / min (sccm).

[0042] Prior to the measurement, the catalyst may be pretreated. As the pretreatment, the following steps 1 to 6 may be carried out in order. Then, the temperature is raised as described above, and NH 3 is desorbed from the catalyst, the desorption temperature and the amount of desorption are measured, and the amount of Lewis acid sites is analyzed. 3 is diluted with He and NH 3 The concentration of is 5.05% by volume. Therefore, the gas composition of the following 5 is: He: 90 + 10 × 0.9495 = 99.495 sccm, NH 3 : 10 x 0.0505 = 0.505 sccm.

[0043]

[0044] The form of the catalyst is not particularly limited, and may be a powder, pellet, or sphere. α-alumina is preferably in the form of a molded body such as a sphere or pellet, from the viewpoints of packing properties when filling a reactor, excellent flowability of reaction gas, and ease of handling when used for about 10 hours. A molded body differs from a powder and is obtained, for example, by placing the powder in a mold and compression molding it.

[0045] (Reaction Conditions) In the fluoroolefin production method of the present disclosure, the feedstock gas only needs to contain the fluorocarbon represented by formula (1), and may contain components other than the fluorocarbon represented by formula (1). The feedstock gas may consist solely of the fluorocarbon represented by formula (1), or may contain isomers, disproportionation products, impurities, and the like obtained during the production of the fluorocarbon represented by formula (1). From the viewpoint of suppressing side reactions and catalyst deactivation, the feedstock gas preferably contains an inert gas such as nitrogen, argon, helium, carbon dioxide, or octafluorocyclobutane in addition to the fluorocarbon represented by formula (1). The inert gas can dilute the target product and the by-product hydrogen fluoride. The content of the fluorocarbon represented by formula (1) is preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 75 mol% or more, and particularly preferably 80 mol% or more, based on the total amount of the feedstock gas.

[0046] The method for producing a fluoroolefin of the present disclosure may be carried out in a gas phase or a liquid phase. Since the fluorocarbon represented by formula (1) is a gas at room temperature, it is preferable to contact the fluorocarbon with the catalyst in a gas phase.

[0047] The reactor in which the fluorocarbon is brought into contact with the catalyst may be any reactor capable of withstanding the temperatures and pressures described below, and its shape and structure are not particularly limited. Examples of reactors include cylindrical vertical reactors. Examples of reactor materials include glass, stainless steel, iron, nickel, and alloys containing iron or nickel as a main component. The reactor may be equipped with a heating means, such as an electric heater, for heating the interior of the reactor.

[0048] The catalyst may be accommodated in any of the forms of a fixed bed, a fluidized bed, or a moving bed. In the case of a fixed bed, it may be either a horizontal fixed bed or a vertical fixed bed.

[0049] The reaction may be carried out in a flow manner or a batch manner.

[0050] Fixed-bed reactors are filled with various catalyst-supported molded bodies to reduce pressure loss in the reaction fluid. Similar to fixed-bed reactors, a catalyst is packed, moved by gravity, and then removed from the bottom of the reactor for regeneration. This is called a moving bed. In fluidized-bed reactors, the catalyst bed is operated in a way that makes it appear as if it were a fluid, and the catalyst particles are suspended in the reaction fluid and move within the reactor. Fixed-bed reactors are preferred because of the wide range of catalyst shape options and the ability to minimize catalyst wear. Fixed-bed reactors include tubular and tank-type reactors, with tubular reactors being preferred due to their ease of reaction temperature control. Furthermore, multi-tube heat exchange reactors, in which multiple small-diameter reaction tubes are arranged in parallel and a heat transfer medium is circulated outside, can be used. When multiple reactors are arranged in series, multiple catalyst layers are installed. At least one catalyst layer is sufficient, but two or more are also acceptable.

[0051] From the viewpoint of improving the conversion rate, the fluoroolefin production method of the present disclosure is preferably carried out in a flow system using a fixed-bed reactor (particularly a vertical fixed-bed reactor).

[0052] From the viewpoint of improving industrial productivity, the feed rate of fluorocarbon to the catalyst (raw material feed rate) is 350 kg / hr / m 3 More than 375 kg / hr / m is preferable. 3 More preferably, 400 kg / hr / m or more 3 From the viewpoint of maintaining a certain conversion rate or higher, the raw material supply rate is more preferably 3000 kg / hr / m 3 Preferably less than 2500 kg / hr / m 3 More preferably, 2000 kg / hr / m or less 3 The amount of raw material supplied is more preferably: 3The amount of fluorocarbon (raw material) supplied per unit time (kg / hr) is preferably in the above range, and the amount of fluorocarbon that comes into contact with the catalyst by being supplied to the catalyst is preferably in the above range.

[0053] In the fluoroolefin production method of the present disclosure, the fluorocarbon and the catalyst are preferably contacted at a temperature of 300 to 800° C., more preferably at a temperature of 400 to 700° C., and even more preferably at a temperature of 400 to 600° C. When the contact temperature is 300° C. or higher, the conversion rate of the fluoroolefin is improved. On the other hand, when the contact temperature is 800° C. or lower, decomposition of the fluoroolefin can be suppressed.

[0054] When the contact temperature is 300° C. or higher, the reaction proceeds appropriately. On the other hand, when the contact temperature is 800° C. or lower, the selectivity decreases due to cleavage of the carbon-carbon bonds of the raw material, and the disproportionation reaction of the product (unsaturated compound) is suppressed.

[0055] Since the dehydrofluorination reaction is generally an endothermic reaction, a decrease in the conversion rate can be suppressed by appropriately maintaining the reaction temperature. As the reaction temperature in the catalyst layer increases, the conversion rate of the raw material increases. Therefore, it is preferable to maintain the reaction temperature in the catalyst layer at a desired temperature so as to maintain a high conversion rate. One way to maintain the reaction temperature in the catalyst layer at a desired temperature is, for example, to heat the catalyst layer externally with a heat medium or the like. Catalysts typically deteriorate over time as the reaction progresses. Even when a decrease in the conversion rate of the raw material occurs due to catalyst deterioration, the decrease in the conversion rate can be suppressed by heating the catalyst layer with a heat medium or the like and appropriately maintaining or increasing the reaction temperature. When maintaining or increasing the temperature of the catalyst layer, it is preferable to limit the temperature increase to 50° C. or less in order to suppress rapid catalyst deterioration.

[0056] At the start of the reaction, the reaction zone begins at the inlet of the raw material gas. As the catalyst at the inlet of the raw material gas deteriorates over time as the reaction progresses, the reaction zone moves downstream in the gas flow direction. Because the low-temperature product gas generated in the reaction zone flows into the vicinity of the downstream side of the reaction zone, the vicinity of the downstream side is usually the coldest in the catalyst layer. In the present disclosure, the temperature of this lowest temperature region of the catalyst layer is referred to as the "lowest temperature of the catalyst layer." The temperature further downstream from the vicinity of the downstream side usually increases from the lowest temperature of the catalyst layer as it moves away from the reaction zone.

[0057] In the fluoroolefin production method of the present disclosure, the fluorocarbon-containing raw material gas may be supplied to the reactor at room temperature. However, it is preferable to appropriately heat (preheat) the raw material gas before supplying it to the reactor. When preheating is performed, it is preferable to heat the raw material gas to a temperature of 80 to 600°C before supplying it to the reactor. Preheating to 80°C or higher makes it difficult for the internal temperature of the reactor to decrease, making it easier to achieve the set conversion rate. Furthermore, preheating to 600°C or lower makes it difficult for the internal temperature of the reactor to increase, suppressing undesirable reactions and improving selectivity.

[0058] The dehydrofluorination reaction in the present disclosure is a reaction in which the number of molecules increases, and therefore increasing the pressure makes the forward reaction unfavorable. The pressure when contacting the fluorocarbon with the catalyst is not particularly limited, but from the viewpoint of improving the conversion rate, it is preferably −0.05 to 2 MPa, more preferably −0.01 to 1 MPa, and even more preferably atmospheric pressure to 0.5 MPa. In the present disclosure, pressure means gauge pressure.

[0059] The contact time (seconds) between the fluorocarbon and the catalyst is preferably 0.5 to 100.0 seconds, more preferably 1.0 to 50.0 seconds, and even more preferably 2.0 to 20.0 seconds.

[0060] The contact time (seconds) is calculated using the following formula: Contact time (seconds) = [length of catalyst packed in reactor (cm)] / [linear velocity (cm / second)] The linear velocity means the speed at which the fluorocarbon passes through the catalyst per unit time.

[0061] Furthermore, the contact time (g sec / mL) between the fluorocarbon and the catalyst is preferably 1 to 200 g sec / mL, more preferably 5 to 175 g sec / mL, even more preferably 7 to 150 g sec / mL, and particularly preferably 10 to 125 g sec / mL. When the contact time (g sec / mL) is 1 g sec / mL or more, the conversion rate is improved. When the contact time (g sec / mL) is 200 g sec / mL or less, equipment costs can be reduced.

[0062] The contact time (g·sec / mL) is calculated using the following formula: Contact time (g·sec / mL) = [Catalyst loading (g)] / [Fluorocarbon flow rate (mL / sec)]

[0063] From the viewpoint of further suppressing a decrease in conversion, it is preferable to contact the fluorocarbon with the catalyst in the presence of an inert gas. The inert gas is preferably at least one selected from the group consisting of nitrogen, helium, argon, octafluorocyclobutane, and carbon dioxide. Among these, nitrogen is preferred as the inert gas. In the present disclosure, the inert gas refers to a gas that is inert to reaction with the raw material.

[0064] The molar ratio of the fluorocarbon to the inert gas in the gas phase is preferably 0.1 to 30, more preferably 0.5 to 25.

[0065] From the viewpoint of further suppressing a decrease in conversion, it is preferable that the fluorocarbon and the catalyst are contacted in the gas phase in the presence of water, and the water concentration is less than 500 ppm by mass relative to the total amount of the feed gas containing the fluorocarbon. When the dehydrofluorination reaction is carried out in the gas phase in the presence of water, water is adsorbed to the Lewis acid sites on the surface of the catalyst. It is presumed that by making the water concentration less than 500 ppm by mass relative to the total amount of the feed gas containing the fluorocarbon, the Lewis acid sites on the surface of the catalyst are prevented from collapsing and forming a structure similar to Bronsted acid sites, thereby suppressing a decrease in catalytic activity. It is presumed that this increases the conversion and enables the target product to be obtained with high selectivity. From the viewpoint of further improving the conversion and obtaining the target compound with even higher selectivity, the water concentration is preferably 300 ppm by mass or less, more preferably 100 ppm by mass or less, even more preferably 50 ppm by mass or less, and particularly preferably 10 ppm by mass or less. A lower water concentration is preferable, but from the viewpoint of the cost of dehydration treatment of fluorocarbon and inert gas and the difficulty of process control, the water concentration is preferably 0.5 ppm by mass or more, and more preferably 1 ppm by mass or more.

[0066] A common method for measuring the water concentration is to use a commercially available Karl Fischer moisture meter.

[0067] The water concentration is the water content in the feed gas when the fluorocarbon is brought into contact with the catalyst. Note that the water concentration may be replaced with the water content in the feed gas before it is introduced into the reactor.

[0068] The fluoroolefin production method of the present disclosure preferably further includes a step of drying the catalyst before contacting the catalyst with the fluorocarbon. Drying the catalyst removes water contained in the catalyst, increasing its reactivity with the fluorocarbon and improving the conversion rate.

[0069] The method for drying the catalyst is not particularly limited, and the catalyst may be dried before being packed into the reactor, or may be dried after being packed into the reactor. Drying the catalyst after being packed into the reactor is preferred because it allows the reactor to be preheated in addition to drying the catalyst. Specifically, it is preferred to dry the catalyst by packing the catalyst into the reactor and heating the reactor while flowing an inert gas through it.

[0070] In the fluoroolefin production method of the present disclosure, hydrogen fluoride is produced as a by-product. Hydrogen fluoride has the function of fluorinating oxides contained in the catalyst and strengthening its acidity. Therefore, it is preferable to reduce the concentration of hydrogen fluoride. Reducing the hydrogen fluoride concentration maintains selectivity, suppresses catalyst deactivation, and suppresses a decrease in reaction activity due to a decrease in the specific surface area of ​​the catalyst. One method for reducing the hydrogen fluoride concentration is to dilute it with an inert gas. Since the use of an inert gas increases the energy load in the purification process after the reaction, it is preferable to appropriately control the use of the inert gas. It is preferable to keep the hydrogen fluoride concentration during the reaction at 15 mol% or less. From the viewpoint of extending the catalyst life, the hydrogen fluoride concentration is more preferably 13 mol% or less, even more preferably 10 mol% or less, particularly preferably 8 mol% or less, and most preferably 7 mol% or less. Furthermore, from the viewpoints of productivity and energy load in the purification step, the concentration of hydrogen fluoride is preferably 0.5 mol % or more, more preferably 0.8 mol % or more, even more preferably 1.0 mol % or more, particularly preferably 1.3 mol % or more, and most preferably 1.5 mol % or more.

[0071] The fluoroolefin production method of the present disclosure is preferably carried out in the presence of an oxidizing agent. The oxidizing agent is preferably oxygen, chlorine, bromine, or iodine, from the viewpoints of high conversion and high selectivity for obtaining the target compound. Of these, oxygen is more preferred as the oxidizing agent. In the present disclosure, the concentration of the oxidizing agent is preferably 0.01 to 21 mol% relative to the raw material gas. The concentration of the oxidizing agent is more preferably 1 to 20 mol%, even more preferably 5 to 18 mol%, and particularly preferably 7.5 to 16 mol%, relative to the raw material compound, from the viewpoints of further improving the conversion and obtaining the target compound with higher selectivity.

[0072] In the present disclosure, the conversion rate refers to the ratio (mol %) of the total molar amount of compounds other than the raw material compounds contained in the gas effluent from the reactor outlet to the molar amount of the raw material compounds supplied to the reactor. Generally, a higher conversion rate is preferable from the viewpoint of productivity. However, in the dehydrofluorination reaction of the present disclosure, it is preferable to appropriately control the conversion rate. When the conversion rate is controlled, the concentration of hydrogen fluoride produced in the gas phase is reduced, and it is thought that deactivation of the catalyst by hydrogen fluoride is suppressed. A method of diluting the gas phase with an inert gas is also possible, but the use of an inert gas increases the energy load in the purification process after the reaction, so the use of an excessive inert gas is not preferable. From the viewpoint of extending the catalyst life, it is preferable to suppress the hydrogen fluoride concentration during the reaction to 15 mol % or less.

[0073] From the above viewpoint, it is preferable to select operating conditions such that the conversion rate after 10 hours from the contact of the fluorocarbon with the catalyst is 7 to 13%, and it is more preferable to select operating conditions such that the conversion rate after 10 hours is 7.5 to 12.5%.

[0074] It is preferable to select operating conditions that result in a conversion rate of 4.0% or higher 50 hours after contacting the fluorocarbon with the catalyst, more preferably 4.5% or higher, even more preferably 5.0% or higher, and most preferably 5.5% or higher.

[0075] It is preferable to select operating conditions that result in a conversion rate of 1.0% or higher 100 hours after contacting the fluorocarbon with the catalyst, more preferably 2.0% or higher, even more preferably 3.0% or higher, and most preferably 4.0% or higher.

[0076] The conversion maintenance rate, which is the ratio of the conversion rate after 50 hours to the conversion rate after 10 hours, is preferably 69% or more. The conversion maintenance rate after 100 hours from the contact of the fluorocarbon with the catalyst is preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more.

[0077] In particular, in the fluoroolefin production method of the present disclosure, by using HFC-134a as the fluorocarbon, the conversion rate after 10 hours does not become too high and catalyst deactivation is suppressed.Furthermore, by using a catalyst containing 65 mass% or more of α-alumina and having an amount of Lewis acid sites of 0.005 to 0.10 mmol / g as measured by ammonia temperature programmed desorption spectrometry, the conversion rate after 10 hours does not become too high and catalyst deactivation is suppressed.

[0078] In the present disclosure, selectivity refers to the ratio (mol %) of the molar amount of the target product contained in the reactor outlet gas to the total molar amount of compounds other than the raw material compounds contained in the reactor outlet gas. A selectivity of 100% is preferable because a post-reaction purification step is unnecessary, but side reactions may occur in the reaction temperature range required to obtain a desired conversion. A higher selectivity is preferable because it reduces the amount of waste, the energy load in the post-reaction purification step, and the catalyst life can be extended. The selectivity 50 hours after contacting the fluorocarbon with the catalyst is preferably 90% or more, more preferably 93% or more, and even more preferably 95% or more. In particular, in the fluoroolefin production method of the present disclosure, HFO-1123 can be obtained with high selectivity by using HFC-134a as the fluorocarbon.

[0079] Examples of compounds other than the raw material compounds and the target product contained in the reactor outlet gas include hydrogen fluoride, carbon monoxide, carbon dioxide, water, etc. For example, when HFC-134a is used as the fluorocarbon raw material compound, examples of other compounds include HFC-134, 1,1-difluoroethylene (VdF), E / Z-1,2-difluoroethylene (HFO-1132(E) / (Z)), etc.

[0080] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure. Examples 1 to 6 are examples, and Examples 7 and 8 are comparative examples.

[0081] Example 1 1 mL of α-alumina (product name "α-alumina, average particle size 0.5 μm", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was weighed out and used as a catalyst. A stainless steel (SUS304) reaction tube having an inner diameter of 1.02 cm and a length of 30 cm was packed with the catalyst and placed in a tubular electric furnace. The catalyst-packed section was heated to 475°C in the tubular furnace while flowing nitrogen, thereby dehydrating the catalyst. Thereafter, a 0.1 / 1 (mol / mol) mixed gas of nitrogen / HFC-134a was passed through the tube for a contact time of 4.7 seconds, thereby carrying out a dehydrogenation reaction to produce HFO-1123. The water concentration in the 0.1 / 1 (mol / mol) mixed gas of nitrogen / HFC-134a was measured using a Karl Fischer moisture content analyzer and was found to be 5 ppm by mass.

[0082] [Examples 2 to 8] In Examples 2 to 8, the HF removal reaction was carried out in the same manner as in Example 1, except that the catalyst was changed and the various conditions were changed to the values ​​shown in Table 2. The catalysts used in Examples 2 to 8 are described below.

[0083] Example 2 α-alumina (product name "SA52124", manufactured by Saint-Gobain) was used as a catalyst.

[0084] Example 3 α-alumina (product name "SA52238", manufactured by Saint-Gobain) was used as a catalyst.

[0085] Example 4 α-alumina (product name "FGL-40", manufactured by Iwatani Chemical Industries, Ltd.) was used as a catalyst.

[0086] Example 5 α-alumina (product name "LT303D", manufactured by Nippon Light Metal Co., Ltd.) was used as a catalyst.

[0087] Example 6 α-alumina (product name "C500", manufactured by Nippon Light Metal Co., Ltd.) was used as a catalyst.

[0088] Example 7 γ-alumina (product name "N612N", manufactured by JGC Catalysts and Chemicals) was used as a catalyst.

[0089] Example 8 A catalyst containing θ-alumina as the main component and α-alumina as a part thereof (product name "SA3177", manufactured by Saint-Gobain) was used.

[0090] The Lewis acid sites of each catalyst were determined by NH 3 The Lewis acid point was measured by TPD under the conditions described above. The Lewis acid point was measured before the catalyst was packed into the reaction tube.

[0091] XRD measurement was performed on the catalyst of Example 6 using a Rigaku Corporation X-ray diffractometer "SmartLab." The resulting diffraction pattern is shown in FIG. 1. In the diffraction pattern of FIG. 1, the presence of peaks at 2θ = 26.62, 35.21, 37.85, 43.43, 52.65, and 57.61 Å confirmed the presence of α-alumina. Furthermore, the presence of peaks at 2θ = 31.51, 32.78, 36.74, 38.87, 44.86, and 67.40 Å confirmed the presence of θ-alumina. Then, Rietveld analysis was performed on the diffraction peaks of each crystalline phase observed above, confirming that the α-alumina content in the catalyst was 65.2 mass% and the θ-alumina content was 34.8 mass%. Similarly, the α-alumina contents of the catalysts of Examples 1 to 5 and 7 to 8 were determined by XRD measurement.

[0092] The contact time (seconds) was calculated using the following formula: Contact time (seconds) = [length of catalyst packed in reactor (cm)] / [linear velocity (cm / second)] The linear velocity refers to the speed at which the fluorocarbon passes through the catalyst per unit time.

[0093] The contact time (g·sec / mL) was calculated using the following formula: Contact time (g·sec / mL) = [catalyst loading (g)] / [fluorocarbon flow rate (mL / sec)]

[0094] In the reactions of Examples 1 to 8, the product gas (hereinafter also referred to as "reactor outlet gas") taken out from the outlet of the reactor 10 hours and 50 hours after the start of the reaction was analyzed by gas chromatography. Specifically, a column (product name "DB-1301", manufactured by Agilent, length 60 m, inner diameter 0.25 mm, film thickness 1 μm) was attached to a gas chromatograph (product name "GC6850", manufactured by Agilent) and the analysis was performed. The conversion rate of HFC-134a and the selectivity of HFO-1123 were calculated using the molar amount calculated from the area ratio (GCArea%) of the reactor outlet gas.

[0095] (Conversion rate of HFC-134a) The molar amount M of HFC-134a fed to the reactor 134a The conversion rate of HFC-134a (%) is calculated by the following formula: M1 / M 134a ) x 100

[0096] (Selectivity of HFO-1123) The molar amount M of HFO-1123 contained in the reactor outlet gas relative to the total molar amount M1 of compounds other than HFC-134a contained in the reactor outlet gas is 1123 The selectivity of HFO-1123 (%) = (M 1123 / M1) x 100

[0097]

[0098] As shown in Table 2, Examples 1 to 6 include a step of contacting a fluorocarbon represented by formula (1) with a catalyst to produce a fluoroolefin represented by formula (2). The catalyst contains 65 mass% or more of α-alumina and has a Lewis acid site content of 0.005 to 0.10 mmol / g as measured by ammonia temperature programmed desorption. Therefore, it was found that the conversion rate was higher than that of conventional catalysts and that the decrease in conversion rate was suppressed during long-term production. On the other hand, Example 7, which did not contain α-alumina and had a Lewis acid site content of more than 0.10 mmol / g, had a significantly lower conversion rate than Examples 1 to 6. Furthermore, Example 8, which contained α-alumina but had a Lewis acid site content of more than 0.10 mmol / g, had a conversion rate after 10 hours comparable to that of Examples 1 to 6, but showed a significant decrease in conversion rate during long-term production of 50 hours.

[0099] Furthermore, as shown by the results of Examples 1 to 6, the process includes a step of producing a fluoroolefin represented by formula (2) by contacting a fluorocarbon represented by formula (1) with a catalyst, and the conversion rate 10 hours after contacting the fluorocarbon with the catalyst is 7 to 13%, which shows that a decrease in conversion rate is suppressed during long-term production.

[0100] [Examples 9 and 10] Furthermore, for the catalysts used in Examples 4 and 5, HF desorption reactions were carried out in the same manner as in Example 1, except that the various conditions were changed to the values ​​shown in Table 3, to obtain Examples 9 and 10. The conversion of HFC-134a and the selectivity of HFO-1123 were calculated 10 hours and 100 hours after the start of the reaction.

[0101]

[0102] As shown in Table 3, in Example 9, in which the amount of Lewis acid sites was within the range of 0.008 to 0.05 mmol / g, it was found that the decrease in conversion rate was more effectively suppressed in the production for a longer period of time, such as 100 hours, than in Example 10, in which the amount of Lewis acid sites was outside this range.

[0103] The raw material supply rate in this example was 1257 kg / hr / m 3 and the raw material supply rate in Non-Patent Document 1 is 307 kg / h / m 3This is about four times larger than the above, and is a condition that results in a low conversion rate. However, even when the amount of raw material supplied is increased in this manner, it is clear that, when a process including a step of contacting a fluorocarbon represented by formula (1) with a catalyst to produce a fluoroolefin represented by formula (2), in which the catalyst contains 65 mass % or more of α-alumina and the amount of Lewis acid sites measured by ammonia temperature programmed desorption is 0.005 to 0.10 mmol / g, the conversion rate is excellent and a decrease in the conversion rate over a long period of production is suppressed.

[0104] The disclosure of Japanese Patent Application No. 2023-072720 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A method for producing a fluoroolefin, comprising the step of contacting a fluorocarbon represented by the following formula (1) with a catalyst to produce a fluoroolefin represented by the following formula (2), wherein the catalyst contains 65 mass% or more of α-alumina and has an amount of Lewis acid sites of 0.005 to 0.10 mmol / g as measured by ammonia temperature programmed desorption method. 1 X 2 F-CX 3 X 4 H ... (1) CX 1 X 2 = C.X. 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.

2. The method for producing a fluoroolefin according to claim 1, wherein the amount of the Lewis acid sites is 0.005 to 0.05 mmol / g.

3. The method for producing a fluoroolefin according to claim 1, wherein the amount of the Lewis acid sites is 0.008 to 0.05 mmol / g.

4. The amount of the fluorocarbon fed to the catalyst is 350 kg / hr / m 3 The method for producing a fluoroolefin according to claim 1, 5. The method for producing a fluoroolefin according to claim 1 or 4, wherein the fluorocarbon is at least one selected from the group consisting of 1,1,1-trifluoroethane, 1,1,2-trifluoroethane, 1,1,2,2-tetrafluoroethane, and 1,1,1,2-tetrafluoroethane.

6. The method for producing a fluoroolefin according to claim 1 or 4, wherein the fluoroolefin is at least one selected from the group consisting of 1,2-difluoroethylene, 1,1-difluoroethylene, and trifluoroethylene.

7. A method for producing a fluoroolefin according to claim 1 or 4, wherein the fluorocarbon is 1,1,1,2-tetrafluoroethane and the fluoroolefin is trifluoroethylene.

8. The method for producing a fluoroolefin according to claim 1 or 4, wherein the fluorocarbon is contacted with the catalyst at a temperature of 300 to 800°C.

9. The method for producing a fluoroolefin according to claim 1 or 4, wherein the fluorocarbon and the catalyst are contacted in the presence of an inert gas, and the inert gas is at least one selected from the group consisting of nitrogen, helium, argon, octafluorocyclobutane, and carbon dioxide.

10. The method for producing a fluoroolefin according to claim 1 or 4, further comprising the step of drying the catalyst prior to contacting the fluorocarbon with the catalyst.

11. The method for producing a fluoroolefin according to claim 1 or 4, wherein the fluorocarbon and the catalyst are contacted in a gas phase in the presence of water, and the concentration of the water is less than 500 ppm by mass based on the total amount of the feed gas containing the fluorocarbon.

12. A method for producing a fluoroolefin, comprising the step of contacting a fluorocarbon represented by the following formula (1) with a catalyst to produce a fluoroolefin represented by the following formula (2), wherein the conversion rate 10 hours after contacting the fluorocarbon with the catalyst is 7.0 to 13.0%, and the conversion rate maintenance rate, which is the ratio of the conversion rate after 50 hours to the conversion rate after 10 hours, is 69% or more. CX 1 X 2 F-CX 3 X 4 H ... (1) CX 1 X 2 = C.X. 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.

Citation Information

Patent Citations

  • Catalyst for preparing trifluoroethylene or vinyl fluoride and preparation method thereof

    CN103071516A

  • Method for co-production of trifluoroethylene and hydrogen fluoride

    CN103288589A

  • Synthesis of perfluoroolefins

    JP2004504283A

  • Manufacturing method of fluoroolefin

    JP2019196347A

  • Fluoroolefin production method

    WO2024057657A1

Cited By

  • Method for producing alkene halogens

    JP7925445B1