Zirconia sintered body

The zirconia sintered body with a balanced crystal grain size distribution and Y2O3 content achieves both high transparency and fracture toughness, addressing the trade-off issues in existing technologies and enabling efficient production by pressureless sintering.

WO2024225323A1PCT designated stage expired Publication Date: 2024-10-31NAKASHIMA SANGYO CO LTD

Patent Information

Application Number
PCT/JP2024/016093
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

There is a trade-off between achieving high transparency and mechanical properties such as strength and fracture toughness in zirconia sintered bodies, making it difficult to improve both simultaneously, especially when using the pressureless sintering method, which results in inferior mechanical properties compared to the HIP method.

Method used

A zirconia sintered body with a composition of 2.5 to 6 mol% Y2O3, having a relative density of 99% or more, and a specific crystal grain size distribution where the area ratio of zirconia crystal particles in certain size ranges is carefully balanced to achieve both high transparency and fracture toughness, while being easily producible by pressureless sintering.

Benefits of technology

The solution enables the attainment of high levels of transparency and fracture toughness in zirconia sintered bodies, overcoming the limitations of traditional methods by optimizing the crystal structure and processing conditions, specifically through the use of a unique particle size distribution and concentration gradient in the sintered body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016093_31102024_PF_FP_ABST
    Figure JP2024016093_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a zirconia sintered body with which both transparency and fracture toughness value can be achieved at high levels and which can be easily manufactured even by pressureless sintering. The Y2O3 content in the entire composition of the sintered body is 2.5-6 mol%, the remainder comprising ZrO2 and unavoidable impurities. The zirconia crystal grains have an area-average grain size of 0.4-0.9 μm. The area ratio of a first region ranging in grain size from 0.1 μm to less than 0.5 μm is 5-80%, the area ratio of a second region ranging in grain size from 0.8 μm to less than 2 μm is 5-80%, and the area ratio of a third region ranging in grain diameter from 0.5 μm to less than 0.8 μm is 10% to less than 55%. The zirconia crystal grains forming the second region have an average Y2O3 concentration of 3.5-7.0 mol%, and the zirconia crystal grains forming the first region have an average Y2O3 concentration C1 of 1.7-5 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

Zirconia sintered body

[0001] The present invention relates to a zirconia sintered body, and more particularly to a zirconia sintered body that has a good fracture toughness value and is also excellent in visible light transmittance.

[0002] As shown in Fig. 9 of Non-Patent Document 1 (referred to herein as Fig. 15), pure ZrO 2 (Zirconium oxide) is converted from CaF 2 There are polymorphs of the cubic phase (C phase), tetragonal phase (T phase) and monoclinic phase (M phase). 2 O 3 When 2 to 5 mol% of stabilizers such as yttrium oxide (yttrium oxide) or calcium oxide (CaO) are added, partially stabilized zirconia (PSZ) containing a metastable T phase at room temperature is formed, and when 8 mol% or more is added, a C phase, i.e., fully stabilized zirconia (FSZ), is formed. It has been revealed that the excellent mechanical properties of PSZ are due to the martensitic transformation from the high-temperature T phase to the low-temperature M phase. When a crack propagates within a PSZ sintered body, the resulting stress causes a transformation from the T phase to the M phase, and at that time, the volume expands by about 4%. This expansion applies compressive stress to the tip of the crack, suppressing the propagation of the crack (hereinafter, the toughening of zirconia sintered bodies by this mechanism will be referred to as "transformation toughening"). In particular, Y 2 O 3 PSZ, which uses as a stabilizer, is chemically stable and has high strength and toughness, and is therefore widely used as a material for engines, cutting tools, dies, sealing materials, mechanical structural materials such as bearings, and biomaterials such as dental bone materials.

[0003] Incidentally, industrial products using zirconia sintered bodies made of PSZ (hereinafter simply referred to as "zirconia sintered bodies" in this specification) may require a certain level of transparency in order to improve their appearance and aesthetics. Examples of such industrial products include dental materials and decorative items such as accessories. For example, in the case of dental materials, if the transparency of the zirconia sintered body used is too low, the difference in appearance from actual teeth will be significant, impairing aesthetics and making it unsuitable.

[0004] The zirconia sintered body disclosed in Patent Document 1 contains 5 mol% Y, which further stabilizes the C phase. 2 O 3 The publication discloses a sintered body manufactured using a HIP process with minimal residual bubbles. The total light transmittance measured at a sample thickness of 1 mm is high, ranging from 41 to 46%. While the sample thickness used for measuring total light transmittance varies between 0.5 mm and 1.0 mm depending on the literature, Figure 3 in Non-Patent Document 2 discloses the total light transmittance values ​​for various zirconia sintered body products when the sample thickness is varied from 0.5 to 1.5 mm. By referring to this, the total light transmittance value for a 1.0 mm thick sample can be estimated by multiplying the total light transmittance value for a 1.0 mm thick sample by a coefficient of 1.21. The total light transmittance value disclosed in Patent Document 2 is considered to be as high as 49.6 to 55.7% for a 0.5 mm thick sample. Meanwhile, the bending strength of the sintered body is approximately 800 to 1100 MPa, and the fracture toughness value is 3.5 to 4.0 MPa m 0.5 It is also disclosed that the average crystal grain size of the sintered body measured by the line intercept method is about 0.49 to 0.95 μm. The raw material powder used has an average grain size of 0.028 to 0.030 μm and a specific surface area of ​​15 to 16 m. 2 / g and fine particles are used.

[0005] Patent Document 2 describes a method for producing a 1.6 to 2 mol% Y alloy. 2 O 3The sintered body is manufactured by HIP method using zirconia of the composition. Because a composition with a higher T phase content, which is a factor in increasing transformation toughness, is used, the bending strength of the sintered body is 1470 MPa to 2140 MPa, and the fracture toughness is 6.0 to 10.3 MPa m 0.5 It has high strength and toughness. However, the total light transmittance measured with a sample thickness of 1 mm was 27-34% (the converted value for a sample thickness of 0.5 mm is estimated to be 32.7-41.2%), which is lower than those of Patent Documents 1-3. The average crystal grain size of the sintered body measured by the planimetric method was 0.28-0.55 μm. The raw material powder used had a bimodal distribution with peaks at 0.14 μm and 0.34-0.35 μm, a median diameter of 0.15-0.18 μm, and a specific surface area of ​​15.1-17.9 m. 2 / g (specific surface area value is 10.3 m 2 / g and 11.6m 2 For the powders of Synthesis Examples 3 and 6 with a sintered body having a total light transmittance of 1 / g, the total light transmittance of the sintered body was not evaluated.

[0006] Patent Document 3 describes a compound containing mainly 3 mol% Y. 2 O 3 The publication discloses a sintered body manufactured by pressureless sintering of zirconia of the same composition. The total light transmittance measured at a sample thickness of 1 mm is high at 34-40% (estimated to be 41.2-48.4% converted to a sample thickness of 0.5 mm), and the bending strength of the sintered body is 980-1280 MPa. The average crystal grain size of the sintered body measured by the planimetric method is 0.30-0.34 μm. The raw material powder used has an average grain size of 0.4-0.7 μm and a specific surface area of ​​11-15 m. 2 The raw material powder used had an average particle size of 0.4 to 0.7 μm and a specific surface area of ​​11 to 15 m 2 / g.

[0007] Patent Document 4 describes a compound containing mainly 4 mol% Y. 2 O 3 The sintered body of zirconia of the composition is manufactured by the atmospheric sintering method. The bending strength of the sintered body is 1016 to 1220 MPa. 2 O 3The content is increased to the same extent as that of Patent Document 3, which has a lower content. In addition, the fracture toughness value is 4.0 to 4.5 MPa m 0.5 Although the optical transmittance measured with a sample thickness of 0.5 mm was relatively good at about 100%, the total optical transmittance measured with a sample thickness of 0.5 mm was about 28 to 30%. Although the specific surface area of ​​the powder used is not disclosed, the description in 0043 states that the particle size distribution of the zirconia crystal particles in the raw material powder has at least two peaks, with the first peak preferably existing between 0.05 μm and 0.11 μm (small particle size powder) and the second peak preferably existing between 0.1 μm and 0.7 μm (large particle size powder). Specifically, a mixture of equal amounts of a small particle size powder with a peak of 0.08 μm and a large particle size powder with a peak of 0.4 μm is used. This raw material is considered to be similar in concept to the raw material powder with a bimodal distribution disclosed in Patent Document 2.

[0008] Furthermore, Patent Document 4 analyzes the crystal grain size distribution using SEM images of sintered bodies, and discloses that, in the circular equivalent particle size distribution of each crystal grain observed in the image, the cross-sectional area ratio of zirconia particles in the class of less than 0.4 μm is preferably 4% to 35%, the cross-sectional area ratio of zirconia particles in the class of 0.4 μm to less than 0.76 μm is preferably 24% to 57%, and the cross-sectional area ratio of zirconia particles in the class of 0.76 μm or more is preferably 16% to 62%. Although the average crystal grain size is not disclosed, it is estimated from the area ratio of each class of crystal grain that this value is in the range of 0.06 μm to 0.085 μm. Table 1 summarizes the disclosures of the above patent documents.

[0009]

[0010] JP 2008-222450 A JP 2022-008052 A JP 2010-150063 A JP 2018-165243 A

[0011] "Phase diagram and structure of Y2O3-added partially stabilized ZrO2" (Journal of the Japan Institute of Metals, Vol. 50, No. 12 (1986) pp. 1101-1108); "Evaluation of physical properties of ultra-transparent zirconia" (Proceedings of the 33rd Annual Meeting of the Japanese Academy of Dentistry, P-34 (2017)); "Evaluation of fracture toughness of zirconia (Y-TZP) by SEVNB and IF methods" (Ann Jpn Prosthodont Soc 5: P165-173, 2013); "Fracture toughness testing method for ceramics by indentation (IF) method" (Synthesiology Vol. 13 No. 1 (2021) P29-44); "Sintering mechanism of yttria-stabilized zirconia: Effect of grain boundary segregation of yttrium ions (III)" (TOSOH Research & Technology Review Vol. 55 (2011) pp. 7-18) "Spinodal Decomposition of Ceramics" (Iron and Steel, 73rd Year (1987) No. 11, pp. 1453-1460)

[0012] In order to improve the mechanical properties of the zirconia sintered body, Y 2 O 3 It is believed that it is effective to reduce the content of Y to increase the proportion of the T phase, which contributes to transformation toughening, and to refine the crystal grain size of the sintered body. On the other hand, to improve transparency, it is necessary to increase the proportion of crystal grains grown to a level larger than the wavelength of visible light and reduce the proportion of fine crystal grains, which cause light scattering. 2 O 3 It is believed that increasing the content of C is effective in further stabilizing the C phase and suppressing the formation of fine crystal domains of the T phase or M phase within grown crystal grains.

[0013] However, as is clear from a comparison of the disclosures of Patent Documents 1 to 3 (see Table 1), in zirconia sintered bodies, there is often a trade-off between transparency and mechanical properties such as strength and fracture toughness, making it difficult to simultaneously improve both. Meanwhile, paragraph 0071 of Patent Document 4 states that "a balance in grain size distribution or area balance is believed to contribute to improving bending strength, fracture toughness, and phase transition suppression," but the disclosed property values ​​suggest that transparency and mechanical properties (particularly fracture toughness) are not consistently achieved at a high level. For example, as shown in Figure 30, the total light transmittance value of Patent Document 4 tends to increase with increasing area fraction of crystal grains 0.76 μm or larger, but the rate of increase in light transmittance relative to this area fraction is not very high. Furthermore, as shown in Figure 31, there is almost no correlation between fracture toughness and the area fraction of crystal grains less than 0.4 μm, suggesting that reducing the size of crystal grains does not necessarily contribute to improving fracture toughness.

[0014] Furthermore, since the HIP method requires large-scale equipment, it would be desirable to adopt the simple atmospheric sintering method in the case of dental materials, etc. However, as is clear from the disclosures of Patent Documents 3 and 4, there is a problem in that the mechanical properties of zirconia sintered bodies obtained by atmospheric sintering are significantly inferior to those of zirconia sintered bodies obtained by HIP. Therefore, there is a particular demand for zirconia sintered bodies that combine high levels of mechanical properties and translucency and that can be realized by atmospheric sintering.

[0015] Although bending strength and fracture toughness are the same mechanical properties, as mentioned in 0010 of Patent Document 4, there is a trade-off between them, making it difficult to increase both. For example, a two-dimensional plot of the bending strength and fracture toughness values ​​disclosed in Patent Documents 1, 2, and 3 is shown in Figure 32, which makes it difficult to say that a clear correlation exists between these two properties. The data points enclosed by dashed lines in the figure are values ​​for the sintered bodies of Patent Documents 1 and 2 manufactured using the HIP method, and it appears that there is indeed a negative correlation between bending strength and fracture toughness for these bodies. However, the remaining data points for the sintered bodies manufactured using the atmospheric sintering method are significantly different from the data points for the sintered bodies manufactured using the HIP method, indicating that a clear correlation between bending strength and fracture toughness cannot be understood.

[0016] According to Non-Patent Document 4, fracture of brittle materials occurs when stress concentrates, causing cracks to form, which then grow rapidly and lead to fracture. This rapid crack growth is called unstable fracture, while stable fracture occurs when fracture is achieved by controlling crack propagation in response to slowly applied stress, as in bending strength tests. As mentioned above, when a crack propagates within a zirconia sintered body, the stress concentrated at the crack tip causes the T phase around the tip to transform into martensitic M phase. The volume expansion caused by this transformation results in compressive stress, which prevents crack propagation. Unstable fracture occurs when a crack propagates despite this compressive stress, and fracture toughness refers to the critical stress intensity factor at which unstable fracture begins. On the other hand, if the sintered body transitions to unstable fracture, crack propagation cannot be controlled, leading to fracture. Therefore, it is believed that most phase transformations during bending strength tests occur during stable fracture.

[0017] As described above, the manner in which phase transformation contributes to test values ​​is fundamentally different between fracture toughness tests and bending strength tests. It should be noted that, for example, in cases where the results of fracture toughness tests are not disclosed, as in Patent Document 3, it is fundamentally impossible to estimate the fracture toughness value from the disclosed value of the bending strength test.

[0018] The object of the present invention is to provide a stabilizer 2 O 3 The present invention provides a zirconia sintered body that can achieve high levels of both transparency and fracture toughness by improving the crystal structure while taking into consideration the distribution of components, and that can be easily produced by atmospheric sintering.

[0019] In order to solve the above problems, the zirconia sintered body of the present invention contains Y in the total composition of the sintered body. 2 O 3 The content of is 2.5 mol % or more and 6 mol % or less, and the balance is ZrO 2 and unavoidable impurities and has a relative density of 99% or more, wherein, in an electron microscope image of the sintered body structure, the area-average particle size of the zirconia crystal particles is 0.4 μm or more and 0.9 μm or less, the area ratios of zirconia crystal particles having a particle size of less than 0.1 μm and zirconia crystal particles having a particle size of more than 2 μm are both less than 1%, the area ratio of a first region consisting of zirconia crystal particles having a particle size of 0.1 μm or more and less than 0.5 μm is 5% or more and 80% or less, the area ratio of a second region consisting of zirconia crystal particles having a particle size of 0.8 μm or more and less than 2 μm is 5% or more and 80% or less, the area ratio of a third region consisting of zirconia crystal particles having a particle size of 0.5 μm or more and less than 0.8 μm is 10% or more and less than 55%, and the average Y of the zirconia crystal particles constituting the second region is 2 O 3 The concentration is 3.5 mol % or more and 7.0 mol % or less, and the average Y of the zirconia crystal grains constituting the first region is 2 O 3 The concentration C1 is 1.7 mol% or more and 5 mol% or less, and 2 O 3 The difference in concentration is ΔC≡C2-C1, the value of ΔC / C2 is 0.2 or more and 0.5 or less, and the fracture toughness value measured by the IF method is 4.5 MPa m 0.5 12MPa・m or more 0.5 The present invention is characterized by the following:

[0020] According to the above-described configuration of the zirconia sintered body of the present invention, both high levels of transparency and fracture toughness can be achieved, and the body can be easily produced by atmospheric sintering.

[0021] Y for producing zirconia sintered body test pieces of the examples2 O 3 1 is a histogram showing the powder particle size distribution (volume basis) of a sintering raw material powder having a concentration of 4.5 mol % measured by a laser scattering particle size analyzer, together with its statistical characteristic values. 2 O 3 1 is a histogram showing the powder particle size distribution (volume basis) of a sintering raw material powder with a concentration of 4.5 mol% measured by a laser scattering particle size analyzer, together with its statistical characteristic values. FIG. 1 is a scanning electron microscope image (magnification 10,000 times) of a zirconia sintered body (example product) No. 10 in Table 1, which was produced by atmospheric sintering at 1500°C for 2 hours in air using the sintering raw material powder of FIG. 1. FIG. 2 is a scanning electron microscope image (magnification 10,000 times) of a zirconia sintered body (comparison product) No. 22 in Table 1, which was produced by atmospheric sintering at 1500°C for 2 hours in air using the sintering raw material powder of FIG. 2. FIG. 3 is a diagram showing an example of setting crystal grain sampling lines on the observation image of FIG. 3, together with the concept of measuring crystal grain dimensions. The representative crystal grains of the first region and the second region observed in the observation image of FIG. 3 are shown as Y. 2 O 3 1 is a diagram showing an example of the concentration analysis circle, with markings. It is a histogram showing the texture crystal grain size distribution (area basis) of the zirconia sintered body (example product) of No. 10 in Table 1, analyzed using the observation image of FIG. 3. It is a histogram showing the texture crystal grain size distribution (area basis) of the zirconia sintered body (example product) of No. 22 in Table 1, analyzed using the observation image of FIG. 4. It is a diagram showing an observation image (10,000 times magnification) of the zirconia sintered body (example product) of No. 10 in Table 1 in a different field of view by a scanning electron microscope, with a Y-axis along an analysis line that crosses the background region and a plurality of coarse dispersed particles in the field of view. 2 O 3FIG. 1 is a diagram showing the correlation between the results of EPMA line analysis in which the concentration was measured and the results of Zr and Y linear analysis in which the concentration was measured. FIG. 2 is an explanatory diagram showing a schematic diagram of the process of forming a crystalline structure of a zirconia sintered body of an example. FIG. 3 is an explanatory diagram showing a schematic diagram of the process of forming a crystalline structure of a zirconia sintered body of a conventional example. FIG. 4 is a diagram showing a schematic diagram of the estimated diffusion form of Zr and Y when small crystal particles having similar particle sizes coalesce and grow during the sintering process of a zirconia sintered body. FIG. 5 is a diagram showing a schematic diagram of the estimated diffusion form from small crystal particles of various sizes toward large crystal particles in contact with them during the sintering process of a zirconia sintered body of an embodiment performed using a raw material powder with a narrow particle size distribution width. FIG. 6 is a diagram showing a schematic diagram of the estimated diffusion form when most of the small crystal particles with a larger particle size difference than the large crystal particles are absorbed during the sintering process of a zirconia sintered body of a conventional example performed using a raw material powder with a wide particle size distribution width. 2 -Y 2 O 3 This is a binary phase diagram. 2 O 3 -0 mol% La 2 O 3 3 is an image (magnification 10,000 times) of the zirconia sintered body No. 3 in Table 2 (Example product: 3 mol % Y 2 O 3 -0.4mol%La 2 O 3 14 ) observed by a scanning electron microscope (magnification 10,000 times). 15 ) for the zirconia sintered body of No. 1 in Table 2 (Example product) is a histogram showing the texture and crystal grain size distribution (area basis) analyzed using the observation image of FIG. 14 . 16 ) for the zirconia sintered body of No. 3 in Table 2 (Example product) is a histogram showing the texture and crystal grain size distribution (area basis) analyzed using the observation image of FIG. 15 . 17 ) for the zirconia sintered body of No. 5 in Table 2 (Example product: 4 mol % Y 2 O 3 -0 mol% La 2 O 3 1 is an image (magnification 10,000 times) of the zirconia sintered body No. 7 in Table 2 (Example product: 4 mol % Y 2 O 3 -0.4mol%La2 O 3 19 is a scanning electron microscope image (magnification 10,000 times) of the zirconia sintered body No. 5 in Table 2 (Example product). It is a histogram showing the texture and crystal grain size distribution (area basis) analyzed using the observation image of FIG. 18 for the zirconia sintered body No. 5 in Table 2 (Example product). It is a histogram showing the texture and crystal grain size distribution (area basis) analyzed using the observation image of FIG. 19 for the zirconia sintered body No. 7 in Table 2 (Example product). It is a histogram showing the texture and crystal grain size distribution (area basis) analyzed using the observation image of FIG. 2 O 3 -0 mol% La 2 O 3 1 is an image (magnification 10,000 times) of the zirconia sintered body No. 15 in Table 2 (Example product: 4 mol % Y 2 O 3 -0.4mol%La 2 O 3 22 ) observed by a scanning electron microscope (magnification 10,000 times). For the zirconia sintered body No. 13 (Example) in Table 2, a histogram showing the texture crystal grain size distribution (area basis) analyzed using the observation image of FIG. 22 . For the zirconia sintered body No. 15 (Example) in Table 2, a histogram showing the texture crystal grain size distribution (area basis) analyzed using the observation image of FIG. 23 . For the zirconia sintered body No. 15 (Example) in Table 2, a histogram showing the texture crystal grain size distribution (area basis) analyzed using the observation image of FIG. 23 . For the zirconia sintered body No. 15 (Example) in Table 2, a histogram showing the texture crystal grain size distribution (area basis) analyzed using the observation image of FIG. 23 . For the zirconia sintered body No. 15 (Example) in Table 2, a histogram showing the texture crystal grain size distribution (area basis) analyzed using the observation image of FIG. 23 . For the zirconia sintered body No. 15 (Example), ... 1 is a graph in which the values ​​of total light transmittance of the zirconia sintered body disclosed in Patent Document 4 are plotted against the area ratio of crystal grains of 0.76 μm or more. 2 is a graph in which the values ​​of bending strength and fracture toughness of the zirconia sintered bodies disclosed in Patent Documents 1, 2, and 3 are two-dimensionally plotted.

[0022] In the zirconia sintered body of the embodiment, Y in the total composition of the sintered body 2 O 3The content of is 2.5 mol % or more and 6 mol % or less, and the balance is ZrO 2 and unavoidable impurities. 2 O 3 If the content of Y is less than 2.5 mol%, the amount of T phase produced will be excessive, and cracks will easily occur in the sintered body when sintered at room temperature. In addition, the crystal grains will be excessively refined, making it difficult to ensure the transparency of the sintered body. 2 O 3 If the content of Y exceeds 6 mol%, the amount of T phase produced will be small, excessive growth of crystal grains will occur, and it will be difficult to ensure the fracture toughness value of the sintered body. 2 O 3 The content of CaF is more preferably 3.0 mol % or more and 5.5 mol % or less, and more preferably 3.5 mol % or more and 5.2 mol % or less. 2 The term "T phase" refers to a tetragonal phase, and the term "M phase" refers to a monoclinic phase.

[0023] Furthermore, the zirconia sintered body must have a relative density of 99% or more, preferably 99.5% or more, so that it can have sufficient mechanical properties.

[0024] In the zirconia sintered body of the embodiment, the area-average particle size of the zirconia crystal particles is 0.4 μm or more and 0.9 μm or less in an electron microscope image of the sintered body structure. If the area-average particle size is less than 0.4 μm, it becomes difficult to ensure the transparency of the sintered body, and if it exceeds 0.8 μm, the fracture toughness value of the sintered body becomes insufficient. The area-average particle size of the zirconia crystal particles is preferably 0.5 μm or more and 0.8 μm or less. Furthermore, the area ratios of zirconia crystal particles having a particle size of less than 0.1 μm and zirconia crystal particles having a particle size of more than 2 μm are both less than 1%. If the area ratio of zirconia crystal particles having a particle size of more than 2 μm becomes 1% or more, the fracture toughness value of the sintered body becomes insufficient. Furthermore, it is difficult to achieve 1% or more of zirconia crystal particles having a particle size of less than 0.1 μm in normal pressure sintering.

[0025] The area ratio of the first region made of zirconia crystal grains having a grain size of 0.1 μm or more and less than 0.5 μm is 5% or more and 80% or less, while the area ratio of the second region made of zirconia crystal grains having a grain size of 0.8 μm or more and less than 2 μm is 5% or more and 80% or less. 2 O 3 The concentration is 3.5 mol % or more and 7.0 mol % or less, while the average Y of the zirconia crystal grains forming the first region is 2 O 3 The concentration is 1.7 mol % or more and 5 mol % or less, and 2 O 3 The difference in density is ΔC≡C2−C1, and the value of ΔC / C2 is set to 0.2 or more and 0.5 or less.

[0026] In the zirconia sintered body of the embodiment, the first region, which is composed of zirconia crystal grains with a grain size of 0.1 μm or more but less than 0.5 μm, is a region mainly composed of fine crystal grains, and increasing the number of crystal grains in this region has generally been considered advantageous for improving the mechanical strength of the material. However, from the perspective of improving fracture toughness, as is clear from the disclosure of Patent Document 4 (see Figure 31), simply increasing the number of crystal grains in this region is not expected to significantly improve fracture toughness. The reason for this is that if the proportion of T phase, which contributes to suppressing rapid crack propagation, i.e., unstable fracture, is low, even a refined crystal grain region is not thought to lead to improved fracture toughness.

[0027] On the other hand, the second region, which is made up of zirconia crystal grains with a grain size of 0.8 μm or more but less than 2 μm, is a region mainly composed of coarse crystal grains larger than the wavelength of visible light, and an increase in the crystal grains in this region is considered to be advantageous in improving the effect of light scattering at the crystal grain boundaries. However, as mentioned above, even in the test sample disclosed in Patent Document 4 in which the area ratio of the crystal grains in this region has increased to about 60%, the total light transmittance at a thickness of 0.5 mm is at most about 30%, and it is difficult to say that the transparency has been dramatically improved. For example, in Patent Document 4, 2 O 3As is clear from FIG. 15, in the composition around the sintering temperature (for example, 1500° C.), the C phase (equilibrium Y 2 O 3 The concentration is around 6.3 mol%) and M phase (equilibrium Y 2 O 3 The equilibrium ratio of the two (concentration is around 1.5 mol%) is close to 1:1, and the crystal grains in the sintered body contain Y. 2 O 3 High-concentration C phase domains and Y 2 O 3 It is believed that a modulated structure is created in which the Y phase domains and the T phase domains with low concentration are finely mixed (see, for example, Non-Patent Documents 5 and 6). 2 O 3 The difference in concentration and lattice constant is a major factor in light scattering. As a result, even if the crystal grain size itself is large, the contribution to improving transparency is thought to be relatively small, with the effect of suppressing light scattering at the crystal grain boundaries.

[0028] In the structure shown in Patent Document 4, in which a first region with fine crystal grains and a second region with coarse crystal grains are mixed, it is believed that there is almost no difference in the distribution of the T-phase domains and the C-phase domains in each region. Even though the zirconia sintered body is toughened, the fracture morphology is essentially brittle fracture, and the cracks accompanying the fracture propagate through the crystal grains. Considering that the toughening mechanism of the zirconia sintered body is the prevention of unstable fracture due to martensitic transformation of the T-phase domains, it is believed that, in a state in which there is no difference in the distribution of the T-phase and the C-phase, it is difficult to achieve high fracture toughness and transparency at the same time, even if the ratio of the first region to the second region is controlled.

[0029] Therefore, in the zirconia sintered body of the embodiment, the Y of the first region with fine crystal grains 2 O 3 The concentration of Y in the second region with coarse grains is 2 O 3 The characteristic of this method is that the concentration of zirconia is adjusted to a certain level lower than the concentration of zirconia. By configuring the material in this way, it is possible to realize a zirconia sintered body that combines high levels of transparency and fracture toughness. From a microstructural perspective, the mechanism is presumed to be as follows.

[0030] That is, as described above, Y is formed between the first region having fine crystal grains and the second region having coarse crystal grains. 2 O 3 The difference in concentration causes a large difference in the distribution of the T-phase domains and the C-phase domains between the second region and the first region. Specifically, the ratio of the T-phase, which contributes to toughening by transformation into the M-phase, is Y. 2 O 3 The first region with low density becomes high, and Y 2 O 3 Conversely, the ratio of the stable C phase, which does not transform into the M phase, is low in the second region where the concentration is high. 2 O 3 It becomes higher in the second region where the concentration is high, and Y 2 O 3 It is lower in the first region where the concentration is low. 2 O 3 In the second region with a high concentration, the proportion of the highly stable C phase increases, the T phase domain boundaries are reduced, and the region is less susceptible to the strain field caused by martensitic transformation to the T phase, which reduces light scattering and significantly contributes to translucency. Therefore, if the second region has such a structure, the transparency of the sintered body can be significantly improved by increasing its area ratio.

[0031] On the other hand, crack propagation within the sintered body is relatively easy within the coarse crystal grains of the second region, which has a low T-phase domain density. However, when the crack tip reaches the fine crystal grains of the first region surrounding it, the increased T-phase domain density in the first region increases the probability that the crack propagation will be stopped by martensitic transformation of the T-phase. As a result, even if the area ratio of the second region is increased to some extent to improve transparency, the fracture toughness value is less likely to be impaired because the crystal grains of the first region, which have a strong crack propagation prevention effect, are dispersed at an appropriate area ratio. Therefore, it is presumed that high levels of transparency and fracture toughness can be achieved.

[0032] If the area ratio of zirconia crystal particles in the first region is less than 5% or the area ratio of zirconia crystal particles in the second region exceeds 80%, the fracture toughness of the zirconia sintered body cannot be sufficiently ensured. Furthermore, if the area ratio of zirconia crystal particles in the first region exceeds 80% or the area ratio of zirconia crystal particles in the second region is less than 5%, the transparency of the sintered body cannot be sufficiently ensured. The area ratio of zirconia crystal particles in the first region is more preferably 10% to 45%, and the area ratio of the second region is more preferably 20% to 50%. Furthermore, when the area ratios of zirconia crystal particles in the first region and the second region are adjusted to fall within the above-mentioned ranges, the area ratio of the third region, which is made up of zirconia crystal particles having a particle size of 0.5 μm to less than 0.8 μm, is 10% to less than 55%. Here, the total area ratio of the first region, second region, and third region is 98% or more (the remainder is, for example, a region occupied by zirconia crystal particles having a particle size of less than 0.1 μm or zirconia crystal particles having a particle size of more than 2 μm).

[0033] In addition, the average Y of the zirconia crystal grains in the first and second regions 2 O 3 Regarding concentrations C1 and C2, the crystal grains of the zirconia sintered body are composed of two phases, C phase and T phase, at the sintering temperature, and Y in the total composition of the sintered body is 2 O 3 Since the content of is 2.5 mol % or more and 6 mol % or less, the average Y of the zirconia crystal grains in the second region having a high C phase ratio is 2 O 3 The concentration C2 falls within the range of 3.5 mol % to 7.0 mol %, and the average Y content of the zirconia crystal grains forming the first region with a high T phase ratio is 2 O 3 The concentration C1 falls within the range of 1.7 mol % to 5 mol %. 2 O 3 If the difference in concentration is ΔC≡C2-C1, and the value of ΔC / C2 is less than 0.2, the T phase ratio in the first region becomes insufficient, and the fracture toughness value of the zirconia sintered body cannot be sufficiently secured. 2 O 3It is difficult to obtain a sintered body with a specified concentration C1 by normal atmospheric sintering. The value of ΔC / C2 is more preferably 0.25 or more and 0.5 or less, and even more preferably 0.3 or more and 0.45 or less. By satisfying these requirements, the fracture toughness value of the zirconia sintered body of the embodiment is 4.5 MPa m 0.5 12MPa・m or more 0.5 The fracture toughness is preferably 5.5 MPa m 0.5 10MPa・m or more 0.5 It should be the following:

[0034] The fracture toughness values ​​used in this embodiment are values ​​measured by the IF (Indentation Fracture) method. Non-Patent Documents 3 and 4 point out that fracture toughness values ​​measured and calculated by the IF method tend to be lower than fracture toughness values ​​measured by other methods due to the accuracy of crack tip reading. On the other hand, the IF method has the advantage that it can be measured without any problems even when it is difficult to remove a test piece from a sintered product. Furthermore, the fact that the fracture toughness measurement value appears low can be considered to provide a safety margin in ensuring a higher fracture toughness value of the material. The aforementioned IF method is a method in which a Vickers hardness tester conforming to JIS R 1607 is used to press a Vickers indenter into a test piece under conditions of a load of 30 kgf and an indentation time of 15 seconds, and the length of the indentation and crack generated are measured. From this measurement, the fracture toughness value "K IC " is calculated. Fracture toughness value K IC =0.018×(E / H) 0.5 × (P / c 1.5 ) K IC : Fracture toughness value (MPa m 0.5 E: Young's modulus (GPa), where 205 GPa was applied to the Young's modulus. H: Vickers hardness (HV) = 0.1891 P / (2a) 2 c: Half the average crack length (m) a: Half the average indentation length (m) P: Vickers indenter indentation load (N) (1 kgf = 9.80665 N)

[0035] The transparency of the zirconia sintered body is evaluated by measuring the total light transmittance of a test piece of the zirconia sintered body processed to a thickness of 0.5 mm using CIE standard illuminant D65 in the visible light wavelength range of 380 nm to 780 nm. The total light transmittance is preferably 40% to 60%, which is higher than the value disclosed in, for example, Patent Document 4, and more preferably 45% to 56%.

[0036] The zirconia sintered body of the above embodiment can be produced by atmospheric sintering using a zirconia raw material powder having the following specific particle size distribution: In other words, the zirconia powder is produced using a raw material powder having a particle size distribution measured on a volume basis with a laser scattering particle sizer, in which: an arithmetic mean particle size of 0.10 μm or more and 0.15 μm or less, an arithmetic standard deviation of 0.03 μm or more and 0.05 μm or less, no particles with particle sizes exceeding 0.8 μm or less and no particles with particle sizes less than 0.03 μm are measured, and the measured values ​​of particles with particle sizes exceeding 0.4 μm and particles equal to or less than 0.04 μm are both 0.5% or less.

[0037] The particle size distribution measurement results of an example of a zirconia raw material powder that satisfies the above conditions (hereinafter referred to as a "recommended zirconia raw material powder") are shown in FIG. 2 O 3 The content was 4.5 mol%, and the particle size distribution measured on a volume basis using a laser scattering particle size analyzer (apparatus used: HORIBA LA-960) showed: - Arithmetic mean particle size: 0.129 μm - Arithmetic standard deviation: 0.040 μm - The measured values ​​of particles exceeding 0.4 μm and particles equal to or less than 0.04 μm were zero (thus, the measured values ​​of particles exceeding 0.8 μm and particles less than 0.03 μm were also zero). More specifically, the maximum value of the class in which particles were measured was 0.39 μm, and the class exceeding 0.35 μm, which is the large diameter peak of the bimodal powder of Patent Document 2, was 1% or less (zero in Figure 1). This powder was obtained by mixing commercially available pure zirconia powder and pure Y 2 O 3 A total of 1 kg of the powder, 15 kg of zirconia media with a diameter of 3 mm, and 1.7 kg of pure water were placed in a pot with an inner diameter of approximately 800 mm, and pulverized at a rotation speed of 78 rpm for 20 hours to obtain the powder.

[0038] On the other hand, the particle size distribution measurement results of an example of a zirconia raw material powder (hereinafter referred to as a "reference zirconia raw material powder") that does not satisfy the above conditions are shown in FIG. 2 O 3 The content was 4.5 mol%, and the particle size distribution measured on a volume basis using a laser scattering particle size analyzer was as follows: Arithmetic mean particle size: 0.251 μm Arithmetic standard deviation: 0.124 μm The measured value of particles of 0.04 μm or less was zero, while the measured value of particles of more than 0.4 μm was 10.28%. The powder was prepared by adding yttrium chloride to a hydrated zirconia sol obtained by hydrolyzing an aqueous solution of zirconium oxychloride, followed by drying and calcining. 2 O 3 The powder was obtained by placing 1 kg of calcined zirconia powder, 15 kg of zirconia media with a diameter of 3 mm, and 1.7 kg of pure water in a pot with an inner diameter of approximately 800 mm, and pulverizing the mixture at a rotation speed of 78 rpm for 10 hours.

[0039] In both cases, the zirconia media used was Y 2 O 3 The material used is a partially stabilized zirconia sintered body with a content of 4.5 mol%. Table 2 shows the volumetric frequency of each particle size class of the raw material powders shown in Figures 1 and 2, as well as the surface area and surface area ratio for each class per gram of powder, calculated by approximating the crystal grains to spheres.

[0040]

[0041] The recommended zirconia raw material powder is one that contains zirconia components in the state before grinding. 2 O 3 The zirconia particles are formulated in the form of zirconia particles that do not contain Y (i.e., pure zirconia powder particles). In addition, Y is contained as a stabilizer for the zirconia phase after firing. 2 O 3 The ingredients are pure Y 2 O 3 In other words, the recommended zirconia raw material powder contains Y as a solid solution component. 2 O 3The zirconia powder particles having a zirconia content of less than 1.2 mol % (including 0 mol %: in FIG. 15 , the region where the M-phase is the only phase at room temperature) and the yttria powder particles having a zirconia content of less than 1.0 mol % (including 0 mol %) as a solid solution component are blended and ball milled to obtain the zirconia powder particles.

[0042] The zirconia powder particles in the recommended zirconia raw material powder are Y 2 O 3 Since the amount of solid solution of the components is small, transformation toughening is difficult to achieve, and partially stabilized zirconia sintered body (Y 2 O 3 Compared to tough zirconia media with a solid solution content of, for example, 2.0 mol% or more and 5.0 mol% or less, yttria has a lower hardness and fracture cracks are more likely to propagate. Therefore, fine pulverization due to the impact force from the zirconia media is more likely to proceed, the average diameter of the powder particles can be reduced in a relatively short pulverization time, and coarse powder particles are less likely to remain. This is extremely advantageous for obtaining a zirconia raw material powder having the aforementioned specific particle size distribution (see FIG. 1 ) with a sharpened particle size distribution. Furthermore, since yttria powder particles have an even lower hardness than zirconia powder particles, pulverization also proceeds through contact with zirconia powder particles contained as a raw material, and finer pulverization than zirconia powder particles and uniform mixing with zirconia powder particles can be expected. The concept of such a recommended zirconia raw material powder is based on a composition range (Y 2 O 3 The method can also be employed in the production of a zirconia sintered body having a zirconia content of less than 2.5 mol %.

[0043] On the other hand, in the reference zirconia raw powder, the zirconia powder particles are formed by calcination. 2 O 3It is believed that transformation toughening is already manifested at the particle stage as a result of the solid solution of the components. Therefore, the zirconia powder particles to be milled have a high hardness comparable to that of the zirconia media, and even if fracture cracks attempt to occur within the particles, their propagation is suppressed by the transformation toughening mechanism. Therefore, fine milling due to the impact force from the zirconia media is difficult to proceed, and coarse powder particles are likely to remain. Therefore, it is presumed that it is difficult to obtain a zirconia raw material powder with the aforementioned characteristic particle size distribution (see Figure 1), which has a sharp particle size distribution, using conventional ball milling.

[0044] In addition to the above-mentioned recommended zirconia raw material powder prepared using pure zirconia powder and pure yttria powder, the recommended zirconia raw material powder is also prepared using Y powder within the above-mentioned composition range. 2 O 3 The zirconia powder may be prepared using a zirconia powder containing a solid solution of the zirconia component, or a yttria powder containing a solid solution of the zirconia component. However, since the pulverization of zirconia powder particles becomes easier as the amount of the yttria component in solid solution decreases, it is more desirable to use a pure zirconia powder and a pure yttria powder when it is desired to further refine the obtained zirconia raw material powder and to sharpen the particle size distribution.

[0045] Figure 3 is a scanning electron microscope image (magnification 10,000x) of the surface of a zirconia sintered body (Table 1: Number 10, corresponding to an example of the embodiment (present invention)) produced by atmospheric pressure sintering at 1500°C for 2 hours in air using the raw material powder of Figure 1 (Table 1: Number 10, corresponding to an example of the embodiment (present invention)). It can be seen that the structure is a mixture of relatively fine crystal grains of 0.4 μm or less (first region) and somewhat coarse crystal grains of over 0.8 μm (second region). On the other hand, Figure 4 is a scanning electron microscope image (magnification 10,000x) of a zirconia sintered body (Table 1: Number 22, corresponding to a comparative example of the embodiment (present invention)) produced by atmospheric pressure sintering at 1500°C for 2 hours in air using the raw material powder of Figure 2 (Table 1: Number 22, corresponding to a comparative example of the embodiment (present invention)). It can be seen that the zirconia sintered body exhibits a completely different structure from the sintered body of Figure 3, despite using a raw material powder with a substantially identical composition. The sintered body structure of the comparative example exhibits an equiaxed structure in which closely spaced crystal grains exceeding 0.4 μm in size are uniformly observed, with almost no fine crystal grains being observed.

[0046] In this specification, the crystal grain size distribution on an electron microscope image is quantified using the following method. First, 300 to 400 crystal grains are randomly extracted from the image. In this specification, as shown in FIG. 5, multiple sampling lines SL are set on the image, and crystal grains crossed by each sampling line are selected as extraction targets. The intervals between the sampling lines are adjusted so that no single crystal grain is crossed by multiple sampling lines. Then, for each crystal grain passing through each sampling line, parallel lines circumscribing the outline of the crystal grain are drawn vertically and horizontally on the image. When the intervals between the parallel lines are D1 and D2, the value Dm = (D1 + D2) / 2 is calculated, and the diameter of a circle having the same area as Dm is defined as the particle size of each extracted crystal grain.

[0047] Fig. 7 is a histogram showing the texture crystal grain size distribution (area basis) of the zirconia sintered body No. 10 in Table 1, analyzed by the above method using the observation image of Fig. 3. Fig. 8 is a histogram showing the texture crystal grain size distribution (area basis) of the zirconia sintered body No. 22 in Table 1, analyzed in the same manner using the observation image of Fig. 4. It can be seen that the area ratio of the crystal grains in the first region having a crystal grain size of 0.4 µm or less reaches 14.5% for the zirconia sintered body of the example of the embodiment (Fig. 7), whereas the area ratio of the crystal grains in the first region for the zirconia sintered body of the comparative example (Fig. 8) is significantly lower at 4.9%.

[0048] Since all sintered bodies had relatively smooth surfaces, no special polishing was performed, and the as-sintered surfaces were directly observed under magnification. To be sure, the surfaces of the sintered bodies were mirror-polished, and then thermally etched for 1 hour at 1450°C, 50°C lower than the sintering temperature, and the grain size distribution was measured using the same method on the structures. It should be noted that, within the range discussed in this specification, the calculation results for the area ratios of the first and second regions agreed within ±5% with the results obtained when using observation images of the unpolished sintered body surface.

[0049] In addition, the average Y 2 O 3The concentrations were analyzed using a field emission electron probe microanalyzer (EPMA: JXA-8530F (JEOL Ltd.)) by the following method. That is, as shown in FIG. 6, in the observation field of the electron microscope (magnification 10,000 times), for the first region where crystal particles of 0.4 μm or less are densely concentrated (region PA surrounded by a white dashed line in the figure; each region PA also contains some crystal particles of the third region of intermediate size, and the area of ​​region PA does not mean that it is the area of ​​only the first region), the spot diameter was adjusted in the range of 0.3 to 0.8 μm so that 3 to 4 crystal particles of 0.4 μm or less were contained within the spot of the irradiated electron beam, as shown by the solid white circle AC1 in FIG. 6, and the concentrations of Zr, Y, and O were analyzed. Then, the same measurement was carried out five times while changing the spot position on the field of view, and the Y concentration was calculated from the average value of these results. 2 O 3 The concentration was calculated.

[0050] On the other hand, for the crystal grains in the second region exceeding 0.8 μm (crystal grains SA exemplified by white arrows in the figure), as shown by the solid black circle AC2 in Figure 6, the spot diameter is adjusted in the range of 0.5 to 0.8 μm so that the spot of the irradiated electron beam sufficiently covers the region inside the crystal grain, including the center, and the concentration analysis of Zr, Y, and O is performed. Then, the same measurement is performed on 10 crystal grains while changing the spot position on the field of view, and Y is calculated from the average value of the results. 2 O 3 For the zirconia sintered body of the comparative example in which the area ratio of crystal grains of 0.4 μm or less was small, 10 crystal grains of 0.4 μm or less were individually extracted, and the spot diameter was adjusted so that the spot of the irradiated electron beam was contained within each crystal grain, and then analysis was performed.

[0051] 7 and 8 show the average Y 2 O 3 The analysis results of the concentration are also shown in the table, along with the measurement results of the fracture toughness value and the total light transmittance. For the zirconia sintered body of the example of the embodiment (FIG. 7), the average Y of the first region having a crystal grain size of 0.4 μm or less is 2 O 3 The concentration of Y in the entire sintered body 2 O3 The average Y concentration in the second region having a crystal grain size of more than 0.8 μm is 3.6 mol%, which is lower than the 4.5 mol% concentration in the first region. 2 O 3 The concentration was 5.7 mol%, which is the same as the Y concentration of the entire sintered body. 2 O 3 On the other hand, for the zirconia sintered body of the comparative example (FIG. 8), the average Y concentration in the first region was 2 O 3 The concentration is 4.7 mol%, and the average Y 2 O 3 The concentration was 4.4 mol%, and both were the same as the Y concentration of the entire sintered body. 2 O 3 The concentration (4.5 mol%) was similar to that of the Y 2 O 3 No significant difference in concentration was observed. It can be seen that the zirconia sintered bodies of the examples of the embodiment have significantly higher fracture toughness and total light transmittance than the zirconia sintered bodies of the comparative examples.

[0052] Furthermore, as a result of more detailed analysis by EPMA, it was found that the zirconia sintered body of the example product has a Y-type crystal grain at the center of the zirconia crystal grain that forms the second region in the sintered body structure. 2 O 3 The outer Y 2 O 3 The crystal grains in the second region have a size of 0.8 μm or more, which is larger than the wavelength of visible light, and 2 O 3 As already explained, the ratio of the highly concentrated and highly phase-stable C phase increases, and the T-phase domain boundaries are reduced, resulting in a significant contribution to translucency. With the above structure, the central portion of the crystal grain in the second region is occupied by the highly phase-stable C phase, which is thought to be even more advantageous in improving the transparency of the sintered body.

[0053] As shown in Figure 6, the sintered body structure has a rock garden-like structure in which zirconia crystal particles SA (crystal particles outlined with a white dashed line) belonging to the second region are dispersed as coarse dispersed particles against a background region consisting of zirconia crystal particles PA (crystal particles surrounded by a white solid line) belonging to the first region and zirconia crystal particles belonging to the third region. The structure of such a zirconia sintered body can be said to be morphologically similar to that disclosed in Patent Document 4. On the other hand, the sintered body of Patent Document 4 has a composition almost identical to that of the Examples, but its fracture toughness value and total light transmittance value are significantly inferior to those of the Examples, and therefore, although no specific disclosure is made, it is possible that the Y in the structure 2 O 3 The concentration distribution is thought to be significantly different from that of the example product.

[0054] FIG. 9 shows an image (magnification: 10,000 times) of the zirconia sintered body of the above-mentioned example product observed by a scanning electron microscope in another field of view, and a Y line along an analysis line that crosses the background region and a plurality of coarse dispersed particles in the field of view. 2 O 3 The figure shows the results of EPMA line analysis in which the concentration was measured. What is distinctive is that the Y distribution is shown in the form of a maximum point within each coarse dispersed particle and a minimum point within the background region. 2 O 3 The concentration profile shows a continuous wave-like change in concentration. 2 O 3 The concentration profile is particularly remarkable when the area ratio of the second region is 15% or more and 50% or less. The resistance to crack propagation is relatively low in the coarse dispersed particles (crystal grains of the second region) mainly composed of C phase domains. However, the resistance to crack propagation is relatively low in the crystal grains belonging to the first region (and the third region). 2 O 3 A region where the concentration is reduced, i.e., a region where the T phase domain ratio increases, is formed around the coarse dispersed particles, and based on the concentration profile described above, the Y 2 O 3 It is believed that a structure in which the concentration reduction amount is large, that is, a structure in which the T-phase domain ratio increases gradually with increasing distance from the coarse dispersed particles, can more easily ensure a good fracture toughness value.

[0055] By using raw material powder with a sharp particle size distribution as shown in FIG. 1, the average Y 2 O 3 The mechanism by which the characteristic structure with different concentrations is obtained can be assumed to be as follows. That is, the raw material powder contains almost no particles with a particle size exceeding 0.4 μm, and almost all of the powder particles have a sharp particle size distribution peak within the range of 0.06 to 0.3 μm. When such raw material powder is molded and sintered, in the initial stage of sintering, as shown in State 1 in Figure 10, there are almost no large crystal particles exceeding 0.4 μm, and small crystal particles SG predominate. At this stage, as shown in Figure 12, the mechanism by which adjacent small crystal particles SG bond and coalesce with each other is predominant, and it is thought that the slow, uniform growth continues for a while without producing protruding large particles.

[0056] However, a small number of relatively large powder particles near the large particle size tail of the particle size distribution tend to grow larger than the others. When the particle size exceeds a certain critical value, they rapidly grow into large crystal particles BG by consuming the surrounding fine crystal particles FG, as shown in State 2. However, because the number of these large crystal particles BG is small, they form islands independent of the surrounding particles. On the other hand, small crystal particles SG that are separated from the large crystal particles BG continue to grow relatively slowly, primarily through the coalescence mechanism shown in Figure 12. Because the number of island-like large crystal particles BG is limited, they do not coarsen the entire structure, as shown in State 3. Meanwhile, small crystal particles FG that do not reach the large crystal particles to which they coalesce remain stranded between the large crystal particles BG. These become crystal particles in the first to third regions that form the background region, and the large crystal particles BG become crystal particles (coarse dispersed particles) SA in the second region that are dispersed in island-like shapes in the background region (see Figure 6).

[0057] If there are few large crystal grains BG that grow extremely large, the average difference in particle size between the large crystal grains BG and the adjacent small crystal grains SG (SG(1) to (3)) will remain relatively small, as shown in Figure 13. According to the known theory of neck formation in solid-phase sintering, the larger the dimensional difference between the adjacent large crystal grains SG and the adjacent large crystal grains BG, the smaller the radius of curvature ρ of the neck N at the junction, which reduces the vapor pressure and generates an increment in vacancy concentration ΔC in the neck N that is greater than that in the bulk. The vacancy concentration gradient in the neck N is expressed as ΔC / ρ, which acts as the driving force for vacancies to diffuse into the interior of the crystal grains, while in turn, the constituent atoms of the crystal grains flow into the voids V between the crystal grains. This causes the voids V to shrink and solid-phase sintering to proceed. Since the excess vacancy concentration increase ΔC is thought to be concentrated on the side of the small crystal grains SG with a small radius of surface curvature, atomic diffusion proceeds in the direction of filling the voids V, causing the small crystal grains SG to shrink and the large crystal grains BG to grow.

[0058] At this time, the smaller small crystal particles SG(3), which have a large size difference with the large crystal particles BG, have a large atomic diffusion flux toward the large crystal particles BG, and are absorbed and disappear. Since the small crystal particles SG(3) are entirely taken up by the large crystal particles BG, the Y of the large crystal particles BG 2 O 3 This also applies to the case where the fine crystal particles FG (or the small crystal particles SG) shown in FIG.

[0059] On the other hand, the atomic diffusion flux of the larger small crystal particles SG(1) or SG(2) toward the large crystal particles BG is relatively small, and many of them remain without being absorbed by the large crystal particles BG. In this case, it is presumed that the atomic diffusion coefficient from the small crystal particles SG(1) and SG(2) toward the large crystal particles BG is larger for Y than for Zr. In other words, it is thought that the larger the particle size of the small crystal particles SG(1), the more likely it is that Y will diffuse toward the large crystal particles BG.

[0060] Y of large crystal grains BG that have grown using small crystal grains as seeds 2 O 3If we consider that the concentration is increased by this estimated mechanism, then the large crystal grains are in contact with small crystal grains with a lower Y concentration. In other words, the concentration gradient of Y atoms is formed in the direction from the large crystal grains to the small crystal grains, i.e., in the opposite direction to the estimated diffusion direction of Y atoms. However, the EPMA analysis results shown in the figure strongly suggest that Y diffuses from the small crystal grains to the large crystal grains, overcoming this concentration gradient.

[0061] According to the equilibrium diagram of FIG. 2 -Y 2 O 3 The binary composition is ZrO 2 According to Fig. 10 of Non-Patent Document 1, which is the source of the reference, the Y 2 O 3 In the concentration range, the free energy ΔGv of the T phase is lower than that of the C phase, and the difference between the two is Y 2 O 3 The larger the concentration, the smaller the crystal size. When the size of the crystal grains is taken into consideration, the total energy of the crystal can be expressed as the sum of the above-mentioned phase free energy term (volume energy) and interfacial tension energy term (area energy). As the crystal grains become finer, the contribution of the interfacial tension energy term to the total energy increases. Therefore, if a large amount of T phase, which has a low phase free energy, is produced, the total energy of the crystal decreases, making it energetically stable. Therefore, it can be thought that small crystal grains cause Y to flow toward large crystal grains in order to increase the T phase ratio.

[0062] If the outflow of Y from the small crystal grains SG to the large crystal grains BG progresses, the Y 2 O 3 The concentration increases, and the Y 2 O 3 In this case, the smaller the crystal grains SG that are left behind, the greater the Y concentration. 2 O 3 As the concentration decreases, the larger the grain size BG, the more Y the outer region that is thickened later in time. 2 O 3The concentration is expected to be low.

[0063] If the voids V are reduced, the shrinkage of the sintered body slows down, and the vacancy concentration, which acts as the driving force for atomic diffusion, also decreases, so that the remaining small crystal grains SG are less likely to coalesce or be absorbed into the large crystal grains BG. 2 O 3 While the concentration profile is being formed, Y is formed between the small crystal grains SG and the large crystal grains BG. 2 O 3 It is thought that the formation of tissue with a large concentration difference is largely completed. 2 O 3 The lower the concentration of small crystal particles SG, the higher the T phase ratio, and the greater the difference in phase free energy between them and the large crystal particles BG, which have a high C phase ratio, making it more difficult for them to coalesce with the large crystal particles BG.

[0064] Next, when raw material powder with a broad particle size distribution as shown in FIG. 2 is used, the Y 2 O 3 The reason why concentration differences are less likely to occur can be presumed as follows. As shown in State 1 in Figure 11, when such a raw material powder is used, large crystal particles BG that are originally present in the raw material powder are already present in large numbers at the early stage of sintering, and as shown in Figure 14, their dimensions are considerably larger than when the raw material powder in Figure 1 is used. In particular, in the case of bimodal powders having two peaks, one at 0.3 to 0.5 μm and the other at 0.15 μm or less, as in Patent Documents 2 and 4, the content ratio of large crystal particles exceeding 0.4 μm is particularly high.

[0065] The Y of such large crystal particles BG originated from powder particles with large dimensions already in the raw material stage. 2 O 3 The concentration is close to the composition at the time of blending, 2 O 3In this case, as shown in Fig. 14, in the early stage of sintering when many voids remain, the number ratio of fine powder particles FG and small crystal particles SG with a small growth rate among the particles in contact with the large crystal particles BG becomes much larger than in the case of Fig. 13, and most of them are absorbed into the large crystal particles BG and disappear, similar to the small crystal particles SG(3) in Fig. 13. In such a case, the Y of the large crystal particles BG 2 O 3 As already explained, the concentration is unlikely to increase.

[0066] Therefore, until the critical size is reached at which absorption into the large crystal grains BG becomes difficult, the surrounding small crystal grains SG are absorbed into one of the many large crystal grains BG and disappear, and this process continues for a long time, resulting in a state like state 2 in Figure 11. Therefore, until the large crystal grains BG grow considerably large, there is not much inflow of Y from the small crystal grains SG, and the Y between the large crystal grains BG and the small crystal grains SG is 2 O 3 When a raw material powder with a bimodal distribution as in Patent Documents 2 and 4 is used, the Y concentration remains small. 2 O 3 Sintering is completed with a relatively large number of small crystal grains SG, whose concentration has not decreased significantly, remaining between the large crystal grains BG (Fig. 11: left side of State 3). Also, when a raw material powder with a relatively large average grain size and a broad, single-peak particle size distribution is used as in Fig. 2 of the present invention, the growth of the large crystal grains BG continues until they have almost completely consumed the small crystal grains SG, and it is thought that an equiaxed crystal structure with a large average crystal grain size is reached (Fig. 11: left side of State 3). It has been confirmed that in zirconia sintered bodies exhibiting an equiaxed crystal structure such as the latter, Y segregates near the grain boundaries where large crystal grains are adjacent (Non-Patent Document 5). Such Y 2 O 3 It should be noted that the concentration distribution shows a tendency that is completely opposite to that of the embodiment shown in FIG. 9, in that the Y concentration is low in the outer periphery of the large crystal grains BG and in the surrounding small crystal grains.

[0067] If the raw material powder for producing the zirconia sintered body of the above embodiment deviates from any of the above-mentioned: an arithmetic mean particle size of 0.10 μm or more and 0.15 μm or less; an arithmetic standard deviation value of 0.03 μm or more and 0.05 μm or less; particles with particle sizes exceeding 0.8 μm and particles less than 0.03 μm are not measured; and the measured values ​​of particles with particle sizes exceeding 0.4 μm and particles equal to or less than 0.04 μm are both 0.5% or less, the average Y of the zirconia crystal particles constituting the first region is considered to be low. 2 O 3 Concentration C1 (first Y 2 O 3 The concentration C1) is the average Y of the zirconia crystal grains forming the second region. 2 O 3 Concentration C2 (second Y 2 O 3 In this case, it becomes difficult to obtain a characteristic concentration distribution form in which the specific surface area of ​​the raw material powder measured by the BET method is 13 m or less (specifically, when ΔC≡C2-C1, the value of ΔC / C2 is 0.2 or more and 0.5 or less). In addition, taking into consideration the formation of secondary particles in the powder, the inclusion of particles of 0.04 μm or less at the primary particle level is more reliably excluded. 2 The specific surface area of ​​the raw material powder is preferably 8 m / g or less in relation to the arithmetic mean particle size being 0.10 μm or more and 0.15 μm or less. 2 It is preferable to set it to 1 / g or more.

[0068] Next, in the zirconia sintered body of the embodiment, the remaining ZrO 2 A part of the sintered body has a La content of 0.1 mol % or more and 1 mol % or less in the total composition of the sintered body. 2 O 3 In this composition range, La can be substituted with lanthanum oxide. 2 O 3 By adding La 2 O 3 The total light transmittance of the zirconia sintered body can be further improved compared to that of the zirconia sintered body not containing ZrO. 2 La 2 O 3The amount of substitution is more preferably 0.15 mol % or more and 0.8 mol % or less, and even more preferably 0.15 mol % or more and 0.6 mol % or less, in terms of content in the entire composition of the sintered body.

[0069] In the zirconia sintered body of the embodiment, the remainder is ZrO 2 A part of the 2 O 3 (aluminum oxide). 2 (titanium oxide). 2 O 3 or TiO 2 The inclusion of does not particularly hinder the realization of the characteristic structure and component distribution form of the zirconia sintered body of the embodiment described above in detail, and furthermore, the fracture toughness value and total light transmittance brought about thereby.

[0070] In the embodiment, the term "unavoidable impurities" refers to components that can be contained within a range that does not impair the characteristics of the zirconia sintered body of the embodiment, and does not necessarily mean only residual components that cannot be actively removed in the raw material powder and manufacturing process of the zirconia sintered body, but the total amount thereof does not exceed 0.5 mol%. For example, in the embodiment, Y is used as a stabilizer. 2 O 3 is used, but other stabilizers include CaO, MgO (magnesium oxide) and CeO 2 (cerium oxide) may be contained as an inevitable impurity in this concept. 2 Silicon dioxide may also be contained as an unavoidable impurity, and its content in the total composition of the sintered body is preferably 0.1 mass % or less.

[0071] The zirconia sintered body according to the embodiment configured as described above preferably has a Vickers hardness Hv of 1150 or more, more preferably 1200 or more. As for the bending strength, it is desirable that a three-point bending strength test be carried out to ensure a bending strength of 600 MPa or more, assuming that atmospheric sintering is employed.

[0072] Although the method for producing the zirconia sintered body of the embodiment has already been partially explained, it is preferable to do it as follows. First, pure zirconia powder (average particle size: for example, 5 μm or less) and pure Y sintered powder as a stabilizer powder are mixed. 2 O 3 The powder (and oxide powders constituting other components) are blended to the desired composition, and then zirconia media with a diameter of 1.5 mm to 9 mm (preferably 1.5 mm to 5 mm) and a solvent (e.g., pure water) are mixed and placed in a pot, where they are pulverized at a predetermined rotation speed that causes an avalanche phenomenon in the contents. At this time, an appropriate amount of water-soluble binder is added, and after pulverization, the mixture is dried using a spray dryer or the like to obtain a composition for molding.

[0073] The composition may be press-molded into a green body, which may then be subjected to secondary processing such as cutting as necessary, followed immediately by sintering. Alternatively, a calcined body may be first prepared, and the calcined body may be subjected to secondary processing such as cutting, followed by sintering. When preparing a calcined body, the sintering temperature is preferably, for example, 800°C to 1200°C, and more preferably 900°C to 1000°C. The sintering temperature is preferably 1400°C to 1580°C, and more preferably 1420°C to 1550°C. Both the calcination and the sintering may be carried out in an atmospheric atmosphere at normal pressure.

[0074] When the green compact is immediately sintered, the sintering time to obtain a sufficiently dense sintered body is, for example, 70 to 180 minutes. On the other hand, if a calcined body is produced using a raw material powder with a particle size distribution that satisfies the above-mentioned conditions, the sintering time to densify the calcined body can be significantly reduced. When using such a calcined body, the sintering time is 60 minutes or less, preferably 30 minutes or less, and more preferably 20 minutes or less.

[0075] The method for producing a zirconia sintered body according to the embodiment can be appropriately modified and carried out as long as it does not particularly hinder the realization of the characteristic structure and component distribution form of the zirconia sintered body, and furthermore, the fracture toughness value and total light transmittance brought about thereby.

[0076] Furthermore, the zirconia sintered body of the embodiment can be used for various purposes, such as dental materials such as prosthetic materials, optical fiber connection parts such as ferrules and sleeves, various tools (e.g., grinding balls, grinding tools), various parts (e.g., screws, bolts and nuts), various sensors, electronics parts, decorative items (e.g., watch bands), etc. When the zirconia sintered body is used as a dental material, it can be used for, for example, copings, frameworks, crowns, crown bridges, abutments, implants, implant screws, implant fixtures, implant bridges, implant bars, brackets, denture bases, inlays, onlays, onlays, orthodontic wires, laminate veneers, etc.

[0077] Hereinafter, more detailed examples will be described using experiments conducted to confirm the effects and the results thereof. First, as raw material powder, commercially available pure zirconia powder was mixed with various ratios of pure Y. 2 O 3 Powder and pure La 2 O 3 A total of 1 kg of the powder blend, 15 kg of zirconia media with a diameter of 3 mm, and 1.7 kg of pure water were placed in a pot with an inner diameter of approximately 244 mm, and pulverized for 20 hours at a rotation speed of 78 rpm. After that, an appropriate amount of binder was added and mixed, and the slurry was dried with a spray dryer to obtain raw material powders of various compositions. 2 O 3 The composition with a concentration of 4.5 mol% was prepared by adding yttrium chloride to a hydrated zirconia sol obtained by hydrolyzing an aqueous solution of zirconium oxychloride, followed by drying and calcining. 2 O 3 A sample was also prepared using 3 mm diameter zirconia media per kg of calcined zirconia-containing powder, with a milling time of 10 hours (Table 1, No. 22, below). A portion of the slurry was not dried and was subjected to measurement of the powder particle size distribution using a laser scattering particle size analyzer. All powders, except for No. 22, had particle size distributions nearly identical to those shown in Figure 1, with the arithmetic mean diameter falling within the ranges of 0.115 to 0.130 μm and the arithmetic standard deviation falling within the ranges of 0.035 to 0.042 μm.

[0078] The raw material powder was then molded into a green compact (N = 3) using a hydraulic press, and sintered at 1500°C in atmospheric air to produce a zirconia sintered body. The sintered body was a plate measuring 40 mm x 30 mm x 3 mm. The density of the sintered body was measured using the Archimedes method, and by comparing it with the calculated true density for each composition, it was confirmed that all of the sintered bodies were densified to 99.5% or more.

[0079] Next, one of the three sintered bodies was cut into a first test piece measuring 30 mm × 30 mm × 3 mm and a second test piece measuring 30 mm × 10 mm × 3 mm. One of the main surfaces of the second test piece was observed using a Schottky electron microscope (HITACHI: SU5000) in low vacuum mode at a magnification of 10,000 times to obtain a structural image. Using the obtained structural image, the crystal grain size distribution was measured using the method already described to create a histogram, and the area ratios of the first region consisting of crystal grains with a crystal grain size of 0.1 μm or more but less than 0.5 μm, the third region consisting of crystal grains with a crystal grain size of 0.5 μm or more but less than 0.8 μm, and the second region consisting of crystal grains with a crystal grain size of 0.8 μm or more were calculated as a ratio to the total area of ​​the crystal grains sampled for particle size measurement. In addition, using the measured data of the crystal grain size distribution, the area-average diameter of the sampled crystal grains (a value obtained by weighting the particle diameter of each crystal grain by the equivalent circle particle area on the image, summing the weighted value, and dividing the sum by the total area of ​​the sampled crystal grains) was calculated. In addition, for the second test piece, the average Y of the first region was measured by the above-mentioned method using EPMA. 2 O 3 Concentration CM1 and average Y of the second region 2 O 3 The concentrations CM2 and CM2 were measured, and the value of ΔCM / CM2 was calculated.

[0080] Next, both sides of the first test piece were ground to a thickness of 0.5 mm, and then mirror-polished using diamond abrasive grains. Using this test piece, a commercially available ultraviolet-visible spectrophotometer (Japan Spectroscopy: V-780) was used to measure the total light transmittance using CIE standard illuminant D65 in the visible light wavelength range of 380 nm to 780 nm. In addition, using one of the mirror-polished surfaces of the first test piece, a commercially available Vickers hardness tester was used to measure the Vickers hardness and fracture toughness at a load of 49 N. The Vickers hardness and fracture toughness were measured at 12 different positions per sample, and the maximum and minimum measured values ​​were excluded and averaged.

[0081] The remaining two sintered bodies were machined into 3 mm x 4 mm x 40 mm bending test pieces and subjected to a bending strength test by three-point bending. The bending strength was measured at 10 points per sample, and the maximum and minimum measured values ​​were excluded to calculate the average value. The results are shown in Table 2 (in the table, * indicates that the value is outside the scope of the embodiment (present invention)).

[0082]

[0083] For test pieces Nos. 1 to 19 in which the area ratio of the first region and the area ratio of the second region are within the ranges described in the claims of the present invention and the value of ΔCM / CM2 is 0.3 or more, the fracture toughness value is 4.5 MPa m 0.5 12MPa・m or more 0.5 It can be seen that the total light transmittance is as high as 40% or more. 2 O 3 Of the test samples with a concentration of 5.5 mol%, number 20 has an area ratio of the first region that is equal to or less than the lower limit of the range of the present invention, and an area ratio of the second region that exceeds the upper limit of the range of the present invention. Also, number 21 has an area ratio of the first region that is less than the lower limit of the range of the present invention, and an area ratio of the second region that exceeds the upper limit of the range of the present invention. It can be seen that the total light transmittance of these test samples is good, but the fracture toughness remains low. Also, Y 2 O 3 Test piece No. 23, with a concentration of 2 mol%, had significant cracks in the sintered body, and evaluation was abandoned. A comparison of the results of No. 10 (Example) and No. 22 (Comparative Example) has already been described in detail, so a detailed explanation is omitted here.

[0084] Figures 16 and 17 show electron microscope images of test samples Nos. 1 and 3, and Figures 18 and 19 are histograms showing the results of measuring the crystal grain size distribution of those test samples. Figures 20 and 21 show electron microscope images of test samples Nos. 5 and 7, and Figures 22 and 23 are histograms showing the results of measuring the crystal grain size distribution of those test samples. Furthermore, Figures 24 and 25 show electron microscope images of test samples Nos. 13 and 15, and Figures 26 and 27 are histograms showing the results of measuring the crystal grain size distribution of those test samples.

[0085] Each Y 2 O 3 The concentrations are 3 mol%, 4 mol%, and 5 mol%, and numbers 1, 5, and 13 are La 2 O 3 Concentration is 0 mol%, numbers 3, 7, and 15 are La 2 O 3 The concentrations are 0 and 4 mol%. From the comparison of these results, when compared at the same baking temperature, Y 2 O 3 The higher the concentration, the easier it is for grain growth to proceed, and 2 O 3 It can be seen that there is a tendency for grain growth to proceed more easily in the case of the alloy containing the additives compared to the case of the alloy not containing the additives.

[0086] Of the test sample compositions Nos. 1 to 21 in Table 3, except for Nos. 3 and 4, the same raw material powder was used. 2 O 3 and La 2 O 3 Several raw material powders (numbers 45 to 47) with different compositions and concentrations were added, and the mixtures were fired at slightly lower temperatures of 1425°C to 1475°C, and the resulting test products were evaluated in the same manner. The results are shown in Table 4.

[0087]

[0088] It can be seen that by slightly lowering the firing temperature, the area ratio of the first region increases compared to the 1500°C fired product in Table 3, and the fracture toughness value is better. In addition, in the case of Y, where the area ratio of the first region is insufficient at 1500°C, the fracture toughness value is outside the range of the present invention. 2 O 3 For the two test samples with a concentration of 5.5 mol% (Nos. 43 and 44: corresponding to Nos. 20 and 21 in Table 3), La 2 O 3 It can be seen that the fracture toughness values ​​of the test piece No. 45, in which the concentration was increased to 0.8 mol%, also fell within the range of the present invention. 2 O 3 In the test sample 46 in which the concentration was set to 3 mol% and the firing temperature was lowered to 1425°C, the area ratio and area average diameter of the second regions were both below the lower limit values ​​of the present invention, and it was found that the total light transmittance was not sufficient. 2 O 3 In the test piece No. 47, in which the concentration exceeds the upper limit of the present invention, the area ratio of the first region is insufficient, and the fracture toughness value is insufficient.

[0089] Next, among the test sample compositions numbered 1 to 21 in Table 3, Y 2 O 3 The concentration was set to 3, 4, and 5 mol%, and La 2 O 3 For six samples with a concentration of 0 or 0.4 mol%, ZrO 2 A part of the 2 O 3 (Nos. 51 to 56), and 0.05 mol% TiO 2 The raw material powders substituted with (numbers 57 to 62) were used and fired at 1500° C., and the obtained test pieces were evaluated in the same manner. The results are shown in Table 5.

[0090]

[0091] The evaluation results for these test products were almost the same as those for the corresponding compositions in Table 1. 2 O 3 and TiO 2 It can be seen that there is no adverse effect due to the addition.

[0092] Regarding the above results, the area ratio of the first region in the sintered compact structure is S1, and the average Y of the first region is 2 O 3 The concentration is CM1, and the value PT calculated by PT (%) = S1 × {(7.4 - CM1) / 6} × 100 (A) is used. The area ratio of the second region in the sintered compact structure is S2, and the average Y of the second region is used. 2 O 3 The values ​​of SC calculated by the following formula, where CM2 is the concentration, are shown in Tables 3 to 5. In both formulas A and B, the value of "6" in the denominator corresponds to the ZrO concentration at 800°C where atomic diffusion slows to some extent in the equilibrium diagram of FIG. 2 Y for 2 O 3 Point A (Y 2 O 3 Concentration: about 1.4 mol%) and Y 2 O 3 ZrO 2 Point B (Y 2 O 3 The concentration (approximately 7.4 mol%) is shown as the distance from the equilibrium point. In FIG. 15, when the given composition point is O, the abundance ratio of the C phase in the phase equilibrium state can be expressed by AO / AB, and the abundance ratio of the T phase can be expressed by BO / AB. Therefore, the right side of formula (A) gives the upper limit of the area fraction of the T phase in the first region expected in the equilibrium state, and the right side of formula (B) gives the upper limit of the area fraction of the C phase in the second region expected in the equilibrium state. PT is named the converted tetragonal area fraction, and SC is named the converted cubic area fraction. These values ​​do not directly represent the amount of T phase or C phase actually present in the zirconia sintered body. However, it is expected from the theory of phase equilibrium that the larger the PT value, the larger the area fraction of the actual tetragonal crystals, and the larger the SC value, the larger the area fraction of the actual cubic crystals.

[0093] The fracture toughness values ​​(KIC) in Tables 3 and 4 are plotted against the PT values ​​in Figure 28. The white plotted points in the figure represent La. 2 O 3The black plotted points are the data for the unadded test sample. 2 O 3 The data for the test products added are shown below (the shape of the black plotted points indicates La 2 O 3 The values ​​are displayed differently depending on the amount of La added. 2 O 3 Regardless of the addition of , the fracture toughness value increases almost linearly with the value of PT, clearly demonstrating that the above inference is not incorrect. From this result, for example, when the converted tetragonal crystal area fraction PT (%) in the first region is 7% or more and 32% or less, the fracture toughness value measured by the IF method is 5.5 MPa m 0.5 10MPa・m or more 0.5 It can be seen that the converted tetragonal crystal area ratio PT can be satisfactorily secured within the range below. 2 O 3 It is preferable that the content of is 3.7 mol % or more and 5.3 mol % or less, and the area ratio of the first region in the sintered body structure is 10% or more and 45% or less.

[0094] Next, the total light transmittance in Tables 3 and 4 is plotted against the SC value, and the results are shown in FIG. 29. The white plotted points in the figure are La 2 O 3 The black plotted points are the data for the unadded test sample. 2 O 3 The data for the test products added are shown below (the shape of the black plotted points indicates La 2 O 3 The total light transmittance tends to increase monotonically as the value of PT increases. 2 O 3 The increase in the amount of La varies depending on the amount of La added. 2 O 3 The data points for the total light transmittance of the added test specimen are La 2 O 3 It can be seen that the data points for the total light transmittance of the test sample without additives are almost always on the larger side. 2 O 3 The results of logarithmic regression analysis for each added amount are added to the figure.2 O 3 The dotted line indicates the amount of La 2 O 3 The logarithmic regression curves for the addition amounts of 0.4 mol% and 0.8 mol% are shown (La 2 O 3 The curves for the amounts of addition of 0.4 mol% and 0.8 mol% are almost overlapping.) According to this result, 2 O 3 Up to an addition amount of about 0.4 mol% to 0.6 mol%, the total light transmittance of the sintered body tends to increase, and 2 O 3 It can be seen that the improvement in total light transmittance reaches a plateau depending on the amount of addition. 2 O 3 When adding ZrO, the balance 2 A part of the sintered body is made to have a La content of 0.1 mol % or more and 0.8 mol % or less in the total composition of the sintered body. 2 O 3 It is recommended that the

[0095] From this result, it can be seen that, for example, when the converted cubic area fraction SC (%) in the second region is 15% or more and 45% or less, the total light transmittance value measured in the visible light wavelength range of 380 nm to 780 nm using CIE standard illuminant D65 for a test piece of zirconia sintered body processed to a thickness of 0.5 mm can be satisfactorily secured in the range of 45% or more. 2 O 3 It is preferable that the content of is 3.7 mol % or more and 5.3 mol % or less, and the area ratio of the second region in the sintered body structure is 20% or more and 50% or less.

[0096] When preparing the raw material powder, the 15 kg of 3 mm diameter zirconia media was replaced with a mixture of 11.6 kg of 3 mm diameter zirconia media and 3.4 kg of 2 mm diameter zirconia media, and the same grinding was carried out using the same pot as above with 1 kg of raw material and 1.5 kg of pure water. For both raw material compositions, raw material powders with approximately the same particle size distribution were obtained in a grinding time that was 50 to 60% shorter than when 3 mm diameter zirconia media was used. These raw material powders were then fired under the same conditions as above, yielding sintered bodies with approximately the same properties.

Claims

1. Y in the overall composition of the sintered body 2 O 3 The content of is 2.5 mol % or more and 6 mol % or less, and the balance is ZrO 2 and unavoidable impurities and has a relative density of 99% or more, wherein in an electron microscope image of the sintered body structure, the area average grain size of the zirconia crystal grains is 0.4 μm or more and 0.9 μm or less, the area ratios of the zirconia crystal grains having a grain size of less than 0.1 μm and the zirconia crystal grains having a grain size of more than 2 μm are both less than 1%, the area ratio of a first region consisting of zirconia crystal grains having a grain size of 0.1 μm or more and less than 0.5 μm is 5% or more and 80% or less, the area ratio of a second region consisting of zirconia crystal grains having a grain size of 0.8 μm or more and less than 2 μm is 5% or more and 80% or less, the area ratio of a third region consisting of zirconia crystal grains having a grain size of 0.5 μm or more and less than 0.8 μm is 10% or more and less than 55%, and the average Y of the zirconia crystal grains constituting the second region is 0.02 to 0.04 μm. 2 O 3 The concentration C2 is 3.5 mol % or more and 7.0 mol % or less, and the average Y 2 O 3 The concentration C1 is 1.7 mol% or more and 5 mol% or less, and 2 O 3 The difference in concentration is ΔC≡C2-C1, the value of ΔC / C2 is 0.2 or more and 0.5 or less, and the fracture toughness value measured by the IF method is 4.5 MPa m 0.5 12MPa・m or more 0.5 A zirconia sintered body characterized by the following:

2. The remainder being ZrO 2 A part of the sintered body has a La content of 0.1 mol % or more and 1 mol % or less in the total composition of the sintered body. 2 O 3 The zirconia sintered body according to claim 1, wherein the zirconia sintered body is substituted with 3. The remainder is ZrO 2 A part of the sintered body has an Al content of 0.2 mol% or less in the total composition of the sintered body. 2 O 3 The zirconia sintered body according to claim 1, wherein the zirconia sintered body is substituted with 4. The remainder being ZrO 2 A part of the sintered body has a TiO content of 0.1 mol% or less in the total composition of the sintered body. 2 The zirconia sintered body according to claim 1, wherein the zirconia sintered body is substituted with 5. The zirconia sintered body according to claim 1, having a Vickers hardness Hv of 1,150 or more.

6. The zirconia sintered body according to claim 1, wherein the total light transmittance measured on a test piece processed to a thickness of 0.5 mm using CIE standard light D65 in the visible light wavelength range of 380 nm to 780 nm is 40% to 60%.

7. The area ratio of the first region in the sintered body structure is S1, and the average Y of the first region is 2 O 3 The zirconia sintered body according to claim 1, wherein the converted tetragonal area ratio PT (%) in the first region is calculated as PT = S1 × {(7.4 - CM1) / 6} × 100, where CM1 is the concentration, and is 3% or more and 60% or less.

8. The area ratio of the first region in the sintered body structure is S1, the area ratio of the second region in the sintered body structure is S2, and the average Y of the second region is 2 O 3 The zirconia sintered body according to claim 1, wherein the converted cubic crystal area ratio SC (%) in the second region is calculated as SC = S1 × {(CM2-1.4) / 6} × 100, where CM2 is the concentration, and is 4% or more and 70% or less.

9. In the sintered body structure, the zirconia crystal grains forming the second region have Y at the center of the zirconia crystal grains. 2 O 3 The outer periphery of Y is more sensitive than the density. 2 O 3 The zirconia sintered body according to claim 1, wherein the concentration is low.

10. The sintered body structure has an area ratio of the second region of 15% or more and 50% or less, and has a rock garden-like structure in which the zirconia crystal particles belonging to the second region are dispersed as coarse dispersed particles against a background region consisting of zirconia crystal particles belonging to the first region and zirconia crystal particles belonging to the second region, and has a Y-shaped structure along an analysis line that crosses the background region and a plurality of the coarse dispersed particles. 2 O 3 When the concentration is measured, a maximum point is shown in each of the coarse dispersed particles, and a minimum point is shown in the background region, so that Y is continuously 2 O 3 The zirconia sintered body according to claim 9, which exhibits a concentration profile in which the concentration changes in a wave shape.

11. Y 2 O 3 the area ratio of the first region in the sintered body structure is 10% or more and 45% or less, the area ratio of the first region in the sintered body structure is S1, the average Y of the first region is 2 O 3 The converted tetragonal area ratio PT (%) in the first region is 7% or more and 32% or less, and is calculated as PT = S1 × {(7.4 - CM1) / 6} × 100, where CM1 is the concentration. The fracture toughness value measured by the IF method is 5.5 MPa m 0.5 10MPa・m or more 0.5 The zirconia sintered body according to claim 1, wherein:

12. Y 2 O 3 the area ratio of the first region in the sintered body structure is S1, the area ratio of the second region in the sintered body structure is S2, and the average Y of the second region is 2 O 3 The zirconia sintered body according to claim 1, wherein the converted cubic crystal area ratio SC (%) in the second region is 15% to 45% and is calculated as follows: SC = S1 × {(CM2-1.4) / 6} × 100, where CM2 is the concentration. A test piece of the zirconia sintered body processed to a thickness of 0.5 mm has a total light transmittance of 45% or more, measured in a visible light wavelength range of 380 nm to 780 nm using CIE standard light D65.

13. The remainder being ZrO 2 A part of the sintered body has a La content of 0.1 mol % or more and 0.8 mol % or less in the total composition of the sintered body. 2 O 3 The zirconia sintered body according to claim 11, wherein the total light transmittance is 50% or more.

Citation Information

Patent Citations

  • Translucent yttria-containing zirconia sintered compact, manufacturing method and utilization of the same

    JP2008222450A

  • Light-transmitting zirconia sintered compact, method for producing the same and use thereof

    JP2010150063A

  • Zirconia sintered body, and composition and calcined body of zirconia

    JP2018165243A

  • Sintered body and manufacturing method thereof

    JP2022008052A

  • Translucent zirconia sintered compact and production method therefor, and application thereof

    JP2017214266A

Cited By

  • Compositions comprising bacterial strains

    CN108883139A

  • Zirconia sintered body

    WO2026088915A1

  • Zirconia sintered body

    WO2026088916A1