Optical member, lens unit, and method for manufacturing optical member

The hydrophilic lens with a specific titanium dioxide particle size distribution and antireflection film restores hydrophilicity upon dirt adhesion, addressing the maintenance of hydrophilicity and visibility issues in outdoor applications by using UV irradiation and reducing reflectance.

WO2024225000A1PCT designated stage expired Publication Date: 2024-10-31NIDEC CORP(JP)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014205
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-08
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing hydrophilic lenses fail to maintain hydrophilicity over a long period due to dirt adhesion, and UV irradiation does not sufficiently restore the hydrophilic function, leading to reduced visibility in outdoor applications.

Method used

A hydrophilic lens with a translucent member and a hydrophilic layer containing aggregated titanium dioxide particles, where the primary particles have an average diameter of 5-20 nm and secondary particles have an average diameter of 15-100 nm, along with an antireflection film and a coating layer, is used. The hydrophilic layer is formed through a coating and drying process, and the lens is designed to restore hydrophilicity by UV irradiation when dirt adheres.

Benefits of technology

The lens effectively maintains hydrophilicity and suppresses ghost and flare phenomena, ensuring improved visibility and wear resistance by restoring hydrophilicity through UV exposure and reducing reflectance to less than 1.5% in the visible light range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014205_31102024_PF_FP_ABST
    Figure JP2024014205_31102024_PF_FP_ABST
Patent Text Reader

Abstract

An optical member 100 includes a light-transmissive member 10 and a hydrophilic layer 20. The light-transmissive member 10 transmits visible light. The hydrophilic layer 20 covers the light-transmissive member 10. The hydrophilic layer 20 contains secondary particles obtained by aggregating a plurality of primary particles of titanium dioxide. The average particle diameter of the primary particles of titanium dioxide is 5-20 nm. The average particle diameter of the secondary particles of titanium dioxide is 15-100 nm. The thickness of a coating layer is preferably 5-20 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Optical member, lens unit, and method of manufacturing optical member

[0001] The present disclosure relates to an optical member, a lens unit, and a method for manufacturing an optical member.

[0002] Visibility is impaired by water droplets on window glass of buildings or automobiles exposed to outdoor wind and rain. One solution to this problem is to make the surface of the window glass hydrophilic. This turns the adhering water into a film, preventing the adhesion of water droplets and ensuring visibility on the window glass.

[0003] However, the surface of hydrophilic materials is prone to the adhesion of organic contaminants, such as those from automobile exhaust fumes or factory smoke. When organic contaminants adhere to the surface, water droplets adhere to the surface, significantly reducing visibility.

[0004] Therefore, a hydrophilic lens including a glass substrate and a hydrophilic layer formed on the glass substrate has been disclosed (for example, Patent Document 1). In the hydrophilic lens of Patent Document 1, the hydrophilic layer contains a silicate material in which fine particles having photocatalytic activity are dispersed, the film thickness of the hydrophilic layer is 30 nm or less, the average particle diameter of the fine particles is 30 nm or less, and the arithmetic mean roughness Ra of the surface of the hydrophilic layer is 0.7 to 1.9 nm.

[0005] Japanese Patent Publication No. 2018-77260

[0006] However, the hydrophilic lens of Patent Document 1 was unable to maintain its hydrophilicity for a long period of time. For example, when the hydrophilic function was reduced due to the adhesion of dirt, the hydrophilic function could not be fully restored even when irradiated with sunlight containing ultraviolet rays.

[0007] The present disclosure has been made in consideration of the above-mentioned problems, and its purpose is to provide an optical element, a lens unit, and a method for manufacturing an optical element that can fully restore hydrophilic function by irradiating with ultraviolet light when the hydrophilic function is reduced due to the adhesion of dirt.

[0008] An exemplary optical member of the present disclosure includes a translucent member and a hydrophilic layer. The translucent member transmits visible light. The hydrophilic layer covers the translucent member. The hydrophilic layer contains secondary particles formed by agglomeration of a plurality of titanium dioxide primary particles. The average particle size of the titanium dioxide primary particles is 5 nm or more and 20 nm or less. The average particle size of the titanium dioxide secondary particles is 15 nm or more and 100 nm or less.

[0009] An exemplary lens unit of the present disclosure includes the optical member described above.

[0010] An exemplary method for manufacturing an optical member according to the present disclosure includes a coating step and a drying step. In the coating step, a hydrophilic material is coated. In the drying step, the hydrophilic material is dried to form a hydrophilic layer. The hydrophilic material contains a plurality of primary particles of titanium dioxide. The primary particles of titanium dioxide have an average particle size of 5 nm or more and 20 nm or less. The hydrophilic layer contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide. The secondary particles of titanium dioxide have an average particle size of 15 nm or more and 100 nm or less.

[0011] According to the exemplary embodiment of the present disclosure, for example, when the hydrophilic function is reduced due to the adhesion of dirt, the hydrophilic function can be sufficiently restored by irradiating with ultraviolet light.

[0012] Fig. 1 is a schematic diagram showing an example of an optical unit according to the present embodiment, and Fig. 2 is a schematic diagram showing an example of an optical member according to the present embodiment.

[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the drawings, identical or corresponding parts are designated by the same reference numerals, and descriptions thereof will not be repeated. The dimensions, shapes, and dimensional relationships between components in the drawings are not necessarily identical to the actual dimensions, shapes, and dimensional relationships between components. In particular, the thickness ratios and curvatures of the hydrophilic layer and the translucent member in the drawings may differ significantly from those in reality.

[0014] In this specification, "thickness" refers to the length of an optical member in the optical axis direction. The "outside" of an optical member refers to the direction from the light-transmitting member toward the hydrophilic layer. The "inside" of an optical member refers to the direction from the hydrophilic layer toward the light-transmitting member.

[0015] The optical member according to this embodiment is suitable, for example, as an optical member used in an optical unit including one or more optical members (particularly an optical unit used outdoors). The optical member according to this embodiment is particularly suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle. FIG. 1 is a schematic diagram showing an example of an optical unit according to this embodiment. As shown in FIG. 1, an optical unit 1000 includes an optical member 100. The optical unit is an example of a "lens unit."

[0016] The static contact angle of the surface of the optical element 100 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and particularly preferably 10.0° or less. Hereinafter, the static contact angle with pure water may be simply referred to as the "contact angle." Note that the contact angle of the surface of the optical element according to this embodiment is a value measured in an environment at a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0017] Furthermore, the maximum reflectance of the optical element 100 for light with a wavelength of 480 nm or more and 780 nm or less is preferably 1.5% or less, and more preferably 1.0% or less. The optical element 100 according to this embodiment can suppress the occurrence of image defects known as ghost phenomena and flare phenomena as the maximum reflectance described above decreases. In particular, the lower the maximum reflectance described above, the more effectively the ghost phenomenon can be suppressed. When the maximum reflectance described above is 1.5% or less, the ghost phenomenon can be suppressed. When the maximum reflectance described above is 1.0% or less, the ghost phenomenon can be more effectively suppressed. Note that light with a wavelength of 480 nm or more and 780 nm or less corresponds to light in the visible light region.

[0018] An example of the optical member 100 according to this embodiment will be described below with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the optical member 100 according to this embodiment. The optical member 100 includes a light-transmitting member 10, a hydrophilic layer 20, and an anti-reflection film 30.

[0019] <Light-Transmitting Member> The light-transmitting member 10 has light-transmitting properties. That is, the light-transmitting member 10 transmits visible light. The light-transmitting member 10 may be transparent or translucent. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0020] The light-transmitting member 10 functions as, for example, a lens (specifically, for example, a biconvex lens, a biconcave lens, a plano-convex lens, a plano-concave lens, a convex meniscus lens, or a concave meniscus lens). In this specification, when the light-transmitting member 10 is a lens, the lens surface of the light-transmitting member 10 may be spherical or aspherical. The radius of curvature of the lens surface of the light-transmitting member 10 is preferably 9 mm or more and 16 mm or less.

[0021] <Hydrophilic Layer> The hydrophilic layer 20 covers the light-transmitting member 10. Specifically, the hydrophilic layer 20 is disposed on the anti-reflection film 30. The hydrophilic layer 20 has hydrophilic properties.

[0022] The thickness of the hydrophilic layer 20 is preferably 20 nm to 200 nm, more preferably 30 nm to 100 nm. If the thickness of the hydrophilic layer 20 is less than 20 nm, the hydrophilicity recovery function tends to be insufficient. If the thickness of the hydrophilic layer 20 is more than 200 nm, the transmittance to visible light tends to be insufficient.

[0023] In the present specification, "thickness" may be determined using a stylus-type step gauge. Specifically, a sharp needle is traced across the surface to measure the step between areas with and without a layer (film). Steps are measured at three arbitrary locations, and the average value of the step differences at the three locations is taken as the "thickness."

[0024] The hydrophilic layer 20 contains secondary particles formed by aggregation of multiple titanium dioxide primary particles. Titanium dioxide has a photocatalytic function. For example, when the optical element 100 is used for a long period of time, dirt accumulates on the optical element 100, reducing the hydrophilic function. When the optical element 100 is irradiated with ultraviolet light (sunlight), the dirt is broken down and the hydrophilic property can be restored.

[0025] The average particle size of the primary particles of titanium dioxide is 5 nm or more and 20 nm or less, and preferably 5 nm or more and 10 nm or less. If the average particle size of the primary particles of titanium dioxide is less than 5 nm, sufficient hydrophilicity cannot be maintained. If the average particle size of the primary particles of titanium dioxide is more than 20 nm, sufficient transmittance to visible light cannot be obtained, or a uniform film cannot be formed.

[0026] In the present specification, the "average particle size of primary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 primary particles that can be observed in their entirety, the maximum diameter and the minimum diameter of each primary particle are measured, and the average value of the maximum diameter and the minimum diameter is defined as the particle size of the single primary particle. The average value of the particle sizes of each of the 50 primary particles is defined as the "average particle size of primary particles."

[0027] Examples of titanium dioxide include anatase type titanium dioxide, rutile type titanium dioxide, and brookite type titanium dioxide. From the viewpoint of photocatalytic activity, anatase type titanium dioxide is preferred.

[0028] The average particle size of the secondary particles of titanium dioxide is 15 nm or more and 100 nm or less, and preferably 20 nm or more and 60 nm or less. If the average particle size of the secondary particles of titanium dioxide is less than 15 nm, the hydrophilicity of the hydrophilic layer 20 cannot be sufficiently restored. If the average particle size of the secondary particles of titanium dioxide is more than 100 nm, sufficient transmittance to visible light cannot be obtained.

[0029] In the present specification, the "average particle size of secondary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 secondary particles for which the entire particle can be observed, the maximum diameter and minimum diameter of each secondary particle are measured, the average value of the maximum diameter and minimum diameter is defined as the particle size of the single secondary particle, and the average value of the particle diameters of each of the 50 secondary particles is defined as the "average particle size of secondary particles."

[0030] The content of titanium dioxide in the hydrophilic layer 20 is preferably 50% by mass or more and 70% by mass or less. By setting the content of titanium dioxide to 50% by mass or more and 70% by mass or less, the hydrophilicity of the hydrophilic layer 20 can be more effectively restored and an increase in reflectance can be more effectively suppressed.

[0031] As described above with reference to FIG. 1 , in this embodiment, the hydrophilic layer 20 contains secondary particles of a predetermined size formed by aggregation of primary particles of a predetermined size. Therefore, when the hydrophilic function is reduced due to the adhesion of dirt, the hydrophilic function can be sufficiently restored by irradiating the hydrophilic layer with ultraviolet light.

[0032] Preferably, the hydrophilic layer 20 further contains tetraethoxysilane, which further improves the abrasion resistance of the optical member 100. The hydrophilic layer 20 may further contain silicon dioxide.

[0033] <Anti-reflection film> The anti-reflection film 30 covers the light-transmitting member 10. The anti-reflection film 30 is disposed between the light-transmitting member 10 and the hydrophilic layer 20. The anti-reflection film 30 suppresses reflection of light. Specifically, by including the anti-reflection film 30, the optical member 100 suppresses light that attempts to enter the light-transmitting member 10 from the anti-reflection film 30 from being reflected by the surface on the anti-reflection film 30 side.

[0034] The anti-reflection film 30 has a multi-layer structure. Specifically, the anti-reflection film 30 has low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction). The refractive indices of the low-refractive index layers and high-refractive index layers are not limited as long as the combination allows the anti-reflection film 30 to exhibit an anti-reflection effect. The refractive index of the low-refractive index layers is, for example, 1.80 or less. The refractive index of the high-refractive index layers is, for example, greater than 1.80. The outermost layer of the low-refractive index layers and high-refractive index layers is the low-refractive index layer. The innermost layer of the low-refractive index layers and high-refractive index layers is the low-refractive index layer.

[0035] The refractive index of the low-refractive index layer may be less than the refractive index of the high-refractive index layer. For example, the refractive index of the low-refractive index layer is preferably 1.30 or more and 1.80 or less, and more preferably 1.40 or more and 1.60 or less. When the refractive index of the low-refractive index layer is 1.30 or more and 1.80 or less, the reflectance of the optical member 100 is further reduced. The low-refractive index layer preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2.

[0036] The refractive index of the high-refractive index layer may be higher than that of the low-refractive index layer. For example, the refractive index of the high-refractive index layer is preferably 2.40 or more and 3.00 or less, and more preferably 2.40 or more and 2.60 or less. When the refractive index of the high-refractive index layer is 2.40 or more and 3.00 or less, the reflectance of the optical element 100 is further reduced. The high-refractive index layer preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4.

[0037] The refractive indices of the low-refractive-index layer and the high-refractive-index layer described above are merely examples and are not limited to these. The refractive indices of the low-refractive-index layer and the high-refractive-index layer may be set to values ​​that are optimal for the refractive index of the light-transmitting member 10.

[0038] The total film thickness of the antireflection coating 30 is preferably 200 nm or more and 700 nm or less, and more preferably 200 nm or more and 650 nm or less. If the total film thickness of the antireflection coating 30 is less than 200 nm, a sufficient antireflection effect tends to be insufficient. If the total film thickness of the antireflection coating 30 exceeds 700 nm, the productivity of the optical member 100 tends to decrease. Furthermore, if the total film thickness exceeds 700 nm, the production cost of the optical member 100 tends to increase.

[0039] The thickness of one low refractive index layer is, for example, 5.0 nm or more and 200.0 nm or less, and the thickness of one high refractive index layer is, for example, 5.0 nm or more and 200.0 nm or less.

[0040] The total number of low refractive index layers and high refractive index layers is usually an odd number, but may be an even number.

[0041] <Coating Layer> The optical member 100 preferably further includes a coating layer 60. The coating layer 60 is disposed on the hydrophilic layer 20. The coating layer 60 contains a plurality of primary silica particles. At least a portion of the hydrophilic layer 20 is partially or completely coated with the primary silica particles. As a result, the abrasion resistance of the optical member 100 is further improved. The coating layer 60 may further contain tetraethoxysilane.

[0042] The average particle size of the primary silica particles is preferably 5 nm or more and 20 nm or less. If the average particle size of the primary silica particles is less than 5 nm, the cost tends to increase. If the average particle size of the primary silica particles is more than 20 nm, sufficient transmittance for visible light tends to be insufficient.

[0043] The content of silica in the hydrophilic layer 20 is preferably 20% by mass or more and 50% by mass or less. When the content of silica is 20% by mass or more and 50% by mass or less, the abrasion resistance of the optical member 100 is further improved and an increase in reflectance can be further suppressed.

[0044] The thickness of the coating layer 60 is preferably 5 nm or more and 20 nm or less. If the thickness of the coating layer 60 is less than 5 nm, sufficient abrasion resistance tends to be insufficient. If the thickness of the coating layer 60 is more than 20 nm, sufficient transmittance for visible light tends to be insufficient.

[0045] <Method for Manufacturing Optical Member> An example of a method for manufacturing the optical member 100 according to this embodiment will be described below. The method for manufacturing the optical member 100 includes a preparation step, a coating step, and a drying step.

[0046] <Preparation Step> A light-transmitting member 10 is prepared. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component. An anti-reflection film 30 may be disposed on the light-transmitting member 10. The anti-reflection film 30 has low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction).

[0047] <Coating Step> A hydrophilic material is coated. The hydrophilic material contains a plurality of primary particles of titanium dioxide. The average particle size of the primary particles of titanium dioxide is 5 nm or more and 20 nm or less.

[0048] The hydrophilic material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include nitric acid, formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0049] The content of the solvent in the hydrophilic material is preferably 50.0% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50.0% by mass or more and 99.9% by mass or less, coating can be easily performed.

[0050] The method for applying the hydrophilic material is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, and a combination of two or more of these (e.g., dip spin coating). Preferred wet processes are spin coating, dip coating, and dip spin coating.

[0051] <Drying Step> The hydrophilic material is dried to form the hydrophilic layer 20. The hydrophilic layer 20 contains secondary particles formed by agglomeration of a plurality of titanium dioxide primary particles. The average particle diameter of the titanium dioxide secondary particles is 15 nm or more and 100 nm or less.

[0052] It is preferable to heat-treat the coated hydrophilic material. Heat treatment promotes the removal of the solvent in the hydrophilic material. Heating conditions can be, for example, a treatment temperature of 60°C to 200°C and a treatment time of 10 minutes to 2 hours.

[0053] Preferably, the method for manufacturing the optical element 100 further includes a coating material application step.

[0054] <Coating Material Application Step> A coating material is applied. The coating material contains a plurality of primary silica particles. The average particle size of the primary silica particles is 5 nm or more and 20 nm or less.

[0055] The coating material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0056] The content of the solvent in the coating material is preferably 50.0% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50.0% by mass or more and 99.9% by mass or less, coating can be easily performed.

[0057] The coating material is preferably applied by a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, and a combination of two or more of these (e.g., dip spin coating). Preferred wet processes are spin coating, dip coating, and dip spin coating.

[0058] The above describes embodiments of the present disclosure with reference to the drawings. However, the above embodiments are merely examples of the present disclosure, and the present disclosure is not limited to the above embodiments and can be implemented in various forms without departing from the spirit and scope of the present disclosure. The drawings mainly show each component in a schematic manner for ease of understanding, and the thickness, length, number, etc. of each component shown in the drawings may differ from the actual components due to the convenience of creating the drawings. Furthermore, the materials, shapes, dimensions, etc. of each component shown in the above embodiments are merely examples and are not particularly limited. Various modifications are possible within a scope that does not substantially deviate from the effects of the present disclosure. The configuration of the embodiments may be appropriately modified within a scope that does not deviate from the technical concept of the present disclosure. Furthermore, the embodiments may be implemented in combination within the scope of possibility.

[0059] The present technology can also employ the following configuration.

[0060] (1) An optical element comprising: a translucent member that transmits visible light; and a hydrophilic layer that covers the translucent member, wherein the hydrophilic layer contains secondary particles formed by agglomeration of a plurality of titanium dioxide primary particles, the average particle diameter of the titanium dioxide primary particles being 5 nm or more and 20 nm or less, and the average particle diameter of the titanium dioxide secondary particles being 15 nm or more and 100 nm or less.

[0061] (2) The optical member according to (1), wherein the thickness of the hydrophilic layer is 20 nm or more and 200 nm or less.

[0062] (3) The optical member according to (1) or (2), wherein the titanium dioxide is anatase type titanium dioxide.

[0063] (4) The optical element according to any one of (1) to (3), further comprising a coating layer disposed on the hydrophilic layer, the coating layer containing a plurality of primary silica particles, and the average particle diameter of the primary silica particles being 5 nm or more and 20 nm or less.

[0064] (5) The optical element according to (4), wherein the thickness of the coating layer is 5 nm or more and 20 nm or less.

[0065] (6) The optical member according to any one of (1) to (5), further comprising an anti-reflection film disposed between the light-transmitting member and the hydrophilic layer.

[0066] (7) A lens unit including the optical element according to any one of (1) to (6).

[0067] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.

[0068] <Production of Optical Members> Optical members according to Examples 1 to 7 and optical members according to Comparative Examples 1 to 4 were produced.

[0069] Example 1 Preparation Steps A lens (manufactured by HOYA Corporation, "TAFD-5G", composition: glass, diameter: 12.9 mm, refractive index: 1.835) was prepared as a light-transmitting member. One surface of the lens was convex (radius of curvature: 12 mm) and the other surface was concave (radius of curvature: 3.07 mm).

[0070] An antireflection coating was formed on the convex surface of the lens by vapor deposition. The total number of low-refractive-index layers and high-refractive-index layers in the antireflection coating was nine. Of these, the first, third, fifth, seventh, and ninth layers were low-refractive-index layers, and the second, fourth, sixth, and eighth layers were high-refractive-index layers.

[0071] <Coating Step> A hydrophilic material according to Example 1 was prepared, containing 0.5 parts by mass of titanium dioxide particles (anatase-type titanium dioxide, average primary particle size of 7 nm), 0.5 parts by mass of silicon dioxide, 2 parts by mass of water, 76 parts by mass of isopropyl alcohol, 20 parts by mass of methanol, and 1 part by mass of nitric acid.

[0072] The hydrophilic material according to Example 1 was applied onto the anti-reflection film. Specifically, 100 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member. Next, using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), the light-transmitting member was rotated at a rotation speed of 5000 rpm. At this time, the rotation axis was aligned with the optical axis of the light-transmitting member.

[0073] <Drying Step> A heat treatment was carried out at 90° C. for 30 minutes to form a hydrophilic layer having a thickness of 200 nm. The average particle size of the secondary particles of titanium dioxide was 60 nm.

[0074] <Coating Material Application Step> A coating material according to Example 1 containing 1 part by mass of silica particles (average primary particle diameter of 5 nm), 99 parts by mass of water, and 0.2 parts by mass of ammonia was prepared. The coating material according to Example 1 was applied onto the hydrophilic layer. Specifically, 60 μL of the coating material according to Example 1 was dropped onto the optical axis of the light-transmitting member. Next, using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), the light-transmitting member was rotated at a rotation speed of 5,000 rpm. At this time, the rotation axis was aligned with the optical axis of the light-transmitting member. A heat treatment was performed at 120°C for 30 minutes to form a coating layer with a thickness of 5 nm, thereby obtaining an optical member according to Example 1.

[0075] Example 2 An optical member according to Example 2 was manufactured in the same manner as in Example 1, except that in the <Coating Step>, 0.5 parts by mass of titanium dioxide particles (anatase titanium dioxide, average primary particle size of 20 nm) were used instead of 0.5 parts by mass of titanium dioxide particles (anatase titanium dioxide, average primary particle size of 7 nm), and 80 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member instead of 100 μL of the hydrophilic material according to Example 1. The thickness of the hydrophilic layer was 100 nm.

[0076] Example 3 An optical member according to Example 3 was produced in the same manner as in Example 1, except that in the drying step, heat treatment at 80°C for 30 minutes was performed instead of at 90°C for 30 minutes. The average particle size of the secondary particles of titanium dioxide was 100 nm.

[0077] Example 4 An optical member according to Example 4 was manufactured in the same manner as in Example 1, except that in the <Coating Step>, 50 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member instead of 100 μL of the hydrophilic material according to Example 1. The thickness of the hydrophilic layer was 19 nm.

[0078] Example 5 An optical member according to Example 5 was manufactured in the same manner as in Example 1, except that in the <Coating Step>, 110 μL of the hydrophilic material according to Example 1 was dropped onto the optical axis of the light-transmitting member instead of 100 μL of the hydrophilic material according to Example 1. The thickness of the hydrophilic layer was 201 nm.

[0079] Example 6 An optical member according to Example 6 was manufactured in the same manner as in the manufacturing of the optical member according to Example 1, except that the coating material application step was not performed.

[0080] Example 7 An optical element according to Example 7 was manufactured in the same manner as in the manufacture of the optical element according to Example 6, except that in the preparation step, instead of forming an antireflection film on the convex surface of the lens, no antireflection film was formed on the convex surface of the lens.

[0081] Comparative Example 1 An optical member according to Comparative Example 1 was manufactured in the same manner as in Example 1, except that in the coating step, 0.5 parts by mass of titanium dioxide particles (anatase-type titanium dioxide, average primary particle size of 7 nm) were used instead of 0.5 parts by mass of titanium dioxide particles (anatase-type titanium dioxide, average primary particle size of 4 nm).

[0082] <Comparative Example 2> An optical member according to Comparative Example 2 was produced in the same manner as in Example 1, except that in the <Coating Step>, 0.5 parts by mass of titanium dioxide particles (anatase-type titanium dioxide, average primary particle size of 7 nm) were used instead of 0.5 parts by mass of titanium dioxide particles (anatase-type titanium dioxide, average primary particle size of 25 nm).

[0083] Comparative Example 3 An optical member according to Comparative Example 3 was produced in the same manner as in Example 1, except that in the drying step, heat treatment at 120°C for 30 minutes was performed instead of at 90°C for 30 minutes. The average particle size of the secondary particles of titanium dioxide was 14 nm.

[0084] Comparative Example 4 An optical member according to Comparative Example 4 was produced in the same manner as in Example 1, except that in the drying step, heat treatment at 70°C for 30 minutes was performed instead of at 90°C for 30 minutes. The average particle size of the secondary particles of titanium dioxide was 250 nm, and the thickness of the hydrophilic layer was 250 nm.

[0085] <Evaluation> By the following methods, the reflectance, contact angle, and abrasion test were measured for the optical members according to Examples 1 to 7 and Comparative Examples 1 to 4. The measurement results are shown in Table 1 below. All measurements were carried out in an environment of a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0086] <Reflectance> Using a reflectance measuring device ("USPM-RU" manufactured by Olympus Corporation), the maximum reflectance of the optical member for light with a wavelength of 480 nm or more and 780 nm or less was measured. The incident angle of the incident light was set to 0 degrees. The maximum reflectance of the optical member was evaluated according to the following criteria. The evaluation results are shown in Table 1.

[0087] 〇: 1.0% or less △: More than 1.0% and 1.5% or less ×: More than 1.5%

[0088] <Contact Angle Recovery Degree> Before using the optical element, the static contact angle with pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). After using the optical element, the static contact angle with pure water was measured using an ultraviolet light source (peak wavelength 365 nm, FL15BL-B, manufactured by Toshiba Corporation) with an illuminance of 1 mW / cm. 2 The optical component was irradiated with ultraviolet light of 1000 kJ / s. Thereafter, the static contact angle with respect to pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). The static contact angle before use was then calculated relative to the static contact angle after irradiation. The degree of recovery of the contact angle of the optical component was evaluated according to the following criteria. The evaluation results are shown in Table 1.

[0089] 〇: 80% or more △: 70% or more but less than 80% ×: Less than 70%

[0090] <Abrasion Test> The optical element was placed in an abrasion tester and subjected to 1,000 abrasion tests using a car wash brush with a load of 1 kg applied to the surface. The optical element was then observed at 466x magnification using a laser microscope. The durability of the optical element was evaluated according to the following criteria. The evaluation results are shown in Table 1.

[0091] 〇: No optical effect △: Slightly optical effect ×: Optical effect

[0092]

[0093] The optical members according to Comparative Examples 1 to 4 were not good in terms of the degree of recovery of the contact angle. In contrast, the optical members according to Examples 1 to 7 were good in terms of the degree of recovery of the contact angle. In particular, the optical members according to Examples 1 to 3, 6, and 7 were good in terms of the degree of recovery of the contact angle.

[0094] 10... Transparent member 20... Hydrophilic layer 100... Optical member

Claims

1. An optical component comprising: a translucent member that transmits visible light; and a hydrophilic layer covering the translucent member, wherein the hydrophilic layer contains secondary particles formed by agglomeration of a plurality of titanium dioxide primary particles, the average particle diameter of the titanium dioxide primary particles being 5 nm or more and 20 nm or less, and the average particle diameter of the titanium dioxide secondary particles being 15 nm or more and 100 nm or less.

2. The optical member according to claim 1, wherein the hydrophilic layer has a thickness of 20 nm or more and 200 nm or less.

3. The optical member according to claim 1, wherein the titanium dioxide is anatase type titanium dioxide.

4. The optical element according to claim 1, further comprising a coating layer disposed on the hydrophilic layer, the coating layer containing a plurality of primary silica particles, and an average particle diameter of the primary silica particles being 5 nm or more and 20 nm or less.

5. The optical member according to claim 4, wherein the coating layer has a thickness of 5 nm or more and 20 nm or less.

6. The optical member according to claim 1, further comprising an anti-reflection film disposed between said light-transmitting member and said hydrophilic layer.

7. A lens unit comprising the optical member according to any one of claims 1 to 6.

8. A method for manufacturing an optical component, comprising: a coating step of coating a hydrophilic material; and a drying step of drying the hydrophilic material to form a hydrophilic layer, wherein the hydrophilic material contains a plurality of primary particles of titanium dioxide, the primary particles of titanium dioxide having an average particle diameter of 5 nm or more and 20 nm or less, and the hydrophilic layer contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide, and the secondary particles of titanium dioxide having an average particle diameter of 15 nm or more and 100 nm or less.

Citation Information

Patent Citations

  • Photocatalytic hydrophilic member and its production

    JP1998085610A

  • Photocatalytic hydrophilic member, its production and photocatalytic hydrophilic coating composition

    JP1998225639A

  • Hydrophilic member and its production method

    JP2002080830A

  • Transparent laminate

    JP2021192090A

  • Optical member and method for manufacturing same

    WO2020202875A1