Molded body, composite material, and method for producing composite material

By removing particulate matter from poly(p-phenylenebenzobisoxazole) fibers and coating them with a resin, the composite material achieves reduced thermal expansion and improved stability, addressing the thermal expansion issues in molded articles made from poly(p-phenylenebenzobisoxazole) fibers.

WO2024225245A1PCT designated stage expired Publication Date: 2024-10-31MITSUBISHI GAS CHEM CO INC +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015819
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Molded articles made from composite materials using poly(p-phenylenebenzobisoxazole) fibers are prone to thermal expansion due to the attachment of poly(p-phenylenebenzobisoxazole) particles on the fiber surface, which affects their thermal stability and performance.

Method used

The use of poly(p-phenylenebenzobisoxazole) fibers with particulate matter removed, where the fibers are coated with a resin and have a high mass proportion in the composition, and are oriented in the in-plane direction of the film, to create a composite material that suppresses thermal expansion.

Benefits of technology

The resulting composite material exhibits reduced thermal expansion and improved thermal stability, with enhanced mechanical properties such as high elastic modulus and efficient heat diffusion, making it suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015819_31102024_PF_FP_ABST
    Figure JP2024015819_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose is to provide a molded body, a composite material for producing the molded body, and a method for producing a composite material. Provided is a molded body formed from a composition containing a resin and fibers (X) of poly(p-phenylenebenzobisoxazole), wherein the ratio of the fibers (X) to 100 mass% of the poly(p-phenylenebenzobisoxazole) contained in the composition is 50 mass% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Molded body, composite material, and method for producing composite material

[0001] The present invention relates to a molded article, a composite material, and a method for producing a composite material, and more particularly to a molded article using poly(p-phenylene benzobisoxazole) fibers.

[0002] Conventionally, composite materials using poly(p-phenylene benzobisoxazole) fibers have been known as one type of fiber-reinforced resin composite material. Regarding the poly(p-phenylene benzobisoxazole) fibers used in such composite materials, Patent Document 1 describes that nanofiber poly(p-phenylene benzobisoxazole) fibers can be produced by completely dissolving poly(p-phenylene benzobisoxazole) in sulfuric acid or the like to prepare a solution, and then quenching this solution at a rate of 0.2°C / min or more. Patent Document 2 discloses a method for producing a composite material in which poly(p-phenylene benzobisoxazole) crystals are dispersed in a matrix resin. The poly(p-phenylene benzobisoxazole) nanofibers have a length dimension of 0.01 μm or more in the longitudinal direction and a dimension of 1 nm to 1 μm in the direction perpendicular to the longitudinal direction, are parallel to each other in the longitudinal direction, and are bonded in the direction perpendicular to the longitudinal direction to accumulate in bundles. The method includes the steps of: dispersing the poly(p-phenylene benzobisoxazole) crystals in a dispersion solution to prepare a first solution; dissolving a matrix resin in the same dispersion solution used for the first solution to prepare a second solution; mixing the first solution and the second solution to prepare a mixed solution in which the poly(p-phenylene benzobisoxazole) crystals are dispersed; and pouring the mixed solution into a predetermined container and drying it.

[0003] JP 2015-110854 A International Publication No. 2016 / 178427

[0004] The present inventors investigated the method described in Patent Document 2 and found that molded articles obtained from the composite material are prone to thermal expansion. Further investigation into the reason for this revealed that the poly(p-phenylene benzobisoxazole) crystals described in Patent Document 2 are aggregates in which poly(p-phenylene benzobisoxazole) particles are bonded to the surfaces of poly(p-phenylene benzobisoxazole) fibers, as shown in FIG. 1, for example, and that molded articles obtained by dispersing such aggregates in a resin are prone to thermal expansion. The present invention aims to solve this problem by providing a molded article that is resistant to thermal expansion, a composite material for producing the molded article, and a method for producing the composite material.

[0005] In light of the above-mentioned problems, the present inventors have conducted research and found that the above-mentioned problems can be solved by using poly(p-phenylene benzobisoxazole) fibers (X) obtained by subjecting poly(p-phenylene benzobisoxazole) aggregates, as described in Patent Document 2, etc., to ultrasonic treatment or the like to remove surface particulate matter. In particular, the inventors have found that moldings using poly(p-phenylene benzobisoxazole) fibers (X) partially or entirely coated with a resin can produce molded articles that are resistant to thermal expansion. Specifically, the above-mentioned problems have been solved by the following means. <1> A molded article formed from a composition containing a resin and poly(p-phenylene benzobisoxazole) fibers (X), wherein the proportion of the fibers (X) relative to 100% by mass of poly(p-phenylene benzobisoxazole) contained in the composition is 50% by mass or more. <2> The molded article according to <1>, wherein the difference (ΔW) between the maximum and minimum widths of the fibers (X) is 35 nm or less. <3> The molded article according to <1>, wherein the difference (ΔW) between the maximum and minimum widths of the fibers (X) is 30 nm or less. <4> The molded article according to any one of <1> to <3>, wherein the ratio of the fibers (X) to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composition is 80 mass% or more. <5> The molded article according to any one of <1> to <4>, wherein the composition contains 0.01 to 30 parts by mass of the fibers (X) per 100 parts by mass of the resin. <6> The molded article according to any one of <1> to <5>, wherein the molded article is a film. <7> The molded article according to <6>, wherein the fibers (X) are oriented in the in-plane direction of the film. <8> The molded body according to any one of <1> to <7>, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 30 nm or less, a ratio of the fiber (X) to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the molded body is 80 mass% or more, the composition contains 0.01 to 30 mass parts of the fiber (X) to 100 mass parts of the resin, the molded body is a film, and the fiber (X) is oriented in an in-plane direction of the film.<9> A composite material comprising a fiber (X) of poly(p-phenylene benzobisoxazole) and a resin that coats part or all of the fiber (X), wherein a proportion of the fiber (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composite material is 50 mass% or more. <10> The composite material according to <9>, wherein the difference (ΔW) between the maximum and minimum widths of the fiber (X) is 35 nm or less. <11> The composite material according to <9>, wherein the difference (ΔW) between the maximum and minimum widths of the fiber (X) is 30 nm or less. <12> The composite material according to any one of <9> to <11>, wherein a proportion of the fiber (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composite material is 80 mass% or more. <13> The composite material according to any one of <9> to <12>, wherein the composite material contains 100 to 9,900 parts by mass of the resin relative to 100 parts by mass of the fiber (X). <14> The composite material according to any one of <9> to <13>, wherein the fiber (X) has a difference (ΔW) between its maximum and minimum widths of 30 nm or less, the proportion of the fiber (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composite material is 80 mass% or more, and the composite material contains 100 to 9,900 parts by mass of the resin relative to 100 parts by mass of the fiber (X). <15> The method for producing a composite material according to any one of <9> to <14>, comprising: a step of ultrasonically treating aggregates of poly(p-phenylene benzobisoxazole) in a solvent; a step of separating poly(p-phenylene benzobisoxazole) fibers (X) from the ultrasonically treated liquid to obtain a dispersion of poly(p-phenylene benzobisoxazole) fibers (X); a step of mixing the dispersion with a resin to obtain a mixture containing poly(p-phenylene benzobisoxazole) fibers (X), the resin, and a solvent; and a step of removing the solvent from the mixture. <16> The method for producing a composite material according to <15>, in which a content of the resin in 100% by mass of the mixture is 0.05 to 50% by mass.<17> A method for producing a molded body, comprising the steps of: ultrasonically treating aggregates of poly(p-phenylene benzobisoxazole) in a solvent; separating poly(p-phenylene benzobisoxazole) fibers (X) from the ultrasonically treated liquid to obtain a dispersion of poly(p-phenylene benzobisoxazole) fibers (X); mixing the dispersion with a thermosetting resin to obtain a mixture containing poly(p-phenylene benzobisoxazole) fibers (X), the thermosetting resin, and a solvent; removing the solvent from the mixture; and curing the thermosetting resin. <18> A method for producing a molded body according to <17>, wherein the thermosetting resin is soluble in the solvent contained in the dispersion at 23°C. <19> A mat formed using poly(p-phenylene benzobisoxazole) containing fibers (X) of poly(p-phenylene benzobisoxazole), wherein the proportion of the fibers (X) relative to 100 mass% of the poly(p-phenylene benzobisoxazole) contained in the mat is 50 mass% or more. <20> The mat according to <19>, wherein the difference (ΔW) between the maximum and minimum widths of the fibers (X) is 35 nm or less. <21> The mat according to <19>, wherein the difference (ΔW) between the maximum and minimum widths of the fibers (X) is 30 nm or less. <22> The mat according to any one of <19> to <21>, wherein the proportion of the fibers (X) relative to 100 mass% of the poly(p-phenylene benzobisoxazole) contained in the mat is 80 mass% or more.

[0006] The present invention makes it possible to provide a molded body that is resistant to thermal expansion, a composite material for producing the molded body, and a method for producing the composite material.

[0007] 1 is a photograph of an example of an aggregate of poly(p-phenylene benzobisoxazole) fibers with poly(p-phenylene benzobisoxazole) particles attached to their surfaces, observed with an electron microscope. This is an image of the ultrasonic treatment of poly(p-phenylene benzobisoxazole) aggregates. This is a photograph of a single poly(p-phenylene benzobisoxazole) fiber (X) obtained in Example 1, observed with an electron microscope. This shows the distribution of fiber widths of the fibers obtained in Example 1 and Comparative Example 1. This shows the distribution of the difference (ΔW) between the maximum and minimum widths of the fibers obtained in Example 1 and Comparative Example 1. This shows the distribution of the length of the fibers obtained in Example 1 and Comparative Example 1. This shows the distribution of the aspect ratios of the fibers obtained in Example 1 and Comparative Example 1. This shows the results of observation of the molded product obtained in Example 1 by scanning probe microscopy (SPM). This shows the results of observation of the molded product obtained in Example 3 by scanning probe microscopy (SPM). 1 shows the results of X-ray diffraction measurement when X-rays are incident from the in-plane direction of a mat of PBO fibers (X).

[0008] Hereinafter, a detailed description of an embodiment of the present invention (hereinafter simply referred to as "the present embodiment") will be provided. The following present embodiment is an example for explaining the present invention, and the present invention is not limited to this embodiment. In this specification, the term "to" is used to mean that the numerical values ​​before and after the term are included as lower and upper limits. In this specification, various physical property values ​​and characteristic values ​​are those at 23°C unless otherwise specified. In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved. In this specification, a film refers to a generally flat molded product that is thin relative to its length and width. In this specification, the term "film" also includes a "sheet." The film may be either single-layer or multi-layer, although single-layer is preferred. If the measurement methods and other information described in the standards set forth in this specification vary from year to year, they shall be based on the standards as of January 1, 2023, unless otherwise specified. Figure 2 may not be consistent with reality.

[0009] The molded article of this embodiment is formed from a composition containing a resin and poly(p-phenylene benzobisoxazole) fibers (X), characterized in that the ratio of the fibers (X) to 100% by mass of poly(p-phenylene benzobisoxazole) contained in the composition is 50% by mass or more. This configuration makes it possible to provide a molded article that is resistant to thermal expansion. Poly(p-phenylene benzobisoxazole) (hereinafter sometimes abbreviated as "PBO") aggregates had particulate matter attached to the surface of the PBO fibers. In this embodiment, it is presumed that significant suppression of thermal expansion of the molded article was achieved by producing the molded article using PBO fibers (X) from which the particulate matter had been removed. It is presumed that thermal diffusion was achieved in the molded article of this embodiment because the PBO fibers (X) could be sufficiently dispersed in the resin. That is, since PBO fibers (X) usually have higher thermal conductivity than resins, it is presumed that the PBO fibers (X) are in a state where paths are connected in a mesh-like or similar manner, which makes heat diffusion easier. Furthermore, the molded body of this embodiment tends to be more susceptible to thermal expansion. This is presumed to be because the PBO fibers (X) and resin are bonded to each other in a compatible manner in the molded body of this embodiment. That is, when a resin molded body is heated, the resin tends to flow, although this depends on the type of resin. Since the multilayer body of this embodiment is bonded to PBO fibers (X), which are less likely to expand, it is presumed that thermal expansion when heated can be effectively suppressed.

[0010] Here, PBO (poly(p-phenylene-2,6-benzobisoxazole)) is a compound having the following structural unit, and typically, 90% by mass or more (preferably 95% by mass or more) of the structural units have the following structure:

[0011] The weight average molecular weight of the PBO is determined from the intrinsic viscosity measured using a viscometer, and is preferably 10,000 or more and 100,000 or less.

[0012] The proportion of the PBO fiber (X) relative to 100% by mass of poly(p-phenylene benzobisoxazole) contained in the composition is 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more, and the upper limit may be 100% by mass. Furthermore, the difference (ΔW) between the maximum and minimum widths of the PBO fiber (X) is preferably 35 nm or less, more preferably 30 nm or less. Ideally, the lower limit of the difference (ΔW) between the maximum and minimum widths of a single fiber is 0 nm, but a value greater than 0 nm is practical. The fiber width refers to the length of the fiber in the direction perpendicular to the fiber length (longitudinal direction). Specifically, this value is measured according to the method described in the Examples below. In this embodiment, the PBO fiber (X) is preferably not in the form of a bundle or a block, but is preferably a single fiber (single fiber). Furthermore, the fiber (X) in this embodiment is preferably a nanofiber. Nanofibers are difficult to produce by melt spinning. This embodiment is highly valuable in that such nanofibers can be obtained.

[0013] PBO fiber (X) can be obtained, for example, by ultrasonically treating PBO agglomerates and separating the PBO fiber (X). Figure 2 is an image diagram of the process of ultrasonically treating PBO agglomerates to obtain PBO fiber (X). That is, when PBO agglomerates 1 are ultrasonically treated, particulate matter 2 adhering to the surface of the PBO agglomerates 1 is separated from PBO fiber (X) 3. Then, in this separated state, PBO fiber (X) 3 can be separated by filtration or the like. The method for separating PBO fiber (X) will be described later.

[0014] As described above, the molded article of this embodiment is formed from a composition containing a resin and poly(p-phenylenebenzobisoxazole) fibers (X). The content of the PBO fibers (X) in this composition is preferably 0.01 parts by mass or more, more preferably 0.025 parts by mass or more, even more preferably 0.05 parts by mass or more, and even more preferably 0.10 parts by mass or more, relative to 100 parts by mass of the resin. By setting the content at or above the lower limit, a molded article that is less prone to thermal expansion tends to be obtained. Furthermore, the upper limit of the resin content is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the resin. By setting the content at or below the upper limit, a molded article with a high elastic modulus tends to be obtained. Of the PBO contained in the composition, the total amount of non-fibrous PBO (i.e., PBO in the form of aggregates or particles) is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the PBO contained in the composition. The lower limit may be 0% by mass.

[0015] The PBO fibers (X) contained in the composition preferably have a longitudinal length (fiber length) of 1 μm or more, more preferably 1.5 μm or more, and preferably 5 μm or less, more preferably 4 μm or less. The PBO fibers (X) contained in the composition preferably have a length in the direction perpendicular to the longitudinal direction (fiber width) of 50 nm or more, more preferably 60 nm or more, and preferably 150 nm or less, more preferably 130 nm or less.

[0016] The PBO fiber (X) contained in the composition preferably has an aspect ratio of 50 or less, and preferably 10 or more. The fiber length, fiber width, and aspect ratio of the PBO fiber (X) are the median values ​​of values ​​obtained by randomly sampling 20 to 25 fibers from the composition.

[0017] The PBO fiber (X) of this embodiment can be used as a mat. Specifically, a mat formed using poly(p-phenylene benzobisoxazole) containing poly(p-phenylene benzobisoxazole) fiber (X) is disclosed, wherein the proportion of the fiber (X) relative to 100 mass% of the poly(p-phenylene benzobisoxazole) contained in the mat is 50 mass% or more. The size of the PBO fiber (X) in the mat and the proportion of the PBO fiber (X) contained in the mat are the same as those for the molded product described above, and the preferred ranges are also the same. The mat can be obtained by dispersing the PBO fiber (X) in a dispersion medium (e.g., water), removing the dispersion medium, and then press-molding the mixture into a mat shape. The proportion of the PBO fiber (X) in the dispersion medium is preferably 0.0001 to 99 mass%. The dispersion medium is preferably removed by filtration.

[0018] The molded article of this embodiment can be produced, for example, by directly blending PBO fibers (X) into a resin. The term "resin" as used herein refers not only to thermoplastic resins but also to components that harden through a polymerization reaction, including, for example, thermosetting oligomers and low-molecular-weight thermosetting compounds. The method of producing a molded article by directly blending PBO fibers (X) into a resin is preferably used when the resin is a thermosetting resin, particularly when the resin is soluble in a solvent or is a liquid at room temperature (e.g., 23°C). That is, an example of a method for producing a molded article of this embodiment includes the steps of ultrasonically treating PBO aggregates in a solvent, separating PBO fibers (X) from the ultrasonically treated liquid to obtain a dispersion of PBO fibers (X), mixing the dispersion with a thermosetting resin to obtain a mixture containing PBO fibers (X), a thermosetting resin, and a solvent, removing the solvent from the mixture, and curing the thermosetting resin. In this embodiment, the thermosetting resin is preferably soluble in the solvent contained in the dispersion at 23°C. The solvent used to ultrasonically treat the PBO aggregates and the solvent contained in the dispersion of PBO fiber (X) may be the same or different. The resin soluble in the solvent is not particularly limited, but examples include thermosetting resins, with thermosetting polyimide resins, epoxy resins, phenolic resins, thermosetting polyester resins, melamine resins, vinyl ester resins, and cyanate resins being more preferred, and epoxy resins being even more preferred. Furthermore, when a thermosetting resin is used, it is preferable to further contain a curing accelerator such as imidazole. The curing accelerator is not particularly limited, and examples include those commonly used in resin compositions for electronic materials. For details of the curing accelerator, please refer to paragraphs 0195 to 0196 of WO 2024 / 034276, the contents of which are incorporated herein by reference. When contained, the content of the curing accelerator is, for example, 0.001 mass % or more and, for example, 10 mass % or less, preferably 5 mass % or less, based on the mass of the composition or molded article.

[0019] Another example of a method for producing a molded article according to this embodiment is to produce the article using a composite material in which PBO fibers (X) are partially or entirely coated with a resin, rather than PBO aggregates. That is, in this embodiment, a composite material containing PBO fibers (X) and a resin that partially or entirely coats the fibers (X), wherein the ratio of the fibers (X) to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composite material is preferably used. In this way, by molding a composite material in which PBO fibers (X), obtained by separating PBO granules from PBO aggregates and partially or entirely coating the PBO fibers (X) with a resin, and then further incorporating a resin (a post-added resin, as described below), the PBO fibers (X) can be appropriately oriented in the molded article, resulting in a molded article in which thermal expansion is effectively suppressed. In particular, when the molded article is a film, the fibers (X) can be oriented in the in-plane direction of the film, further effectively suppressing thermal expansion. Such a method for producing a molded article via a composite material is preferably used when the resin is a thermoplastic resin, preferably a polycarbonate resin, a polyolefin resin, a styrene resin, an acrylic resin, a thermoplastic polyester resin, a thermoplastic polyimide resin, a polyacetal resin, a polyamide resin, a polyphenylene ether resin, or a polyamideimide resin, more preferably a polycarbonate resin.

[0020] The PBO fiber (X) contained in the composite material is synonymous with the PBO fiber (X) contained in the composition. Therefore, the size (width, etc.) of the fiber (X) contained in the composite material and the ratio of the PBO fiber (X) to 100% by mass of the total amount of PBO are the same as those for the composition, and the preferred ranges are also the same.

[0021] On the other hand, in a composite material, the resin may be present in an amount sufficient to partially or entirely cover the PBO fibers (X). Specifically, the resin content in the composite material is preferably 100 parts by mass or more, more preferably 150 parts by mass or more, even more preferably 200 parts by mass or more, and even more preferably 233 parts by mass or more, per 100 parts by mass of the PBO fibers (X). By setting the resin content at or above the lower limit, the PBO fibers (X) tend to be more easily dispersed in a molded product during production. Furthermore, the upper limit of the resin content is preferably 9,900 parts by mass or less, more preferably 3,233 parts by mass or less, even more preferably 1,900 parts by mass or less, even more preferably 900 parts by mass or less, and even more preferably 233 parts by mass or less, per 100 parts by mass of the PBO fibers (X). Setting the resin content at or below the upper limit tends to make it easier to control the amount of PBO fibers (X) in a molded product. The composite material of this embodiment may contain only one type of resin, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range. Furthermore, in the composite material of this embodiment, the total of the resin and the PBO fiber (X) usually accounts for 95% by mass or more, preferably 97% by mass or more, more preferably 99% by mass or more, and may even be 100% by mass.

[0022] Furthermore, the resins used in this embodiment, for example, the resins contained in the composite material and the resins contained in the composition other than the resins constituting the composite material (hereinafter sometimes referred to as "later-added resins"), may each be thermoplastic resins or thermosetting resins, with thermoplastic resins being preferred. Examples of thermoplastic resins include polycarbonate resins, polyolefin resins, styrene resins, acrylic resins, thermoplastic polyester resins, thermoplastic polyimide resins, polyacetal resins, polyamide resins, polyphenylene ether resins, and polyamideimide resins, with polycarbonate resins being preferred. Examples of thermosetting resins include thermosetting polyimide resins, epoxy resins, phenolic resins, thermosetting polyester resins, melamine resins, vinyl ester resins, and cyanate resins, with epoxy resins being preferred. Photocurable resins and polymerizable compounds that polymerize with a catalyst such as (meth)acrylate can also be used. The resins used in this embodiment, for example, the resins contained in the composite material and the later-added resins, may each contain only one type of resin or two or more types of resins. In this embodiment, the resin contained in the composite material and the later-added resin may be the same or different. In one example of this embodiment, the resin contained in the composite material and the post-added resin preferably share 80% by mass or more in common, more preferably 85% by mass or more in common, even more preferably 90% by mass or more in common, and may even share 100% by mass.

[0023] In addition to the resin and PBO fiber (X), the composition or molded article of this embodiment may contain other components within the scope of this embodiment. Specific examples include release agents, colorants, stabilizers (such as heat stabilizers and antioxidants), flame retardants, flame retardant assistants, anti-dripping agents, UV absorbers, fluorescent brighteners, impact modifiers, anti-fogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, and antiviral agents. For details of these components, please refer to paragraphs

[0107] to

[0115] of JP 2014-136710 A, paragraphs

[0106] to

[0128] of JP 2015-117298 A, and paragraphs

[0055] to

[0061] of JP 2018-095706 A, the contents of which are incorporated herein by reference. When contained, the content of the other components is, for example, 0.001 mass% or more and, for example, 5 mass% or less, preferably 3 mass% or less, and more preferably 1 mass% or less, based on the mass of the composition or molded body.

[0024] In addition, in the composition or molded article of the present embodiment, the total amount of the resin and the PBO fiber (X) usually accounts for 95% by mass or more, preferably 97% by mass or more, more preferably 99% by mass or more, and may also be 100% by mass.

[0025] Next, a method for separating PBO fibers (X), producing a composite material of this embodiment, and using the composite material to produce a molded article of this embodiment will be described. In this embodiment, the composite material is preferably obtained by a method including the steps of: ultrasonically treating poly(p-phenylene benzobisoxazole) aggregates in a solvent; separating poly(p-phenylene benzobisoxazole) fibers (X) from the ultrasonically treated solution to obtain a dispersion of poly(p-phenylene benzobisoxazole) fibers (X); mixing the dispersion with a resin to obtain a mixture containing poly(p-phenylene benzobisoxazole) fibers (X), a resin, and a solvent; and removing the solvent from the mixture. By producing a molded article using the separated PBO fibers (X) and then blending them with a resin to form a masterbatch, a molded article with reduced thermal expansion can be obtained. The solvent used in the ultrasonic treatment is not particularly limited as long as it can effectively disperse the PBO fibers (X), and may be an organic solvent or an inorganic solvent, an example of which is water. The PBO aggregates can be produced by known methods, for example, by the method for producing poly(p-phenylene benzobisoxazole) crystals described in Patent Document 2 (WO 2016 / 178427).

[0026] In this embodiment, it is preferable to separate the PBO fibers (X) from the ultrasonically treated liquid to obtain a dispersion of the PBO fibers (X). The method for separating the PBO fibers (X) from the ultrasonically treated liquid is not particularly limited, and any method capable of separating the PBO fibers (X) from the PBO particulates may be used. Specifically, examples of methods for separating the PBO fibers (X) include filtration, sieving, air classification, and vibration classification, with filtration being preferred. The PBO fibers (X) obtained here are typically the same as the PBO fibers (X) contained in the above-mentioned composition.

[0027] In this embodiment, poly(p-phenylene benzobisoxazole) fibers (X) are separated from the ultrasonically treated liquid to obtain a dispersion of poly(p-phenylene benzobisoxazole) fibers (X). The dispersion typically contains PBO fibers (X) and a solvent, and it is preferred that 95% by mass or more (preferably 97% by mass or more, more preferably 99% by mass or more, and for example, 100% by mass or less) of the dispersion be PBO fibers (X). The solvent for the dispersion is not particularly limited as long as it is a solvent that can effectively disperse PBO fibers (X), and may be an organic solvent or an inorganic solvent. One example of the solvent is tetrahydrofuran.

[0028] In this embodiment, a step is performed in which the dispersion of PBO fiber (X) is mixed with a resin to obtain a mixture containing poly(p-phenylenebenzobisoxazole) fiber (X), resin, and a solvent. By producing such a mixture, the PBO fiber (X) can be partially or entirely coated with the resin. The type of resin added to the dispersion of PBO fiber (X) and the amount of resin added relative to the PBO fiber (X) are the same as those described above for the composite material. A first embodiment for obtaining a mixture is to add the resin directly to the dispersion of PBO fiber (X). In this embodiment, it is preferable to crush the resin into powder and add it, or to use a liquid resin during mixing. A second embodiment for obtaining a mixture is to mix the dispersion of PBO fiber (X) with a dispersion of resin. The resin dispersion in this embodiment can be determined depending on the type of resin and is preferably selected from the examples of solvents used in the ultrasonic treatment. The solvent used for the dispersion of the PBO fiber (X) and the solvent used for the dispersion of the resin may be the same or different. In particular, it is preferable that the resin is mixed with the dispersion in a state dissolved in a solvent. By adopting such a configuration, the surface of the PBO fiber (X) can be more easily coated with the resin. For the second embodiment, the description of WO 2016 / 178427 can be referred to.

[0029] In this embodiment, the content of the PBO fibers (X) in 100% by mass of the mixed solution is preferably 0.0001% by mass or more, more preferably 0.0005% by mass or more, even more preferably 0.001% by mass or more, even more preferably 0.003% by mass or more, even more preferably 0.005% by mass or more, and may be 0.01% by mass or more, 0.03% by mass or more, or 0.05% by mass or more. By setting the content at or above the lower limit, a composite material tends to be obtained efficiently. Furthermore, the upper limit of the content of the PBO fibers (X) in 100% by mass of the mixed solution is preferably 30% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, even more preferably 3% by mass or less, and even more preferably 1% by mass or less. By setting the content at or below the upper limit, a resin tends to be more effectively coated on the surface of the PBO fibers (X) while suppressing aggregation of the PBO fibers (X).

[0030] Furthermore, the resin content in 100% by mass of the mixed liquid is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 20% by mass or less, and even more preferably 10% by mass or less. By setting the content below the upper limit, the viscosity of the mixed liquid suitable for dispersing the PBO fiber (X) tends to be maintained, and the effect of efficiently coating the surface of the PBO fiber (X) with the resin tends to be further improved. The lower limit of the resin content in 100% by mass of the mixed liquid is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and even more preferably 5% by mass or more. Setting the content above the lower limit tends to be further improved, and the effect of efficiently obtaining a composite material tends to be further improved. The mixed liquid of this embodiment may contain only one type of resin, or may contain two or more types. When two or more types of resins are contained, the total amount preferably falls within the above range.

[0031] The mixed solution used in this embodiment preferably contains 98 to 100 mass % of the PBO fiber (X), solvent, and resin.

[0032] In this embodiment, a composite material is obtained through a step of removing the solvent from the mixed solution. By removing the solvent, a composite material is obtained in which the PBO fibers (X) are partially or entirely coated with a resin in the mixed solution. This composite material has the same meaning as the composite material described above. The step of removing the solvent from the mixed solution is not particularly limited, but preferably involves heating to volatilize the solvent, and more preferably thermal vacuum drying. The obtained composite material may also be washed with a solvent.

[0033] In this embodiment, as described above, it is preferable to produce a molded article using the composite material obtained above. More preferably, it is formed from a composition containing a resin and a composite material. The resin here is the above-mentioned post-added resin. In the above composition, the ratio of the post-added resin to the composite material is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, and preferably 200 parts by mass or less, more preferably 100 parts by mass or less, per 100 parts by mass of the post-added resin.

[0034] The molded article of this embodiment is preferably formed from a composition containing a resin and a composite material, and examples of the molding method include extrusion molding, cast molding, and injection molding. The shape of the molded article of this embodiment is not particularly specified, but a film is one example. Uses of the molded article can be found in paragraph 0044 of JP 2016-089169 A and paragraph 0028 of JP 2009-242810 A, the contents of which are incorporated herein by reference.

[0035] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.

[0036] Example 1 <Production of PBO Aggregates> PBO (synthesized by condensation polymerization of 4,6-diaminoresorcinol and terephthalic acid using polyphosphoric acid as a polymerization catalyst, weight average molecular weight 16,600) was dissolved in 94.5% by mass sulfuric acid at 120°C under a nitrogen atmosphere to a concentration of 0.1% by mass. The resulting solution was rapidly cooled in an ice bath at 0°C and then added dropwise to distilled water at 0°C for rapid crystallization to obtain PBO aggregates. The resulting PBO aggregates were washed to prepare an aqueous dispersion (0.003% by mass) of PBO aggregates.

[0037] <Production of PBO Fiber (X)> The aqueous dispersion of the PBO aggregates was subjected to a homogenizer treatment for 1 hour. The resulting aqueous dispersion was irradiated with ultrasound at a frequency of 42 kHz to separate the PBO into fibrous and particulate matter. The morphology of the PBO in the resulting aqueous dispersion was observed using a scanning electron microscope (SEM), confirming that the PBO fibers and PBO particulate matter had been separated. Furthermore, the aqueous dispersion after ultrasound irradiation was filtered using a membrane filter (1.0 μm diameter) to obtain PBO fiber (X). The particulate matter passed through the filter, while the fibrous matter was filtered onto the filter. Figure 3 shows a photograph of PBO fiber (X). Of the resulting PBO fibers (X), those that were not entangled with other fibers and provided clear SEM images were measured to determine the width, the difference between the maximum and minimum fiber widths (ΔW), and the fiber length. In the present invention, the width and fiber length of PBO fibers (X) are measured for at least 10 or more fibers. For example, measurements may be made for all PBO fibers (X) that are not entangled with other fibers when observed under an SEM and for which clear SEM images are obtained. That is, the width and length in this embodiment refer to the width and length of the fibers measured in the SEM image. The results are shown in Table 1 below and Figures 4 to 7. Figure 4 shows the distribution of fiber widths, with the horizontal axis representing the width (nm). "Up to 50" means that the width is 50 nm or less, and "up to 75" means that the width is greater than 50 nm and less than 75 nm. The same applies to the following widths. The vertical axis represents the number of fibers corresponding to each width. Figure 5 shows the distribution of the difference (ΔW) between the maximum and minimum widths of the fibers, with the horizontal axis representing the difference (ΔW) between the maximum and minimum widths (unit: nm). "Up to 10" means that ΔW is 10 nm or less, and "up to 20" means that ΔW is more than 10 nm and less than or equal to 20 nm. The same applies below. The vertical axis indicates the number of fibers corresponding to each ΔW. Figure 6 shows the distribution of fiber lengths, with the horizontal axis indicating length (unit: μm). "Up to 1" means that the length is 1 μm or less, and "up to 2" means that the length is more than 1 μm and less than or equal to 2 μm. The same applies below. The vertical axis indicates the number of fibers corresponding to each length.FIG. 7 shows the aspect ratios of the fibers, with the horizontal axis representing the aspect ratio. "Up to 10" means that the aspect ratio is 10 or less, and "up to 20" means that the aspect ratio is greater than 10 and less than 20. The same applies below. The vertical axis represents the number of fibers exhibiting each aspect ratio. The same is true for Comparative Example 1. In FIGS. 4 to 7, the black areas represent the distribution of Example 1, and the shaded areas represent Comparative Example 1.

[0038] <Production of Composite Material (Masterbatch)> The purified PBO fiber (X) was added to tetrahydrofuran (THF) so that the concentration of the PBO fiber (X) was 0.005% by mass, and the mixture was dispersed using ultrasonic irradiation (frequency 42 kHz). Powdered polycarbonate resin (Mitsubishi Engineering Plastics Corporation, product number: Iupilon E-2000) was added to the dispersion so that the mass ratio of the PBO fiber (X) to the polycarbonate resin was 100:1, and the mixture was dissolved at 60°C. The dispersion in which the polycarbonate resin was dissolved was allowed to stand until it reached room temperature, and then distilled water was added dropwise to precipitate the polycarbonate resin, thereby obtaining PBO fiber (X) at least partially coated with the polycarbonate resin. The obtained PBO fiber (X) at least partially coated with polycarbonate resin was washed with THF and distilled water, and then thermally dried under vacuum to produce a composite material (PBO fiber (X) at least partially coated with polycarbonate resin, masterbatch).

[0039] <Production of a Molded Product of Polycarbonate Resin / PBO Fiber (X)> Using a micro-type high-shear molding machine (IMC-11FD, manufactured by Imoto Machinery Works, Ltd.), powdered polycarbonate resin (Mitsubishi Engineering Plastics Corporation, product number: Iupilon E-2000) was added to the composite material (masterbatch) obtained above so that the concentration was 0.1% by mass. Using a vacuum heating press (IMC-11FD, manufactured by Imoto Machinery Works, Ltd.), the material obtained above was vacuum-pressed at 250°C and a press thickness of 4 MPa, followed by rapid cooling in an ice bath to produce a molded product (film). During this process, the highly viscous fluid (polycarbonate resin) flowed from the inside to the outside, and the PBO fiber (X) was oriented in the direction of the fluid flow, i.e., the in-plane direction. The resulting molded product was measured for fracture elongation, fracture energy, and linear thermal expansion coefficient. The results are shown in Table 2. The obtained molded body was observed by scanning probe microscopy (SPM). The results are shown in Figure 8. From the left, Figure 8 shows a height image, a microdispersion image of height change, and a hardness image. It was found that in the molded body, the PBO fibers (X) maintained their fibrous form while being dispersed, forming a state in which paths were connected (percolation). Since the PBO fibers (X) have a higher thermal conductivity than polycarbonate resin, it is presumed that the formation of percolation facilitates thermal diffusion.

[0040] <<Method for measuring breaking elongation (%)>> A test piece (dumbbell-shaped (effective length 10 mm × 2 mm)) was prepared from the obtained molded body (film), and the breaking elongation (%) was measured at a tension rate of 4 mm / min using a tension and compression testing machine (SV-201NA model, manufactured by Imada Seisakusho).

[0041] << Breaking energy (MJ / m 3 ) measurement method >> The breaking energy (MJ / m 3 ) was measured.

[0042] << Linear thermal expansion coefficient (×10 -5Measurement method for the coefficient of linear thermal expansion (×10 -5 - Measurement conditions - Load (N): 0.1 Temperature rise rate (°C / min): 3 Temperature range (°C): 30 to 120

[0043] Example 2 The same procedure as in Example 1 was performed except that the concentration of PBO fiber (X) was changed from 0.1% by mass to 0.3% by mass. The resulting molded body was measured for breaking elongation, breaking energy, and linear thermal expansion coefficient. The results are shown in Table 2.

[0044] Comparative Example 1 The same procedures as in Example 1 were carried out except that in the above-mentioned <Production of PBO Fiber (X)>, the step of filtering the aqueous dispersion after ultrasonic irradiation using a membrane filter (1.0 μm diameter) was omitted. An example of the obtained fiber is shown in the photograph in Figure 1. The analysis results of the obtained fiber are also shown in Table 1 and Figures 4 to 7. The fracture elongation, fracture energy, and linear thermal expansion coefficient of the obtained molded body were measured. The results are shown in Table 2.

[0045] Comparative Example 2: The same procedure as in Example 2 was repeated except that the step of filtering the aqueous dispersion after ultrasonic irradiation using a membrane filter (1.0 μm diameter) was omitted. The resulting molded body was measured for breaking elongation, breaking energy, and linear thermal expansion coefficient. The results are shown in Table 2.

[0046] Comparative Example 3: The same procedure as in Example 1 was repeated except that the composite material was not produced, and an aqueous dispersion of PBO fiber (X) was mixed with a polycarbonate resin. The resulting molded article was measured for breaking elongation, breaking energy, and linear thermal expansion coefficient. The results are shown in Table 2.

[0047]

[0048]

[0049] The molded article of the present invention had a small thermal expansion coefficient, a high breaking elongation, and a high breaking energy.

[0050] Example 3 <Production of Epoxy Resin / PBO Fiber (X) Molded Article> The PBO fiber (X) obtained in the above <Production of PBO Fiber (X)> was added to ethyl methyl ketone (MEK) so that the concentration of PBO fiber (X) was 0.2% by mass, and the mixture was dispersed by ultrasonic irradiation (frequency 28 kHz). The mass of PBO fiber (X) per part by mass of liquid epoxy resin (Mitsubishi Chemical Corporation, product number: JER828) was adjusted to the ratio shown in Table 3, and the mixture was irradiated with ultrasonic irradiation (frequency 28 kHz) and further stirred to perform dispersion and degassing treatment. 2-Ethyl-4-methylimidazole was added to the epoxy resin-dissolved dispersion so that the mass was 5% by mass relative to the epoxy resin, and the mixture was irradiated with ultrasonic irradiation (frequency 28 kHz), stirred, and degassed for 1.5 minutes at 2200 rpm using an Awatori Mixer. The degassed dispersion was concentrated by distilling off MEK at 50°C under a nitrogen flow. The dispersion was then degassed for 1.5 minutes at 2200 rpm using a THINNER MIXER and allowed to stand for 12 hours. The concentrated dispersion was then dried by holding it at 80°C for 1 hour without applying pressure using a vacuum heating press (IMC-11FD, manufactured by Imoto Machinery Co., Ltd.). A molded product (film) was then produced by vacuum pressing at 120°C for 2 hours at a press thickness of 4 MPa. During this process, the highly viscous fluid (epoxy resin) flowed from the inside to the outside, and the PBO fibers (X) were oriented in the direction of the fluid flow, i.e., the in-plane direction. The resulting molded product was observed using scanning probe microscopy (SPM). The results are shown in Figure 9. FIG. 9 shows, from the left, a height image and a hardness image, and it was found that in the molded product, the PBO fibers (X) were dispersed while maintaining their fibrous form, forming a state in which paths were connected (percolation). Since the PBO fibers (X) have a higher thermal conductivity than the epoxy resin, it is presumed that the formation of percolation facilitates thermal diffusion. The fracture elongation, fracture energy, and linear thermal expansion coefficient of the obtained molded product (film) were measured in the same manner as in Example 1. The results are shown in Table 3.

[0051] The breaking strength and thermal diffusivity were evaluated as follows, and the results are shown in Table 3.

[0052] <Breaking Strength> A test piece (dumbbell-shaped (effective length 10 mm × 2 mm)) was prepared from the obtained molded body (film), and the breaking strength (MPa) was measured at a tension rate of 4 mm / min using a tension and compression testing machine (SV-201NA model, manufactured by Imada Seisakusho).

[0053] <Thermal diffusivity (in-plane direction)> A strip-shaped test piece measuring 5 mm × 20 mm (test area 5 mm × 10 mm) was cut out from the obtained molded body (film), and then blackened using a carbon spray. The thermal diffusivity was measured using a thermal property measuring device (Thermowave Analyzer TA-LT manufactured by BETHEL).

[0054] Example 4 The same procedure was carried out as in Example 3, except that the amount of PBO fiber (X) obtained in the above <Production of PBO fiber (X)> was changed to the amount shown in Table 3 per part by mass of epoxy resin. The resulting molded article was measured for breaking strength, breaking elongation, breaking energy, thermal diffusivity, and linear thermal expansion coefficient. The results are shown in Table 3.

[0055] Comparative Example 4 The same procedure as in Example 3 was carried out, except that the PBO fiber (X) was not blended. The resulting molded article was measured for breaking strength, breaking elongation, breaking energy, thermal diffusivity, and linear thermal expansion coefficient. The results are shown in Table 3.

[0056] Comparative Example 5 The same procedure was carried out as in Example 3, except that the PBO fiber (X) obtained in the above <Production of PBO fiber (X)> was replaced with the PBO fiber obtained in Comparative Example 1. The resulting molded article was measured for breaking strength, breaking elongation, breaking energy, thermal diffusivity, and linear thermal expansion coefficient. The results are shown in Table 3.

[0057] Comparative Example 6 The same procedure was carried out as in Example 4, except that the PBO fiber (X) obtained in the above <Production of PBO fiber (X)> was replaced with the PBO fiber obtained in Comparative Example 1. The resulting molded article was measured for breaking strength, breaking elongation, breaking energy, thermal diffusivity, and linear thermal expansion coefficient. The results are shown in Table 3.

[0058]

[0059] As is clear from the above results, the molded article of the present invention exhibited improvements in breaking strength, breaking elongation, breaking energy, thermal diffusivity, and coefficient of linear thermal expansion.

[0060] Example 5: A mat was formed using PBO fiber (X). Specifically, the PBO fiber (X) obtained in Example 1 was added to distilled water to prepare a suspension of PBO fiber (X) (PBO fiber (X) concentration: 0.1% by mass). The resulting suspension was subjected to homogenizer treatment and ultrasonic (frequency: 28 kHz) treatment, and then the suspension of PBO fiber (X) was filtered under reduced pressure using a membrane filter (pore size: 0.4 μm). A mat of PBO fiber (X) was produced by pressing the filtered PBO fiber (X) laminate using a vacuum heating press (IMC-11FD, manufactured by Imoto Machinery Co., Ltd.) under conditions of 60°C, a pressing pressure of 10 MPa, and a pressing time of 1 hour. X-ray diffraction measurement and thermal diffusivity measurement were performed using the prepared PBO fiber (X) mat to evaluate the physical properties of the PBO fiber (X) mat. Figure 10 shows the results of X-ray diffraction measurement when X-rays were incident from the in-plane direction of the mat of PBO fiber (X). In Figure 10, (a) shows the peak in the in-plane direction, and (b) shows the peak in the thickness direction. Since peaks of the PBO (001) and (005) planes were observed only in the reflection in the in-plane direction of the mat, it was found that the PBO fiber (X) was oriented in the in-plane direction in the mat of PBO fiber (X). The thermal diffusivity (in-plane direction and thickness direction) of the obtained mat was measured using the same method as in Example 3. The thermal conductivity was calculated using the specific heat determined by differential scanning calorimetry (Rigaku Thermo Plus EV2 DSC Vesta). The results are shown in Table 4.

[0061] Comparative Example 7: A fiber mat was produced in the same manner as in Example 5, except that the PBO fiber (X) obtained in the above <Production of PBO fiber (X)> was replaced with the PBO fiber obtained in Comparative Example 1. The results of measuring the thermal diffusivity and thermal conductivity of the obtained fiber mat are shown in Table 4.

[0062]

[0063] As is clear from the results in Table 4 above, the mat of PBO fiber (X) obtained in Example 5 had improved density and thermal diffusivity in the in-plane direction of the mat, compared to the mat of fiber obtained in Comparative Example 7. Therefore, the thermal conductivity in the in-plane direction of the mat of PBO fiber (X) obtained in Example 5 was improved by about 1.5 times compared to the mat of fiber obtained in Comparative Example 7. The mat of fiber obtained in Comparative Example 7 contained a mixture of PBO fibers and attachments, while the mat of PBO fiber (X) obtained in Example 5 contained only linear PBO fibers (X) densely oriented in-plane, which is thought to have resulted in the improved thermal conductivity of the mat of PBO fiber (X) in the in-plane direction.

[0064] 1 PBO aggregate 2 Granules 3 PBO fiber (X)

Claims

1. A molded article formed from a composition containing a resin and a fiber (X) of poly(p-phenylene benzobisoxazole), wherein the proportion of the fiber (X) relative to 100% by mass of the poly(p-phenylene benzobisoxazole) contained in the composition is 50% by mass or more.

2. The molded body according to claim 1, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 35 nm or less.

3. The molded body according to claim 1, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 30 nm or less.

4. The molded article according to any one of claims 1 to 3, wherein the proportion of the fibers (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composition is 80 mass% or more.

5. The molded article according to any one of claims 1 to 3, wherein the composition contains 0.01 to 30 parts by mass of the fiber (X) per 100 parts by mass of the resin.

6. The molded article according to any one of claims 1 to 3, which is a film.

7. The molded article according to claim 6, wherein the fibers (X) are oriented in the in-plane direction of the film.

8. The molded body according to claim 1, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 30 nm or less, the ratio of the fiber (X) to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the molded body is 80 mass% or more, the composition contains 0.01 to 30 mass parts of the fiber (X) to 100 mass parts of the resin, the molded body is a film, and the fiber (X) is oriented in the in-plane direction of the film.

9. A composite material comprising a fiber (X) of poly(p-phenylene benzobisoxazole) and a resin that covers all or part of the fiber (X), wherein the proportion of the fiber (X) relative to 100% by mass of the poly(p-phenylene benzobisoxazole) contained in the composite material is 50% by mass or more.

10. The composite material according to claim 9, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 35 nm or less.

11. The composite material according to claim 9, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 30 nm or less.

12. The composite material according to any one of claims 9 to 11, wherein the proportion of the fibers (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composite material is 80 mass% or more.

13. The composite material according to any one of claims 9 to 11, wherein the composite material contains 100 to 9,900 parts by mass of the resin per 100 parts by mass of the fibers (X).

14. The composite material according to claim 9, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 30 nm or less, the proportion of the fiber (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the composite material is 80 mass% or more, and the composite material contains 100 to 9,900 mass parts of the resin relative to 100 mass parts of the fiber (X).

15. A method for producing a composite material according to any one of claims 9 to 11 and 14, comprising the steps of: ultrasonically treating poly(p-phenylene benzobisoxazole) aggregates in a solvent; separating poly(p-phenylene benzobisoxazole) fibers (X) from the ultrasonically treated liquid to obtain a dispersion of poly(p-phenylene benzobisoxazole) fibers (X); mixing the dispersion with a resin to obtain a mixture containing poly(p-phenylene benzobisoxazole) fibers (X), a resin, and a solvent; and removing the solvent from the mixture.

16. The method for producing a composite material according to claim 15, wherein the content of the resin in 100% by mass of the mixed liquid is 0.05 to 50% by mass.

17. A method for producing a molded body, comprising: ultrasonically treating poly(p-phenylene benzobisoxazole) aggregates in a solvent; separating poly(p-phenylene benzobisoxazole) fibers (X) from the ultrasonically treated liquid to obtain a dispersion of poly(p-phenylene benzobisoxazole) fibers (X); mixing the dispersion with a thermosetting resin to obtain a mixture containing poly(p-phenylene benzobisoxazole) fibers (X), a thermosetting resin, and a solvent; removing the solvent from the mixture; and curing the thermosetting resin.

18. The method for producing a molded product according to claim 17, wherein the thermosetting resin is soluble in the solvent contained in the dispersion at 23°C.

19. A mat formed using poly(p-phenylene benzobisoxazole) containing fiber (X) of poly(p-phenylene benzobisoxazole), wherein the proportion of fiber (X) relative to 100 mass% of poly(p-phenylene benzobisoxazole) contained in the mat is 50 mass% or more.

20. The mat according to claim 19, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 35 nm or less.

21. The mat according to claim 19, wherein the difference (ΔW) between the maximum width and the minimum width of the fiber (X) is 30 nm or less.

22. The mat according to any one of claims 19 to 21, wherein the proportion of the fibers (X) relative to 100 mass% of the poly(p-phenylene benzobisoxazole) contained in the mat is 80 mass% or more.

Citation Information

Patent Citations

  • Fiber-reinforced composite material and manufacturing method therefor

    JP2009242810A

  • Aromatic polycarbonate resin composition and molded product thereof

    JP2014136710A

  • Polycarbonate resin composition

    JP2015117298A

  • Polyamide resin composition and molded article

    JP2018095706A

  • Method for manufacturing metal foil clad laminated sheet, resin composition, resin composite sheet, method for manufacturing printed wiring board, and method for manufacturing semiconductor device