Photosensitive resin composition, production method for cured relief pattern, and cured film
The photosensitive resin composition, featuring a polyimide with controlled molecular weight and additional components, addresses the challenges of flatness, film stability, and adhesion in semiconductor manufacturing, resulting in high-performance cured films with improved chemical resistance and mechanical properties.
Patent Information
- Application Number
- PCT/JP2024/014790
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional photosensitive resin compositions used in semiconductor manufacturing face challenges in achieving high flatness of pre-baked films, maintaining film thickness stability before and after curing, ensuring excellent adhesion to metal wiring, and minimizing oxygen permeability, particularly in multilayered rewiring structures.
A photosensitive resin composition comprising a polyimide with a specific molecular weight range, a solvent, and a photopolymerization initiator, optionally including radically polymerizable compounds, silane coupling agents, and thermal crosslinking agents, which is formulated to achieve high flatness, stable film thickness, excellent metal adhesion, and low oxygen permeability.
The composition enables the production of cured films with improved chemical resistance, resolution, and mechanical properties, ensuring reliable semiconductor packaging with reduced film shrinkage and enhanced adhesion to metal wiring.
Smart Images

Figure JP2024014790_31102024_PF_FP_ABST
Abstract
Description
Photosensitive resin composition, method for producing cured relief pattern, and cured film
[0001] The present disclosure relates to a photosensitive resin composition, a method for producing a cured relief pattern, and a cured film.
[0002] Resins (e.g., polyimide, polybenzoxazole, and phenolic resins) advantageous in heat resistance, electrical properties, and mechanical properties have been used as insulating materials for electronic components, and passivation films, surface protection films, and interlayer insulating films for semiconductor devices. Among these, those provided in the form of photosensitive resin compositions can easily form relief patterns by applying, exposing, developing, and curing the composition to a ring closure process (e.g., imidization and benzoxazole formation), or by thermal crosslinking of the composition. Therefore, such compositions have the advantage of enabling significant process shortening compared to non-photosensitive compositions, and are therefore suitable for use in the fabrication of semiconductor devices.
[0003] Semiconductor devices (hereinafter sometimes simply referred to as "elements") are mounted on printed circuit boards using various methods depending on their purpose. Conventional elements were often fabricated using wire bonding, which connects the element's external terminals (pads) to a lead frame with thin wires. However, as elements have become faster and their operating frequencies have reached the GHz level, differences in the wiring length (wiring distance) of each terminal during mounting have come to affect the operation of the element. Therefore, while precise control of the mounting wiring length is required for the mounting of elements for high-end applications, it has been difficult to meet this requirement using wire bonding.
[0004] To address this issue, flip-chip mounting has been proposed, in which a redistribution layer is formed on the surface of a semiconductor chip, bumps (electrodes) are formed on the redistribution layer, and then the chip is flipped over and directly mounted on a printed circuit board. Because flip-chip mounting allows for precise control of wiring distance, it is sometimes used in high-end devices that handle high-speed signals, and in mobile phones and other devices due to its compact packaging size, and demand for this technology is rapidly expanding. Recently, fan-out wafer-level packaging (FOWLP) has been proposed, in which individual chips manufactured by dicing a pre-processed wafer are mounted on a support and encapsulated with a molding resin. After the support is peeled off, a redistribution layer is formed thereon (see, for example, Patent Document 1). FOWLP is advantageous for thinning the redistribution layer, which in turn is advantageous for thinning the package, and also has many advantages in terms of high-speed transmission and low cost.
[0005] On the other hand, in FOWLP, the rewiring layer is often multi-layered. Therefore, it has been pointed out that if the flatness of the photosensitive resin composition in the photolithography process, particularly the flatness of the film after prebaking (prebaked film) is poor, the focus depth of the exposure light in the subsequent exposure process is likely to shift, and the resolution is likely to deteriorate. Therefore, the photosensitive resin composition is required to be able to realize, for example, a prebaked film with high flatness.
[0006] Furthermore, due to the structure of the semiconductor package, wiring and a rewiring layer are in contact with each other, and the photosensitive resin composition is required to have adhesion to metal (e.g., copper when the wiring is copper wiring) and high reliability under harsh environments such as high temperature and high humidity (e.g., low elongation and low ion migration).
[0007] For the planarization of the redistribution layer, it is advantageous to improve the flatness of the film (in-plane uniformity) and to suppress the film shrinkage that may occur during heating (curing). As a method advantageous for improving the flatness of the film, for example, it is known to use a polyimide precursor that is highly soluble in a solvent or a low molecular weight polymer. In addition, it is known to be advantageous to form a resin composition using a polyimide that has a closed ring structure in order to suppress the amount of film shrinkage during heating.
[0008] For example, Patent Document 1 discloses a technique for constructing a photosensitive resin composition using a polyimide precursor having a low molecular weight (for example, a weight average molecular weight (Mw) of 3,000 or more and 13,000 or less) and for attempting to improve the flatness of the resulting film. Patent Document 2 discloses a technique for using a polyfunctional (meth)acrylate compound and for attempting to suppress film shrinkage during curing.
[0009] Furthermore, as a method advantageous for improving adhesion to copper, it is known to use a heterocyclic compound to form a photosensitive resin composition. For example, Patent Document 3 discloses a technology for attempting to improve adhesion to a substrate by forming a photosensitive resin composition using a compound having a reactive group such as an epoxy group and a five-membered nitrogen-containing heterocyclic group.
[0010] International Publication No. 2018 / 037997 Japanese Patent Application Laid-Open No. 2021-162834 International Publication No. 2022 / 202907
[0011] However, from the viewpoint of realizing a pre-baked film having excellent flatness, and from the viewpoint of realizing a cured film (cured relief pattern) that satisfies the requirements of being able to suppress a change in film thickness before and after curing, being able to have excellent adhesion to metal wiring, and being able to realize low oxygen permeability, the photosensitive resin compositions described in Patent Documents 1 to 3 have room for improvement.
[0012] Therefore, an object of the present disclosure is to provide a photosensitive resin composition that can realize a prebaked film with excellent flatness, and can also realize a cured film (cured relief pattern) that satisfies the following: the ability to suppress changes in film thickness before and after curing, excellent adhesion to metal wiring, and low oxygen permeability. Another object of the present disclosure is to provide a method for producing a cured relief pattern using such a photosensitive resin composition, and a cured film.
[0013] One aspect of the present invention is as follows: [1] A negative photosensitive resin composition comprising: (A) a polyimide; (B) a solvent; and (C) a photopolymerization initiator, wherein the polyimide (A) is represented by the following general formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group.}, and the polyimide (A) does not have a polymerizable functional group in a side chain, and the weight average molecular weight (Mw) of the polyimide (A) and a molecular weight (Mw) of the polyimide (A) are expressed by the following formula (b): R(F Cont. ) = (Mw f +1) / (Mw x +Mw Y -36)...(b) (In the formula, Mw f is the total mass of fluorine atoms that may be contained in the polyimide (A), Mw X is the molecular weight of the tetracarboxylic dianhydride constituting the polyimide (A), Mw Y is the molecular weight of the diamine constituting the polyimide (A).) and the product {Mw × R(F Cont.)} satisfies the following formula (a): 300≦Mw×R≦948 (a). [2] The photosensitive resin composition according to item 1, wherein the weight-average molecular weight of the (A) polyimide is 8,000 or more and 23,000 or less. [3] The photosensitive resin composition according to item 1 or 2, further comprising a (D) radically polymerizable compound. [4] The photosensitive resin composition according to item 3, wherein the (D) radically polymerizable compound comprises a (D1) monofunctional monomer and a (D2) polyfunctional monomer. [5] The photosensitive resin composition according to item 4, wherein the mass ratio (D1 / D2) of the (D1) monofunctional monomer to the (D2) polyfunctional monomer is more than 0.01 and less than 0.5. [6] The photosensitive resin composition according to item 1 or 2, further comprising at least one selected from the group consisting of (E) a silane coupling agent, (F) an organic titanium compound, (G) a thermal crosslinking agent, (H) a rust inhibitor, (I) a thermal polymerization initiator, and (J) a plasticizer. [7] The photosensitive resin composition according to item 1 or 2, comprising 30 to 1,000 parts by mass of the (B) solvent, and 1 to 30 parts by mass of the (C) photopolymerization initiator, relative to 100 parts by mass of the (A) polyimide. [8] X in formula (1) is selected from the group consisting of the following formulas (2) to (9): [9] The photosensitive resin composition according to item 1 or 2, wherein Y in formula (1) is represented by at least one structure selected from the group consisting of the following formulas (10) to (19):
[10] The photosensitive resin composition according to item 1 or 2, wherein the (A) polyimide has a polymerizable functional group at its terminal.
[11] A method for producing a cured relief pattern, comprising the following steps: (1) applying the photosensitive resin composition according to item 1 or 2 onto a substrate and forming a photosensitive resin layer on the substrate, (2) exposing the photosensitive resin layer to light, (3) developing the exposed photosensitive resin layer and forming a relief pattern, and (4) heat-treating the relief pattern and forming a cured relief pattern.
[12] A cured film comprising a cured product of the photosensitive resin composition according to item 1 or 2.
[13] A negative photosensitive resin composition comprising (A) polyimide, (B) a solvent, and (C) a photopolymerization initiator, wherein the (A) polyimide is represented by the following general formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group.}, and the oxygen permeability (cc / m) of a cured film obtained by heating the composition at 230°C for 2 hours in a nitrogen atmosphere is 2 24h·atm) is less than 1000.
[0014] According to the present disclosure, it is possible to provide a photosensitive resin composition that can realize a prebaked film with excellent flatness, and can realize a cured film (cured relief pattern) that satisfies the following: the ability to suppress change in film thickness before and after curing, excellent adhesion to metal wiring, and low oxygen permeability. Furthermore, according to the present disclosure, it is possible to provide a method for producing a cured relief pattern and a cured film realized using such a photosensitive resin composition.
[0015] FIG. 1 is a schematic diagram for explaining the evaluation method in this example.
[0016] Hereinafter, embodiments of the present disclosure will be described. In this specification, when a plurality of structures represented by the same symbol exist in the same general formula, unless otherwise specified, the structures may be independently selected and may be the same or different from each other. In addition, when a plurality of structures represented by the same symbol exist in different general formulas, unless otherwise specified, the structures may be independently selected and may be the same or different from each other. In this specification, various measurements are performed based on the methods described in the examples unless otherwise specified. In the contents shown in the drawings, the scale, shape, length, etc. may be exaggerated to further improve clarity.
[0017] In this specification, the upper or lower limit of a numerical range described in stages may be replaced by the upper or lower limit of a corresponding numerical range described in another stage, and may also be replaced by a corresponding value described in the Examples. The term "step" includes not only an independent step but also a step that cannot be clearly distinguished from other steps as long as the function of the step is achieved.
[0018] [Photosensitive Resin Composition (Negative Photosensitive Resin Composition)] The photosensitive resin composition of this embodiment (hereinafter also simply referred to as "photosensitive resin composition") contains (A) a polyimide, (B) a solvent, and (C) a photopolymerization initiator. If desired, the photosensitive resin composition may further contain at least one component selected from the group consisting of (D) a radically polymerizable compound, (E) a silane coupling agent, (F) an organotitanium compound, (G) a thermal crosslinking agent, (H) a rust inhibitor, (I) a thermal polymerization initiator, and (J) a plasticizer, in addition to the above components. If desired, the photosensitive resin composition may further contain components (other components) other than the above components (A) to (J). Each of these components (A) to (J) and other components may be used alone, or two or more may be used.
[0019] The photosensitive resin composition is a negative photosensitive resin composition containing: (A) a polyimide; (B) a solvent; and (C) a photopolymerization initiator. In the photosensitive resin composition, the polyimide (A) is represented by the following general formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group.}, and (A) polyimide does not have a polymerizable functional group in its side chain, and (A) polyimide has a weight average molecular weight (Mw) of the polyimide and a polymerizable functional group represented by the following formula (b): R(F Cont. ) = (Mw f +1) / (Mw x +Mw Y -36)...(b) (In the formula, Mw f is the total mass of fluorine atoms that may be contained in (A) polyimide, Mw X is the molecular weight of the tetracarboxylic dianhydride constituting the polyimide (A), Mw Y is the molecular weight of the diamine constituting the polyimide (A).) The product of R calculated by (Mw × R(F Cont. )} satisfies the following formula (a): 300≦Mw×R≦948 (a).
[0020] The prior art has room for improvement as follows. For example, in Patent Document 1, when the photosensitive resin composition is cured, ring closure of the polyimide precursor (the polyimide precursor described in Patent Document 1) may affect film shrinkage, making it difficult to obtain a highly flat rewiring layer. Furthermore, in Patent Document 2, the interaction between the polymer and the copper interface may be inhibited due to the influence of the polyfunctional (meth)acrylate (the polyfunctional (meth)acrylate described in Patent Document 2), which may lead to a decrease in adhesion to copper. Furthermore, in Patent Document 3, the condensation between polyfunctional (meth)acrylates may be inhibited due to the influence of the heterocyclic compound having a reactive group (the heterocyclic compound described in Patent Document 3), which may result in a decrease in oxygen permeability.
[0021] In recent years, the diversification of package mounting technologies has led to a greater variety of support types and multilayered rewiring layers, resulting in a demand for highly planarized insulating materials (e.g., insulating layers obtained using photosensitive resin compositions) used to form wiring. To planarize photosensitive resin compositions, polyfunctional (meth)acrylates and soluble polyimides are used, among others. The former may inhibit the interaction between the polymer and copper, while the latter may reduce solubility in solvents. For these reasons, the use of fluorine atoms, which have good solubility in solvents, is considered for planarizing photosensitive resin compositions. However, photosensitive resin compositions prepared using polymers containing fluorine atoms may result in a reduced film density. In this case, the resulting film is likely to have high oxygen permeability and water vapor permeability, raising concerns about short circuits during reliability testing.
[0022] On the other hand, according to this embodiment, it is possible to realize a prebaked film having excellent flatness, and also to realize a cured film (cured relief pattern) that satisfies the following: the ability to suppress a change in film thickness before and after curing, excellent adhesion to metal wiring, and low oxygen permeability. Furthermore, according to a preferred aspect of this embodiment, it is possible to provide a photosensitive resin composition that can realize a cured film having excellent resistance (chemical resistance) to chemicals used in the process of producing metal wiring, and further it is possible to provide a photosensitive resin composition that can realize a cured film having excellent resolution.
[0023] <<(A) Polyimide>> The photosensitive resin composition contains, as the (A) polyimide, a polyimide represented by the following formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group having 6 to 40 carbon atoms.} This makes it easier to achieve the effects of this embodiment. In addition, in the formula, the tetravalent group and the divalent group may each be an organic group. The "organic group" referred to here means a group containing carbon.
[0024] Polyimide (A) is synthesized from a tetracarboxylic dianhydride and a diamine, and therefore, X in formula (1) represents a structure derived from the tetracarboxylic dianhydride, and Y represents a structure derived from the diamine. From the viewpoint of chemical resistance, it is preferable that X and Y each do not contain an ester structure in the main chain skeleton.
[0025] (A) The weight average molecular weight (Mw) of the polyimide and the following formula (b): R(F Cont. ) = (Mw f +1) / (Mw x +Mw Y -36) ... (b) and the product of R calculated by {Mw × R(F Cont. )} satisfies the following formula (a): 300≦Mw×R≦948 (a).
[0026] The weight average molecular weight (Mw) of the polyimide (A) is measured based on the method described in the Examples. f is the total mass of fluorine atoms that may be contained in the polyimide (A), particularly the total mass of fluorine atoms that may be contained in the tetracarboxylic dianhydride and diamine that constitute the polyimide (A), and Mw x is the molecular weight of the tetracarboxylic dianhydride constituting the polyimide (A), and Mw Y is the molecular weight of the diamine constituting the polyimide (A). The mass of the fluorine atom is "19".
[0027] Generally, polyimides have a rigid planar structure as a resin structure, and therefore form an ordered structure when thermal energy is applied, such as by heating. This tends to result in high thermomechanical properties. On the other hand, the rigid planar structure may reduce solubility in solvents, which may lead to poor moldability. In this regard, the introduction of fluorine atoms into the polyimide skeleton, particularly into the skeleton corresponding to the tetracarboxylic dianhydride and / or diamine, tends to improve solubility in solvents. On the other hand, the bulkiness of the fluorine atoms tends to reduce resin density, resulting in a decrease in barrier properties against gases (oxygen and / or water vapor, etc.). Therefore, when used to protect conductors such as copper and aluminum, or as an interlayer insulating film, corrosion may occur due to high oxygen permeability and / or water vapor permeability. Therefore, when introducing fluorine atoms into (A) polyimide, the amount of fluorine atoms introduced must be considered, and methods for controlling the fluorine atoms in the resin and introducing them into the resin may also need to be devised. For example, in order to maintain solubility in a solvent, it becomes necessary to consider the molecular weight of the resin depending on the amount of fluorine atoms introduced, and ultimately to strike a balance between the amount of fluorine atoms introduced and the molecular weight of the resin.
[0028] The flatness of the prebaked film of the photosensitive resin composition tends to be advantageous when the weight-average molecular weight (Mw) of the (A) polyimide is small and when the amount of fluorine atoms incorporated is large. On the other hand, the oxygen permeability of the cured film tends to be advantageous when the amount of fluorine atoms incorporated is small, and the thermomechanical properties, and therefore the adhesion to metal wiring, tend to be advantageous when the weight-average molecular weight (Mw) of the (A) polyimide is large.
[0029] Therefore, from the viewpoint of realizing a pre-baked film having excellent flatness, and from the viewpoint of realizing a cured film (cured relief pattern) that satisfies the requirements of being able to suppress a change in film thickness before and after curing, having excellent adhesion to metal wiring, and being able to achieve low oxygen permeability, it is meaningful to pay attention to the balance between the amount of fluorine atoms introduced and the molecular weight of the resin, and this significance is expressed as the product (Mw×R).
[0030] By controlling the product (Mw × R) within a predetermined numerical range, for example, it is possible to achieve both solubility in solvents and oxygen permeability. Furthermore, by controlling the product (Mw × R) within a predetermined numerical range, for example, the mechanical properties of the cured film become good, and therefore copper adhesion is also excellent. The product (Mw × R) is 300 or more and 948 or less, and from the viewpoint of oxygen permeability, it is preferably 300 or more and 900 or less, more preferably 300 or more and 800 or less, and even more preferably 400 or more and 700 or less. If the product (Mw × R) is less than 300, it is disadvantageous from the viewpoint of adhesion to metal wiring, and if it exceeds 948, it is disadvantageous from the viewpoint of flatness of the prebaked film and / or low oxygen permeability. In relation to the product (Mw × R), the lower limit of "300" has technical significance for achieving the effects of the present invention, particularly for satisfying the thermomechanical properties required to ensure the reliability of a semiconductor package device, and the upper limit of "948" has technical significance for ensuring the storage stability of the liquid photosensitive resin composition and the reliability of a semiconductor package device.
[0031] Here, in this embodiment, R(F Cont. ) (Mw f +1) and (Mw x +Mw Y -36) and the ratio of R (F Cont. ) means, for example, that the proportion of raw materials containing fluorine atoms is high, and R(F Cont. A small Mw ) means, for example, that the proportion of raw materials containing fluorine atoms is small. Raw materials containing fluorine atoms may not be used. When the total mass of fluorine atoms in the polyimide is below the detection limit, Mw f may be treated as 0. f When is 0, "Mw f "Mw +1" is the minimum, i.e., it is treated as "1". x +Mw Y Regarding "Mw -36", x +Mw Y The "36" subtracted from "R(F)" corresponds to the component (2 mol of water molecules) that is not included in the repeating unit of tetracarboxylic dianhydride and diamine. Cont.) is also understood to relate to the total mass of fluorine atoms per repeat unit.
[0032] (A) Weight average molecular weight (Mw) of polyimide, Mw f , Mw x , and Mw Y can be controlled by appropriately selecting the types of raw materials constituting the (A) polyimide, specifically, the tetracarboxylic dianhydride and the diamine, and by appropriately changing the ratio thereof.
[0033] In the above formula (1), X is represented by the following formulas (2) to (9): Examples of the structure include at least one selected from the group consisting of:
[0034] From the viewpoint of suitably suppressing the oxygen permeability of the cured film, X preferably has a structure represented by at least one selected from the group consisting of formulas (2) to (8), and from the viewpoint of the chemical resistance of the cured film, X more preferably has a structure represented by at least one selected from the group consisting of formulas (2), (3), (5), (7), and (8), and further preferably has a structure represented by at least one selected from the group consisting of formulas (2) and (3), and at least one selected from (7) and (8). Furthermore, X may have a structure represented by formula (9) from the viewpoint of ensuring the total mass of fluorine atoms contained in the (A) polyimide.
[0035] In the above formula (1), Y is represented by the following formulas (10) to (19): Examples of the structure include at least one selected from the group consisting of:
[0036] From the viewpoint of suitably suppressing the oxygen permeability of the cured film, Y preferably has a structure represented by at least one selected from the group consisting of formulas (10) to (16) and (19). From the viewpoint of chemical resistance, Y more preferably has a structure represented by at least one selected from the group consisting of formulas (10), (12), (13), and (19), thereby suppressing shrinkage of the cured film. It is even more preferable for Y to have a structure represented by formulas (12), (13), or (19), and particularly preferable for Y to have a structure represented by formulas (12) or (13). From the viewpoint of ensuring the total mass of fluorine atoms contained in the polyimide (A), Y may have a structure represented by formula (17) and / or formula (18). Furthermore, since the polyimide (A) does not have a side chain polymerizable group, the photosensitive resin composition of this embodiment has excellent copper adhesion.
[0037] The molecular weight distribution (Mw / Mn) of the polyimide (A) is preferably 1.0 or more and 1.8 or less. From the viewpoint of production efficiency of the molecular weight distribution, the lower limit is more preferably 1.15 or more, and even more preferably 1.25 or more. From the viewpoint of resolution, the upper limit is more preferably 1.7 or less, and even more preferably 1.6 or less.
[0038] The weight average molecular weight (Mw) of the (A) polyimide is preferably 8,000 or more and 23,000 or less from the viewpoint of the mechanical properties of the cured film and the flatness of the spin-coated film (coating film). From the viewpoint of the mechanical properties of the cured film, the lower limit is preferably 8,000 or more, more preferably 10,000 or more, even more preferably 12,000 or more, and particularly preferably 18,000 or more. From the viewpoint of the solubility in (B) solvents and the flatness of the spin-coated film (coating film), the weight average molecular weight (Mw) is preferably 23,000 or less, more preferably 20,000 or less, and even more preferably 16,000 or less.
[0039] From the viewpoints of mechanical properties, chemical resistance, and resolution, the (A) polyimide preferably has a polymerizable functional group (terminal functional group) at its terminal, preferably at the terminal of its main chain.
[0040] <<Method for Producing Polyimide>> (A) An example of a method for producing a polyimide includes the steps of: reacting a tetracarboxylic dianhydride with a diamine to obtain a polyamic acid; and performing dehydration ring closure of the polyamic acid by heating and / or chemical imidization using a catalyst to obtain a polyimide. The production method may optionally include the step of introducing a desired functional group (e.g., a polymerizable functional group) into a terminal of the polyimide, preferably into a main chain terminal.
[0041] When polyamic acid is subjected to dehydration ring closure by heating, the heating temperature is preferably 150° C. or higher, more preferably 160° C. or higher, from the viewpoint of favorably proceeding the ring closure reaction, and is preferably 200° C. or lower, more preferably 180° C., from the viewpoint of suppressing side reactions at high temperatures.
[0042] When polyamic acid is subjected to dehydration ring closure using a catalyst, examples of the catalyst include base catalysts, and specific examples include acetic anhydride-pyridine and acetic anhydride-triethylamine.
[0043] Examples of tetracarboxylic dianhydrides include pyromellitic anhydride (PMDA), 4,4'-oxydiphthalic anhydride (ODPA), 3,4'-oxydiphthalic anhydride, 4,4'-biphenyl dianhydride (BPDA), 3,4'-biphenyl dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5'',6,6' 1,2,3,4-cyclobutanetetracarboxylic acid anhydride (CBDA), 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), and the like.
[0044] Examples of diamines include 4,4'-diaminodiphenyl ether (DADPE), 3,4'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPEQ), 2-phenoxybenzene-1,4-diamine, 9,9-bis(4-aminophenyl)fluorene (BAFL), 6-(4-aminophenoxy)biphenyl-3-amine (PDPE), ), 3,3'-diphenyl-4,4'-bis(4-aminophenoxy)biphenyl (APBP-DP), 2,2-bis[3-phenyl-4-(4-aminophenoxy)phenyl]propane (DAOPPA), 2,2'-dimethylbenzidine (m-TB), 2,2'-bis(trifluoromethyl)benzidine (TFMB), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP).
[0045] <Method for producing polyimide having polymerizable functional groups at the main chain terminals> A polyimide having polymerizable functional groups at its terminals can be obtained by reacting the polyimide obtained by the above method with a compound having a polymerizable functional group at its terminal. The terminal structure of the polyimide before the introduction of the polymerizable functional group may be a carboxyl group or an acid anhydride group derived from a tetracarboxylic dianhydride, or may be an amino group derived from a diamine.
[0046] The compound having a polymerizable functional group at its terminal is preferably at least one selected from the group consisting of an isocyanate-based compound, a chloride-based compound, and an alcohol-based compound, all of which have the polymerizable functional group. Examples of the polymerizable functional group include a (meth)acryloyl group.
[0047] Examples of compounds having a polymerizable functional group at their terminals include isocyanate compounds such as 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate; chloride compounds such as acryloyl chloride and methacryloyl chloride; and alcohol compounds such as 2-hydroxyethyl methacrylate (2-hydroxyethyl methacrylate: HEMA), 2-hydroxyethyl acrylate, 4-hydroxyethyl methacrylate, and 4-hydroxyethyl acrylate.
[0048] The isocyanate-based compound reacts with the amino group of the dehydrated, ring-closed polyimide to form a urea bond. The chloride-based compound reacts with the amino group of the dehydrated, ring-closed polyimide to form an amide bond. The alcohol-based compound reacts with the carboxyl group or acid anhydride group of the dehydrated, ring-closed polyimide to form an ester bond. The isocyanate-based compound, chloride-based compound, and / or alcohol-based compound may react with the terminal, preferably the main chain terminal, of the dehydrated, ring-closed polyimide.
[0049] Examples of methods for reacting an isocyanate compound with the amino groups of a dehydrated, ring-closed polyimide include mixing the two and stirring them at room temperature. Examples of methods for reacting a chloride compound with the amino groups of a dehydrated, ring-closed polyimide include ice-cooling a solution of the dehydrated, ring-closed polyimide and adding the chloride compound dropwise. Examples of methods for reacting an alcohol compound with the carboxyl groups or acid anhydride groups of a dehydrated, ring-closed polyimide include using a condensing agent such as N,N'-dicyclohexylcarbodiimide (DCC) or an esterification catalyst such as p-toluenesulfonic acid.
[0050] By these reactions, the polar terminal groups of the polymer are substituted with polymerizable functional groups, which makes it easier to reduce the interaction caused by the polar functional groups, and in this case, the flatness of the prebaked film tends to improve. Examples of the polymerizable functional group (terminal functional group) include those represented by the following formula: {wherein * represents a bonding site with an end of the polyimide (A).} From the viewpoints of resolution and suppression of cure shrinkage, it is preferable that the polymer has a radical polymerizable functional group at the end of its main chain.
[0051] (A) In the production of polyimide, a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is preferably one that can uniformly dissolve or suspend the tetracarboxylic dianhydride, diamine, and optional components (e.g., a compound having a polymerizable functional group at its terminal). Examples of reaction solvents include γ-butyrolactone (GBL), dimethyl sulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0052] The polyimide (A) may be purified by a known method such as that described in JP 2012-194520 A. Examples of the purification method include a method in which the polyimide (A) solution is dropped into water to cause reprecipitation, thereby removing unreacted substances, a method in which a condensing agent insoluble in the reaction solvent is removed by filtration, and a method in which the catalyst is removed using an ion exchange resin. After performing these purification methods, the polyimide (A) may be dried by a known method, and in this case, may be isolated in a powder state.
[0053] The (A) polyimide may be contained in the photosensitive resin composition in an amount of, for example, 35% by mass, preferably 20 to 70% by mass, more preferably 25 to 65% by mass, and, based on the solid content of the photosensitive resin composition, in an amount of, for example, 50% by mass or more, preferably 55 to 90% by mass, more preferably 60 to 80% by mass.
[0054] (B) Solvent The (B) solvent can dissolve or suspend the (A) polyimide and the (C) photopolymerization initiator. Examples of the (B) solvent include γ-butyrolactone (GBL), dimethyl sulfoxide, tetrahydrofurfuryl alcohol, ethyl acetoacetate, N,N-dimethylacetoacetamide, ε-caprolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0055] The (B) solvent can be appropriately selected depending on the thickness of the coating film of the photosensitive resin composition and the viscosity of the composition. The (B) solvent can be used in an amount of, for example, 30 to 1,000 parts by mass, preferably 140 to 1,000 parts by mass, per 100 parts by mass of the (A) polyimide.
[0056] The higher the solubility of the (A) polyimide in the (B) solvent, the more the flatness of the prebaked film tends to improve. On the other hand, the higher the solubility of the (A) polyimide, the more likely the solvent is to remain in the prebaked film, and the greater the shrinkage of the cured film tends to be. When an alcohol having no olefinic double bond is contained, the proportion of the alcohol having no olefinic double bond in the total solvent is preferably 5 to 50 mass%. From the viewpoint of the storage stability of the photosensitive resin composition, this proportion is more preferably 10 mass% or more. Furthermore, from the viewpoint of the solubility of the (A) polyimide, it is more preferably 30 mass% or less.
[0057] (C) Photopolymerization Initiator The (C) photopolymerization initiator is a compound capable of initiating polymerization by actinic rays, preferably a compound capable of generating radicals by actinic rays and polymerizing an ethylenically unsaturated group-containing compound, etc. Examples of initiators that generate radicals by actinic rays include benzophenone, N-alkylaminoacetophenone, oxime ester, acridine, and phosphine oxide, as well as compounds containing a structure such as lophine. Examples of the above include aromatic ketones such as benzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N,N',N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, acrylated benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide; benzoin ether compounds such as benzoin methyl ether, benzoin ethyl ether, and benzoin phenyl ether; benzoin compounds such as benzoin, methylbenzoin, and ethylbenzoin;1,2-Octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime) (manufactured by BASF Japan Ltd., Irgacure Oxe02), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(o-benzoyloxime) (manufactured by Changzhou Powerful Electronic New Materials Co., Ltd., PBG305), 1-(6-O-methylbenzoyl-9-ethylcarbazol-3-yl)-(3-cyclopentylacetone)-1-oxime acetate (manufactured by Changzhou Powerful Electronic New Materials Co., Ltd., TR-PBG-304), trade name: TR-PBG-3057 (manufactured by Changzhou Powerful Electronic New Materials Co., Ltd.), 1,2-propanedione, 3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-, 2-(o-acetyloxime) (Nikko Chemtech Examples of suitable oxime ester compounds include NCI-831 (trade name, manufactured by ADEKA Corporation, product name: TR-PBG-326), NCI-831 (trade name, manufactured by ADEKA Corporation), etc.; benzyl derivatives such as benzyl dimethyl ketal; acridine derivatives such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; N-phenylglycine derivatives such as N-phenylglycine; coumarin compounds; oxazole compounds; phosphine oxide compounds such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and lophine compounds such as 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole;
[0058] Among the (C) photopolymerization initiators, from the viewpoint of resolution, an oxime ester compound is preferred, and an oxime ester having a diphenyl sulfide structure represented by the following general formula (28) or a carbazole structure represented by the following general formula (29) is more preferred. From the viewpoint of surface curability, the photosensitive resin composition of the present embodiment further preferably contains an oxime ester having a carbazole structure. {In the formula, R 1 represents a hydrocarbon group having 1 to 10 carbon atoms, and * represents a bond to another structure.
[0059] The proportion of the photopolymerization initiator (C) is preferably 1 part by mass or more and 30 parts by mass or less relative to 100 parts by mass of the polyimide (A). From the viewpoint of photocurability, the proportion is more preferably 2 parts by mass or more. Furthermore, from the viewpoint of good curability, including the bottom of the relief pattern, the proportion is more preferably 20 parts by mass or less.
[0060] (D) Radically Polymerizable Compound From the viewpoint of improving the resolution of the cured relief pattern and suppressing film shrinkage during heating, the photosensitive resin composition may optionally contain a radically polymerizable compound.
[0061] The radical polymerizable compound is preferably a (meth)acrylate compound that undergoes a suitable radical polymerization reaction in the presence of a (C) photopolymerization initiator. The radical polymerizable compound more preferably contains a (D1) monofunctional monomer containing one polymerizable functional group in the molecule and a (D2) polyfunctional monomer containing two or more polymerizable functional groups in the molecule. The polymerizable functional group is preferably a (meth)acryloyl group.
[0062] Examples of the monofunctional monomer (D1) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexyl (meth)acrylate, butoxydiethylene glycol methacrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, m-phenoxybenzyl acrylate, o-phenylphenoxyethyl acrylate, 4-methacryloyloxybenzophenone, EO-modified para-cumylphenol acrylate, nonylphenoxyethyl acrylate, 6-acrylamidohexanoic acid, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate (for example, product name "AM-90G", manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0063] Examples of the polyfunctional monomer (D2) include di(meth)acrylates of ethylene glycol or polyethylene glycol, such as diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, di(meth)acrylates of propylene glycol or polypropylene glycol, di(meth)acrylates or tri(meth)acrylates of glycerol, cyclohexane di(meth)acrylate, di(meth)acrylates of 1,4-butanediol, di(meth)acrylates of 1,6-hexanediol, di(meth)acrylates of neopentyl glycol, di(meth)acrylates of bisphenol A, (meth)acrylamide, derivatives thereof, trimethylolpropane tri(meth)acrylate, di(meth)acrylates or tri(meth)acrylates of glycerol, Examples of the urethane acrylate include tri(meth)acrylate, pentaerythritol di(meth)acrylate, tri(meth)acrylate, or tetra(meth)acrylate, ethylene oxide or propylene oxide adducts of these compounds, urethane acrylates such as EBECRYL230 (product name, manufactured by Daicel-Allnex Corporation), EBECRYL8402 (product name, manufactured by Daicel-Allnex Corporation), EBECRYL8465 (product name, manufactured by Daicel-Allnex Corporation), EBECRYL8667 (product name, manufactured by Daicel-Allnex Corporation), EBECRYL4740 (product name, manufactured by Daicel-Allnex Corporation), and KRM9276 (product name, manufactured by Daicel-Allnex Corporation), and compounds such as tris-(2-hydroxyethyl)isocyanurate acrylate.
[0064] Among the radical polymerizable compounds, from the viewpoint of suppressing film shrinkage, it is preferable to contain a polyfunctional monomer (D2), and in particular, it is more preferable to contain a compound having three or more polymerizable functional groups in the molecule. The mass ratio (D1 / D2) of the monofunctional monomer (D1) to the polyfunctional monomer (D2) is preferably more than 0.01 and less than 0.5. From the viewpoint of the flatness of the prebaked film, the mass ratio is preferably more than 0.02, and from the viewpoint of the flatness of the cured film, it is preferably less than 0.5. From the same viewpoint, the mass ratio is more preferably 0.05 or more and 0.45 or less, and even more preferably 0.1 or more and 0.4 or less.
[0065] The proportion of the radical polymerizable compound in the photosensitive resin composition is preferably 0.5 parts by mass to 100 parts by mass relative to 100 parts by mass of the (A) polyimide. From the viewpoint of photocurability, the lower limit is more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and particularly preferably 20 parts by mass. From the viewpoint of good curability, including copper adhesion and the bottom of the pattern, the upper limit is more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less.
[0066] (E) Silane Coupling Agent The photosensitive resin composition may optionally contain a silane coupling agent to improve the adhesion of the cured relief pattern to the substrate.
[0067] Examples of silane coupling agents include 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name KBM803, manufactured by Chisso Corporation: trade name Sila-Ace S810), 3-mercaptopropyltriethoxysilane (manufactured by Azmax Corporation: trade name SIM6475.0), 3-mercaptopropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name LS1375, manufactured by Azmax Corporation: trade name SIM6474.0), mercaptomethyltrimethoxysilane (manufactured by Azmax Corporation: trade name SIM6473.5C), and mercaptomethylmethyldimethoxysilane (manufactured by Azmax Corporation: trade name SIM6473.0), 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldiethoxypropoxysilane, 3-mercaptopropylethoxydipropoxysilane, 3-mercaptopropyldimethoxypropoxysilane, 3-mercaptopropylmethoxydipropoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyldiethoxy mercaptoethyltripropoxysilane, 2-mercaptoethylethoxydimethoxysilane, 2-mercaptoethyltrippropoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethylethoxydipropoxysilane, 2-mercaptoethyldimethoxypropoxysilane, 2-mercaptoethylmethoxydipropoxysilane, 4-mercaptobutyltrimethoxysilane, 4-mercaptobutyltriethoxysilane, 4-mercaptobutyltrippropoxysilane, and the like.
[0068] Examples of the silane coupling agent include N-(3-triethoxysilylpropyl)urea (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name LS3610, manufactured by Azmax Corporation: trade name SIU9055.0), N-(3-trimethoxysilylpropyl)urea (manufactured by Azmax Corporation: trade name SIU9058.0), N-(3-diethoxymethoxysilylpropyl)urea, N-(3-ethoxydimethoxysilylpropyl)urea, N-(3-tripropoxysilylpropyl)urea, N-(3-diethoxypropoxysilylpropyl)urea, N-(3-ethoxydipropoxysilylpropyl)urea, N-(3-dimethoxypropoxysilylpropyl)urea, N-(3-methoxydipropoxysilylpropyl)urea, N-(3-trimethoxysilylethyl)urea, and N-(3-ethoxydimethoxysilylethyl)urea. N-(3-tripropoxysilylethyl)urea, N-(3-tripropoxysilylethyl)urea, N-(3-ethoxydipropoxysilylethyl)urea, N-(3-dimethoxypropoxysilylethyl)urea, N-(3-methoxydipropoxysilylethyl)urea, N-(3-trimethoxysilylbutyl)urea, N-(3-triethoxysilylbutyl)urea, N-(3-tripropoxysilylbutyl)urea, 3-(m-aminophenoxy)propyltrimethoxysilane (trade name, manufactured by Azmax Corporation), Other examples include aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0598.0), m-aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.0), p-aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.1), and aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.2).
[0069] Examples of silane coupling agents include 2-(trimethoxysilylethyl)pyridine (manufactured by Azmax Corporation: trade name SIT8396.0), 2-(triethoxysilylethyl)pyridine, 2-(dimethoxysilylmethylethyl)pyridine, 2-(diethoxysilylmethylethyl)pyridine, (3-triethoxysilylpropyl)-t-butylcarbamate, (3-glycidoxypropyl)triethoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-t-butoxysilane, tetrakis(methacryloylsilane), ... bis(triethoxysilane), tetrakis(methoxy-n-propoxysilane), tetrakis(ethoxyethoxysilane), tetrakis(methoxyethoxyethoxysilane), bis(trimethoxysilyl)ethane, bis(trimethoxysilyl)hexane, bis(triethoxysilyl)methane, bis(triethoxysilyl)ethane, bis(triethoxysilyl)ethylene, bis(triethoxysilyl)octane, bis(triethoxysilyl)octadiene, bis[3-(triethoxysilyl)propyl]disulfide, bis[ 3-(triethoxysilyl)propyl]tetrasulfide, di-t-butoxydiacetoxysilane, di-i-butoxyaluminoxytriethoxysilane, phenyl silanetriol, methyl phenyl silanediol, ethyl phenyl silanediol, n-propyl phenyl silanediol, isopropyl phenyl silanediol, n-butyldiphenyl silanediol, isobutylphenyl silanediol, tert-butylphenyl silanediol, diphenyl silanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, ethyl methyl phenyl silanol, n-propyl methyl phenyl silanol, isopropyl methyl phenyl silanol, n-butylmethyl phenyl silanol, isobutylmethyl phenyl silanol, tert-butylmethyl phenyl silanol, ethyl n-propyl phenyl silanol, ethyl isopropyl phenyl silanol, n-butylethyl phenyl silanol, isobutylethyl phenyl silanol, tert-butylethyl phenyl silanol,Other examples include methyldiphenylsilanol, ethyldiphenylsilanol, n-propyldiphenylsilanol, isopropyldiphenylsilanol, n-butyldiphenylsilanol, isobutyldiphenylsilanol, tert-butyldiphenylsilanol, and triphenylsilanol.
[0070] Among silane coupling agents, from the viewpoint of adhesion to a substrate and storage stability, a silane coupling agent represented by the following general formula (30): {In the formula, R 10 is at least one selected from the group consisting of substituents containing an epoxy group, a phenylamino group, a ureido group, an isocyanate group, and an isocyanuric group, and R 11 is an alkyl group having 1 to 4 carbon atoms, and R 12 is a hydroxyl group or an alkyl group having 1 to 4 carbon atoms, a is an integer of 1 to 3, and i is an integer of 1 to 6.
[0071] In formula (30), from the viewpoint of adhesion to the metal redistribution layer, a is preferably 2 or 3, and more preferably 3. From the viewpoint of adhesion to the metal redistribution layer, i is preferably 1 or more and 4 or less, and from the viewpoint of resolution, it may be 2 or more and 5 or less.
[0072] R 10 Among the above, from the viewpoints of resolution and adhesion of the metal redistribution layer, R is preferably at least one selected from the group consisting of a substituent containing a phenylamino group and a substituent containing a ureido group, and a substituent containing a phenylamino group is more preferred. 11 , and R 12 Examples of the alkyl groups having 1 to 4 carbon atoms mentioned above are each independently a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, and a t-butyl group.
[0073] Examples of silane coupling agents containing an epoxy group include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0074] Examples of silane coupling agents containing a phenylamino group include N-phenyl-3-aminopropyltrimethoxysilane. Examples of silane coupling agents containing a ureido group include 3-ureidopropyltrialkoxysilane. Examples of silane coupling agents containing an isocyanate group include 3-isocyanatepropyltriethoxysilane.
[0075] The proportion of the silane coupling agent in the photosensitive resin composition may be 0.2 to 10 parts by mass relative to 100 parts by mass of the polyimide (A), and from the viewpoint of copper adhesion, it is preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more. From the viewpoint of suppressing the generation of foreign matter due to precipitation, it is preferably 8 parts by mass or less, and more preferably 6 parts by mass or less.
[0076] (F) Organotitanium Compound In order to improve the chemical resistance of the cured film, the photosensitive resin composition may optionally contain an organotitanium compound.
[0077] Usable organic titanium compounds include those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of organic titanium compounds are shown below in I) to VII): I) Titanium chelate compounds: Specific examples include titanium(IV) oxide acetylacetonate, titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), titanium diisopropoxide bis(acetylacetonate), etc.
[0078] II) Tetraalkoxytitanium compounds: for example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], etc.
[0079] III) Titanocene compounds: for example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like.
[0080] IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc.
[0081] V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, etc.
[0082] VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate.
[0083] VII) Titanate coupling agents: for example, isopropyl tridodecylbenzenesulfonyl titanate.
[0084] Among them, from the viewpoint of better chemical resistance, it is preferable that the organic titanium compound is at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η 5 At least one compound selected from the group consisting of titanium(IV) oxide acetylacetonate, titanium(IV) oxide acetylacetonate, titanium(IV) difluoro-3-(1H-pyrrol-1-yl)phenyl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and titanium(IV) oxide acetylacetonate is preferred.
[0085] When the negative photosensitive resin composition contains an organotitanium compound, the content thereof may be 0.05 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the polyimide (A), preferably 0.5 parts by mass or more from the viewpoint of the heat resistance and chemical resistance of the cured film, and preferably 2 parts by mass or less from the viewpoint of the storage stability of the photosensitive resin composition.
[0086] (G) Thermal Crosslinking Agent From the viewpoint of the flatness of the prebaked film and the chemical resistance of the cured film, the photosensitive resin composition may optionally contain a thermal crosslinking agent.
[0087] The thermal crosslinking agent is a compound that undergoes an addition reaction or a condensation polymerization reaction by heat. These reactions occur between the combination of (A) polyimide and the thermal crosslinking agent, between the thermal crosslinking agents themselves, and between the thermal crosslinking agent and other components described below, and the reaction temperature is preferably 150°C or higher.
[0088] Examples of the thermal crosslinking agent include an alkoxymethyl compound, an epoxy compound, an oxetane compound, a bismaleimide compound, an allyl compound, and a blocked isocyanate compound. From the viewpoint of suppressing film shrinkage, the thermal crosslinking agent preferably contains a nitrogen atom.
[0089] Examples of alkoxymethyl compounds include the following compounds: Examples include:
[0090] Examples of epoxy compounds include 4-hydroxybutyl acrylate glycidyl ether, epoxy compounds containing a bisphenol A group, and hydrogenated bisphenol A diglycidyl ether (for example, Epolight 4000 manufactured by Kyoeisha Chemical Co., Ltd.).
[0091] Examples of thermal crosslinkers also include epoxy resins. Examples of epoxy resins include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, bisphenol S type epoxy resin, hydrogenated bisphenol A type epoxy resin, bisphenol M type epoxy resin (4,4'-(1,3-phenylenediisopridiene)bisphenol type epoxy resin), bisphenol P type epoxy resin (4,4'-(1,4-phenylenediisopridiene)bisphenol type epoxy resin), bisphenol Z type epoxy resin (4,4'-cyclohexidiene bisphenol type epoxy resin), and tetramethyl bisphenol F type epoxy resin; novolac type epoxy resins such as phenol novolac type epoxy resin, brominated phenol novolac type epoxy resin, cresol novolac type epoxy resin, tetraphenol group ethane type novolac type epoxy resin, and novolac type epoxy resin having a condensed ring aromatic hydrocarbon structure; biphenyl type epoxy resin; aralkyl type epoxy resins such as xylylene type epoxy resin and biphenyl aralkyl type epoxy resin; Epoxy resins having a naphthalene skeleton, such as naphthylene ether type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, naphthalene diol type epoxy resins, di- to tetrafunctional epoxy type naphthalene resins, binaphthyl type epoxy resins, and naphthalene aralkyl type epoxy resins; anthracene type epoxy resins; phenoxy type epoxy resins; dicyclopentadiene type epoxy resins; norbornene type epoxy resins; adamantane type epoxy resins; fluorene type epoxy resins, phosphorus-containing epoxy resins, alicyclic epoxy resins, aliphatic linear epoxy resins, bisphenol A novolac type epoxy resins, bixylenol type epoxy resins, trihydroxyphenylmethane type epoxy resins, stilbene type epoxy resins, tetraphenylolethane type epoxy resins, and heterocyclic epoxy resins such as triglycidyl isocyanurate; Glycidylamines such as N,N,N',N'-tetraglycidylmetaxylenediamine, N,N,N',N'-tetraglycidylbisaminomethylcyclohexane, and N,N-diglycidylaniline;Examples of the copolymer include a copolymer of glycidyl (meth)acrylate and a compound having an ethylenically unsaturated double bond; an epoxy resin having a butadiene structure; a diglycidyl ether of a bisphenol; a diglycidyl ether of a naphthalenediol; and a glycidyl ether of a phenol.
[0092] Examples of epoxy compounds or epoxy resins include glycidyl ethers such as n-butyl glycidyl ether, 2-ethoxyhexyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, glycerol polyglycidyl ether, sorbitol polyglycidyl ether, and glycidyl ether of bisphenol A (or F); and glycidyl esters such as adipic acid diglycidyl ester and o-phthalic acid diglycidyl ester. esters, 3,4-epoxycyclohexylmethyl (3,4-epoxycyclohexane) carboxylate, 3,4-epoxy-6-methylcyclohexylmethyl (3,4-epoxy-6-methylcyclohexane) carboxylate, bis(3,4-epoxy-6-methylcyclohexylmethyl) adipate, dicyclopentanediene oxide, bis(2,3-epoxycyclopentyl) ether, and alicyclic epoxy resins such as Celloxide 2021P, Celloxide 2081, Celloxide 2083, Celloxide 2085, Celloxide 8000, and Epolead GT401 manufactured by Daicel Corporation; Aliphatic polyglycidyl ethers such as 2,2'-(((((1-(4-(2-(4-(oxiran-2-ylmethoxy)phenyl)propan-2-yl)phenyl)ethane-1,1-diyl)bis(4,1-phenylene))bis(oxy))bis(methylene))bis(oxirane)) (for example, Techmore VG3101L manufactured by Printec Co., Ltd.: this product is a trifunctional epoxy resin), Epolite 100MF (manufactured by Kyoeisha Chemical Industry Co., Ltd.), and Epiol TMP (manufactured by NOF Corporation); 1,1,3,3,5,5-hexamethyl-1,5-bis(3-(oxiran-2-ylmethoxy)propyl)trisiloxane (for example, DMS-E09 manufactured by Gelest Co., Ltd.); and the like.
[0093] Examples of the oxetane compound include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, bis[1-ethyl(3-oxetanyl)]methyl ether, 4,4'-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl, 4,4'-bis(3-ethyl-3-oxetanylmethoxy)biphenyl, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, diethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, bis(3-ethyl-3-oxetanylmethyl) 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, OXT121 (manufactured by Toagosei Co., Ltd., trade name), and OXT221 (manufactured by Toagosei Co., Ltd., trade name).
[0094] Examples of bismaleimide compounds include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,3-phenylenebis(maleimide), N,N'-1,4-phenylenebis(maleimide), 3-methyl-N,N'-1,4-phenylenebis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane.
[0095] Examples of the allyl compound include allyl alcohol, allyl anisole, allyl benzoate, allyl cinnamate, N-allyloxyphthalimide, allylphenol, allylphenylsulfone, allyl urea, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl maleate, diallyl isocyanurate, triallylamine, triallyl isocyanurate, triallyl cyanurate, triallylamine, triallyl 1,3,5-benzenetricarboxylate, triallyl trimellitate, triallyl phosphate, triallyl phosphite, and triallyl citrate.
[0096] Examples of the blocked isocyanate compound include hexamethylene diisocyanate-based blocked isocyanates (e.g., Duranate SBN-70D, SBB-70P, SBF-70E, TPA-B80E, 17B-60P, MF-B60B, E402-B80B, MF-K60B, and WM44-L70G manufactured by Asahi Kasei Corporation, Takenate B-882N manufactured by Mitsui Chemicals, Inc., and 7960, 7961, 7982, 7991, and 7992 manufactured by Baxenden, etc.), and tolylene diisocyanate-based blocked isocyanates (e.g., Takenate B-830 manufactured by Mitsui Chemicals, Inc., etc.). , 4,4'-diphenylmethane diisocyanate-based blocked isocyanates (e.g., Takenate B-815N manufactured by Mitsui Chemicals, Inc., and Coronate PMD-OA01 and PMD-MA01 manufactured by Daiei Sangyo Co., Ltd.), 1,3-bis(isocyanatomethyl)cyclohexane-based blocked isocyanates (e.g., Takenate B-846N manufactured by Mitsui Chemicals, Inc., and Coronate BI-301, 2507, and 2554 manufactured by Tosoh Corporation), and isophorone diisocyanate-based blocked isocyanates (e.g., 7950, 7951, and 7990 manufactured by Baxenden).
[0097] Among these, a blocked isocyanate compound or a bismaleimide compound is preferred for the thermal crosslinking agent from the viewpoint of storage stability. A thermal crosslinking agent having two or more crosslinkable functional groups in one molecule is preferred from the viewpoint of mechanical properties and chemical resistance.
[0098] The proportion of the thermal crosslinking agent in the photosensitive resin composition is preferably 0.2 to 40 parts by mass relative to 100 parts by mass of the polyimide (A). From the viewpoint of chemical resistance, the proportion is more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more. Furthermore, from the viewpoint of storage stability of the photosensitive resin composition, the proportion is more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less.
[0099] (H) Rust Inhibitor When a photosensitive resin composition is used to form a cured film on a substrate made of copper or a copper alloy, the photosensitive resin composition may optionally contain a rust inhibitor to improve adhesion. Examples of the rust inhibitor include an azole compound and a purine compound.
[0100] Examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, 2-(3,5-di- t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 3-mercapto-1,2,4-triazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, and 1H-tetrazole-5-acetic acid.
[0101] Particularly preferred examples include 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, and 1H-tetrazole-5-acetic acid.
[0102] Examples of purine compounds include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-amino ...1-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 1-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 1-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 1-methyladenine, 1-methyladenine, 1-methyladenine, 1-methyladenine, 1-methyladenine, 1- Examples thereof include adenine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, 8-azahypoxanthine, and derivatives thereof.
[0103] When the photosensitive resin composition contains a rust inhibitor, the proportion thereof is preferably 0.01 to 20 parts by mass relative to 100 parts by mass of the polyimide (A). From the viewpoint of suppressing discoloration of the copper or copper alloy surface when the photosensitive resin composition is formed on copper or a copper alloy, the proportion is more preferably 0.03 to 0.05 parts by mass, and even more preferably 0.05 parts by mass. Furthermore, from the viewpoint of photosensitivity, the proportion is more preferably 10 to 5 parts by mass.
[0104] (I) Thermal Polymerization Initiator The photosensitive resin composition may optionally contain a thermal polymerization initiator from the viewpoint of suppressing film shrinkage. The thermal polymerization initiator is a compound that can initiate polymerization by heat, preferably a compound that generates radicals by heat.
[0105] Examples of the thermal polymerization initiator include: organic peroxides such as dialkyl peroxides, diacyl peroxides, peroxy esters, and peroxy ketals; and azo polymerization initiators such as azonitriles, azo esters, and azoamides. Among these, dialkyl peroxides and diacyl peroxides (e.g., dicumyl peroxide) are preferred from the viewpoint of chemical resistance.
[0106] When the photosensitive resin composition contains a thermal polymerization initiator, the proportion thereof is preferably 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide. From the viewpoint of suppressing film shrinkage, the proportion thereof is more preferably 0.5 parts by mass or more. Furthermore, from the viewpoint of storage stability of the photosensitive resin composition, the proportion thereof is more preferably 5 parts by mass or less.
[0107] (J) Plasticizer The photosensitive resin composition may optionally contain a plasticizer from the viewpoint of improving the flatness of the prebaked film and, in turn, further improving adhesion to copper. The plasticizer is a compound that improves the fluidity of the (A) polyamide-imide precursor resin when a relief pattern formed using the photosensitive resin composition is heated (cured). The inclusion of a plasticizer makes it easier to suppress the amount of change in film thickness during curing.
[0108] Examples of the plasticizer include polycarboxylic acid ester plasticizers, sulfonamide plasticizers, phosphate ester plasticizers, polyester plasticizers, and polyalkylene glycol plasticizers.
[0109] Examples of polycarboxylic acid ester plasticizers include benzoate esters such as methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, pentyl benzoate, heptyl benzoate, normal octyl benzoate, nonyl benzoate, isononyl benzoate, isodecyl benzoate, 2-ethylhexyl benzoate, isodecyl benzoate, butylbenzyl benzoate, cyclopropyl benzoate, cyclobutyl benzoate, cyclopentyl benzoate, cyclohexyl benzoate, cycloheptyl benzoate, allyl benzoate, butylbenzyl benzoate, and phenyl benzoate. phthalates such as dimethyl phthalate, diethyl phthalate, dipropyl phthalate, dibutyl phthalate, dipentyl phthalate, diheptyl phthalate, di-n-octyl phthalate, dinonyl phthalate, diisononyl phthalate, diisodecyl phthalate, bis(2-ethylhexyl) phthalate, diisodecyl phthalate, butyl benzyl phthalate, dicyclopropyl phthalate, dicyclobutyl phthalate, dicyclopentyl phthalate, dicyclohexyl phthalate, dicycloheptyl phthalate, diallyl phthalate, bisbutyl benzyl phthalate, and diphenyl phthalate Trimethyl trimellitate, Triethyl trimellitate, Tripropyl trimellitate, Tributyl trimellitate, Tripentyl trimellitate, Triheptyl trimellitate, Tri-n-octyl trimellitate, Trinonyl trimellitate, Triisononyl trimellitate, Triisodecyl trimellitate, Tris(2-ethylhexyl) trimellitate, Triisodecyl trimellitate, Trisbutylbenzyl trimellitate, Tricyclopropyl trimellitate, Tricyclobutyl trimellitate, Tricyclopentyl trimellitate trimellitic acid esters such as methyl trimellitate, tricyclohexyl trimellitate, tricycloheptyl trimellitate, triallyl trimellitate, trisbutylbenzyl trimellitate, and triphenyl trimellitate; dimethyl adipate, diethyl adipate, dipropyl adipate, dibutyl adipate, dipentyl adipate, diheptyl adipate, di-n-octyl adipate, dinonyl adipate, diisononyl adipate, diisodecyl adipate, bis(2-ethylhexyl) adipate, diisodecyl adipate, butyl benzyl adipate,adipic acid esters such as dicyclopropyl adipate, dicyclobutyl adipate, dicyclopentyl adipate, dicyclohexyl adipate, dicycloheptyl adipate, diallyl adipate, bisbutylbenzyl adipate, and diphenyl adipate; trimethyl trimellitate, triethyl trimellitate, tripropyl trimellitate, tributyl trimellitate, tripentyl trimellitate, triheptyl trimellitate, tri-n-octyl trimellitate, trinonyl trimellitate, and triisononyl trimellitate; Trimellitic acid esters such as triisodecyl trimellitate, tris(2-ethylhexyl) trimellitate, triisodecyl trimellitate, trisbutylbenzyl trimellitate, tricyclopropyl trimellitate, tricyclobutyl trimellitate, tricyclopentyl trimellitate, tricyclohexyl trimellitate, tricycloheptyl trimellitate, triallyl trimellitate, trisbutylbenzyl trimellitate, and triphenyl trimellitate; dimethyl sebacate, diethyl sebacate, dipropyl sebacate; Sebacate esters such as dibutyl sebacate, dipentyl sebacate, diheptyl sebacate, di-n-octyl sebacate, dinonyl sebacate, diisononyl sebacate, diisodecyl sebacate, bis(2-ethylhexyl) sebacate, diisodecyl sebacate, butyl benzyl sebacate, dicyclopropyl sebacate, dicyclobutyl sebacate, dicyclopentyl sebacate, dicyclohexyl sebacate, dicycloheptyl sebacate, diallyl sebacate, bisbutyl benzyl sebacate, and diphenyl sebacate; Examples of the succinate include dimethyl succinate, diethyl succinate, dipropyl succinate, dibutyl succinate, dipentyl succinate, diheptyl succinate, di-n-octyl succinate, dinonyl succinate, diisononyl succinate, diisodecyl succinate, bis(2-ethylhexyl) succinate, diisodecyl succinate, butylbenzyl succinate, dicyclopropyl succinate, dicyclobutyl succinate, dicyclopentyl succinate, dicyclohexyl succinate, dicycloheptyl succinate, diallyl succinate, bisbutylbenzyl succinate, and diphenyl succinate.
[0110] Examples of sulfonamide plasticizers include aromatic sulfonamide plasticizers, and specific examples include N-butylbenzenesulfonamide, p-toluenesulfonamide, o-toluenesulfonamide, p-toluenesulfonamide, N-ethyl-p-toluenesulfonamide, N-ethyl-o-toluenesulfonamide, N-n-butylbenzenesulfonamide, and N-cyclohexyl-p-toluenesulfonamide. N-butylbenzenesulfonamide is preferred.
[0111] Examples of phosphate ester plasticizers include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tris(2-ethylhexyl) phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and 2-ethylhexyl diphenyl phosphate.
[0112] Examples of polyester plasticizers include: polyesters composed of an acid component such as adipic acid, terephthalic acid, isophthalic acid, or diphenyldicarboxylic acid and a diol component such as propylene glycol, 1,3-butanediol, 1,4-butanediol, ethylene glycol, or diethylene glycol; and polyesters composed of hydroxycarboxylic acids such as polycaprolactone. These polyesters may be end-capped with a monofunctional carboxylic acid or a monofunctional alcohol, or may be end-capped with an epoxy compound or the like.
[0113] Examples of polyalkylene glycol plasticizers include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, ethylene oxide addition polymers of bisphenols, and propylene oxide addition polymers of bisphenols; and terminal-blocking compounds such as the above-mentioned terminal epoxy-modified compounds, terminal ester-modified compounds, and terminal ether-modified compounds.
[0114] Other plasticizers include, for example, glycerin fatty acid esters such as glycerin monoacetomonolaurate, glycerin diacetomonolaurate, and glycerin monoacetomonostearate; fatty acid amides such as stearic acid amide; aliphatic carboxylic acid esters such as butyl oleate; oxyacid esters such as methyl acetylricinoleate and butyl acetylricinoleate; pentaerythritol; and various sorbitols.
[0115] When the photosensitive resin composition contains a plasticizer, the proportion thereof is preferably 0.5 parts by mass or more and 40 parts by mass or less relative to 100 parts by mass of the (A) polyimide. From the viewpoint of the flatness of the coating film when the photosensitive composition is applied, the proportion thereof is more preferably 1 part by mass or more. Furthermore, from the viewpoint of suppressing film shrinkage, the proportion thereof is more preferably 30 parts by mass or less.
[0116] Components other than the above components (A) to (J) (other components) The photosensitive resin composition may further contain optional components (other components) other than the above components (A) to (J). Examples of other components include hindered phenol compounds, adhesion promoters, sensitizers, thermal polymerization inhibitors, surfactants, and thermal base generators.
[0117] From the viewpoint of suppressing discoloration of the copper surface, the photosensitive resin composition may optionally contain a hindered phenol compound. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), and 4,4'-butylidene-bis(3-methyl-6-t-butyl). phenol), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl-6-t-butylphenyl)propionate 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4, 6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethyl benzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, Examples include 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione.
[0118] Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione and the like are particularly preferred.
[0119] When the photosensitive resin composition contains a hindered phenol compound, the content thereof is preferably 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the polyimide (A). When the photosensitive resin composition is formed on copper or a copper alloy, the content thereof is more preferably 0.5 parts by mass or more from the viewpoint of preventing discoloration and corrosion of the copper or copper alloy. Furthermore, the content thereof is more preferably 10 parts by mass or less from the viewpoint of photosensitivity.
[0120] From the viewpoint of improving the adhesion between the cured film and the substrate, the photosensitive resin composition may optionally contain an adhesion promoter other than the silane coupling agent. Examples of such adhesion promoters include aluminum-based adhesion promoters.
[0121] Examples of aluminum-based adhesion promoters include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0122] When the photosensitive resin composition contains an adhesion aid, the proportion thereof is preferably 0.01 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the (A) polyimide. From the viewpoint of adhesiveness, the proportion is more preferably 0.5 parts by mass or more. Furthermore, from the viewpoint of storage stability of the photosensitive resin composition, the proportion is more preferably 20 parts by mass or less.
[0123] The photosensitive resin composition may optionally contain a sensitizer from the viewpoint of improving photosensitivity. Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, and p-dimethylaminocinnamylideneindano. p-dimethylaminobenzylidene indanone, 2-(p-dimethylaminophenylbiphenylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl
[0039] Examples of the methylaminobenzoate include methylaminobenzoate, ...
[0124] When the photosensitive resin composition contains a sensitizer, the proportion thereof is preferably 0.1 parts by mass or more and 25 parts by mass or less per 100 parts by mass of the polyimide (A).
[0125] The photosensitive resin composition may optionally contain a thermal polymerization inhibitor, from the viewpoint of improving the stability of viscosity and photosensitivity, particularly when stored in the form of a solution containing a solvent.
[0126] Examples of the thermal polymerization inhibitor include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0127] The photosensitive resin composition may optionally contain a surfactant from the viewpoint of film flatness. Examples of the surfactant include fluorine-based surfactants, silicone-based surfactants, and hydrocarbon-based surfactants.
[0128] The fluorine-based surfactant preferably contains a fluorine atom in the molecule. Examples of the fluorine-based surfactant include perfluoroalkyl sulfonates, perfluoroalkyl carboxylates, perfluoroalkyl alcohols, perfluoroalkyl alkylene oxide adducts, and perfluoroalkyl phosphates. More specifically, the following surfactants are available under the trade names: Megafac F-114, Megafac F-251, Megafac F-253, Megafac F-281, Megafac F-410, Megafac F-430, Megafac F-477, Megafac F-510, Megafac F-551, Megafac F-552, Megafac F-553, Megafac F-554, Megafac F-555, Megafac F-556, Megafac F-557, Megafac F-558, Megafac F-559, Megafac F-560, Megafac F-561, Megafac F-562, Megafac F-563, Megafac F-565, Megafac F-566, Megafac F-567, Megafac F-568, Megafac F-569, Megafac F-570, Megafac F-571, Megafac F-572, Megafac F-573, Megafac F-574, Megafac F-575, Megafac F-576, Megafac F-577, Megafac F-578, Megafac F-579, Megafac F-580, Megafac F-581, Megafac F-582, Megafac F-583, Megafac F-585, Megafac F-586, Megafac F-587, Megafac F-588, Megafac F-589, Megafac F-581, Megafac F-582, Megafac F-58 Fack F-568, Megafack F-569, Megafack F-570, Megafack F-572, Megafack F-574, Megafack F-575, Megafack F-576, Megafack R-40, Megafack R-40-LM, Megafack R-41, Megafack R-94, Megafack RS-56, Megafack RS-72-K, Megafack RS-75, Megafack RS-76-E, Megafack RS-76-NS, Megafack RS-78, Megafack RS-90, Examples of such a resin include Megafac DS-21 (manufactured by DIC Corporation), FC-4430, FC-4432 (manufactured by 3M Japan Ltd.), Surflon S-211, Surflon S-221, Surflon S-231, Surflon S-232, Surflon S-233, Surflon S-241, Surflon S-242, Surflon S-243, Surflon S-420, Surflon S-431, Surflon S-386, Surflon S-611, Surflon S-647, Surflon S-651, Surflon S-653, Surflon S-656, Surflon S-658, Surflon S-693, Surflon S-CFJ, and Surflon FPE-50 (manufactured by AGC Seimi Chemical Co., Ltd.).
[0129] The silicone surfactant preferably has a disiloxane structure as a non-polar moiety. Examples of the silicone surfactant include polyether-modified silicones, such as linear polyether-modified silicones, linear alkyl-co-modified polyether-modified silicones, branched polyether-modified silicones, and branched alkyl-co-modified polyether-modified silicones. More specifically, the product names are KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-644, KF-6020, KF-6204, X-22-4515, KF-6011, KF-6012, KF-6015, KF-6017, KP-301, KP-306, KP-109, KP-310, KP-310B, KP-323, KP-326, KP-341, and KP-10. 4, KP-110, KP-112 (all manufactured by Shin-Etsu Chemical Co., Ltd.); DBE-224, DBE-621, DBE-712, DBE-814, DBE-821, DBE-921, DBP-732, YAD-122, YBD-125, YMS-T31, CMS-626, CMS-222, DBP-534, CMS-832, DBP-C22, QMS-435, ABP-263, DMS-R05, DMS-R11, DMS-R18, DMS-R22, DMS-R31 (all manufactured by Gelest);BYK-300, BYK-301, BYK-302, BYK-306, BYK-307, BYK-310, BYK-313, BYK-315 N, BYK-320, BYK-322, BYK-323, BYK-325 N, BYK-326, BYK-327, BYK-330, BYK-331, BYK-332, BYK-333, BYK-342, BYK-345, BYK-34 6, BYK-347, BYK-348, BYK-349, BYK-350, BYK-352, BYK-354, BYK-355, BYK-356, BYK-358 N, BYK-359, BYK-360 P, BYK-361 N, BYK-364 P, BYK-366 P, BYK-368 P, BYK-370, BYK-375, BYK-377, BYK-378, BYK-381, BYK-390, BYK-392, BYK-394, BYK-399, BYK-UV 3500, BYK-UV 3505, BYK-UV 3510, BYK-UV 3530, BYK-UV 3535, BYK-UV 3570, BYK-UV 3575, BYK-UV 3576 (all manufactured by BYK Japan); Newcol 2302, Newcol 2303, Newcol 2305, Newcol 2307, Newcol 2308, Newcol 2308-HEN, Newcol 2310, Newcol 2312, Newcol 2314, Newcol 2318, Newcol 2320, Newcol 2327(20), Newcol 2330, Newcol 2344, Newcol 2327(20), Newcol 2330, Newcol 2344, Newcol 2327(20), Newcol 2327, ... Examples of such silicone rubbers include Nycol 2360, Newcol 2399-S, and Newcol 2399-S (25) (all manufactured by Nippon Nyukazai Co., Ltd.); DMC6038, OW1500, SPG128VP, L03, L033, L053, and L066 (all manufactured by Wacker Asahi Kasei Silicone Co., Ltd.); and SH-28PA, SH-190, SH-193, SZ-6032, SF-8428, DC-57, and DC-190 (all manufactured by Dow Corning Toray Co., Ltd.).
[0130] The surfactant may have a crosslinkable group in the molecule. Examples of such surfactants include silicone surfactants having a crosslinkable group in the molecule and fluorine surfactants having a crosslinkable group in the molecule.
[0131] Examples of the crosslinkable group include thermally crosslinkable groups such as epoxy groups, N-methylolamide groups, oxazoline groups, and allyl groups, as well as ultraviolet (UV) crosslinkable groups (such as vinyl groups, (meth)acryloyl groups, and epoxy groups). More specific examples of surfactants having a crosslinkable group in the molecule include, by trade name, Megafac RS-75-A, Megafac RS-72-K, Megafac RS-75-NS, Megafac RS-78, Megafac RS-90, and Megafac RS-56 (all manufactured by DIC Corporation); and BYK-UV3500, BYK-UV3505, BYK-UV3530, BYK-UV3570, BYK-UV3575, and BYK-UV3576 (all manufactured by BYK-Chemie).
[0132] The surfactant may be one in which the fluorine-containing group is eliminated by heat treatment, such as Megafac DS-21 (manufactured by DIC Corporation).
[0133] When the photosensitive resin composition contains a surfactant, the proportion of the surfactant is preferably 0.001 parts by mass or more and 1 part by mass or less, and more preferably 0.01 parts by mass or more and 0.1 parts by mass or less, relative to 100 parts by mass of the polyimide (A).
[0134] According to a further aspect of the present embodiment, there is provided a negative photosensitive resin composition comprising: (A) a polyimide; (B) a solvent; and (C) a photopolymerization initiator, wherein the polyimide (A) is represented by the following general formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group.} and has no polymerizable functional groups in the side chains, and the negative photosensitive resin composition is heated at 230°C for 2 hours to produce a cured film having an oxygen permeability of less than 1000. With such a composition, metal wiring is protected from oxidation in the atmosphere during reliability testing. Therefore, ion diffusion is suppressed in reliability tests performed by applying a voltage such as bHAST, making it possible to produce electronic devices with high insulation reliability. The oxygen permeability (cc / m 2The oxygen permeability (24h atm) is preferably less than 500 or less than 200. The oxygen permeability can be measured by the method described in the examples below. The oxygen permeability may be greater than 0.
[0135] <Method for Producing Cured Relief Pattern> The method for producing a cured relief pattern of the present disclosure includes: (1) a step of applying the above-described negative photosensitive resin composition of the present disclosure onto a substrate to form a photosensitive resin layer on the substrate (resin layer forming step); (2) a step of exposing the photosensitive resin layer to light (exposure step); (3) a step of developing the exposed photosensitive resin layer to form a relief pattern (relief pattern forming step); and (4) a step of heat-treating the relief pattern to form a cured relief pattern (cured relief pattern forming step).
[0136] (1) Resin Layer Formation Step In this step, the negative photosensitive resin composition of the present disclosure is applied to a substrate, and then dried as necessary to form a photosensitive resin layer. As the application method, a method conventionally used for applying negative photosensitive resin compositions, such as application using a spin coater, bar coater, blade coater, curtain coater, screen printing machine, etc., or spray application using a spray coater, etc., can be used.
[0137] If necessary, the coating film containing the negative photosensitive resin composition can be dried. Drying methods include air drying, heat drying using an oven or a hot plate, and vacuum drying. Specifically, in the case of air drying or heat drying, drying can be carried out at 20°C to 150°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on the substrate.
[0138] (2) Exposure Step In this step, the photosensitive resin layer formed above is exposed to an ultraviolet light source or the like using an exposure device such as a contact aligner, mirror projection, or stepper, either directly or through a patterned photomask or reticle. This exposure causes the polymerizable functional groups of the polyimide (A) contained in the negative photosensitive resin composition to crosslink due to the action of the photopolymerization initiator (C). This crosslinking makes the exposed portion insoluble in the developer described below, enabling the formation of a relief pattern.
[0139] Thereafter, for the purpose of improving photosensitivity, etc., post-exposure baking (PEB) or pre-development baking, or both, may be performed at any combination of temperature and time, as necessary. The baking conditions are preferably a temperature of 40°C to 120°C and a time of 10 seconds to 240 seconds, but are not limited to these ranges as long as the properties of the negative-type photosensitive resin composition of the present disclosure are not impaired.
[0140] (3) Relief Pattern Forming Step In this step, the unexposed portions of the exposed photosensitive resin layer are developed and removed to form a relief pattern. As a development method for developing the exposed (irradiated) photosensitive resin layer, any method can be selected from conventionally known photoresist development methods, such as a rotary spray method, a paddle method, and an immersion method accompanied by ultrasonic treatment. After development, post-development baking may be performed at any combination of temperature and time, as necessary, for the purpose of adjusting the shape of the relief pattern, etc.
[0141] The developer used for development is preferably, for example, a good solvent for the negative-tone photosensitive resin composition, or a combination of a good solvent and a poor solvent. Examples of good solvents include N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, and α-acetyl-γ-butyrolactone. Examples of poor solvents include toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, and water. When a mixture of a good solvent and a poor solvent is used, it is preferable to adjust the ratio of the poor solvent to the good solvent depending on the solubility of the polymer in the negative-tone photosensitive resin composition. Two or more solvents, for example, a combination of several solvents, can also be used.
[0142] (4) Cured Relief Pattern Formation Step In this step, the relief pattern obtained by development is heat-treated to dissolve the photosensitive component, thereby forming a cured relief pattern composed of polyimide. Heat treatment can be performed using a variety of methods, including a hot plate, an oven, or a temperature-programmable heating oven. Heat treatment can be performed, for example, at 160°C to 350°C for 30 minutes to 5 hours. The heat treatment temperature is preferably 300°C or less, more preferably 250°C or less. Air may be used as the ambient gas during heat curing, or an inert gas such as nitrogen or argon may also be used. A cured film containing a cured product of the negative photosensitive resin composition of the present disclosure also constitutes one aspect of the present invention.
[0143] <Semiconductor Device> The present disclosure also provides a semiconductor device having a cured relief pattern obtained from the above-described negative photosensitive resin composition. Specifically, the present disclosure provides a semiconductor device having a substrate that is a semiconductor element and a cured relief pattern. The cured relief pattern may be produced by the above-described method for producing a cured relief pattern using the above-described negative photosensitive resin composition.
[0144] The present disclosure also provides a method for manufacturing a semiconductor device, which uses a semiconductor element as a substrate and includes, as part of its steps, the method for manufacturing a cured relief pattern according to the present embodiment. In this case, the cured relief pattern formed by the method for manufacturing a cured relief pattern according to the present disclosure can be formed as a surface protective film for a semiconductor device, an interlayer insulating film, an insulating film for redistribution wiring, a protective film for a flip-chip device, or a protective film for a semiconductor device having a bump structure, and can be manufactured by combining the formed cured relief pattern with a known method for manufacturing a semiconductor device.
[0145] <Display Device> The present disclosure also provides a display device including a display element and a cured film provided on the display element, the cured film having the cured relief pattern described above. The cured relief pattern may be laminated in direct contact with the display element, or may be laminated via another layer. The cured film may be applied to, for example, surface protection films, insulating films, planarizing films, etc. of TFT liquid crystal display elements and color filter elements; protrusions for MVA-type liquid crystal display devices; and partition walls for cathodes of organic EL elements.
[0146] The negative photosensitive resin composition of the present disclosure is useful not only for application to the semiconductor devices described above, but also for applications such as an interlayer insulating film in a multilayer circuit, a cover coat for a flexible copper-clad board, a solder resist film, and a liquid crystal alignment film.
[0147] <Method for Producing Negative-Type Photosensitive Resin Composition> The method for producing a negative-type photosensitive resin composition according to the present disclosure may include the steps of producing (A) a polyimide by the method according to the present disclosure as described above in "(A) Method for Producing Polyimide," and obtaining a negative-type photosensitive resin composition by mixing (A) a polyimide, (B) a solvent, and (C) a photopolymerization initiator. Optionally, the negative-type photosensitive resin composition may further contain additives selected from the above-described (D) monomer having a polymerizable functional group (radical polymerizable compound), (E) a silane coupling agent, (F) an organic titanium compound, (G) a thermal crosslinking agent, (H) a rust inhibitor, (I) a thermal polymerization initiator, and (J) a plasticizer, as well as other components.
[0148] The present embodiment will be described in more detail with reference to examples. The present embodiment is not limited to the examples. The physical properties of the examples were measured and evaluated according to the following methods.
[0149] [Measurement and Evaluation] (1-1) Weight-average molecular weight (Mw) and number-average molecular weight (Mn) The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of each resin in the Examples and Comparative Examples were measured using gel permeation chromatography (GPC) under the following conditions. In addition, (Mw) / (Mn) was calculated and used as the molecular weight distribution.
[0150] The solvent used was N-methyl-2-pyrrolidone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., prepared by dissolving 30 mmol / L of lithium bromide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.5%) and 50 mmol / L of phosphoric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., for high performance liquid chromatography) immediately before GPC measurement). A calibration curve for calculating the weight-average molecular weight (Mw) was prepared using standard polystyrene (Easy Type PS-1, manufactured by Agilent Technologies).
[0151] (Conditions) Apparatus: HLC-8320 GPC (manufactured by Tosoh Corporation) Column: 2 Tsk gel Super HM-H columns / 1 Tsk gel Super H-RC column (manufactured by Tosoh Corporation) connected in series Flow rate: 0.5 mL / min Column temperature: 40°C Detector: UV-8320 (UV-VIS: ultraviolet-visible spectrophotometer, manufactured by Tosoh Corporation)
[0152] (1-2) Total mass of fluorine atoms (Mw f ) Total mass of fluorine atoms (Mw f ) may be determined based on the raw material components for producing (A) polyimide.
[0153] (2) Cured relief pattern used to evaluate the flatness of prebaked film A photosensitive resin composition prepared by the method described below was spin-coated onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a coater developer (D-Spin 60A model, manufactured by SOKUDO Co., Ltd.), and prebaked on a hot plate at 110°C for 180 seconds. Using a test pattern mask, this coating film was subjected to a 300 mJ / cm irradiation with Prisma GHI (manufactured by Ultratech Co., Ltd.). 2 The coating was then spray-developed with a coater developer (D-Spin 60A model, manufactured by SOKUDO Co., Ltd.) using cyclopentanone as a developer for a time equal to the time required for the unexposed areas to completely dissolve and disappear, multiplied by 1.4. Thereafter, the coating was rotary-sprayed (washed) with propylene glycol methyl ether acetate for 10 seconds to obtain a relief pattern on the silicon.
[0154] The wafer with the relief pattern formed on the Si was subjected to heat treatment in a temperature-programmable curing furnace (VF-2000 model, manufactured by Koyo Lindberg) in a nitrogen atmosphere at 230°C for 2 hours, thereby obtaining a cured relief pattern on the Si that was approximately 15 μm thick and consisted of the resin composition and had vias (circular openings) with a diameter of 26 μm.
[0155] 1(a) is a schematic diagram showing an example of the configuration of the obtained cured relief pattern. As shown in the figure, the cured relief pattern 1 is formed on a Si wafer (not shown) that forms an xy plane, and has circular openings (vias) 10 that open in the z direction. Here, the cured relief pattern 1 has 3x3 vias 10 (a total of nine vias, formed by arranging three in the x direction and three in the y direction).
[0156] On the obtained cured relief pattern, a 200 nm thick Ti film and a 400 nm thick Cu film were sputtered in this order using a sputtering device (Model L-440S-FHL, manufactured by Canon Anelva Corporation).
[0157] (3) Flatness of Prebaked Film The flatness (in-plane uniformity) of the prebaked film was evaluated as follows. A photosensitive resin composition prepared by the method described below was applied onto the relief pattern obtained by the method (2) above by spin coating using a coater developer (D-Spin 60A model, manufactured by SOKUDO Corporation) so that the film would have a dry thickness of 7 μm, and then dried at 110° C. for 180 seconds to form a prebaked film. In this way, a substrate with a prebaked film (film-coated substrate) was obtained.
[0158] The obtained film-coated substrate was split along an imaginary line passing through the center of the via, and the cross section was polished. Then, a cross-sectional SEM image was obtained. The image was observed, and the surface irregularities of the photosensitive resin composition film were evaluated based on the following criteria.
[0159] (Evaluation criteria) "Excellent": Less than 1.0 μm "Good": 1.0 μm or more and less than 2.0 μm "Fair": 2.0 μm or more and less than 4.0 μm "Fail": 4.0 μm or more
[0160] The numerical value of the surface irregularities (average value of the heights at two locations) was calculated as follows: the difference between the total thickness of the film thickness of the cured relief pattern obtained by the method (2) above and the pre-baked film formed on the pattern, and the thickness of the pre-baked film formed in the via was calculated as the numerical value of the surface irregularities.
[0161] 1(b) is a schematic diagram showing an example of the cross-sectional configuration of the film-coated substrate. As shown in the figure, a pre-baked film 2 is formed to cover vias 10 in a cured relief pattern 1, and surface irregularities can be observed at positions corresponding to the vias 10. The film-coated substrate was divided along an imaginary line L (here, line A-A in the x-direction) passing through the center C of the central via 10C among the 3 x 3 vias 10, and the cross-section was polished to obtain a cross-section. In this example, the "numerical value of irregularities" was calculated using the cross-section obtained. Specifically, the "numerical value of irregularities" was calculated as the difference between the total thickness T(1+2) of the film thickness T1 of the cured relief pattern and the pre-baked film T2 formed on that pattern and the film thickness T3 of the pre-baked film formed in the via. In FIG. 1(b), "film thickness T3 of the pre-baked film formed in the via" corresponds to the bottom height of via 10C located at the center of the 3x3 matrix, and "total thickness T(1+2)" corresponds to the average value of the maximum height TL of the left edge of via 10C and the maximum height TR of the right edge of via 10C. Here, maximum height TL corresponds to the maximum height of the convex portion between via 10C and via 10L located to the left of via 10C, and maximum height TR corresponds to the maximum height of the convex portion between via 10C and via 10R located to the right of via 10C. That is, in FIG. 1(b), "numerical value of unevenness" is calculated as the difference between "{(TL+TR) / 2}" and "TC".
[0162] (4) Change in Film Thickness Before and After Heating (Curing) A 200 nm thick Ti film and a 400 nm thick Cu film were sputtered in this order onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a sputtering apparatus (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated onto this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Co., Ltd.), and prebaked on a hot plate at 110°C for 180 seconds to form a coating film approximately 7.5 μm thick. This coating film was then exposed to 800 mJ / cm using a Prisma GHI S / N5503 projection exposure apparatus (manufactured by Ultratech Co., Ltd.) equipped with a gh-ray cut filter. 2The entire surface was exposed to an exposure dose of 1000 ppm. Thereafter, the coating film formed on the wafer was spray-developed using cyclopentanone in a developing machine (D-SPIN636 model, manufactured by Dai-Nippon Screen Mfg. Co., Ltd., Japan). Then, after washing with propylene glycol methyl ether acetate, drying was performed by spin drying. The film thickness after this development and drying was measured, and the resulting film thickness was defined as film thickness 1. The film after this development and drying was further heat-treated at 230°C for 2 hours in a nitrogen atmosphere using a temperature-programmed curing oven (VF-2000 model, manufactured by Koyo Lindberg Co., Ltd.), thereby obtaining a cured film (polyimide film). The film thickness of the cured film was measured, and the resulting film thickness was defined as film thickness 2. Using these film thicknesses, the film thickness change rate before and after heating was calculated using the following formula: Change rate (%) = (film thickness 2 / film thickness 1) × 100, and evaluated based on the following criteria.
[0163] (Evaluation criteria) "Excellent": The rate of change in film thickness before and after heating is 95% or more. "Good": The rate of change in film thickness before and after heating is 92% or more and less than 95%. "Fair": The rate of change in film thickness before and after heating is 90% or more and less than 92%. "Poor": The rate of change in film thickness before and after heating is less than 90%.
[0164] (5) Copper Adhesion A 200 nm thick Ti film and a 400 nm thick Cu film were sputtered in this order onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated onto this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Corporation), and the wafer was pre-baked at 110°C for 180 seconds on a hot plate to form a coating film on the Cu. This coating film was then subjected to 800 mJ / cm irradiation using a Prisma GHI (manufactured by Ultratech Corporation) without using a test pattern mask. 2The cured film was then heated for 2 hours at 230°C in a nitrogen atmosphere using a temperature-programmed curing oven (VF-2000 model, manufactured by Koyo Lindberg Co., Ltd.), to obtain a cured film of the resin composition having a thickness of approximately 7 µm on the Cu. The cured film was evaluated for adhesion between the copper substrate and the cured film according to the cross-cut method of JIS K 5600-5-6, based on the following criteria.
[0165] (Evaluation criteria) "Excellent": The number of lattices of the cured film adhered to the substrate is more than 100. "Good": The number of lattices of the cured film adhered to the substrate is 80 to 100. "Fair": The number of lattices of the cured film adhered to the substrate is 50 to less than 80. "Poor": The number of lattices of the cured film adhered to the substrate is less than 50.
[0166] (6) Cured Relief Pattern Used for Measuring Oxygen Permeability A 100 nm thick Al film was sputtered onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated onto this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Co., Ltd.), and then prebaked on a hot plate at 110°C for 180 seconds to form a coating film on the Al. The resulting photosensitive resin film was then subjected to 800 mJ / cm irradiation using a Prisma GHI (manufactured by Ultratech Co., Ltd.) without using a test pattern mask. 2 After that, the film was heated at 230°C for 2 hours in a nitrogen atmosphere using a temperature programmable curing oven (VF-2000 model, manufactured by Koyo Lindberg Co., Ltd.). As a result, a cured film made of the resin composition and having a thickness of about 7 µm was formed on the Al.
[0167] (7) Oxygen Permeability The cured film on the aluminum obtained in (6) above was treated with 10% hydrochloric acid to obtain a free-standing polyimide film. The oxygen permeability of the obtained free-standing film (polyimide film) was measured under the following conditions. The obtained oxygen permeability results were averaged (n=6) and evaluated based on the following criteria.
[0168] (Conditions) Apparatus used: GTR-10XF (manufactured by GTR Tech Co., Ltd.) Measurement method: JIS K-7126-2 (isobaric GC method) Measurement conditions: temperature and humidity 23°C, 65% RH / gas type: oxygen / cell diameter 35 mmΦ, permeation area 9.62 cm 2
[0169] (Evaluation criteria) "Excellent": Oxygen permeability (cc / m 2 ・24h・atm) Less than 200 "Good": Oxygen permeability (cc / m 2 ・24h・atm) 200 or more and less than 500 "Acceptable": Oxygen permeability (cc / m 2 ・24h・atm) 500 or more and less than 1000 "Not acceptable": Oxygen permeability (cc / m 2 ・24h・ATM) 1000 or more
[0170] (8) Preparation of a cured relief pattern on Cu A 200 nm thick Ti film and a 400 nm thick Cu film were sputtered in this order onto a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a sputtering apparatus (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated onto this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Co., Ltd.), and the wafer was pre-baked on a hot plate at 110°C for 180 seconds to form a coating film. A test pattern mask was used to apply a cured relief pattern to this coating film using a Prisma GHI (manufactured by Ultratech Co., Ltd.) at 300 mJ / cm. 2 The coating was then spray-developed using a coater developer (D-Spin 60A, manufactured by SOKUDO Co., Ltd.) using cyclopentanone as a developer for a time calculated by multiplying the time required for the unexposed areas to completely dissolve and disappear by 1.4. A relief pattern was then obtained on the Cu by rotary spraying (washing) with propylene glycol methyl ether acetate for 10 seconds.
[0171] The wafer with the relief pattern formed on Cu was heat-treated in a temperature-programmable curing furnace (VF-2000 model, manufactured by Koyo Lindberg) in a nitrogen atmosphere at 230°C for 2 hours, thereby forming a cured relief pattern made of the resin composition with a film thickness of approximately 5 μm on Cu.
[0172] (9) Resolution of Cured Relief Pattern on Cu The cured relief pattern obtained in (8) above was observed under an optical microscope, and the size of the smallest opening pattern was determined. For the smallest opening pattern, if the area of the opening in the obtained pattern was at least half the area of the mask opening of the corresponding pattern, it was considered to be resolved. The length of the mask opening side corresponding to the smallest area among the resolved openings was treated as the resolution, and the resolution was evaluated based on the following criteria.
[0173] (Evaluation criteria) "Excellent": Less than 7 μm "Good": 7 μm or more and less than 10 μm "Fair": 10 μm or more and less than 15 μm "Poor": 15 μm or more
[0174] (10) Chemical Resistance Test A 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) was sputtered with a 200 nm thick Ti film and a 400 nm thick Cu film in this order using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Subsequently, a photosensitive resin composition prepared by the method described below was spin-coated on this wafer using a coater developer (D-Spin 60A model, manufactured by SOKUDO Corporation), and then heated and dried on a hot plate at 110°C for 3 minutes to form a photosensitive resin layer. Using a test pattern mask, this photosensitive resin layer was subjected to 500 mJ / cm irradiation using a Prisma GHI (manufactured by Ultratech) equipped with an i-line filter. 2 The coating film formed on the wafer was then spray-developed using cyclopentanone in a developer (D-SPIN636 model, manufactured by Dai-Nippon Screen Mfg. Co., Ltd., Japan). The unexposed areas were then developed and rinsed with propylene glycol methyl ether acetate to obtain a relief pattern of polyimide or a polyimide precursor.
[0175] The wafer on which the relief pattern was formed was heat-treated in a temperature-programmable curing oven (VF-2000, manufactured by Koyo Lindberg) under a nitrogen atmosphere at 230°C for 2 hours to obtain a cured relief pattern made of resin approximately 5 μm thick. The resulting polyimide pattern was immersed in a solution consisting of 1 wt% potassium hydroxide, 39 wt% 3-methoxy-3-methyl-1-butanol, and 60 wt% dimethyl sulfoxide at 50°C for 10 minutes. After rinsing with water and air-drying, the polyimide coating film was evaluated by film thickness measurement and observation under an optical microscope. The dissolution rate (DR) per unit minute was calculated from the measured film thickness, and the chemical resistance of the coating film after immersion was evaluated according to the following evaluation criteria.
[0176] (Evaluation criteria) "Excellent": The change in thickness of the coating film compared to before immersion is within ±3%, and no cracks have occurred. "Good": The change in thickness of the coating film compared to before immersion is more than ±3% but within ±5%, and no cracks have occurred. "Fair": The change in thickness of the coating film compared to before immersion is more than ±5% but within ±7%, and no cracks have occurred. "Poor": The change in thickness of the coating film compared to before immersion is more than ±7%, or cracks have occurred.
[0177] Each abbreviation stands for the name of the compound shown below: ODPA: 4,4'-oxydiphthalic dianhydride BPDA: 4,4'-biphenylic dianhydride BPADA: 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride PMDA: pyromellitic anhydride BCD: bicyclo[2.2.2. ]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic anhydride PDPE: 4,4'-diamino-2-phenyldiphenyl ether m-TB: 4,4'-dimethylbiphenyl-4,4'-diamine TFMB: 2,2'-bis(trifluoromethyl)benzidine HFBAPP: 4,4'-(hexafluoroisopropylidene)bis(4-aminophenoxy)benzene TPEQ: 1,4-bis(4-aminophenoxy)benzene DADPE: 4,4'-diaminodiphenyl ether HEMA: 2-hydroxyethyl methacrylate DCC: dicyclohexylcarbodiimide NMP: N-methylpyrrolidone GBL: γ-butyrolactone
[0178] Synthesis Example 1 (A) Synthesis of Polyimide A-1) 200.0 g of NMP and 22.1 g (0.08 mol) of PDPE were added to a three-neck flask equipped with a Dean-Stark extractor and purged with nitrogen. 31.0 g (0.10 mol) of ODPA and 48.4 g of toluene were then mixed with this and heated to 180°C. It was confirmed that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor. Thereafter, heating was stopped and the mixture was cooled to room temperature. This yielded a reaction liquid.
[0179] The resulting reaction solution was mixed with 800 g of ethyl alcohol, thereby obtaining a precipitate consisting of a crude polymer. The resulting crude polymer was filtered off and mixed with 300 g of GBL to obtain a crude polymer solution. The resulting crude polymer solution was added dropwise to 3 kg of water to precipitate the polymer, and the resulting precipitate was filtered off. The resulting solution was then vacuum dried to obtain a powdery polymer (Polyimide A-1). The molecular weight of Polyimide A-1 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 13,600, and the Mw / Mn was 1.54.
[0180] <Synthesis Example 2> (A) Synthesis of Polyimide A-2) Polyimide A-2 was obtained in the same manner as in Synthesis Example 1, except that 52.0 g of BPADA was used instead of ODPA in Synthesis Example 1. The molecular weight of polyimide A-2 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 15,200, and Mw / Mn was 1.58.
[0181] <Synthesis Example 3> (A) Synthesis of Polyimide A-3) Polyimide A-3 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 10.9 g of PMDA and 15.5 g of ODPA. The molecular weight of Polyimide A-3 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 16,000 and Mw / Mn was 1.61.
[0182] <Synthesis Example 4> (A) Synthesis of Polyimide A-4) Polyimide A-4 was obtained in the same manner as in Synthesis Example 1, except that 24.8 g of BCD was used instead of ODPA in Synthesis Example 1. The molecular weight of Polyimide A-4 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 8,800 and Mw / Mn was 1.41.
[0183] <Synthesis Example 5> (A) Synthesis of Polyimide A-5) Polyimide A-5 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 24.8 g of BCD and the amount of PDPE was changed to 24.6 g. The molecular weight of Polyimide A-5 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 12,800 and Mw / Mn was 1.52.
[0184] <Synthesis Example 6> (A) Synthesis of Polyimide A-6) Polyimide A-6 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 24.8 g of BCD and 25.5 g of PDPE. The molecular weight of Polyimide A-6 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 24,200 and Mw / Mn was 1.72.
[0185] <Synthesis Example 7> (A) Synthesis of Polyimide A-7) Polyimide A-7 was obtained in the same manner as in Synthesis Example 1, except that 19.6 g of CBDA was used instead of ODPA in Synthesis Example 1. The molecular weight of polyimide A-7 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 16,800 and Mw / Mn was 1.62.
[0186] <Synthesis Example 8> (A) Synthesis of Polyimide A-8) Polyimide A-8 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 11.8 g of CBDA and 8.7 g of PMDA. The molecular weight of polyimide A-8 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 15,600 and Mw / Mn was 1.58.
[0187] <Synthesis Example 9> (A) Synthesis of Polyimide A-9) Polyimide A-9 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 45.8 g of BPAF, 13.3 g of PDPE, and 6.8 g of m-TB. The molecular weight of polyimide A-9 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 11,600 and Mw / Mn was 1.49.
[0188] <Synthesis Example 10> (Synthesis of (A) Polyimide A-10) Polyimide A-10 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 6.5 g of PMDA and 21.7 g of ODPA, and the PDPE was changed to 15.5 g and 6.0 g of TFMB. The molecular weight of polyimide A-10 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 11,600 and Mw / Mn was 1.54.
[0189] <Synthesis Example 11> (Synthesis of (A) Polyimide A-11) Polyimide A-11 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 6.5 g of PMDA and 21.7 g of ODPA, and the PDPE was changed to 15.5 g and 9.7 g of HFBAPP. The molecular weight of polyimide A-11 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 10,640, and Mw / Mn was 1.56.
[0190] <Synthesis Example 12> (Synthesis of (A) Polyimide A-12) Polyimide A-12 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 24.8 g of BCD and the amount of PDPE was changed to 31.1 g. The molecular weight of polyimide A-12 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 12,000 and Mw / Mn was 1.51.
[0191] Synthesis Example 13 (Synthesis of (A) Polyimide A-13) 200 g of GBL and 24.6 g of PDPE were added to a three-neck flask equipped with a Dean-Stark extractor and purged with nitrogen. 24.8 g of BCD and 48.4 g of toluene were then mixed with this and heated to 180°C. It was confirmed that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor. Thereafter, heating was stopped and the mixture was cooled to room temperature. This yielded a reaction mixture.
[0192] Next, a solution of 18.6 g of DCC and 18.6 g of GBL was mixed with the above reaction mixture under ice cooling while stirring, and then 12.0 g of HEMA was mixed. 5.3 g of 4-dimethylaminopyridine was further mixed and stirred at room temperature. A precipitate formed in the reaction mixture was removed by filtration to obtain a reaction mixture.
[0193] The resulting reaction solution was mixed with 500 g of ethyl alcohol, thereby obtaining a precipitate consisting of a crude polymer. The resulting crude polymer was filtered off and then mixed with 300 g of GBL, thereby obtaining a crude polymer solution. The resulting crude polymer solution was added dropwise to 3 kg of water to precipitate the polymer, and the resulting precipitate was filtered off. The resulting solution was then vacuum dried to obtain a powdery polymer (polyimide A-13). The molecular weight of polyimide A-13 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 13,200, and the Mw / Mn was 1.52.
[0194] Synthesis Example 14 (Synthesis of (A) Polyimide A-14) 200 g of GBL and 31.1 g of PDPE were added to a three-neck flask equipped with a Dean-Stark extractor and purged with nitrogen. 24.8 g of BCD and 48.4 g of toluene were then mixed and heated to 180°C. It was confirmed that the theoretical amount of water and the added toluene had been extracted into the Dean-Stark extractor. Thereafter, heating was stopped and the mixture was cooled to room temperature. This yielded a reaction mixture. The resulting reaction mixture was mixed with 7.2 g of Karenz MOI (trade name; manufactured by Showa Denko KK) and stirred to yield a reaction mixture.
[0195] The resulting reaction solution was mixed with 500 g of ethyl alcohol, thereby obtaining a precipitate consisting of a crude polymer. The resulting crude polymer was filtered off and then mixed with 300 g of GBL to obtain a crude polymer solution. The resulting crude polymer solution was added dropwise to 3 kg of water to precipitate the polymer, and the resulting precipitate was filtered off. The resulting solution was then vacuum dried to obtain a powdery polymer (Polyimide A-14). The molecular weight of Polyimide A-14 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 12,320, and the Mw / Mn was 1.51.
[0196] <Synthesis Example 15> (Synthesis of (A) Polyimide A-15) Polyimide A-15 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 52.0 g of BPADA and the PDPE was changed to 36.5 g of TPEQ. The molecular weight of polyimide A-15 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 12,400 and Mw / Mn was 1.52.
[0197] <Synthesis Example 16> (Synthesis of (A) Polyimide A-16) Polyimide A-16 was obtained in the same manner as in Synthesis Example 1, except that 25.0 g of 2-phenoxybenzene-1,4-diamine was used instead of the PDPE in Synthesis Example 1. The molecular weight of polyimide A-16 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 14,000 and Mw / Mn was 1.56.
[0198] <Synthesis Example 17> (Synthesis of (A) Polyimide A-17) Polyimide A-17 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 29.4 g of BPDA and the amount of PDPE was changed to 23.0 g. The molecular weight of polyimide A-17 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 20,000 and Mw / Mn was 1.63.
[0199] <Synthesis Example 18> (A) Synthesis of Polyimide A-18) Polyimide A-18 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 12.4 g of BCD and 10.9 g of PMDA, and the amount of PDPE was changed to 32.2 g. The molecular weight of polyimide A-18 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 23,000, and Mw / Mn was 1.67.
[0200] <Synthesis Example 19> (A) Synthesis of Polyimide A-19) Polyimide A-19 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 12.4 g of BCD and 10.9 g of PMDA, and the amount of PDPE was changed to 33.1 g. The molecular weight of polyimide A-19 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 21,200, and Mw / Mn was 1.64.
[0201] <Synthesis Example 20> (A) Synthesis of Polyimide A-20) Polyimide A-20 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 11.8 g of CBDA and 12.4 g of ODPA, and the PDPE was changed to 24.0 g of 2-phenoxybenzene-1,4-diamine. The molecular weight of polyimide A-20 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 19,000, and the Mw / Mn was 1.60.
[0202] <Synthesis Example 21> (Synthesis of (A) Polyimide A-21) Polyimide A-21 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 12.4 g of BCD and 15.5 g of ODPA, and the PDPE was changed to 29.0 g of BAFL. The molecular weight of polyimide A-20 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 18,500, and Mw / Mn was 1.59.
[0203] <Synthesis Example 22> (Synthesis of (A) Polyimide A-22) Polyimide A-22 was obtained in the same manner as in Synthesis Example 1, except that the ODPA in Synthesis Example 1 was changed to 44.4 g of 6-FDA and the PDPE was changed to 29.1 g of TFMB. The molecular weight of polyimide A-22 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 24,000 and Mw / Mn was 1.52.
[0204] <Synthesis Example 23> (Synthesis of (A) Polyimide A-23) Polyimide A-23 was obtained in the same manner as in Synthesis Example 1, except that the PDPE in Synthesis Example 1 was changed to 30.4 g of TFMB. The molecular weight of polyimide A-23 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 40,000 and Mw / Mn was 1.82.
[0205] Synthesis Example 24 Synthesis of Polyimide Precursor Polymer A-24 31.0 g of ODPA as an acid component was placed in a 1-liter separable flask, and then 26.2 g of HEMA and 81.7 g of GBL were mixed therein. 16.3 g of pyridine was added thereto with stirring at room temperature to obtain a reaction mixture. After the heat generated by the reaction had ceased, the mixture was allowed to cool to room temperature and then allowed to stand for a further 16 hours.
[0206] Next, a solution containing 41.3 g of DCC and 41.3 g of GBL was mixed with the reaction mixture over 40 minutes under ice cooling while stirring. Furthermore, a solution containing 15.0 g of DADPE (diamine component) and 75.1 g of GBL was mixed with the reaction mixture over 60 minutes while stirring. After stirring for 2.5 hours at room temperature, 15 g of ethyl alcohol was added and stirred for 30 minutes, followed by mixing with 97 g of GBL, thereby obtaining a reaction mixture. The precipitate that formed in the reaction mixture was removed by filtration to obtain a reaction solution.
[0207] The resulting reaction solution was mixed with 800 g of ethyl alcohol, thereby obtaining a precipitate consisting of a crude polymer. The resulting crude polymer was filtered off and then mixed with 300 g of GBL, thereby obtaining a crude polymer solution. The resulting crude polymer solution was added dropwise to 3 kg of water to precipitate the polymer, and the resulting precipitate was filtered off. The resulting solution was then vacuum dried to obtain a powdery polymer (Polyimide A-24). The molecular weight of Polyimide A-24 was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 13,600, and the Mw / Mn was 1.49.
[0208] [Preparation of Photosensitive Resin Compositions] <Examples 1 to 56 and Comparative Examples 1 to 3> Resin composition solutions were prepared by mixing (A) polyimide, (B) solvent, (C) photopolymerization initiator, (D) radical polymerizable compound, (E) silane coupling agent, (F) organotitanium compound, (G) thermal crosslinking agent, (H) rust inhibitor, (I) thermal polymerization initiator, and (J) plasticizer in the proportions shown in the tables. The proportions shown in the tables are the parts by mass of each component when component (A) is taken as 100 parts by mass.
[0209] The resulting solution was filtered through a polyethylene filter with pores of 0.2 μm to obtain the resin compositions of Examples 1 to 56 and Comparative Examples 1 to 3. The symbols in the tables represent the following components, respectively.
[0210] B-1: γ-butyrolactone B-2: dimethyl sulfoxide B-3: N-methyl-2-pyrrolidone B-4: 3-methoxy-N,N-dimethylpropanamide C-1: TR-PBG-3057 (product name, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) C-2: Irugacure OXE02 (product name, manufactured by BASF Japan Ltd.) D-1: 2-(o-phenylphenoxy)ethyl acrylate D-2: AM-90G (product name, manufactured by Shin-Nakamura Chemical Co., Ltd.) D-3: dicyclopentanyl acrylate D-4: tris-(2-acryloxyethyl) isocyanurate D-5: ditrimethylolpropane tetraacrylate D-6: tetraethylene glycol dimethacrylate E-1: N-phenyl-3-aminopropyltrimethoxysilane E-2: 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane F-1: Titanium diisopropoxide bis(ethylacetoacetate) F-2: Titanium diisopropoxide bis(acetylacetonate) G-1: 1,3,4,6-tetrakis(methoxymethyl)glycoluril G-2: 1,3-bis(methoxymethyl)urea G-3: Trifunctional epoxy resin VG3101L (product name, manufactured by Printec Co., Ltd.) G-4: 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane H-1: 8-azaadenine H-2: 5-amino-1H-tetrazole H-3: 3-mercapto-1,2,4-triazole H-4: 1H-tetrazole-5-acetic acid I-1: Dicumyl peroxide J-1: Disparlon 1711EF (product name, manufactured by Kusunoki Chemicals Co., Ltd.)
[0211] In Table 6, "a / b" indicates the ratio of the number of moles of the acid component (a) to the number of moles of the diamine acid component (b).
[0212] The Examples were able to achieve both flatness and low oxygen permeability in the prebaked film, and as a result, a better balance was confirmed compared to Comparative Examples 1 and 2. Furthermore, because the Examples used a soluble polyimide with a closed ring structure, it was confirmed that the change in film thickness before and after curing could be suppressed compared to when the polyimide precursor used in Comparative Example 3 was used as component (A).
[0213] By using the present invention, a photosensitive resin composition can be obtained that can form a cured relief pattern in which the prebaked film has excellent flatness, copper adhesion, and low oxygen permeability, and in which film shrinkage due to heating (curing) is suppressed. Furthermore, by using the present invention, a method for producing a cured relief pattern using such a photosensitive resin composition and a cured film can be obtained. The present invention can be suitably used in the field of photosensitive materials that are useful for producing electrical and electronic materials, such as semiconductor devices and multilayer wiring boards.
[0214] 1: Hardened relief pattern 2: Pre-baked film 10: Opening (via)
Claims
1. A negative photosensitive resin composition comprising: (A) a polyimide; (B) a solvent; and (C) a photopolymerization initiator, wherein the polyimide (A) is represented by the following general formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group.}, and the polyimide (A) has no polymerizable functional group in a side chain, and the weight average molecular weight (Mw) of the polyimide (A) and the following formula (b): R(F Cont. ) = (Mw f +1) / (Mw x +Mw Y -36)...(b) (In the formula, Mw f is the total mass of fluorine atoms that may be contained in the polyimide (A), Mw X is the molecular weight of the tetracarboxylic dianhydride constituting the polyimide (A), Mw Y is the molecular weight of the diamine constituting the polyimide (A). Cont. )} satisfies the following formula (a): 300≦Mw×R≦948 (a).
2. The photosensitive resin composition according to claim 1, wherein the weight average molecular weight of the polyimide (A) is 8,000 or more and 23,000 or less.
3. The photosensitive resin composition according to claim 1 or 2, further comprising (D) a radically polymerizable compound.
4. The photosensitive resin composition according to claim 3, wherein the radical polymerizable compound (D) comprises a monofunctional monomer (D1) and a polyfunctional monomer (D2).
5. The photosensitive resin composition according to claim 4, wherein the mass ratio (D1 / D2) of the monofunctional monomer (D1) to the polyfunctional monomer (D2) is greater than 0.01 and less than 0.
5.
6. The photosensitive resin composition according to claim 1 or 2, further comprising at least one selected from the group consisting of: (E) a silane coupling agent, (F) an organotitanium compound, (G) a thermal crosslinking agent, (H) a rust inhibitor, (I) a thermal polymerization initiator, and (J) a plasticizer.
7. The photosensitive resin composition according to claim 1 or 2, comprising 100 parts by mass of the polyimide (A), 30 to 1,000 parts by mass of the solvent (B), and 1 to 30 parts by mass of the photopolymerization initiator (C).
8. X in the formula (1) is any one of the following formulas (2) to (9): The photosensitive resin composition according to claim 1 or 2, which has at least one structure selected from the group consisting of:
9. Y in the formula (1) is any one of the following formulas (10) to (19): The photosensitive resin composition according to claim 1 or 2, which has at least one structure selected from the group consisting of:
10. The photosensitive resin composition according to claim 1 or 2, wherein the polyimide (A) has a polymerizable functional group at its terminal.
11. A method for producing a cured relief pattern, comprising the following steps: (1) applying the photosensitive resin composition according to claim 1 or 2 onto a substrate, and forming a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer; (3) developing the exposed photosensitive resin layer, and forming a relief pattern; and (4) heat-treating the relief pattern, and forming a cured relief pattern.
12. A cured film comprising a cured product of the photosensitive resin composition according to claim 1 or 2.
13. A negative-type photosensitive resin composition comprising (A) a polyimide, (B) a solvent, and (C) a photopolymerization initiator, wherein the polyimide (A) is represented by the following general formula (1): {wherein n is a positive integer, X is a tetravalent group having 6 to 31 carbon atoms, and Y is a divalent group.} and has no polymerizable functional group in a side chain, and the composition is heated at 230° C. for 2 hours in a nitrogen atmosphere to obtain a cured film having an oxygen permeability (cc / m 2 24h atm) is less than 1,000.
Citation Information
Patent Citations
Negative photosensitive resin composition and method for manufacturing cured relief pattern using the same
JP2022091355A
Resin composition
WO2018047688A1
Cited By
Polymer, negative photosensitive resin composition, patterning process, method for forming cured film, interlayer insulating film, surface protective film, and electronic component
EP4636011A1
Resin composition, method for producing cured product, cured product, and electronic component