Joining material and method for producing joining body
A bonding material with spherical metal particles and a solvent achieves dense sintering with minimal pores at low pressures, addressing porosity and thermal stress issues in existing technologies, and ensuring the reliability and stability of bonded portions.
Patent Information
- Application Number
- PCT/JP2024/015619
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing bonding materials containing silver or copper particles face issues with porosity when sintered at low pressures, leading to thermal stress and reduced thermal conductivity, and high-pressure methods risk damaging semiconductor chips or requiring frequent maintenance.
A bonding material comprising substantially spherical metal particles with specific particle size distributions and a solvent, allowing for the formation of a dense sintered film with minimal pores even at low pressures, suppressing cracking and porosity formation.
The solution effectively reduces porosity and cracking in bonded portions, enhancing thermal shock resistance and reliability while avoiding damage to semiconductor chips and reducing maintenance needs.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000042_0000
Abstract
Description
Bonding material and method for manufacturing bonded body
[0001] The present invention relates to a bonding material and a method for manufacturing a bonded body. This application claims priority to Japanese Patent Application No. 2023-071339, filed on April 25, 2023, the contents of which are incorporated herein by reference.
[0002] Silver and copper, with their high thermal conductivity and high melting points, are considered promising materials for joining conductive components as an alternative to solder. Silver and copper are particularly promising as packaging materials for power semiconductors, which have high heat density. However, when using a joining material containing silver or copper particles, the joining material is typically sintered at temperatures below the melting points of these metals to join conductive components (in other words, sintered diffusion bonding). Therefore, the joint formed by sintering becomes porous, containing many voids within. However, when the operating temperature of the semiconductor fluctuates significantly, thermal stress occurs at the joint, and these voids become a concentration source, causing the joint to break. Furthermore, the presence of voids reduces the thermal conductivity of the joint. Therefore, it is preferable to have fewer voids within the joint.
[0003] In contrast, to form a dense sintered film with few voids, a method is usually adopted in which the bonding material is heated while simultaneously pressurizing the laminate of the conductive parts and the bonding material in the stacking direction. As a method for forming such a sintered film, for example, a method has been disclosed in which a bonding material containing silver nanoparticles (particle diameter 20 nm) is used to heat a laminate of the conductive parts and the bonding material at 300 °C while pressing it at a pressure of 60 MPa to form a sintered film with a porosity of approximately 2.5%. It has also been disclosed that a sintered film with a porosity of approximately 8% was formed using a bonding material containing silver nanoparticles (particle diameter 18 nm), silver submicron particles (particle diameter 150 nm), and silver microparticles (particle diameter 5063 nm) (see Non-Patent Document 1). Thus, a bonded body obtained by bonding conductive parts using a bonding material containing silver nanoparticles has the advantage of high thermal shock test resistance and high reliability.
[0004] Degradation Mechanism of Pressure-Assisted Sintered Silver by Thermal Shock Test, Energy 2021, 14, 5532
[0005] However, in the method described in Non-Patent Document 1, applying pressure as high as 60 MPa poses the risk of cracking the semiconductor chip or deforming the substrate, and furthermore, the press used during application of pressure requires frequent maintenance. To avoid these problems, it is necessary to limit the pressure during application to 20 MPa or less, but Non-Patent Document 1 does not disclose such a means. Furthermore, in the method described in Non-Patent Document 1, when the thickness of the bonded portion (sintered film) is increased, particularly when the thickness is increased to 100 μm or more, cracks may be more likely to occur due to shrinkage of the dried material when the bonding material is dried during the bonding portion formation process.
[0006] The present invention addresses the problem of providing a bonding material for forming a joint that joins conductive parts together, which can suppress cracking when forming a joint from the bonding material even if the dried bonding material is thick, and can form a joint with few voids even when the dried bonding material is fired while being pressurized at a low pressure of about 20 MPa or less.
[0007] In order to solve the above problems, the present invention employs the following configurations. [1] A bonding material for bonding conductive parts, comprising metal particles including substantially spherical metal particles (A) and a solvent for dispersing the metal particles, wherein the metal particles (A) have a particle diameter D50 of 0.3 to 0.5 μm at 50% cumulative volume as measured by laser diffraction / scattering particle size distribution measurement, and the minimum particle diameter Dmin of the metal particles (A) is greater than 0.08 μm. [2] The bonding material according to [1], wherein the metal particles include metal particles (B) different from the metal particles (A), and the minimum particle diameter Dmin of the metal particles (B) is greater than 0.08 μm as measured by laser diffraction / scattering particle size distribution measurement. [3] The bonding material according to [1] or [2], wherein the solvent further contains a resin component which is a curable resin, a non-curable resin, or a thermoplastic resin, and the ratio of the content of the resin component to the content of the metal particles in the bonding material is less than 0.01% by mass. [4] The bonding material according to [1] or [2], wherein the solvent does not contain a resin component which is a curable resin, a non-curable resin, or a thermoplastic resin. [5] The bonding material according to any one of [1] to [4], wherein the particle diameter D90 of the metal particles (A) at 90% accumulation on a volume basis, measured by laser diffraction / scattering particle size distribution measurement, is less than 0.8 μm. [6] The bonding material according to any one of [1] to [5], wherein the metal particles (A) and the metal particles (B) are both silver particles. [7] The specific surface area of the metal particles (A) is 0.95 to 1.5 m. 2 The bonding material according to any one of [1] to [6], wherein the bonding strength is in the range of / g.
[0008] [8] A method for manufacturing a bonded body in which a conductive first component and a conductive second component are bonded via a conductive bonding portion, the method comprising the steps of: applying the bonding material according to any one of [1] to [7] to a first surface of the first component or a second surface of the second component; drying the applied bonding material to form a dried bonding material; stacking the first component and the second component with the dried bonding material interposed therebetween to form a laminate; and firing the dried bonding material in the laminate at a temperature higher than the temperature at which the bonding material was dried to form the bonded portion from the dried bonding material. [9] A method for manufacturing the bonded body according to [8], in which a thickness of the bonded portion is 100 μm or more.
[0009] According to the present invention, there is provided a bonding material for forming a joint that joins conductive parts together, which can suppress cracking when forming a joint from the bonding material even if the dried bonding material is thick, and can form a joint with few voids even when the dried bonding material is fired while being pressurized at a low pressure of about 20 MPa or less.
[0010] 2B. A diagram illustrating a firing step following the step of FIG. 2C. A diagram illustrating a bonded body after the step of FIG. 2E. A diagram illustrating a drying step following the step of FIG. 3A. A diagram illustrating a firing step following the step of FIG. 3B. A diagram illustrating a bonded body after the step of FIG. 3E. A diagram illustrating an SEM image of metal particles (A)-1 used in Example 1. A diagram illustrating an SEM image of metal particles (A)-1 used in Example 2. A diagram illustrating an SEM image of metal particles (B)-1 used in Comparative Example 1. 1 shows image data obtained by SEM of metal particles (B)-2 used in Comparative Example 2. FIG. 2 shows image data obtained by SEM of metal particles (B)-3 used in Comparative Example 3.
[0011] Bonding Material A bonding material according to one embodiment of the present invention comprises metal particles including substantially spherical metal particles (A) and a solvent for dispersing the metal particles. The particle diameter D50 of the metal particles (A) at 50% cumulative volume, as measured by laser diffraction / scattering particle size distribution measurement, is 0.3 to 0.5 μm, and the minimum particle diameter Dmin of the metal particles (A) is greater than 0.08 μm. This configuration allows cracking of the dried bonding material, which is the dried product of the bonding material, to be suppressed when forming a bonded joint, even if the dried bonding material is thick. Furthermore, in a laminate obtained by stacking conductive components together via the dried bonding material, a bonded joint with few voids can be formed even when the dried bonding material is fired under pressure at a low pressure of approximately 20 MPa or less.
[0012] The bonding material of this embodiment will be described below. Note that in the bonding material, the ratio of the total content of one or more components contained in the bonding material, which will be described later, to the total mass of the bonding material does not exceed 100 mass%.
[0013] <<Metal Particles>> In this embodiment, the metal particles contained in the bonding material include at least metal particles (A). As will be described in detail later, the metal particles may further include metal particles (B). The metal particles (A) have a substantially spherical shape. In this specification, the term "substantially spherical" refers not only to the metal particles (A) but also to a spherical or spherical-like shape. More specifically, it refers to a particle shape having an aspect ratio calculated by [major axis of particle] / [minor axis of particle] of 2 or less. The aspect ratio is preferably 1.6 or less, and more preferably 1.3 or less. The surface of the substantially spherical particles may be composed of only curved surfaces, or may have flat surfaces, or may have corners formed by two flat surfaces connected at a predetermined angle to each other. The surface of the substantially spherical particles may be smooth or may have irregularities. As the metal particles (A), any commercially available spherical or substantially spherical shape can be used as long as it satisfies the above particle size requirements.
[0014] The metal species of the metal particles (A) preferably has high thermal conductivity and a high melting point. For example, the thermal conductivity (e.g., bulk thermal conductivity) of the metal species of the metal particles (A) is preferably 350 W / mK or higher, and may be 350 to 450 W / mK. This allows heat to be quickly released, for example, even when the heat generation temperature of a semiconductor or the like in contact with the bonding material becomes high (e.g., 150°C or higher). For example, the melting point of the metal species of the metal particles (A) is preferably 900°C or higher, and may be 900 to 1100°C.
[0015] The metal species of the metal particles (A) contained in the bonding material may be one kind or two or more kinds, and when there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.
[0016] Among these, the metal species of the metal particles (A) is preferably silver or copper, and more preferably silver. That is, the metal particles (A) are preferably silver particles or copper particles, and more preferably silver particles. Note that the metal species of the metal particles (A) is not limited to pure silver or pure copper, and may be a silver alloy or a copper alloy.
[0017] Among the metal particles (A), silver particles include, for example, silver particles obtained by a reduction method and silver particles obtained by an atomization method. The silver particles may be surface-treated products whose surfaces have been chemically treated (treated with chemical substances), or may be surface-untreated products whose surfaces have not been chemically treated. Usually, silver particles obtained by a reduction method are surface-treated products, and silver particles obtained by an atomization method are surface-untreated products.
[0018] <Particle Size Distribution of Metal Particles> In this embodiment, the particle size distribution of the metal particles was measured by laser diffraction / scattering particle size distribution measurement. Hereinafter, the minimum particle size of the metal particles measured by laser diffraction / scattering particle size distribution measurement will be referred to as "Dmin," the particle size at 10% cumulative volume of the metal particles will be referred to as "D10," the particle size at 50% cumulative volume of the metal particles will be referred to as "D50," the particle size at 90% cumulative volume of the metal particles will be referred to as "D90," and the maximum particle size of the metal particles will be referred to as "Dmax."
[0019] The D50 of the metal particles (A) is 0.3 to 0.5 μm, and may be, for example, any one of 0.3 to 0.4 μm, 0.45 to 0.5 μm, and 0.35 to 0.45 μm. When the D50 is equal to or greater than the lower limit, the effect of suppressing cracking of the dried bonding material is enhanced even if the dried bonding material is thick. When the D50 is equal to or less than the upper limit, the effect of forming a bonding portion with fewer voids is enhanced even if the dried bonding material is fired while being pressurized at a low pressure.
[0020] The Dmin of the metal particles (A) is greater than 0.08 μm, and the bonding material does not need to contain metal particles (A) whose particle diameter is 0.08 μm or less. In other words, when the particle diameter of the metal particles (A) is measured on a volume basis by, for example, laser diffraction / scattering particle size distribution measurement, no particles having a particle diameter of 0.08 μm or less are observed. By using such metal particles (A), cracking of the dried bonding material can be suppressed even if the dried bonding material is thick.
[0021] The Dmin of the metal particles (A) is preferably greater than 0.08 μm and 0.09 μm or greater, and may be, for example, 0.12 μm or greater, or 0.15 μm or greater. Having a Dmin in this range enhances the effect of suppressing cracking of the dried bonding material, even when the dried bonding material is thick. On the other hand, the Dmin is preferably 0.21 μm or less. Such metal particles (A) are easier to prepare and readily available. For example, particles with a D50 in the range of 0.3 to 0.5 μm and a Dmin greater than 0.21 μm (i.e., particles with a narrow particle size distribution) may be difficult to manufacture. In one embodiment, the Dmin may be, for example, greater than 0.08 μm and 0.21 μm or less, 0.09 to 0.21 μm, 0.12 to 0.21 μm, or 0.15 to 0.21 μm. However, these are just examples of Dmin.
[0022] The D90 of the metal particles (A) is not particularly limited, but is preferably less than 0.8 μm, more preferably 0.78 μm or less, and may be, for example, 0.72 μm or less, or 0.65 μm or less. Having a D90 in this range enhances the effect of forming a bonded joint with fewer voids, even when the dried bonding material is fired under low pressure. On the other hand, D90 is preferably 0.45 μm or more. Such metal particles (A) are easier to prepare and are readily available. For example, particles with a D50 in the range of 0.3 to 0.5 μm and a D90 smaller than 0.45 μm (i.e., particles with a narrow particle size distribution) may be difficult to manufacture. In one embodiment, D90 may be, for example, any one of 0.45 μm or more and less than 0.8 μm, 0.45 to 0.78 μm, 0.45 to 0.72 μm, and 0.45 to 0.65 μm, although these are just examples of D90.
[0023] The D10 of the metal particles (A) is not particularly limited, but is preferably 0.18 μm or more, and may be, for example, 0.24 μm or more, or 0.3 μm or more. Having a D10 in this range enhances the effect of suppressing cracking of the dried bonding material, even if the dried bonding material is thick. On the other hand, D10 is preferably 0.34 μm or less. Such metal particles (A) are easier to prepare and are readily available. This is because, as described above, particles with a narrow particle size distribution may be more difficult to manufacture. In one embodiment, D10 may be, for example, 0.18 to 0.34 μm, 0.24 to 0.34 μm, or 0.3 to 0.34 μm. However, these are just examples of D10.
[0024] The Dmax of the metal particles (A) is preferably 2 μm or less. In other words, when the particle size of the metal particles (A) is measured on a volume basis by, for example, laser diffraction / scattering particle size distribution measurement, it is preferable that no particles with a particle size greater than 2 μm are observed. Furthermore, the Dmax may be, for example, 1.85 μm or less, or 1.7 μm or less. With a Dmax in this range, the effect of forming a bonded portion with fewer voids is enhanced even when the dried bonding material is fired under low pressure. On the other hand, the Dmax is preferably 1.5 μm or more. Such metal particles (A) are easier to prepare and are readily available. This is because, as described above, particles with a narrow particle size distribution may be more difficult to manufacture. In one embodiment, the Dmax may be, for example, 1.5 to 2 μm, 1.5 to 1.85 μm, or 1.5 to 1.7 μm. However, these are just examples of Dmax.
[0025] The specific surface area of the metal particles (A) is not particularly limited, but is preferably 0.8 to 1.7 m 2 / g, for example, 0.8 to 1.3 m 2 / g, 1.1-1.7m 2 / g, and 1.1 to 1.3 m 2 When the specific surface area of the metal particles (A) is in this range, the bonding material has a viscosity that is more suitable for application of adhesion means such as printing or coating.
[0026] The specific surface area of particles, including metal particles (A), can be measured by known methods such as a permeation method and a gas adsorption method using gas molecules such as nitrogen.
[0027] In the bonding material, the ratio of the content of the metal particles (A) to the total mass of the bonding material ([content of metal particles (A) in bonding material (parts by mass)] / [total mass of bonding material (parts by mass)]×100) is preferably 60 to 93 mass%, and may be, for example, 70 to 93 mass% or 80 to 93 mass%. When the ratio is equal to or greater than the lower limit, the bonding portion can be formed more efficiently. When the ratio is equal to or less than the upper limit, the fluidity of the bonding material is increased, and the handling of the bonding material is improved.
[0028] <<Solvent>> The bonding material contains a solvent, which gives the bonding material fluidity and good handleability. The bonding material is typically in a paste or liquid form.
[0029] In this specification, unless otherwise specified, the term "solvent" is a concept that encompasses both a component that is liquid at room temperature and that dissolves a solute, and a component that is liquid at room temperature and that functions as a dispersion medium for dispersing a dispersoid. In this specification, "room temperature" means a temperature that is not particularly cooled or heated, that is, an ordinary temperature, and examples thereof include a temperature of 15 to 25°C.
[0030] The solvent is not particularly limited as long as it can be removed (vaporized) under heating conditions, and it is preferable that the solvent does not have reactivity with components other than the solvent, such as the metal particles (A) in the bonding material. Examples of the solvent include aromatic hydrocarbons such as toluene, o-xylene, m-xylene, and p-xylene; aliphatic hydrocarbons such as pentane, hexane, cyclohexane, heptane, octane, cyclooctane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, and decahydronaphthalene; halogenated hydrocarbons such as dichloromethane and chloroform; alcohols such as hexanol (e.g., 1-hexanol), heptanol (e.g., 1-heptanol), octanol (e.g., 1-octanol), nonanol (e.g., 1-nonanol), decanol (e.g., 1-decanol), benzyl alcohol, cyclohexanol, and terpineol (also known as terpineol); esters such as ethyl acetate, monomethyl glutarate, and dimethyl glutarate; ethers such as diethyl ether, tetrahydrofuran (THF), and 1,2-dimethoxyethane (dimethyl cellosolve); and propylene glycol monomethyl Examples of suitable alcohol ethers (compounds having both a hydroxyl group and an ether bond in one molecule) include alcohol ethers (also known as 1-methoxy-2-propanol), 3-methoxy-3-methyl-1-butanol, and butyl carbitol (also known as diethylene glycol monobutyl ether); ketones such as acetone, methyl ethyl ketone (MEK), cyclohexanone, 2-octanone, and diisobutyl ketone (also known as 2,6-dimethyl-4-heptanone); hydroxyketones such as diacetone alcohol (also known as 4-hydroxy-4-methyl-2-pentanone); enones such as isophorone (also known as 3,5,5-trimethylcyclohex-2-en-1-one); nitriles such as acetonitrile; amides such as N,N-dimethylformamide (DMF) and N,N-dimethylacetamide; and alcohol esters (compounds having both a hydroxyl group and an ester bond in one molecule) such as texanol (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate).
[0031] The bonding material may contain only one type of solvent, or two or more types of solvents. When two or more types of solvents are contained, the combination and ratio thereof can be selected arbitrarily.
[0032] In the bonding material, the ratio of the solvent content to the total mass of the bonding material ([solvent content (parts by mass) of bonding material] / [total mass (parts by mass) of bonding material]×100) is preferably 7 to 40 mass%, and may be, for example, 7 to 30 mass% or 7 to 20 mass%. When the ratio is equal to or greater than the lower limit, the fluidity of the bonding material becomes higher, and the handleability of the bonding material becomes higher. When the ratio is equal to or less than the upper limit, the content of metal particles (A) in the bonding material can be increased, and the bonded portion can be formed more efficiently.
[0033] <<Other Components>> The bonding material may or may not contain other components that do not fall under either the metal particles (A) or the solvent, as long as the effects of the present invention are not impaired. The other components are not particularly limited as long as the effects of the present invention are not impaired, and can be selected as desired depending on the purpose.
[0034] The bonding material may contain only one type of other component, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.
[0035] Examples of the other components contained in the bonding material include metal particles (B) other than the metal particles (A) and a resin component. That is, the bonding material may further contain either or both of the metal particles (B) and the resin component.
[0036] <Metal Particles (B)> The metal particles (B) are different from the metal particles (A). In this embodiment, the metal particles (A) and the metal particles (B) being different from each other means, for example, that the metal species, particle size distribution, or shape of the two types of metal particles are different from each other. For example, when the metal species of the metal particles (A) is silver, the metal species of the metal particles (B) may be a metal species other than silver (e.g., copper). When the shape of the metal particles (A) is approximately spherical, the shape of the metal particles (B) may be other than approximately spherical (e.g., plate-like). The particle size distributions of the two types of metal particles being different from each other include cases where the D50s are different from each other and cases where the spreads of the particle size distributions are different from each other. When the D50s are different from each other, the particle size distribution of the mixture obtained by mixing the two types of particles will have two peak particle size portions. Furthermore, even if the D50 of two types of particles is the same, cases where the particle size distribution spreads of the two types of metal particles are different are also included in the "cases where the particle size distributions of metal particles (A) and metal particles (B) are different." The case where the particle size distribution spreads of two types of metal particles are different refers to, for example, cases where at least one of Dmin, D10, D90, or Dmax is different from each other. That is, cases where the particle size distribution spread of two types of particles mixed is different from the tail spread of a single type of particle size distribution. The Dmin of metal particles (B) is greater than 0.08 μm, and the bonding material does not need to contain metal particles (B) with a particle size of 0.08 μm or less. In other words, when the particle size of metal particles (B) is measured on a volume basis using, for example, laser diffraction / scattering particle size distribution measurement, no particle size of 0.08 μm or less is observed.
[0037] The metal particles (B) are not particularly limited as long as they satisfy the above conditions. Examples of the metal species of the metal particles (B) include the same metal species as those of the metal particles (A). Examples of the metal particles (B) include metal particles having a shape other than a substantially spherical shape; substantially spherical metal particles having a D50 of less than 0.3 μm; and substantially spherical metal particles having a D50 of more than 0.5 μm. A representative example of the shape of the metal particles (B) other than a substantially spherical shape is a plate shape.
[0038] In this specification, the term "plate-like" refers to a metal particle having two main surfaces, and the shape of the main surfaces is an approximately polygonal shape such as a substantially triangular shape (a triangular shape or a shape that can be considered to be a triangular shape), a substantially pentagonal shape (a pentagonal shape or a shape that can be considered to be a pentagonal shape), or a substantially hexagonal shape (a hexagonal shape or a shape that can be considered to be a hexagonal shape), or an irregular shape that can be considered to be a polygonal shape with some sides or corners missing. The thickness of the plate (i.e., the width between the two main surfaces, i.e., the thickness of the plate in the direction perpendicular to the main surfaces) is 40 nm or less, and the maximum length of the two main surfaces (in other words, the particle diameter) is 10 to 1000 nm. The aspect ratio of the plate-like metal particles (= [maximum length of the main surfaces (particle diameter)] / [width between the main surfaces]) is 3 or more.
[0039] The metal species of the metal particles (B) contained in the bonding material may be one kind or two or more kinds, and when there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.
[0040] The metal species of the metal particles (B) is preferably silver or copper, and is preferably silver. Note that the metal species of the metal particles (B) is not limited to pure silver or pure copper, and may be a silver alloy or a copper alloy. It is preferable that both the metal particles (A) and the metal particles (B) contained in the bonding material are silver particles.
[0041] In the bonding material, the ratio of the content of the metal particles (B) to the total mass of the bonding material ([content of metal particles (B) in bonding material (parts by mass)] / [total mass of bonding material (parts by mass)]×100) is preferably 1 mass% or less, and may be, for example, 0.5 mass% or less, 0.3 mass% or less, or 0.1 mass% or less. When the ratio is equal to or less than the upper limit, the effect obtained by using the metal particles (A) is further enhanced.
[0042] When the volume-based particle size of the metal particles in the bonding material is measured by laser diffraction / scattering particle size distribution measurement, if multiple peaks are observed in the particle size distribution, the presence of metal particles (B) can be confirmed. If the difference between the D50 of metal particles (B) and the D50 of metal particles (A) is relatively large, multiple peaks can be easily confirmed. When observing the bonding material with an SEM or the like, if metal particles having a shape other than a substantially spherical shape, such as a plate shape, are observed, the presence of metal particles (B) can be confirmed.
[0043] <Resin Component> The resin component can be selected arbitrarily depending on the purpose and is not particularly limited. The resin component may be, for example, either a curable resin or a non-curable resin, or a thermoplastic resin. The resin component may be dissolved in a solvent or dispersed in a solvent. The resin component may be a binder that contributes to bonding between metal particles or between a bonding material and an adherend, or may be spacer particles that are dispersed in a solvent and serve as spacers between metal particles. Note that resins provided on the surfaces of metal particles for chemically treating the surfaces of the metal particles are not included in the resin component of this embodiment.
[0044] It should be noted that it is not essential for the bonding material of this embodiment to contain a resin component (e.g., a binder or spacer particles). The lower the resin component content, the better. In the bonding material, the ratio of the resin component content to the total metal particle content ([resin component content (parts by mass) of the bonding material] / [total metal particle content (parts by mass) of the bonding material] × 100) is preferably less than 0.01% by mass, and may be 0.005% by mass or less. When the resin component is contained in an amount of less than 0.01% by mass, the resin component may reduce the porosity of the bonding material and suppress the occurrence of cracks. However, if the resin component remains in the fired bonding material, the remaining resin component may increase the porosity. For this reason, it is preferable that the resin component content of the bonding material be less than 0.01% by mass, or that the bonding material contain no resin component at all. Therefore, it can be said that the resin component content is preferably 0% by mass or more and less than 0.01% by mass. When the ratio is less than 0.01 mass % or when the dried bonding material does not contain a resin component, the effect of suppressing cracking of the dried bonding material even when the dried bonding material is thick and the effect of forming a bonding portion with fewer voids even when the dried bonding material is fired while being pressurized at a low pressure are further enhanced.
[0045] The resin component contained in the bonding material may be one type only, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.
[0046] In the bonding material, when the metal particles include metal particles (A) and metal particles (B), the ratio of the content of the resin component to the total content of the metal particles (A) and the metal particles (B) is [content of the resin component in the bonding material (parts by mass)] / [total content of the metal particles (A) and the metal particles (B) in the bonding material (parts by mass)] × 100. Even in this case, the content of the resin component may be less than 0.01% by mass, for example, 0.005% by mass or less. Here, when the bonding material does not contain metal particles (B), the content of the metal particles (B) in the bonding material is 0 parts by mass. Similarly, when the bonding material does not contain a resin component, the content of the resin component in the bonding material is 0 parts by mass.
[0047] The bonding material may contain, as the other component, a component (X) that does not fall into either the metal particles (B) or the resin component. In this case, the ratio of the content of the component (X) to the total mass of the bonding material ([content (parts by mass) of the component (X)] / [total mass (parts by mass) of the bonding material] × 100) is preferably 5% by mass or less, and may be, for example, 3% by mass or less or 1% by mass or less. When the ratio is equal to or less than the upper limit, the effect of suppressing cracking of the dried bonding material even when the dried bonding material is thick and the effect of forming a bonded portion with fewer voids even when the dried bonding material is fired under low pressure are enhanced. On the other hand, the content ratio of the component (X) is 0% by mass or more.
[0048] In the bonding material, the ratio of the total content of the metal particles (A) and the solvent to the total mass of the bonding material ([total content (parts by mass) of the metal particles (A) and the solvent in the bonding material] / [total mass (parts by mass) of the bonding material] × 100) is preferably 95% by mass or more, and may be, for example, 97% by mass or more or 99% by mass or more. When the ratio is equal to or more than the lower limit, the effect of suppressing cracking of the dried bonding material even if the dried bonding material is thick and the effect of forming a bonded portion with fewer pores even when the dried bonding material is fired while being pressurized at a low pressure are enhanced. On the other hand, the ratio of the total content of the metal particles (A) and the solvent to the total mass of the bonding material is 100% by mass or less.
[0049] As described above, the bonding material according to this embodiment includes metal particles (A) containing substantially spherical metal particles and a solvent for dispersing the metal particles. The particle diameter D50 of the metal particles (A) at 50% cumulative volume, as measured by laser diffraction / scattering particle size distribution measurement, is 0.3 to 0.5 μm, and the minimum particle diameter Dmin of the metal particles (A) is greater than 0.08 μm. In this configuration, since D50 is in the range of 0.3 to 0.5 μm, cracking of the dried bonding material can be suppressed even when the dried bonding material is thick. Furthermore, even when the dried bonding material is fired under pressure at a low pressure of approximately 20 MPa or less, a bonded portion with few voids can be formed. Furthermore, since Dmin is greater than 0.08 μm, cracking of the dried bonding material can be suppressed even when the dried bonding material is thick. As a result, in a laminate in which the bonding material of this embodiment is sandwiched between conductive parts, even if the laminate is fired while being pressurized at a low pressure of about 20 MPa or less, a bonding portion with few voids can be formed.
[0050] The metal particles may include metal particles (B) different from the metal particles (A). The minimum particle size Dmin of the metal particles (B) measured by laser diffraction / scattering particle size distribution measurement is greater than 0.08 μm.
[0051] The solvent may further contain a resin component that is a curable resin, a non-curable resin, or a thermoplastic resin, and the ratio of the resin component content to the metal particle content in the bonding material may be less than 0.01 mass %. Alternatively, the bonding material may not contain a resin component that is a curable resin, a non-curable resin, or a thermoplastic resin in the solvent. This makes it possible to reduce the porosity of the bonding material and suppress the occurrence of cracks.
[0052] <<Method for manufacturing bonding material>> The bonding material of the present embodiment is obtained by blending metal particles (A), a solvent, and, if necessary, the other components. After blending the components, the resulting material may be used as is as a bonding material, or may be used as a bonding material after, if necessary, performing a known post-treatment or purification operation.
[0053] The order in which the components are mixed is not particularly limited. The method for mixing the components is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a three-roll mill, a kneader, a bead mill, or the like, and a method of mixing by applying ultrasound.
[0054] The temperature during blending of the components is not particularly limited as long as the components do not deteriorate, but is preferably 0 to 40° C. The blending time for the components is also not particularly limited as long as the components do not deteriorate, but is preferably 10 minutes to 12 hours.
[0055] ◇Method for Manufacturing a Bonded Body A method for manufacturing a bonded body according to one embodiment of the present invention is a method for manufacturing a bonded body configured by joining a conductive first part (sometimes simply referred to as a "first part" in this specification) and a conductive second part (sometimes simply referred to as a "second part" in this specification) via a conductive bonding portion (sometimes simply referred to as a "bonding portion" in this specification), and includes the steps of: attaching the bonding material according to the embodiment described above to a first surface of the first part or a second surface of the second part (sometimes referred to as an "attaching step" in this specification); drying the attached bonding material to form a dried bonding material (sometimes referred to as a "drying step" in this specification); stacking the first part and the second part via the dried bonding material to produce a laminate (sometimes referred to as a "stacking step" in this specification); and a step of forming the joint from the dried bonding material by firing the dried bonding material in the laminate at a temperature higher than the temperature at which the bonding material was dried (sometimes referred to as a "firing step" in this specification).
[0056] The conductive parts such as the first part and the second part are not particularly limited as long as they are conductive. Examples of the conductive parts include metal parts (metal members). The metal parts may be, for example, metal layers formed by sputtering or plating on the surface of a semiconductor chip or semiconductor element such as a silicon chip, or may be metal layers such as electrodes formed on a resin substrate or a ceramic substrate.
[0057] The bonding portion is formed using the bonding material according to the embodiment described above and is a metal sintered body. For example, when the bonding material contains silver particles as the metal particles (A), the metal sintered body is a silver sintered body, and when the bonding material contains copper particles as the metal particles (A), the metal sintered body is a copper sintered body. The bonding portion has electrical conductivity and thermal conductivity and is useful as a substitute for solder.
[0058] In the manufacturing method, all steps can be performed in the atmosphere. When the constituent material of one or both of the first and second components to be joined is a metal that is easily oxidized (e.g., copper), all steps in the manufacturing method can be performed in an inert gas atmosphere. Examples of the inert gas include nitrogen gas and helium gas.
[0059] Hereinafter, the method for manufacturing a bonded body according to the present embodiment will be described with reference to the drawings. First, a bonded body to which the manufacturing method according to the present embodiment is applied will be described.
[0060] <<Jointed Body>> Fig. 1 is a cross-sectional view schematically showing an example of the joined body. The joined body 1 shown here is configured by joining a conductive first component 11 and a conductive second component 12 via a conductive joint 13. A first surface 11a of the first component 11 is in contact with the joint 13. A second surface 12a of the second component 12 is in contact with the joint 13. The joined body 1 is configured by stacking the first component 11, the joint 13, and the second component 12 in this order in the thickness direction. Hereinafter, the stacking direction of the first component 11, the joint 13, and the second component 12 will be referred to as the thickness direction.
[0061] The area of the first surface 11 a of the first component 11 is preferably equal to or greater than the area of the second surface 12 a of the second component 12 .
[0062] The first part 11 has a sheet, plate or block shape.
[0063] The first component 11 preferably contains a metal, and more preferably is made of metal. Examples of metals that form the first component 11 include silver, copper, aluminum, gold, and nickel.
[0064] The first component 11 may be made of one layer (single layer) or may be made of two or more layers. When the first component 11 is made of multiple layers, these multiple layers may be the same or different from one another, and the combination of these multiple layers is not particularly limited. In this specification, not limited to the case of the first component, "multiple layers may be the same or different from one another" means "all layers may be the same, all layers may be different, or only some layers may be the same," and further, "multiple layers are different from one another" means "at least one of the constituent materials and thicknesses of the layers is different from one another."
[0065] When the first component 11 is made up of multiple layers, for example, one or more layers on the bonding portion 13 side of the first component 11 may be layers that improve adhesion to the bonding portion 13.
[0066] There are no particular limitations on the thickness of the first component 11, and the thickness can be set arbitrarily depending on the purpose of the bonded body 1. The thickness of the first component 11 may be, for example, 10 to 10,000 μm.
[0067] When the first component 11 is made up of a plurality of layers, it is preferable that the total thickness of the layers be the thickness of the first component 11 described above.
[0068] Here, the first part 11 is shown to be in the shape of a sheet, a plate, or a block, but the first part 11 may have any other shape, and the shape of the first part 11 can be selected arbitrarily depending on the purpose.
[0069] The second part 12 is in the form of a sheet, a plate, or a block.
[0070] The second component 12 is preferably composed of a metal, and more preferably is made of metal, and examples of the metals that compose the second component 12 include the same metals that compose the first component 11 described above.
[0071] The second component 12 may be made of one layer (single layer) or may be made of two or more layers. When the second component 12 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.
[0072] When the second component 12 is made up of multiple layers, for example, one or more layers on the bonding portion 13 side of the second component 12 may be layers that improve adhesion to the bonding portion 13 .
[0073] The thickness of the second component 12 is not particularly limited and can be set arbitrarily depending on the purpose of the bonded body 1. The thickness of the second component 12 is preferably 0.05 to 10,000 μm, and may be, for example, 0.05 to 500 μm, or may be greater than 500 μm and not greater than 10,000 μm. When the second component 12 is made up of multiple layers, the total thickness of the layers is preferably the thickness of the second component 12 described above.
[0074] Here, the second part 12 is shown to be in the shape of a sheet, a plate, or a block, but the second part 12 may have any other shape, and the shape of the second part 12 can be selected arbitrarily depending on the purpose.
[0075] The joint 13 is in the form of a sheet, a plate, or a block. The joint 13 may be made of one layer (single layer), or may be made of two or more layers. When the joint 13 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.
[0076] It is preferable that the entire surface of the joint portion 13 on the first component 11 side be in contact with the first surface 11 a of the first component 11 .
[0077] The thickness of the joint 13 may be, for example, 10 μm or more but less than 100 μm, but is preferably 100 μm or more, and may be, for example, 200 μm or more or 300 μm or more. When the thickness of the joint 13 is as thick as 100 μm or more, the thickness of the dried bonding material must also be 100 μm or more. However, when the thickness of the dried bonding material is increased in this manner, the effect of the present invention, that is, cracking of the dried bonding material can be suppressed, is more significantly achieved by using the bonding material of this embodiment. On the other hand, the thickness of the joint 13 is preferably 400 μm or less, in that it is easier to form the joint 13.
[0078] Here, the joint 13 is shown to be sheet-shaped, plate-shaped, or block-shaped, but the joint 13 may be in any other shape, and the shape of the joint 13 can be selected arbitrarily depending on the purpose.
[0079] The area of the contact region of the surface of the joining portion 13 with the first component 11 (more specifically, the first surface 11a) and the area of the contact region with the second component 12 (more specifically, the second surface 12a) may be the same or different. The area of each of the contact regions is 9 to 2500 mm 2 It is preferable that the length is 9 to 1225 mm. 2 More preferably, for example, 9 to 576 mm 2 , and 9 to 144 mm 2 or 225 to 1225 mm 2 , and 625 to 1225 mm 2 or 225 to 576 mm 2 However, these are just examples of the area of the contact area. When the area of the contact area is in the above range, the bonding strength and heat dissipation between the components 11 and 12 and the joint 13 are improved.
[0080] The area of the second surface 12a of the second component 12 is preferably 50 to 150% of the area of the surface of the joint 13 facing the second component 12. The area of the second surface 12a of the second component 12 that is in contact with the joint 13 is preferably 50 to 100% of the area of the entire second surface 12a. It is preferable that the entire surface of the joint 13 facing the first component 11 be in contact with the first component 11.
[0081] In the joined body 1, one first component 11 and one second component 12 are joined by one joint 13, but the joining form is not limited to this. In the joined body, for example, one first component and two or more second components may be joined by one joint. In this case, the two or more second components may be all the same, all different, or only partially different. In the joined body, for example, one first component and two or more second components may be joined by two or more joints. In this case, the number of second components and the number of joints may be the same or different. In addition, the two or more second components may be all the same, all different, or only partially different. The number of first components and the number of second components illustrated here may be reversed.
[0082] The bonded body to which the manufacturing method of the present embodiment is applied is not limited to that shown in FIG. 1 . For example, the bonded body 1 shown in FIG. 1 may have some components modified, deleted, or added within the scope of the present invention.
[0083] <<Porosity>> The porosity was measured by forming a cross section of the joint and observing the cross section using a scanning electron microscope (SEM). The observed joint 13 was a portion where a dried bonding material was sandwiched between the first surface 11a and the second surface 12a and sintered. That is, the porosity was measured for the joint 13 sintered while being pressed at a predetermined pressure by the first component 11 and the second component 12. Here, the "porosity" was defined as the ratio of the area of the portion corresponding to the pores to the area of the cross section ([area of the portion corresponding to the pores in the cross section] / [area of the cross section] × 100). For example, the "porosity" may be defined as the ratio of the area of the portion corresponding to the pores in the region surrounded by a predetermined outline to the total area of the region surrounded by the outline on the cross section of the joint 13 ([area of the portion corresponding to the pores in the region surrounded by the outline] / [area of the region surrounded by the outline] × 100). The porosity is preferably 5% or less. By using the bonding material of this embodiment, even if the dried bonding material is fired while being pressurized at a low pressure of about 20 MPa or less, a bonding part with few pores (low porosity) can be formed. As is clear from the explanation of the method for calculating the porosity, the "cross-sectional area" in the formula for calculating the porosity includes not only the area of the metal sintered body itself but also the area of the area corresponding to the pores.
[0084] When determining the porosity of the joint, as will be described later in the Examples, the image data of the cross section obtained using an SEM is subjected to binarization processing using image processing software, the pores are identified, and the porosity is calculated, thereby enabling the porosity to be calculated with higher accuracy.
[0085] When there is no bias in the locations of the pores in the cross section, when determining the porosity of the joint, for example, the porosity may be calculated from each of the areas surrounded by a predetermined contour line in the SEM image data at several representative locations (e.g., 2 to 3 locations) on the cross section, and the average value of these porosity values may be used as the porosity of the joint.
[0086] Next, the manufacturing method of this embodiment will be described by taking as an example the case of manufacturing the bonded body shown in FIG.
[0087] 2A to 2E are cross-sectional views for schematically illustrating an example of a method for manufacturing a bonded body according to this embodiment (sometimes referred to in this specification as "manufacturing method (1)"). In each figure, the same components as those shown in figures that have already been described are denoted by the same reference numerals as in the figures that have already been described, and detailed description thereof will be omitted.
[0088] 2A , in the attachment step of the manufacturing method (1), the bonding material 130 is attached to the first surface 11a of the first component 11. Examples of a method for attaching the bonding material 130 to the first component 11 include known methods such as a printing method and a coating method.
[0089] Examples of the printing method include screen printing, flexographic printing, offset printing, dip printing, inkjet printing, dispenser printing, jet dispenser printing, gravure printing, gravure offset printing, and pad printing.
[0090] Examples of the coating method include methods using various coaters such as a spin coater, an air knife coater, a curtain coater, a die coater, a blade coater, a roll coater, a gate roll coater, a bar coater, a rod coater, and a gravure coater; methods using a wire bar; and methods using a coating device such as a slot die.
[0091] When the bonding material 130 is applied to the first component 11, a mask such as a metal mask may be used to apply the bonding material 130 only to the desired locations.
[0092] <<Drying Step>> After the adhering step of the manufacturing method (1), in the drying step, the adhered bonding material 130 is dried to form a dried bonding material 130′, as shown in Fig. 2B . The drying step volatilizes the solvent in the bonding material 130, so that the dried bonding material 130′ does not contain any solvent or has a significantly reduced solvent content compared to the bonding material 130.
[0093] The dried bonding material 130' is not a metal sintered body and typically does not have the luster characteristic of metal, and this external appearance feature also makes it possible to distinguish it from the target metal sintered body.
[0094] The bonding material 130 can be dried by a known method, and is preferably dried by heating under normal pressure.
[0095] The heating temperature (drying temperature) of the bonding material 130 in the drying process can be adjusted appropriately depending on the type of solvent, but is preferably 70°C or higher, and may be, for example, 100°C or higher or 130°C or higher. When the heating temperature is equal to or higher than the lower limit, the drying of the bonding material 130 proceeds more quickly. Furthermore, since the solvent can be sufficiently evaporated in the drying process, bumping due to residual solvent can be prevented in the firing process described below, and the generation of voids can be suppressed. On the other hand, the heating temperature is preferably 160°C or lower. When the heating temperature is equal to or lower than the upper limit, deterioration of the dried bonding material 130' is suppressed. For example, if the drying temperature is excessively high, metal particles may neck (fuse) together before the firing process, making it difficult to reduce pores when pressurized.
[0096] The heating time (drying time) of the bonding material 130 in the drying step can be adjusted appropriately depending on the heating temperature, but is preferably 1 to 40 minutes, and may be, for example, 3 to 30 minutes or 5 to 20 minutes. By setting the heating time within this range, the desired dried bonding material 130' can be formed more efficiently.
[0097] The thickness of the dried bonding material 130' may be, for example, 10 μm or more and less than 100 μm, but is preferably 100 μm or more, and may be, for example, 200 μm or more or 300 μm or more. Dried products of ordinary bonding materials are prone to cracking when they are thick. In contrast, the dried bonding material 130' uses the bonding material 130, so cracking is suppressed even when the thickness is as thick as 100 μm or more. Meanwhile, the thickness of the dried bonding material 130' is preferably 400 μm or less, in that it is easier to form the dried bonding material 130'.
[0098] <<Laminating Step>> After the drying step of manufacturing method (1), in the laminating step, as shown in Fig. 2C , the first component 11 and the second component 12 are laminated with the dried bonding material 130' interposed therebetween to produce a laminated body 101. That is, the laminated body 101 is configured by laminating the first component 11, the dried bonding material 130', and the second component 12 in this order in the thickness direction, with the dried bonding material 130' in close contact with the first component 11. The first surface 11a of the first component 11 is in contact with the dried bonding material 130'. The second surface 12a of the second component 12 is in contact with the dried bonding material 130'.
[0099] 2D , in the firing step after the lamination step of the manufacturing method (1), the dried bonding material 130′ in the laminate 101 is fired at a temperature (sometimes referred to as a “firing temperature” in this specification) higher than the temperature at which the bonding material 130 was dried. When the bonding material 130 is dried by heating, the firing temperature of the dried bonding material 130′ (the firing temperature) is set higher than the heating temperature (drying temperature) of the bonding material 130.
[0100] When the dried bonding material 130' is fired, the temperature rise rate of the dried bonding material 130' during heating is not particularly limited, but is preferably 30 to 70°C / min, and may be, for example, 40 to 60°C / min. When the temperature rise rate is in such a range, a metal sintered body (bonding portion 13) having the desired characteristics can be produced more efficiently.
[0101] The firing temperature of the dried bonding material 130' (the temperature at which the metal particles (A) are sintered) is preferably 180°C or higher, and may be, for example, any one of 200°C or higher, 220°C or higher, and 240°C or higher. When the firing temperature is equal to or higher than the lower limit, a metal sintered body (bonding portion 13) with higher purity can be obtained. On the other hand, the firing temperature of the dried bonding material 130' is preferably 320°C or lower, and may be, for example, any one of 300°C or lower and 280°C or lower, in order to prevent excessive heating and obtain a metal sintered body (bonding portion 13) with good properties.
[0102] The firing time of the dried bonding material 130' (the time for sintering the metal particles (A)) is preferably 3 to 120 minutes, and may be, for example, 3 to 60 minutes, 50 to 90 minutes, or 80 to 120 minutes. By setting the firing time (sintering time) within this range, a metal sintered body with the desired characteristics can be more efficiently manufactured. In the firing step, it is preferable to fire the dried bonding material 130' at a firing temperature within the above-mentioned numerical range and for a firing time within the numerical range shown here.
[0103] In the firing step, the dried bonding material 130′ is preferably fired (sometimes referred to as “pressure firing” in this specification) while pressurizing the laminate 101 in the thickness direction. By firing the dried bonding material 130′ under pressure in this manner, a bonded portion with fewer voids can be formed.
[0104] When the laminate 101 is pressed in the thickness direction, the pressure applied to the laminate 101 is a pressure P 1 and the pressure P applied from the second component 12 side. 2 In this specification, "pressurization" means increasing the pressure applied to an object by actively applying force to the object, and for example, simply supporting the object (applying normal force) without actively applying force is not considered pressurization. In the case of pressurization, for example, the position of the pressurizing means changes by itself with acceleration.
[0105] During pressurized firing, heating for firing the dried bonding material 130′ (laminate 101) and pressurizing the dried bonding material 130′ (laminate 101) may be started simultaneously, or heating for firing the dried bonding material 130′ may be started before pressurizing the dried bonding material 130′, or heating for firing the dried bonding material 130′ may be started before pressurizing the dried bonding material 130′.
[0106] The pressure applied to the dried bonding material 130' during pressure firing is preferably 20 MPa or less, and may be, for example, 16 MPa or less. Normally, when the pressure during pressure firing is low, the number of voids in the bonded portion increases, preventing a dense bonded portion from being obtained. However, by using the bonding material 130 of this embodiment, a dense bonded portion with few voids can be obtained even at a low pressure below the upper limit. Furthermore, by keeping the pressure below the upper limit, damage such as cracking and deformation of the first component 11 or the second component 12 are suppressed. On the other hand, the pressure during pressure firing is preferably 1 MPa or more, for example, in order to effectively obtain the effects of pressure. Here, the pressure applied to the dried bonding material 130' (the pressure during pressure firing) is the load applied to the laminate 101 during pressure firing divided by the area of the region of the dried bonding material 130' that receives this load. The pressure P applied from the first component 11 side is 1 and the pressure P applied from the second component 12 side. 2 When both of the pressures P and P are applied to the bonding material 130′, the pressure during pressurized firing per unit area is 1 / Pressure P 1 The area of the first surface 11a receiving the pressure P 2 / Pressure P 2 (area of the second surface 12a that receives the load).
[0107] 2E, the firing step forms the bonding portion 13 from the dried bonding material 130′, thereby obtaining the desired bonded body 1. The bonding portion 13 is a metal sintered body formed from the bonding material 130 via the dried bonding material 130′.
[0108] The use of the bonding material 130 reduces the number of voids in the bonding portion 13. Therefore, even if the temperature of the bonded body 1 fluctuates significantly, concentration of thermal stress is suppressed in the bonding portion 13, and damage to the bonding portion 13 is suppressed. Furthermore, since the bonding portion 13 is formed from metal particles with high thermal conductivity, the thermal conductivity of the bonding portion 13 is high.
[0109] So far, we have explained a method for manufacturing a bonded body (manufacturing method (1)) in which the bonding material is attached to a first surface of a first component and a bonded joint is formed from this bonding material. However, the manufacturing method of this embodiment may also be a method for manufacturing a bonded body (sometimes referred to in this specification as "manufacturing method (2)") in which the bonding material is attached to a second surface of a second component and a bonded joint is formed from this bonding material.
[0110] Manufacturing Method (2) FIGS. 3A to 3E are cross-sectional views for schematically illustrating another example of the manufacturing method for the bonded body of this embodiment, that is, the manufacturing method (2).
[0111] 3A , in the attachment step of the manufacturing method (2), the bonding material 130 is attached to the second surface 12 a of the second component 12. The attachment step in the manufacturing method (2) can be performed in the same manner as the attachment step in the manufacturing method (1), except that the bonding material 130 is attached to the second surface 12 a of the second component 12, not the first surface 11 a of the first component 11.
[0112] <<Drying Step>> After the adhesion step of manufacturing method (2), in the drying step, the adhered bonding material 130 is dried to form a dried bonding material 130', as shown in FIG. 3B . The drying step in manufacturing method (2) can be performed in the same manner as the drying step in manufacturing method (1), except that the second component 12 to which the bonding material 130 is adhered is used instead of the first component 11 to which the bonding material 130 is adhered. The dried bonding material 130' formed in manufacturing method (2) is the same as the dried bonding material 130' formed in manufacturing method (1), except that the dried bonding material 130' is in close contact with the second component 12 instead of the first component 11. In manufacturing method (2), the dried bonding material 130' uses the bonding material 130, thereby suppressing cracking even when the dried bonding material 130' is thick, such as 100 μm or thicker.
[0113] <<Lamination Step>> After the drying step of manufacturing method (2), in the lamination step, as shown in Fig. 3C , the first component 11 and the second component 12 are laminated with the dried bonding material 130' interposed therebetween to produce a laminated body 102. That is, the laminated body 102 is configured by laminating the first component 11, the dried bonding material 130', and the second component 12 in this order in the thickness direction, with the dried bonding material 130' in close contact with the second component 12. The laminated body 102 is the same as the laminated body 101 except that the dried bonding material 130' is in close contact with the second component 12 instead of the first component 11. The lamination step in manufacturing method (2) can be performed in the same manner as the lamination step in manufacturing method (1), except that the second component 12 having the dried bonding material 130′ is used instead of the first component 11 having the dried bonding material 130′, and the first component 11 having no dried bonding material 130′ is used instead of the second component 12 having no dried bonding material 130′.
[0114] <<Firing Step>> After the lamination step of manufacturing method (2), in the firing step, the dried bonding material 130' in the laminate 102 is fired at a temperature higher than the temperature at which the bonding material 130 was dried, as shown in Fig. 3D. The firing step in manufacturing method (2) can be performed in the same manner as in the firing step in manufacturing method (1). In the firing step in manufacturing method (2), it is also preferable to pressurize and fire the dried bonding material 130'.
[0115] By carrying out the firing step of the manufacturing method (2), as shown in FIG. 3E, the joint 13 is formed from the dried joining material 130′, and the desired joined body 1 is obtained. The joint 13 is a metal sintered body formed from the joining material 130 via the dried joining material 130′. The joined body 1 obtained by the manufacturing method (2) is the same as the joined body 1 obtained by the manufacturing method (1).
[0116] In the case of manufacturing method (2), the bonding material 130 is also used, so that the bonding portion 13 has few voids. Therefore, even if the temperature of the bonded body 1 fluctuates greatly, the concentration of thermal stress in the bonding portion 13 is suppressed, and damage to the bonding portion 13 is suppressed. Furthermore, since the bonding portion 13 is formed from metal particles having high thermal conductivity, the thermal conductivity of the bonding portion 13 is high.
[0117] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the examples shown below.
[0118] The metal particles (A) and metal particles (B) used in the following examples and comparative examples are both silver particles produced by a reduction method.
[0119] Example 1 Production of Bonding Material Metal particles (A)-1 (approximately spherical silver particles) (87 parts by mass) having the metal species, shape, particle size distribution, and specific surface area shown in Table 1 and Texanol (13 parts by mass) were weighed into an agate mortar at room temperature and kneaded for 15 minutes. The resulting kneaded mixture was then passed through a triple roll mill three times to obtain the desired paste-like bonding material. Image data of the metal particles (A)-1 at 10,000x magnification obtained using a scanning electron microscope (SEM) is shown in FIG. 4.
[0120] <<Manufacturing of Bonded Structure>> <Formation of Dried Bonding Material and Evaluation of Its Crack Suppression Effect> A silver-plated copper plate measuring 20 mm x 20 mm and 1 mm thick, with a 5 μm-thick silver-plated layer on its surface, was prepared. A 300 μm-thick metal mask was placed on the silver-plated surface of the silver-plated copper plate. A 7 mm x 7 mm square shape was printed using a bonding material. This resulted in a rectangular bonding material being attached to the surface of the silver-plated copper plate (adhesion process). Next, the silver-plated copper plate with the attached bonding material was heated at 145°C for 15 minutes in a hot air oven to volatilize the Texanol in the bonding material and dry it, forming a film-like dried bonding material with a rectangular planar shape (drying process). Next, the dried bonding material was visually observed, and the crack suppression effect of the dried bonding material was evaluated according to the following criteria. The results are shown in Table 1. [Evaluation criteria] A: No cracks were observed in the dried bonding material, and the crack suppression effect was high. B: Slight cracks were observed in the dried bonding material, and the silver-plated copper plate was not visible through the cracks, but the crack suppression effect was poor. C: Clear cracks were observed in the dried bonding material, and the silver-plated copper plate was visible through the cracks, and the crack suppression effect was not observed or was low.
[0121] <Production of Bonded Body> A silicon carbide (SiC) chip having a size of 5 mm x 5 mm and a thickness of 0.35 mm, on one side (i.e., the back side), was prepared by sputtering a 50 nm titanium film and a 100 nm silver film, in that order. The entire exposed surface of the silver film in the back-side coated silicon carbide chip was superimposed on the side (i.e., the exposed surface) of the dried bonding material formed above opposite the silver-plated copper plate side, thereby producing a laminate in which the silver-plated copper plate, the dried bonding material, and the back-side coated silicon carbide chip were stacked in this order in the thickness direction (lamination process). Furthermore, a carbon sheet ("PERMA-FOIL (registered trademark)" manufactured by Toyo Tanso Co., Ltd.) was placed on the surface of the silicon carbide chip in the back-side coated silicon carbide chip of the laminate as a cushioning material.
[0122] Next, the carbon sheet-attached laminate obtained above was pressed in the thickness direction using a servo press. Pressurization of the dried bonding material was initiated at a pressure of 15 MPa, and simultaneously heating was initiated at a temperature increase rate of approximately 50°C / min. The carbon sheet-attached laminate was placed between a pair of press plates in the servo press. The pair of press plates included a first press plate located on the backside-coated silicon carbide chip side of the carbon sheet-attached laminate, and a second press plate located on the silver-plated copper plate side. The first press plate was fixed to the servo press. The second press plate was then moved toward the first press plate, supporting the carbon sheet-attached laminate with the first press plate, while applying pressure to the carbon sheet-attached laminate from its silver-plated copper plate side. In other words, pressure was applied to the carbon sheet-attached laminate from the silver-plated copper plate side. After the heating temperature (i.e., the temperature of the laminate) reached 250°C, this temperature was maintained for 5 minutes. Specifically, heating and pressurization were performed at a temperature of 250°C and a pressure of 15 MPa for 5 minutes. In this way, the dried bonding material was pressurized and fired to form a bonded joint (firing process). Next, cooling was started by running cooling water through the servo press, and when the temperature of the laminate reached 60°C, the pressure was released. This resulted in the desired bonded body. The thickness of the bonded body was greater than 100 μm.
[0123] <<Evaluation of Bonded Body>> <Evaluation of the Effect of Suppressing Void Generation at the Bonded Portion> The side surfaces of the bonded body obtained above were mechanically polished to form a cross section of the bonded body, and polishing marks were removed by flat milling. Next, using an SEM, an area near the center of the bonded portion in the width direction of the cross section was observed randomly from three fields of view at an acceleration voltage of 4 kV and a magnification of 5000x. The image data obtained was binarized using image processing software (Image J.), and black areas were classified as voids, and the porosity of the bonded portion was calculated. The effect of suppressing void generation at the bonded portion was evaluated according to the following criteria. The results are shown in Table 1 together with the porosity. [Evaluation Criteria] A: The average porosity of the three fields of view was 5% or less, indicating a high void generation suppression effect. B: The average porosity of the three fields of view was greater than 5% and less than 10%, indicating a poor void generation suppression effect. C: The average porosity in three visual fields is greater than 10%, and the effect of suppressing the generation of pores is not observed or is extremely low.
[0124] <<Production of Bonding Material, Production of Bonded Body, and Evaluation of Bonded Body>> [Example 2] A bonding material was produced, and a bonded body was produced and evaluated in the same manner as in Example 1, except that metal particles (A)-2 (approximately spherical silver particles) (87 parts by mass) were used instead of metal particles (A)-1 (87 parts by mass) as shown in Table 1. The results are shown in Table 1. The thickness of the bonded portion in the bonded body was greater than 100 μm. Image data of metal particles (A)-2 at a magnification of 10,000 times, obtained using an SEM, is shown in FIG. 5.
[0125] Example 3 A bonding material was produced and a bonded body was produced and evaluated in the same manner as in Example 1, except that metal particles (A)-3 (approximately spherical silver particles) (87 parts by mass) were used instead of metal particles (A)-1 (87 parts by mass) as shown in Table 1. The results are shown in Table 1. The thickness of the bonded portion in the bonded body was greater than 100 μm.
[0126] Comparative Example 1 A bonding material was produced and a bonded body was produced and evaluated in the same manner as in Example 1, except that metal particles (B)-1 (approximately spherical silver particles) (87 parts by mass) were used instead of metal particles (A)-1 (87 parts by mass) as shown in Table 1. The results are shown in Table 1. The thickness of the bonded portion in the bonded body was greater than 100 μm. Image data of metal particles (B)-1 at a magnification of 10,000 times, obtained using an SEM, is shown in FIG. 6.
[0127] Comparative Example 2 A bonding material was produced and a bonded body was produced and evaluated in the same manner as in Example 1, except that metal particles (B)-2 (approximately spherical silver particles) (87 parts by mass) were used instead of metal particles (A)-1 (87 parts by mass) as shown in Table 2. The results are shown in Table 2. The thickness of the bonded portion in the bonded body was greater than 100 μm. Image data of metal particles (B)-2 at a magnification of 10,000 times, obtained using an SEM, is shown in FIG. 7.
[0128] Comparative Example 3 A bonding material was produced in the same manner as in Example 1, except that metal particles (B)-3 (approximately spherical silver particles) (87 parts by mass) were used instead of metal particles (A)-1 (87 parts by mass) as shown in Table 2, and a bonded body was produced and evaluated. The results are shown in Table 2. Image data of metal particles (B)-3 at a magnification of 10,000 times, obtained using an SEM, is shown in FIG. 8.
[0129] Comparative Example 4 A bonding material was produced in the same manner as in Example 1, except that metal particles (B)-4 ("N300", plate-shaped silver particles manufactured by Tokusen Kogyo Co., Ltd.) (87 parts by mass) were used instead of metal particles (A)-1 (87 parts by mass) as shown in Table 2. The results are shown in Table 2.
[0130]
[0131]
[0132] As is clear from the above results, in Examples 1 to 3, cracking was suppressed even when the dried bonding material was thick. Furthermore, even when the dried bonding material was fired under a low pressure of 15 MPa, a bonded joint with few pores was formed. In Examples 1 to 3, the porosity of the bonded joint was 3.2% or less (2.6 to 3.2%).
[0133] In Examples 1 to 3, the bonding material contained only metal particles (A) as metal particles, the D50 of the metal particles (A) was 0.32 to 0.48 μm, the Dmin of the metal particles (A) was 0.11 μm or more (0.11 to 0.19 μm), and the bonding material did not contain a resin component.
[0134] In Examples 1 to 3, the D90 of the metal particles (A) is 0.75 μm or less (0.52 to 0.75 μm), the D10 of the metal particles (A) is 0.21 μm or more (0.21 to 0.32 μm), and the specific surface area of the metal particles (A) is 0.95 to 1.5 m 2 / g, which is presumed to result in the bonding material having more desirable properties.
[0135] In contrast, cracking of the dried bonding material could not be suppressed in Comparative Example 1. In Comparative Example 1, the bonding material contained metal particles (B) instead of metal particles (A). The Dmin of the metal particles (B) was 0.08 μm.
[0136] In Comparative Example 2, there were many pores in the joint, and the porosity was 6.6%. In Comparative Example 2, the bonding material contained metal particles (B) instead of metal particles (A). The Dmin of the metal particles (B) was 0.08 μm, and furthermore, the D90 of the metal particles (B) was large at 0.82 μm.
[0137] In Comparative Example 3, the dried bonding material had significant cracks, and the silver-plated copper plate was visible through the cracks, making it impossible to produce a bonded body. In Comparative Example 3, the bonding material contained metal particles (B) instead of metal particles (A). The D50 of the metal particles (B) was 0.20 μm, which was too small, and the Dmin of the metal particles (B) was 0.06 μm, which was too small.
[0138] In Comparative Example 4, as in Comparative Example 3, the dried bonding material had significant cracks, and the silver-plated copper plate was visible through the cracks, making it impossible to produce a bonded body. In Comparative Example 4, the bonding material contained metal particles (B) instead of metal particles (A). The metal particles (B) had a plate-like shape.
[0139] The present invention can be used to manufacture conductive junctions, particularly semiconductor devices.
[0140] REFERENCE SIGNS LIST 1... Bonded body, 11... First part, 11a... First surface, 12... Second part, 12a... Second surface, 13... Bonding portion, 130... Bonding material, 130'... Dried bonding material, 101, 102... Laminate
Claims
1. A bonding material for bonding conductive parts together, comprising: metal particles including substantially spherical metal particles (A); and a solvent for dispersing the metal particles, wherein the metal particles (A) have a volume-based 50% accumulated particle diameter D50 of 0.3 to 0.5 μm as measured by a laser diffraction / scattering particle size distribution measurement, and the minimum particle diameter Dmin of the metal particles (A) is greater than 0.08 μm.
2. The bonding material according to claim 1, wherein the metal particles include metal particles (B) different from the metal particles (A), and the minimum particle size Dmin of the metal particles (B) measured by a laser diffraction / scattering particle size distribution measurement is greater than 0.08 μm.
3. The bonding material according to claim 1 or 2, further comprising a resin component in the solvent, which is a curable resin, a non-curable resin, or a thermoplastic resin, and wherein the ratio of the content of the resin component to the content of the metal particles in the bonding material is less than 0.01 mass%.
4. The bonding material according to claim 1 or 2, wherein the solvent does not contain a resin component which is a curable resin, a non-curable resin, or a thermoplastic resin.
5. The bonding material according to claim 1 or 2, wherein the metal particles (A) have a volume-based 90% cumulative particle diameter D90 of less than 0.8 μm as measured by laser diffraction / scattering particle size distribution measurement.
6. The bonding material according to claim 2, wherein the metal particles (A) and the metal particles (B) are both silver particles.
7. The specific surface area of the metal particles (A) is 0.95 to 1.5 m 2 The bonding material according to claim 1 or 2, wherein the bonding strength is in the range of / g.
8. A method for manufacturing a bonded body in which a conductive first part and a conductive second part are bonded via a conductive bonding part, comprising the steps of: attaching the bonding material according to claim 1 or 2 to a first surface of the first part or a second surface of the second part; forming a dried bonding material by drying the attached bonding material; stacking the first part and the second part via the dried bonding material to produce a laminate; and forming the bonded part from the dried bonding material by firing the dried bonding material in the laminate at a temperature higher than the temperature at which the bonding material was dried.
9. The method for producing a joint according to claim 8, wherein the thickness of the joint is 100 μm or more.
Citation Information
Patent Citations
Antifreeze water tap post
JP2023071339A
Joining material and joining method using the same
JP2011080147A
Silver-containing paste, and manufacturing method of bonded body
JP2022083624A
Method of Fabricating High-Power Module
US20200171578A1
Film-like firing material and film-like firing material with support sheet
WO2019163568A1