Spherical titanium dioxide composite nanoparticles, and method for preparing same by using sol-gel process
Spherical titanium dioxide composite nanoparticles with a sol-gel method and heat treatment maintain shape and refractive index, solving toxicity and clumping issues in existing technologies, enhancing UV blocking and cosmetic applications.
Patent Information
- Application Number
- PCT/KR2024/002619
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-31
AI Technical Summary
Existing titanium dioxide nanoparticles used in sunscreens and cosmetics often have toxicity issues and clumping problems due to their needle-shaped form, and spherical particles lose their shape during high-temperature heat treatment, leading to irregular forms and reduced refractive index.
Development of spherical titanium dioxide composite nanoparticles with a compound formula Ti_xSi_1-xO_2, where 0.5
The method produces nanoparticles that maintain their spherical shape and high refractive index, addressing toxicity and clumping issues while enabling effective UV ray blocking and broader applications in cosmetics, paints, and solar cells.
Smart Images

Figure KR2024002619_31102024_PF_FP_ABST
Abstract
Description
Spherical titanium dioxide composite nanoparticles and their preparation method using sol-gel method
[0001] The present invention relates to spherical titanium dioxide composite nanoparticles and a method for producing the same using a sol-gel method.
[0002] Ultraviolet rays from sunlight are known to cause skin erythema, freckles, skin cancer, and skin aging, and research on skin diseases caused by ultraviolet rays is actively being conducted.
[0003] To block ultraviolet rays contained in sunlight, high-refractive-index inorganic substances capable of reflecting ultraviolet rays or organic substances capable of absorbing ultraviolet rays are used in sunscreens. Examples of high-refractive-index inorganic substances include titanium dioxide and zinc oxide.
[0004] Conventionally used titanium dioxide is primarily needle-shaped, measuring tens of nanometers in diameter. When used in cosmetics, needle-shaped nanoparticles pose toxicity concerns due to their shape, and the friction generated by their shape can easily cause the cosmetics to clump together.
[0005] Meanwhile, spherical titanium dioxide particles, in their amorphous form, have a low refractive index, making them unsuitable for use in sunscreens. Therefore, heat treatment at high temperatures can increase their refractive index. However, when spherical particles are exposed to high temperatures, they lose their spherical shape during the phase change process and instead transform into a crystalline phase. This process, in turn, can cause the particle shape to become irregular.
[0006] Therefore, there is a need for the development of technology for composite nanoparticles containing titanium dioxide that can maintain a spherical shape even when subjected to high-temperature heat treatment and a method for manufacturing the same.
[0007] An object of the present invention is to provide composite nanoparticles containing titanium dioxide that remain in a spherical shape during a high-temperature heat treatment process.
[0008] Another object of the present invention is to provide a manufacturing method capable of simply manufacturing spherical composite nanoparticles containing titanium dioxide using a sol-gel method.
[0009] According to one aspect of the present invention, spherical titanium dioxide composite nanoparticles comprising a compound represented by the following chemical formula 1 are provided.
[0010] [Chemical Formula 1]
[0011] Ti x Si 1-x O2
[0012] In the above chemical formula 1,
[0013] x is 0.5 <x<1일 수 있다.
[0014] Additionally, the diameter of the spherical composite nanoparticles may be 0.01 to 10 μm.
[0015] Additionally, the spherical composite nanoparticles may include a rutile crystal structure.
[0016] Additionally, some of the oxygen atoms (O) chemically bonded with the titanium atoms (Ti) can chemically bond with the silicon atoms (Si).
[0017] Additionally, the chemical bond may include at least one of a covalent bond and an ionic bond.
[0018] According to another aspect of the present invention, at least one selected from the group consisting of a UV blocker, a paint, a material for solar cells and a catalyst for water decomposition, comprising spherical titanium dioxide composite nanoparticles, is provided, preferably a UV blocker and a paint.
[0019] According to another aspect of the present invention, a method for producing spherical titanium dioxide composite nanoparticles is provided, comprising the steps of: (a) preparing a mixture comprising a solvent, a titanium dioxide precursor, and a silica precursor; (b) subjecting the mixture to a sol-gel reaction; and (c) heat-treating the resultant of the sol-gel reaction to produce spherical titanium dioxide composite nanoparticles comprising a compound represented by the following chemical formula 1.
[0020] [Chemical Formula 1]
[0021] Ti x Si 1-x O2
[0022] In the above chemical formula 1,
[0023] x is 0.5 <x<1일 수 있다.
[0024] Additionally, some of the oxygen atoms (O) chemically bonded with the titanium atoms (Ti) can chemically bond with the silicon atoms (Si).
[0025] Additionally, the chemical bond may include at least one of a covalent bond and an ionic bond.
[0026] Additionally, the solvent may include a polar aprotic solvent, a C1 to C4 alcohol, and water.
[0027] Additionally, the polar aprotic solvent may include at least one selected from the group consisting of acetonitrile, acetone, dimethylformamide, dimethylsulfoxide, ethyl acetate, dichloromethane, and dimethylacetamide.
[0028] Additionally, the C1 to C4 alcohol may include at least one selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, and butanol.
[0029] In addition, the titanium dioxide precursor is titanium isopropoxide (C 12 H 28 O4Ti), titanium tetrachloride (TiCl4), titanium butoxide (C16 H 36 O4Ti), titanium methoxide (C4H 12 O4Ti) and titanium ethoxide (C8H 24 It may include at least one selected from the group consisting of O4Ti).
[0030] In addition, the silica precursor is selected from the group consisting of tetraethoxysilane (TEOS), tetramethyl orthosilicate, tetrapropyl orthosilicate, methyl triethyl orthosilicate, dimethyldiethyl orthosilicate, tetraisopropyl orthosilicate, tetrabutyl orthosilicate, tetrasecondarybutyl orthosilicate, tetratertiarybutyl orthosilicate, tetrahexyl orthosilicate, and tetracyclohexyl orthosilicate. It may include at least one selected from the group consisting of tetradodecyl orthosilicate and tetradodecyl orthosilicate.
[0031] Additionally, the ratio of the number of moles of the silica precursor to the total number of moles of the titanium dioxide precursor (A) and the number of moles of the silica precursor (B) (B / (A+B)x100) may be 0.1 to 10 mole%.
[0032] Additionally, the mixture of (a) may further include an organic amine.
[0033] Additionally, the organic amine may include at least one selected from the group consisting of dodecylamine, octadecylamine, hexadecylamine, propylamine, and butylamine.
[0034] Additionally, the organic amine may be a compound represented by the chemical formula 2 below.
[0035] [Chemical Formula 2]
[0036]
[0037] In the above chemical formula 2,
[0038] R 1 This may be a C2 to C18 alkylene group or a C2 to C18 alkenylene group.
[0039] Also, the above R 1 This may be a C6 to C14 alkylene group.
[0040] In addition, the step (a) may include (a-1) a step of mixing and stirring the solvent and the organic amine; (a-2) a step of mixing and stirring the titanium dioxide precursor and the silica precursor; and (a-3) a step of adding and mixing the resultant product of the step (a-2) to the resultant product of the step (a-1) to prepare a mixture.
[0041] Additionally, the sol-gel reaction of step (b) can be performed at room temperature.
[0042] Additionally, the heat treatment of the above step (c) can be performed at 700 to 1,000°C.
[0043] The spherical titanium dioxide composite nanoparticles of the present invention can maintain a spherical particle shape during a high-temperature heat treatment process while also having a high refractive index.
[0044] In addition, the spherical titanium dioxide composite nanoparticles of the present invention can have a uniform size distribution.
[0045] In addition, the method for producing spherical titanium dioxide composite nanoparticles of the present invention can produce spherical titanium dioxide composite nanoparticles in large quantities simply by a sol-gel method.
[0046] In addition, the method for producing spherical titanium dioxide composite nanoparticles of the present invention can produce spherical titanium dioxide composite nanoparticles by performing heat treatment once, thereby saving time and cost.
[0047] These drawings are for reference in explaining exemplary embodiments of the present invention, and therefore, the technical idea of the present invention should not be interpreted as being limited to the attached drawings.
[0048] Figure 1 is a method for manufacturing spherical titanium dioxide composite nanoparticles according to the present invention.
[0049] Figure 2 shows the rutile phase of spherical titanium dioxide composite nanoparticles manufactured according to Example 2 of the present invention.
[0050] Figure 3 shows the results of XRD (X-ray diffraction data) analysis manufactured according to Example 4 of the present invention.
[0051] FIG. 4 is a TEM and EDS Mapping photograph that can confirm the atomic unit mixing of spherical titanium dioxide composite nanoparticles manufactured according to Example 2 of the present invention.
[0052] Figure 5 shows the refractive index of spherical titanium dioxide composite nanoparticles manufactured according to Example 4 of the present invention.
[0053] Figure 6 shows the size distribution results of spherical titanium dioxide composite nanoparticles manufactured according to Example 4 of the present invention.
[0054] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings so that a person having ordinary skill in the art to which the present invention pertains can easily practice the invention.
[0055] However, the following description is not intended to limit the present invention to a specific embodiment, and when explaining the present invention, if it is determined that a detailed description of a related known technology may obscure the gist of the present invention, the detailed description is omitted.
[0056] The terminology used herein is for the purpose of describing specific embodiments only and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this application, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, or combination thereof described in the specification, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, or combinations thereof.
[0057] Additionally, terms including ordinal numbers, such as "first," "second," etc., which will be used hereinafter, may be used to describe various components, but these components are not limited by these terms. These terms are used solely to distinguish one component from another. For example, without departing from the scope of the present invention, a first component could be referred to as a second component, and similarly, a second component could also be referred to as a first component.
[0058] Additionally, when it is said that a component is "formed on" or "laminated on" another component, it should be understood that it may be formed or laminated directly on the entire surface or one side of the other component, but there may also be other components present in between.
[0059] Hereinafter, the spherical titanium dioxide composite nanoparticles of the present invention and their manufacturing method using the sol-gel method will be described in detail. However, these are provided as examples and the present invention is not limited thereto, and the present invention is defined solely by the scope of the claims set forth below.
[0060] The present invention provides spherical titanium dioxide composite nanoparticles comprising a compound represented by the following chemical formula 1.
[0061] [Chemical Formula 1]
[0062] Ti x Si 1-x O2
[0063] In the above chemical formula 1,
[0064] x is 0.5 <x<1이다.
[0065] The diameter of the above spherical titanium dioxide composite nanoparticles may be 0.01 to 10 μm, preferably 0.05 to 1 μm, and more preferably 0.1 to 0.5 μm. If the diameter of the above spherical titanium dioxide composite nanoparticles is less than 0.01 μm, it is undesirable because it is difficult for the particles to maintain a spherical shape, and if it exceeds 10 μm, it is undesirable because it is difficult to implement through the sol-gel method.
[0066] The above spherical titanium dioxide composite nanoparticles may include a rutile crystal structure.
[0067] Some of the oxygen atoms (O) chemically bonded with the titanium atoms (Ti) can chemically bond with the silicon atoms (Si).
[0068] The above chemical bond may include at least one of a covalent bond and an ionic bond.
[0069] The spherical titanium dioxide composite nanoparticles according to the present invention are high-refractive index particles capable of reflecting ultraviolet rays, and thus can be used in inorganic UV blockers, paints, solar cell materials, water-splitting catalysts, and the like. In particular, when used in cosmetics, the spherical nanoparticles possess high refractive index characteristics, thereby resolving the issue of toxicity due to their shape, and the disadvantage of cosmetics easily clumping due to friction caused by their shape can be resolved.
[0070] According to another aspect of the present invention, at least one selected from the group consisting of a UV blocker, a paint, a material for solar cells and a catalyst for water decomposition, comprising spherical titanium dioxide composite nanoparticles, is provided, preferably a UV blocker and a paint.
[0071] FIG. 1 is a drawing regarding a method for manufacturing spherical titanium dioxide composite nanoparticles according to the present invention. Hereinafter, with reference to FIG. 1, the method for manufacturing spherical titanium dioxide composite nanoparticles according to the present invention will be described in detail.
[0072] The present invention provides a method for producing spherical titanium dioxide composite nanoparticles, comprising the steps of: (a) preparing a mixture comprising a solvent, a titanium dioxide precursor, and a silica precursor; (b) subjecting the mixture to a sol-gel reaction; and (c) heat-treating the resultant of the sol-gel reaction to produce spherical titanium dioxide composite nanoparticles comprising a compound represented by the following chemical formula 1.
[0073] [Chemical Formula 1]
[0074] Ti x Si 1-x O2
[0075] In the above chemical formula 1,
[0076] x is 0.5 <x<1일 수 있다.
[0077] Some of the oxygen atoms (O) chemically bonded with the titanium atoms (Ti) can chemically bond with the silicon atoms (Si).
[0078] The above chemical bond may include at least one of a covalent bond and an ionic bond.
[0079] The solvent may include a polar aprotic solvent, a C1 to C4 alcohol, and water.
[0080] The above polar aprotic solvent may include at least one selected from the group consisting of acetonitrile, acetone, dimethylformamide, dimethylsulfoxide, ethyl acetate, dichloromethane, and dimethylacetamide.
[0081] The above C1 to C4 alcohol may include at least one selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, and butanol.
[0082] The above water can be used in a sol-gel reaction.
[0083] Specifically, the volume ratio of the alcohol and the polar aprotic solvent may be mixed at a volume ratio of 6:4 to 9:1, preferably 7.5:2.5 to 8:2, and more preferably 7:3. When the volume ratio of the alcohol and the polar aprotic solvent is less than 6:4, or more than 9:1, the size of the particles is formed unevenly, which is undesirable.
[0084] The above titanium dioxide precursor is titanium isopropoxide (C 12 H 28 O4Ti), titanium tetrachloride (TiCl4), titanium butoxide (C 16 H 36 O4Ti), titanium methoxide (C4H 12 O4Ti) and titanium ethoxide (C8H 24 It may include at least one selected from the group consisting of O4Ti).
[0085] The above silica precursor is selected from the group consisting of tetraethoxysilane (TEOS), tetramethyl orthosilicate, tetrapropyl orthosilicate, methyltriethyl orthosilicate, dimethyldiethyl orthosilicate, tetraisopropyl orthosilicate, tetrabutyl orthosilicate, tetrasecondarybutyl orthosilicate, tetratertiarybutyl orthosilicate, tetrahexyl orthosilicate, and tetracyclohexyl orthosilicate. It may include at least one selected from the group consisting of tetradodecyl orthosilicate and tetradodecyl orthosilicate.
[0086] The ratio of the number of moles of the silica precursor to the total number of moles of the titanium dioxide precursor (A) and the number of moles of the silica precursor (B) (B / (A+B)x100) may be 0.1 to 10 mol%, preferably 1 to 5 mol%. When the ratio of the number of moles of the silica precursor to the total number of moles is less than 0.1 mol%, the amount of silica contained is insufficient, so that the characteristics of the composite nanoparticles cannot be exhibited, which is undesirable. When it exceeds 10 mol%, the characteristics of titania cannot be exhibited due to the excessive inclusion of silica, which is undesirable.
[0087] The mixture of the above (a) may further contain an organic amine.
[0088] The above organic amine may include at least one selected from the group consisting of dodecylamine, octadecylamine, hexadecylamine, propylamine, and butylamine.
[0089] The above dodecylamine can act as a catalyst. It can also participate in the reaction to form a precursor complex. The above dodecylamine can reduce the reactivity of the titanium dioxide precursor, which can aid in the formation of spherical titanium dioxide.
[0090] The above organic amine may be a compound represented by the chemical formula 2 below.
[0091] [Chemical Formula 2]
[0092]
[0093] In the above chemical formula 2,
[0094] R 1 This may be a C2 to C18 alkylene group or a C2 to C18 alkenylene group.
[0095] The above R 1 This may be a C6 to C14 alkylene group.
[0096] The above step (a) may include (a-1) a step of mixing and stirring the solvent and the organic amine; (a-2) a step of mixing and stirring the titanium dioxide precursor and the silica precursor; and (a-3) a step of adding and mixing the resultant product of step (a-2) to the resultant product of step (a-1) to prepare a mixture.
[0097] The sol-gel reaction of step (b) above can be performed at room temperature.
[0098] The heat treatment of the above step (c) may be performed at 700 to 1,000°C, preferably 750 to 950°C. If the heat treatment is performed at a temperature lower than 700°C, the rutile crystal phase may not be completely formed, which is undesirable. If the heat treatment is performed at a temperature higher than 1,000°C, the composite nanoparticles may melt and lose their original shape, which is undesirable.
[0099] Since the heat treatment of the present invention is performed only once during the entire manufacturing process, time and cost can be saved compared to the conventional technology that requires two or more heat treatments.
[0100] [Example]
[0101] Hereinafter, preferred embodiments of the present invention will be described. However, these are provided for illustrative purposes only and the scope of the present invention is not limited thereby.
[0102] Manufacturing of spherical titanium dioxide composite nanoparticles
[0103] Example 1: 0.1 mol%
[0104] A precursor mixture was prepared by mixing and stirring titanium isopropoxide, a precursor of titanium dioxide, and tetraethyl silicate, a precursor of silica, so that the molar % of tetraethyl orthosilicate (TEOS) was 0.1 mol% with respect to the total molar number of tetraethyl orthosilicate.
[0105] A mixture was prepared by adding 0.2 ml of distilled water and 0.5 ml of dodecylamine to 50 ml of a 7:3 mixture of methanol and acetonitrile and stirring using a magnetic stirrer for more than 30 minutes.
[0106] After stirring the above mixture and the precursor mixture for more than 30 minutes, 1 ml of the precursor mixture was quickly added to 50.7 ml of the mixture. The mixture containing the precursor mixture was stirred at room temperature for more than 24 hours to perform a sol-gel reaction, and then the impurities and unreacted precursor were removed using a centrifuge and then dried.
[0107] The dried result was heat-treated in a sintering furnace at 900°C for 6 hours to produce spherical titanium dioxide composite nanoparticles.
[0108] Example 2: 0.5 mol%
[0109] Spherical titanium dioxide composite nanoparticles were prepared in the same manner as in Example 1, except that the molar percentage of tetraethyl silicate was used as 0.5 mol% instead of 0.1 mol% based on the total molar number of titanium isopropoxide, a precursor of titanium dioxide, and tetraethyl silicate, a precursor of silica.
[0110] Example 3: 1 mol%
[0111] Spherical titanium dioxide composite nanoparticles were prepared in the same manner as in Example 1, except that the molar percentage of tetraethyl silicate, a silica precursor, and titanium isopropoxide, a titanium dioxide precursor, was used at 1 mol% instead of 0.1 mol% based on the total molar number of tetraethyl silicate, a silica precursor.
[0112] Example 4: 2 mol%
[0113] Spherical titanium dioxide composite nanoparticles were prepared in the same manner as in Example 1, except that the molar percentage of tetraethyl silicate, a silica precursor, and titanium isopropoxide, a titanium dioxide precursor, was used at 2 mol% instead of 0.1 mol% based on the total molar number of tetraethyl silicate, a silica precursor.
[0114] Example 5: 5 mol%
[0115] Spherical titanium dioxide composite nanoparticles were prepared in the same manner as in Example 1, except that the molar percentage of tetraethyl silicate, a silica precursor, and titanium isopropoxide, a titanium dioxide precursor, was used at 5 mol% instead of 0.1 mol% based on the total molar number of tetraethyl silicate, a silica precursor.
[0116] Example 6: 10 mol%
[0117] Spherical titanium dioxide composite nanoparticles were prepared in the same manner as in Example 1, except that the molar percentage of tetraethyl silicate, a silica precursor, and titanium isopropoxide, a titanium dioxide precursor, was used at 10 mol% instead of 0.1 mol% based on the total molar number of tetraethyl silicate, a silica precursor.
[0118] The molar percentages of titanium isopropoxide, a precursor of titanium dioxide, and tetraethyl silicate, a precursor of silica, in Examples 1 to 6 are summarized in Table 1 below.
[0119] Classification TTIP (mol%) TEOS (mol%) Example 199.9 0.1 Example 299.5 0.5 Example 399 1 Example 498 2 Example 595 5 Example 690 10
[0120] [Example Exam]
[0121] Test Example 1: Shape Analysis
[0122] Figure 2 shows the morphology of the composite nanoparticles of Example 2 observed using a scanning electron microscope (SEM, Hitachi, S-4300) and a transmission electron microscope (TEM, JEOL LTD, JEM2100F). Referring to Figure 2, the spherical titanium dioxide composite nanoparticles according to the present invention are in a rutile phase. It can be confirmed that the spherical titanium dioxide composite nanoparticles can be simply manufactured by the sol-gel reaction method even with high-temperature heat treatment by including a silica precursor.
[0123] Test Example 2: Crystallinity Evaluation
[0124] Figure 3 shows the results of X-ray diffraction (XRD) analysis to confirm crystallinity of spherical titanium dioxide composite nanoparticles according to Example 4 of the present invention. The sample was prepared using 2 mol% of TEOS, and the precursor molar ratio (mol%:mol%) TTIP:TEOS = 98:2.
[0125] Referring to Figure 3, one can confirm the X-ray diffraction peaks that appear due to the crystal structure of the rutile crystal phase.
[0126] Test Example 3: Atomic Unit Bonding
[0127] FIG. 4 is a TEM and EDS Mapping photograph that can confirm the atomic unit mixing of spherical titanium dioxide composite nanoparticles according to Example 2 of the present invention.
[0128] Referring to FIG. 4, it was confirmed that the spherical titanium dioxide composite nanoparticles according to the present invention were bonded at the atomic level.
[0129] Test Example 4: Refractive Index Analysis
[0130] Figure 5 is a graph showing the refractive index of spherical titanium dioxide composite nanoparticles according to Example 4 of the present invention measured using holographic characterization equipment (xSight, Spheryx, Inc.). Here, each dot represents the measurement result for one sample, and the color of the dot represents the distribution ratio.
[0131] Referring to Figure 5, each dot represents the measurement results of the refractive index and diameter of a single rutile titania particle, and the color of the dots represents the distribution. The brighter the dot, the more dots there are together, indicating a high distribution ratio. This shows that the spherical titanium dioxide composite nanoparticles according to the present invention have a high refractive index. As the refractive index increases, light scattering becomes stronger, and effects such as the expression of scattered colors and UV blocking can be enhanced.
[0132] Test Example 5: Checking Size Distribution
[0133] Figure 6 shows the size distribution of spherical titanium dioxide composite nanoparticles according to Example 4 of the present invention. As a result of diameter observation through SEM, the size distribution was less than 10%.
[0134] Referring to FIG. 6, it can be seen that the spherical titanium dioxide composite nanoparticles according to the present invention have a uniform size distribution.
[0135] The scope of the present invention is indicated by the claims described below rather than the detailed description above, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.
Claims
1. Spherical titanium dioxide composite nanoparticles comprising a compound represented by the chemical formula 1 below. [Chemical Formula 1] Of x To 1-x O2 In the above chemical formula 1, x is 0.5 <x<1이다.
2. In paragraph 1, Spherical titanium dioxide composite nanoparticles, characterized in that the diameter of the composite nanoparticles is 0.01 to 10 μm.
3. In paragraph 1, Spherical titanium dioxide composite nanoparticles characterized in that the composite nanoparticles include a rutile crystal structure.
4. In paragraph 1, A spherical titanium dioxide composite nanoparticle characterized in that a portion of the oxygen atoms (O) chemically bonded with the titanium atoms (Ti) chemically bonds with the silicon atoms (Si).
5. In paragraph 4, A spherical titanium dioxide composite nanoparticle characterized in that the chemical bond is at least one of a covalent bond and an ionic bond.
6. A sunscreen, a paint, a material for solar cells, and a catalyst for water decomposition comprising spherical titanium dioxide composite nanoparticles according to Article 1. 7.(a) A step of preparing a mixture comprising a solvent, a titanium dioxide precursor and a silica precursor; (b) a step of subjecting the mixture to a sol-gel reaction; and (c) a step of heat-treating the result of the sol-gel reaction to produce spherical titanium dioxide composite nanoparticles containing a compound represented by the chemical formula 1 below; A method for producing spherical titanium dioxide composite nanoparticles comprising: [Chemical Formula 1] Of x To 1-x O2 In the above chemical formula 1, x is 0.5 <x<1이다.
8. In paragraph 7, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that a portion of the oxygen atoms (O) chemically bonded with the titanium atoms (Ti) chemically bonds with the silicon atoms (Si).
9. In paragraph 8, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the chemical bond is at least one of a covalent bond and an ionic bond.
10. In paragraph 7, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the solvent comprises a polar aprotic solvent, a C1 to C4 alcohol, and water.
11. In paragraph 10, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the polar aprotic solvent comprises at least one selected from the group consisting of acetonitrile, acetone, dimethylformamide, dimethylsulfoxide, ethyl acetate, dichloromethane, and dimethylacetamide.
12. In paragraph 10, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the C1 to C4 alcohol comprises at least one selected from the group consisting of methanol, ethanol, n-propanol, isopropanol, and butanol.
13. In paragraph 7, The above titanium dioxide precursor is titanium isopropoxide (C 12 H 28 O4Ti), titanium tetrachloride (TiCl4), titanium butoxide (C 16 H 36 O4Ti), titanium methoxide (C4H 12 O4Ti) and titanium ethoxide (C8H 24 A method for producing spherical titanium dioxide composite nanoparticles, characterized in that it comprises at least one selected from the group consisting of O4Ti).
14. In paragraph 7, The above silica precursor is tetraethoxysilane (TEOS), tetramethyl orthosilicate, tetrapropyl orthosilicate, methyl triethyl orthosilicate, dimethyldiethyl orthosilicate, tetraisopropyl orthosilicate, tetrabutyl orthosilicate, tetrasecondarybutyl orthosilicate, tetratertiarybutyl orthosilicate, tetrahexyl orthosilicate, tetracyclohexyl orthosilicate. A method for producing spherical titanium dioxide composite nanoparticles, characterized in that it comprises at least one selected from the group consisting of tetradodecyl orthosilicate and tetradodecyl orthosilicate.
15. In paragraph 7, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the ratio of the number of moles of the silica precursor to the total number of moles of the titanium dioxide precursor (A) and the number of moles of the silica precursor (B) (B / (A+B)x100) is 0.1 to 10 mol%.
16. In paragraph 7, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the mixture of the above (a) further contains an organic amine.
17. In paragraph 16, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the organic amine comprises at least one selected from the group consisting of dodecylamine, octadecylamine, hexadecylamine, propylamine, and butylamine.
18. In paragraph 16, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the organic amine is a compound represented by the chemical formula 2 below. [Chemical Formula 2] In the above chemical formula 2, R 1 This is a C2 to C18 alkylene group or a C2 to C18 alkenylene group.
19. In paragraph 7, The above step (a) (a-1) A step of mixing and stirring the solvent and the organic amine; (a-2) a step of mixing and stirring the titanium dioxide precursor and the silica precursor; and (a-3) A method for producing spherical titanium dioxide composite nanoparticles, characterized by comprising a step of adding the result of step (a-2) to the result of step (a-1) and mixing to produce a mixture.
20. In paragraph 7, A method for producing spherical titanium dioxide composite nanoparticles, characterized in that the heat treatment in the above step (c) is performed at 700 to 1,000°C.
Citation Information
Patent Citations
Method for preparing titania microspheres with high refractive index
KR1020130051229A
A device that sterilizes and cleans air