Conductive dispersion and production method therefor

The conductive dispersion with a dual-resin component system effectively addresses the stability and dispersibility challenges by optimizing molecular weights and viscosities, ensuring long-term stability and high dispersibility for electrochemical applications.

WO2024225004A1PCT designated stage expired Publication Date: 2024-10-31PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014275
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-08
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing conductive carbon material dispersions face challenges in maintaining high dispersibility and stability, as improving one property often compromises the other, and fibrous carbon nanomaterials tend to settle due to the form of particles and solvents used.

Method used

A conductive dispersion is developed with a fibrous or aggregate-like conductive carbon material dispersed in a liquid component, using a resin component with two distinct molecular weight components and viscosities to enhance dispersibility and stability, where the first component has a lower molecular weight and higher viscosity, and the second component has a higher molecular weight and lower viscosity, ensuring both properties are optimized.

Benefits of technology

The approach achieves a conductive dispersion that maintains high dispersibility and stability, preventing aggregation and sedimentation, making it suitable for electrochemical devices like secondary batteries and capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A conductive dispersion comprising: a conductive carbon material; a liquid component; and a resin component dissolved in the liquid component, wherein the conductive carbon material is dispersed in the liquid component, the conductive carbon material is in the form of fibers or aggregates, the resin component includes a first component and a second component, the weight average molecular weight Mw1 of the first component and the weight average molecular weight Mw2 of the second component satisfy Mw1<Mw2, or the viscosity V1 of a first solution in which the first component is dissolved in the liquid component at a predetermined concentration and the viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the same concentration as that of the first solution satisfy V1<V2.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive dispersion and method for producing the same CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This disclosure claims the benefit of priority to Japanese Patent Application No. 2023-072686, filed on April 26, 2023, in the Japan Patent Office, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a conductive dispersion and a method for producing the same.

[0003] Patent Document 1 proposes "a carbon nanotube dispersion containing carbon nanotubes, carboxymethyl cellulose or a salt thereof, and water, wherein the carboxymethyl cellulose or the salt thereof has a weight-average molecular weight of 10,000 to 100,000 and a degree of etherification of 0.5 to 0.9, and the product (X×Y) of the complex elastic modulus X (Pa) and the phase angle Y (°) of the carbon nanotube dispersion is 100 or more and 1,500 or less."

[0004] Patent Document 2 proposes a conductive material paste composition for secondary battery electrodes, which includes "a fibrous carbon nanomaterial, a binder, and a solvent, wherein the binder contains an alkylene structural unit and a nitrile group-containing monomer unit and is a first copolymer having a weight average molecular weight of 170,000 or more and less than 1,500,000," and further includes "a second copolymer wherein the binder contains an alkylene structural unit and a nitrile group-containing monomer unit and is having a weight average molecular weight of 10,000 or more and less than 170,000."

[0005] JP 2021-175699 A Public Relations International Publication No. 2017 / 056488 A

[0006] The conductive dispersion is required to have high dispersibility of the conductive carbon material and high stability so that the conductive carbon material can be maintained in a dispersed state for a long period of time without settling.

[0007] However, Patent Document 1 uses a specific carboxymethyl cellulose or a salt thereof alone, and in this case, the control of dispersibility and stability by the physical properties of the carboxymethyl cellulose or a salt thereof usually results in a trade-off relationship in which an improvement in one property reduces the other.

[0008] Furthermore, the copolymer containing alkylene structural units and nitrile group-containing monomer units of Patent Document 2 is particulate and does not dissolve in solvents, so the fibrous carbon nanomaterial is prone to settling, making it difficult to improve stability.

[0009] One aspect of the present disclosure relates to a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the conductive carbon material is dispersed in the liquid component, the conductive carbon material is in a fibrous or aggregate state, the resin component comprises a first component and a second component, and a weight-average molecular weight Mw1 of the first component and a weight-average molecular weight Mw2 of the second component satisfy Mw1 < Mw2.

[0010] Another aspect of the present disclosure relates to a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the conductive carbon material is dispersed in the liquid component, the conductive carbon material is in a fibrous or aggregate state, the resin component comprises a first component and a second component, and wherein a viscosity V1 of a first solution obtained by dissolving the first component in the liquid component at a predetermined concentration and a viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the predetermined concentration satisfy V1 < V2.

[0011] Yet another aspect of the present disclosure relates to a method for producing a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the resin component comprises a first component and a second component, the conductive carbon material is fibrous or aggregate-like, and the weight-average molecular weight Mw1 of the first component and the weight-average molecular weight Mw2 of the second component satisfy Mw1 < Mw2, the method comprising: (i) a step of dispersing the conductive carbon material and a portion of the resin component in the liquid component to obtain an intermediate dispersion; and (ii) a step of dispersing the remainder of the resin component in the intermediate dispersion, wherein the portion of the resin component used in step (i) contains more of the first component than the second component, and the remainder of the resin component used in step (ii) contains more of the second component than the first component.

[0012] Yet another aspect of the present disclosure relates to a method for producing a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the resin component comprises a first component and a second component, the conductive carbon material is fibrous or aggregate-like, a viscosity V1 of a first solution obtained by dissolving the first component in the liquid component at a predetermined concentration, and a viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the predetermined concentration satisfy V1 < V2, and the method includes: (i) a step of dispersing the conductive carbon material and a portion of the resin component in the liquid component to obtain an intermediate dispersion; and (ii) a step of dispersing the remainder of the resin component in the intermediate dispersion, wherein the portion of the resin component used in step (i) contains more of the first component than the second component, and the remainder of the resin component used in step (ii) contains more of the second component than the first component.

[0013] According to the present disclosure, a conductive dispersion that can achieve both high dispersibility and stability can be obtained. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0014] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified, but other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be components of known secondary batteries. In this specification, when a "range from numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B. When multiple materials are exemplified, one may be selected from the materials and used alone, or two or more may be used in combination.

[0015] The conductive dispersion according to the present disclosure (hereinafter also referred to as "dispersion (D)") contains a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, and has fluidity. Dispersion (D) is a material used in the manufacture of electrodes for electrochemical devices. The type of electrode is not limited, and includes electrodes that generate capacitance through a faradaic reaction, electrodes that generate capacitance through a non-faradaic reaction, and electrodes that have both of these properties.

[0016] The electrochemical device may be a capacitor or a secondary battery. The capacitor may be a lithium ion capacitor, an electric double layer capacitor, or the like. The secondary battery may be a non-aqueous electrolyte secondary battery such as a lithium ion secondary battery, a lithium secondary battery (lithium metal secondary battery), or an all-solid-state secondary battery. The dispersion (D) is, for example, mixed with an electrode material of the non-aqueous electrolyte secondary battery. In this case, the dispersion (D) constitutes a part of the electrode material of the non-aqueous electrolyte secondary battery. In particular, since the positive electrode of a non-aqueous electrolyte secondary battery is mainly composed of a ceramic material, the use of a conductive carbon material is often essential.

[0017] In the dispersion (D), the conductive carbon material is dispersed in a liquid component. The liquid component may be any component that can dissolve the resin component and disperse the conductive carbon material.

[0018] The conductive carbon material is in the form of fibers or aggregates. One type of conductive carbon material may be used alone, or a combination of two or more types may be used.

[0019] Typical examples of fibrous conductive carbon materials are carbon nanotubes (CNTs) and carbon nanofibers (CNFs).

[0020] The CNT may be a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), a multi-walled carbon nanotube (MWCNT), or a mixture of these. MWCNT is a general term for carbon nanotubes with two or more walls. Examples of MWCNT include DWCNT, triple-walled CNT, and four or more-walled CNT.

[0021] Among CNTs, even a small amount of SWCNT can significantly improve the conductivity of an electrode when incorporated into the electrode. However, SWCNT is a material that is difficult to maintain in a highly dispersed state in a liquid component for a long period of time without settling. On the other hand, according to the present disclosure, a conductive dispersion can be obtained that contains SWCNT as a conductive carbon material and achieves both high dispersibility and stability. For example, 50 mass% or more of the conductive carbon material in the dispersion (D) may be SWCNT.

[0022] The average diameter of the CNTs is not particularly limited and may be in the range of 1 nm to 50 nm. Carbon nanotubes with an average diameter of 5 nm or less contain many SWCNTs. When N carbon nanotubes (for example, 100≦N) are arbitrarily selected, 50% or more (0.5N), or even 80% (0.8N) or more of these carbon nanotubes may have individual diameters of 5 nm or less, or even 3 nm or less. CNTs with a diameter of 3 nm or less may be considered SWCNTs.

[0023] The average length of the CNTs is not particularly limited, but may be 0.5 μm or more, or may be 1 μm or more and 25 μm or less. When N carbon nanotubes (e.g., 100≦N) are arbitrarily selected, the individual lengths of 50% or more (0.5N), or even 80% (0.8N) or more of the selected carbon nanotubes may be 1 μm or more, 1 μm or more and 25 μm or less, or 1 μm or more and 20 μm or less.

[0024] CNFs are, for example, a type of MWCNT and are produced as vapor-grown carbon fibers (VGCFs). CNFs are typically larger in diameter than CNTs and have at least a partially graphitic structure.

[0025] The average diameter of the CNFs is, for example, 10 nm to 1000 nm, preferably 100 nm to 200 nm, and the average length of the CNFs is, for example, 5 μm to 500 μm, preferably 50 μm to 100 μm.

[0026] The average diameter and length of CNTs and CNFs can be determined by image analysis using a scanning electron microscope (SEM). For example, the length can be determined by measuring the lengths and diameters of a number of randomly selected CNTs or CNFs (e.g., about 100 to 1000), and averaging these measurements.

[0027] The aggregate-like conductive carbon material is an agglomeration of minute carbon particles, and may be amorphous carbon having a structure. A typical example of the aggregate-like conductive carbon material is carbon black. Carbon black has a structure in which carbon particles with a primary particle diameter of, for example, 5 nm to 500 nm are linked in a chain shape. The carbon black may be acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, or the like.

[0028] The resin component includes a first component and a second component. The resin component acts as a dispersant for dispersing the conductive carbon material in the liquid component, and also has the effect of increasing the viscosity of the dispersion (D). Increasing the viscosity of the dispersion (D) suppresses aggregation and sedimentation of the conductive carbon material. The resin component satisfies at least one of the following conditions (A) and (B). As long as at least one of conditions (A) and (B) is satisfied, the first component and the second component may be the same type of resin or different types of resin.

[0029] <Condition (A)> The weight average molecular weight Mw1 of the first component and the weight average molecular weight Mw2 of the second component satisfy Mw1<Mw2.

[0030] <Condition (B)> The viscosity V1 of a first solution obtained by dissolving a first component in a liquid component at a predetermined concentration and the viscosity V2 of a second solution obtained by dissolving a second component in a liquid component at the same predetermined concentration satisfy the relationship V1<V2.

[0031] When only the first component is used, many molecules of the first component adsorb to the conductive carbon material in the liquid component, making it easy to disperse the conductive carbon material, but they tend to aggregate and settle over time. On the other hand, when only the second component is used, few molecules of the second component adsorb to the conductive carbon material in the liquid component, making it difficult to disperse the conductive carbon material, but they are also less likely to aggregate and settle. By using the first component and the second component in combination, it is possible to achieve both high dispersibility of the conductive dispersion and high stability of the dispersion (D).

[0032] The weight average molecular weights of the first component and the second component may satisfy 5≦Mw2 / Mw1, 7≦Mw2 / Mw1, 20≦Mw2 / Mw1, or 30≦Mw2 / Mw1. The larger the Mw2 / Mw1 ratio, the higher the stability of the dispersion (D).

[0033] The weight-average molecular weight Mw1 of the first component is more preferably, for example, 20,000 to 2,000,000. A sufficiently small Mw1 improves the dispersibility of the first component itself in the liquid component, and also increases the number of molecules of the first component adsorbed to the conductive carbon material, thereby improving the dispersibility of the conductive carbon material. On the other hand, in order to increase the viscosity of the liquid component to a certain level or more when dispersing the conductive carbon material and apply sufficient shear force to the conductive carbon material, it is preferable that the weight-average molecular weight Mw1 of the first component be equal to or greater than the above-mentioned lower limit.

[0034] The weight-average molecular weight Mw2 of the second component is more preferably, for example, 50,000 to 10,000,000. A sufficiently large Mw2 stabilizes the floating state of the second component itself in the liquid component, and increases the viscosity of the dispersion (D). This suppresses aggregation and sedimentation of the conductive carbon material, improving the stability of the dispersion (D). On the other hand, excessively increasing the viscosity of the dispersion (D) reduces ease of handling, so it is preferable to set the weight-average molecular weight Mw2 of the second component to the above-mentioned upper limit or less.

[0035] The viscosity V1 of a first solution obtained by dissolving a first component in a liquid component at a predetermined concentration (e.g., a content of 1% by mass) and the viscosity V2 of a second solution obtained by dissolving a second component in a liquid component at the same concentration may satisfy 5≦V2 / V1, 7≦V2 / V1, 100≦V2 / V1, or 500≦V2 / V1. The larger the V2 / V1 ratio, the higher the stability of the dispersion (D). The viscosities V1 and V2 may be measured at the same temperature, for example, at 25°C. The viscosity may be measured using a Brookfield viscometer at a rotation speed of 20 rpm.

[0036] The viscosity V1 (1% / 25°C) of a solution of the liquid component containing the first component at 1% by mass at 25°C is preferably, for example, 1 to 2000 mPa·s. A sufficiently small viscosity V1 (1% / 25°C) not only improves the dispersibility of the first component itself in the liquid component but also increases the number of molecules of the first component adsorbed to the conductive carbon material, thereby improving the dispersibility of the conductive carbon material. On the other hand, in order to increase the viscosity of the liquid component to a certain level or more when dispersing the conductive carbon material and apply sufficient shear force to the conductive carbon material, it is preferable to set the viscosity V1 (1% / 25°C) to be equal to or greater than the above-mentioned lower limit.

[0037] The viscosity V2 (1% / 25°C) of a solution of the liquid component containing the second component at 1% by mass at 25°C is preferably, for example, 2 to 50,000 mPa. A sufficiently high viscosity V2 (1% / 25°C) stabilizes the floating state of the second component itself in the liquid component, and increases the viscosity of the dispersion (D). This suppresses aggregation and sedimentation of the conductive carbon material, thereby increasing the stability of the dispersion (D). On the other hand, excessively increasing the viscosity of the dispersion (D) reduces ease of handling, so it is preferable to set the viscosity V2 (1% / 25°C) to the above upper limit or less.

[0038] The liquid component may be a dispersion medium for dispersing an electrode material in the production of an electrode. Such a liquid component may be a polar solvent. Examples of polar solvents include water, N-methyl-2-pyrrolidone (NMP), cyclohexanone, alcohol, and ether. Of these, water or NMP is preferred. 80% by mass or more of the liquid component may be a polar solvent. 80% by mass or more of the liquid component may be water. 80% by mass or more of the liquid component may be NMP.

[0039] When the liquid component contains a polar solvent, it is preferable that both the first component and the second component are water-soluble polymers. The polar solvent is a good solvent for the water-soluble polymer. The water-soluble polymer may be a water-soluble polymer compound having a hydrophilic group in the main chain or side chain. The hydrophilic group of the water-soluble polymer may be a polyoxyalkylene chain, a hydroxy group, a carboxyl group, an acid anhydride group, an amino group, a C 2-3 It may also be an alkylene oxide group.

[0040] Specific examples of the water-soluble polymer include polyalkylene glycol compounds, water-soluble polyamides, water-soluble polyimides, water-soluble acrylic resins (such as polyacrylic acid), polyvinyl alcohol, polyvinylpyrrolidone, and cellulose derivatives.

[0041] Among water-soluble polymers, cellulose derivatives are preferred because they are inexpensive and easily soluble in water or NMP. Examples of cellulose derivatives include methyl cellulose, carboxymethyl cellulose (CMC), ammonium salts of CMC, and alkali metal salts of CMC. The alkali metal salts may be sodium salts, potassium salts, lithium salts, etc.

[0042] In the dispersion (D), the conductive carbon material and the resin component may form aggregated particles, and the aggregated particles may be dispersed in the liquid component. The aggregated particles may be formed by the conductive carbon material and the resin component being entangled with each other.

[0043] The average particle size of the aggregated particles in the liquid component is preferably, for example, 0.1 μm or more and 50 μm or less. The average particle size of the aggregated particles may be measured using a particle size measuring device based on dynamic light scattering. The average particle size of the aggregated particles is the median diameter in the volume particle size distribution measured by dynamic light scattering.

[0044] The mass content Mp1 of the first component contained in the agglomerated particles and the mass content Mp2 of the second component contained in the agglomerated particles preferably satisfy the relationship Mp1 > Mp2. By incorporating a larger amount of the first component, which has a significant effect of increasing the dispersibility of the conductive carbon material, into the agglomerated particles, the effect of increasing the stability of the dispersion (D) while increasing the dispersibility of the conductive carbon material or the agglomerated particles becomes greater. The Mp1 / Mp2 ratio preferably satisfies 1.1 ≦ Mp1 / Mp2, and may also satisfy 1.2 ≦ Mp1 / Mp2 or 1.5 ≦ Mp1 / Mp2.

[0045] The mass content Mp1 of the first component and the mass content Mp2 of the second component contained in the aggregated particles can be calculated by separating the aggregated particles from the dispersion (D), separating the resin component from the separated aggregated particles by centrifugation, and analyzing the resin component. Since the resin component contains the first component and the second component, two main peaks are observed when the molecular weight distribution of the resin component is measured by gel permeation chromatography. If the two main peaks partially overlap, the two peaks are separated by waveform separation. The Mp1 / Mp2 ratio can be calculated from the integral of the areas of the two peaks. If three or more peaks are observed in the molecular weight distribution, the peak with the largest area and the peak with the second largest area are considered to represent one of the first component and the second component, respectively.

[0046] The mass content Ms1 of the first component and the mass content Ms2 of the second component contained in the liquid component excluding the aggregated particles may satisfy the relationship Ms1 < Ms2. The stability of the dispersion (D) is further improved by including a larger amount of the second component, which has a significant effect of enhancing the stability of the dispersion (D), in the liquid component than in the first component. The Ms2 / Ms1 ratio preferably satisfies 1.1 ≦ Ms2 / Ms1, and may also satisfy 1.2 ≦ Ms2 / Ms1 or 1.5 ≦ Ms2 / Ms1.

[0047] The amount of the resin component per 100 parts by mass of the conductive carbon material contained in the dispersion (D) is preferably, for example, 10 parts by mass or more and 1,000 parts by mass or less. In particular, when the conductive carbon material is CNT, the amount of the resin component per 100 parts by mass of the CNT is preferably, for example, 50 to 1,000 parts by mass. Furthermore, when the conductive carbon material is carbon black, the amount of the resin component per 100 parts by mass of the carbon black is preferably, for example, 10 to 500 parts by mass.

[0048] Increasing the amount of the resin component within the above range allows a larger amount of the first component to be adsorbed onto the conductive carbon material, thereby improving the dispersibility of the conductive carbon material and improving the stability of the dispersion (D) due to the action of the second component. Furthermore, by setting the amount of the resin component to be equal to or less than the upper limit of the above range, it becomes easy to increase the content of the conductive carbon material in the electrode while limiting the content of the resin component in the electrode. Therefore, the degree of freedom in the blending amount of the dispersion (D) relative to the electrode material is improved.

[0049] The amount of the resin component per 100 parts by mass of the conductive carbon material can be calculated by separating the agglomerated particles from the dispersion (D), separating the resin component and the conductive carbon material from the separated agglomerated particles by a method such as centrifugation, further separating the resin component from the residual liquid after separating the agglomerated particles by removing the liquid component by drying or the like, and then summing the resin component separated from the agglomerated particles and the resin component separated from the residual liquid.

[0050] Furthermore, by analyzing the separated resin component, the content C1 of the first component and the content C2 of the second component in the dispersion (D) can be calculated. Since the resin component contains the first component and the second component, two main peaks are observed when measuring the molecular weight distribution of the resin component. If the two main peaks partially overlap, the two peaks are separated by waveform separation. The C1, C2, and C1 / C2 ratio can be calculated from the integrated values ​​of the areas of the two peaks and a previously prepared calibration curve. If three or more peaks are observed in the molecular weight distribution, the peak with the largest area and the peak with the second largest area are considered to represent one of the first and second components, respectively.

[0051] The content C1 of the first component is preferably, for example, 0.2 mass % or more and 5 mass % or less. The larger the amount of the first component within the above range, the more the first component can be adsorbed onto the conductive carbon material, thereby improving the dispersibility of the conductive carbon material. Furthermore, by setting the amount of the first component to be equal to or less than the upper limit of the above range, it becomes easy to increase the content of the conductive carbon material in the electrode while limiting the content of the first component in the electrode.

[0052] The content C2 of the second component is, for example, preferably 0.05% by mass or more and 10% by mass or less. The greater the amount of the second component within the above range, the more the stability of the dispersion (D) can be improved.

[0053] The C1 / C2 ratio is, for example, not more than 40, and preferably not less than 1. The larger the C1 / C2 ratio, the more the stability of the dispersion (D) can be improved.

[0054] Furthermore, from the viewpoint of improving the dispersibility of the conductive carbon material or the agglomerated particles while enhancing the stability of the dispersion (D), it is preferable to include a relatively larger amount of the first component, which has a significant effect of enhancing the dispersibility of the conductive carbon material, in the agglomerated particles than in the liquid component. That is, it is preferable to satisfy C1 / C2<Mp1 / Mp2. In this case, C1 / C2>Ms1 / Ms2 is also satisfied. 1.1≦(Mp1 / Mp2) / (C1 / C2) may be satisfied, or 1.1≦(Mp1 / Mp2) / (C1 / C2) may be satisfied. Also, 1.1≦(C1 / C2) / (Ms1 / Ms2) may be satisfied, or 1.1≦(C1 / C2) / (Ms1 / Ms2) may be satisfied.

[0055] The viscosity Vd(25°C) of the dispersion (D) at 25°C is preferably, for example, 100 to 10,000 mPa s. When the viscosity Vd(25°C) is within the above range, the dispersion (D) has high stability and is easily highly dispersed in the electrode material when blended with the electrode material.

[0056] <Method for Producing Dispersion (D)> The method for producing dispersion (D) includes (i) a step of dispersing a conductive carbon material and a portion of the resin component in a liquid component to obtain an intermediate dispersion, and (ii) a step of dispersing at least a portion of the remaining resin component in the intermediate dispersion. In step (i), the entire amount of the portion of the resin component may be dispersed in the liquid component at once, or may be dispersed in multiple batches. Similarly, in step (ii), the entire amount of the remaining resin component may be dispersed in the intermediate dispersion at once, or may be dispersed in multiple batches. The entire amount of the liquid component may be blended with the conductive carbon material in step (i), or the liquid component may be blended separately in steps (i) and (ii).

[0057] A portion of the resin component used in step (i) contains more of the first component than the second component. Step (i) is primarily a step for adsorbing the first component to the conductive carbon material. It is desirable to use as little or no second component as possible in step (i) so as not to inhibit contact between the first component and the conductive carbon material. The first component may account for 90% by mass or more of the portion of the resin component used in step (i). That is, the amount of the first component used relative to the total amount of the first component and the second component used in step (i) may be 90% by mass or more, 95% by mass or more, or even 100%. The entire amount of the liquid component may be blended with the conductive carbon material in step (i), or the liquid component may be blended separately in steps (i) and (ii).

[0058] The remainder of the resin component used in step (ii) contains more of the second component than the first component. Step (ii) is a step of dissolving the second component in an intermediate dispersion to obtain a dispersion (D) having a higher viscosity and reduced fluidity than the intermediate dispersion. In order to avoid excessively increasing the content of the resin component contained in dispersion (D), it is desirable to use as little of the first component as possible in step (ii), or to use no first component at all. The remainder of the resin component used in step (ii) may be 90% by mass or more of the second component. That is, the amount of the second component used relative to the total amount of the first component and the second component used in step (ii) may be 90% by mass or more, 95% by mass or more, or even 100%.

[0059] (Additional Notes) The above description of the embodiments discloses the following techniques: (Technology 1) A conductive dispersion comprising: a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the conductive carbon material is dispersed in the liquid component, the conductive carbon material is in a fibrous or aggregate state, the resin component comprises a first component and a second component, and a weight average molecular weight Mw1 of the first component and a weight average molecular weight Mw2 of the second component satisfy Mw1 < Mw2. (Technology 2) A conductive dispersion comprising: a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component; the conductive carbon material is dispersed in the liquid component; the conductive carbon material is in a fibrous or aggregate state; the resin component comprises a first component and a second component; and a viscosity V1 of a first solution obtained by dissolving the first component in the liquid component at a predetermined concentration and a viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the predetermined concentration satisfy V1 < V2. (Technology 3) A conductive dispersion according to Technology 1, which satisfies 5≦Mw2 / Mw1. (Technology 4) A conductive dispersion according to Technology 2, which satisfies 5≦V2 / V1. (Technology 5) A conductive dispersion according to any one of Technology 1 to 4, wherein the liquid component contains a polar solvent, and both the first component and the second component are water-soluble polymers. (Technology 6) A conductive dispersion according to Technology 5, wherein the water-soluble polymer is a cellulose derivative. (Technology 7) The conductive dispersion according to any one of Technologies 1 to 6, wherein the conductive carbon material is at least one selected from the group consisting of carbon nanotubes (CNT), carbon nanofibers (CNF), and carbon black (CB). (Technology 8) The conductive dispersion according to any one of Technologies 1 to 7, wherein the amount of the resin component per 100 parts by mass of the conductive carbon material is 10 parts by mass or more and 1,000 parts by mass or less. (Technology 9) The conductive dispersion according to any one of Technologies 1 to 8, wherein the content C1 of the first component is 0.2% by mass or more and 5% by mass or less. (Technology 10) The conductive dispersion according to any one of Technologies 1 to 9, wherein the content C2 of the second component is 0.05% by mass or more. (Technology 11) The conductive dispersion according to any one of Technologies 1 to 10, wherein the ratio C1 / C2 is 40 or less.(Technology 12) The conductive dispersion according to any one of Techniques 1 to 11, wherein the conductive carbon material and the resin component constitute agglomerated particles, and the agglomerated particles are dispersed in the liquid component. (Technology 13) The conductive dispersion according to Technique 12, wherein a mass content Mp1 of the first component contained in the agglomerated particles and a mass content Mp2 of the second component contained in the agglomerated particles satisfy C1 / C2<Mp1 / Mp2. (Technology 14) The conductive dispersion according to Technique 12 or 13, wherein a mass content Ms1 of the first component contained in the liquid component excluding the agglomerated particles and a mass content Ms2 of the second component contained in the liquid component satisfy C1 / C2>Ms1 / Ms2. (Technology 15) The conductive dispersion according to any one of Techniques 12 to 14, wherein an average particle size of the agglomerated particles in the liquid component is 0.1 μm or more and 50 μm or less. (Technology 16) The conductive dispersion according to any one of Technologies 1 to 15, which is mixed with an electrode material for a lithium ion secondary battery. (Technology 17) A method for producing a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the resin component comprises a first component and a second component, the conductive carbon material is fibrous or aggregate-like, a weight average molecular weight Mw1 of the first component and a weight average molecular weight Mw2 of the second component satisfy Mw1 < Mw2, the method comprising: (i) a step of dispersing the conductive carbon material and a portion of the resin component in the liquid component to obtain an intermediate dispersion, and (ii) a step of dispersing the remainder of the resin component in the intermediate dispersion, wherein the portion of the resin component used in step (i) contains the first component in a larger amount than the second component, and at least a portion of the remainder of the resin component used in step (ii) contains the second component in a larger amount than the first component.(Technology 18) A method for producing a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the resin component comprises a first component and a second component, and the conductive carbon material is fibrous or aggregate-like, wherein a viscosity V1 of a first solution obtained by dissolving the first component in the liquid component at a predetermined concentration and a viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the predetermined concentration satisfy V1 < V2, and the method comprises: (i) a step of dispersing the conductive carbon material and a portion of the resin component in the liquid component to obtain an intermediate dispersion, and (ii) a step of dispersing the remainder of the resin component in the intermediate dispersion, wherein the portion of the resin component used in step (i) contains more of the first component than the second component, and at least a portion of the remainder of the resin component used in step (ii) contains more of the second component than the first component. (Technology 19) The method for producing a conductive dispersion according to Technology 17 or 18, wherein 90 mass % or more of the part of the resin component used in step (i) is the first component.

[0060] [Examples] The conductive dispersion according to the present disclosure will be described in more detail below based on examples and comparative examples, although the present disclosure is not limited to the following examples.

[0061] Example 1 Step (i) 100 parts by mass of CNT, which is a conductive carbon material, 100 parts by mass of first CMC (Na salt of CMC), which is a first component of the resin components, and 9,800 parts by mass of water, which is a liquid component, were mixed, and the mixture was subjected to a dispersion treatment 10 times using a high-pressure homogenizer, to obtain an intermediate dispersion.

[0062] The weight average molecular weight Mw1 of the first CMC measured by gel permeation chromatography (GPC method) was 70,000, and the viscosity V1 of the first solution containing the first CMC at a content of 1 mass% was 2 mPa·s at 25°C.

[0063] The CNTs had an average diameter of 1.4 nm and an average length of 1 μm, and were substantially entirely SWCNTs.

[0064] Step (ii) Next, 100 parts by mass of second CMC (Na salt of CMC) was added to the intermediate dispersion, and water was added as needed to adjust the CNT concentration, thereby obtaining a dispersion (D1).

[0065] The weight average molecular weight Mw2 of the second CMC measured by GPC was 3,000,000, and the viscosity V2 of the second solution containing 1% by mass of the second CMC was 2,000 mPa s at 25° C. Therefore, Mw2 / Mw1 = 43, and V2 / V1 = 1,000.

[0066] The amount of resin component (total amount of the first CMC and the second CMC) per 100 parts by mass of CNT was 200 parts by mass, the CNT content in dispersion (D) was 1.0% by mass, the first CMC content C1 was 1.0% by mass, the second CMC content C2 was 1.0% by mass, and the C1 / C2 ratio was 1.

[0067]

[0068] [Evaluation] (Stability of Dispersion (D)) Dispersion (D1) was left to stand for 10 days, and the solid content of the supernatant was measured and used as an index of the degree of sedimentation. The sedimentation resistance was defined by the following formula. The larger the value, the higher the stability.

[0069] Sedimentation resistance (%) = 100 × (solid content of supernatant) / solid content of dispersion (D)

[0070] (Viscosity of Dispersion (D)) The viscosity of Dispersion (D1) was measured at 25° C. using a Brookfield viscometer at a rotation speed of 20 rpm, and was found to be 500 mPa / s.

[0071] (Average particle size of aggregated particles) The average particle size of the aggregated particles contained in the obtained dispersion (D1) was measured using a laser diffraction / scattering particle size measuring device (MT3000 II manufactured by Microtrac Co., Ltd.). The median diameter in the volume particle size distribution was 10 μm, confirming that the aggregated particles were small and had high dispersibility.

[0072] Comparative Example 1: 100 parts by mass of CNT, a conductive carbon material, 100 parts by mass of first CMC, a first component of the resin component, and 9,800 parts by mass of a liquid component were mixed and dispersed 10 times using a high-pressure homogenizer to obtain a dispersion (CD1). The average particle size of the aggregated particles contained in the resulting dispersion (CD1) was measured in the same manner as in Example 1. The median diameter in the volumetric particle size distribution was 10 μm, confirming that the aggregated particles were small and had high dispersibility. Meanwhile, when the stability of the dispersion (CD1) was evaluated, the sedimentation resistance was 69%, indicating insufficient stability. The viscosity of the dispersion (CD1) was 100 mPa / s.

[0073] Comparative Example 2 A dispersion (CD2) was obtained in the same manner as in Comparative Example 1, except that the weight-average molecular weight of the first CMC was changed to 200,000. The average particle size of the aggregated particles contained in the obtained dispersion (CD2) was measured in the same manner as in Example 1, and the median diameter in the volume particle size distribution was 15 μm, confirming that the aggregated particles were small and had high dispersibility. On the other hand, when the stability of dispersion (CD2) was evaluated, the sedimentation resistance was 68%, indicating insufficient stability. The viscosity of dispersion (CD1) was 300 mPa / s.

[0074] Comparative Example 3: A dispersion (CD3) was obtained in the same manner as in Comparative Example 1, except that the weight-average molecular weight of the first CMC was changed to 3,000,000. The average particle size of the aggregated particles contained in the obtained dispersion (CD3) was measured in the same manner as in Example 1. The median diameter in the volume particle size distribution was 30 μm, confirming that the aggregated particles were large and had low dispersibility. Meanwhile, when the stability of dispersion (CD3) was evaluated, the sedimentation resistance was 66%, indicating insufficient stability. The viscosity of dispersion (CD1) was 500 mPa / s.

[0075] Examples 2 to 10, Comparative Examples 4 to 5 Each dispersion (D2 to D10, CD4, CD5) was prepared in the same manner as in Example 1, except that the weight average molecular weight and amount of the first CMC and second CMC were changed as shown in Table 1, and the stability (sedimentation resistance) and viscosity were measured. The results are shown in Table 1.

[0076] In Comparative Examples 1 to 3, the weight-average molecular weight of the first CMC used during the dispersion treatment of the CNT was different. When the weight-average molecular weight was small, the number of molecules that could be adsorbed to the CNT increased, making dispersion easier and resulting in small CNT agglomerated particles after the dispersion treatment. On the other hand, the viscosity of the dispersion (CD) was low, resulting in low sedimentation resistance. When a first CMC with a large weight-average molecular weight was used, the viscosity of the dispersion (CD) increased, but the size of the CNT agglomerated particles increased, resulting in low sedimentation resistance.

[0077] On the other hand, as shown in each example, when a second CMC with a large weight-average molecular weight was added to the intermediate dispersion after the CNT dispersion treatment, aggregation and sedimentation were suppressed due to the effect of increasing the viscosity of the dispersion (D) and the steric hindrance effect of the second CMC, which inhibits contact between the CNTs. However, when a second CMC with a weight-average molecular weight close to that of the first CMC was added, the effect of suppressing aggregation and sedimentation was small. Furthermore, the greater the amount of second CMC, the greater the effect of suppressing aggregation and sedimentation. Furthermore, even when the weight-average molecular weight of the first CMC was quite large, the effect of suppressing aggregation and sedimentation was obtained as long as the weight-average molecular weight of the second CMC was sufficiently large.

[0078] The conductive dispersion according to the present disclosure can be used to improve the conductivity of electrodes (particularly positive electrodes) of electrochemical devices (particularly lithium secondary batteries).

[0079] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

Claims

1. A conductive dispersion comprising: a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component; the conductive carbon material is dispersed in the liquid component; the conductive carbon material is in a fibrous or aggregate state; the resin component comprises a first component and a second component; and a weight average molecular weight Mw1 of the first component and a weight average molecular weight Mw2 of the second component satisfy Mw1<Mw2.

2. A conductive dispersion comprising: a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the conductive carbon material is dispersed in the liquid component, the conductive carbon material is in a fibrous or aggregate state, the resin component comprises a first component and a second component, and a viscosity V1 of a first solution obtained by dissolving the first component in the liquid component at a predetermined concentration, and a viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the predetermined concentration satisfy V1 < V2.

3. The conductive dispersion according to claim 1, wherein Mw2 / Mw1 satisfies 5≦Mw2 / Mw1.

4. The conductive dispersion according to claim 2, which satisfies 5≦V2 / V1.

5. The conductive dispersion according to claim 1 or 2, wherein the liquid component contains a polar solvent, and the first component and the second component are both water-soluble polymers.

6. The conductive dispersion according to claim 5, wherein the water-soluble polymer is a cellulose derivative.

7. The conductive dispersion according to claim 1 or 2, wherein the conductive carbon material is at least one selected from the group consisting of carbon nanotubes (CNT), carbon nanofibers (CNF) and carbon black (CB).

8. The conductive dispersion according to claim 1 or 2, wherein the amount of the resin component per 100 parts by mass of the conductive carbon material is 10 parts by mass or more and 1,000 parts by mass or less.

9. A conductive dispersion according to claim 1 or 2, wherein the content C1 of the first component is 0.2 mass % or more and 5 mass % or less.

10. The conductive dispersion according to claim 9, wherein the content C2 of the second component is 0.05 mass % or more.

11. The conductive dispersion according to claim 1 or 2, wherein the ratio C1 / C2 is 40 or less.

12. The conductive dispersion according to claim 1 or 2, wherein the conductive carbon material and the resin component form agglomerated particles, and the agglomerated particles are dispersed in the liquid component.

13. The conductive dispersion according to claim 12, wherein the average particle size of the aggregated particles in the liquid component is 0.1 μm or more and 50 μm or less.

14. A conductive dispersion as described in claim 12, wherein the mass content Mp1 of the first component contained in the agglomerated particles and the mass content Mp2 of the second component contained in the agglomerated particles satisfy C1 / C2<Mp1 / Mp2.

15. A conductive dispersion as described in claim 12, wherein the mass content Ms1 of the first component and the mass content Ms2 of the second component contained in the liquid component excluding the agglomerated particles satisfy C1 / C2>Ms1 / Ms2.

16. The conductive dispersion according to claim 1 or 2, which is mixed with an electrode material of a lithium-ion secondary battery.

17. A method for producing a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the resin component comprises a first component and a second component, the conductive carbon material is in a fibrous or aggregate state, a weight average molecular weight Mw1 of the first component and a weight average molecular weight Mw2 of the second component satisfy Mw1 < Mw2, the method comprising: (i) a step of dispersing the conductive carbon material and a portion of the resin component in the liquid component to obtain an intermediate dispersion, and (ii) a step of dispersing the remainder of the resin component in the intermediate dispersion, wherein the portion of the resin component used in step (i) contains the first component in a greater amount than the second component, and the remainder of the resin component used in step (ii) contains the second component in a greater amount than the first component.

18. A method for producing a conductive dispersion comprising a conductive carbon material, a liquid component, and a resin component dissolved in the liquid component, wherein the resin component comprises a first component and a second component, and the conductive carbon material is in a fibrous or aggregate state, a viscosity V1 of a first solution obtained by dissolving the first component in the liquid component at a predetermined concentration, and a viscosity V2 of a second solution obtained by dissolving the second component in the liquid component at the predetermined concentration satisfy V1 < V2, the method comprising: (i) a step of dispersing the conductive carbon material and a portion of the resin component in the liquid component to obtain an intermediate dispersion; and (ii) a step of dispersing the remainder of the resin component in the intermediate dispersion, wherein the portion of the resin component used in step (i) contains the first component in a greater amount than the second component, and the remainder of the resin component used in step (ii) contains the second component in a greater amount than the first component.

19. A method for producing a conductive dispersion described in claim 17 or 18, wherein 90 mass% or more of the portion of the resin component used in step (i) is the first component.

Citation Information

Patent Citations

  • Carbon nanotube dispersion, secondary battery electrode composition using the same, electrode film, and secondary battery.

    JP6860740B1

  • Carbon nanotube dispersion, and electrode coating material, electrode, and non-aqueous electrolyte secondary battery using the same

    JP7194860B1