Method for producing surface-treated substrate, method for selectively modifying substrate surface, composition, and compound

The use of an onium salt-based surface modification composition with a nitrogen-containing heterocycle and monovalent organic group in a water-based solution addresses storage stability and selectivity issues in semiconductor manufacturing, enhancing the semiconductor manufacturing process by ensuring high-density, impurity-resistant surface modification.

WO2024225048A1PCT designated stage expired Publication Date: 2024-10-31JSR CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014597
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-10
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

In the semiconductor manufacturing process, existing methods for forming organic films on substrates to protect specific areas face challenges with storage stability and selectivity, particularly when using water-based compositions, which can lead to precipitation and reduced storage stability, and require high-density modification to prevent impurity adherence.

Method used

A method involving a surface modification composition containing an onium salt with a nitrogen-containing heterocycle and a monovalent organic group, combined with 1% or more water by mass, to selectively and densely modify substrate surfaces, enhancing storage stability and selectivity while providing water repellency and heat resistance.

Benefits of technology

The approach ensures high storage stability and selective surface modification with high density, effectively preventing impurity adherence and maintaining film integrity, thus improving the semiconductor manufacturing process yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

According to the present invention, manufactured is a surface-treated substrate by a method including a step for selectively modifying the surface of a substrate by coating the surface of the substrate with a composition. The composition contains: an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms; and 1 mass% or more of water with respect to the total amount of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing surface-treated substrate, method for selectively modifying substrate surface, composition and compound

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to Japanese Patent Application No. 2023-73379, filed April 27, 2023, the entire contents of which are incorporated herein by reference. The present disclosure relates to a method for producing a surface-treated substrate, a method for selectively modifying a substrate surface, a composition, and a compound.

[0002] In a semiconductor manufacturing process, an organic film is formed on a portion of a substrate surface to cover and protect that portion, and the substrate after the organic film formation is subjected to various surface treatments such as forming a metal layer or etching. When forming an organic film on the substrate surface to protect that portion of the substrate surface, with the increasing miniaturization of semiconductor devices, it is required to be able to form the film with high selectivity on the region of the substrate surface that is to be protected (see, for example, Patent Document 1).

[0003] Patent Literature 1 discloses a method for selectively surface-modifying the first region with the first polymer by applying a composition containing a first polymer and a solvent, the first polymer having, at the end of its main chain or side chain, a group containing a first functional group that bonds to the metal contained in the first region, and then heating the coating film formed by applying the composition. Patent Literature 1 also discloses that the solvent used to prepare the composition is a solvent capable of dissolving or dispersing the first polymer, such as an alcohol solvent, an ether solvent, a ketone solvent, an amide solvent, or a hydrocarbon solvent.

[0004] International Publication No. 2018 / 043304

[0005] If the main component of the solvent in a composition used for selectively modifying a substrate surface can be water, it is expected that the environmental impact can be reduced and the handling of the composition will be improved. However, compositions containing water tend to easily cause precipitation of the components contained in the composition, and the storage stability of the composition tends to be reduced. In particular, when the substrate surface is to be given water repellency or heat resistance by selectively modifying the substrate surface, a highly hydrophobic material is used as the film-forming material. In this case, there is a concern that the storage stability of the composition is likely to be reduced due to insufficient solubility of the film-forming material in water.

[0006] Furthermore, when protecting a partial region on the surface of a substrate, it is necessary to selectively protect the region to be protected from the viewpoint of stabilizing the quality of products in semiconductor manufacturing processes, suppressing a decrease in product yield, etc. Furthermore, it is necessary to highly densely modify the region to be protected and make it difficult for impurities to adhere to the protected region (i.e., high blocking performance).

[0007] The present disclosure has been made in view of the above-mentioned problems, and has as its object to provide a method for selectively modifying a substrate surface, which has high storage stability and is capable of highly selectively and densely modifying the substrate surface. Another object is to provide a composition that has high storage stability and is capable of highly selectively and densely modifying the substrate surface.

[0008] In order to solve the above-described problems, the present disclosure provides, in one aspect, a method for producing a surface-treated substrate, the method including a step of selectively modifying the surface of a substrate by applying a composition to the surface of the substrate, the composition containing an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition.

[0009] In another aspect of the present disclosure, there is provided a method for selectively modifying a substrate surface, comprising a step of applying a composition to the surface of the substrate, the composition containing an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition.

[0010] Furthermore, in one aspect of the present disclosure, there is provided a composition for use in selectively modifying a substrate surface, the composition comprising an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition.

[0011] Furthermore, in one embodiment of the present disclosure, there is provided a compound represented by the following formula (3): (In formula (3), R 7 and R 8 are each independently an alkyl group having 16 to 22 carbon atoms. - is R 5 SO 3 - or R 5 SO 2 N - R 6 It is. 5 is a monovalent fluorinated hydrocarbon group. 6 is a monovalent organic group having one or more carbon atoms.

[0012] According to the present disclosure, the storage stability of a composition used for selectively modifying a substrate surface can be improved even when the composition contains water. Furthermore, the composition can modify a substrate surface highly selectively and at high density.

[0013] Matters related to the embodiments will be described in detail below. In this specification, a numerical range described using "to" means that the numerical values ​​described before and after "to" are included as the lower and upper limits. Unless otherwise specified, each component may be used alone or in combination of two or more.

[0014] <Method and Composition> The method of the present disclosure includes a step of applying a composition (hereinafter also referred to as a "surface-modifying composition") to the surface of a substrate. The surface-modifying composition is an aqueous liquid composition containing an onium salt (hereinafter also referred to as an "onium salt (A)") having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and water. The surface-modifying composition will be described below first, followed by a method for selectively modifying a substrate surface using the surface-modifying composition and a method for producing a substrate having a treated substrate surface. Hereinafter, the "method for producing a surface-treated substrate" will also be referred to simply as the "method for producing a substrate," and the "method for selectively modifying a substrate surface" will also be referred to simply as the "selective modification method." The "method for producing a substrate" and the "selective modification method" will also be collectively referred to simply as the "method."

[0015] <Surface-modifying composition> The surface-modifying composition is used as a surface treatment liquid for forming a film on the surface of a substrate to modify the surface of the substrate. The area where the film is formed by the surface-modifying composition is endowed with water repellency, heat resistance, and blocking properties. The film formed by the surface-modifying composition is typically a self-assembled monolayer (SAM) formed by adsorption of the onium salt (A) onto the substrate surface. Below, each component contained in the surface-modifying composition and optional components that may be blended as needed are described.

[0016] Onium Salt (A) The onium salt (A) is a compound having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms (hereinafter referred to as the “monovalent organic group R A By using the onium salt (A) as a monomolecular film forming material, the nitrogen-containing heterocyclic moiety exhibits the ability to adsorb to a substrate (particularly a metal region), and the monovalent organic group R AIt is believed that water repellency, heat resistance, and blocking performance are exhibited depending on the portion. In particular, it is believed that the onium salt (A) has a nitrogen-containing heterocycle, and by interacting with the metal, it can highly selectively and densely modify the metal region of the substrate. The "interaction" referred to here refers to, for example, a chemical bond, such as a covalent bond, an ionic bond, or a coordinate bond. When a nitrogen atom in the nitrogen-containing heterocycle forms a coordinate bond with the metal, it is possible to increase the bonding strength between the metal atom and the nitrogen-containing heterocycle.

[0017] The onium salt (A) is preferably a compound composed of an organic cation and an anion. From the viewpoint of ensuring solubility in water, the molecular weight of the onium salt (A) is preferably 1,000 or less, more preferably 800 or less, even more preferably 700 or less, and even more preferably 600 or less. Furthermore, from the viewpoint of obtaining a film with good heat resistance, the molecular weight of the onium salt (A) is preferably 120 or more, more preferably 150 or more, and even more preferably 200 or more.

[0018] When the onium salt (A) contains an organic cation, the organic cation in the onium salt (A) is a nitrogen-containing heterocycle and a monovalent organic group R A Hereinafter, the nitrogen-containing heterocycle and the monovalent organic group R contained in the onium salt (A) will be referred to as A This article explains:

[0019] The nitrogen-containing heterocycle contained in the onium salt (A) may be an aromatic heterocycle or a non-aromatic heterocycle. The nitrogen-containing heterocycle contained in the onium salt (A) may be a monocycle or a fused ring. The nitrogen-containing heterocycle may have only a nitrogen atom as a heteroatom in the ring skeleton, or may have an atom other than the nitrogen atom (preferably a sulfur atom or an oxygen atom).

[0020] Specific examples of nitrogen-containing aromatic heterocycles include a pyrrole ring, an imidazole ring, a pyrazole ring, a triazole ring, a tetrazole ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, a quinoline ring, an isoquinoline ring, a benzimidazole ring, a benzotriazole ring, a substituted benzotriazole ring, a carbazole ring, an acridine ring, a pyrazine ring, a thiazole ring, a benzothiazole ring, an oxazole ring, and a benzoxazole ring. Examples of the substituted benzotriazole ring include rings having a substituent such as an alkyl group having 1 to 3 carbon atoms, a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), or a nitro group at the 5th or 6th position. Specific examples of nitrogen-containing non-aromatic heterocycles include a piperidine ring, a piperazine ring, a hexamethyleneimine ring, diazabicycloundecene, diazabicyclo[4.3.0]non-5-ene, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

[0021] The nitrogen-containing heterocycle of the onium salt (A) is preferably an aromatic heterocycle, more preferably a ring having a plurality of heteroatoms in the ring skeleton. Specifically, an imidazole ring, a benzimidazole ring, a thiazole ring, a benzothiazole ring, an oxazole ring, or a benzoxazole ring is preferred. In terms of being able to form a film with higher selectivity and density, the heterocycle of the onium salt (A) is preferably an imidazole ring, a benzimidazole ring, a thiazole ring, or a benzothiazole ring, among the above.

[0022] The monovalent organic group R contained in the onium salt (A) A is preferably a monovalent hydrocarbon group or halogenated hydrocarbon group having 4 or more carbon atoms, from the viewpoint of forming a film having excellent heat resistance on the substrate by applying the surface modifying composition to the surface of the substrate. A The carbon number of is, for example, 4 to 40.

[0023] Here, in this specification, the term "hydrocarbon group" includes chain hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. "Chain hydrocarbon group" refers to a straight-chain hydrocarbon group or a branched hydrocarbon group that does not contain a cyclic structure and is composed only of a chain structure. Chain hydrocarbon groups may be saturated or unsaturated. "Alicyclic hydrocarbon group" refers to a hydrocarbon group that contains only an alicyclic hydrocarbon structure as a ring structure and does not contain an aromatic ring structure. Alicyclic hydrocarbon groups do not necessarily have to be composed only of alicyclic hydrocarbon structures, and also include those that have a chain structure as part of them. "Aromatic hydrocarbon group" refers to a hydrocarbon group that contains an aromatic ring structure as a ring structure. However, it does not necessarily have to be composed only of an aromatic ring structure, and may contain a chain structure or an alicyclic hydrocarbon structure as part of it.

[0024] Monovalent organic group R A Specific examples of the monovalent hydrocarbon group include a monovalent chain hydrocarbon group having 4 to 40 carbon atoms, a monovalent alicyclic hydrocarbon group having 4 to 40 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 40 carbon atoms. Specific examples of these include monovalent chain hydrocarbon groups having 4 to 40 carbon atoms, such as alkyl groups such as n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, eicosyl, and docosyl; alkenyl groups such as propenyl, butenyl, hexenyl, octenyl, decenyl, and dodecenyl; and alkynyl groups such as propynyl and butynyl.

[0025] Examples of the monovalent alicyclic hydrocarbon group having 4 to 40 carbon atoms include monocyclic alicyclic saturated hydrocarbon groups such as a cyclopentyl group, a cyclohexyl group, a methylcyclopentyl group, an ethylcyclopentyl group, a methylcyclohexyl group, and an ethylcyclohexyl group; monocyclic alicyclic unsaturated hydrocarbon groups such as a cyclopentenyl group, a cyclohexenyl group, a methylcyclopentenyl group, and a methylcyclohexenyl group; polycyclic alicyclic saturated hydrocarbon groups such as a norbornyl group, an adamantyl group, and a tricyclodecyl group; and polycyclic alicyclic unsaturated hydrocarbon groups such as a norbornenyl group and a tricyclodecenyl group.

[0026] Examples of the monovalent aromatic hydrocarbon group having 6 to 40 carbon atoms include aryl groups such as a phenyl group, a tolyl group, a xylyl group, a naphthyl group, an anthryl group, a vinylphenyl group, and an allylphenyl group; and aralkyl groups such as a benzyl group, a phenethyl group, a naphthylmethyl group, and an anthrylmethyl group.

[0027] Examples of the monovalent halogenated hydrocarbon group include groups in which any hydrogen atom in the groups exemplified as the monovalent hydrocarbon group has been substituted with a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom).

[0028] The monovalent organic group R A Among the above, is preferably a monovalent hydrocarbon group, more preferably a monovalent chain hydrocarbon group, further preferably a linear or branched alkyl group, and even more preferably a linear alkyl group. A From the viewpoint of forming a film having excellent heat resistance and blocking performance, the number of carbon atoms in the monovalent organic group R is preferably 5 or more, more preferably 8 or more, and even more preferably 9 or more. A The number of carbon atoms is preferably 30 or less, and more preferably 25 or less, from the viewpoint of improving the solubility of the onium salt (A) in water and preventing a decrease in the adsorption ability of the onium salt (A) to a substrate.

[0029] The onium salt (A) is a monovalent organic group R having 4 or more carbon atoms. AAs long as it has the formula (I), it may further have a monovalent organic group having 1 to 3 carbon atoms. Specific examples of such groups include a methyl group, an ethyl group, a propyl group, an acetyl group, and a formyl group.

[0030] The anion of the onium salt (A) is not particularly limited as long as it is an anionic counter ion. For example, the anion of the onium salt (A) may be an inorganic anion or an organic anion. From the viewpoint of improving the heat resistance of the film formed by the onium salt (A), the anion of the onium salt (A) may be a halide ion (e.g., a chloride ion, a bromide ion, an iodide ion), PF 6 - , B.F. 4 - , SbF 6 - , C.N. - , (CN) 2 N - , SCN - , R 3 SO 3 - , R 3 COO - or R 3 SO 2 N - R 4 (However, R 3 and R 4 are each independently a monovalent organic group having one or more carbon atoms (the same applies hereinafter).

[0031] R 3 or R 4 The monovalent organic group represented by the formula (I) is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms, and any methylene group in the hydrocarbon group is -O-, -S-, -CO-, -COO-, -SO 2 - and the like.

[0032] R 3 or R 4Specific examples of the monovalent hydrocarbon group having 1 to 12 carbon atoms in the monovalent organic group represented by the formula (I) include a monovalent chain hydrocarbon group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 12 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 12 carbon atoms. Specific examples of these groups include a methyl group, an ethyl group, a propyl group, a vinyl group, an allyl group, and the monovalent organic group R A Among the groups exemplified as R, groups with the corresponding carbon number can be mentioned. 3 or R 4 When is a substituted monovalent hydrocarbon group, examples of the substituent include a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), a nitro group, and the like.

[0033] The anion contained in the onium salt (A) is a bromide ion, PF 6 - , R 3 SO 3 - or R 3 SO 2 N - R 4 is preferred, and R 3 SO 3 - or R 3 SO 2 N - R 4 is more preferred. 3 SO 3 - and R 3 SO 2 N - R 4 Further specific examples include a methanesulfonate anion, a trifluoromethanesulfonate anion, a vinylsulfonate anion, a p-vinylbenzenesulfonate anion, a p-toluenesulfonate anion, an o-nitrobenzenesulfonate anion, and a bis(trifluoromethanesulfonyl)imide anion.

[0034] In the onium salt (A), the monovalent organic group R A is preferably bonded to a nitrogen-containing heterocycle. From the viewpoint of improving the solubility of the onium salt (A) in water, the monovalent organic group RA is preferably bonded to a nitrogen atom constituting the nitrogen-containing heterocycle.

[0035] A preferred specific example of the onium salt (A) is a compound represented by the following formula (2). (In formula (2), R 11 is a monovalent organic group. 2 is -NR 12 -, a sulfur atom, or an oxygen atom. 12 is a monovalent organic group. 2 Ga-NR 12 In the case of -, R 11 and R 12 At least one of X has 4 or more carbon atoms; 2 When is a sulfur atom or an oxygen atom, R 11 has 4 or more carbon atoms. 13 is a hydrogen atom or a monovalent organic group. 14 and R 15 are each independently a hydrogen atom or a monovalent organic group, or R 14 and R 15 are combined together, R 14 and the carbon atom to which R 15 represents a ring structure formed together with the carbon atom to which Z is attached. - is an anion.)

[0036] In the above formula (2), R 11 or R 12 The monovalent organic group represented by R preferably has 4 or more carbon atoms in order to impart excellent heat resistance and blocking performance to the surface of the substrate. 11 or R 12 Preferred examples of the monovalent organic group represented by the formula (I) include the above-mentioned monovalent organic group R A Examples of the groups include the same groups as those shown in the above.

[0037] R 13 When R is a monovalent organic group, examples of the monovalent organic group include a monovalent hydrocarbon group or a halogenated hydrocarbon group having 1 to 40 carbon atoms. 13 is preferably a hydrogen atom.

[0038] X 2 Ga-NR 12 -, the heat resistance of the film formed by the onium salt (A) can be improved. 11 and R 12 have the same number of carbon atoms, or R 11 and R 12 and R preferably have an even or odd number of carbon atoms. 11 and R 12 It is more preferable that the number of carbon atoms in R 11 and R 12 It is more preferred that are the same groups.

[0039] R 14 or R 15 When R is a monovalent organic group, examples of the monovalent organic group include a monovalent hydrocarbon group or a halogenated hydrocarbon group having 1 to 40 carbon atoms. 14 and R 15 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, more preferably a hydrogen atom.

[0040] R 14 and R 15 The ring structure formed by combining R with each other is preferably an aromatic ring structure, more preferably a benzene ring structure, from the viewpoint of forming a film with high heat resistance using the onium salt (A). 14 and R 15 The ring structure formed by combining these may have a substituent. Examples of the substituent include a monovalent hydrocarbon group or halogenated hydrocarbon group having 1 to 40 carbon atoms, and an alkyl group having 1 to 3 carbon atoms is preferred.

[0041] X 2 is -NR 12 - or a sulfur atom is preferred. 2 Ga-NR 12 When X is a - or sulfur atom, a film with higher density can be formed on the surface of the substrate, and blocking performance can be further improved. From the viewpoint of ease of synthesis of the onium salt (A) and from the viewpoint of increasing the adsorption of the onium salt (A) to the substrate by the generation of carbene, X 2 Ha-NR 12 - is preferred.

[0042] In particular, when the nitrogen-containing heterocycle contained in the onium salt (A) has a partial structure represented by the following formula (1), it is preferable in that a film with higher density can be formed on the substrate surface and the blocking performance of the film-forming portion can be further improved. (In formula (1), R 1 is a monovalent organic group. 1 Ha-NR 2 - or a sulfur atom. 2 is a monovalent organic group. 1 Ga-NR 2 In the case of -, R 1 and R 2 At least one of X has 4 or more carbon atoms; 1 When is a sulfur atom, R 1 has 4 or more carbon atoms. "*" represents a bond.)

[0043] In the above formula (1), X 1 Ga-NR 2 In the case of -, R 1 or R 2 Each of the monovalent organic groups represented by the following formula (I) preferably has 4 or more carbon atoms, from the viewpoint of imparting excellent water repellency, heat resistance, and blocking performance to the surface of the substrate. 1 or R 2 Preferred specific examples of the monovalent organic group represented by the formula: A The explanation in paragraph 1 applies.

[0044] X 1 Ga-NR 2 -, then R 1 and R 2 In order to improve the heat resistance of the film formed from the onium salt (A), R 1 and R 2 have the same number of carbon atoms, or R 1 and R 2 and R preferably have an even number of carbon atoms or an odd number of carbon atoms. 1 and R 2 It is more preferable that the carbon numbers of R and R are the same in that they can provide excellent heat resistance to the surface of the substrate while ensuring the ease of synthesis of the onium salt (A). 1 and R2 It is more preferred that are the same group.

[0045] In addition, X 1 Ga-NR 2 In the case of -, it is considered that the carbene generated in the nitrogen-containing heterocycle functions as a ligand, thereby increasing the adsorption ability of the onium salt (A) to the substrate, thereby enabling the formation of a denser film on the substrate surface.

[0046] Specific examples of the onium salt (A) include compounds represented by the following formulas (a1-1) to (a1-16). (In formulas (a1-1) to (a1-16), Y - is a halide ion, PF 6 - , B.F. 4 - , SbF 6 - , C.N. - , (CN) 2 N - , SCN - , R 3 SO 3 - , R 3 COO - or R 3 SO 2 N - R 4 It is.)

[0047] The onium salt (A) can be obtained by appropriately combining standard methods in organic chemistry. For example, it can be obtained by reacting a nitrogen-containing heterocyclic compound such as imidazole, thiazole, or oxazole with an alkyl halide having 4 or more carbon atoms in an appropriate solvent, optionally in the presence of a catalyst (for example, by interlayer transfer in a two-layer system consisting of an organic phase and an aqueous phase). The product obtained by this reaction can also be reacted with a compound having a desired anionic structure to substitute the anionic moiety, thereby obtaining the desired onium salt. The synthesis method for the onium salt (A) is not limited to the above.

[0048] From the viewpoint of high-density modification of the substrate surface, the content of the onium salt (A) in the surface-modifying composition is preferably 0.01% by mass or more, and more preferably 0.02% by mass or more, relative to the total amount of the surface-modifying composition. From the viewpoint of highly selective modification of the substrate surface, the content of the onium salt (A) in the surface-modifying composition is preferably 1.0% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.1% by mass or less, relative to the total amount of the surface-modifying composition.

[0049] The surface-modifying composition is an aqueous composition containing water as a solvent component. The water content in the surface-modifying composition is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 15% by mass or more, still more preferably 30% by mass or more, even more preferably 50% by mass or more, and even more preferably 55% by mass or more, based on the total amount of the surface-modifying composition.

[0050] The solvent component of the surface-modifying composition may be water alone or may further contain an organic solvent. By using a mixed solvent of water and an organic solvent as the solvent component of the surface-modifying composition, the storage stability of the surface-modifying composition can be further improved. The organic solvent is preferably at least one selected from the group consisting of alcohols, ethers, ketones, sulfones, amides, cyclic amines, lactams, and esters.

[0051] Specific examples of organic solvents that may be added to the surface-modifying composition include alcohols, such as chain monoalcohols having 1 to 18 carbon atoms, such as methanol, ethanol, propanol, isopropyl alcohol, 4-methyl-2-pentanol, and n-hexanol; alicyclic monoalcohols having 3 to 18 carbon atoms, such as cyclohexanol; polyhydric alcohols having 2 to 18 carbon atoms, such as 1,2-propylene glycol; and partial ethers of polyhydric alcohols having 3 to 19 carbon atoms, such as propylene glycol monomethyl ether (1-methoxy-2-propanol), 2-methoxy-1-propanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monobutyl ether (butyl cellosolve), propylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol ethyl methyl ether, and diethylene glycol monobutyl ether.

[0052] Examples of ethers include tetrahydrofuran. Examples of ketones include acetone, methyl ethyl ketone, acetonyl acetone, and diacetone alcohol. Examples of sulfones include sulfolane and dimethyl sulfoxide. Examples of amides include cyclic amides such as N,N'-dimethylimidazolidinone and N-methylpyrrolidone; and linear amides such as N-methylformamide, N,N-dimethylformamide, N,N-diethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, and N-methylpropionamide. Examples of cyclic amines include morpholine and N-(3-aminopropyl)morpholine. Examples of lactams include 1-methyl-2-pyrrolidone. Examples of esters include linear esters such as monocarboxylic acid esters, such as ethyl lactate; and cyclic esters such as γ-butyrolactone and δ-valerolactone.

[0053] Of these, the organic solvent is preferably an alcohol, more preferably at least one selected from the group consisting of chain monoalcohols having 1 to 18 carbon atoms, polyhydric alcohols having 2 to 18 carbon atoms, and polyhydric alcohol partial ethers having 3 to 19 carbon atoms, and even more preferably a polyhydric alcohol partial ether having 3 to 19 carbon atoms. Furthermore, the number of carbon atoms in the at least one compound selected from the group consisting of chain monoalcohols having 1 to 18 carbon atoms, polyhydric alcohols having 2 to 18 carbon atoms, and polyhydric alcohol partial ethers having 3 to 19 carbon atoms is preferably 1 to 15, more preferably 1 to 12, and even more preferably 1 to 10.

[0054] When the surface-modifying composition contains an organic solvent, the content of the organic solvent in the surface-modifying composition is preferably 65% ​​by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and even more preferably 40% by mass or less, based on the total amount of the surface-modifying composition, from the viewpoint of minimizing the amount of organic solvent used and enabling the onium salt (A) to form a higher-density film. Furthermore, from the viewpoint of improving the storage stability of the surface-modifying composition, the content of the organic solvent in the surface-modifying composition is preferably 1% by mass or more, more preferably 2% by mass or more, based on the total amount of the surface-modifying composition.

[0055] Other Components In addition to the onium salt (A) and solvent component described above, the surface-modifying composition may further contain a component other than the onium salt (A) and the solvent component (hereinafter also referred to as "other component"). In terms of enhancing the storage stability of the surface-modifying composition, the surface-modifying composition preferably contains a pH adjuster in addition to the onium salt (A) and water. Furthermore, the surface-modifying composition may contain a cleaning component as the other component.

[0056] (pH Adjuster) The pH adjuster is a component for adjusting the hydrogen ion concentration in the surface modifying composition. The pH adjuster may be any of an inorganic acid, an organic acid, an inorganic base, and an organic base, or a salt thereof. A buffer solution may also be used as the pH adjuster to be blended in the surface modifying composition.

[0057] Specific examples of pH adjusters include inorganic acids such as phosphoric acid, boric acid, hydrochloric acid, sulfuric acid, and nitric acid; organic acids such as acetic acid, lactic acid, malonic acid, succinic acid, citric acid, gluconic acid, cis-2-butenedioic acid, and N-propylpiperazine-N'-ethanesulfonic acid; inorganic bases such as ammonia, potassium hydroxide, and sodium hydroxide; and organic bases such as monoethanolamine, diethanolamine, triethanolamine, trimethylamine, triethylamine, propylamine, and dibutylamine. Examples of salts include salts of the acids or bases listed above that exhibit buffering properties, such as ammonium chloride, ammonium acetate, and sodium citrate. Examples of buffer solutions include sodium phosphate buffer, sodium acetate buffer, sodium citrate phosphate buffer, sodium tartrate buffer, potassium borate buffer, and sodium borate buffer. The organic acids and organic bases used as pH adjusters preferably have 10 or fewer carbon atoms, more preferably 8 or fewer carbon atoms, and even more preferably 7 or fewer carbon atoms.

[0058] From the viewpoint of minimizing the metal content in the surface modifying composition, the pH adjuster is preferably an organic acid, an organic base, or ammonia, and more preferably a carboxyl group-containing chain compound, a chain monoamine compound, or ammonia. The carboxyl group-containing chain compound preferably has 8 or less carbon atoms, more preferably 2 to 7 carbon atoms. The chain monoamine compound preferably has 6 or less carbon atoms, more preferably 2 to 4 carbon atoms.

[0059] Of the above, at least one selected from the group consisting of ammonia, monoethanolamine, diethanolamine, triethanolamine, citric acid, malonic acid, and cis-2-butenedioic acid can be preferably used as the pH adjuster.

[0060] When a pH adjuster is blended into the surface-modifying composition, the content of the pH adjuster in the surface-modifying composition may be set appropriately depending on the type of pH adjuster used, as long as the pH of the surface-modifying composition can be adjusted to the desired pH. The pH of the surface-modifying composition can be set appropriately depending on, for example, the type of onium salt (A).

[0061] (Cleaning Component) A cleaning component may be blended into the surface-modifying composition for the purpose of removing components remaining on the substrate before forming a monomolecular film on the substrate using the surface-modifying composition (e.g., residues from dry etching for hole formation, etc.). By blending the cleaning component together with the onium salt (A), it is possible to form a monomolecular film composed of the onium salt (A) on the substrate while removing components remaining on the substrate. This allows the step of removing components remaining on the substrate before forming the monomolecular film and the step of forming the monomolecular film to be carried out in a single step, which is advantageous in that it can simplify the semiconductor manufacturing process.

[0062] From the viewpoint of forming a high-density film on the substrate using the onium salt (A) while obtaining a sufficient cleaning effect on the substrate surface, the molecular weight of the cleaning component is preferably smaller than the molecular weight of the onium salt (A). Specifically, the molecular weight of the cleaning component is preferably 300 or less, more preferably 200 or less, even more preferably 100 or less, and even more preferably 80 or less. Moreover, the molecular weight of the cleaning component is preferably 10 or more, more preferably 15 or more.

[0063] Examples of cleaning components include fluorine-containing compounds, hydrogen peroxide, citric acid, ethylenediaminetetraacetic acid (EDTA), or two or more of these. Specific examples of fluorine-containing compounds include hydrofluoric acid (hydrofluoric acid), ammonium fluoride, tetramethylammonium fluoride, and hexafluorosilicic acid. Fluorine-containing compounds are preferably used as cleaning components because of their high cleaning effect.

[0064] When a cleaning component is blended into the surface-modifying composition, the content of the cleaning component is preferably 0.0001% by mass or more, and more preferably 0.001% by mass or more, relative to the total amount of the surface-modifying composition, from the viewpoint of obtaining a sufficient cleaning effect on the substrate. Furthermore, from the viewpoint of not interfering with the selective modification of the substrate surface by the onium salt (A), the content of the cleaning component is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less, relative to the total amount of the surface-modifying composition.

[0065] In addition to the above, other components that may be blended into the surface modifying composition include antioxidants, etc. The blending amounts of the other components can be appropriately selected depending on each component within a range that does not impair the effects of the present disclosure.

[0066] Considering the application of the surface-modifying composition to a semiconductor manufacturing process, the surface-modifying composition preferably has a low metal content. Specifically, the total amount of sodium, potassium, and calcium contained in the surface-modifying composition is preferably 3.0 ppm or less, more preferably 2.5 ppm or less, even more preferably 1.0 ppm or less, even more preferably 0.5 ppm or less, and particularly preferably 0.1 ppm or less. The metal content in the surface-modifying composition is a value measured by inductively coupled plasma mass spectrometry (ICP-MS).

[0067] The surface-modifying composition can be prepared by mixing the onium salt (A), water, and other components that are blended as necessary, and dissolving the onium salt (A) etc. in the water. The solids concentration of the surface-modifying composition (i.e., the proportion of the total mass of the components other than the solvent component in the surface-modifying composition to the total mass of the surface-modifying composition) is preferably 0.0001 to 0.30% by mass, and more preferably 0.0002 to 0.15% by mass, from the viewpoint of forming a high-density film while ensuring good coatability.

[0068] <Compound Represented by Formula (3)> According to the present disclosure, there is provided a compound represented by the following formula (3). (In formula (3), R 7 and R 8are each independently an alkyl group having 16 to 22 carbon atoms. - is R 5 SO 3 - or R 5 SO 2 N - R 6 It is. 5 is a monovalent fluorinated hydrocarbon group. 6 is a monovalent organic group having one or more carbon atoms.

[0069] In the above formula (3), R 7 or R 8 The alkyl group having 16 to 22 carbon atoms represented by the formula (3) is preferably linear. In terms of being able to form a film having excellent heat resistance while ensuring the ease of synthesis of the compound represented by the formula (3), R 7 and R 8 are preferably the same group.

[0070] X - Specific examples of the anion include the R 3 SO 3 - and R 3 SO 2 N - R 4 The same groups as those shown below can be mentioned. - Among these, a methanesulfonate anion, a trifluoromethanesulfonate anion, a vinylsulfonate anion, a p-vinylbenzenesulfonate anion, a p-toluenesulfonate anion, an o-nitrobenzenesulfonate anion, or a bis(trifluoromethanesulfonyl)imide anion is preferred, and a trifluoromethanesulfonate anion or a bis(trifluoromethanesulfonyl)imide anion is more preferred.

[0071] Preferred specific examples of the compound represented by the above formula (3) include compounds represented by the following formulas (3-1) to (3-6). (In formulas (3-1) to (3-6), Tf represents a trifluoromethylsulfonyl group.)

[0072] <Method for producing a surface-treated substrate and method for selectively modifying a substrate surface> Next, a method for producing a surface-treated substrate and a method for selectively modifying a substrate surface, which are carried out using the above-mentioned surface-modifying composition, will be described. The method for producing a surface-treated substrate and the method for selectively modifying a substrate surface according to the present disclosure include a coating step of coating the surface of the substrate with the surface-modifying composition.

[0073] Coating Process (Substrate) As the substrate, a substrate having a surface layer including a first region and a second region made of a material different from that of the first region can be preferably used. The first region is preferably made of a different material from the second region, thereby differing in adsorption ability of the onium salt (A) from that of the second region. For example, the first region is a region having a higher adsorption ability of the onium salt (A) than the second region. From the viewpoint of selectively and densely modifying the surface of the substrate with the onium salt (A), the first region is preferably formed of a conductive material, and the second region is preferably formed of an insulating material. Furthermore, the substrate to be selectively modified with the surface-modifying composition preferably has a first region formed of a conductive material and a second region formed of an insulating material.

[0074] When the first region is a region formed of a conductive material, the first region contains a metal element. Examples of the metal element include at least one selected from the group consisting of copper, iron, zinc, cobalt, aluminum, titanium, tin, tungsten, zirconium, tantalum, germanium, molybdenum, ruthenium, gold, silver, platinum, palladium, and nickel. The metal element contained in the first region may be a simple metal, an alloy (nickel-copper alloy, cobalt-nickel alloy, gold-silver alloy, etc.), a conductive nitride (tantalum nitride, titanium nitride, etc.), or the like. Among these, the first region preferably contains a simple metal, an alloy, or a conductive nitride, more preferably at least one selected from the group consisting of copper, cobalt, tungsten, tantalum, titanium, molybdenum, and ruthenium, and even more preferably at least one selected from the group consisting of tungsten, tantalum, titanium, and ruthenium.

[0075] When a substrate is surface-treated with a surface-modifying composition, the type of onium salt (A) contained in the surface-modifying composition may be appropriately selected depending on the metal species contained in the first region. When the nitrogen-containing heterocycle contained in the onium salt (A) is an aromatic heterocycle, from the viewpoint of highly selectively forming a high-density film on the substrate surface, the first region preferably contains at least one selected from the group consisting of tungsten, cobalt, copper, molybdenum, and ruthenium, and more preferably contains at least one selected from the group consisting of tungsten and ruthenium. Furthermore, when the first region contains at least one selected from the group consisting of tungsten, cobalt, copper, molybdenum, and ruthenium, the onium salt (A) preferably contains an aromatic heterocycle as the nitrogen-containing heterocycle, and more preferably contains an imidazole ring, benzimidazole ring, thiazole ring, benzothiazole ring, oxazole ring, or benzoxazole ring.

[0076] When the second region is formed of an insulating material, the second region may be formed of a silicon-containing compound such as silicon oxide, silicon nitride, silicon oxynitride, or silicide (e.g., SiO 2 , SiOC, Si 3 N 4 The second region is preferably formed of a silicon oxide, a silicon nitride, a silicon oxynitride, a silicide, or a metal oxide (e.g., silicon nitride, silicon oxynitride, silicide, or metal oxide).

[0077] In particular, when the substrate to which the surface modification composition is applied has, as the first region, a region containing at least one element selected from the group consisting of tungsten, tantalum, titanium, molybdenum, and ruthenium, and has, as the second region, a region containing silicon oxide, silicon nitride, silicon oxynitride, or a metal oxide, the surface modification composition is suitable in that the onium salt (A) can be highly selectively and densely adsorbed to the first region out of the first and second regions.

[0078] The shape of the coated surface of the substrate is not particularly limited. The coated surface may be, for example, flat, arc-shaped, concave, or protruding. Furthermore, when the coated surface has a first region and a second region, the arrangement of the first region and the second region is not particularly limited. For example, the first region and the second region may be arranged adjacent to each other in a predetermined direction on a plane. Alternatively, multiple first and second regions may be arranged within one of the other regions. Furthermore, one of the first and second regions may form the bottom surface of a hole or groove formed in the substrate, and the other may form the side surface thereof.

[0079] The surface of the substrate to which the film-forming composition is applied may be coated with, for example, H 2 , N 2 and H 2 Mixture of gas with O 2 Pretreatment such as plasma treatment using gas or the like, cleaning treatment of the substrate surface, or wet modification treatment may be performed.

[0080] (Coating Method) Examples of methods for coating the surface-modifying composition on the surface of a substrate include spraying, roll coating, spin coating, slit die coating, bar coating, and inkjet coating. Among these, it is preferable to coat the surface of a substrate with the surface-modifying composition by spin coating, slit die coating, or bar coating. The thickness of the coating film formed on the substrate can be appropriately set so that the thickness of the film finally formed on the substrate is the desired thickness.

[0081] By applying the surface-modifying composition to the surface of the substrate in the coating process, a film (specifically, a monomolecular film) of the onium salt (A) is formed on the first region. After applying the surface-modifying composition to the substrate surface, the solvent component in the surface-modifying composition may be removed by natural drying, thereby forming a film on the first region. Alternatively, a heat treatment may be performed to remove the solvent component from the surface-modifying composition applied to the substrate surface. The heat treatment may be performed using a heating device such as an oven or a hot plate. The heating temperature is, for example, 40°C or higher, and may be 50°C or higher. The heating time is, for example, 0.5 to 60 minutes. The onium salt (A) has high adsorption ability to metals, allowing a film to be formed on the first region without heat treatment, which is advantageous in that it simplifies the manufacturing process. The thickness of the film formed on the substrate is, for example, several nanometers (e.g., approximately 0.5 to 20 nm).

[0082] Preferably, the method of the present disclosure further includes a step (hereinafter also referred to as a "cleaning step") of contacting the surface of the substrate with a rinse solution after coating with the surface-modifying composition in the coating step described above, thereby cleaning the substrate surface and thereby removing components derived from the surface-modifying composition from the second region. This cleaning step can remove residues from the second region of components derived from the surface-modifying composition (more specifically, the composition itself, the onium salt (A), a residual film formed by the composition, etc.) that remain on the second region. This allows the region of the substrate surface to be protected to be more selectively coated with a film formed by the onium salt (A), thereby selectively protecting the substrate surface.

[0083] Cleaning Step: An organic solvent can be preferably used as the rinse solution. Specific examples of organic solvents used as the rinse solution include at least one selected from the group consisting of alcohols, ethers, ketones, sulfones, amides, cyclic amines, lactams, and esters. Further specific examples of the rinse solution include propylene glycol monomethyl ether acetate, isopropanol, acetone, methyl ethyl ketone, methyl-n-propyl ketone, and mixed solvents of two or more of these.

[0084] Components derived from the surface-modifying composition on the second region can be removed from the second region using a rinse liquid by contacting the substrate surface after the coating step with the rinse liquid. The method for contacting the substrate surface with the rinse liquid is not particularly limited, and examples of applicable methods include showering, spraying, dipping, and puddling. When contacting the substrate surface with the rinse liquid, for example, the rinse liquid may be supplied to the substrate and contacted multiple times, or the rinse liquid or the substrate may be shaken. The temperature of the rinse liquid when contacting the substrate surface with the rinse liquid is, for example, 5 to 50°C. The contact time is, for example, 5 seconds to 30 minutes. The amount of rinse liquid used can be appropriately determined taking into account the method for contacting the substrate surface with the rinse liquid. After contacting the substrate surface with the rinse liquid, a further treatment to remove the rinse liquid from the substrate may be performed using a spin coater or the like.

[0085] The method including the coating step and washing step described above allows the substrate surface to be surface-modified highly selectively and densely by a simple treatment. In the method for producing a substrate according to the present disclosure, the substrate obtained by the coating step and the optionally included washing step may be further subjected to various treatments, for example, the following steps (contact step, metal layer formation step, film removal step).

[0086] Contacting Step The contacting step is a step of contacting the substrate surface with alcohol, dilute acid, hydrogen peroxide, ozone, plasma, ammonia, or an ammonium fluoride salt aqueous solution after forming a film on the first region in the coating step (preferably, the substrate surface after contact with the rinse solution in the cleaning step). In the manufacturing process of semiconductors, etc., an oxide film layer may be formed on the surface of the substrate that comes into contact with air (on the second region). Therefore, by providing the contacting step, the oxide film layer formed on the second region can be removed. Among the above, examples of dilute acids include dilute hydrochloric acid, dilute sulfuric acid, dilute citric acid, dilute oxalic acid, dilute maleic acid, dilute acetic acid, dilute isobutyric acid, and dilute 2-ethylhexanoic acid.

[0087] Metal Layer Formation Step The metal layer formation step is a step of forming a metal layer on the second region after forming a film on the first region in the coating step (preferably after contact with a rinse solution in the cleaning step, more preferably after the contact step). After the cleaning step, the first region of the substrate surface is covered with a protective film (monomolecular film) formed from the onium salt (A). Therefore, when forming a metal layer in the metal layer formation step, the metal layer can be selectively formed on the second region of the first and second regions. The method for forming the metal layer is not particularly limited, but from the viewpoint of highly selective pattern formation in fine regions, it is preferable to form a metal pattern by chemical vapor deposition (CVD) or atomic layer deposition (ALD). The metal layer formed on the second region may be a barrier layer for separating the metal portion from the insulating portion or for suppressing metal diffusion from the metal portion. The thickness of the metal layer can be appropriately set depending on the application of the substrate, and is, for example, 1 to 30 nm.

[0088] Film Removal Step The film removal step is a step of removing the film formed on the first region after the metal layer is formed on the second region in the metal layer formation step. The film can be removed by etching. Examples of etching methods include known methods such as reactive ion etching (RIE) and physical etching. Examples of reactive ion etching include CF 4 Ya O 2 Examples of the etching method include chemical dry etching, which uses a gas or the like and utilizes the difference in etching rate between layers; and chemical wet etching (wet development), which uses a liquid etching solution such as an organic solvent or hydrofluoric acid. Examples of physical etching include sputter etching and ion beam etching. Of these, reactive ion etching is preferred, and chemical dry etching or chemical wet etching is more preferred.

[0089] Examples of solvents used in chemical wet etching include acetic acid, APM (a mixture of ammonia, hydrogen peroxide, and water), SPM (a mixture of sulfuric acid and hydrogen peroxide), a 2.38% by mass TMAH aqueous solution, diluted hydrofluoric acid, and water.

[0090] By carrying out the above steps (coating step, cleaning step, contact step, metal layer forming step, and film removing step), a metal layer is selectively formed on the second region out of the first and second regions, and a substrate can be produced in which the surface (e.g., the metal surface) of the first region is exposed. The obtained substrate may further be subjected to various treatments such as plating. When plating is performed, the plating method is not particularly limited, and known electroplating, electroless plating, hot-dip plating, vacuum plating, vapor-phase plating, etc. can be used. When the method of the present disclosure is applied to a semiconductor manufacturing process, electroplating or electroless plating is preferred. After plating, if necessary, the substrate surface may be planarized (CMP treatment, etc.).

[0091] The present disclosure described above provides the following aspects. [Aspect 1] A method for producing a surface-treated substrate, comprising the step of selectively modifying the surface of a substrate by applying a composition to the surface of the substrate, the composition containing an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition. [Aspect 2] A method for selectively modifying a substrate surface, comprising the step of applying a composition to the surface of the substrate, the composition containing an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition. [Aspect 3] The method of [Aspect 1] or [Aspect 2], wherein the substrate includes a first region and a second region made of a material different from that of the first region, and the composition is applied to the surface of the substrate including the first region and the second region to form a film on the first region. [Aspect 4] The method of [Aspect 3], wherein the first region is formed of a conductive material, and the second region is formed of an insulating material. [Aspect 5] The method of [Aspect 3] or [Aspect 4], further comprising the step of contacting the surface of the substrate with a rinse solution after application of the composition to remove components derived from the composition on the second region. [Aspect 6] The method of [Aspect 5], further comprising the step of contacting the surface of the substrate after contact with the rinse solution with an alcohol, a dilute acid, hydrogen peroxide, ozone, plasma, ammonia, or an aqueous solution of ammonium fluoride salt. [Aspect 7] The method of [Aspect 5] or [Aspect 6], further comprising the step of forming a metal layer on the second region after contact with the rinse solution. [Aspect 8] The method of [Aspect 7], further comprising the step of removing the film formed from the composition on the first region after formation of the metal layer. [Aspect 9] The method of any one of [Aspects 1] to [Aspect 8], wherein the onium salt comprises an organic cation and an anion, and the organic cation has the nitrogen-containing heterocycle and the monovalent organic group having 4 or more carbon atoms. [Aspect 10] The anion is selected from the group consisting of a halide ion, PF 6 - , B.F. 4 - , SbF 6 - , C.N. - , (CN) 2 N- , SCN - , R 3 SO 3 - , R 3 COO - or R 3 SO 2 N - R 4 (However, R 3 and R 4 are each independently a monovalent organic group having one or more carbon atoms. [Aspect 11] The method of any one of [Aspect 1] to [Aspect 10], wherein the monovalent organic group having four or more carbon atoms is bonded to a nitrogen atom constituting the nitrogen-containing heterocycle. [Aspect 12] The method of any one of [Aspect 1] to [Aspect 11], wherein the nitrogen-containing heterocycle is an imidazole ring, a benzimidazole ring, a thiazole ring, a benzothiazole ring, an oxazole ring, or a benzoxazole ring. [Aspect 13] The method of any one of [Aspect 1] to [Aspect 12], wherein the nitrogen-containing heterocycle has a partial structure represented by the above formula (1). [Aspect 14] The method of any one of [Aspect 1] to [Aspect 12], wherein R in the above formula (1) 1 and R 2and are the same group. [Aspect 15] The method of any one of [Aspect 1] to [Aspect 14], wherein the composition further contains a pH adjuster. [Aspect 16] The method of [Aspect 15], wherein the pH adjuster is an organic acid, an organic base, or ammonia. [Aspect 17] The method of [Aspect 16], wherein the pH adjuster is a carboxy group-containing chain compound, a chain monoamine compound, or ammonia. [Aspect 18] The method of any one of [Aspect 1] to [Aspect 17], wherein the monovalent organic group having 4 or more carbon atoms is a monovalent hydrocarbon group or a halogenated hydrocarbon group. [Aspect 19] The method of any one of [Aspect 1] to [Aspect 18], wherein the composition further contains an organic solvent, and the content of the organic solvent in the composition is 60 mass % or less based on the total amount of the composition. [Aspect 20] The method of [Aspect 19], wherein the organic solvent contained in the composition is at least one selected from the group consisting of alcohols, ethers, ketones, sulfones, amides, cyclic amines, lactams, and esters. [Aspect 21] A composition used for selectively modifying a substrate surface, comprising an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition. [Aspect 22] A compound represented by the above formula (3).

[0092] The present disclosure will be specifically described below based on examples, but the present disclosure is not limited to these examples. Measurement methods for each physical property value are shown below.

[0093] <Synthesis of Onium Salt (A)>

[0094] The structural formulae of onium salts (A-1) to (A-14) obtained in the following synthesis examples are shown below: In the following formulae, "Tf" represents a trifluoromethylsulfonyl group, and "Ms" represents a methylsulfonyl group.

[0095] Synthesis Example 1 Synthesis of 1,3-didodecylimidazole bromide (onium salt (A-1)) 2.38 g (35 mmol) of imidazole, 24.9 g (100 mmol) of 1-bromododecane, 1.51 g (11 mmol) of potassium carbonate, and 150 mL of methyl ethyl ketone were added to a 300 mL three-neck flask and stirred for 7 hours under heated dry distillation in a nitrogen atmosphere. After the reaction was completed, the mixture was returned to room temperature, the salt was removed using pleated filter paper, and the filtrate was recovered. The filtrate was concentrated under reduced pressure using an evaporator to obtain a concentrate. 150 mL of methylene chloride and 150 mL of ultrapure water were added to the concentrate, and the mixture was washed three times with water. The organic layer was recovered and dehydrated using anhydrous sodium sulfate. The filtrate was recovered using pleated filter paper and concentrated under reduced pressure using an evaporator. 150 mL of acetonitrile, 135 mL of hexane, and 15 mL of diisopropyl ether were added to the concentrate, and liquid-liquid purification was performed. The lower acetonitrile layer was collected and concentrated to obtain the target product. 1 H NMR, 13 C NMR was used. 1 H NMR (CDCl3, 400MHz); δ 10.86 (imidazole, position-2, 1H, s), 7.23 (imidazole, position-4,5, 2H, s), 4.36 (CH2, 4H, q), 1.92 (CH2, 4H, m), 1.33-1.24 (CH2, 36H, br), 0.88 (CH3, 6H, t). 13 C NMR (CDCl3, 100MHz); δ 137.7, 121.6, 50.3, 31.9, 30.4, 29.6, 29.5, 29.4, 29.3, 29.1, 26.3, 22.8, 14.2.

[0096] Synthesis Example 2 Synthesis of 1,3-dihexadecylimidazole bromide (onium salt (A-2)) 100 mL of acetone, 3.40 g (50 mmol) of imidazole, 15.3 g (50 mmol) of 1-bromohexadecane, and 13.8 g (100 mmol) of potassium carbonate were added to a 300 mL three-neck flask equipped with a Dimroth condenser, and the mixture was refluxed at 72°C for 7 hours under a nitrogen atmosphere. After completion of the reaction, salts were removed by filtration through pleated filter paper. 100 mL each of methylene chloride and purified water (DIW) was added, and the mixture was washed three times with water. The organic layer was recovered, dried over anhydrous sodium sulfate, and the filtrate was recovered by filtration through pleated filter paper and concentrated using an evaporator. The resulting mixture was then purified by column chromatography (methylene chloride / methanol = 10 / 1 (vol %)). 4.97 g (17 mmol) of N-hexadecyl imidazole and 4.21 g (17 mmol) of hexadecyl bromide were added to a 200 mL eggplant-shaped flask equipped with a Dimroth condenser, and the mixture was heated and stirred in 100 mL of acetonitrile under a nitrogen atmosphere at 92°C. After the reaction was completed and concentrated, 200 mL of diisopropyl ether was added to cause crystallization, and the mixture was stirred at room temperature for 0.5 hours to dissolve only the components derived from the raw materials. The precipitate was then recovered using a Buchner funnel, washed with diisopropyl ether, and the white solid was dried in a vacuum dryer. The structure was confirmed. 1 H NMR, 13 C NMR was used. 1 H NMR (CDCl3, 400MHz); δ 10.75 (imidazole, position-2, 1H, s), 7.31 (imidazole, position-4,5, 2H, s), 4.36 (CH2, 4H, q), 1.92 (CH2, 4H, m), 1.33-1.24 (CH2, 52H, br), 0.88 (CH3, 6H, t). 13 C NMR (CDCl3, 100MHz); δ 137.1, 129.5, 118.8, 47.1, 32.0, 31.2, 29.8, 29.7, 29.6, 29.5, 29.4, 29.

[0097] Synthesis Example 3 Synthesis of 1,3-dihexadecylimidazol-3-ium trifluoromethanesulfonate (onium salt (A-3)) 2.0 g (3.55 mmol) of 1,3-dihexadecylimidazole, 0.66 g (3.35 mmol) of potassium trifluoromethanesulfonate, 50 mL of methylene chloride, and 50 mL of DIW were added to a 200 mL recovery flask and stirred at room temperature under air for 4 hours or more. After completion of the reaction, the mixture was washed with water three times, and the methylene chloride layer was recovered and dried over anhydrous sodium sulfate, then concentrated in an evaporator, and dried in a vacuum dryer. The structure was confirmed. 1 H NMR, 13 C NMR, 19 F NMR was used. 1 H NMR (CDCl3, 400MHz); δ 9.32 (imidazole ring-2 position), 7.27 (imidazole ring-3,4-position), 4.23 (CH2, 4H, q), 1.88 (CH2, 4H, m), 1.31-1.16 (CH2, 52H, m), 0.88 (CH3, 6H, t). 13 C NMR (CDCl3, 100MHz); δ 151.7, 121.8, 50.3, 32.0, 30.2, 29.8 29.7, 29.6, 29.5, 29.4, 29.0, 26.2, 22.7, 14.2. 19 F NMR (CDCl3, 97MHz); δ-78.3.

[0098] Synthesis Example 4 Synthesis of 1,3-dihexadecylimidazol-3-ium bistrifluoromethanesulfonimide (onium salt (A-6)) 1.5 g (2.5 mmol) of 1,3-dihexadecylimidazole, 0.7981 g (2.5 mmol) of potassium bistrifluoromethanesulfonimide, 50 mL of methylene chloride, and 50 mL of DIW were added to a 200 mL recovery flask and stirred at room temperature under air for 4 hours or more. After completion of the reaction, the mixture was washed with water three times, and the methylene chloride layer was recovered and dried over anhydrous sodium sulfate, then concentrated in an evaporator, and dried in a vacuum dryer. The structure was confirmed. 1 H NMR, 13 C NMR,19 F NMR was used. 1 H NMR (CDCl3, 400MHz); δ 8.86 (imidazole ring-2 position), 7.30 (imidazole ring-3,4-position), 4.19 (CH2, 4H, q), 1.86 (CH2, 4H, m), 1.31-1.16 (CH2, 52H, m), 0.88 (CH3, 6H, t). 13 C NMR (CDCl3, 100MHz); δ 135.7, 122.2, 50.3, 32.0, 30.2, 29.8 29.7, 29.6, 29.5, 29.4, 28.9, 26.2, 22.7, 14.2. 19 F NMR (CDCl3, 97MHz); δ-78.6.

[0099] Synthesis Examples 5 to 14 Onium salts (A-4), (A-5), and (A-7) to (A-14) were also synthesized in the same manner as above.

[0100] <Preparation of Surface-Modifying Composition> The components used in preparing the surface-modifying composition are as follows: Low-molecular-weight compounds A-1 to A-14: the above-described onium salts (A-1) to (A-14) A-15: Emal 0 (manufactured by Kao Corporation, anionic surfactant, sodium lauryl sulfate)

[0101] (B) pH adjuster B-1: Monoethanolamine B-2: 25% aqueous ammonia solution B-3: Citric acid B-4: Malonic acid B-5: cis-2-butenedioic acid B-6: Potassium hydroxide B-7: N-propylpiperazine-N'-ethanesulfonic acid

[0102] (C) Solvent C-1: Water C-2: Diethylene glycol mono-n-butyl ether C-3: Diethylene glycol monomethyl ether C-4: 2-methoxy-1-propanol C-5: Ethylene glycol mono-n-butyl ether C-6: Sulfolane C-7: Gamma butyrolactone

[0103] 1. Preparation of Surface-Modifying Composition [Example 1] 99.95 g of solvent (C-1) was added to 0.05 g of onium salt (A-1) and stirred, and then filtered through a high-density polyethylene filter having 0.45 μm pores to prepare a composition (SM-1) with a solids concentration of 0.050%.

[0104] Examples 2 to 16 and Comparative Examples 1 to 3 Compositions (SM-2) to (SM-16) and compositions (SR-1) to (SR-3) were prepared in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1. The amount of compound (B-2) represents the amount of aqueous ammonia solution.

[0105]

[0106] 2. Evaluation The following evaluations were carried out using compositions (SM-1) to (SM-16) and compositions (SR-1) to (SR-3) prepared in 1. The results are shown in Table 2.

[0107] <Evaluation of Solubility> The solubility of each composition obtained in 1 above was visually observed, and a rating of "good (◯)" was given when transparency was present, and a rating of "poor (×)" was given when at least one of cloudiness and residual dissolution was observed.

[0108] <Evaluation of Foaming Resistance> Each composition obtained in 1 above was subjected to rotational stirring at a speed of 500 rpm in a ball mill for 30 minutes, and then allowed to stand, and the time until the foam disappeared was measured. If the foam disappeared within 1 minute, it was rated as "good (○)", if the foam disappeared in more than 1 minute but less than 3 minutes, it was rated as "fair (△)", and if it took 3 minutes or more for the foam to disappear, it was rated as "poor (×)".

[0109] <Evaluation of Coatability> The coatability of each composition was evaluated using the following substrates: W: 8-inch tungsten substrate, Ru: 8-inch ruthenium substrate, Al: 8-inch tungsten substrate, 2 O 3: 8-inch alumina substrate, SiN: 8-inch silicon nitride substrate, low-k: low-dielectric silicon oxide substrate. These substrates were obtained from Advantec Co., Ltd. The various substrates listed above were cut into 3 cm x 3 cm pieces, and each composition prepared in 1. above was spin-coated using a spin coater ("MS-B300" manufactured by Mikasa Co., Ltd.) at 1,500 rpm for 20 seconds (coating step). The coated substrates were then baked at 150°C for 180 seconds. Thereafter, the substrates were washed using propylene glycol monomethyl ether acetate as a rinse (washing step). In the washing step, if the components in the composition are not adsorbed to the substrate surface, the composition is removed by the rinse, and no film is formed on the substrate. The coated surface of the substrate was observed using an optical microscope to check for the presence or absence of voids and film breaks on the film surface. Those with no voids or membrane ruptures were rated "good (◯)", those with voids but no membrane ruptures were rated "fair (△)", and those with both voids and membrane ruptures were rated "poor (x)".

[0110] <Evaluation of Selective Modification by Static Contact Angle> Various substrates used to evaluate coatability were cut into 3 cm x 3 cm pieces, and each composition prepared in 1 above was spin-coated using a spin coater ("MS-B300" manufactured by Mikasa Co., Ltd.) at 1,500 rpm for 20 seconds. The substrates were then washed with isopropyl alcohol. The static contact angle of the coated surface of the washed substrates was measured using a contact angle meter ("Drop master DM-501" manufactured by Kyowa Interface Science Co., Ltd.). It can be said that a film is selectively formed on a substrate where the static contact angle is significantly increased compared to the static contact angle of the substrate (Reference Example 1) before surface treatment with the surface-modifying composition.

[0111] <Evaluation of storage stability> 10 g of each surface modifying composition prepared in 1 above was placed in a vial and stored for 2 weeks at 50° C. The change in viscosity before and after the storage stability test was represented as Δη, with a change in viscosity of less than 1 Pa s being rated "good (○)", a change in viscosity of 1 Pa s or more but less than 3 Pa s being rated "fair (△)", and a change in viscosity of 3 Pa s or more being rated "poor (×)".

[0112] <Evaluation of Metal Corrosion Resistance (Evaluation by Etching Rate)> A wafer piece with a 100 nm-thick ruthenium film and a wafer piece with a 200 nm-thick molybdenum film were each cut into 30 mm × 10 mm pieces to prepare wafer pieces for etching rate evaluation (hereinafter also referred to as "evaluation wafer pieces"). Each composition prepared in 1. above was heated to 60°C, and the evaluation wafer piece was immersed in each composition for 5 minutes. Thereafter, the evaluation wafer piece was removed and washed with running water, and the thicknesses of the ruthenium film and molybdenum film were measured. The thicknesses of the ruthenium film and molybdenum film were calculated using the following formula, with the resistance measured by a DC four-probe method using a resistivity meter (manufactured by KLA Tencor Corporation, model "RS-100") and the obtained resistance value (hereinafter referred to as "sheet resistance value"; unit: Ω / sq) and the volume resistivity of ruthenium or molybdenum. Ruthenium film thickness (nm) = [volume resistivity of ruthenium film (Ω·m) ÷ sheet resistance value (Ω / sq)] × 10 9 Molybdenum film thickness (nm) = [volume resistivity of molybdenum film (Ω·m) ÷ sheet resistance value (Ω / sq)] × 10 9The etching rate was calculated from the change in thickness of the ruthenium or molybdenum film before and after immersion in the surface-modifying composition using the following formula: Etching rate of ruthenium film (nm / min) = (thickness of ruthenium film before etching (nm) - thickness of ruthenium film after etching (nm)) / etching time (min) Etching rate of molybdenum film (nm / min) = (thickness of molybdenum film before etching (nm) - thickness of molybdenum film after etching (nm)) / etching time (min) The evaluation criteria for the etching rate of the ruthenium film are as follows. The lower the etching rate of the ruthenium film, the better the metal corrosion resistance of the surface-modifying composition. (Evaluation Criteria) A: When the etching rate was less than 1.5 nm / min, it was judged to be very good. B: When the etching rate was 1.5 nm / min or more but less than 3 nm / min, it was judged to be good because it was practically usable. C: When the etching rate was 3 nm / min or more, it was judged to be poor because the etching rate was too high and difficult to use in practice. The evaluation criteria for the etching rate of the molybdenum film are as follows. The lower the etching rate of the molybdenum film, the better the metal corrosion resistance of the surface modifying composition. (Evaluation Criteria) A: If the etching rate is less than 20 nm / min, it is judged as very good. B: If the etching rate is 20 nm / min or more, it is judged as poor because the etching rate is too high and difficult to use.

[0113] <Evaluation of Metal Oxide Blocking Performance (Evaluation of ALD Resistance)> A metal oxide blocking evaluation was performed on a tungsten substrate (W substrate) surface-coated with each of the surface modification compositions prepared in 1 above (referred to as "surface-treated substrate") to evaluate the degree of inhibition of oxide layer formation by ALD. As a control, a W substrate (referred to as "untreated substrate") that had not been surface-treated with each of the surface modification compositions was used, and ALD was performed in the same manner as for the surface-treated substrate. ALD was performed using Cambridge Nanotech FIJI at Stanford University under the conditions shown below. Trimethylaluminum was used as the precursor, and water was used as the co-catalyst. The ALD cycle was fixed at 47 cycles. (ALD Conditions) Film Type: ALD Al2 O 3 Chamber: Cambridge Nanotech Fiji Stage temperature: 200°C Treatment time: 0.3 seconds Trimethylaluminum / 15 seconds Purge / 0.06 seconds Water / 23 seconds Purge Thickness on W substrate: 5.4 nm (ellipsometry) Loading: Cool the stage for 5 minutes before loading Queue time: Within 3 hours after removal The Al component on the substrate surface of the W substrate (surface-treated substrate and untreated substrate) after ALD was quantified by X-ray photoelectron spectroscopy (ESCA). ESCA was performed using ULVAC's "Quantum 2000" and the Al component excluding the film component and substrate component under the 100 μmφ condition was quantified using Al2p (72-78 eV). The quantitative value of the Al component measured on an untreated substrate was then used as a reference value, and the degree to which the quantitative value of the Al component on the surface-treated substrate had decreased from the reference value was calculated, and this was taken as the blocking rate (%). The larger the blocking rate, the more likely it is that the film formed on the W substrate using the surface-modifying composition is formed by the components (low-molecular-weight compounds in Table 1) in the surface-modifying composition being adsorbed to the W substrate surface at a high density, and the higher the blocking performance against metal oxide formation by ALD. A blocking rate of 98% or more was rated "good (○)," a blocking rate of less than 98% but 90% or more was rated "fair (△)," and a blocking rate of less than 90% was rated "poor (×)."

[0114] <Measurement of Metal Content> Each composition was diluted 20 times with diethylene glycol butyl ether / ultrapure water = 80 / 20 (parts by mass), and the metal contents of sodium, potassium, and calcium were measured using a NexION 5000 ICP mass spectrometer (manufactured by Perkin Elmer). The evaluation was made as "good (○)" when the total amount of sodium, potassium, and calcium was 125 ppb or less, "fair (△)" when it was more than 125 ppb and 150 ppb or less, and "unacceptable (×)" when it was more than 150 ppb.

[0115]

[0116] As can be seen from the above results, the surface-modifying compositions of Examples 1 to 16, which used an onium salt (A) as a film-forming material and contained water, exhibited good solubility of the onium salt (A) in water, and also exhibited good foaming resistance, coatability, and storage stability. Furthermore, the results of evaluating the selective modification and ALD resistance using static contact angles indicate that the surface-modifying compositions of Examples 1 to 16 were able to form films with high selectivity and density on metal surfaces. Furthermore, the films formed by the surface-modifying compositions of Examples 1 to 16 exhibited good metal corrosion resistance. Furthermore, by further blending a pH adjuster with the onium salt (A) and water, surface-modifying compositions with improved storage stability were obtained (Examples 2 to 16).

[0117] Furthermore, when onium salts (A-1) to (A-9) were used as film-forming materials, ALD resistance was better than when onium salts (A-10) to (A-12) were used. Among these results, a comparison with the case where onium salts (A-10) or (A-11) were used shows that when the nitrogen-containing heterocycle in onium salt (A) is an imidazole ring, a benzimidazole ring, a thiazole ring, or a benzothiazole ring, a higher-density film can be formed. Furthermore, a comparison with the case where onium salt (A-12) was used shows that when a hydrogen atom is bonded to a carbon atom constituting a carbon-nitrogen double bond in the nitrogen-containing heterocycle in onium salt (A), a higher-density film can be formed than when a substituent is bonded to the carbon atom.

[0118] In contrast, the surface-modifying composition of Comparative Example 1, which used onium salt (A-13) as the film-forming material, and the surface-modifying composition of Comparative Example 2, which used onium salt (A-14), were insufficient in selective modification of metal surfaces and ALD resistance. Of these, Comparative Example 1 was also rated as poor in metal corrosion resistance to ruthenium, and the metal content was also high. Furthermore, the surface-modifying composition of Comparative Example 3, which used compound (A-15), was inferior to Examples 1 to 16 in selective modification of metal surfaces, metal corrosion resistance, ALD resistance, and foaming resistance, as well as insufficient metal content.

Claims

1. A method for producing a surface-treated substrate, comprising a step of selectively modifying the surface of a substrate by applying a composition to the surface of the substrate, the composition containing an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition.

2. The method for manufacturing a substrate according to claim 1, wherein the substrate includes a first region and a second region made of a material different from that of the first region, and a film is formed on the first region by applying the composition to a surface of the substrate including the first region and the second region.

3. The method for manufacturing a substrate according to claim 2, wherein the first region is formed of a conductive material, and the second region is formed of an insulating material.

4. The method for producing a substrate according to claim 2, further comprising a step of removing components derived from the composition on the second region by contacting the surface of the substrate with a rinsing liquid after application of the composition.

5. The method for producing a substrate according to claim 4, further comprising a step of contacting the surface of the substrate after contact with the rinsing liquid with an alcohol, a dilute acid, a hydrogen peroxide solution, ozone, plasma, ammonia or an aqueous solution of an ammonium fluoride salt.

6. The method for producing a substrate according to claim 4 or 5, further comprising the step of forming a metal layer on the second region after contact with the rinsing liquid.

7. The method for producing a substrate according to claim 6, further comprising the step of removing the film on the first region formed by the composition after the formation of the metal layer.

8. The method for producing a substrate according to claim 1 or 2, wherein the onium salt comprises an organic cation and an anion, and the organic cation has the nitrogen-containing heterocycle and the monovalent organic group having 4 or more carbon atoms.

9. The method for producing a substrate according to claim 8, wherein the monovalent organic group having 4 or more carbon atoms is bonded to a nitrogen atom constituting the nitrogen-containing heterocycle.

10. The anion is a halide ion, PF 6 - , B.F. 4 - , SbF 6 - , C.N. - , (CN) 2 N - , S.C.N. - , R 3 SO 3 - , R 3 COO - Or R 3 SO 2 N - R 4 (However, R 3 and R 4 The method for producing a substrate according to claim 8 , wherein each of the groups independently represents a monovalent organic group having one or more carbon atoms.

11. The method for producing a substrate according to claim 1 or 2, wherein the nitrogen-containing heterocycle is an imidazole ring, a benzimidazole ring, a thiazole ring, a benzothiazole ring, an oxazole ring, or a benzoxazole ring.

12. The method for producing a substrate according to claim 1 or 2, wherein the nitrogen-containing heterocycle has a partial structure represented by the following formula (1): (In formula (1), R 1 is a monovalent organic group. 1 Ha-NR 2 - or a sulfur atom. 2 is a monovalent organic group. 1 -NR 2 In the case of -, R 1 and R 2 At least one of X has 4 or more carbon atoms; 1 When is a sulfur atom, R 1 has 4 or more carbon atoms. "*" represents a bond.) 13. In the above formula (1), R 1 and R 2 The method for producing a substrate according to claim 12 , wherein and are the same group.

14. The method for producing a substrate according to claim 1 or 2, wherein the composition further contains a pH adjuster.

15. The method for producing a substrate according to claim 14, wherein the pH adjuster is an organic acid, an organic base, or ammonia.

16. The method for producing a substrate according to claim 15, wherein the pH adjuster is a carboxy group-containing chain compound, a chain monoamine compound, or ammonia.

17. The method for producing a substrate according to claim 1 or 2, wherein the monovalent organic group having 4 or more carbon atoms is a monovalent hydrocarbon group or a halogenated hydrocarbon group.

18. The method for producing a substrate according to claim 1 or 2, wherein the composition further contains an organic solvent, and the content of the organic solvent in the composition is 60 mass % or less based on the total amount of the composition.

19. The method for producing a substrate according to claim 18, wherein the organic solvent contained in the composition is at least one selected from the group consisting of alcohols, ethers, ketones, sulfones, amides, cyclic amines, lactams, and esters.

20. A method for selectively modifying a substrate surface, comprising a step of applying a composition to the surface of the substrate, the composition containing an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms, and 1 mass % or more of water relative to the total amount of the composition.

21. A composition used for selectively modifying a substrate surface, comprising: an onium salt having a nitrogen-containing heterocycle and a monovalent organic group having 4 or more carbon atoms; and 1 mass % or more of water relative to the total amount of the composition.

22. A compound represented by the following formula (3): (In formula (3), R 7 and R 8 are each independently an alkyl group having 16 to 22 carbon atoms. - is R 5 SO 3 - Or R 5 SO 2 N - R 6 It is. 5 R is a monovalent fluorinated hydrocarbon group. 6 is a monovalent organic group having one or more carbon atoms.

Citation Information

Patent Citations

  • Coating composition

    JP2007070370A

  • Organic thin-film transistor, method of manufacturing the same, and gate-insulating layer used for it

    JP2010219530A

  • Ultraviolet-curable hard coat resin composition simultaneously using metal oxide fine particle and onium salt having halogen as anion, and hard coat layer obtained by curing the same

    JP2014136740A

  • In-situ CMP self-assembled monolayer for enhancing metal-dielectric adhesion and preventing metal diffusion

    US20220115267A1