Glass, window glass for vehicles, glass for sensors, and laminated glass
A tailored glass composition addresses the challenge of achieving high strength and bending formability by balancing Young's modulus, fracture toughness, and viscosity, making it suitable for vehicle windows and sensor glasses.
Patent Information
- Application Number
- PCT/JP2024/014902
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-31
AI Technical Summary
Glass used for mobility, such as vehicle windows and sensor cover glasses, requires higher strength for extended life cycles and carbon neutrality, but glasses with high Young's modulus and fracture toughness are not suitable for bending applications due to high viscosity.
A specific glass composition range is developed, including SiO2 60-72%, Al2O3 3.0-9.0%, B2O3 0.0-4.0%, MgO 3.0-15%, CaO 0.0-5.0%, SrO 0.0-5.0%, BaO 0.0-2.0%, Li2O 1.0-10%, Na2O 6.0-16%, K2O 0.0-3.0%, ZrO2 0.0-1.0%, Y2O3 0.0-1.0%, and RO 11-25%, which balances Young's modulus, fracture toughness, and bending formability.
The glass achieves a Young's modulus of 75 GPa or more, fracture toughness of 0.76 MPa·m1/2, and a yield point of 670°C or less, enabling excellent bending formability and resistance to impact fractures, suitable for vehicle windows and sensor glasses.
Smart Images

Figure JP2024014902_31102024_PF_FP_ABST
Abstract
Description
Glass, vehicle window glass, sensor glass and laminated glass
[0001] The present invention relates to glass, vehicle window glass, sensor glass, and laminated glass.
[0002] In recent years, glass used in mobility, such as glass for vehicles and cover glass for sensors such as LiDAR (Light Detection and Ranging), has been required to have high strength in order to extend its life cycle from the perspective of carbon neutrality.
[0003] In order to improve the strength of glass, it is effective to increase the Young's modulus or fracture toughness of the glass (see, for example, Patent Document 1).
[0004] Japan Special Table No. 2019-529298 Publication Japanese Special Table No. 2019-536728
[0005] However, glasses with high Young's modulus and fracture toughness tend to be viscous, making them unsuitable for applications requiring bending, such as vehicle window glass or cover glass for sensors such as LiDAR.
[0006] For example, the glass described in Patent Document 1 has a Young's modulus of 85 GPa or more and a fracture toughness value of 0.86 MPa m 1/2 Although the annealing point is high at 800° C. or more, the annealing point is high at 800° C. or more. Furthermore, Patent Document 2 discloses glass that has excellent bend formability and can be used for windshields, but the Young's modulus is low at 70 GPa.
[0007] In view of the above problems, an object of the present invention is to provide glass, a vehicle window glass, a sensor glass, and a laminated glass that have excellent fracture toughness and excellent bend formability.
[0008] The present inventors have found that the above problems can be solved by using glass having a specific composition range, and have completed the present invention.
[0009] That is, the present invention is as follows: [1] In mole % on an oxide basis, SiO 2 : 60 to 72% Al 2 O3 :3.0~9.0%B 2 O 3 :0.0~4.0% MgO:3.0~15% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~2.0% Li 2 O: 1.0-10% Na 2 O: 6.0-16% K 2 O: 0.0 to 3.0% ZrO 2 :0.0~1.0% TiO 2 :0.0~1.0% Y 2 O 3 :0.0~1.0% R 2 O: 11 to 25% RO: 7.0 to 20% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 [2] The glass according to [1], having a Young's modulus of 75 GPa or more. [3] The glass according to [1], having a fracture toughness value K measured by the SEPB method. IC is 0.76 MPa m 1/2 [4] The glass according to [1], having a deformation point of 670°C or less. [5] The glass according to [4], having a ratio (H / L) of the H value to the L value calculated by the following formula of 0.10 or less: H=[K 2 O] + [CaO] + [SrO] + [BaO] + [ZrO 2 ]+[TiO 2 ]+[Y 2 O 3 ] L = [SiO 2 ]+[Al 2 O 3 ]+[MgO]+[Li 2 O] + [Na 2 O] (where [ ] means the content of each component in the brackets expressed in mole percent on an oxide basis.) [6] Fracture toughness value K measured by SEPB method IC is 0.80 MPa m 1/2The glass according to [5], wherein the critical impact fracture speed is 35 km / h or more when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm. [8] The glass according to [1], wherein the critical impact fracture speed is 53 km / h or more when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm. [9] The glass according to [8], wherein the thickness is 2.5 mm or more.
[10] A window glass for a vehicle, comprising the glass according to any one of [1] to [9].
[11] A glass for a sensor, comprising the glass according to any one of [1] to [9].
[12] A laminated glass comprising a first glass plate, a second glass plate, and an interlayer sandwiched between the first and second glass plates, wherein the first glass plate is the glass according to any one of [1] to [9].
[13] The laminated glass according to
[12] , wherein the first glass plate has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm, and wherein a critical impact fracture speed when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the surface of the first glass plate is 35 km / h or more.
[14] The laminated glass according to
[12] , wherein a critical impact fracture speed when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the surface of the first glass plate is 53 km / h or more.
[15] The laminated glass according to
[14] , wherein the total thickness of the first glass sheet, the second glass sheet, and the interlayer film is 4.5 mm or more.
[16] The thickness t 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2) is 1.5 or more.
[17] Laminated glass having a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are the glass plates according to any one of [1] to [9].
[18] Laminated glass according to
[12] , wherein the second glass plate is soda lime glass.
[19] Laminated glass according to
[12] , wherein the second glass plate is aluminosilicate glass.
[20] Laminated glass according to
[12] , wherein the second glass plate has been subjected to a chemical strengthening treatment.
[0010] According to the present invention, it is possible to provide glass, a window glass for a vehicle, a glass for a sensor, and a laminated glass that have excellent fracture toughness and excellent bend formability.
[0011] Fig. 1 is a graph showing the relationship between H / L and fracture toughness value. Fig. 2 is a graph showing the relationship between H / L and density. Fig. 3 is a cross-sectional view of an example of laminated glass according to an embodiment of the present invention. Fig. 4 is a conceptual diagram showing a state in which laminated glass according to an embodiment of the present invention is used as a window glass for a vehicle. Fig. 5 is an enlarged view of part S in Fig. 4. Fig. 6 is a cross-sectional view taken along line Y-Y in Fig. 5.
[0012] The present invention will be described in detail below based on embodiments, but the present invention is not limited to these embodiments. Furthermore, in the following drawings, components and parts that perform the same function may be denoted by the same reference numerals, and redundant explanations may be omitted or simplified. Furthermore, the embodiments shown in the drawings are schematic to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the actual product. Furthermore, in this specification, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively.
[0013] <Glass Composition> In this embodiment, the glass composition is expressed in mole percent based on oxides, and contains: SiO 2 : 60 to 72% Al 2 O 3 :3.0~9.0%B 2 O 3:0.0~4.0% MgO:3.0~15% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~2.0% Li 2 O: 1.0-10% Na 2 O: 6.0-16% K 2 O: 0.0 to 3.0% ZrO 2 :0.0~1.0% TiO 2 :0.0~1.0% Y 2 O 3 :0.0~1.0% R 2 O: 11 to 25% RO: 7.0 to 20% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 and O).
[0014] Specific embodiments of the glass of this embodiment will be described below. The composition range of each component is expressed in mole percent based on the oxide unless otherwise specified. The phrase "substantially free of" each component means that the component is not contained except as an unavoidable impurity mixed in from raw materials, etc., that is, the component is not intentionally contained.
[0015] SiO 2 is a component that constitutes the network structure of the glass and is an essential component of the glass of this embodiment. 2 In the glass of this embodiment, the content of SiO 2 When the content of SiO is 60% or more, the structure of the glass becomes strong, and the Young's modulus and fracture toughness value can be increased. In addition, the density of the glass can be easily reduced, and further, moisture resistance and chemical durability can be ensured. Furthermore, an increase in the average linear expansion coefficient can be suppressed, and thermal cracking of the glass can be suppressed. 2 The content is preferably 63% or more, more preferably 64% or more, even more preferably 65% or more, particularly preferably 66% or more, and most preferably 67% or more.
[0016] In addition, in the glass of this embodiment, SiO2 By making the content of SiO 72% or less, an increase in viscosity during glass melting is suppressed, making glass production easier and improving the formability of glass for vehicles, particularly windshields and cover glasses for sensors. 2 The content is preferably 71% or less, more preferably 70% or less, even more preferably 69% or less, and particularly preferably 68% or less.
[0017] Al 2 O 3 is a component that constitutes the network structure of the glass and is an essential component of the glass of this embodiment. 2 O 3 The content is 3.0 to 9.0%. 2 O 3 By making the Al content 3.0% or more, the Young's modulus can be increased. In addition, the weather resistance, moisture resistance, and chemical durability are improved. Furthermore, the average linear expansion coefficient does not become too large, which can suppress thermal cracking of the glass, and also makes it possible to perform chemical strengthening treatment using ion exchange. 2 O 3 The content is preferably 3.2% or more, more preferably 3.4% or more, even more preferably 3.6% or more, particularly preferably 3.8% or more, and most preferably 4.0% or more.
[0018] In addition, in the glass of this embodiment, Al 2 O 3 By ensuring that the Al content is 9.0% or less, an increase in viscosity during glass melting is suppressed, and bending formability is improved, as well as formability for vehicle glass, particularly windshields and cover glass for sensors, etc., is improved. 2 O 3 The content is preferably 7.0% or less, more preferably 6.5% or less, even more preferably 6.0% or less, particularly preferably 5.5% or less, and most preferably 5.0% or less.
[0019] B 2 O 3 is a component that constitutes the network structure of the glass, and is a component that reduces the viscosity of the glass and improves the melting property and bending formability. It also contributes to improving the fracture toughness value. 2 O 3Generally, B is contained in an amount of 0.0 to 4.0%. 2 O 3 Glass containing alkali metals is difficult to manufacture because the alkali metals tend to volatilize during glass manufacturing and corrode the furnace materials. 2 O 3 If the content of B is too high, in addition to the above-mentioned influence on the manufacturing equipment, the homogeneity of the glass may decrease, resulting in a deterioration in optical quality, making the glass unsuitable for sensor applications. 2 O 3 The content of is preferably small, preferably 3.5% or less, more preferably 3.0% or less, even more preferably 2.5% or less, particularly preferably 2.0% or less, and most preferably substantially absent. 2 O 3 The term "substantially free of B" means that the glass 2 O 3 This means that the content is 0.050 mol % or less.
[0020] Also, B 2 O 3 When it contains B 2 O 3 The content may be 0.20% or more, 0.50% or more, 0.80% or more, 1.0% or more, or 1.2% or more.
[0021] MgO is a component that reduces the viscosity of the glass and improves its meltability, and also contributes to improving the Young's modulus and the surface fracture energy described below. The glass of this embodiment contains 3.0 to 15% MgO. By adding 3.0% or more MgO to the glass of this embodiment, the viscosity of the glass can be reduced and the melting of the glass raw materials can be promoted. In addition, the Young's modulus can be increased. The MgO content is preferably 4.0% or more, more preferably 5.0% or more, even more preferably 6.0% or more, particularly preferably 7.0% or more, and most preferably 8.0% or more.
[0022] Furthermore, in the glass of this embodiment, if the MgO content is 15% or less, the glass is less susceptible to devitrification and the viscosity of the glass is prevented from increasing excessively, thereby improving the formability of vehicle glass, particularly windshields, cover glass for sensors, etc. The MgO content is preferably 14% or less, more preferably 13% or less, even more preferably 12% or less, and particularly preferably 11% or less.
[0023] CaO is a component that reduces the viscosity of the glass and improves its bend formability. The glass of this embodiment contains 0.0 to 5.0% CaO. By including CaO in the glass of this embodiment, the meltability of the glass raw materials is improved and the viscosity is further reduced, thereby improving the formability of vehicle glass, particularly windshields and cover glass for sensors. In the glass of this embodiment, the CaO content is preferably 0.20% or more, more preferably 0.40% or more, even more preferably 0.60% or more, particularly preferably 0.80% or more, and most preferably 1.0% or more.
[0024] Furthermore, in the glass of this embodiment, by setting the CaO content to 5.0% or less, an increase in the density of the glass can be suppressed, and the average linear expansion coefficient can be reduced, thereby suppressing thermal cracking of the glass. The CaO content in the glass of this embodiment is preferably 4.5% or less, more preferably 4.0% or less, particularly preferably 3.5% or less, and most preferably 3.0% or less.
[0025] SrO is a component that reduces the viscosity of the glass and improves its bendability. The glass of this embodiment contains 0.0 to 5.0% SrO. By including SrO in the glass of this embodiment, the viscosity of the glass can be reduced. In the glass of this embodiment, the SrO content is preferably 0.20% or more, more preferably 0.40% or more, even more preferably 0.60% or more, particularly preferably 0.80% or more, and most preferably 1.0% or more.
[0026] Furthermore, in the glass of this embodiment, an increase in the density of the glass can be suppressed by setting the SrO content to 5.0% or less. In the glass of this embodiment, the SrO content is preferably 4.5% or less, more preferably 4.0% or less, even more preferably 3.5% or less, even more preferably 3.0% or less, particularly preferably 2.5% or less, and most preferably 2.0% or less.
[0027] In this embodiment, BaO is a component that reduces the viscosity of the glass and improves its bendability. The glass of this embodiment contains 0.0 to 2.0% BaO. By including BaO in the glass of this embodiment, the viscosity of the glass is reduced. When BaO is included in the glass of this embodiment, the BaO content is preferably 0.10% or more, more preferably 0.20% or more, even more preferably 0.30% or more, particularly preferably 0.40% or more, and most preferably 0.50% or more.
[0028] Furthermore, in the glass of this embodiment, an increase in the density of the glass can be suppressed by setting the BaO content to 2.0% or less. In the glass of this embodiment, the BaO content is preferably 1.8% or less, more preferably 1.6% or less, even more preferably 1.4% or less, particularly preferably 1.2% or less, and most preferably 1.0% or less.
[0029] Li 2 O is a component that improves the melting property of glass and reduces the viscosity, and also makes it easier to increase the Young's modulus and contributes to the average linear expansion coefficient of glass. Furthermore, the strength of the glass can be increased by performing a chemical strengthening treatment by ion exchange with Na ions. In the glass of this embodiment, Li 2 The content of O is 1.0 to 10%. 2 By containing 1.0% or more of O, the viscosity of the glass can be reduced. 2 The O content is preferably 1.5% or more, more preferably 2.0% or more, further preferably 2.5% or more, particularly preferably 3.0% or more, and most preferably 3.5% or more.
[0030] Also, Li 2By making the O content 10% or less, the glass is less susceptible to devitrification and thermal cracking of the glass due to an excessively large average linear expansion coefficient can be suppressed. In addition, the moisture resistance of the glass is improved, making it suitable for use as glass exposed to the atmosphere for long periods of time, such as vehicle window glass. 2 The O content is preferably 9.0% or less, more preferably 8.0% or less, further preferably 7.0% or less, and particularly preferably 6.0% or less.
[0031] Na 2 O is a component that improves the melting property of glass and reduces the viscosity, and also makes it easier to increase the Young's modulus and contributes to the average linear expansion coefficient of glass. Furthermore, the strength of the glass can be increased by performing a chemical strengthening treatment by ion exchange with K ions. In the glass of this embodiment, Na 2 The content of O is 6.0 to 16%. 2 By containing 6.0% or more of O, the viscosity of the glass can be reduced. In addition, the Young's modulus and the average linear expansion coefficient can be increased. 2 The O content is preferably 7.0% or more, more preferably 8.0% or more, even more preferably 9.0% or more, and particularly preferably 10% or more.
[0032] Also, Na 2 By keeping the O content at 16% or less, thermal cracking of the glass due to an excessively large average linear expansion coefficient can be suppressed. In addition, the moisture resistance of the glass is improved, making it suitable for use as glass exposed to the atmosphere for long periods of time, such as vehicle window glass. 2 The O content is preferably 15% or less, more preferably 14% or less, further preferably 13% or less, and particularly preferably 12% or less.
[0033] K 2 O is a component that improves the meltability of the glass and reduces the viscosity, and also makes it easier to increase the Young's modulus and contributes to the average linear expansion coefficient of the glass. 2 The O content is 0.0 to 3.0%.
[0034] The glass of this embodiment is K 2By including O, the viscosity of the glass can be reduced. In addition, the Young's modulus and the average coefficient of linear expansion can be increased. 2 The O content is preferably 0.10% or more, more preferably 0.20% or more, even more preferably 0.30% or more, particularly preferably 0.40% or more, and most preferably 0.50% or more.
[0035] On the other hand, K 2 O is Li 2 O and Na 2 Compared to O, it has the effect of increasing the average linear expansion coefficient and density. 2 When the O content is 3.0% or less, thermal cracking of the glass due to an excessively large average linear expansion coefficient can be suppressed. 2 The O content is preferably 2.5% or less, more preferably 2.0% or less, and even more preferably 1.5% or less.
[0036] ZrO 2 is a component that improves chemical durability and Young's modulus. 2 The glass of this embodiment contains 0.0 to 1.0% of ZrO 2 When it is contained, the content is preferably 0.010% or more, more preferably 0.050% or more, further preferably 0.10% or more, and particularly preferably 0.20% or more.
[0037] Furthermore, from the viewpoint of suppressing an increase in the density and viscosity of the glass, ZrO 2 The content is preferably 0.80% or less, more preferably 0.70% or less, further preferably 0.60% or less, and particularly preferably 0.50% or less.
[0038] TiO 2 is a component that improves chemical durability and Young's modulus. 2 The glass of this embodiment contains 0.0 to 1.0% of TiO 2 When it is contained, the content is preferably 0.010% or more, more preferably 0.025% or more, even more preferably 0.050% or more, particularly preferably 0.10% or more, and most preferably 0.20% or more.
[0039] Also, TiO 2When the content of TiO is 1.0% or less, thermal cracking of the glass due to an excessively large average linear expansion coefficient can be suppressed. 2 Since TiO has color in the visible range, there is a risk of a decrease in visible light transmittance. 2 The content is preferably 0.90% or less, more preferably 0.80% or less, further preferably 0.70% or less, and particularly preferably 0.60% or less.
[0040] Y 2 O 3 is a component that improves Young's modulus. 2 O 3 The glass of this embodiment contains 0.0 to 1.0% of Y. 2 O 3 When it is contained, the content is preferably 0.010% or more, more preferably 0.050% or more, further preferably 0.10% or more, and particularly preferably 0.20% or more.
[0041] Also, Y 2 O 3 By making the content of Y 1.0% or less, increases in the density and viscosity of the glass can be suppressed. 2 O 3 The content of is preferably 0.90% or less, more preferably 0.80% or less, further preferably 0.70% or less, particularly preferably 0.60% or less.
[0042] In the glass of this embodiment, Li 2 O, Na 2 O and K 2 The total content of O (hereinafter referred to as R 2 O) is 11 to 25%. 2 When the O content is 11% or more, the Young's modulus increases and the viscosity of the glass decreases, improving the formability of vehicle glass, particularly windshields and cover glass for sensors. 2 The O content is preferably 12% or more, more preferably 13% or more, even more preferably 14% or more, and particularly preferably 15% or more.
[0043] Also, R 2If the O content is 25% or less, the increase in density can be suppressed and the fracture toughness value can be improved. In addition, the weather resistance and moisture resistance can also be improved. 2 O is preferably 23% or less, more preferably 20% or less, even more preferably 19% or less, particularly preferably 18% or less, and most preferably 17% or less.
[0044] In addition, the glass of this embodiment has R 2 Li to O 2 Ratio of O content (Li 2 O / R 2 O) is preferably 0.050 or more. 2 O / R 2 When O is 0.050 or more, the glass has a high Young's modulus and fracture toughness, a low density, and excellent melting properties and bending formability. 2 O / R 2 O is more preferably 0.080 or more, even more preferably 0.10 or more, even more preferably 0.12 or more, particularly preferably 0.15 or more, and most preferably 0.17 or more.
[0045] In addition, from the viewpoint of suppressing the occurrence of devitrification and lowering the devitrification temperature, Li 2 O / R 2 O is preferably 0.60 or less, more preferably 0.50 or less, even more preferably 0.45 or less, particularly preferably 0.42 or less, and most preferably 0.38 or less.
[0046] In addition, the glass of this embodiment has R 2 Na to O 2 O and Li 2 The ratio of the total content of O ((Na 2 O + Li 2 O) / R 2 O) is preferably 0.70 or more. 2 O + Li 2 O) / R 2 When O is 0.70 or more, the glass has a high Young's modulus and fracture toughness, a low density, and excellent melting properties and bending formability. 2 O + Li 2 O) / R 2O is more preferably 0.80 or more, even more preferably 0.85 or more, even more preferably 0.90 or more, particularly preferably 0.92 or more, and most preferably 0.94 or more.
[0047] In the glass of this embodiment, the total content of MgO, CaO, SrO, and BaO (hereinafter sometimes referred to as RO) is 7.0 to 20%. Having an RO content of 7.0% or more can improve the Young's modulus and reduce the viscosity of the glass, thereby improving the meltability and bend formability of the glass. RO is preferably 8.0% or more, more preferably 9.0% or more, and even more preferably 10% or more.
[0048] Furthermore, if RO is 20% or less, an increase in the density of the glass can be suppressed, improving the crack resistance of the glass. Furthermore, moisture resistance and devitrification of the glass can be suppressed. RO is preferably 19% or less, more preferably 18% or less, even more preferably 17% or less, even more preferably 16% or less, particularly preferably 15% or less, and most preferably 14% or less.
[0049] Furthermore, in the glass of this embodiment, the ratio of the MgO content to the RO content (MgO / RO) is preferably 0.20 or more. When MgO / RO is 0.20 or more, the glass has a high Young's modulus and fracture toughness, a low density, and excellent meltability and bend formability. MgO / RO is more preferably 0.25 or more, even more preferably 0.33 or more, even more preferably 0.50 or more, particularly preferably 0.70 or more, and most preferably 0.75 or more.
[0050] Furthermore, from the viewpoint of suppressing devitrification caused by the inclusion of MgO and lowering the devitrification temperature, MgO / RO is preferably 1.0 or less, more preferably 0.98 or less, even more preferably 0.95 or less, particularly preferably 0.90 or less, and most preferably 0.85 or less.
[0051] In the glass of this embodiment, the ratio of the H value to the L value (H / L) calculated by the following formula is preferably 0.10 or less: H=[K 2 O] + [CaO] + [SrO] + [BaO] + [ZrO 2 ]+[TiO 2 ]+[Y 2 O3 ] L = [SiO 2 ]+[Al 2 O 3 ]+[MgO]+[Li 2 O] + [Na 2 O] (where [ ] means the content of each component in the brackets expressed in mole percent on an oxide basis.)
[0052] Here, the H value contributes to improving the Young's modulus and fracture toughness value, but ZrO, which is a component that tends to increase the viscosity of glass, 2 , TiO 2 and Y 2 O 3 and K, a component that contributes to an increase in density. 2 The L value is the total content of SiO, CaO, SrO, and BaO. 2 and Al 2 O 3 The increase in density is small, and MgO and Li, which are components that contribute to improving Young's modulus and fracture toughness, 2 O and Na 2 The total content of O.
[0053] The inventors have found that the ratio of the H value to the L value (H / L) correlates with fracture toughness and density. Specifically, as shown in FIG. 1 , the smaller the H / L, the higher the fracture toughness, and as shown in FIG. 2 , the smaller the H / L, the lower the density. In this embodiment, if H / L is preferably 0.10 or less, the fracture toughness can be increased while the density can be reduced. H / L is more preferably 0.080 or less, even more preferably 0.070 or less, even more preferably 0.060 or less, particularly preferably 0.050 or less, and most preferably 0.040 or less.
[0054] [Other Components] Fe 2 O 3 is a component that improves the heat insulating properties of the glass and also contributes to the color of the glass, and therefore may be contained in the glass of the present embodiment. 2 O 3 The total iron content converted to iron is preferably 0.0025 to 1.2%. 2O 3 The total iron content converted to ferrous iron is the total iron content of FeO, which is an oxide of divalent iron, and Fe, which is an oxide of trivalent iron. 2 O 3 This refers to the total amount of iron, including Fe. 2 O 3 By containing Fe, the material is suitable for applications requiring heat insulation properties. 2 O 3 By including the glass, it is possible to suppress the load on the melting furnace caused by heat radiation reaching the bottom surface of the melting furnace during glass melting.
[0055] When the glass of this embodiment is used for vehicle glass, Fe in the glass of this embodiment is preferably used in order to improve heat insulation, provide design, and facilitate heat transfer to the glass during bending. 2 O 3 The total iron content, calculated as % iron, is preferably 0.0025% or more, more preferably 0.0040% or more, even more preferably 0.039% or more, still more preferably 0.097% or more, particularly preferably 0.11% or more, particularly preferably 0.15% or more, and most preferably 0.17% or more.
[0056] In addition, from the viewpoint of suppressing the decrease in light transmittance in the visible range, Fe 2 O 3 The total iron content, calculated as iron content, is preferably 1.0% or less, more preferably 0.80% or less, even more preferably 0.60% or less, particularly preferably 0.50% or less, and most preferably 0.40% or less.
[0057] Furthermore, when the glass of this embodiment is used for the cover glass of LiDAR or a camera, from the viewpoint of facilitating melting of raw materials during glass production and reducing the amount of expensive high-purity raw materials used, Fe 2 O 3 The total iron content converted into % is preferably 0.0030% or more, more preferably 0.0032% or more, even more preferably 0.0034% or more, still more preferably 0.0036% or more, particularly preferably 0.0038% or more, particularly preferably 0.0040% or more, and most preferably 0.0042% or more.
[0058] In addition, from the viewpoint of suppressing the decrease in light transmittance in the visible and near-infrared regions, Fe 2 O 3 The total iron content, calculated as iron content, is preferably 0.020% or less, more preferably 0.010% or less, even more preferably 0.0080% or less, particularly preferably 0.0070% or less, and most preferably 0.0060% or less.
[0059] The glass of this embodiment contains Fe 2 O 3 Fe in total iron converted to 2 O 3 It is preferable that the mass percentage (%) of divalent iron converted to Fe (hereinafter referred to as Fe-Redox) is 15% or more. 2 O 3 Fe relative to the total iron content converted 2 O 3 Conversion Fe 2+ The percentage of content.
[0060] The glass of this embodiment has an Fe-Redox content of 15% or more, and therefore has an absorption in the near-infrared region. 2+ Since the content of [beta] can be increased, heat is more easily transferred to the molten glass during glass production, improving manufacturability. In addition, the transmittance in the near-infrared region is reduced, improving heat insulation, making the glass suitable for applications requiring heat insulation, such as vehicle glass.
[0061] When the glass of this embodiment is used for a vehicle glass, the Fe-Redox is more preferably 20% or more, further preferably 22% or more, and particularly preferably 24% or more. Furthermore, the Fe-Redox is preferably 50% or less. By having the Fe-Redox content of 50% or less, deterioration of the melting equipment can be suppressed, and the amount of SO in the fining agent can be reduced. 3 When Fe-Redox is used, amber coloring can be suppressed and a decrease in visible light transmittance can be suppressed. Fe-Redox is more preferably 45% or less, further preferably 40% or less, and particularly preferably 38% or less.
[0062] On the other hand, when the glass of this embodiment is used as a cover glass for LiDAR, Fe-Redox is more preferably 16% or more, even more preferably 17% or more, and particularly preferably 18% or more. Furthermore, Fe-Redox is preferably 35% or less. By having Fe-Redox 35% or less, a decrease in transmittance in the near-infrared region can be suppressed. Fe-Redox is more preferably 32% or less, even more preferably 30% or less, and particularly preferably 28% or less.
[0063] Fe-Redox can be adjusted by the raw material composition, melting temperature, and melting atmosphere. Fe-Redox can also be adjusted by using a reducing agent such as coke or ammonium chloride as a raw material to control the degree of oxidation-reduction of the glass melt.
[0064] The glass of the present embodiment may contain components other than the above components (hereinafter also referred to as "other components").
[0065] Other components include, for example, CeO 2 , Nd 2 O 5 , GaO 2 , GeO 2 , MnO 2 , NiO, Cr 2 O 3 , V 2 O 5 , Au 2 O 3 , Ag 2 O, CuO, CdO, MoO 3 , S.O. 3 , Cl, F, SnO 2 , Sb 2 O 3 and the like, which may be metal ions or oxides. Other components may be contained, for example, in a total amount of 3.0% or less for various purposes (e.g., clarification, coloring, chemical durability, etc.). If the total content of other components is 3.0% or less, the necessary properties for vehicle glass and cover glass for sensors such as LiDAR can be maintained. The total content of other components is preferably 2.5% or less, more preferably 2.0% or less, even more preferably 1.5% or less, particularly preferably 1.0% or less, and most preferably 0.50% or less.
[0066] In addition, to prevent environmental impact, 2 O 3 The content of each of PbO is preferably less than 0.0010%, and more preferably substantially none is contained.
[0067] In the glass of this embodiment, if NiO is contained, NiS may be generated, which may cause glass breakage, so the NiO content is preferably 0.0080% or less, more preferably 0.0040% or less, even more preferably 0.0020% or less, and particularly preferably substantially zero.
[0068] The glass of this embodiment contains CeO 2 It may contain CeO 2 Since CeO absorbs light in the ultraviolet region, it reduces the ultraviolet transmittance Tuv and improves UV blocking performance. It also acts as an oxidizing agent and can control Fe-Redox. 2 When CeO is contained, its content is preferably 0.010% or more, more preferably 0.020% or more, further preferably 0.040% or more, and particularly preferably 0.070% or more. 2 may absorb ultraviolet light, causing solarization and reducing transmittance in the visible range. 2 The content is preferably 0.25% or less, more preferably 0.18% or less, further preferably 0.14% or less, particularly preferably 0.10% or less.
[0069] The glass of this embodiment is Cr 2 O 3 Cr 2 O 3 acts as an oxidizing agent and can control Fe-Redox. 2 O 3 When Cr is contained, its content is preferably 0.0020% or more, and more preferably 0.0040% or more. 2 O 3 Since Fe has coloration in the visible range, there is a risk of a decrease in visible light transmittance. 2+Therefore, the glass of the present embodiment is preferably made of Cr. 2 O 3 When it is contained, the content is preferably 0.020% or less, more preferably 0.016% or less, further preferably 0.012% or less, and particularly preferably 0.0080% or less.
[0070] The glass of this embodiment is SnO 2 It may contain SnO 2 acts as a reducing agent to control Fe-Redox. It also acts as a fining agent. 2 When SnO is contained, its content is preferably 0.010% or more, more preferably 0.040% or more, further preferably 0.060% or more, and particularly preferably 0.080% or more. 2 In order to suppress defects caused by SnO in the glass of this embodiment, 2 The content of is preferably 0.40% or less, more preferably 0.30% or less, further preferably 0.20% or less, particularly preferably 0.15% or less.
[0071] The glass of this embodiment is SO 3 SO 3 acts as a fining agent to improve the bubble quality of the glass. 3 When SO is contained, its content is preferably 0.0010% or more, more preferably 0.0040% or more, further preferably 0.0070% or more, and particularly preferably 0.015% or more. 3 If the Fe-Redox is high, amber coloring occurs, turning the glass brown, and there is a risk of a decrease in visible light transmittance. 3 When it is contained, the content is preferably 0.070% or less, more preferably 0.060% or less, further preferably 0.050% or less, and particularly preferably 0.040% or less.
[0072] The glass of this embodiment may contain Cl. Cl acts as a fining agent and improves the bubble quality of the glass. When the glass of this embodiment contains Cl, the Cl content is preferably 0.080% or more, more preferably 0.15% or more, even more preferably 0.20% or more, particularly preferably 0.25% or more, and most preferably 0.30% or more. If the Cl content is high, Cl volatilized from the glass melt may be easily dissolved. 2 The gas may corrode surrounding members. When the glass of the present embodiment contains Cl, the Cl content is preferably 1.0% or less, more preferably 0.80% or less, even more preferably 0.60% or less, and particularly preferably 0.50% or less.
[0073] [Characteristics] (Fracture toughness value K IC The glass of this embodiment has a fracture toughness value K measured by the SEPB method. IC is 0.76 MPa m 1/2 The fracture toughness value K is preferably equal to or greater than the above. IC is an index of glass strength, and the fracture toughness value K IC The larger the fracture toughness value K, the more difficult it is for cracks to progress and the higher the resistance to cracking. IC is 0.76 MPa m 1/2 If the fracture toughness value K is 1.0 or more, sufficient resistance to cracking can be obtained, making the glass suitable for use as a cover glass for vehicles or sensors. IC is 0.78 MPa m 1/2 More preferably, 0.80 MPa m 1/2 More preferably, 0.82 MPa m 1/2 More preferably, 0.84 MPa m 1/2 More preferably, 0.86 MPa m 1/2 More than 0.88 MPa m is particularly preferred. 1/2 More preferably, 0.90 MPa m 1/2 The above is most preferable.
[0074] Fracture toughness value K ICis measured using a pre-crack introduction fracture test method (SEPB method: Single-Edge-Precracked-Beam method) based on JIS R1607:2015 "Fracture toughness test method for fine ceramics".
[0075] In order to set the fracture toughness value within the above range, SiO 2 Increase the content of RO, increase the proportion of alkaline earth metal components with small element numbers, 2 In particular, the proportion of alkali metal components with small atomic numbers in the O range can be increased. 2 Since R is a component that forms a network structure, increasing the content strengthens the glass structure, thereby improving the fracture toughness value. Furthermore, the smaller the atomic number of the alkaline earth metal component of RO, the higher the Young's modulus, and as a result, the more the fracture toughness value can be improved. 2 Regarding O, the smaller the atomic number of the alkali metal component, the more the tendency similar to that of RO is shown.
[0076] Fracture toughness value K IC (MPa m 1/2 ) is Young's modulus E (GPa), surface fracture energy γ (J / m 2 ) and Poisson's ratio ν (unitless) using the following formula:
[0077]
[0078] As shown in the above formula, the fracture toughness value K IC The value of γ increases as the Young's modulus E and the surface fracture energy γ increase.
[0079] (Young's modulus) The Young's modulus of the glass of this embodiment is preferably 75 GPa or more. With a Young's modulus of 75 GPa or more, the glass has high rigidity and an improved fracture toughness value, making it more suitable as a window glass for a vehicle or a cover glass for a sensor such as LiDAR. The Young's modulus of the glass of this embodiment is more preferably 76 GPa or more, even more preferably 77 GPa or more, particularly preferably 78 GPa or more, and most preferably 79 GPa or more.
[0080] Furthermore, from the viewpoint of suppressing deformation and cracking when the glass is subjected to an external force, the Young's modulus is preferably 87 GPa or less, more preferably 86 GPa or less, even more preferably 85 GPa or less, and particularly preferably 84 GPa or less.
[0081] In order to set the Young's modulus within the above range, R 2 By adjusting the type and amount of O, MgO and Li 2 Increase the O content, 2 O 3 , TiO 2 , ZrO 2 The Young's modulus can be measured by an ultrasonic pulse method based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0082] (Surface fracture energy) The surface fracture energy of the glass of this embodiment is 3.6 J / m 2 The larger the surface fracture energy, the better the fracture toughness value, so it is preferable. The surface fracture energy is 3.7 J / m 2 More preferably, 3.8 J / m or more 2 More preferably, 3.9 J / m or more 2 More than 4.0 J / m is particularly preferred. 2 The above is most preferable.
[0083] The surface fracture energy can be determined by measuring the fracture toughness value, Young's modulus, and Poisson's ratio and calculating from the relational expression (1) above.
[0084] (Rigidity Modulus) The rigidity modulus of the glass of this embodiment is preferably 31 GPa or more. If the rigidity modulus is 31 GPa or more, the glass is less likely to deform when subjected to an external force. The rigidity modulus of the glass is more preferably 32 GPa or more, and even more preferably 33 GPa or more.
[0085] Furthermore, when the glass is subjected to an external force, deformation occurs, consuming energy and thereby suppressing cracking, so the modulus of rigidity is preferably 38 GPa or less, more preferably 37 GPa or less, even more preferably 36 GPa or less, and particularly preferably 35 GPa or less. The modulus of rigidity can be measured by an ultrasonic pulse method based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0086] (Poisson's ratio) The Poisson's ratio of the glass of this embodiment is preferably 0.26 or less. If the Poisson's ratio is 0.26 or less, the stress generated when an external force is applied to the glass can be reduced. Furthermore, the fracture toughness value can be improved. The Poisson's ratio is more preferably 0.25 or less, even more preferably 0.24 or less, and particularly preferably 0.23 or less.
[0087] The Poisson's ratio can be measured by an ultrasonic pulse method based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0088] (T 2 In the glass of this embodiment, the glass viscosity η, which is a criterion for the meltability of glass, is 10 2 [dPa s] Temperature T 2 It is preferable that T is 1650°C or less. 2 By keeping the temperature at 1650°C or less, the consumption of fuel used in melting the glass raw materials can be reduced, and the life of the brick members used in the melting furnace can be extended.
[0089] T 2 As a method for making the temperature 1650°C or less, for example, the R 2 The content of O and RO was increased, and Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 The method for reducing the content of
[0090] T 2is more preferably 1600°C or less, further preferably 1575°C or less, even more preferably 1550°C or less, particularly preferably 1525°C or less, and most preferably 1500°C or less. From the viewpoint of maintaining the fracture toughness of the glass and preventing the average linear expansion coefficient of the glass from becoming too large, T 2 The heating temperature is preferably 1400°C or higher, more preferably 1425°C or higher, and even more preferably 1450°C or higher.
[0091] (T 4 In the glass of this embodiment, the glass viscosity η, which is the standard for formability during float forming, is 10 4 [dPa s] Temperature T 4 It is preferable that T is 1200°C or less. 4 Since the temperature is 1200°C or less, it is suitable for forming into a plate by the float method.
[0092] T 4 As a method for reducing the temperature to 1200°C or less, for example, 2 Increased O and RO content, Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 The method for reducing the content of
[0093] T 4 is more preferably 1175°C or less, even more preferably 1150°C or less, even more preferably 1125°C or less, particularly preferably 1100°C or less, and most preferably 1075°C or less. From the viewpoint of maintaining the fracture toughness of the glass and preventing the average linear expansion coefficient of the glass from becoming too large, T 4 The heating temperature is preferably 950°C or higher, more preferably 975°C or higher, even more preferably 1000°C or higher, and particularly preferably 1025°C or higher.
[0094] (T 11 In the glass of this embodiment, the glass viscosity η, which is the standard for bending workability, is 10 11 [dPa s] Temperature T 11 It is preferable that T is 640°C or less. 11By keeping the temperature at 640°C or less, bending forming can be performed at a low temperature.
[0095] T 11 As a method for making the temperature to 640°C or less, for example, 2 Increased O and RO content, Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 The method for reducing the content of
[0096] In the glass of this embodiment, T 11 The temperature is more preferably 635°C or lower, even more preferably 630°C or lower, even more preferably 625°C or lower, particularly preferably 620°C or lower, particularly preferably 615°C or lower, and most preferably 610°C or lower.
[0097] In addition, from the viewpoint of maintaining the fracture toughness of the glass, preventing the average linear expansion coefficient of the glass from becoming too large, and the firing temperature of the black ceramic printed on the windshield, T 11 The temperature is preferably 570°C or higher, more preferably 575°C or higher, even more preferably 580°C or higher, particularly preferably 585°C or higher, and most preferably 590°C or higher.
[0098] (T 12 In the glass of this embodiment, the glass viscosity η, which is the standard for bending workability, is 10 12 [dPa s] Temperature T 12 It is preferable that T is 610°C or less. 12 By keeping the temperature at 610°C or less, bending forming can be performed at a low temperature.
[0099] T 12 As a method for reducing the temperature to 610°C or less, for example, the R 2 Increased O and RO content, Al 2 O 3 A method for reducing the content of R 2 Among O, Li 2 Method for incorporating O, SiO 2 The method for reducing the content of
[0100] T 12 is more preferably 605°C or less, even more preferably 600°C or less, even more preferably 595°C or less, particularly preferably 590°C or less, particularly preferably 585°C or less, and most preferably 580°C or less. From the viewpoint of maintaining the fracture toughness of the glass, preventing the average linear expansion coefficient of the glass from becoming too large, and from the viewpoint of the firing temperature of the black ceramic printed on the windshield, T 12 The temperature is preferably 540°C or higher, more preferably 545°C or higher, even more preferably 550°C or higher, particularly preferably 555°C or higher, and most preferably 560°C or higher.
[0101] (Density) The density of the glass of this embodiment is 2.68 g / cm 3 It is preferable that the density is 2.68 g / cm or less. 3 By satisfying the condition of 0.1 to 1.0%, it is possible to improve Young's modulus, fracture toughness, sound insulation, etc., while suppressing increases in fuel consumption and electricity consumption due to weight increase. Generally, glass having a high Young's modulus and fracture toughness has a high density and tends to require a high bending temperature. 2 By adjusting the composition and contents of O and RO, it is possible to achieve a low density, a high Young's modulus and fracture toughness, and excellent bending formability.
[0102] The density of the glass of this embodiment is 2.66 g / cm 3 More preferably, 2.60 g / cm or less 3 More preferably, 2.55 g / cm 3 Even more preferably, 2.53 g / cm 3 The following is particularly preferred: 3 The following is particularly preferred: 2.49 g / cm 3 The following are most preferred:
[0103] Furthermore, from the viewpoint of improving sound insulation, the density of the glass of this embodiment is 2.40 g / cm 3 More than 2.42 g / cm 3 More preferably, 2.43 g / cm 3 More than 2.44 g / cm is particularly preferred. 3The above is most preferable.
[0104] (T g ) the glass transition temperature (T g ) is preferably in the range of 460°C or higher and lower than 600°C. g If the temperature is within this predetermined range, the glass can be bent within the range of normal manufacturing conditions. g By ensuring that the temperature is 460°C or higher, the alkali metal content or alkaline earth metal content does not become too large, and the average linear expansion coefficient of the glass can be prevented from increasing. In addition, moisture resistance and devitrification of the glass are suppressed, and formability is improved. g The heating temperature is more preferably 480°C or higher, even more preferably 490°C or higher, and particularly preferably 500°C or higher.
[0105] In addition, from the viewpoint of preventing the bending temperature of the glass from becoming excessive and facilitating production, T g is preferably less than 600°C, more preferably 590°C or less, even more preferably 585°C or less, even more preferably 580°C or less, particularly preferably 575°C or less, and most preferably 570°C or less.
[0106] (Sag Point) The sag point of the glass of the present embodiment is preferably 670°C or lower. When the sag point is within the above range, excellent bending formability can be obtained. The sag point of the glass is more preferably 660°C or lower, further preferably 650°C or lower, particularly preferably 640°C or lower, and most preferably 630°C or lower.
[0107] The yield point is preferably 580°C or higher. If the yield point is 580°C or higher, the bending temperature can be prevented from becoming too low, and the black ceramic printed on the windshield can be fired simultaneously with bending. The yield point is more preferably 585°C or higher, even more preferably 590°C or higher, particularly preferably 595°C or higher, and most preferably 600°C or higher. The yield point can be measured using a differential thermal dilatometer (TMA).
[0108] (Average coefficient of linear expansion) The average coefficient of linear expansion (CTE) of the glass of this embodiment at 50 to 350°C is 100 × 10 -7 / °C or less. The average linear expansion coefficient is preferably 100 x 10 -7 / °C or less, cracking due to heat shock can be suppressed when the glass of this embodiment is used as glass for vehicles or sensors. Furthermore, when the glass of this embodiment is made into bent glass, the difference in thermal expansion due to differences in in-plane thermal history can be suppressed, and bent glass with good dimensional and surface accuracy can be obtained.
[0109] The average linear expansion coefficient of the glass of this embodiment at 50 to 350°C is 100 x 10 -7 / °C or less, and 95 x 10 -7 / °C or less is more preferable, and 92 × 10 -7 / °C or less is more preferable, and 90 x 10 -7 / °C or less is particularly preferred.
[0110] In addition, the glass of this embodiment has an average linear expansion coefficient of 70×10 from the viewpoint of suppressing cracking of the black ceramic due to the difference in thermal expansion with the black ceramic printed on the windshield. -7 / °C or more. -7 / °C or more, the difference in thermal expansion with the black ceramic is small, and cracking of the black ceramic can be suppressed. -7 / °C or more is more preferable, and 74 x 10 -7 / °C or more is more preferable, and 76 x 10 -7 / °C or more is particularly preferred, and 78 x 10 -7 / °C or more is particularly preferred, and 80 x 10 -7 / °C or more is particularly preferred, and 82 x 10 -7 / °C or more is most preferred.
[0111] In order to set the average linear expansion coefficient within the above range, the SiO 2 Increase the content of R 2 O, RO and Al 2 O 3 The method for adjusting the content of
[0112] (Solar transmittance: Te) When the glass of this embodiment is used for vehicle glass, the solar transmittance Te of the glass of this embodiment, when converted to a thickness of 2.00 mm, according to ISO-9050:2003 is preferably 90% or less. If Te is 90% or less, excellent heat shielding properties can be obtained. Te is more preferably 88% or less, even more preferably 86% or less, even more preferably 84% or less, particularly preferably 82% or less, and most preferably 80% or less. There is no particular restriction on the lower limit of Te, but it is usually 30% or more, preferably 32% or more, more preferably 34% or more, and particularly preferably 36% or more. To make Te fall within the above range, Fe 2 O 3 This can be achieved by adjusting the content to 0.030% or more.
[0113] (Visible Light Transmittance: Tv) When the glass of this embodiment is used for vehicle glass, the glass of this embodiment preferably has a visible light transmittance Tv of 75% or more, calculated by measuring the transmittance with a spectrophotometer using a D65 light source in accordance with the specifications of ISO-9050:2003 when converted to a thickness of 2.00 mm. A Tv of 75% or more provides excellent transparency, making the glass more suitable for vehicle glass, particularly windshields and door glass. Tv is more preferably 78% or more, even more preferably 80% or more, and even more preferably 82% or more. 84% or more is particularly preferred, and 86% or more is most preferred. The upper limit of Tv is not particularly limited, but is, for example, 92% or less.
[0114] In order to set Tv within the above range, the glass composition, particularly SiO 2 and Fe 2 O 3 This can be achieved by adjusting the content of
[0115] (Ultraviolet Transmittance: Tuv) When the glass of this embodiment is used for vehicle glass, it is preferable that the glass of this embodiment has low ultraviolet transmittance, and when converted to a thickness of 2.00 mm, the ultraviolet transmittance Tuv defined in ISO-9050:2003 is preferably 70% or less. A Tuv of 70% or less can suppress deterioration of components such as interlayers and seats inside the vehicle cabin when the glass of this embodiment is used for laminated glass. Tuv is more preferably 68% or less, even more preferably 66% or less, even more preferably 64% or less, particularly preferably 62% or less, and most preferably 60% or less. The lower limit of Tuv is, for example, 10% or more.
[0116] To set Tuv within the above range, the glass composition, particularly SiO 2 and Fe 2 O 3 , TiO 2 and CeO 2 Alternatively, this can be achieved by adjusting Fe-Redox.
[0117] When the glass of this embodiment is used as a cover glass for LiDAR, it is preferable that the glass of this embodiment has high transmittance at wavelengths of 905 nm or 1550 nm, which are used in LiDAR. Therefore, the transmittance of the glass of this embodiment at a wavelength of 905 nm or 1550 nm when converted to a thickness of 4.0 mm is preferably 86% or more, more preferably 87% or more, even more preferably 88% or more, even more preferably 89% or more, particularly preferably 90% or more, and most preferably 91% or more.
[0118] The shape of the glass of this embodiment is not particularly limited. When the glass of this embodiment is used for a vehicle glass, the area of the main surface is 0.25 m 2 More than 0.45m is preferable. 2 More preferably, 0.90 m or more 2 The above is even more preferable. When the area of the glass is within the above range, it can be adapted to various vehicle models. Furthermore, if the area of the glass is too large, it becomes difficult to handle, the temperature distribution during heating becomes uneven, the dimensional accuracy after bending becomes poor, and so on, making bending more difficult. Therefore, the glass of this embodiment is designed so that the area of the main surface is within 10 m 2Preferably less than 7m 2 Less than 5m is more preferable. 2 The following is even more preferred:
[0119] When the glass of this embodiment is used as a cover glass for a sensor, the shape of the glass of this embodiment is not particularly limited, but the area of the main surface is preferably 0.00010 m 2 More than 0.010 m is preferable. 2 More preferably, 0.020 m or more 2 More preferably, 0.040 m or more 2 More than 0.090 m is particularly preferable. 2 The above is most preferable. When the glass area is within the above range, it can be used as a cover glass for various LiDARs. Furthermore, if the glass area is too large, the temperature distribution during heating becomes uneven, the dimensional accuracy after bending becomes poor, and so on, making bending more difficult. Therefore, the glass of this embodiment has a main surface area of 1.0 m 2 Preferably less than 0.90 m 2 Less than 0.80 m is more preferable. 2 The following is even more preferred:
[0120] Furthermore, the glass of this embodiment preferably has a surface roughness Ra of 5.0 nm or less, a thickness of 2.5 mm, a tip curvature radius of 200 μm, an apex angle of 120°, and a critical impact fracture speed of 35 km / h or more when impacted with a tungsten carbide cemented carbide having a weight of 1.365 g. A critical impact fracture speed of 35 km / h or more can improve resistance to flying stones. The critical impact fracture speed is more preferably 36 km / h or more, even more preferably 37 km / h or more, even more preferably 38 km / h or more, even more preferably 39 km / h or more, particularly preferably 40 km / h or more, and most preferably 42 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less. The surface roughness Ra can be measured according to JIS B0601:2001.
[0121] Furthermore, the glass of the embodiment preferably has a critical impact fracture speed of 53 km / h or more when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass. A critical impact fracture speed of 53 km / h or more can improve resistance to flying stones. The critical impact fracture speed is more preferably 54 km / h or more, even more preferably 55 km / h or more, and particularly preferably 56 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less. The critical impact fracture speed can be measured by the method described in the Examples below.
[0122] The thickness of the glass of this embodiment is preferably 2.5 mm or more. In particular, when the glass of this embodiment has the above-mentioned properties, the thickness of the glass is preferably 2.5 mm or more. A glass thickness of 2.5 mm or more can improve the critical impact fracture speed of glass with a high fracture toughness value. The thickness of the glass is more preferably 2.8 mm or more, even more preferably 2.9 mm or more, even more preferably 3.0 mm or more, particularly preferably 3.1 mm or more, even more preferably 3.2 mm or more, even more preferably 3.3 mm or more, particularly preferably 3.4 mm or more, and most preferably 3.5 mm or more.
[0123] Moreover, from the viewpoint of suppressing increases in fuel economy and electricity consumption due to an increase in the weight of the glass, the thickness of the glass of the present embodiment is preferably 6.0 mm or less, more preferably 5.5 mm or less, even more preferably 5.0 mm or less, particularly preferably 4.8 mm or less, and most preferably 4.5 mm or less.
[0124] Examples of methods for adjusting the thickness of the glass include a method of adjusting the thickness of the glass using the float method or down-draw method described below, and a method of polishing the glass in the thickness direction using a grinding stone and then polishing it to a mirror finish using an abrasive such as cerium oxide. The surface roughness Ra after molding or polishing is preferably 5.0 nm or less, more preferably 2.0 nm or less, even more preferably 1.5 nm or less, particularly preferably 1.0 nm or less, and most preferably 0.50 nm or less.
[0125] The glass of the present embodiment is preferably float glass formed by, for example, the well-known float method, in which a molten glass base is floated on a molten metal such as tin, and strict temperature control is used to form glass with uniform thickness and width, as well as large area glass.
[0126] The glass of the present embodiment may be glass formed by a known roll-out method or down-draw method, or may be glass with a polished surface and a uniform thickness. Here, the down-draw method is broadly divided into a slot down-draw method and an overflow down-draw method (fusion method), both of which are techniques for continuously letting molten glass flow down from a forming body to form a band-shaped glass ribbon.
[0127] The glass of this embodiment may be glass that has been subjected to tempering treatment such as air-cooling tempering or chemical tempering. By performing the above treatment, the strength of the glass can be increased.
[0128] Here, air-cooling tempering is a process in which a compressive stress layer is formed on the surface of glass by thermal tempering. Specifically, uniformly heated glass is rapidly cooled from a temperature near its softening point, and compressive stress is formed on the surface of the glass due to the temperature difference between the surface and the interior of the glass. The compressive stress is generated uniformly over the entire surface of the glass, and a compressive stress layer of uniform depth is formed over the entire surface of the glass. Thermal tempering is more suitable for tempering thick glass than chemical tempering.
[0129] Chemical strengthening is a process in which alkali metal ions with a small ionic radius (typically Li ions or Na ions) on the surface of glass are exchanged with alkali metal ions with a larger ionic radius (typically Na ions or K ions) by ion exchange at a temperature below the glass transition point, thereby forming a compressive stress layer on the surface of the glass. Chemical strengthening can be performed by known methods, such as ion exchange. In the ion exchange process, a glass plate is immersed in a treatment solution (e.g., potassium nitrate molten salt) and ions with a small ionic radius (e.g., Na ions) contained in the glass are exchanged with ions with a large ionic radius (e.g., K ions), thereby generating compressive stress on the surface of the glass.
[0130] The magnitude of the compressive stress on the surface of the glass (hereinafter also referred to as surface compressive stress CS) and the depth DOL of the compressive stress layer formed on the surface of the glass can be adjusted by the glass composition, the immersion time in the treatment liquid, and the temperature of the treatment liquid, respectively.
[0131] The glass of this embodiment may be in a flat plate shape, or may be bent glass formed into a curved shape by gravity forming, press forming, or the like.
[0132] When the glass of this embodiment is glass that curves with a predetermined curvature, it may be single-curve glass that curves in only one direction, either up and down or left and right, or double-curve glass that curves in both up and down and left and right directions.
[0133] When the glass of this embodiment is bent glass, the minimum value of the radius of curvature is preferably 500 mm or more and 100,000 mm or less. The radius of curvature of bent glass is calculated by performing a shape simulation on a sample using a laser displacement meter (Dyvoce manufactured by Kohzu Seiki Co., Ltd.) based on the amount of warp inherent to the sample determined by weight deflection correction in a double-sided differential mode, and the radius of curvature is determined from the shape obtained by the simulation.
[0134] The glass of this embodiment can be made into bent glass by heating and bending the glass. A more specific forming method includes a method in which flat glass is heated, placed on a forming mold, and pressed from above by a press means to bend the glass.
[0135] Another example is a method in which a flat glass sheet is placed on a mold having a bending surface corresponding to the desired curved surface, and the mold is then carried into a heating furnace in which the glass is heated to a temperature close to the glass softening point. According to this forming method, the glass is curved by its own weight along the bending surface of the mold as it softens, thereby producing bent glass having the desired curved surface.
[0136] In this embodiment, bending by the press means is preferred from the viewpoint of improving productivity and improving surface accuracy after forming. The bending method by the press means is not particularly limited, and for example, the method described in International Publication No. 2016 / 093031 can be appropriately adopted. Hereinafter, the bending method by the press means will be described as an example.
[0137] First, the glass of this embodiment is transported to a press area by a transport conveyor, etc. Then, in the press area, the glass is heated to a temperature at which it can be bent and softened.
[0138] Here, the temperature at which bending is possible is, for example, a temperature at which the glass viscosity is 10 12 [dPa s] Temperature T 12 The heating may be performed by a heater or the like in a heating furnace during the process of transporting the material to the pressing area on a transport conveyor or the like.
[0139] In addition, the heating temperature (≧T 12 The bending time under the condition of maintaining the above condition can be set to, for example, 1 second or more.
[0140] A lower press mold (female mold) and an upper press mold (male mold) are arranged at predetermined positions in the press area, and the upper surface shape of the female mold and the lower surface shape of the male mold correspond to the curved shape of the glass to be bent in the conveying direction and the perpendicular direction. The female mold can be raised and lowered between a standby position below the conveyor and a press position above it, and after the glass is transferred from the conveyor, the female mold, with the glass placed on it, is raised from a predetermined raised position to a press position above the conveyor, thereby press-forming the glass.
[0141] Next, the press-formed glass is transported to a cooling area by a transport shuttle, etc. In the cooling area, the glass is cooled by blowing cooled air onto it, etc.
[0142] The above steps allow the bent glass to be formed. Although the bending of the glass of this embodiment has been described above, the bending may also be carried out in the form of laminated glass, which will be described later.
[0143] [Laminated Glass] The laminated glass according to this embodiment includes a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, and the first glass plate is the glass according to this embodiment.
[0144] FIG. 3 is a diagram showing an example of a laminated glass 10 according to the present embodiment. The laminated glass 10 includes a first glass plate 11, a second glass plate 12, and an interlayer film 13 sandwiched between the first glass plate 11 and the second glass plate 12. The laminated glass 10 according to the present embodiment is not limited to the configuration shown in FIG. 3 and can be modified without departing from the spirit of the present invention. For example, the interlayer film 13 may be formed of a single layer as shown in FIG. 3 or may be formed of two or more layers. The laminated glass 10 according to the present embodiment may also include three or more glass plates, in which case an organic resin or the like may be interposed between adjacent glass plates. Hereinafter, the laminated glass 10 according to the present embodiment will be described as having only two glass plates, a first glass plate 11 and a second glass plate 12, sandwiching the interlayer film 13.
[0145] In the laminated glass of this embodiment, from the viewpoint of bend formability, the second glass sheet 12 is preferably the glass of this embodiment. When the first glass sheet 11 and the second glass sheet 12 are the glass of this embodiment, the first glass sheet 11 and the second glass sheet 12 may be glass sheets having the same composition or different compositions.
[0146] When the second glass plate 12 is not the glass of this embodiment, the type of the glass plate is not particularly limited, and any conventionally known glass plate used for vehicle window glass, etc., can be used. Specific examples include alkali aluminosilicate glass, alkali aluminoborosilicate glass, and soda-lime glass. These glass plates may or may not be colored to the extent that their transparency is not impaired.
[0147] In this embodiment, the second glass plate 12 is made of Al 2 O 3 Alkali aluminosilicate glass containing 1.0% or more of Al 2 O 3 Contains 1.0% or more of B 2O 3 By using the alkali aluminosilicate glass or alkali aluminoborosilicate glass for the second glass plate 12, chemical strengthening becomes possible as described below, and the strength can be increased.
[0148] The alkali aluminosilicate glass and alkali aluminoborosilicate glass are made of Al, from the viewpoint of improving weather resistance, moisture resistance, and chemical strengthening properties. 2 O 3 The content of Al is more preferably 5.0% or more, further preferably 8.0% or more, and particularly preferably 10% or more. 2 O 3 The content is preferably 18% or less, more preferably 15% or less.
[0149] The alkali aluminosilicate glass and alkali aluminoborosilicate glass are R 2 The content of O is preferably 10% or more, more preferably 12% or more, and even more preferably 13% or more. 2 The O content is preferably 22% or less, more preferably 20% or less, and even more preferably 18% or less.
[0150] The alkali aluminoborosilicate glass is made of B to increase its strength when it comes into contact with flying stones, car keys, etc. 2 O 3 The content of B is preferably 2.0% or more, more preferably 3.0% or more, and even more preferably 4.0% or more. In alkali aluminoborosilicate glass, from the viewpoint of improving chemical durability and weather resistance, B 2 O 3 The content is preferably 9.0% or less, more preferably 8.0% or less, and even more preferably 7.0% or less.
[0151] Specific examples of the alkali aluminosilicate glass include glasses having the following compositions, where each component is expressed as a mole percentage based on oxide: 61%≦SiO 2 ≦75% 1.0%≦Al2 O 3 ≦20% 0.0%≦MgO≦15% 0.0%≦CaO≦10% 0.0%≦SrO≦1.0% 0.0%≦BaO≦1.0% 0.0%≦Li 2 O≦15% 2.0%≦Na 2 O≦15% 0.0%≦K 2 O≦6.0% 0.0%≦ZrO 2 ≦4.0% 0.0%≦TiO 2 ≦1.0% 0.0%≦Y 2 O 3 ≦2.0% 10%≦R 2 O≦25% 0.0%≦RO≦20% (R 2 O is Li 2 O, Na 2 O and K 2 RO represents the total content of MgO, CaO, SrO, and BaO.
[0152] Specific examples of the alkali aluminoborosilicate glass include glasses having the following compositions, where each component is expressed as a mole percentage based on oxide: 61%≦SiO 2 ≦75% 1.0%≦Al 2 O 3 ≦20% 1.0%≦B 2 O 3 ≦10% 0.0%≦MgO≦15% 0.0%≦CaO≦10% 0.0%≦SrO≦1.0% 0.0%≦BaO≦1.0% 0.0%≦Li 2 O≦15% 2.0%≦Na 2 O≦15% 0.0%≦K 2 O≦6.0% 0.0%≦ZrO 2 ≦4.0% 0.0%≦TiO 2 ≦1.0% 0.0%≦Y 2 O 3 ≦2.0% 10%≦R 2 O≦25% 0.0%≦RO≦20% (R 2 O is Li 2 O, Na 2 O and K 2 RO represents the total content of MgO, CaO, SrO, and BaO.
[0153] In the laminated glass of this embodiment, the second glass sheet 12 may be soda lime glass. 2 O 3 Soda-lime glass containing 3.5% or less of SiO may also be used. Specifically, examples of glass having the following composition can be given. Each component is expressed in mole percentage based on oxide. 60%≦SiO 2 ≦75% 0.0%≦Al 2 O 3 ≦3.5% 2.0%≦MgO≦11% 2.0%≦CaO≦10% 0.0%≦SrO≦3.0% 0.0%≦BaO≦3.0% 10%≦Na 2 O≦18% 0.0%≦K 2 O≦8.0% 0.0%≦ZrO 2 ≦4.0% 0.0010%≦Fe 2 O 3 ≦5.0%
[0154] The thickness of the first glass plate 11 is preferably 2.5 mm or more. By making the thickness of the first glass plate 11 2.5 mm or more, the critical impact fracture speed of glass having a high fracture toughness value can be improved. The thickness of the first glass plate 11 is more preferably 2.8 mm or more, even more preferably 2.9 mm or more, even more preferably 3.0 mm or more, particularly preferably 3.1 mm or more, even more preferably 3.2 mm or more, even more preferably 3.3 mm or more, particularly preferably 3.4 mm or more, and most preferably 3.5 mm or more.
[0155] Furthermore, from the viewpoint of suppressing increases in fuel consumption and electricity consumption due to an increase in the weight of the glass, the thickness of the first glass plate 11 is preferably 6.0 mm or less, more preferably 5.5 mm or less, even more preferably 5.0 mm or less, particularly preferably 4.8 mm or less, and most preferably 4.5 mm or less.
[0156] The thickness of the second glass plate 12 is preferably 0.50 mm or more, more preferably 0.60 mm or more, even more preferably 0.70 mm or more, particularly preferably 0.80 mm or more, particularly preferably 0.90 mm or more, and most preferably 1.0 mm or more. A thickness of 0.50 mm or more is preferable from the viewpoint of impact resistance.
[0157] The thickness of the second glass sheet 12 is preferably 2.0 mm or less, more preferably 1.9 mm or less, even more preferably 1.8 mm or less, particularly preferably 1.7 mm or less, particularly preferably 1.6 mm or less, and most preferably 1.5 mm or less. A thickness of 2.0 mm or less for the second glass sheet 12 prevents the weight of the laminated glass 10 from becoming too large, which is preferable in terms of improving fuel efficiency when used in a vehicle.
[0158] The first glass plate 11 and the second glass plate 12 may have the same thickness or different thicknesses, but it is preferable that the first glass plate 11 be thicker than the second glass plate 12. Examples of methods for adjusting the thickness of the first glass plate 11 and the second glass plate 12 include a method of adjusting the glass thickness using a float method or a down-draw method, and a method of polishing the glass in the thickness direction using a grinding stone and then polishing it to a mirror finish using an abrasive such as cerium oxide. The surface roughness Ra after molding or polishing is preferably 5.0 nm or less, more preferably 2.0 nm or less, even more preferably 1.5 nm or less, particularly preferably 1.0 nm or less, and most preferably 0.50 nm or less.
[0159] In the laminated glass 10 of this embodiment, the thickness of the first glass sheet 11 and the second glass sheet 12 may be constant over the entire surface, or may vary from location to location as needed, such as forming a wedge shape in which the thickness of one or both of the first glass sheet 11 and the second glass sheet 12 gradually decreases.
[0160] At least one of the first glass plate 11 and the second glass plate 12 may be chemically strengthened glass that has been tempered to improve its strength. The chemical strengthening method is the same as the chemical strengthening method for glass described above. Examples of chemically strengthened glass include the alkali aluminosilicate glass and the alkali aluminoborosilicate glass that have been chemically strengthened.
[0161] The first glass sheet 11 and the second glass sheet 12 may have a flat shape or a curved shape having a curvature entirely or partially. If the first glass sheet 11 and the second glass sheet 12 are curved, they may have a single-curve shape, i.e., a curved shape in only one of the vertical or horizontal directions, or a complex-curve shape, i.e., a curved shape in both the vertical and horizontal directions. If the first glass sheet 11 and the second glass sheet 12 are curved, the radius of curvature in the vertical and horizontal directions may be the same or different. If the first glass sheet 11 and the second glass sheet 12 are curved, the radius of curvature in the vertical and / or horizontal directions is preferably 1000 mm or more. The shapes of the main surfaces of the first glass sheet 11 and the second glass sheet 12 are adapted to fit the window opening of the vehicle in which they are installed.
[0162] The interlayer film 13 is sandwiched between the first glass sheet 11 and the second glass sheet 12. By including the interlayer film 13, the laminated glass 10 of this embodiment can firmly bond the first glass sheet 11 and the second glass sheet 12 together and can also absorb the impact force when flying fragments collide with the glass sheets.
[0163] Various organic resins that are commonly used in laminated glass for conventional vehicles can be used as the interlayer film 13. Examples of organic resins include polyethylene (PE), ethylene vinyl acetate copolymer (EVA), polypropylene (PP), polystyrene (PS), methacrylic resin (PMA), polyvinyl chloride (PVC), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), cellulose acetate (CA), diallyl phthalate resin (DAP), urea resin (UP), melamine resin (MF), unsaturated polyester (UP), polyvinyl butyral (PVB), and polyvinyl hol. Examples of materials that can be used include marl (PVF), polyvinyl alcohol (PVAL), vinyl acetate resin (PVAc), ionomer (IO), polymethylpentene (TPX), vinylidene chloride (PVDC), polysulfone (PSF), polyvinylidene fluoride (PVDF), methacrylic-styrene copolymer resin (MS), polyarate (PAR), polyallylsulfone (PASF), polybutadiene (BR), polyethersulfone (PESF), and polyetheretherketone (PEEK). Among these, EVA and PVB are preferred from the viewpoints of transparency and adhesion, and PVB is particularly preferred because it can impart sound insulation properties.
[0164] From the viewpoints of impact force absorption and sound insulation, the thickness of the interlayer film 13 is preferably 0.300 mm or more, more preferably 0.500 mm or more, and even more preferably 0.700 mm or more. From the viewpoint of suppressing a decrease in visible light transmittance, the thickness of the interlayer film 13 is preferably 1.00 mm or less, more preferably 0.900 mm or less, and even more preferably 0.800 mm or less. The thickness of the interlayer film 13 is preferably in the range of 0.300 mm to 1.00 mm, and more preferably in the range of 0.700 mm to 0.800 mm.
[0165] The thickness of the intermediate film 13 may be constant over the entire surface, or may vary from place to place as required.
[0166] If the difference in linear expansion coefficient between the interlayer film 13 and the first glass sheet 11 or the second glass sheet 12 is large, cracks or warping may occur in the laminated glass 10 when the laminated glass 10 is produced through the heating step described below, which may result in poor appearance. Therefore, it is preferable that the difference in linear expansion coefficient between the interlayer film 13 and the first glass sheet 11 or the second glass sheet 12 is as small as possible. The difference in linear expansion coefficient between the interlayer film 13 and the first glass sheet 11 or the second glass sheet 12 may be expressed as the difference between the average linear expansion coefficients within a predetermined temperature range.
[0167] In particular, since the resin constituting the interlayer film 13 has a low glass transition point, a predetermined difference in the average linear expansion coefficient may be set within a temperature range equal to or lower than the glass transition point of the resin material. The difference in the linear expansion coefficient between the first glass sheet 11 or the second glass sheet 12 and the resin material may be set at a predetermined temperature equal to or lower than the glass transition point of the resin material.
[0168] Alternatively, an adhesive layer containing an adhesive may be used for interlayer film 13. The adhesive is not particularly limited, but examples thereof include an acrylic adhesive, a silicone adhesive, etc. When interlayer film 13 is an adhesive layer, a heating step is not required in the process of joining first glass plate 11 and second glass plate 12, and therefore the risk of the above-mentioned cracking or warping occurring is reduced.
[0169] [Other Layers] The laminated glass 10 of the present embodiment may include layers (hereinafter also referred to as "other layers") other than the first glass sheet 11, the second glass sheet 12, and the interlayer film 13, provided that the effects of the present invention are not impaired. For example, the laminated glass 10 may include a coating layer that imparts water-repellent properties, hydrophilic properties, anti-fogging properties, or the like, an infrared reflective film, or the like.
[0170] The positions at which the other layers are provided are not particularly limited, and the other layers may be provided on the surface of the laminated glass 10, or may be sandwiched between the first glass sheet 11, the second glass sheet 12, or the interlayer film 13. The laminated glass 10 of this embodiment may also include a black ceramic layer or the like arranged in a strip shape along part or all of the peripheral edge for the purpose of concealing the attachment portion to the frame or the wiring conductors.
[0171] In the laminated glass 10 of this embodiment, the first glass sheet 11 has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm. When a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the surface of the first glass sheet 11, the critical impact fracture speed is preferably 35 km / h or more. A critical impact fracture speed of 35 km / h or more can improve resistance to flying stones. The critical impact fracture speed is more preferably 36 km / h or more, even more preferably 37 km / h or more, even more preferably 38 km / h or more, even more preferably 39 km / h or more, particularly preferably 40 km / h or more, and most preferably 42 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less.
[0172] Furthermore, the laminated glass of this embodiment preferably has a critical impact fracture speed of 35 km / h or more when a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is struck against the surface of the first glass sheet 11. A critical impact fracture speed of 35 km / h or more can further improve resistance to flying stones. The critical impact fracture speed is more preferably 37 km / h or more, even more preferably 40 km / h or more, even more preferably 45 km / h or more, even more preferably 50 km / h or more, particularly preferably 55 km / h or more, and most preferably 60 km / h or more. The upper limit of the critical impact fracture speed is, for example, 120 km / h or less.
[0173] The total thickness of the first glass plate 11, the second glass plate 12, and the interlayer film 13 is preferably 4.5 mm or more. In particular, when the laminated glass of this embodiment has the above-mentioned properties, the total thickness of the first glass plate 11, the second glass plate 12, and the interlayer film 13 is preferably 4.5 mm or more. A total thickness of 4.5 mm or more can improve sound insulation. The total thickness is more preferably 4.6 mm or more, even more preferably 4.7 mm or more, even more preferably 4.8 mm or more, particularly preferably 4.9 mm or more, and most preferably 5.0 mm or more. Furthermore, from the viewpoint of weight reduction, the total thickness is preferably 8.0 mm or less, more preferably 7.8 mm or less, even more preferably 7.6 mm or less, particularly preferably 7.4 mm or less, particularly preferably 7.2 mm or less, and most preferably 7.0 mm or less.
[0174] When the total thickness of the first glass plate 11, the second glass plate 12, and the interlayer film 13 varies depending on the location, it is preferable that the total thickness at the thinnest location be 4.5 mm or more.
[0175] In addition, the laminated glass of this embodiment has a thickness t 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2 It is preferable that the ratio (t 1 / t 2 When the ratio (t) is 1.5 or more, a high critical impact destruction speed can be achieved. 1 / t 2 ) is more preferably 2.0 or more, even more preferably 2.5 or more, even more preferably 3.0 or more, particularly preferably 3.5 or more, and most preferably 4.0 or more. In addition, in order to approximate the curvature when the glass after bending is made into laminated glass, the ratio (t 1 / t 2 ) is preferably 6.0 or less, more preferably 5.5 or less, and even more preferably 5.0 or less.
[0176] The laminated glass 10 of this embodiment preferably has a visible light transmittance Tv as defined in ISO-9050:2003 using a D65 light source of 70% or more, more preferably 71% or more, and even more preferably 72% or more. Furthermore, Tv is, for example, 90% or less.
[0177] The total solar transmittance (Tts) of the laminated glass 10 of this embodiment, as defined in ISO-13837:2008 Convention A and measured at a wind speed of 4 m / s, is preferably 70% or less. When the total solar transmittance (Tts) of the laminated glass 10 of this embodiment is 70% or less, sufficient heat-shielding properties are obtained. Tts is more preferably 68% or less, and even more preferably 66% or less. Furthermore, Tts is, for example, 55% or more.
[0178] The laminated glass 10 of this embodiment can be manufactured by a method similar to that of conventionally known laminated glass. For example, by laminating a first glass sheet 11, an interlayer film 13, and a second glass sheet 12 in this order and then subjecting them to a heating and pressurizing process, a laminated glass 10 is obtained in which the first glass sheet 11 and the second glass sheet 12 are bonded together via the interlayer film 13.
[0179] The method for manufacturing the laminated glass 10 of this embodiment may, for example, include a step of heating and shaping the first glass sheet 11 and the second glass sheet 12, followed by a step of inserting the interlayer film 13 between the first glass sheet 11 and the second glass sheet 12 and applying heat and pressure. By performing these steps, the laminated glass 10 may be configured such that the first glass sheet 11 and the second glass sheet 12 are joined together via the interlayer film 13.
[0180] [Uses] The glass of the present embodiment has excellent fracture toughness and bend formability, and therefore can be suitably used as glass to be installed in vehicles or sensors, and more specifically, as vehicle window glass or sensor cover glass. In particular, the glass of the present embodiment has excellent fracture toughness and bend formability, and therefore is suitable for vehicle window glass, specifically, components such as windshields, side glass, rear glass, and roof glass. From the same viewpoint, the glass can be suitably used as cover glass for sensors such as LiDAR, cameras, and millimeter-wave radar mounted on vehicles and unmanned or manned eVTOLs (Electric Vertical Take-Off and Landing aircraft) such as drones.
[0181] Hereinafter, as a specific application, an example in which the glass of this embodiment is used as a window glass for a vehicle will be described with reference to the drawings.
[0182] 4 is a conceptual diagram showing a state in which a laminated glass 10 including the glass of this embodiment is attached to an opening 110 formed in the front of an automobile 100 and used as a window glass of the automobile. The laminated glass 10 used as a window glass of an automobile may have a housing (case) 120, which houses an information device or the like, attached to its surface on the interior side of the vehicle to ensure the traveling safety of the vehicle.
[0183] The information device housed in the housing is a device that uses a camera, radar, etc. to prevent rear-end collisions with vehicles ahead, pedestrians, obstacles, etc., and to alert the driver to danger. For example, it is an information receiving device and / or information transmitting device, etc., and includes millimeter-wave radar, stereo cameras, infrared lasers, etc., which send and receive signals. The "signal" refers to electromagnetic waves including millimeter waves, visible light, infrared light, etc.
[0184] 5 is an enlarged view of the portion S in FIG. 4 and is a perspective view showing the portion of the laminated glass 10 of this embodiment where the housing 120 is attached. The housing 120 houses a millimeter-wave radar 201 and a stereo camera 202 as information devices. The housing 120 housing the information devices is usually attached on the outer side of the vehicle relative to the rearview mirror 150 and on the inner side of the vehicle relative to the laminated glass 10, but may also be attached to other portions.
[0185] 6 is a cross-sectional view taken along line Y-Y in FIG. 5 and perpendicular to the horizontal line. It is preferable that the first glass sheet 11 of the laminated glass 10 be disposed on the exterior side of the vehicle. This configuration allows for a lightweight windshield with excellent fracture toughness. Furthermore, the glass of this embodiment has low viscosity, making it easy to bend when manufacturing the windshield.
[0186] As described above, the present specification discloses the following configurations: <1> Indicated in mole percent on an oxide basis, SiO 2 : 60 to 72% Al 2 O 3 :3.0~9.0%B 2 O 3 :0.0~4.0% MgO:3.0~15% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~2.0% Li 2 O: 1.0-10% Na 2 O: 6.0-16% K 2 O: 0.0 to 3.0% ZrO 2 :0.0~1.0% TiO 2 :0.0~1.0% Y 2 O 3 :0.0~1.0% R 2 O: 11 to 25% RO: 7.0 to 20% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2<2> The glass according to <1>, having a Young's modulus of 75 GPa or more. <3> The glass according to <1>, having a fracture toughness value K measured by the SEPB method. IC is 0.76 MPa m 1/2 <4> The glass according to any one of <1> to <3>, having a deformation point of 670°C or less. <5> The glass according to any one of <1> to <4>, having a ratio (H / L) of the H value to the L value calculated by the following formula of 0.10 or less: H=[K 2 O] + [CaO] + [SrO] + [BaO] + [ZrO 2 ]+[TiO 2 ]+[Y 2 O 3 ] L = [SiO 2 ]+[Al 2 O 3 ]+[MgO]+[Li 2 O] + [Na 2 O] (where [ ] means the content of each component in the brackets expressed in mole percent on an oxide basis.) <6> Fracture toughness value K measured by SEPB method IC is 0.80 MPa m 1/2The glass according to <5>, wherein the critical impact fracture speed is 35 km / h or more when a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm. <8> The glass according to any one of <1> to <6>, wherein the critical impact fracture speed is 53 km / h or more when a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm. <9> The glass according to any one of <1> to <8>, wherein the critical impact fracture speed is 2.5 mm or more when a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the glass when the surface roughness Ra is 5.0 nm or less and the thickness is 2.5 mm. <10> A window glass for a vehicle, comprising the glass according to any one of <1> to <9>. <11> A glass for a sensor, comprising the glass according to any one of <1> to <9>. <12> Laminated glass comprising a first glass plate, a second glass plate, and an interlayer film sandwiched between the first and second glass plates, wherein the first glass plate is the glass according to any one of <1> to <9>. <13> The laminated glass according to <12>, wherein the first glass plate has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm, and wherein a critical impact fracture speed when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the surface of the first glass plate is 35 km / h or more. <14> The laminated glass according to <12>, wherein a critical impact fracture speed when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120°, and a weight of 1.365 g is collided with the surface of the first glass plate is 53 km / h or more. <15> The laminated glass according to any one of <12> to <14>, wherein the total thickness of the first glass sheet, the second glass sheet, and the interlayer film is 4.5 mm or more. <16> The thickness t 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2<17> A laminated glass according to any one of <12> to <15>, in which the coefficient of thermal expansion (Tc) is 1.5 or more. <17> A laminated glass comprising a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are the glass plates according to any one of <1> to <9>. <18> The laminated glass according to any one of <12> to <16>, in which the second glass plate is soda-lime glass. <19> The laminated glass according to any one of <12> to <16>, in which the second glass plate is aluminosilicate glass. <20> The laminated glass according to any one of <12> to <16>, in which the second glass plate has been subjected to a chemical strengthening treatment.
[0187] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto.
[0188] <Preparation of Glass Plates of Examples 1 to 18> Raw materials were placed in a platinum crucible and melted at a temperature of 1600°C to 1650°C for 3 hours to obtain molten glass so as to obtain the glass composition (unit: mol%) shown in Table 1. The molten glass was poured onto a carbon plate and slowly cooled. Both sides of the obtained plate-like glass were polished to obtain a glass plate having a thickness of 2.00 mm. Examples 1 to 11 are working examples, and Examples 12 to 18 are comparative examples.
[0189] The glass plates obtained above were subjected to the following evaluations, and the results are shown in Tables 1 and 2. Note that blank spaces in the tables indicate that no measurement was performed.
[0190] (1) Temperature T 2 , temperature T 4 : The glass viscosity η, which is the standard for the melting property of glass, is 10 2 Temperature T when viscosity becomes dPa s 2 and the glass viscosity η is 10 4 Temperature T at which viscosity becomes dPa s 4 was measured using a rotational viscometer.
[0191] (2) Glass transition temperature (T g ): Values measured using a differential thermal dilatometer (TMA) and determined in accordance with JIS R3103-3 (2001).
[0192] (3) Sagging point: A value measured using a differential thermal dilatometer (TMA), T g The temperature at which the thermal expansion curve sags among the above temperatures was taken as the sag point.
[0193] (4) Average coefficient of linear expansion (CTE) from 50 to 350 °C 50-350 ): Measured using a differential thermal dilatometer (TMA) and determined in accordance with JIS R3102 (1995).
[0194] (5) Density: A glass block of about 20 g containing no bubbles cut out from a glass plate was measured by Archimedes' method.
[0195] (6) Young's modulus: Measured at 25° C. by an ultrasonic pulse method (Olympus, DL35) based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0196] (7) Rigidity Modulus: Measured at 25° C. by an ultrasonic pulse method (Olympus, DL35) based on JIS R1602:1995 "Testing Method for Elastic Modulus of Fine Ceramics."
[0197] (8) Poisson's ratio: Measured at 25° C. by an ultrasonic pulse method (Olympus, DL35) based on JIS R1602:1995 "Testing method for elastic modulus of fine ceramics."
[0198] (9) Fracture toughness value @ SEPB method The fracture toughness of the glass plate obtained above was measured using a pre-crack introduction fracture test method (SEPB method: Single-Edge-Precracked-Beam method) based on JIS R1607:2015 “Fracture toughness test method for fine ceramics”.
[0199] (10) Surface Fracture Energy: Calculated using the Young's modulus and fracture toughness values obtained above according to the above formula (1).
[0200]
[0201] The glasses of Examples 1 to 11, which are working examples, were found to have a high Young's modulus of 75 GPa or more and excellent fracture toughness. In addition, since the yield point was 670°C or less, the glasses had low viscosity and excellent bending formability. On the other hand, Example 12, which is a comparative example, contained Al 2 O 3 is less than 3.0%, CaO is more than 5.0%, and Li 2 Since the O content was less than 1.0%, the Young's modulus and fracture toughness were lower than those of the Examples. 2 is less than 60%, and Li 2 O is less than 1.0%, and K 2 O is more than 3.0%, and TiO 2 is more than 1.0%, and Y 2 O 3 In addition, Example 14, which is a comparative example, had a high yield point because the content of Al was more than 1.0%. 2 O 3 is more than 9.0%, and Li 2 Since O was less than 1.0%, T g The yield point was T g Therefore, it was found that Example 14 had a yield point higher than 700°C and was inferior in bending formability. 2 is less than 60%, and Al 2 O 3 is more than 9.0%, and Li 2 O is less than 1.0%, and Na 2 O is less than 6.0%, and K 2 O is more than 3.0%, and R 2 Since O is less than 11%, T g The yield point was T g Therefore, it was found that Example 15 had a yield point higher than 702°C and was inferior in bend formability. 2 O 3 In addition, Example 17, which is a comparative example, had a high yield point because the Al content was more than 9.0% and the RO content was less than 7.0%. 2 O 3 is more than 9.0%, RO is less than 7.0%, and TiO 2was more than 1.0%, the yield point was high.
[0202] <Preparation of Laminated Glass> Laminated glasses of Test Examples 1 to 3 were prepared according to the following procedure. Test Examples 1 to 3 are comparative examples, and Test Examples 4 to 7 are working examples.
[0203] (Test Example 1) Glass having a thickness of 2.0 mm and a composition shown in Example 13 of Table 1 with a surface roughness Ra of 2.0 nm or less was used as the first glass plate and the second glass plate. Polyvinyl butyral (PVB) having a thickness of 0.78 mm was used as the interlayer film. The first glass plate, the interlayer film, and the second glass plate were laminated in this order, and after preliminary bonding at 120°C for 15 minutes, pressure bonding was performed under conditions of 130°C and 1 MPa. The laminated glass of Test Example 1 was then produced by returning to room temperature and atmospheric pressure over 90 minutes. The laminated glass of Test Example 1 had a total thickness of 4.8 mm for the first glass plate, the second glass plate, and the interlayer film, and a thickness of t 1 and the thickness t of the second glass plate 2 The ratio (t 1 / t 2 ) was 1.0.
[0204] Test Example 2 A laminated glass was produced in the same manner as in Test Example 1, except that the thicknesses of the first glass plate and the second glass plate were changed to the values shown in Table 2.
[0205] Test Example 3 A laminated glass was produced in the same manner as in Test Example 1, except that the thickness of the first glass plate was changed to the value shown in Table 2 and a soda-lime glass (manufactured by AGC, model number: AS2) having a thickness of 0.7 mm was used as the second glass plate.
[0206] Test Examples 4 to 7 Laminated glasses were produced in the same manner as in Test Example 3, except that the type of the first glass plate was changed to one shown in Table 2 (all of which had a surface roughness Ra of 2.0 nm or less).
[0207] The critical impact fracture velocity Vcrt of the laminated glass sheet obtained above was measured using the following procedure. <Procedure> A tungsten carbide cemented carbide with a tip curvature radius of 200 μm, an apex angle of 120°, and a weight of 1.365 g was injected at a speed of 20 km / h or more and allowed to impact the surface of the first glass sheet. During this impact, the propagation process of a crack generated by the impact of the tungsten carbide cemented carbide was observed from the cross section of the laminated glass using a high-speed camera. The test was carried out while changing the injection velocity, and a crack generated on the surface of the first glass sheet was judged to have occurred when it propagated and reached the surface of the first glass sheet opposite the surface against which the tungsten carbide cemented carbide was impacted. The impact velocity at this time was taken as the critical impact fracture velocity Vcrt.
[0208]
[0209] The laminated glasses of Test Examples 4 to 7, which are working examples, had higher critical impact fracture speeds than the comparative examples.
[0210] This application is based on Japanese Patent Application No. 2023-075162 filed on April 28, 2023, the contents of which are incorporated herein by reference.
[0211] REFERENCE SIGNS LIST 10 Laminated glass 11 First glass sheet 12 Second glass sheet 13 Interlayer 100 Automobile 110 Opening 120 Housing 150 Rearview mirror 201 Millimeter wave radar 202 Stereo camera 300 Radio wave
Claims
1. In mole percent based on oxide, SiO 2 : 60 to 72% Al 2 O 3 :3.0~9.0%B 2 O 3 :0.0~4.0% MgO:3.0~15% CaO:0.0~5.0% SrO:0.0~5.0% BaO:0.0~2.0% Li 2 O: 1.0-10% Na 2 O: 6.0-16% K 2 O: 0.0 to 3.0% ZrO 2 :0.0~1.0% TiO 2 :0.0~1.0% Y 2 O 3 :0.0~1.0%R 2 O: 11-25% RO: 7.0-20% (wherein RO is at least one selected from MgO, CaO, SrO, and BaO; R 2 O is Li 2 O, Na 2 O.K. 2 O).
2. The glass according to claim 1, having a Young's modulus of 75 GPa or more.
3. Fracture toughness value K measured by the SEPB method IC is 0.76MPa·m 1/2 The glass of claim 2 .
4. The glass according to claim 1, having a yield point of 670°C or less.
5. The glass according to claim 4, wherein the ratio (H / L) of the H value to the L value calculated by the following formula is 0.10 or less. 2 O] + [CaO] + [SrO] + [BaO] + [ZrO 2 ]+[TiO 2 ]+[Y 2 O 3 ] L = [SiO 2 ]+[Al 2 O 3 ]+[MgO]+[Li 2 O] + [Na 2 O] (where [ ] means the content of each component in the brackets expressed as mole percent on an oxide basis.) 6. Fracture toughness value K measured by the SEPB method IC is 0.80MPa·m 1/2 The glass according to claim 5 .
7. The glass according to claim 1, which has a critical impact fracture speed of 35 km / h or more when impacted with a tungsten carbide alloy having a tip curvature radius of 200 μm, an apex angle of 120° and a weight of 1.365 g, when the glass has a surface roughness Ra of 5.0 nm or less and a thickness of 2.5 mm.
8. The glass according to claim 1, which has a critical impact fracture speed of 53 km / h or more when impacted with a tungsten carbide hard alloy having a tip curvature radius of 200 μm, an apex angle of 120° and a weight of 1.365 g.
9. The glass of claim 8 having a thickness of 2.5 mm or more.
10. A window glass for a vehicle, comprising the glass according to any one of claims 1 to 9.
11. A glass for a sensor, comprising the glass according to any one of claims 1 to 9.
12. A laminated glass comprising a first glass plate, a second glass plate, and an interlayer film sandwiched between the first glass plate and the second glass plate, wherein the first glass plate is the glass according to any one of claims 1 to 9.
13. The laminated glass according to claim 12, wherein the first glass plate has a surface roughness Ra of 5.0 nm or less, a thickness of 2.5 mm, and a critical impact fracture speed of 35 km / h or more when a tungsten carbide alloy having a tip radius of curvature of 200 μm, an apex angle of 120° and a weight of 1.365 g is collided with a surface of the first glass plate.
14. The laminated glass according to claim 12, wherein the critical impact fracture speed when a tungsten carbide cemented carbide having a tip curvature radius of 200 μm, an apex angle of 120° and a weight of 1.365 g is impacted against the surface of the first glass plate is 53 km / h or more.
15. The laminated glass according to claim 14, wherein the total thickness of the first glass sheet, the second glass sheet, and the interlayer film is 4.5 mm or more.
16. Thickness t of the first glass plate 1 and the thickness t of the second glass plate 2 Ratio to (t 1 / t 2 13. The laminated glass according to claim 12, wherein the ratio of the refractive index to the refractive index of the laminated glass is 1.5 or more.
17. A laminated glass comprising a first glass plate, a second glass plate, and an interlayer sandwiched between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are the glass plates according to any one of claims 1 to 9.
18. The laminated glass of claim 12, wherein the second glass sheet is soda-lime glass.
19. The laminated glass of claim 12, wherein the second glass sheet is an aluminosilicate glass.
20. The laminated glass according to claim 12, wherein the second glass sheet has been subjected to a chemical strengthening treatment.
Citation Information
Patent Citations
Glass for magnetic disk substrate
JP1999199267A
Glass molding with enhanced cleaning property
JP2005247656A
Flat surface-type display device
JP2006160546A
Alkaline earth aluminosilicate glass composition with improved chemical and mechanical durability
JP2015501280A
Automotive glass compositions, articles and hybrid laminates
JP2020525379A
Cited By
Anti-falling and anti-scratching lithium aluminum silicate glass and preparation method thereof
CN120398412A
Glass plate and laminated glass
WO2026075247A1
Automobile window glass
WO2026115937A1
High‑modulus glass, protective film, cover plate layer, display module, and electronic device