Catalyst used for organic hydride generation, production method for said catalyst, and organic hydride production method using said catalyst
The boron-doped catalyst with platinum or rhodium on a metal oxide carrier addresses the inefficiencies of conventional catalysts by enhancing hydrogenation activity, enabling efficient organic hydride production and compact, cost-effective hydrogen storage and transport.
Patent Information
- Application Number
- PCT/JP2024/015701
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional catalysts for hydrogenation reactions are expensive, difficult to manufacture, and have low hydrogenation activity, especially under low pressure conditions, making them inefficient for compact and cost-effective hydrogen storage and transport in organic hydride technology.
A boron-doped catalyst with a metal having hydrogenation activity, such as platinum or rhodium, supported on a metal oxide carrier, where boron is added through impregnation and reduction processes to enhance hydrogenation activity, allowing for efficient hydrogenation reactions at low pressures.
The boron-doped catalyst exhibits higher hydrogenation activity, enabling more efficient production of organic hydrides, reducing equipment size, and facilitating heat management in hydrogenation reactions, while being cost-effective and easier to manufacture.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Catalyst used for producing organic hydrides, method for producing said catalyst, and method for producing organic hydrides using said catalyst
[0001] The present invention relates to organic hydride technology, and more particularly to boron-doped catalysts, methods for making the catalysts, and methods for producing organic hydrides using the catalysts.
[0002] Hydrogen energy utilization technology has been attracting attention as one of the technologies to reduce the pollution and global warming that occurs with the consumption of fossil fuels, as well as the risk of radiation exposure that comes with the use of nuclear energy. Hydrogen can be produced by the electrolysis of water, so it is practically inexhaustible on Earth. It is also a clean energy source that does not produce carbon dioxide after combustion.
[0003] To utilize hydrogen, it is necessary to store and transport gaseous hydrogen safely and efficiently. In recent years, the organic hydride method has attracted attention as a technology for storing and transporting hydrogen. Organic hydrides refer to saturated hydrocarbons such as cyclohexane, methylcyclohexane, and decalin, which are produced by adding hydrogen to unsaturated hydrocarbons, including aromatic compounds such as benzene, toluene, and naphthalene. In the organic hydride method, which uses organic hydrides to store and transport hydrogen, hydrogen is added to unsaturated hydrocarbons at hydrogen production sites to produce organic hydrides that are liquid at room temperature. The organic hydrides are then stored or transported in liquid form. At demand sites, the organic hydrides are separated into hydrogen and unsaturated hydrocarbons by a dehydrogenation reaction. The separated hydrogen is used as an energy source at the demand site, and the unsaturated hydrocarbons are transported back to the hydrogen production site for use in the hydrogenation reaction. In this way, the use of hydrocarbon hydrogenation and dehydrogenation reactions enables the safe and efficient storage and transportation of gaseous hydrogen.
[0004] Conventionally, catalysts in which a noble metal such as platinum is supported on a support such as aluminum oxide have been used in hydrogenation reactions to produce organic hydrides. However, catalysts using noble metals are expensive. Furthermore, hydrogenation reactions are exothermic reactions, requiring heat management (heat removal). To facilitate heat management, it is necessary to make the apparatus for performing the hydrogenation reaction compact. To make the apparatus compact, it is essential to improve the hydrogenation reaction activity (hereinafter referred to as hydrogenation activity) of the catalyst so that organic hydrides can be produced efficiently with a small amount of catalyst.
[0005] Prior art has been proposed that aims to improve the hydrogenation activity of catalysts in hydrogenation reactions. Patent Document 1 (Japanese Patent No. 6099238) and Patent Document 2 (Japanese Patent No. 6734275) are technologies relating to catalysts having a structure that can improve hydrogenation activity. Patent Document 3 (Japanese Patent Laid-Open No. 2006-130378) proposes a technology relating to a catalyst obtained by coating a catalyst material on a support using a sputtering method, and Patent Document 4 (Japanese Patent Laid-Open No. 2018-103158) proposes a technology relating to a catalyst that uses a layered hydroxide as a support that supports a catalytic metal. However, these catalysts have problems such as difficulty in controlling the structure, high manufacturing costs, and difficulty in mass production.
[0006] Regarding technology related to dehydrogenation reactions, the inventors of the present invention have developed a new catalyst in which phosphorus is added to a rhodium-supported aluminum oxide catalyst (Non-Patent Document 1). This catalyst exhibited higher methylcyclohexane dehydrogenation activity than a rhodium catalyst.
[0007] Japanese Patent No. 6099238 Japanese Patent No. 6734275 Japanese Patent Application Laid-Open No. 2006-130378 Japanese Patent Application Laid-Open No. 2018-103158
[0008] Yasuharu Kanda and three others, "Synthesis and Utilization Process of Organic Hydride Ammonia," pp. 85-93, CMC Publishing, 2021. "Remarkable Enhancement in Hydrogenation Ability by Phosphidation of Ruthenium: Specific Surface Structure Having Unique Ru Ensemble," S. Furukawa et al., ACS Catalysis, 8 (2018), 8177-8181. "Efficient hydrogen storage in boron-doped graphene decorated by transition metals - A first-principles study," S. Nachimuthu et al., Carbon, 73 (2014), 132-140. "The double tuning effect of TiO2 on Pt-catalyzed dehydrogenation of methylcyclohexane," X. Yang et al., Mol. Catal., 492 (2020), 110971.
[0009] The present invention aims to provide a catalyst that can be used in hydrogenation reactions, which has high hydrogenation activity even under low-pressure conditions and can be produced relatively easily and at low cost, and a method for producing the same. Another object of the present invention is to provide a method for producing organic hydrides with high efficiency by using the above catalyst.
[0010] The present inventors have discovered that by adding boron to a catalyst used in the production of organic hydrides (hydrogenation reactions), in which a metal active in hydrogenation reactions is supported on a metal oxide, a catalyst with higher hydrogenation activity than conventional catalysts can be obtained, and have completed the present invention.
[0011] One aspect of the present invention provides a catalyst for producing organic hydrides. The catalyst comprises a metal active in a hydrogenation reaction, a support supporting the metal, and boron added to the metal. The molar ratio of boron to the metal is preferably 0.5 to 2.0. The metal active in a hydrogenation reaction is preferably a platinum group metal, more preferably platinum or rhodium, or both. The support supporting the metal is preferably a metal oxide, more preferably aluminum oxide, silicon oxide, titanium oxide, cerium oxide, or a combination thereof.
[0012] Another aspect of the present invention provides a method for producing a catalyst for producing organic hydrides. The production method includes the steps of preparing a raw catalyst in which a metal is supported on a carrier, adding boron to the raw catalyst, and reducing the boron-added raw catalyst. The step of adding boron to the raw catalyst preferably includes the steps of impregnating the raw catalyst with an organic solvent solution of a boron compound and drying the raw catalyst impregnated with the organic solvent solution. The boron compound is preferably any one of triphenylborane, triethylborane, and sodium borohydride, or a combination thereof. The step of reducing the boron-added raw catalyst preferably includes the step of reducing the raw catalyst at 650°C to 850°C in a hydrogen atmosphere.
[0013] Yet another aspect of the present invention provides a method for producing an organic hydride using a catalyst for organic hydride production. This method includes a step of reducing the catalyst for organic hydride production according to the present invention; a reaction step of contacting the reduced catalyst with a raw material containing an unsaturated hydrocarbon and hydrogen; and a separation step of separating the organic hydride from the product containing the organic hydride and hydrogen produced by the reaction step. In one embodiment, the unsaturated hydrocarbon used can be toluene, and the organic hydride produced can be methylcyclohexane. The step of reducing the catalyst preferably includes a step of reducing the catalyst at 150°C to 400°C under a hydrogen atmosphere. The reaction step is preferably carried out at a reaction pressure of 0 MPaG to 10 MPaG, more preferably 0 MPaG to 1 MPaG.
[0014] According to the present invention, by adding boron to a catalyst in which a metal active in hydrogenation reactions is supported on a metal oxide, it is possible to obtain a catalyst with higher hydrogenation activity than conventional catalysts.By using the catalyst of the present invention, organic hydrides can be produced more efficiently than with conventional catalysts, which makes it possible to make the hydrogenation reaction apparatus more compact and facilitates heat management in hydrogenation reactions, for which heat removal is essential.
[0015] The present invention will be described in detail below.
[0016] <Catalyst> The catalyst according to the present invention comprises a metal having activity in a hydrogenation reaction (hydrogenation activity), a support supporting the metal having hydrogenation activity, and boron added to the metal having hydrogenation activity. Conventionally, catalysts used in hydrogenation reactions to produce organic hydrides generally comprise a metal having hydrogenation activity supported on a support. However, conventional catalysts do not have sufficient hydrogenation activity. In contrast, the catalyst according to the present invention, due to the addition of boron, has higher hydrogenation activity than conventional catalysts, enabling the reaction to proceed with high efficiency.
[0017] The metal contained in the catalyst according to the present invention can be a platinum group metal, gold, or silver, which is a metal having hydrogenation activity. Among these, the platinum group metals are more preferred, and platinum and rhodium are even more preferred, because they have higher hydrogenation activity. These metals can be used alone or in combination.
[0018] The carrier contained in the catalyst according to the present invention can be a material generally used in hydrogenation reactions, as needed. It is preferable to use a metal oxide as the carrier, and among metal oxides, it is more preferable to use aluminum oxide, silicon oxide, titanium oxide, and cerium oxide, and it is even more preferable to use aluminum oxide. These metal oxides can be used either alone or in combination.
[0019] The shape of the support is not particularly limited, but may be in the form of porous particles, porous membrane, honeycomb, or monolith. In the case of porous particle shape, the particle size of the support is typically, but not limited to, 5 μm to 500 mm. The support may have a surface area of 1 m or less, but is not limited to this. 2 / g to 200m 2 In the catalyst according to the present invention, the metal having hydrogenation activity is preferably supported on the carrier in the form of particles, but is not limited thereto, and may be supported on the carrier in the form of, for example, needles, rods, films, nets, or the like.
[0020] The amount of metal supported in the catalyst is not limited, but is preferably 0.1 to 50% by mass relative to 100% by mass of the support. If the amount of metal supported is less than 0.1% by mass, the desired catalytic performance may not be obtained. If the amount of metal supported is more than 50% by mass, the cost increases.
[0021] The catalyst according to the present invention is characterized in that boron is added to the hydrogenation-active metal and support. The boron is added to the hydrogenation-active metal in the form of zero-valent boron. The addition of boron enables the catalyst according to the present invention to have improved hydrogenation reaction activity compared to conventional catalysts.
[0022] In the catalyst according to the present invention, the molar ratio of boron to metal is preferably 0.5 to 2.0, more preferably 0.8 to 1.2, and even more preferably about 1.0. If the molar ratio of boron to metal is less than 0.5, the desired catalytic performance may not be achieved. If the molar ratio is more than 2.0, the metal having hydrogenation activity may be covered with boron and not exposed.
[0023] The inventors have conducted experiments described below in which the catalyst according to the present invention was used to produce saturated hydrocarbons (specifically, methylcyclohexane) by hydrogenation of unsaturated hydrocarbons (specifically, toluene) as raw materials, and found that the conversion of the unsaturated hydrocarbons was equal to or higher than that achieved when a conventional catalyst was used. Furthermore, when the CO adsorption amount (equivalent to the amount of exposed metal) of the catalyst used in this experiment was measured, it was found that the CO adsorption amount of the catalyst according to the present invention was less than that of the conventional catalyst. The TOF of the catalyst was calculated using these results, and the TOF of the catalyst according to the present invention was found to be about 2.5 to about 3.4 times that of the conventional catalyst, demonstrating high hydrogenation activity.
[0024] Here, TOF (Turnover frequency) is a value that represents the amount of reactant that one active site (one metal atom) can process per unit time, and the higher this value, the higher the hydrogenation activity of the catalyst. TOF can be calculated using the following formula (1): TOF = (F x X / 100) / (W x U) (1), where F = supply rate of unsaturated hydrocarbon (mol / h), X = conversion rate (%), W = catalyst weight (g), and U = CO adsorption amount (mol / g).
[0025] The inventors of the present invention speculate as follows why the addition of boron increases the hydrogenation activity of the catalyst of the present invention compared to conventional catalysts. First, the inventors measured the XPS (X-ray photoelectron spectroscopy) spectrum of the catalyst of the present invention. As a result, it was found that the catalyst of the present invention contains both negatively charged (δ-) and non-negatively charged metals. Furthermore, unsaturated hydrocarbons, which are raw materials for hydrogenation reactions, are electron-rich and therefore do not easily adsorb to negatively charged metals. Non-Patent Document 2 reports a catalyst in which phosphorus is added to a ruthenium-containing catalyst. This document states that the ruthenium is charged δ+, and electron-rich toluene strongly adsorbs to this, resulting in higher hydrogenation activity than conventional catalysts. Therefore, it is believed that the catalyst of the present invention improves its hydrogenation activity through a mechanism different from that of Non-Patent Document 2.
[0026] The inventors believe that the high hydrogenation activity of the catalyst according to the present invention is due to the increased susceptibility of atomic hydrogen migration (spillover phenomenon) caused by the addition of boron. It is known that the addition of boron to transition metal-supported carbon reduces the activation energy of hydrogen atom migration (Non-Patent Document 3), and that negatively charged metals are more likely to generate spillover hydrogen (Non-Patent Document 4). Therefore, it is believed that the catalyst according to the present invention exhibits high hydrogenation activity due to a dual-functional mechanism in which unsaturated hydrocarbons are adsorbed and hydrogenated by non-negatively charged metals, and unsaturated hydrocarbons adsorbed by non-negatively charged metals are hydrogenated by spillover hydrogen generated by negatively charged metals. It is generally known that hydrogen dissociates (in the atomic form with the H-H bond cleaved) and adsorbs to metal atoms functioning as a catalyst. Depending on the conditions (catalyst metal, support, reaction temperature, etc.), the dissociated and adsorbed hydrogen can migrate across the support. This hydrogen that migrates across the support is called spillover hydrogen.
[0027] <Catalyst Manufacturing Method> Next, a method for manufacturing a catalyst according to the present invention will be described. The manufacturing method includes the steps of preparing a raw catalyst in which a metal is supported on a carrier, and adding boron to the raw catalyst. Hereinafter, a manufacturing method using an impregnation method will be described, but the manufacturing method is not limited to this, and for example, a coprecipitation method can also be used.
[0028] In the process of preparing a raw catalyst in which a metal is supported on a carrier, first, an aqueous solution of a starting material containing a metal having hydrogenation activity is prepared. A salt of a metal element having hydrogenation activity can be used as the starting material. When the metal having hydrogenation activity is platinum, the starting material can be, but is not limited to, chloroplatinic acid, tetraammineplatinum chloride, diamminedinitroplatinum nitrate, etc. When the metal having hydrogenation activity is rhodium, the starting material can be, but is not limited to, rhodium chloride, rhodium nitrate, hexaamminerhodium chloride, etc. The same applies to other metals having hydrogenation activity. The aqueous solution of the starting material can be prepared by adding the above starting material to water and stirring.
[0029] Next, the carrier is impregnated with an aqueous solution of the starting material, and if necessary, allowed to stand. It is preferable to dry the carrier before impregnating with the aqueous solution. After evaporating the water from the impregnated material and drying it, if necessary, the starting material is decomposed by heat treatment to obtain a raw catalyst.
[0030] The method for evaporating the water is not particularly limited, and can be carried out, for example, on a hot plate. The drying and heat treatment are preferably carried out in an inert gas atmosphere to prevent oxidation. The drying temperature, drying time, and heat treatment temperature are not particularly limited.
[0031] In the step of adding boron to the raw catalyst, the raw catalyst prepared as described above is impregnated with an organic solvent solution containing elemental boron, and if necessary, allowed to stand. The solution containing elemental boron is not limited, but can be prepared by adding, for example, triphenylborane, triethylborane, sodium borohydride, or the like to an organic solvent such as toluene, n-octane, or ethanol. The catalyst according to the present invention is obtained by evaporating the water from the raw catalyst impregnated with the solution and drying it.
[0032] The method for evaporating the water is not particularly limited, and can be carried out, for example, on a hot plate. Drying is preferably carried out in an inert gas atmosphere to prevent oxidation. The drying temperature and drying time are not particularly limited.
[0033] Next, the boron-added raw catalyst is reduced. The reduction is preferably carried out in a hydrogen atmosphere at a temperature of 650°C to 850°C for a predetermined period of time. By reducing the boron-added raw catalyst (also called a catalyst precursor) within the above temperature range, an active phase (boride) with high hydrogenation activity can be produced. If the reduction temperature is lower than 650°C, boride will not be produced well, and if the reduction temperature is higher than 850°C, sintering will occur, so neither is preferable.
[0034] <Method for Producing Organic Hydride> Next, a method for producing an organic hydride using the catalyst according to the present invention will be described. The production of organic hydride can be carried out using an apparatus well known to those skilled in the art, for example, but not limited to, a flow-bed reactor, a fixed-bed reactor, etc. The method for producing organic hydride includes a reaction step of bringing a raw material containing an unsaturated hydrocarbon and hydrogen into contact with the catalyst according to the present invention, and a separation step of separating the organic hydride from a product containing the organic hydride and hydrogen produced by the reaction step.
[0035] Examples of unsaturated hydrocarbons used as raw materials include, but are not limited to, benzene, toluene, and naphthalene. If necessary, one or a combination of these can be used as the raw unsaturated hydrocarbon. These compounds are classified as Class 4 Hazardous Materials, Class 1 Petroleum, similar to gasoline, and therefore can be used in existing infrastructure. Among these compounds, toluene is preferred as the raw unsaturated hydrocarbon, from the viewpoints of being a liquid at room temperature and pressure, being a gas at reaction temperatures, having a strong structure, having a stable benzene ring, and having little adverse effect on the environment and human body.
[0036] Examples of the organic hydride produced include, but are not limited to, cyclohexane, methylcyclohexane, and decalin. When toluene is used as a preferred unsaturated hydrocarbon, methylcyclohexane can be obtained as the organic hydride. Like toluene, methylcyclohexane also has advantages such as being a liquid at room temperature and pressure, being a gas at the reaction temperature, having a strong structure, a stable benzene ring, and having little adverse effect on the environment and human body.
[0037] The reaction formula for producing an organic hydride from a raw material containing an unsaturated hydrocarbon and hydrogen is, for example, expressed by the following formula: 6 H 6 +3H 2 → C 6 H 12 (Benzene hydrogenation reaction) C 7 H8 +3H 2 → C 7 H 14 (Toluene hydrogenation reaction) C 10 H 8 +5H 2 → C 10 H 18 (Naphthalene Hydrogenation Reaction)
[0038] In the reaction step, a raw material containing unsaturated hydrocarbons and hydrogen is supplied to the reactor. It is preferable to supply a raw material gas containing a mixture of unsaturated hydrocarbons and hydrogen to the reactor as a raw material. In this case, the unsaturated hydrocarbons are preheated and mixed with hydrogen gas in the form of a gas before being supplied to the reactor. The method of supplying the raw material to the reactor is not limited thereto. For example, the unsaturated hydrocarbons may be supplied to the reactor in a liquid or gaseous state, and hydrogen gas may be added thereto, or hydrogen gas may be supplied to the reactor first, and the unsaturated hydrocarbons in a liquid or gaseous state may be added thereto. In either case, it is sufficient that the reaction between the unsaturated hydrocarbons and hydrogen occurs on the catalyst.
[0039] The reaction temperature in the reaction step is preferably 30°C to 500°C, more preferably 80°C to 250°C, and even more preferably 100°C to 200°C. If the reaction temperature is lower than 30°C, the raw materials will liquefy, reducing the reaction field and reducing the reaction efficiency. Furthermore, a low reaction temperature can cause problems such as the required reaction rate not being achieved and the product being less likely to separate from the catalyst surface. If the reaction temperature is higher than 500°C, coking, which causes catalyst deterioration, will be induced. Therefore, in equilibrium reactions, the equilibrium shifts toward counteracting the exothermic reaction (i.e., toward the endothermic reaction) under high-temperature conditions. Therefore, in the case of a hydrogenation reaction, which is an exothermic reaction, high-temperature conditions are unfavorable in terms of equilibrium, resulting in a reduced reaction rate.
[0040] The reaction pressure in the reaction step is preferably 0 MPaG to 10 MPaG, and more preferably 0 MPaG to 1 MPaG. If the reaction pressure is lower than 0 MPaG, the reaction efficiency decreases. If the reaction pressure is higher than 10 MPaG, the catalyst may deteriorate, reducing the durability of the device. In particular, if the catalyst according to the present invention is used, an efficient hydrogenation reaction can proceed even at a low reaction pressure of 0 MPaG to 1 MPaG. The catalyst according to the present invention is able to increase the hydrogenation activity even in such a low-pressure reaction because, as already explained, the addition of boron makes the spillover phenomenon more likely to occur.
[0041] The inventors of the present invention consider the temperature and pressure of the reaction step using the catalyst of the present invention as follows: From the viewpoints of increasing the conversion rate of the reactants, reducing the energy supplied to the apparatus, and reducing the burden on components such as the reactor, it is preferable that the reaction step be carried out at as low a temperature and pressure as possible. Therefore, the catalyst of the present invention, which has higher hydrogenation activity at lower temperatures and pressures than conventional catalysts, is extremely suitable for producing organic hydrides.
[0042] In order for the reaction to produce organic hydrides to proceed efficiently, it is preferable that the temperature of the reaction step be (1) equal to or higher than the boiling points of the reactants (i.e., unsaturated hydrocarbons) and the product (organic hydride), and lower than (2). Regarding (1), in order to diffuse the reactants and the product throughout the reactor and increase the number of reaction sites, the reactants and the product need to be gaseous, and for this reason, it is important that the temperature of the reaction step be higher than the boiling points of the reactants and the product. Regarding (2), when the temperature of the reaction step increases, the equilibrium shifts from the hydrogenation reaction to the dehydrogenation reaction. Therefore, by carrying out the reaction at a lower temperature, a high conversion rate of the reactants can be obtained, and energy consumption during the reaction can be reduced, thereby reducing the burden on components.
[0043] Taking toluene as an example of a reactant, the boiling point of toluene is about 110°C at atmospheric pressure (0.1 MPaG) and above 200°C at a typical reaction pressure of 0.7 MPaG. When the catalyst of the present invention, which has high hydrogenation activity even at low pressures, is used, the reaction can be carried out at 0 MPaG to 0.3 MPaG, and the reaction step can be carried out at about 110 to 160°C, which is the boiling point of toluene at this pressure. In other words, when conventional catalysts are used, the reaction step is generally carried out at temperatures above 200°C, but when the catalyst of the present invention is used, the apparatus can be operated at a lower temperature.
[0044] Before carrying out the reaction step, it is preferable to reduce the catalyst according to the present invention in a hydrogen atmosphere. The reduction is preferably carried out at a temperature of 150°C to 400°C for a predetermined time. By reducing the catalyst within the above temperature range, it is possible to remove the oxide film on the catalyst surface. It is known that conventional catalysts are also reduced before use for the same purpose, but the reduction temperature for conventional catalysts is approximately 100°C to 200°C. In contrast, the catalyst according to the present invention can be reduced at a higher temperature range than conventional catalysts. As already explained, the catalyst according to the present invention can be reduced at a higher temperature range.
[0045] When an organic hydride is produced in the reaction step, a product containing the produced organic hydride and hydrogen is discharged from the reactor. The discharged product is cooled to form a mixture of liquid organic hydride and hydrogen gas, and the hydrogen gas is removed from this product to separate the liquid organic hydride. The separation step of separating the organic hydride from the product can be performed using a gas-liquid separator well known to those skilled in the art.
[0046] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0047] <Catalyst Production> (Example 1) A boron-doped platinum catalyst supported on alumina (B / Pt / Al 2 O 3First, a platinum catalyst supported on alumina (Pt / Al) was used as the raw catalyst. 2 O 3 As a starting material containing platinum, chloroplatinic acid hexahydrate (H 2 PtCl 6 ・6H 2 Chloroplatinic acid hexahydrate was added to water and stirred to prepare an aqueous solution.
[0048] After drying the alumina carrier at 400°C for 1 hour, the alumina was impregnated with the above aqueous solution and allowed to stand for 24 hours. The amount of platinum supported was adjusted to 5% by mass relative to 95% by mass of alumina. Next, the carrier to which the aqueous solution had been added was evaporated to dryness at 90°C to 100°C on a hot plate, dried at 110°C in a nitrogen stream (70 mL / min) for 24 hours, and further heated at 450°C in a nitrogen stream (200 mL / min) for 1 hour to decompose the platinum chloride. This yielded an alumina-supported platinum catalyst as a raw catalyst.
[0049] Next, triphenylborane (B(C)) manufactured by Strem Chemicals, Inc. 6 H 5 ) 3 ) was dissolved in toluene to prepare a toluene solution. The amount of triphenylborane dissolved was adjusted so that the molar ratio of boron to platinum in the alumina-supported platinum catalyst was 1. The alumina-supported platinum catalyst was impregnated with the toluene solution of triphenylborane and allowed to stand for 24 hours. Next, the alumina-supported platinum catalyst to which the toluene solution had been added was evaporated to dryness on a hot plate at 90°C to 100°C, and then dried at 110°C in a nitrogen stream (70 mL / min) for 24 hours. This yielded a boron-added alumina-supported platinum catalyst.
[0050] Example 2 As Example 2, a boron-doped rhodium catalyst supported on alumina (B / Rh / Al 2 O 3 The catalyst was prepared by using rhodium chloride trihydrate (RhCl) manufactured by Kanto Chemical Co., Inc. as a starting material containing rhodium. 3 ・3H 2 The procedure is the same as in Example 1 except that the cellulose acylate 1 was used.
[0051] <Evaluation of catalyst performance> The catalyst of Example 1 (boron-doped alumina-supported platinum catalyst (B / Pt / Al 2 O 3 )) and the catalyst of Example 2 (boron-loaded alumina-supported rhodium catalyst (B / Rh / Al 2 O 3 ) and the catalyst of Comparative Example 1 (alumina-supported platinum catalyst (Pt / Al 2 O 3 )) and the catalyst of Comparative Example 2 (alumina-supported rhodium catalyst (Rh / Al 2 O 3 )) was used to carry out a toluene hydrogenation reaction. The catalysts of Comparative Example 1 and Comparative Example 2 were the raw material catalysts used to produce the catalysts of Example 1 and Example 2, respectively. In the following, the catalyst of Example 1 will be referred to as "Pt-B", the catalyst of Example 2 as "Rh-B", the catalyst of Comparative Example 1 as "Pt", and the catalyst of Comparative Example 2 as "Rh". The hydrogenation reaction was carried out using an atmospheric pressure fixed-bed flow reactor.
[0052] The hydrogenation reaction conditions were as follows: catalyst amount: 0.02 g catalyst reduction conditions: H 2 (30 mL / min), 850°C, 1 hour Reaction temperature 150°C Raw material gas Toluene:H 2 :N 2 = 3.8:16.25:81.25 kPa Raw material gas flow rate H 2 +N 2 30 mL / min Toluene 1.17 mL / min (3.13 x 10 -3 mol / h) Reaction time: 180 min (product gas analysis every 30 min)
[0053] The experiment was carried out as follows: First, the catalyst was placed in the reactor, and the reactor was assembled into the device. Then, the air in the device was replaced with hydrogen gas (at 30 mL / min for 10 minutes). Next, in both the example and the comparative example, the catalyst was reduced with hydrogen at 850°C for 1 hour. Next, the raw material gas was passed through the reactor and brought into contact with the catalyst, producing methylcyclohexane.
[0054] The reaction product (a mixture of methylcyclohexane, unreacted toluene, and hydrogen) was extracted from the apparatus using a syringe and analyzed using a gas chromatograph equipped with a flame ionization detector. The analysis conditions were as follows: Carrier gas: N 2 (200 kPa) Column DB-1 (30 m) Column temperature 60°C-140°C Analysis time 21 min Sample inlet temperature 280°C Detector temperature 280°C From the area of toluene obtained by analysis, the toluene conversion rate was calculated using the following formula (2): Conversion rate [%] = area of all products / (area of all products + area of unreacted toluene) × 100 (2)
[0055] H 2 In a 10 mL / min flow rate, 0.1 g of catalyst was heated to the reduction temperature at 10°C / min and reduced for 1 hour. After cooling to 25°C in He (30 mL / min), CO was passed through the catalyst layer every 3 minutes using a pulse method with He as the carrier gas. The CO after passing through the catalyst layer was analyzed using a gas chromatograph equipped with a thermal conductivity detector. After 10 pulses of CO adsorption, the CO adsorption amount was calculated from the sum of the difference between the average area at saturated adsorption and the area before saturated adsorption. The TOF of the catalyst was calculated using the above-mentioned formula (1).
[0056]
[0057] The toluene conversion, CO adsorption amount, and TOF obtained for the catalysts of the Examples and Comparative Examples are shown in Table 1. When the catalyst of Example 1 (Pt-B) was used, the toluene conversion was about 73%. In contrast, with the catalyst of Comparative Example 1 (Pt), the toluene conversion was about 36%, which was roughly half the conversion of Example 1. The CO adsorption amount (equivalent to the amount of exposed metal) of the catalyst of Comparative Example 1 was about 59 μmol / g. In contrast, with the catalyst of Example 1, the CO adsorption amount was reduced to about 36 μmol / g. The TOF obtained from these toluene conversion and CO adsorption amount using the above formula (1) was 3.2 × 10 for the catalyst of Example 1. 3 (h -1), whereas the catalyst of Comparative Example 1 had a yield of 9.5 × 10 2 (h -1 ) and the TOF of the catalyst of Example 1 was about 3.4 times that of the catalyst of Comparative Example 1.
[0058] Similarly, in the cases of Example 2 (Rh-B) and Comparative Example 2 (Rh), the TOF was calculated using the toluene conversion rate and the CO adsorption amount. The TOF of the catalyst of Example 2 was 6.4 × 10 2 (h -1 ), while the catalyst of Comparative Example 2 was 2.6 × 10 2 (h -1 ), and the TOF of the catalyst of Example 2 was about 2.5 times that of the catalyst of Comparative Example 2. When Example 2 and Comparative Example 2 are compared, the toluene conversion rate of Example 2 is equivalent to (or slightly lower than) that of Comparative Example 2. However, the CO adsorption amount of Example 2 was significantly smaller than that of Comparative Example 2. As a result, the TOF of the catalyst of Example 2 was larger than that of the catalyst of Comparative Example 2.
[0059] These results show that the addition of boron improves the hydrogenation activity of the catalyst. Comparing the TOF of the catalyst of Example 1 and the catalyst of Example 2, the TOF of Example 1 is higher than the TOF of Example 2. Therefore, the catalyst of Example 1, i.e., the catalyst using platinum as the metal having hydrogenation activity, exhibits superior hydrogenation activity compared to the catalyst of Example 2, i.e., the catalyst using rhodium as the metal having hydrogenation activity.
Claims
1. A catalyst comprising: a metal having activity in a hydrogenation reaction; a support supporting said metal; and boron added to said metal.
2. The catalyst of claim 1, wherein the molar ratio of said boron to said metal is from 0.5 to 2.
0.
3. The catalyst of claim 1, wherein the metal is a platinum group metal.
4. The catalyst of claim 3, wherein the metal is platinum or rhodium or both.
5. The catalyst according to claim 1, wherein the support is a metal oxide.
6. The catalyst according to claim 5, wherein the support is aluminum oxide, silicon oxide, titanium oxide or cerium oxide or a combination thereof.
7. A method for producing a catalyst according to any one of claims 1 to 6, comprising the steps of: preparing a raw catalyst in which a metal is supported on a carrier; adding boron to the raw catalyst; and reducing the raw catalyst to which boron has been added.
8. The method for producing a catalyst according to claim 7, wherein the step of adding boron to the raw catalyst comprises: impregnating the raw catalyst with an organic solvent solution of a boron compound; and drying the raw catalyst impregnated with the organic solvent solution.
9. The method for producing a catalyst according to claim 8, wherein the boron compound is any one or a combination of triphenylborane, triethylborane, and sodium borohydride.
10. The method for producing a catalyst according to claim 7, wherein the step of reducing the raw catalyst to which boron has been added includes reducing the raw catalyst in a hydrogen atmosphere at 650°C to 850°C.
11. A method for producing an organic hydride, comprising: a step of reducing the catalyst according to any one of claims 1 to 6; a reaction step of contacting the reduced catalyst with a raw material containing an unsaturated hydrocarbon and hydrogen; and a separation step of separating the organic hydride from a product containing the organic hydride and hydrogen produced by the reaction step.
12. The method of claim 11, wherein the step of reducing the catalyst comprises reducing the catalyst under a hydrogen atmosphere at 150°C to 400°C.
13. The method according to claim 11, wherein the reaction step is carried out at a reaction pressure of 0 MPaG to 10 MPaG.
14. The method according to claim 13, wherein the reaction step is carried out at a reaction pressure of 0 MPaG to 1 MPaG.
15. The method of claim 11, wherein the unsaturated hydrocarbon is toluene and the organic hydride is methylcyclohexane.
Citation Information
Patent Citations
Benzene saturation hydrogenation supporting type amorphous catalyst and preparation method thereof
CN1465433A
Amorphous alloy catalyst containing boron, its production and use
JP1998296083A
Catalyst composition for hydrogenating aromatic hydrocarbon
JP1999309372A