Thermally-expandable composition and thermally-expandable fire-resistant sheet
The thermally expandable composition with a matrix component and thermally expandable graphite addresses the issue of warping fireproof materials by forming a strong, deformable insulation layer, ensuring effective fire resistance during equipment warping.
Patent Information
- Application Number
- PCT/JP2024/016094
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-22
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Fireproof materials used in construction for doors and windows face warping and deformation during high-temperature fires, leading to increased fire spread due to temperature differences between heated and non-heated surfaces.
A thermally expandable composition containing a matrix component, such as dry-setting, chemically reactive, or hot-melt adhesives, combined with thermally expandable graphite, which forms a fireproof sheet that expands to maintain fire resistance even if equipment warps, using a specific adhesive to ensure strong bonding and follow warpage.
The thermally expandable fireproof sheet effectively maintains good fire resistance by forming a strong insulation layer that is less susceptible to deformation, preventing fire spread and maintaining performance over time.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Thermally expandable composition and thermally expandable fire-resistant sheet
[0001] The present invention relates to a thermally expandable composition and a thermally expandable fire-resistant sheet.
[0002] In the construction industry, fire-resistant materials are used in fire prevention equipment such as doors and windows. Examples of fire-resistant materials include fire-resistant sheets containing resins blended with inorganic fillers and thermally expandable graphite (see, for example, Patent Document 1). Such fire-resistant sheets expand when heated, and combustion residues form a fire-resistant insulating layer, thereby achieving fire-resistant and insulating performance. Specifically, fire-resistant sheets are installed in gaps between doors and windows and the surrounding frames, such as door frames and window frames. In the event of a fire, the sheets expand in their thickness direction to close the gap and prevent the fire from spreading.
[0003] Japanese Patent Application Laid-Open No. 2017-141463
[0004] When fire prevention equipment such as doors and windows are exposed to high temperatures for a long period of time during a fire, a temperature difference occurs between the heated and unheated surfaces, causing deformation due to warping, and this warping can cause the previously closed heated and unheated surfaces to penetrate, expanding the spread of fire. Therefore, an object of the present invention is to provide a thermally expandable composition and a thermally expandable fire-resistant sheet that can maintain good fire resistance even when warping occurs in fire prevention equipment during a fire.
[0005] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a thermally expandable composition containing a matrix component and thermally expandable graphite, wherein the matrix component is at least one adhesive selected from the group consisting of a dry-to-solidify adhesive, a chemical reaction adhesive, and a hot-melt adhesive, and have completed the present invention. That is, the present invention provides the following [1] to
[13] .
[0006] [1] A thermally expandable composition containing a matrix component and thermally expandable graphite, wherein the matrix component is at least one adhesive selected from the group consisting of a dry-and-solidify adhesive, a chemical reaction adhesive, and a hot-melt adhesive. [2] The thermally expandable composition according to [1] above, further containing an inorganic filler, wherein the content of the thermally expandable graphite is 3 to 300 parts by mass and the content of the inorganic filler is 2 to 200 parts by mass per 100 parts by mass of the matrix component, and the expansion initiation temperature of the thermally expandable graphite is lower than the decomposition initiation temperature of the matrix component. [3] The thermally expandable composition according to [1] or [2] above, wherein the matrix component contains at least one adhesive selected from the group consisting of NBR epoxy resins, urea resins, melamine resins, phenolic resins, rubbers, vinyl acetate resins, vinyl acetate copolymer resins, ethylene-vinyl acetate copolymer resins, acrylic resins, aqueous polymer-isocyanate resins, synthetic rubber latexes, epoxy resins (unmodified), cyanoacrylates, polyurethanes, silicone resins (unmodified), modified silicone resins, silylated urethanes, polystyrenes, and polyesters. [4] A thermally expandable fire-resistant sheet molded from the thermally expandable composition according to any one of [1] to [3] above. [5] The thermally expandable fire-resistant sheet according to [4] above, which has an expansion initiation temperature of 160°C or lower. [6] The thermally expandable fire-resistant sheet according to [4] or [5] above, which has an elution rate of 3% or lower after immersion in pure water at 60°C for one week. [7] The heat-expandable fire-resistant sheet according to any one of [4] to [6] above, wherein the matrix component does not contain a phosphorus component. [8] The heat-expandable fire-resistant sheet according to any one of [4] to [7] above, wherein the matrix component does not contain a phosphorus component. [9] The heat-expandable fire-resistant sheet according to any one of [4] to [8] above, wherein the heat-expandable fire-resistant sheet is a rolled body having a length of 1 m or more.
[10] The heat-expandable fire-resistant sheet according to any one of [4] to [9] above, wherein the length is 1 m or more, the thermal shrinkage rate is 1% or less in both the MD and TD directions, the thickness is 0.5 mm or more, and the thickness variation is 0.1 mm or less.
[11] A method for producing a thermally expandable fire-resistant sheet, comprising solidifying, drying, or curing the thermally expandable composition according to any one of [1] to [3] above to obtain a roll having a length of 1 m or more.
[12] A method for producing a thermally expandable material-containing member, comprising applying the thermally expandable composition according to any one of [1] to [3] above to a member and solidifying, drying, or curing the composition to obtain a thermally expandable material-containing member.
[13] Fire protection equipment, at least a part of which is equipped with the thermally expandable fire-resistant sheet according to any one of [4] to
[10] above.
[0007] According to the present invention, it is possible to provide a thermally expandable composition and a thermally expandable fire-resistant sheet that can maintain good fire resistance even if warping occurs in fire prevention equipment during a fire.
[0008] The present invention will be described in detail below. [Thermal Expandable Composition] The thermal expandable composition of the present invention contains a matrix component and thermally expandable graphite, and the matrix component is at least one adhesive selected from the group consisting of a dry-and-solidify adhesive, a chemically reactive adhesive, and a hot-melt adhesive. The thermal expandable composition and the thermally expandable fire-resistant sheet formed therefrom can maintain good fire resistance even when warping of fire-resistant equipment occurs during a fire. The reason for this is unclear, but is presumed to be as follows. The thermally expandable composition and the thermally expandable fire-resistant sheet of the present invention contain a specific adhesive, which allows the thermally expandable graphite to be firmly bonded. More specifically, during a fire, the strength between the thermally expandable graphite in the fire-resistant insulation layer formed by the expansion of the thermally expandable fire-resistant sheet is increased, allowing the fire-resistant insulation layer to follow deformation due to warping of various fire-resistant equipment, thereby maintaining good fire resistance.
[0009] <Matrix Component> The thermally expandable composition of the present invention contains a matrix component. Thermally expandable graphite, which will be described later, and an inorganic filler, if necessary, are dispersed in the matrix component. The matrix component in the thermally conductive composition is an adhesive component and a resin component having various structures. The matrix component also serves as the matrix in the thermally expandable fire-resistant sheet formed from the thermally expandable composition. The matrix component is at least one adhesive selected from the group consisting of a dry-solidifying adhesive, a chemically reactive adhesive, and a hot-melt adhesive. The adhesive has high adhesive strength to the thermally expandable graphite and can easily follow the warping of various fire prevention equipment in the event of a fire. The matrix component may consist of a single adhesive, or a combination of multiple adhesives.
[0010] (Dry-Solidifying Adhesive) Examples of dry-solidifying adhesives include solvent-based adhesives, emulsion-based adhesives, and synthetic rubber latex-based adhesives. When using these adhesives, the thermally expandable composition becomes liquid, which makes it easier to increase the content of thermally expandable graphite and also makes it easier to cover the thermally expandable graphite in the solidified sheet with adhesive. As a result, the fire-resistant heat-insulating layer, which is the expansion residue of the thermally expandable fire-resistant sheet, can more easily follow the warping of various fire prevention equipment.
[0011] A solvent-based adhesive is dissolved in an organic solvent in a thermally expandable composition. Therefore, when such a solvent-based adhesive is used, the thermally expandable composition contains an organic solvent. Furthermore, solidification is possible by volatilizing the organic solvent. Examples of solvent-based adhesives include vinyl acetate resins, vinyl acetate copolymer resins, rubbers, acrylic resins, polyesters, and silicone resins. The silicone resin adhesive is an unmodified silicone resin adhesive. In this specification, examples of vinyl acetate copolymer resins include copolymers of vinyl acetate and monomers copolymerizable with vinyl acetate (e.g., α-olefins, (meth)acrylic acid esters, etc.), such as vinyl acetate-(meth)acrylic acid ester copolymers. The term (meth)acrylic acid encompasses both acrylic acid and methacrylic acid, and the same applies to other similar terms. In this specification, examples of rubber-based adhesives include chloroprene, butadiene, styrene-butadiene, butadiene-acrylonitrile, isobutylene-isoprene, and ethylene-propylene, with chloroprene being preferred. Of solvent-based adhesives, polyester-based, acrylic resin-based, and silicone resin-based (unmodified) adhesives are preferred.
[0012] The emulsion-type adhesive is dispersed in a dispersant, preferably water, in the thermally expandable composition. When an emulsion-type adhesive is used, the thermally expandable composition contains a dispersant such as water. Examples of emulsion-type adhesives include vinyl acetate resin-based, vinyl acetate copolymer resin-based, acrylic resin-based, aqueous polymer-isocyanate-based, and polyurethane-based adhesives, with vinyl acetate copolymer resin-based and polyurethane-based adhesives being preferred.
[0013] In the thermally expandable composition, the synthetic rubber latex adhesive is dispersed in a dispersion medium, preferably water. When a synthetic rubber latex adhesive is used, the thermally expandable composition contains a dispersion medium such as water. Examples of synthetic rubber latex adhesives include chloroprene, butadiene, styrene-butadiene, butadiene-acrylonitrile, isobutylene-isoprene, and ethylene-propylene, with chloroprene being preferred.
[0014] When a dry-to-set adhesive is used, the thermally expandable composition contains water or an organic solvent. When a dry-to-set adhesive is used, the solid content of the thermally expandable composition is, for example, 10 to 90 mass %, and preferably 30 to 70 mass %, from the viewpoint of improving the fire resistance of the resulting thermally expandable fire-resistant sheet.
[0015] (Chemical Reaction Type Adhesive) Examples of chemical reaction type adhesives include a curing agent reaction type, a moisture curing reaction type, and an ultraviolet reaction type.
[0016] <Curing Agent Reaction Type> A curing agent reaction type adhesive is an adhesive that can be cured by a curing agent, and examples thereof include epoxy resin-based (unmodified), rubber-modified epoxy resin-based, melamine resin-based, urea resin-based, and phenolic resin-based adhesives. The epoxy resin-based (unmodified) refers to an epoxy resin other than a modified epoxy resin, and the rubber-modified epoxy resin-based adhesive is a reaction product of an epoxy resin and rubber, such as an NBR epoxy resin-based adhesive obtained by reacting an epoxy resin with acrylonitrile butadiene rubber (NBR). As the curing agent, any commonly used curing agent capable of curing the resins exemplified above can be used without particular limitation, and examples thereof include polyamine-based, imidazole-based, polymercaptan-based, and acid anhydride-based curing agents.
[0017] <Moisture-Curing Reaction Type> A moisture-curing reaction type adhesive is an adhesive that cures with moisture in the air. A thermally expandable composition containing a moisture-curing reaction type adhesive can be cured with moisture and can be kneaded at low temperatures, which particularly reduces the load during kneading and effectively suppresses deterioration of the thermally expandable graphite. As a result, gas generation due to deterioration of the thermally expandable graphite is suppressed, and a long thermally expandable fire-resistant sheet with an extremely good appearance can be obtained.
[0018] Examples of moisture-curing reaction adhesives include cyanoacrylate-based, modified silicone resin-based, and silylated urethane-based adhesives, with modified silicone resin-based and silylated urethane-based adhesives being preferred, and modified silicone resin-based adhesives being more preferred.
[0019] (Modified silicone resin system) Examples of the modified silicone resin moisture-curing reaction adhesive include polymers having crosslinkable silyl groups (crosslinkable silyl group-containing polymers). As the crosslinkable silyl group-containing polymer, at least one selected from crosslinkable silyl group-containing polyoxyalkylene polymers, crosslinkable silyl group-containing acrylic polymers, and crosslinkable silyl group-containing acrylic-modified polyoxyalkylene polymers is preferred. Note that the modified silicone resin moisture-curing reaction adhesive is a compound that does not have a urethane bond or a urea bond in the main chain, unlike the silylated urethane system described below.
[0020] The crosslinkable silyl group-containing polyoxyalkylene polymer is preferably a polymer containing a crosslinkable silyl group in the molecule and having a polyoxyalkylene in the main chain, more preferably a polymer having a polyoxyalkylene in the main chain and a crosslinkable silyl group at the main chain terminal. The polyoxyalkylene is preferably polyoxypropylene.
[0021] The crosslinkable silyl group-containing acrylic-modified polyoxyalkylene polymer is preferably a polymer containing a crosslinkable silyl group in the molecule and having a (meth)acrylic-modified polyoxyalkylene in the main chain, more preferably a polymer having a (meth)acrylic-modified polyoxyalkylene in the main chain and having a crosslinkable silyl group at the main chain terminal. The (meth)acrylic-modified polyoxyalkylene is preferably a (meth)acrylic-modified polyoxypropylene.
[0022] The crosslinkable silyl group-containing acrylic polymer may be a polymer having an acrylic polymer in the main chain skeleton and having one or more crosslinkable silyl groups in the molecule. Here, the acrylic polymer may be a conventionally known one, and is not particularly limited as long as it is an acrylic polymer obtained by polymerizing or copolymerizing one or more acrylic monomers selected from (meth)acrylic acid, (meth)acrylic acid ester, (meth)acrylonitrile, (meth)acrylamide, etc.
[0023] Examples of crosslinkable silyl groups include groups in which one or more reactive groups are bonded to a silicon atom.The reactive groups are selected from halogen atoms, hydrogen atoms, hydroxyl groups, alkoxy groups, acyloxy groups, ketoximate groups, amide groups, acid amide groups, mercapto groups, ketoxime groups, alkenyloxy groups, and aminooxy groups, and when there are multiple reactive groups, the reactive groups may be the same or different groups.Among these, the reactive group is preferably an alkoxy group, and more preferably a methoxy group.That is, the crosslinkable silyl group is preferably an alkoxysilyl group.Examples of alkoxysilyl groups include trialkoxysilyl groups such as trimethoxysilyl groups, triethoxysilyl groups, triisopropoxysilyl groups, and triphenoxysilyl groups, dialkoxysilyl groups such as dimethoxymethylsilyl groups and diethoxymethylsilyl groups, and monoalkoxysilyl groups such as methoxydimethylsilyl groups and ethoxydimethylsilyl groups. Among these, a trialkoxysilyl group or a dialkoxysilyl group is preferred, and a trimethoxysilyl group or a dimethoxymethylsilyl group is more preferred.
[0024] (Silylated urethane-based) A silylated urethane-based moisture-curing reaction adhesive is a polymer having at least one of a urethane bond and a urea bond in the main chain and having a crosslinkable silyl group. The crosslinkable silyl group is preferably present at the end of the main chain. The crosslinkable silyl group is the same as that described for the modified silicone resin-based moisture-curing reaction adhesive described above. Furthermore, the main chain of the silylated urethane-based moisture-curing reaction adhesive preferably has a polyoxyalkylene in the skeleton and at least one of a urethane bond and a urea bond. The polyoxyalkylene is preferably polyoxypropylene.
[0025] (Curing Catalyst) The moisture-curing reaction adhesive is preferably cured using a curing catalyst. Examples of the curing catalyst include dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin laurate) oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), bis(dibutyltin bistriethoxysilicate) oxide, dibutyltin oxybisethoxysilicate, and organic tin compounds such as 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, and organic titanium compounds such as tetra-n-butoxytitanate and tetraisopropoxytitanate. These curing catalysts may be used alone or in combination of two or more. The content of the curing catalyst is preferably 1 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the matrix component.
[0026] <Ultraviolet Reaction Type> Ultraviolet reaction type adhesives are adhesives that cure when irradiated with ultraviolet light, and examples thereof include radical polymerization curing adhesives and cationic polymerization adhesives. Examples of radical polymerization curing adhesives include compounds having a polymerizable double bond such as a (meth)acryloyl group and a vinyl group. Examples of cationic polymerization curing adhesives include compounds having an epoxy group and compounds having an oxetanyl group. Ultraviolet reaction type adhesives can be used in combination with a polymerization initiator, if necessary.
[0027] (Hot-melt adhesive) A hot-melt adhesive is an adhesive that has no fluidity at room temperature but becomes fluid when heated, and is sometimes called a hot-melt adhesive. Furthermore, a heated hot-melt adhesive solidifies when cooled again. By using a hot-melt adhesive in a thermally expandable composition, even if the fire prevention equipment warps during a fire, the fluidity of the hot-melt adhesive increases, making it easier to fill gaps and improve fire resistance. Examples of hot-melt adhesives include vinyl acetate resins, vinyl acetate copolymer resins, ethylene-vinyl acetate copolymer resins, rubbers, acrylic resins, polyurethanes, polystyrenes, polyolefins, polyesters, and polyamides. The polystyrene-based adhesives are polymers containing styrene-based monomers and may be copolymers of styrene-based monomers and aliphatic monomers. Among these, ethylene-vinyl acetate copolymer resins, polyurethanes, polyesters, and polystyrenes are preferred. When using a hot-melt adhesive, a tackifying resin may be used in combination. Examples of tackifying resins include rosin-based, terpene-based, petroleum resin-based, and coumarone resin-based resins.
[0028] The thermally expandable composition of the present invention may be any of a dry-setting adhesive, a chemical reaction adhesive, and a hot-melt adhesive, but from the viewpoint of improving the ability to follow the warping of fire prevention equipment during a fire, a dry-setting adhesive or a hot-melt adhesive is preferred. The type of adhesive is not particularly limited, but is preferably at least one selected from the group consisting of NBR epoxy resins, urea resins, melamine resins, phenolic resins, rubbers, vinyl acetate resins, vinyl acetate copolymer resins, ethylene-vinyl acetate copolymer resins, acrylic resins, aqueous polymer-isocyanate resins, synthetic rubber latexes, epoxy resins, cyanoacrylates, polyurethanes, acrylic resins, silicone resins (unmodified), modified silicone resins, silylated urethanes, polystyrenes, and polyesters.
[0029] In the present invention, the content of the matrix component is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, based on the total solid content of the thermally expandable composition, from the viewpoint of improving fire resistance.
[0030] <Thermal Expandable Graphite> The thermal expandable composition of the present invention contains thermal expandable graphite. Thermal expandable graphite is a conventionally known substance that expands when heated. When heated, it expands to form large-volume voids, thereby suppressing the spread of fire and extinguishing the fire when the fire-resistant sheet catches fire. Thermal expandable graphite is produced by treating powder of natural flaky graphite, pyrolytic graphite, kish graphite, or the like with an inorganic acid and a strong oxidizing agent to produce a graphite intercalation compound. This is a type of crystalline compound that maintains the layered structure of carbon. Examples of inorganic acids include concentrated sulfuric acid, nitric acid, and selenic acid. Examples of strong oxidizing agents include concentrated nitric acid, persulfates, perchloric acid, perchlorates, permanganates, dichromates, dichromates, and hydrogen peroxide. The thermal expandable graphite obtained by the acid treatment described above may be further neutralized with ammonia, aliphatic lower amines, alkali metal compounds, alkaline earth metal compounds, or the like.
[0031] The particle size of the thermally expandable graphite is preferably 20 to 200 mesh. When the particle size of the thermally expandable graphite is within this range, it expands to easily create large-volume voids, thereby improving fire resistance. It also improves dispersibility in resins. The average aspect ratio of the thermally expandable graphite is preferably 2 or more, more preferably 5 or more, and even more preferably 10 or more. There is no particular upper limit to the average aspect ratio of the thermally expandable graphite, but from the viewpoint of preventing cracking of the thermally expandable graphite, it is preferably 1,000 or less. When the average aspect ratio of the thermally expandable graphite is 2 or more, it expands to easily create large-volume voids, thereby improving flame retardancy. The average aspect ratio of the thermally expandable graphite is determined by measuring the maximum dimension (major axis) and minimum dimension (minor axis) of each of 10 pieces of thermally expandable graphite, and then averaging the values obtained by dividing the maximum dimension (major axis) by the minimum dimension (minor axis). The major axis and minor axis of the thermally expandable graphite can be measured using, for example, a field emission scanning electron microscope (FE-SEM).
[0032] The expansion onset temperature of the thermally expandable graphite is not particularly limited, but is preferably 100 to 160°C, and more preferably 120 to 150°C. When the expansion onset temperature of the thermally expandable graphite is within the above range, it becomes easier to adjust the expansion onset temperatures of the thermally expandable composition and the thermally expandable fire-resistant sheet to, for example, 160°C or less, which makes it easier to expand at the early stage of a fire to form a fire-resistant heat insulating layer and maintain good fire resistance for a long period of time. The expansion onset temperature of the thermally expandable graphite is measured by the method described in the Examples.
[0033] The expansion start temperature of the thermally expandable graphite is preferably lower than the decomposition start temperature of the matrix component. This improves the expandability of the thermally expandable fire-resistant sheet and increases the mechanical strength of the formed fire-resistant heat insulating layer, thereby improving fire resistance. The expansion start temperature of the thermally expandable graphite is preferably at least 5°C lower than the decomposition start temperature of the matrix component, and more preferably at least 10°C lower. Here, the decomposition temperature of the matrix component means the decomposition start temperature of the adhesive that constitutes the matrix component, and in the case of a chemical reaction type adhesive, means the decomposition temperature of the adhesive after curing. The decomposition start temperature means the temperature at which the matrix component decomposes and weight loss begins, and is measured using a thermogravimetric analyzer in a dry air atmosphere at a heating rate of 10°C / min.
[0034] The content of thermally expandable graphite is preferably 3 to 300 parts by mass, more preferably 10 to 200 parts by mass, and even more preferably 30 to 100 parts by mass, per 100 parts by mass of the matrix component. When the content of thermally expandable graphite is equal to or greater than these lower limits, the thermally expandable fire-resistant sheet can be imparted with appropriate fire resistance. When the content of thermally expandable graphite is equal to or less than these upper limits, the matrix component can be contained in a certain amount or more, making it easier to cover the thermally expandable graphite with an adhesive and making it easier to follow the warping of the fire prevention equipment.
[0035] <Inorganic Filler> The thermally expandable composition of the present invention may contain an inorganic filler other than the thermally expandable graphite described above. The inorganic filler expands when heated, and when the fireproof heat insulating layer is formed, the inorganic filler increases the heat capacity and suppresses heat transfer, while acting as an aggregate to improve the strength of the expansion residue. The inorganic filler that can be used in the present invention is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite; metal carbonates such as calcium carbonate, zinc carbonate, strontium carbonate, and barium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, and hydrotalcite; calcium sulfate, gypsum fiber, calcium salts such as calcium silicate; silica, diatomaceous earth, dawsonite, barium sulfate, talc, clay, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, silica-based balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fiber, carbon balloons, various metal powders, metal phosphites, potassium titanate, magnesium sulfate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fiber, and zinc borate. The inorganic filler may be used alone or in combination of two or more. Among these, calcium carbonate, iron oxide, and aluminum hydroxide are preferred from the viewpoint of improving the fire resistance of the thermally expandable fire-resistant sheet, and a combination of calcium carbonate and iron oxide or a combination of calcium carbonate and aluminum hydroxide is preferred. The inorganic filler may be used alone or in combination of two or more. From the viewpoint of improving fire resistance, the content of the inorganic filler is preferably 2 to 200 parts by mass, more preferably 10 to 150 parts by mass, and even more preferably 30 to 100 parts by mass per 100 parts by mass of the matrix component.
[0036] <Plasticizer> The thermally expandable composition of the present invention may contain a plasticizer from the viewpoint of improving moldability. Examples of plasticizers include phthalate ester plasticizers such as di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diheptyl phthalate (DHP), and diisodecyl phthalate (DIDP); fatty acid ester plasticizers such as di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), and dibutyl adipate (DBA); epoxidized ester plasticizers such as epoxidized soybean oil; adipate ester plasticizers such as adipate esters and adipic acid polyesters; trimellitate ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM) and triisononyl trimellitate (TINTM); and process oils such as mineral oil. These plasticizers may be used alone or in combination of two or more. When the thermally expandable composition contains a plasticizer, the content of the plasticizer is preferably 1 to 60 parts by mass, more preferably 5 to 50 parts by mass, per 100 parts by mass of the matrix component.
[0037] (Other Components) The thermally expandable composition of the present invention may contain additional components other than those described above, as needed, as long as the object of the present invention is not impaired. The type of these additional components is not particularly limited, and various additives can be used. Examples of such additives include lubricants, anti-shrinkage agents, crystal nucleating agents, colorants (pigments, dyes, etc.), ultraviolet absorbers, antioxidants, antiaging agents, flame retardants, flame retardant assistants, antistatic agents, surfactants, vulcanizing agents, dispersants, and surface treatment agents. The amount of additive added can be appropriately selected within a range that does not impair moldability, etc., and the additives may be used alone or in combination of two or more.
[0038] The thermally expandable composition of the present invention can be prepared by mixing the matrix component, the thermally expandable graphite, and optionally the inorganic filler and other additives. Mixing can be carried out using a known device such as a Banbury mixer, a kneader mixer, a kneading roll, a Raikai mixer, or a planetary mixer.
[0039] [Thermal-Expandable Fire-Resistant Sheet] The thermal-expandable fire-resistant sheet of the present invention is made of the thermal-expandable composition described above and can be obtained by molding the thermal-expandable composition as described below. Therefore, the thermal-expandable fire-resistant sheet contains a matrix component, thermal-expandable graphite, and optionally an inorganic filler and other additives.
[0040] <Expansion Start Temperature> The heat-expandable fire-resistant sheet of the present invention preferably has an expansion start temperature of 160°C or lower. By having an expansion start temperature of 160°C or lower, the sheet expands in the early stages of a fire when temperatures are relatively low, forming a fire-resistant heat insulating layer, making it easier to maintain good fire resistance for a long period of time. The expansion start temperature of the heat-expandable fire-resistant sheet is preferably 155°C or lower, more preferably 150°C or lower, and preferably 120°C or higher. The expansion start temperature of the heat-expandable fire-resistant sheet is measured by the method described in the examples.
[0041] <Elution Rate> The heat-expandable fire-resistant sheet of the present invention preferably has an elution rate of 3% or less after immersion in pure water at 60°C for one week. An elution rate of 3% or less can suppress elution of the components constituting the heat-expandable fire-resistant sheet, preventing a decrease in fire resistance, even when the heat-expandable fire-resistant sheet is placed in a high-humidity environment or in contact with water. Furthermore, when the heat-expandable fire-resistant sheet is installed in a fire-prevention equipment, contamination of the fire-prevention equipment and poor appearance can be prevented. The elution rate of the heat-expandable fire-resistant sheet is preferably 2% or less, more preferably 1% or less. The lower the elution rate, the better, with the lower limit being 0%. The elution rate can be adjusted by appropriately selecting each component to be incorporated into the heat-expandable fire-resistant sheet. Specifically, compounds with low solubility in water can be used for the matrix component, heat-expandable graphite, optional inorganic filler, and other additives. The elution rate is measured by the method described in the examples.
[0042] <Phosphorus Component> The matrix component contained in the thermally expandable fire-resistant sheet of the present invention preferably does not contain a phosphorus component. By using a matrix component that does not contain a phosphorus component, the phosphorus content of the thermally expandable fire-resistant sheet can be reduced. Furthermore, it is also preferable that components other than the matrix component contained in the thermally expandable fire-resistant sheet also do not contain a phosphorus component. That is, the thermally expandable fire-resistant sheet preferably does not contain a phosphorus component. The matrix component and the thermally expandable fire-resistant sheet may contain an unavoidable amount of phosphorus as an impurity. That is, in this specification, "not containing a phosphorus component" means that the phosphorus content is 0.1% by mass or less, preferably 0.01% by mass or less. The absence of a phosphorus component improves water resistance, thereby ensuring excellent expansion ratio, residual hardness, and shape retention after expansion even after long-term exposure to water. Here, the phosphorus component refers to a compound containing a phosphorus atom. It is preferable that compounds containing a phosphorus atom are not used as the matrix component, thermally expandable graphite, and the inorganic filler and other additives that are optionally blended.
[0043] <Long Product> The heat-expandable fire-resistant sheet of the present invention preferably has a length of 1 m or more. The length is the length in the longitudinal direction (MD) of the heat-expandable fire-resistant sheet. A length of 1 m or more improves productivity and broadens the range of applications, which is preferable. The length of the heat-expandable fire-resistant sheet is preferably 5 m or more, more preferably 20 m or more, even more preferably 50 m or more, and even more preferably 100 m or more. Typically, the length of the heat-expandable fire-resistant sheet is 500 m or less. In this specification, the MD direction is an abbreviation for machine direction, which corresponds to the flow direction of the composition during application, etc., as described below, and is the longitudinal direction of the sheet. The TD direction is an abbreviation for transverse direction, which is a direction perpendicular to the MD direction.
[0044] Furthermore, the thermally expandable fire-resistant sheet of the present invention can reduce thickness variation even when the length is 1 m or more, making it possible to obtain long products with high dimensional accuracy. Since the present invention uses a specific matrix component, the kneading load when kneading the composition is small, which is thought to suppress deterioration of the thermally expandable graphite, thereby suppressing gas generation and reducing thickness variation. In particular, in the case of a liquid thermally expandable composition, it is easier to suppress deterioration of the thermally expandable graphite.
[0045] Specifically, the heat-expandable fire-resistant sheet of the present invention, due to its specific composition, can achieve a thickness of 0.5 mm or more and a thickness variation of 0.1 mm or less, even when the sheet is 1 m or longer. Here, a "thickness" of 0.5 mm or more refers to an average thickness, which is the average value obtained by measuring the thickness at 10 equally spaced points along the length of the heat-expandable fire-resistant sheet. The average thickness is preferably 0.8 mm or more, more preferably 1 mm or more, and preferably 5 mm or less. The thickness measurement is performed at the center of the sheet's width. Furthermore, the thickness variation refers to the average of the absolute values A of the differences between the thickness measured at each point and the average thickness measured at 10 equally spaced points along the length of the heat-expandable fire-resistant sheet, as described above. The thickness variation is preferably 0.1 mm or less, more preferably 0.08 mm or less, and even more preferably 0.05 mm or less. The thickness variation is preferably 10% or less of the thickness (average thickness), and more preferably 5% or less.
[0046] The heat-expandable fire-resistant sheet of the present invention preferably has a heat shrinkage rate of 1% or less in both the MD and TD directions, even when the sheet is 1 m or longer, and more preferably 0.5% or less. Such a low heat shrinkage rate suppresses peeling and dimensional inadequacies due to shrinkage, even when heat is applied during the manufacturing process of a rolled sheet. The heat shrinkage rate is calculated by cutting a 100 mm square evaluation sample, heat-treating it at 60°C for 6 hours, and then calculating the heat shrinkage rate from the length before and after heat treatment using the following formula: Heat shrinkage rate (%) = 100 × (length before heat treatment - length after heat treatment) / length before heat treatment. The heat shrinkage rates in the MD and TD directions can be calculated using the above formula from the lengths before and after heat treatment in the MD and TD directions, respectively. Ten or more 100 mm square evaluation samples are prepared at equal intervals along the length of the sheet, and the heat shrinkage rates calculated from the individual evaluation samples are averaged to determine the heat shrinkage rates in the MD and TD directions. The thermal shrinkage rate can be adjusted by adjusting the contents of the various components constituting the heat-expandable fire-resistant sheet.
[0047] The heat-expandable fire-resistant sheet of the present invention can be wound into a roll having a length of 1 m or more. In particular, in the case of a heat-expandable fire-resistant sheet with small thickness variations and high dimensional accuracy, it is easy to efficiently manufacture a roll of long sheets. The rolled body of the present invention is a heat-expandable fire-resistant sheet having a length of 1 m or more wound into a roll shape, for example, a heat-expandable fire-resistant sheet having a length of 1 m or more wound around a cylindrical winding core. The winding core may be omitted. The width of the heat-expandable fire-resistant sheet is not particularly limited, but is, for example, 0.005 to 2.0 m. As described below, a heat-expandable fire-resistant sheet (multilayer sheet) having a substrate or an adhesive layer may also be wound into a roll.
[0048] <Method for manufacturing thermally expandable fire-resistant sheet> The method for manufacturing the thermally expandable fire-resistant sheet of the present invention is not particularly limited, but a method in which the above-mentioned thermally expandable composition is solidified, dried, or cured is preferred. By such a manufacturing method, for example, the above-mentioned rolled body having a length of 1 m or more can be obtained. Specifically, the thermally expandable composition is applied to any object, and the applied thermally expandable composition is solidified, dried, or cured. The thermally expandable composition can be applied using a known coating device, spray, or the like.
[0049] For example, when the above-mentioned dry-and-solidify adhesive is used as the matrix component, the thermally expandable composition is in a liquid state containing a solvent, and therefore the thermally expandable fire-resistant sheet can be formed by drying the thermally expandable composition after application to remove the solvent. Drying can be carried out by leaving it at around room temperature (about 25°C), but it is preferable to carry out drying by heating. Heating is preferably carried out at a temperature below the expansion initiation temperature of the thermally expandable graphite, for example, at about 50 to 160°C, preferably about 60 to 120°C.
[0050] When the above-mentioned chemically reactive adhesive is used as the matrix component, a thermally expandable fire-resistant sheet can be obtained by curing the applied thermally expandable composition. The curing method can be appropriately selected depending on the type of matrix component. When a curing agent-reactive adhesive is used, curing can be promoted by mixing with a curing agent. That is, the thermally expandable composition can be added with a curing agent and then applied to an object to be cured. Alternatively, the thermally expandable composition can be made into a two-part composition consisting of a liquid containing a curing agent and a liquid not containing a curing agent, and the two parts of the two-part thermally expandable composition can be mixed and applied to an object to be cured. In the case of a moisture-curing reactive adhesive, the adhesive can be applied to an object and then left in the atmosphere for a predetermined period of time. This allows curing to proceed due to the moisture in the air. In the case of an ultraviolet-reactive adhesive, the adhesive can be applied to an object and then cured by irradiating ultraviolet light.
[0051] When a hot-melt adhesive is used as the matrix component, the thermally expandable composition is melted by heating, and the molten thermally expandable composition is applied to any desired object. The heating temperature during melting is preferably below the expansion initiation temperature of the thermally expandable graphite, for example, 80 to 160°C, and preferably about 100 to 120°C. After application, the thermally expandable composition is cooled, for example, to room temperature (25°C) to solidify, thereby obtaining a thermally expandable fire-resistant sheet.
[0052] The object to which the thermally expandable composition is applied is not particularly limited, but may be, for example, a release-treated resin film, or when producing a thermally expandable fire-resistant sheet that includes a substrate, the substrate may be the object to which the thermally expandable composition is applied.
[0053] <Substrate, Adhesive Layer, Separator> The heat-expandable fire-resistant sheet of the present invention may be used alone, or may be used as a multilayer sheet by attaching other components as appropriate. Specifically, the heat-expandable fire-resistant sheet may have a substrate or an adhesive layer on at least one surface. For example, the heat-expandable fire-resistant sheet may have a substrate on one surface (a multilayer sheet of substrate / heat-expandable fire-resistant sheet), an adhesive layer on one surface (a multilayer sheet of adhesive layer / heat-expandable fire-resistant sheet), or a substrate on one surface and an adhesive layer on the other surface (a multilayer sheet of adhesive layer / heat-expandable fire-resistant sheet / substrate). Furthermore, the heat-expandable fire-resistant sheet may have a separator, for example, a separator may be provided on the surface of the adhesive layer.
[0054] (Substrate) The substrate is in the form of, for example, a woven fabric, a nonwoven fabric, a film, etc., and is formed from a thermoplastic resin, a thermosetting resin, an elastomer resin, etc., among which a thermoplastic resin is preferred. The substrate may also be formed from glass fiber, ceramic fiber, cellulose fiber, polyester fiber, carbon fiber, graphite fiber, thermosetting resin fiber, etc. A preferred form of the substrate is a film. A film having a cavity therein can also be suitably used as the film.
[0055] Specific examples of thermoplastic resins include polyesters such as polyvinyl chloride, polyethylene terephthalate, and polybutylene terephthalate; polyolefins such as polyethylene, polypropylene, poly(1-butene), and polypentene; polyvinyl acetate, polystyrene, acrylic resins, acrylonitrile-butadiene-styrene (ABS) resins, polycarbonate, polyamide, polyphenylene ether, and polyethersulfone. Among these, from the viewpoint of adhesion to the thermally expandable fire-resistant sheet, preferred thermoplastic resins are polyvinyl chloride, polyethylene terephthalate, polyolefins, and polyvinyl acetate. Furthermore, from the viewpoint of flame retardancy, polyvinyl chloride is more preferred. Also preferred is a polyethylene terephthalate film having internal cavities.
[0056] Specific examples of thermosetting resins include epoxy resins, urethane resins, phenolic resins, unsaturated polyesters, alkyd resins, urea resins, and polyimides.
[0057] Specific examples of elastomer resins include isoprene rubber, butadiene rubber, 1,2-polybutadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, ethylene-propylene rubber, chlorosulfonated polyethylene, acrylic rubber, epichlorohydrin rubber, silicone rubber, fluororubber, urethane rubber, polyisobutylene rubber, and butyl chloride. One or more of the above-mentioned thermoplastic resins, thermosetting resins, and elastomer resins are used.
[0058] The thickness of the substrate is preferably 1 to 20% of the thickness of the multilayer sheet. When the thickness of the substrate is 1% or more of the thickness of the multilayer sheet, the substrate can easily support the heat-expandable fire-resistant sheet. Furthermore, when the thickness of the substrate is 20% or less of the thickness of the multilayer sheet, peeling between the substrate and the heat-expandable fire-resistant sheet and the occurrence of wrinkles in the substrate are suppressed when the multilayer sheet is curved, and the appearance of the multilayer sheet can be maintained in a good condition.
[0059] The thickness of the substrate is, for example, 10 to 500 μm, preferably 20 to 450 μm, and more preferably 30 to 400 μm. By making the thickness of the substrate equal to or greater than these lower limits, the substrate can be provided with the strength to support the thermally expandable fire-resistant sheet. Furthermore, by making the thickness equal to or less than the upper limits, the thickness of the substrate can be prevented from becoming thicker than necessary, making it easier to use the multilayer sheet in fire prevention equipment such as doors.
[0060] (Adhesive Layer) The adhesive layer may be a single layer (hereinafter also referred to as adhesive layer) formed solely from an adhesive, or may be a double-sided adhesive tape in which adhesive layers are provided on both surfaces of a double-sided adhesive tape substrate. However, an adhesive layer is preferred. The adhesive layer of a double-sided adhesive tape is formed by bonding one of the adhesive layers to a heat-expandable fire-resistant sheet or a separator. The adhesive constituting the adhesive layer is not particularly limited, and examples thereof include acrylic adhesives, urethane adhesives, and rubber adhesives. The thickness of the adhesive layer is not particularly limited, but is, for example, 10 to 500 μm, preferably 50 to 200 μm. The substrate for a double-sided adhesive tape is not particularly limited as long as it is a substrate commonly used in double-sided adhesive tapes, and examples thereof include nonwoven fabrics, paper such as Japanese paper, woven fabrics made of natural fibers, synthetic fibers, and the like, resin films made of polyester, polyolefin, soft polyvinyl chloride, hard polyvinyl chloride, acetate, and the like, and flat yarn cloth.
[0061] (Separator) The separator may be, for example, a separator substrate comprising a separator base material and a release layer provided on at least one surface of the separator base material. The release layer can be formed by subjecting the separator base material to a release treatment. The separator may be positioned so that the surface on which the release layer is provided contacts the adhesive layer. Alternatively, both surfaces of the separator base material may be subjected to a release treatment, and release layers may be provided on both surfaces. The release layer is not particularly limited, but may be composed of, for example, an organic resin. As the organic resin, a known release agent may be used, such as a fluorine-based resin, a long-chain alkyl-containing resin, an alkyd-based resin, a polyolefin-based resin, or a rubber-based elastomer. As the separator base material, a resin film, paper, or the like may be used. The resin film may be formed from a thermoplastic resin, a thermosetting resin, an elastomer resin, or the like. Specific examples of the thermoplastic resin, thermosetting resin, or elastomer resin include those listed for the resin film, but thermoplastic resins are preferred.
[0062] The thickness of the separator is preferably 0.3 to 10% of the thickness of the multilayer sheet. When the thickness of the separator is 0.3% or more of the thickness of the multilayer sheet, the separator is more likely to be prevented from breaking. Furthermore, when the thickness of the separator is 10% or less of the thickness of the multilayer sheet, peeling between the heat-expandable fire-resistant sheet and the separator and the occurrence of wrinkles in the separator are prevented when the multilayer sheet is bent, and the appearance of the multilayer sheet can be maintained in a good condition.
[0063] The thickness of the separator is, for example, 1 to 200 μm, preferably 2 to 150 μm, and more preferably 5 to 100 μm. By making the thickness of the separator equal to or greater than these lower limits, the separator can be provided with sufficient strength to withstand breakage. Furthermore, by making the thickness equal to or less than the upper limits, peeling between the fireproof material and the separator and wrinkles on the separator can be prevented when the multilayer sheet is bent.
[0064] <Method for Manufacturing a Thermally Expandable Material-Containing Member> The present invention also provides a method for manufacturing a thermally expandable material-containing member, which involves applying the above-described thermally expandable composition to a member and solidifying, drying, or curing the composition to obtain a thermally expandable material-containing member. The member is an object for which the thermally expandable composition is used, and is preferably a fire prevention facility, as described below. Examples of fire prevention facilities include fittings such as windows, shoji screens, doors, sliding doors, and sliding doors, pillars, walls made of steel-framed concrete, floors, and roofs. The thermally expandable material is formed by solidifying, drying, or curing the thermally expandable composition. The solidification, drying, and curing are as described in the method for manufacturing a thermally expandable fire-resistant sheet. The expansion onset temperature, elution rate, and amount of phosphorus component of the thermally expandable material are in the same ranges as those for the thermally expandable fire-resistant sheet. The thermally expandable material-containing member of the present invention can maintain good fire resistance even if warping occurs during a fire.
[0065] [Fire Prevention Equipment] The present invention can provide fire prevention equipment at least partially equipped with the above-mentioned heat-expandable fire-resistant sheet. Examples of fire prevention equipment include fittings such as windows, shoji screens, doors, sliding doors, and other doors; pillars; walls made of steel-framed concrete; floors; and roofs. The heat-expandable fire-resistant sheet of the present invention is installed in part of such fire prevention equipment and expands during a fire, thereby reducing or preventing the penetration of flames and smoke. In particular, the heat-expandable fire-resistant sheet is preferably used in gaps between windows and window frames, between doors and door frames, and the like. Even if these various fire prevention equipment warp and deform during a fire, the heat-expandable fire-resistant sheet of the present invention easily follows the warp and can continuously prevent the penetration of flames and smoke for a long period of time, thereby maintaining good fire resistance over a long period of time.
[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0067] The measurement and evaluation methods for each physical property are as follows. <Expansion start temperature of thermally expandable graphite> In a rheometer ("Discovery HR-2", manufactured by TA Instruments), 0.5 g of a sample of thermally expandable graphite was placed on the sample stage and wrapped in aluminum foil to prevent the powder from falling off. The sample was grounded with a 25 mmφ cone plate until the load reached 0 [N]. From this state, the sample was heated at a constant heating rate (10°C / min) from a set temperature of 50°C using a Peltier heater, and the point at which the load reached 0.1 N was taken as the expansion start temperature.
[0068] <Expansion Start Temperature of Heat-Expandable Fire-Resistant Sheet> Using a heat-expandable fire-resistant sheet as a sample, the temperature was increased at a rate of 10°C / min using a rheometer ("Discovery HR2" manufactured by TA Instruments), and the temperature at which the normal force rose was measured, and this was taken as the expansion start temperature.
[0069] <Decomposition Initiation Temperature and Heat Shrinkage of Matrix Component> The decomposition initiation temperature and heat shrinkage of the matrix component were measured by the method described in the specification.
[0070] <Thickness Variation> The thickness of the heat-expandable fire-resistant sheet was measured at 10 points at equal intervals along the longitudinal direction, and the average thickness was calculated by averaging these 10 thicknesses. Next, the absolute value A of the difference between the thickness measured at each of the 10 points at equal intervals along the longitudinal direction of the heat-expandable fire-resistant sheet and the average thickness was calculated, and the average of the absolute values A for the 10 points was taken as the thickness variation. If the thickness variation was 10% or less of the thickness (average thickness), it was evaluated as "A," and if it was more than 10%, it was evaluated as "B."
[0071] <Elution Rate> A test piece (10 g) prepared by cutting out the obtained thermally expandable fireproof sheet was immersed in 200 g of pure water and left to immerse in a sealed container at 60°C for one week. The test piece was then removed, the pure water was evaporated and dried, and the mass of the precipitate that formed was measured. Using this value, the elution rate was calculated using the following formula and used as an index of water resistance: Elution Rate (%) = [(Mass of Precipitate) / (Mass of Test Piece Before Immersion in Pure Water)] × 100
[0072] <Fire resistance> The obtained thermally expandable fireproof sheets were evaluated for fire resistance in accordance with ISO 12472:2003. Specifically, a test specimen was prepared based on the diagram described in ISO 12472:2003, heated according to the heating curve of ISO 834, and 15 minutes after the start of heating, a load of 7.5 kg was applied to forcibly deform the specimen, and the specimen was heated for a total of 60 minutes before being observed. Evaluation was based on the following criteria. A: No penetration into the furnace B: Penetration into the furnace
[0073] The components used in the examples and comparative examples are as follows. <Matrix components> Polyurethane-based: "Tyforce HH-600" manufactured by DIC Corporation, hot-melt adhesive Polyurethane-based: "Vondic 1050B-NE" manufactured by DIC Corporation, dry-setting adhesive (emulsion-type adhesive) Chloroprene (rubber-based): "Skyprene LA-710" manufactured by Tosoh Corporation, dry-setting adhesive (synthetic rubber latex-based adhesive) Polyester-based: "Aronmelt PES-111EE" manufactured by Toa Gosei Co., Ltd., hot-melt adhesive Polyester-based: "Aronmelt PES310S30" manufactured by Toa Gosei Co., Ltd., dry-setting adhesive (solvent-based adhesive), solvent (toluene, methyl ethyl ketone), 30% solids Vinyl acetate copolymer resin-based: "Vinyblan 1157" manufactured by Nissin Chemical Industry Co., Ltd., dry-setting adhesive (emulsion-type adhesive) Vinyl acetate copolymer resin-based: "Vinyblan" manufactured by Nissin Chemical Industry Co., Ltd. A70J2M", dry-hardening adhesive (emulsion type adhesive) ・Acrylic resin type: DIC Corporation "ACRYDIC 57-773-BA", dry-hardening adhesive (solvent-based adhesive), solvent (ethyl acetate, butyl acetate) ・Silicone resin type (unmodified): Shin-Etsu Silicones Co., Ltd. "KR220L", dry-hardening adhesive (solvent-based adhesive), solvent (toluene, isopropyl alcohol) ・Ethylene-vinyl acetate copolymer resin type (EVA type), Mitsui Chemicals Inc. "V5774ETWR", hot-melt type adhesive ・Polystyrene type, Mitsui Chemicals Inc. "FTR6100", hot-melt type adhesive ・Modified silicone resin type: polymer with crosslinkable silyl groups, Kaneka Corporation "MS Polymer S-303", moisture-curing type ・Modified silicone resin type: polymer with crosslinkable silyl groups, Toagosei Co., Ltd. "US-6150", moisture-curing type Modified silicone resin system: polymer with crosslinkable silyl groups, AGC "Excestar-S6250", moisture-curing reaction type Modified silicone resin system: polymer with crosslinkable silyl groups, Soken Chemical & Engineering Co., Ltd. "SE-09", moisture-curing reaction type Modified silicone resin system: polymer with crosslinkable silyl groups, Kaneka "Silyl EST280", moisture-curing reaction type Silylated urethane system: Momentive Performance Materials Japan "SPUR3030"
[0074] <Curing catalyst> - "Neostan U220H" manufactured by Nitto Kasei Co., Ltd.
[0075] <Thermal expandable graphite> - Fuji Graphite Industries "EXP-50S150", expansion start temperature 150°C
[0076] <Inorganic fillers> Iron oxide Aluminum hydroxide (Shiraishi Calcium Co., Ltd.) Calcium carbonate (Shiraishi Calcium Co., Ltd.)
[0077] [Example 1] A thermally expandable composition was obtained by mixing the components using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then heated to 120°C to melt, and then coated onto a release PET film using a roll coater. The coated product was then cooled to room temperature (25°C) to solidify, forming a thermally expandable fire-resistant sheet on the release PET film. The thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm) was subjected to various evaluations. The evaluation results are shown in Table 1.
[0078] [Examples 4, 10, and 11] A thermally expandable fire-resistant sheet was obtained in the same manner as in Example 1, except that the composition was changed as shown in Table 1. The thermally expandable fire-resistant sheet was subjected to various evaluations.
[0079] [Example 2] A thermally expandable composition was obtained by mixing the components using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then applied to a release PET film using a roll coater, and the applied product was dried at 120°C to evaporate the solvent, forming a thermally expandable fire-resistant sheet on the release PET film. Various evaluations were performed on the thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm).
[0080] [Examples 3, 5 to 9] A thermally expandable fire-resistant sheet was obtained in the same manner as in Example 2, except that the composition was changed as shown in Table 1. Various evaluations were carried out on the thermally expandable fire-resistant sheet.
[0081] [Examples 12 to 17] A thermally expandable composition was obtained by mixing the components at 25°C using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then applied to a release PET film using a roll coater, and the applied product was cured at 50°C to form a thermally expandable fire-resistant sheet on the release PET film. Various evaluations were performed on the thermally expandable fire-resistant sheet (length 20 mm, thickness 1.5 mm, width 10 mm).
[0082] The thermally expandable compositions used in the examples also contain solvents when a dry-to-solidify adhesive is used, but Table 1 lists the amounts of the solid components of the thermally expandable compositions only.
[0083] The thermally expandable fire-resistant sheets of each Example were formed from a thermally expandable composition containing a matrix component made of a specific adhesive and thermally expandable graphite, and all were evaluated as having good fire resistance. These results demonstrate that the thermally expandable fire-resistant sheets formed from the thermally expandable composition of the present invention can easily conform to the warping of fire prevention equipment during a fire and can maintain good fire resistance for a long period of time.
Claims
1. A thermally expandable composition comprising a matrix component and thermally expandable graphite, wherein the matrix component is at least one adhesive selected from the group consisting of a drying-solidifying type adhesive, a chemically reactive type adhesive, and a hot-melt type adhesive.
2. The thermally expandable composition according to claim 1, further comprising an inorganic filler, the content of the thermally expandable graphite being 3 to 300 parts by mass and the content of the inorganic filler being 2 to 200 parts by mass per 100 parts by mass of the matrix component, and the expansion initiation temperature of the thermally expandable graphite being lower than the decomposition initiation temperature of the matrix component.
3. The thermally expandable composition according to claim 1 or 2, wherein the matrix component contains at least one adhesive selected from the group consisting of NBR epoxy resins, urea resins, melamine resins, phenolic resins, rubbers, vinyl acetate resins, vinyl acetate copolymer resins, ethylene-vinyl acetate copolymer resins, acrylic resins, aqueous polymer-isocyanate resins, synthetic rubber latexes, epoxy resins (unmodified), cyanoacrylates, polyurethanes, silicone resins (unmodified), modified silicone resins, silylated urethanes, polystyrenes, and polyesters.
4. A thermally expandable fire-resistant sheet molded from the thermally expandable composition according to claim 1 or 2.
5. The thermally expandable fire-resistant sheet according to claim 4, having an expansion initiation temperature of 160°C or less.
6. The heat-expandable fire-resistant sheet according to claim 4, which has a dissolution rate of 3% or less after immersion in pure water at 60°C for one week.
7. The thermally expandable fire-resistant sheet according to claim 4, wherein the matrix component does not contain a phosphorus component.
8. The thermally expandable fire-resistant sheet according to claim 4, having a substrate or an adhesive layer on at least one surface.
9. The heat-expandable fire-resistant sheet according to claim 4, which is a rolled body having a length of 1 m or more.
10. A heat-expandable fire-resistant sheet according to claim 4, having a length of 1 m or more, a thermal shrinkage rate of 1% or less in both the MD and TD directions, a thickness of 0.5 mm or more, and a thickness variation of 0.1 mm or less.
11. A method for producing a thermally expandable fire-resistant sheet, comprising solidifying, drying, or curing the thermally expandable composition according to claim 1 or 2 to obtain a roll having a length of 1 m or more.
12. A method for producing a thermally expandable material-containing component, comprising applying the thermally expandable composition according to claim 1 or 2 to a component and solidifying, drying or curing the composition to obtain a thermally expandable material-containing component.
13. A fire protection system having at least a portion mounted with the thermally expandable fireproof sheet according to claim 7.
Citation Information
Patent Citations
Adhesive composition and wallpaper prepared by using the same
JP1998237406A
Bonded body and method of recycling by using the same
JP2004189856A
Epoxy resin adhesive
JP2006225544A
Fire-resistant resin composition
JP2017141463A
Thermally-expandable refractory sheet
JP2018070879A