Methane oxidation catalyst, production method for methane oxidation catalyst, and methane oxidation method

The ceria-zirconia composite oxide catalyst with Pd and Pt supports high methane oxidation efficiency at low temperatures, addressing the low methane oxidation ability of existing catalysts and effectively reducing emissions from natural gas-powered engines.

WO2024225135A1PCT designated stage expired Publication Date: 2024-10-31HITACHI ZOSEN CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015274
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-17
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing hydrocarbon decomposition catalysts have low methane oxidation ability under relatively low-temperature conditions, which is inadequate for effectively oxidizing unburned methane in exhaust gases from internal combustion engines running on natural gas.

Method used

A methane oxidation catalyst comprising a ceria-zirconia composite oxide catalyst carrier with Pd and Pt as active metals, where the ceria content is between 5% to 15% by mass, and the Pd content is 50% or more by mass, supported on the carrier, and calcined at temperatures between 400°C to 600°C, enhancing methane decomposition ability at low temperatures.

Benefits of technology

The catalyst achieves high methane decomposition efficiency under relatively low-temperature conditions, efficiently oxidizing methane in exhaust gases, thereby improving air quality and reducing emissions from natural gas-powered vehicles and industrial processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

A methane oxidation catalyst according to the present invention is a catalyst for oxidizing methane and comprises: a catalyst carrier that includes a ceria-zirconia composite oxide; and an active metal that is carried on the catalyst carrier and includes Pd and Pt. The ceria content fraction of the catalyst carrier is at least 5 mass% but less than 15 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Methane oxidation catalyst, method for producing methane oxidation catalyst, and method for oxidizing methane

[0001] The present invention relates to a methane oxidation catalyst, a method for producing a methane oxidation catalyst, and a method for oxidizing methane.

[0002] Harmful substances (e.g., hydrocarbons, nitrogen oxides, etc.) contained in exhaust gases emitted from internal combustion engines and the like cause air pollution. Specifically, exhaust gases emitted from automobiles contain a large amount of propylene as a hydrocarbon. Furthermore, exhaust gases emitted from internal combustion engines powered by natural gas contain unburned methane, as some of the methane contained in the natural gas does not burn. To decompose the hydrocarbons contained in such exhaust gases, a known technology is to place a catalyst that decomposes hydrocarbons in the exhaust passage through which the exhaust gas flows.

[0003] As such a hydrocarbon decomposition catalyst, a hydrocarbon decomposition catalyst has been proposed in which an active metal is supported on a catalyst carrier made of a metal oxide containing 15 to 100 wt % of a rare earth oxide (e.g., ceria) (see, for example, Patent Document 1).

[0004] The hydrocarbon cracking catalyst of Patent Document 1 is highly active and can maintain its activity for a long period of time even under high temperature conditions (for example, 800° C.).

[0005] Japanese Patent Application Laid-Open No. 2005-270882

[0006] On the other hand, as described above, exhaust gas from an internal combustion engine powered by natural gas contains unburned methane. Methane has a chemically stable structure and is resistant to oxidation. Furthermore, exhaust gas from an internal combustion engine powered by natural gas is emitted at a relatively low temperature. Therefore, among hydrocarbon cracking catalysts, a catalyst that oxidizes methane is required to have a high methane decomposition ability under relatively low temperature conditions.

[0007] However, the hydrocarbon cracking catalyst of Patent Document 1 has a drawback in that it has low methane decomposition ability under relatively low temperature conditions.

[0008] The present invention aims to provide a methane oxidation catalyst having a high methane decomposition ability under relatively low temperature conditions, a method for producing the methane oxidation catalyst, and a method for oxidizing methane.

[0009] The present invention [1] relates to a catalyst for oxidizing methane, the catalyst comprising: a catalyst support containing a ceria-zirconia composite oxide; and an active metal supported on the catalyst support and containing Pd and Pt, wherein the ceria content in the catalyst support is 5% by mass or more and less than 15% by mass.

[0010] The present invention [2] includes the methane oxidation catalyst according to [1], wherein the content of the Pd in ​​the active metal is 50 mass% or more.

[0011] The present invention [3] includes the methane oxidation catalyst according to [1], wherein the amount of the active metal blended is 5 parts by mass or less per 100 parts by mass of the catalyst support.

[0012] The present invention [4] includes the methane oxidation catalyst according to [1], wherein the catalyst support further contains zirconia, the zirconia contains a monoclinic zirconia phase, and the ceria-zirconia mixed oxide contains a tetragonal ceria-zirconia phase.

[0013] The present invention [5] includes a method for producing a methane oxidation catalyst, comprising: a first step of mixing a catalyst support raw material containing ceria-zirconia composite oxide with a solution of an active metal containing Pd and Pt to prepare a slurry; a second step of drying the slurry to obtain a powder; and a third step of calcining the powder at 400°C or higher and 600°C or lower to obtain the methane oxidation catalyst according to any one of [1] to [4], wherein in the first step, the ceria content in the catalyst support raw material is 5% by mass or higher and less than 15% by mass.

[0014] The present invention [6] includes a method for oxidizing methane, comprising an oxidation step of contacting methane with the methane oxidation catalyst according to any one of [1] to [4] and oxidizing the methane, wherein the oxidation temperature in the oxidation step is 450°C or less.

[0015] The methane oxidation catalyst of the present invention comprises a catalyst support containing a ceria-zirconia composite oxide and an active metal supported on the catalyst support and containing Pd and Pt, wherein the ceria content in the catalyst support is 5% by mass or more and less than 15% by mass, and therefore has high methane decomposition ability even under relatively low temperature conditions.

[0016] The method for producing a methane oxidation catalyst of the present invention includes a first step of mixing a catalyst support raw material containing ceria-zirconia composite oxide with a solution of active metals containing Pd and Pt to prepare a slurry, a second step of drying the slurry to obtain a powder, and a third step of calcining the powder at 400°C or higher and 600°C or lower to obtain a methane oxidation catalyst, wherein in the first step, the ceria content in the catalyst support is 5% by mass or higher and less than 15% by mass. Therefore, the above-mentioned methane oxidation catalyst can be produced efficiently.

[0017] The method for oxidizing methane of the present invention includes an oxidation step of contacting methane with the methane oxidation catalyst and oxidizing the methane, wherein the oxidation temperature in the oxidation step is 450° C. or lower. Therefore, methane can be efficiently oxidized under relatively low temperature conditions.

[0018] 1 shows graphs of X-ray diffraction (XRD) patterns of catalyst support raw materials used in each Example and Comparative Example, and X-ray diffraction (XRD) patterns of methane oxidation catalysts used in each Example and Comparative Example.

[0019] 1. Methane oxidation catalyst The methane oxidation catalyst is a catalyst that converts methane (CH 4 ) and CO 2 and H 2 O. Such a methane oxidation catalyst can be used, for example, to remove unburned methane contained in exhaust gas as a methane-containing gas discharged from an LNG-fueled ship, and can also be used to remove methane contained in a methane-containing gas produced in a process such as a gas-phase reaction in a chemical plant.

[0020] The methane oxidation catalyst comprises a catalyst support containing a ceria-zirconia composite oxide, and an active metal supported on the catalyst support and containing Pd and Pt.

[0021] <Catalyst Support> The catalyst support supports an active metal, which will be described later.

[0022] The catalyst support contains a ceria-zirconia composite oxide, and may contain other catalyst supports (for example, zirconia and a particle component described below) in addition to the ceria-zirconia composite oxide.

[0023] Ceria-zirconia composite oxide (Ce X Zr 1-X O 2 ) is, for example, ceria (CeO 2 ) and zirconia (ZrO 2 ) solid solution. X is more than 0 and less than 1.

[0024] That is, raw materials for the ceria-zirconia composite oxide include, for example, ceria and zirconia.

[0025] In the raw material for the ceria-zirconia composite oxide, for example, all of the zirconia may form a ceria-zirconia composite oxide, or, for example, a portion of the zirconia may form a ceria-zirconia composite oxide, with the remaining zirconia existing alone. In the raw material for the ceria-zirconia composite oxide, preferably a portion of the zirconia forms a ceria-zirconia composite oxide, with the remaining zirconia existing alone.

[0026] In the raw material for the ceria-zirconia composite oxide, for example, all of the ceria may form a ceria-zirconia composite oxide, or, for example, a portion of the ceria may form a ceria-zirconia composite oxide, with the remaining ceria being present alone. In the raw material for the ceria-zirconia composite oxide, preferably, all of the ceria forms a ceria-zirconia composite oxide.

[0027] That is, the catalyst support preferably contains zirconia and ceria-zirconia composite oxide, and more preferably consists of zirconia and ceria-zirconia composite oxide.

[0028] When zirconia is present alone, it may be, for example, monoclinic zirconia (m-ZrO 2) phase, and the ceria-zirconia composite oxide contains, for example, tetragonal ceria-zirconia (t-Ce X Zr 1-X O 2 ) phase.

[0029] That is, the catalyst support preferably contains both a monoclinic zirconia phase and a tetragonal ceria-zirconia phase. Specifically, zirconia contained in the catalyst support that does not form a ceria-zirconia composite oxide forms a monoclinic zirconia phase by itself, and the ceria-zirconia composite oxide forms a tetragonal ceria-zirconia phase.

[0030] If the catalyst support contains a monoclinic zirconia phase, which has active metal support sites that are more easily activated than in a tetragonal ceria-zirconia phase, it will have excellent methane decomposition ability.Furthermore, if the catalyst support contains a tetragonal ceria-zirconia phase, it will be able to ensure the surface acidity necessary for the methane oxidation reaction and will have excellent methane decomposition ability.

[0031] The content ratios of zirconia and ceria described below include the content ratios of ceria present alone, zirconia present alone, and ceria and zirconia forming a ceria-zirconia composite oxide in the catalyst support.

[0032] In the catalyst carrier, the zirconia content is, for example, 50 mass% or more, preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 85 mass% or more, particularly preferably 89 mass% or more, and most preferably 90 mass% or more, and for example, less than 95 mass%, preferably 94 mass% or less, more preferably 93 mass% or less, even more preferably 92 mass% or less, and particularly preferably 91 mass% or less.

[0033] When the content of zirconia in the catalyst carrier is within the above range, it can form a monoclinic zirconia phase by itself.

[0034] The catalyst support has a ceria content of 5% by mass or more, preferably 6% by mass or more, more preferably 7% by mass or more, even more preferably 8% by mass or more, and particularly preferably 9% by mass or more. The catalyst support has a ceria content of less than 15% by mass, preferably 14% by mass or less, more preferably 13% by mass or less, even more preferably 12% by mass or less, particularly preferably 11% by mass or less, and most preferably 10% by mass or less.

[0035] When the ceria content in the catalyst support is within the above range, it is possible to form a ceria-zirconia composite oxide while ensuring the amount of zirconia blended to form a monoclinic zirconia phase. As a result, the catalyst support can contain both the monoclinic zirconia phase and the tetragonal ceria-zirconia phase, and has high methane decomposition ability under relatively low temperature conditions.

[0036] The catalyst carrier is monoclinic zirconia (m-ZrO 2 ) phase and tetragonal ceria-zirconia (t-Ce X Zr 1-X O 2 The presence of the α- and β-phases can be confirmed by measuring the X-ray diffraction (XRD) pattern. Details will be described in the Examples below.

[0037] Monoclinic zirconia (m-ZrO 2 ) phase and tetragonal ceria-zirconia (t-Ce X Zr 1-X O 2 The positions of the diffraction peaks (2θ values ​​(θ is the Bragg angle)) of the tetragonal ceria-zirconia (t-Ce) phase are shown. X Zr 1-X O 2 The position of the diffraction peak of the Cr-Cu phase shifts depending on the Ce composition, that is, the value of X.

[0038] Monoclinic zirconia (m-ZrO 2 The diffraction peak position of the (-111) plane of the tetragonal ceria-zirconia (t-Ce) phase is, for example, 28°≦2θ≦29°. X Zr 1-X O 2The diffraction peak position of the (101) plane of the SiO2 phase is, for example, 28°≦2θ≦31°.

[0039] In addition, tetragonal ceria-zirconia (t-Ce X Zr 1-X O 2 ) phase (101) plane diffraction peak, the diffraction peak when X = 0 (t-ZrO 2 The position of the diffraction peak of the (111) plane of the phase is, for example, 30°≦2θ≦31°.

[0040] Furthermore, as described above, the catalyst support may contain a particle component as another catalyst support.

[0041] Particulate components include, for example, silica, alumina, titania, and zeolites.

[0042] The particle components may be used alone or in combination of two or more.

[0043] <Active Metal> The active metal is supported on a catalyst support.

[0044] The active metal may be in the metallic state or in the metallic oxide state, for example. From the viewpoint of catalytic activity, the active metal is preferably in the metallic state.

[0045] The active metals include Pd and Pt.

[0046] The active metal may also contain other active metals in addition to Pd and Pt, such as Ni, Co, Mn, Fe, and Cu.

[0047] The active metal includes Pd and Pt, and is preferably Pd and Pt. That is, the active metal preferably does not include other active metals than Pd and Pt. Note that, when the active metal is Pd and Pt, the total amount of the active metals described below is the sum of the amounts of Pd and Pt.

[0048] The Pd content in the active metals (=Pd content / total amount of active metals×100) is, for example, 30 mass% or more, preferably 40 mass% or more, more preferably 50 mass% or more, even more preferably 70 mass% or more, particularly preferably 75 mass% or more, and most preferably 80 mass% or more, and for example, less than 100 mass%, preferably 95 mass% or less, more preferably 90 mass% or less, and even more preferably 85 mass% or less.

[0049] When the content of Pd in ​​the active metals is within the above range, the methane oxidation catalyst has a high methane decomposition ability under relatively low temperature conditions.

[0050] The Pt content in the active metal (=Pt content / total amount of active metal×100) is, for example, 1 mass% or more, preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 15 mass% or more, and for example, 60 mass% or less, preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, particularly preferably 25 mass% or less, and most preferably 20 mass% or less.

[0051] When the content of Pt in the active metals is within the above range, the methane oxidation catalyst is excellent in terms of production cost.

[0052] The amount of active metal blended relative to 100 parts by mass of the catalyst support is, for example, 1 part by mass or more, preferably 2 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 4 parts by mass or more, and for example, 10 parts by mass or less, preferably 8 parts by mass or less, more preferably 6 parts by mass or less, even more preferably 5 parts by mass or less. Note that parts by mass indicate the ratio of the amount of active metal blended to the amount of catalyst support blended.

[0053] When the amount of active metal blended relative to 100 parts by mass of the catalyst support is within the above range, the methane oxidation catalyst is excellent in terms of production cost.

[0054] The amount of Pd to be blended relative to 100 parts by mass of the catalyst support is, for example, 0.5 parts by mass or more, preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, particularly preferably 4 parts by mass or more, and is, for example, less than 10 parts by mass, preferably 8 parts by mass or less, more preferably 6 parts by mass or less, even more preferably 5 parts by mass or less.

[0055] The amount of Pt to be blended relative to 100 parts by mass of the catalyst support is, for example, 0.1 parts by mass or more, preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.8 parts by mass or more, and for example, less than 5 parts by mass, preferably 3 parts by mass or less, more preferably 2 parts by mass or less, even more preferably 1 part by mass or less.

[0056] <Additives> Additives can be added to the methane oxidation catalyst as needed.

[0057] The additives are not particularly limited as long as they are additives that are commonly used in methane oxidation catalysts, and examples thereof include diluents and binders.

[0058] The diluent component is a substance that is inert to the methane oxidation reaction, and adding the diluent component to the methane oxidation catalyst makes it easier to control the temperature.

[0059] Examples of the diluent component include alumina (eg, α-alumina, θ-alumina, γ-alumina, etc.) and titania (eg, rutile-type titania, anatase-type titania, etc.).

[0060] The diluent may be used alone or in combination of two or more kinds.

[0061] The binder is a binding component that binds together particles of the methane oxidation catalyst when the methane oxidation catalyst is used in a fluidized bed reactor, for example.

[0062] Binders include, for example, silicates, titanates, and aluminates.

[0063] The binders may be used alone or in combination of two or more.

[0064] The proportions of the diluent and binder added are selected arbitrarily depending on the intended use of the methane oxidation catalyst.

[0065] 2. Method for Producing Methane Oxidation Catalyst Next, a method for producing the methane oxidation catalyst of the present invention will be described.

[0066] The method for producing a methane oxidation catalyst includes a first step of mixing a catalyst support raw material containing a ceria-zirconia composite oxide with a solution of active metals containing Pd and Pt to prepare a slurry; a second step of drying the slurry to obtain a powder; and a third step of calcining the powder at a temperature of 400°C or higher and 600°C or lower to obtain the methane oxidation catalyst.

[0067] [Step 1] In Step 1, a catalyst support raw material containing a ceria-zirconia composite oxide is mixed with a solution of an active metal containing Pd and Pt to prepare a slurry. Specifically, a powdery catalyst support raw material containing a ceria-zirconia composite oxide is suspended in the solution of the active metal containing Pd and Pt (active metal-containing solution), and the suspension is stirred to obtain a slurry.

[0068] The catalyst support raw material is not particularly limited as long as it is a raw material that can form the above-mentioned catalyst support. The catalyst support raw material includes a ceria-zirconia composite oxide, preferably includes zirconia and a ceria-zirconia composite oxide, and more preferably includes zirconia and a ceria-zirconia composite oxide.

[0069] The content of ceria in the catalyst support raw material is not particularly limited as long as it satisfies the above-mentioned requirement for the ceria content in the catalyst support. That is, the content of ceria in the catalyst support raw material is 5 mass% or more, preferably 6 mass% or more, more preferably 7 mass% or more, even more preferably 8 mass% or more, and particularly preferably 9 mass% or more. Furthermore, the content of ceria in the catalyst support raw material is less than 15 mass%, preferably 14 mass% or less, more preferably 13 mass% or less, even more preferably 12 mass% or less, particularly preferably 11 mass% or less, and most preferably 10 mass% or less.

[0070] The active metal-containing solution is, for example, a solution containing a salt of the active metal and a solvent.

[0071] Examples of the salt of the active metal include nitrates of the active metal, chlorides of the active metal, and acetates of the active metal, and preferably nitrates of the active metal.

[0072] The active metal includes Pd and Pt, and may also include active metals other than Pd and Pt.

[0073] That is, examples of active metal salts include palladium salts and platinum salts. Specifically, examples of palladium salts include palladium nitrate, palladium chloride, and palladium acetate, with palladium nitrate being preferred. Examples of platinum salts include tetraammineplatinum(II) nitrate, platinum nitrate, and platinum chloride, with tetraammineplatinum(II) nitrate and platinum nitrate being preferred.

[0074] The solvent is not particularly limited as long as it is one that is commonly used as an active metal-containing solution, and examples thereof include ion-exchanged water and ultrapure water, with ion-exchanged water being preferred.

[0075] The active metal-containing solution may be prepared by, for example, mixing solutions of the respective active metals, or by adding salts of the respective active metals to one solvent. From the viewpoint of manufacturability, it is preferable to prepare the solution by mixing solutions of the respective active metals. Specifically, the active metal-containing solution can be prepared by mixing a palladium (II) nitrate solution, a tetraammineplatinum (II) nitrate solution, and ion-exchanged water.

[0076] A catalyst support raw material is added to the active metal-containing solution and stirred to form a slurry.

[0077] The stirring temperature is, for example, 5°C or higher and, for example, 35°C or lower.

[0078] The stirring time can be appropriately set depending on the amount of preparation, and is, for example, 15 hours or more and, for example, 21 hours or less.

[0079] In this way, a slurry containing the active metal and the catalyst support is obtained.

[0080] [Second Step] In the second step, the slurry obtained in the first step is dried to obtain a powder.

[0081] The drying temperature is, for example, 80°C or more, preferably 100°C or more, and for example, 150°C or less, preferably 130°C or less.

[0082] The drying time can be appropriately set to the time required to dry the slurry at the above-mentioned drying temperature, and is, for example, 1 hour or more, preferably 3 hours or more, and for example, 9 hours or less, preferably 7 hours or less.

[0083] [Third Step] In the third step, the powder obtained in the second step is calcined at 400° C. or higher and 600° C. or lower to obtain a methane oxidation catalyst.

[0084] The calcination method is not particularly limited, and any known method can be used as long as the desired catalyst can be obtained.

[0085] The firing temperature is 400° C. or higher, preferably 450° C. or higher, more preferably 480° C. or higher, and 600° C. or lower, preferably 550° C. or lower, more preferably 520° C. or lower.

[0086] The firing time is, for example, 5 hours or more, preferably 7 hours or more, and for example, 13 hours or less, preferably 11 hours or less.

[0087] The obtained methane oxidation catalyst may be pulverized. Examples of the pulverization method include compression pulverization. Alternatively, the pulverized methane oxidation catalyst may be sieved to separate methane oxidation catalysts of the desired size. Furthermore, the methane oxidation catalyst may be compression molded into a predetermined shape before or after pulverization.

[0088] The shape of the methane oxidation catalyst may be, for example, a sphere, a pellet, or a tablet.

[0089] The second and third steps described above show methods for producing a methane oxidation catalyst in the form of a sphere, pellet, tablet, or the like. However, the shape of the methane oxidation catalyst may also be, for example, a plate or a honeycomb (monolith) shape.

[0090] The plate-shaped methane oxidation catalyst can be obtained, for example, by applying or impregnating the slurry obtained in the first step onto an inorganic fiber sheet, followed by drying and calcining.

[0091] Examples of inorganic fiber sheets include glass fiber sheets and ceramic fiber sheets.

[0092] The drying conditions and firing conditions may be, for example, the conditions described in the second and third steps above.

[0093] A honeycomb (monolith) methane oxidation catalyst can be obtained, for example, by coating the methane oxidation catalyst onto a substrate material of a honeycomb structure.

[0094] Examples of substrate materials for honeycomb structures include inorganic fiber sheets (e.g., glass fiber sheets and ceramic fiber sheets), cordierite, silicon carbide, mullite, alumina, zirconia, titania, titanium phosphate, aluminum titanate, betalite, spondumene, aluminosilicate, and magnesium silicate.

[0095] Examples of methods for coating a glass fiber sheet, which is a substrate material for a honeycomb structure, include those described in Japanese Patent Nos. 5,909,436 and 6,228,727.

[0096] Specifically, the slurry obtained in the first step is applied to a glass fiber sheet, the slurry-coated glass fiber sheet is then shaped using a corrugation die and a press jig, the resulting corrugated slurry-coated glass fiber sheet is dried and peeled off from the die, and after drying, the corrugated slurry-coated glass fiber sheet is calcined to obtain a corrugated glass fiber sheet methane oxidation catalyst.

[0097] On the other hand, the slurry obtained in the first step is applied to a glass fiber sheet, and the flat, unshaped, slurry-coated glass fiber sheet is dried. After drying, the flat, slurry-coated glass fiber sheet is calcined to obtain a flat glass fiber sheet of a methane oxidation catalyst.

[0098] The drying temperature for the corrugated slurry-coated glass fiber sheet and the flat slurry-coated glass fiber sheet is, for example, 100°C or higher and, for example, 200°C or lower, and the drying time is, for example, 1 hour or higher and, for example, 2 hours or lower.

[0099] The firing temperature of the corrugated slurry-coated glass fiber sheet and the flat slurry-coated glass fiber sheet is, for example, 300°C or higher and, for example, 550°C or lower, and the firing time is, for example, 1 hour or higher and, for example, 4 hours or lower.

[0100] Next, the methane oxidation catalyst in the form of a corrugated glass fiber sheet and the methane oxidation catalyst in the form of a flat glass fiber sheet are laminated together to obtain a methane oxidation catalyst having a cross-sectional network structure (honeycomb shape).

[0101] In this manner, a methane oxidation catalyst can be produced.

[0102] 3. Method for Oxidizing Methane (Method for Using Methane Oxidation Catalyst) Next, the method for oxidizing methane of the present invention will be described.

[0103] The method for oxidizing methane includes an oxidation step in which methane is brought into contact with the methane oxidation catalyst and oxidized, and in the oxidation step, the oxidation temperature is 450° C. or less.

[0104] Specifically, the methane oxidation method involves filling a reactor (for example, a fixed-bed reactor) with the methane oxidation catalyst and supplying a methane-containing gas through a reactor supply port, whereby the methane comes into contact with the methane oxidation catalyst and the methane is converted into CO 2 and H 2 O is then oxidized to O, which is then discharged from the reactor outlet.

[0105] The amount and volume of the methane oxidation catalyst to be filled can be adjusted appropriately depending on the application.

[0106] The methane oxidation catalyst is used, for example, to remove methane from exhaust gas, which is a methane-containing gas discharged from an LNG-fueled ship. When used in such an application, the loading amount of the methane oxidation catalyst is, for example, 0.5 kg or more, preferably 5 kg or more, more preferably 10 kg or more, even more preferably 50 kg or more, particularly preferably 100 kg or more, and most preferably 150 kg or more. The volume of the methane oxidation catalyst is, for example, 0.003 m 3 More than 0.01 m, preferably 0.01 m 3 More preferably, 0.1 m 3 More preferably, 0.5 m 3 More preferably, 0.8 m 3 More than 1.0 m, most preferably 1.0 m 3 That's all.

[0107] If the loading amount and volume of the methane oxidation catalyst are equal to or greater than the above lower limits, the catalyst can be used to remove methane from exhaust gas, which is a methane-containing gas discharged from an LNG-fueled ship.

[0108] Unlike three-way catalysts used in automobile exhaust gas treatment, methane oxidation catalysts contain Pd and Pt in specific ratios among their active metals. That is, even if they contain other active metals (e.g., Rh in the case of three-way catalysts), the content is low, allowing them to be manufactured relatively inexpensively. Therefore, even when the methane oxidation catalyst is used to remove methane from methane-containing exhaust gas discharged from LNG-fueled ships (when the loading and volume of the methane oxidation catalyst are large), raw material costs can be kept low.

[0109] The methane-containing gas fed to the reactor may be, for example, CH 4 And, O 2 And, H 2 O. Also, other hydrocarbons and N 2 may also include:

[0110] In methane-containing gas, CH 4The concentration is not particularly limited, and is, for example, 100 ppmv-dry or more, preferably 300 ppmv-dry or more, more preferably 500 ppmv-dry or more, even more preferably 800 ppmv-dry or more, and for example, 100,000 ppmv-dry or less, preferably 50,000 ppmv-dry or less, more preferably 30,000 ppmv-dry or less, even more preferably 10,000 ppmv-dry or less.

[0111] O in methane-containing gas 2 The concentration of is, for example, 3 vol% or more, preferably 5 vol% or more, more preferably 8 vol% or more, even more preferably 10 vol% or more, and for example, 30 vol% or less, preferably 25 vol% or less, more preferably 20 vol% or less, even more preferably 15 vol% or less.

[0112] H in methane-containing gas 2 The O concentration is, for example, 1 vol% or more, preferably 3 vol% or more, more preferably 5 vol% or more, and for example, 20 vol% or less, preferably 15 vol% or less, more preferably 12 vol% or less, and still more preferably 10 vol% or less.

[0113] The flow rate of the methane-containing gas is not particularly limited and is, for example, 0.1 NL / min or more, preferably 0.3 NL / min or more, more preferably 0.5 NL / min or more, and for example, 10 NL / min or less, preferably 8 NL / min or less, more preferably 5 NL / min or less.

[0114] The gas hourly space velocity (GHSV) of the methane-containing gas is, for example, 10,000 h -1 More than 20,000 hours, preferably -1 More preferably, 30,000 hours -1 or more, for example, 100,000 h -1 Preferably, 90,000 hours or less -1 Less than or equal to 80,000 hours, more preferably -1 The following is the result.

[0115] The gas hourly space velocity (GHSV) can be calculated using the following formula.

[0116] Gas hourly space velocity (GHSV) = gas flow rate (Nm 3 / h) / catalyst volume (m 3 )

[0117] In the oxidation step in which methane is brought into contact with the methane oxidation catalyst and oxidized, the oxidation temperature is, for example, 200°C or higher, preferably 250°C or higher, more preferably 300°C or higher, even more preferably 350°C or higher, and for example, 700°C or lower, preferably 600°C or lower, more preferably 500°C or lower, even more preferably 450°C or lower, and particularly preferably 400°C or lower.

[0118] That is, the methane oxidation catalyst described above can oxidize methane even under the above-mentioned relatively low temperature conditions.

[0119] The reaction rate constant k of the methane oxidation catalyst at 350°C is, for example, 7,500 h -1 More than 10,000 hours, preferably -1 More preferably, 12,500 hours -1 More preferably, 50,000 hours -1 More preferably, 65,000 h -1 More than 72,000 hours, most preferably -1 The larger the reaction rate constant k, the higher the methane decomposition ability.

[0120] The reaction rate constant k of the methane oxidation catalyst at 350°C can be calculated using the conditions and method for evaluating the performance of the methane oxidation catalyst described in the Examples. Specifically, the methane oxidation rate (%) is measured at six temperatures, and the reaction rate constant k at each temperature is calculated using the following formula (1). Next, the Arrhenius equation for the methane oxidation reaction is determined using the Arrhenius plot method based on the reaction rate constant k at each temperature, and the reaction rate constant k at 350°C can be calculated.

[0121] k = -GHSV × In (1 - methane oxidation rate (%) / 100) (1)

[0122] Methane oxidation rate (%) = (methane concentration at reactor inlet - methane concentration at reactor outlet) / (methane concentration at reactor inlet) x 100

[0123] The methane concentration at the reactor inlet is the concentration of methane supplied to a reactor packed with a methane oxidation catalyst (the concentration of methane before contacting the methane oxidation catalyst), and the methane concentration at the reactor outlet is the concentration of methane discharged from a reactor packed with a methane oxidation catalyst (the concentration of methane after contacting the methane oxidation catalyst).

[0124] The methane oxidation rate (%) of the methane oxidation catalyst at 350°C is, for example, 10% or more, preferably 15% or more, more preferably 20% or more, even more preferably 50% or more, particularly preferably 60% or more, and most preferably 70% or more.

[0125] The methane oxidation rate (%) of the methane oxidation catalyst at 375°C is, for example, 20% or more, preferably 30% or more, more preferably 40% or more, even more preferably 80% or more, particularly preferably 85% or more, and most preferably 90% or more.

[0126] The methane oxidation rate (%) of the methane oxidation catalyst at 400°C is, for example, 40% or more, preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, particularly preferably 90% or more, and most preferably 95% or more.

[0127] The methane oxidation rate (%) at each temperature is calculated using the conditions and method for evaluating the performance of the methane oxidation catalyst described in the Examples. Specifically, the methane oxidation rate (%) is calculated using the reaction rate constant k at each temperature calculated using the above-mentioned method and the above formula (1).

[0128] The methane oxidation catalyst of the present invention comprises a catalyst support containing a ceria-zirconia composite oxide and an active metal supported on the catalyst support and containing Pd and Pt, and the ceria content in the catalyst support is 5% by mass or more and less than 15% by mass. Therefore, the catalyst has high methane decomposition ability even under relatively low temperature conditions.

[0129] The method for producing a methane oxidation catalyst of the present invention can efficiently produce the above-mentioned methane oxidation catalyst.

[0130] The method for oxidizing methane of the present invention includes an oxidation step of contacting methane with the methane oxidation catalyst and oxidizing the methane, wherein the oxidation temperature in the oxidation step is 450° C. or lower. In other words, methane can be efficiently oxidized under relatively low temperature conditions.

[0131] The present invention will be described in more detail below with reference to examples and comparative examples. It should be noted that the present invention is in no way limited to these examples and comparative examples. The specific numerical values ​​of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the "Description of the Invention" above.

[0132] Example 1 <Preparation of methane oxidation catalyst> A palladium (II) nitrate solution (trade name: low-chlorine nitrate Pd solution, manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.), a tetraammine platinum (II) nitrate solution (trade name: tetraammine Pt nitrate solution, manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.), and ion-exchanged water were mixed together so that the mass ratio of palladium (Pd) to platinum (Pt) in the aqueous solution was 1:1, to obtain an aqueous solution (metal solution preparation step). Next, powdered 10% by mass CeO 2 / ZrO 2 (trade name: Z-3284, manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.) was added and mixed to prepare a slurry (slurry preparation step). 2 / ZrO 2 The amount of the active metals (Pd and Pt) blended is 100 parts by mass per 2 parts by mass of the total amount of the active metals (Pd and Pt). 2 / ZrO 2 contains 10 mass % ceria and 90 mass % zirconia, and the X-ray diffraction results shown in FIG. 1 indicate that the material is monoclinic zirconia (m-ZrO 2 ) phase and tetragonal ceria-zirconia (t-Ce X Zr1-X O2) phase. That is, 10 mass % CeO 2 / ZrO 2 contains zirconia alone and ceria-zirconia composite oxide.

[0133] The prepared slurry was then stirred at room temperature for 16 hours and then dried at 110°C to obtain a powder. This powder was then calcined at 500°C for 9 hours to obtain a methane oxidation catalyst. The catalyst was then compressed and crushed, and sieved to separate powders (methane oxidation catalysts) with particle sizes of 16 to 31 mesh (0.5 to 1.00 mm). In this manner, the powdered methane oxidation catalyst of Example 1 (catalyst carrier: 10 mass% CeO 2 / ZrO 2 , active metal: 1.0 part by mass Pd + 1.0 part by mass Pt) was prepared.

[0134] Example 2 A methane oxidative decomposition catalyst (catalyst support: 10 mass% CeO 2 / ZrO 2 , active metal: 4.0 parts by mass Pd + 1.0 parts by mass Pt) was obtained.

[0135] Comparative Example 1 In the slurry preparation step, powdered ZrO 2 The methane oxidative decomposition catalyst of Comparative Example 1 (catalyst carrier: ZrO 2 , active metal: 1.0 part by mass Pd + 1.0 part by mass Pt) was obtained.

[0136] Comparative Example 2 In the slurry preparation step, powdered 20 mass % CeO was added to the aqueous solution prepared in the metal solution preparation step. 2 / ZrO 2The methane oxidative decomposition catalyst of Comparative Example 2 (catalyst carrier: 20 mass % CeO 2 / ZrO 2 , active metal: 1.0 mass part Pd + 1.0 mass part Pt) was obtained. 2 / ZrO 2 contains 20 mass % ceria and 80 mass % zirconia, and the results of X-ray diffraction shown in FIG. 1 indicate that it is tetragonal ceria-zirconia (t-Ce X Zr 1-X O2) phase. That is, 20 mass % CeO 2 / ZrO 2 contains ceria-zirconia composite oxide and does not contain zirconia alone.

[0137] Comparative Example 3 In the slurry preparation step, powdered 70 mass % CeO 2 / ZrO 2 The methane oxidative decomposition catalyst of Comparative Example 3 (catalyst carrier: 70 mass % CeO 2 / ZrO 2 , active metal: 1.0 mass part Pd + 1.0 mass part Pt) was obtained. 2 / ZrO 2 contains 70 mass % of ceria and 30 mass % of zirconia, and the results of X-ray diffraction shown in FIG. 1 indicate that it is tetragonal ceria-zirconia (t-Ce X Zr 1-X O2) phase. That is, 70 mass % CeO 2 / ZrO 2 contains ceria-zirconia composite oxide and does not contain zirconia alone.

[0138] Comparative Example 4 In the slurry preparation step, powdered 20 mass % CeO 2 / ZrO 2The methane oxidative decomposition catalyst of Comparative Example 4 (catalyst carrier: 20 mass % CeO 2 / ZrO 2 , active metal: 4.0 parts by mass Pd + 1.0 parts by mass Pt) was obtained.

[0139] Comparative Example 5 In the slurry preparation step, powdery 70 mass % CeO 2 / ZrO 2 The methane oxidative decomposition catalyst of Comparative Example 5 (catalyst carrier: 70 mass % CeO 2 / ZrO 2 , active metal: 4.0 parts by mass Pd + 1.0 parts by mass Pt) was obtained.

[0140] <Evaluation> [Evaluation of X-ray diffraction pattern (catalyst carrier)] The catalyst carrier (ZrO 2 , 10% by mass CeO 2 / ZrO 2 , 20% by mass CeO 2 / ZrO 2 , and 70 mass% CeO 2 / ZrO 2 ) powder sample was analyzed by X-ray diffraction (XRD) in the same manner as above, and monoclinic zirconia (m-ZrO 2 ) phase peak and tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 The 2θ at the peak top of the peak of the monoclinic zirconia (m-ZrO 2 ) phase peak and tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 The 2θ angles at the peak tops of the peaks of the 2-phase are shown in Table 1. The conditions were as follows:

[0141] {Measurement conditions} X-ray source: CuKα ray (λ=1.54815 Å, Ni filter, applied power: 40 kV, 40 mA) Scanning range: 5° to 90° (2θ range) Scanning speed: 5.0° / min Sampling width: 0.01° Divergence slit: 0.20 mm Divergence vertical limiting slit: 2 mm Scattering slit: 2° Receiving slit: 0.15 mm Offset angle: 0°

[0142] The analysis was performed using analysis software (PDXL 2 (Version 2.7.2.0), manufactured by Rigaku Corporation). 2 The angle 2θ of the peak of the m-ZrO phase was calculated by the analysis software. 2 The diffraction angle of the (-111) plane is the angle at which the tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 The angle 2θ of the peak of the t-Ce phase is calculated by the analysis software. X Zr 1-X O 2 This is the angle at which the (101) plane diffracts.

[0143] [Evaluation of X-ray diffraction patterns (methane oxidation catalyst)] Powder samples of the methane oxidation catalysts of each Example and Comparative Example were subjected to X-ray diffraction (XRD) analysis. 2 ) phase peaks and tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 The 2θ at the peak top of the peak of the monoclinic zirconia (m-ZrO) phase was measured. For the measurement, an X-ray diffractometer (Uitima IV, manufactured by Rigaku Corporation) and an X-ray detector (D / teX Ultra, manufactured by Rigaku Corporation) were used to analyze the crystal structure by the Bragg-Brentano method. The graph of the XRD pattern is shown in Figure 2. 2 ) phase peak and tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2The 2θ angles at the peak tops of the peaks of the ) phase are shown in Table 2. The equipment, measurement conditions, analysis methods, etc. used for the measurement were the same as those used for the evaluation of the X-ray diffraction pattern (catalyst carrier) described above.

[0144] [Evaluation of Methane Oxidation Catalyst Performance] A methane oxidation test was carried out on the methane oxidation catalysts of each Example and Comparative Example, and the methane oxidation rates at 350°C, 375°C and 400°C were determined as catalytic performance.

[0145] Specifically, first, a methane oxidation test was carried out at six temperatures (at intervals of 30 to 40°C) selected from the range of 290 to 460°C, and the methane oxidation rate was measured.

[0146] In the methane oxidation test, a fixed-bed reactor was first filled with a methane oxidation catalyst (mass: 1.0 g, volume: 1.1 mL), and the reactor filled with the methane oxidation catalyst was placed in the middle of the flow path of the test gas, which was a methane-containing gas. Next, the test gas was heated to a predetermined temperature (the temperature at the six points mentioned above) and then supplied to the reactor through the reactor supply port. The composition of the test gas is shown below (note that the methane (CH 4 The methane concentration is the methane concentration before contact with the methane oxidation catalyst. Other conditions were a temperature in the reactor of 400°C, a flow rate of the test gas of 1.09 NL / min, and a gas hourly space velocity (GHSV) of 59,454 h -1 The gas space velocity is the flow rate of the test gas (Nm 3 / h) to the catalyst volume (m 3 ) and then divided by the methane concentration at the reactor outlet. Under these conditions, the test gas was passed through the fixed-bed reactor and contacted with the methane oxidation catalyst, and the methane concentration at the reactor outlet was measured. A gas chromatography system (GC-8A, manufactured by Shimadzu Corporation) equipped with a thermal conductivity detector (TCD) was used to quantify the methane concentration. The measurement conditions are shown below. The methane oxidation rate, expressed by the following formula, was then calculated from the methane concentrations at the reactor inlet and the reactor outlet.

[0147] {Test gas composition} CH 4 Concentration: 1000 ppmv-dry (methane concentration at reactor inlet) O 2 Concentration: 12% by volume - wet H2 O concentration: 8% by volume 2 Density: Balance

[0148] {Measurement conditions for gas chromatography system with TCD} Column: Dual packed column "Shincarbon-ST 50 / 80 mesh" (manufactured by Shinwa Chemical Industry Co., Ltd.) 2.0 m x 3 Carrier gas: He gas (flow rate 50 NmL / min) Column temperature: 180°C Detector temperature: 140°C

[0149] Methane oxidation rate (%) = (methane concentration at reactor inlet - methane concentration at reactor outlet) / (methane concentration at reactor inlet) x 100

[0150] Next, the methane oxidation rate calculated by the above formula is substituted into the following formula (1) to obtain the reaction rate constant k (h -1 ) was calculated. GHSV in equation (1) is the gas hourly space velocity. In this way, the reaction rate constant k(h -1 ) was sought.

[0151] k = -GHSV × ln(1 - methane oxidation rate (%) / 100) (1)

[0152] Next, based on the reaction rate constant k at the six temperatures, the Arrhenius equation for the methane oxidation reaction when using the methane oxidation catalysts of each Example and Comparative Example was determined by the Arrhenius plot method, and the reaction rate constant k (h) at 350°C was determined in the Arrhenius equation. -1 The results are shown in Table 2.

[0153] Furthermore, from the Arrhenius equation for the methane oxidation reaction when the methane oxidation catalysts of each Example and Comparative Example calculated above are used, the reaction rate constant k (h -1 ) was also calculated, and the reaction rate constant k(h -1 ) and the above formula (1), the methane oxidation rates (%) at 350° C., 375° C. and 400° C. were calculated. The results are shown in Table 3.

[0154]

[0155]

[0156]

[0157] <Discussion> As shown in Figures 1 and 2, the methane oxidation catalysts of Examples 1 and 2 and their catalyst carriers (10 mass % CeO 2 / ZrO 2 ) is monoclinic zirconia (m-ZrO 2 ) phase peak and tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 In other words, it was suggested that in the methane oxidation catalysts of Examples 1 and 2, part of the zirconia in the catalyst support formed a tetragonal ceria-zirconia composite oxide, while the remaining zirconia solely formed monoclinic zirconia.

[0158] On the other hand, as shown in Figures 1 and 2, the methane oxidation catalyst of Comparative Example 1 and its catalyst support (ZrO 2 ) is monoclinic zirconia (m-ZrO 2 In other words, the catalyst support in the methane oxidation catalyst of Comparative Example 1 does not contain tetragonal ceria-zirconia composite oxide.

[0159] 1 and 2, the methane oxidation catalysts of Comparative Examples 2 to 5 and their catalyst supports (20 mass % CeO 2 / ZrO 2 and 70 mass% CeO 2 / ZrO 2 ) is a tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 ) phase. This suggests that the catalyst supports in the methane oxidation catalysts of Comparative Examples 2 to 5 form tetragonal ceria-zirconia composite oxide, but do not form monoclinic zirconia alone. Note that the methane oxidation catalysts of Comparative Examples 2 and 4 (catalyst supports containing 20 mass % CeO 2 / ZrO 2 The tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O2 ) phase has a peak position at around 2θ = 30°, and t-ZrO 2 In contrast, the methane oxidation catalysts of Comparative Examples 3 and 5 (catalyst carriers containing 70 mass % CeO 2 / ZrO 2 The tetragonal ceria-zirconia composite oxide (t-Ce X Zr 1-X O 2 ) phase has a peak position at 2θ = 29°, and compared with Comparative Example 2 and Comparative Example 4, 2 It can be seen that the crystalline state of

[0160] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.

[0161] The methane oxidation catalyst and methane oxidation method of the present invention can be used to remove unburned methane contained in methane-containing exhaust gas discharged from LNG-fueled ships, and can also be used to remove methane contained in methane-containing gas produced in processes such as gas-phase reactions in chemical plants. Furthermore, the method for producing the methane oxidation catalyst of the present invention can efficiently produce methane oxidation catalysts for such applications.

Claims

1. A catalyst for oxidizing methane, comprising: a catalyst support containing a ceria-zirconia composite oxide; and an active metal supported on the catalyst support and containing Pd and Pt, wherein the ceria content in the catalyst support is 5 mass% or more and less than 15 mass%.

2. The methane oxidation catalyst according to claim 1, wherein the content of Pd in ​​the active metals is 50 mass% or more.

3. The methane oxidation catalyst according to claim 1, wherein the amount of the active metal is 5 parts by mass or less per 100 parts by mass of the catalyst support.

4. The methane oxidation catalyst according to claim 1, wherein the catalyst support further contains zirconia, the zirconia contains a monoclinic zirconia phase, and the ceria-zirconia mixed oxide contains a tetragonal ceria-zirconia phase.

5. A method for producing a methane oxidation catalyst comprising: a first step of mixing a catalyst support raw material containing a ceria-zirconia composite oxide with a solution of active metals containing Pd and Pt to prepare a slurry; a second step of drying the slurry to obtain a powder; and a third step of firing the powder at 400°C or higher and 600°C or lower to obtain the methane oxidation catalyst according to any one of claims 1 to 4, wherein in the first step, the ceria content in the catalyst support raw material is 5 mass% or higher and less than 15 mass%.

6. A method for oxidizing methane, comprising an oxidation step of contacting methane with the methane oxidation catalyst according to any one of claims 1 to 4 and oxidizing the methane, wherein the oxidation step is carried out at an oxidation temperature of 450°C or lower.

Citation Information

Patent Citations

  • Catalyst

    JP2005270882A

  • Catalyst for purifying exhaust gas and preparation thereof

    JP1990043951A

  • Harmful substance cleaning catalyst and its manufacturing process

    JP2004148173A

  • Three-way catalyst and methane-containing gas cleaning method using the same

    JP2006181569A

  • Catalyst for oxidizing and removing methane in exhaust gas and method for oxidizing and removing methane in exhaust gas

    JP2007090331A