Releasable composition for coating protection

The peelable composition for coating film protection, using a combination of amino-modified fatty acid-based release agents and zinc oxide curing agents in acrylic emulsions, addresses the environmental concerns and adhesion issues of conventional coatings, providing a durable, easily removable, and environmentally friendly solution for protecting painted surfaces.

WO2024225614A1PCT designated stage expired Publication Date: 2024-10-31KCC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003323
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional coating compositions for protecting painted surfaces of automobiles and heavy equipment face issues with environmental pollution due to the use of petroleum-based solvents and alkaline detergents, and they lack a peelable and easily removable solution with excellent adhesion and resistance to contaminants.

Method used

A peelable composition comprising a first acrylic emulsion with an amino-modified fatty acid-based release agent and a second acrylic emulsion with a zinc oxide curing agent, which provides excellent adhesion, water resistance, chemical resistance, and tensile strength, and can be easily removed without leaving residue, using water as the solvent to minimize environmental impact.

Benefits of technology

The composition ensures effective protection against external contaminants and physical trauma, with improved drying speed, crosslinking density, and surface tension for appropriate adhesion, while being environmentally friendly and easy to apply and remove, maintaining the appearance and mechanical properties of the painted surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024003323-APPB-IMG-000001
    Figure PCTKR2024003323-APPB-IMG-000001
  • Figure PCTKR2024003323-APPB-IMG-000002
    Figure PCTKR2024003323-APPB-IMG-000002
  • Figure PCTKR2024003323-APPB-IMG-000003
    Figure PCTKR2024003323-APPB-IMG-000003
Patent Text Reader

Abstract

The present invention relates to a releasable composition for coating protection and a coating protection film manufactured therefrom, the releasable composition comprising a first acrylic emulsion and a second acrylic emulsion, wherein the first acrylic emulsion contains an amino-modified fatty acid-based release agent, and the second acrylic emulsion contains a zinc oxide (ZnO) curing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Peelable composition for coating protection

[0001] The present invention relates to a peelable composition for temporarily protecting the painted surface of an automobile or heavy equipment, etc., and for protecting a paint film that is easy to peel and has excellent adhesive strength.

[0002] Automobiles and heavy equipment, etc., are often temporarily stored outdoors or transported before reaching their final destination. During this time, they are susceptible to damage, stains, discoloration, and contamination of their painted surfaces due to contaminants such as sand, dust, iron, salts, alkalis, acids, exhaust fumes, insect waste, or bodily fluids, as well as sunlight, wind, rain, and other factors. Furthermore, physical damage can also occur to the material.

[0003] Therefore, many peelable coating compositions have been proposed that can be applied to the surface of a vehicle or heavy equipment in advance at the product shipment stage to temporarily protect the surface from contaminants, sunlight, wind and rain, trauma, etc., and can be easily peeled off after a certain period of storage.

[0004] However, conventional coating compositions require the use of petroleum-based solvents for removal, leading to environmental issues such as air pollution. Furthermore, compositions based on alkaline-soluble resins are also being used, but the use of alkaline detergents during removal poses environmental problems such as water contamination.

[0005] Therefore, there is a need to develop a peelable composition for coating protection that is easy to peel and has excellent adhesive strength to protect the coating surface of automobiles or heavy equipment.

[0006] [Prior Art Literature]

[0007] (Patent Document 1) Republic of Korea Patent No. 10-0498717 (June 22, 2005)

[0008] In one aspect, the present invention aims to provide a peelable composition for protecting a coating surface of an automobile or heavy equipment, which is easy to peel and has excellent adhesive strength.

[0009] In another aspect, the present invention provides a coating protection film manufactured from a peelable composition for coating protection that is easy to peel and has excellent adhesive strength for protecting a coating surface of an automobile or heavy equipment, etc.

[0010] In one aspect, the present invention provides a strippable composition for protecting a coating film, comprising a first acrylic emulsion and a second acrylic emulsion, wherein the first acrylic emulsion comprises an amino-modified fatty acid-based release agent, and the second acrylic emulsion comprises a zinc oxide (ZnO) curing agent.

[0011] In another aspect, the present invention provides a coating protection film manufactured by curing a peelable composition for coating protection according to the present invention.

[0012] A peelable composition for film protection according to one aspect of the present invention is characterized by a fast drying speed, excellent initial adhesion and excellent adhesion retention, the film can be removed cleanly, leaves no residue after removal, and has excellent water resistance, chemical resistance, and tensile strength.

[0013] The present invention is described in detail below with reference to examples. However, the present invention is not limited to the following description, and each component may be modified or selectively mixed as needed. Therefore, it should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are included.

[0014] The “glass transition temperature” used herein is measured by a conventional method known in the art, and can be measured by, for example, thermomechanical analysis (TMA) or differential scanning calorimetry (DSC).

[0015] “Weight average molecular weight” is measured by a conventional method known in the art, and can be measured by, for example, the GPC (gel permeation chromatography) method.

[0016] Functional values ​​such as “acid value” and “hydroxyl value” can be measured by conventional methods known in the relevant technical field, and can represent values ​​measured by, for example, a titration method.

[0017] “Particle diameter (D50)” is measured by a conventional method known in the art, and can be measured, for example, by laser light scattering (LLS).

[0018] Additionally, “viscosity” is measured by a conventional method known in the art, and can be measured, for example, using a Brookfield viscometer (rotating spindle viscometer) at room temperature (25°C).

[0019] <Peeling-capable composition for coating protection>

[0020] In one aspect, the present invention can provide a peelable composition for protecting a coating surface of an automobile or heavy equipment, which does not react with a body coating, is easy to peel, and has excellent adhesive strength.

[0021] A peelable composition for film protection according to one embodiment of the present invention comprises a first acrylic emulsion and a second acrylic emulsion.

[0022] The first acrylic emulsion of the present invention includes an amino-modified fatty acid-based release agent, and the second acrylic emulsion includes a zinc oxide (ZnO) curing agent.

[0023] When the peelable composition for protecting a coating film of the present invention comprises a first acrylic emulsion containing an amino-modified fatty acid-based release agent and a second acrylic emulsion containing a zinc oxide (ZnO) curing agent and has properties within a specific range described below, the drying speed and crosslinking density of the film are controlled to improve not only the appearance characteristics of the film but also mechanical properties such as water resistance and solvent resistance, and the surface tension of the composition is controlled to have appropriate adhesion without reacting with the body coating film, thereby having the effect of protecting the coating film.

[0024] The peelable composition for film protection of the present invention may further include one or more additives selected from the group consisting of a neutralizing agent, a dispersing agent, a release agent, an antifreeze agent, an antifoaming agent, and a thickener.

[0025] Below, the above components are described in detail.

[0026] 1st acrylic emulsion

[0027] The first acrylic emulsion serves as a main resin of a peelable composition for film protection, improving storage properties and water resistance, and securing strength, elongation, and adhesiveness of a film protection film manufactured therefrom.

[0028] The first acrylic emulsion may be directly synthesized according to a known method, or a commercially available product may be used. For example, the first acrylic emulsion includes units derived from one or more monomers selected from the group consisting of ethyl acrylate (EA), hydroxyethyl acrylate (HEA), butyl acrylate (BA), methyl methacrylate (MMA), ethyl methacrylate (EMA), butyl methacrylate (BMA), hydroxyethyl methacrylate (HEMA), allyl methacrylate (AMA), acrylic acid (AA), and methacrylic acid (MAA), and units derived from an acrylonitrile (AN) monomer. As another example, the first acrylic emulsion may be prepared from a mixture including n-butyl methacrylate (n-BMA), methyl methacrylate (MMA), butyl acrylate (BA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA), and acrylonitrile (AN) as monomers.

[0029] Here, the first acrylic emulsion contains 30 to 50 parts by weight, or 35 to 45 parts by weight, of acrylonitrile monomer based on 100 parts by weight of the total monomer content contained in the first acrylic emulsion. When the content of the acrylonitrile monomer contained in the first acrylic emulsion is within the above range, the curing density is appropriate, so that the film has excellent peel strength and tensile strength. When it exceeds the above range, the film adhesion may increase, so that the peel strength may increase, and when it is below the above range, the curing density may decrease, which may affect the chemical resistance and water resistance of the film.

[0030] The first acrylic emulsion includes an amino-modified fatty acid-based release agent. When the amino-modified fatty acid-based release agent is included, the release effect is enhanced due to the flexibility of the amino-modified functional group, thereby providing an appropriate film peel strength and adhesion, and improving the problem of the appearance becoming opaque and hazy when a silicone-based release agent is used. In particular, when the amino-modified fatty acid-based release agent is included in the first acrylic emulsion, compared to when it is included only in a peelable composition for film protection, it is dispersed at an appropriate temperature of 40°C or lower, thereby preventing the problem of poor appearance, and the dispersibility is improved, thereby maximizing the release effect.

[0031] The first acrylic emulsion contains 1 to 5 parts by weight, or 2 to 4 parts by weight, of an amino-modified fatty acid-based release agent based on 100 parts by weight of the total monomer content of the first acrylic emulsion. When the content of the amino-modified fatty acid-based release agent contained in the first acrylic emulsion is within the above range, there is an advantage of having appropriate film adhesion and peel strength. When it exceeds the above range, the release property is good, but the film peel strength is low, but the adhesion may be poor, and when it is below the above range, the adhesion to the coating film is good, but the peeling property may be poor.

[0032] Specifically, the amino-modified fatty acid-based release agent that can be used in the present invention may be ADDITOL® XL 6568, available from Allnex.

[0033] The first acrylic emulsion contains a solid content of 40 to 50 wt%, or 43 to 47 wt%, based on the total weight of the first acrylic emulsion. When the solid content of the first acrylic emulsion is within the above range, excellent workability is achieved.

[0034] The first acrylic emulsion may have a viscosity at 25°C of 30 to 200 cps, or 40 to 150 cps. When the viscosity at 25°C of the first acrylic emulsion is within the above range, the viscosity of the peelable composition for film protection is appropriate, thereby improving workability. When the viscosity at 25°C of the first acrylic emulsion is outside the above range, the workability of the composition may be insufficient, resulting in a problem of deterioration in the appearance characteristics of the produced film.

[0035] The first acrylic emulsion may have an acid value (Av) of 1 to 10 mgKOH / g, or 3 to 8 mgKOH / g. When the acid value of the first acrylic emulsion is within the above range, the reactivity of the composition containing it can be adjusted to improve the appearance properties of the film manufactured therefrom. When the acid value of the first acrylic emulsion is below the above range, the resin stability may be lowered, which may cause a problem of lowering the storability of the peelable composition. When the acid value exceeds the above range, the viscosity of the composition may be increased due to increased resin cohesion, which may cause a problem of lowering the workability and water resistance of the film.

[0036] The first acrylic emulsion may have a pH of 7 to 10, or 8 to 10. When the pH of the first acrylic emulsion is within the above range, the viscosity of the peelable composition for film protection is appropriate, thereby improving workability and storability. When the pH of the first acrylic emulsion is outside the above range, the viscosity of the composition is low, resulting in insufficient workability, which may cause a problem of deterioration in the appearance characteristics of the produced film.

[0037] The first acrylic emulsion may have a glass transition temperature (Tg) of -15 to 20°C, or -10 to 10°C. When the glass transition temperature of the first acrylic emulsion is within the above range, it has an effect of having appropriate adhesion without reacting with the body coating, and improving the hardness and solvent resistance of the film. When the glass transition temperature of the first acrylic emulsion is below the above range, the drying speed and crosslinking density of the film may decrease, which may cause a problem in that the hardness and solvent resistance of the manufactured film may be insufficient, and when it exceeds the above range, the film may become brittle, which may result in deterioration of the appearance characteristics and elongation of the manufactured film.

[0038] The first acrylic emulsion may have a weight average molecular weight (Mw) of 100,000 to 200,000 g / mol, or 120,000 to 180,000 g / mol. When the weight average molecular weight of the first acrylic emulsion is within the above range, the long-term physical properties of the manufactured film, such as durability, adhesion, and weather resistance, may be excellent. When the weight average molecular weight of the first acrylic emulsion is less than the above range, the molecular weight is small, so that the water resistance and weather resistance of the manufactured film are insufficient, and when the weight average molecular weight exceeds the above range, the flowability is reduced due to the increase in molecular weight, so that the workability of the peelable composition for film protection containing the same is poor, and the surface smoothness is poor, which may affect the appearance.

[0039] The first acrylic emulsion may be in the form of an emulsion dispersed in deionized water. The first acrylic emulsion may have particles dispersed in the deionized water having an average diameter of 100 to 200 nm, or 130 to 170 nm. When the first acrylic emulsion is in the form of an emulsion dispersed in deionized water, it has the effect of reducing the volatile organic compound (VOC) content of the peelable composition, and when the average particle diameter is within the above range, the appearance and particle stability are good.

[0040] The first acrylic emulsion may be included in the composition in an amount of 60 to 70 wt%, or 61 to 68 wt%, based on the total weight of the peelable composition for film protection. When the first acrylic emulsion is included within the above content range, it has the effect of improving the peel strength and elongation of the film. When the content of the first acrylic emulsion is less than the above range, there is a problem that the peel strength and elongation of the film are lowered, and when it exceeds the above range, there may be problems with the chemical resistance and water resistance of the film.

[0041] Second acrylic emulsion

[0042] The second acrylic emulsion is identical to the first acrylic emulsion except as described below.

[0043] The second acrylic emulsion is an auxiliary resin of a peelable composition for film protection and serves to secure the tensile strength and drying properties of the film protection film produced therefrom.

[0044] In one embodiment, the second acrylic emulsion can be prepared from a mixture comprising n-butyl methacrylate (n-BMA), methyl methacrylate (MMA), acrylic acid (AA), and hydroxyethyl methacrylate (HEMA) as monomers.

[0045] Here, the second acrylic emulsion, unlike the first acrylic emulsion, does not contain butyl acrylate (BA), acrylonitrile (AN), or a release agent.

[0046] On the other hand, the second acrylic emulsion contains 5 to 20 parts by weight, or 10 to 15 parts by weight, of a zinc oxide (ZnO) curing agent based on 100 parts by weight of the total monomer content of the second acrylic emulsion. When the zinc oxide curing agent is included in the second acrylic emulsion, the acid group of the acrylic emulsion has an anionic charge, and the zinc oxide has a cationic charge, so that an ionic bond is formed, thereby improving the tensile strength and mechanical properties of the manufactured film. When the content of the zinc oxide (ZnO) curing agent included in the second acrylic emulsion is within the above range, the curing density is increased, thereby improving the chemical resistance and water resistance of the film. When it exceeds the above range, the zinc oxide may remain without reacting, which may deteriorate the appearance of the film, and when it is below the above range, the curing density may decrease, which may affect the chemical resistance and water resistance of the film.

[0047] The second acrylic emulsion may have a viscosity at 25°C of 150 to 500 cps, or 150 to 250 cps. When the viscosity at 25°C of the second acrylic emulsion is within the above range, the viscosity of the peelable composition for film protection is appropriate, thereby improving workability. When the viscosity at 25°C of the second acrylic emulsion is outside the above range, the workability of the composition may be insufficient, resulting in a problem of deterioration in the appearance properties of the manufactured film.

[0048] The second acrylic emulsion may have a glass transition temperature (Tg) of 40 to 60°C, or 45 to 55°C. When the glass transition temperature of the second acrylic emulsion is within the above range, it has an effect of having appropriate adhesion without reacting with the body coating, and improving the tensile strength of the film. When the glass transition temperature of the second acrylic emulsion is below the above range, the drying speed and crosslinking density of the film may decrease, which may cause problems in that the hardness and solvent resistance of the manufactured film may be insufficient, and when it exceeds the above range, the coating may become brittle, which may cause the appearance characteristics, tensile strength, and elongation of the manufactured film to be insufficient.

[0049] The second acrylic emulsion may have a weight average molecular weight (Mw) of 200,000 to 300,000 g / mol, or 220,000 to 280,000 g / mol. When the weight average molecular weight of the second acrylic emulsion is within the above range, the manufactured film may have excellent long-term physical properties such as durability, adhesion, and weather resistance. When the weight average molecular weight of the second acrylic emulsion is less than the above range, the molecular weight is small, so that the manufactured film has insufficient water resistance and weather resistance, and when it exceeds the above range, the flowability decreases due to the increase in molecular weight, so that the workability of the peelable composition for protecting a coating film including the same is poor, and the surface smoothness is poor, which may cause a problem of deteriorating the appearance.

[0050] The second acrylic emulsion may be in the form of an emulsion dispersed in deionized water. The second acrylic emulsion may have particles dispersed in the deionized water having an average diameter of 150 to 200 nm, or 160 to 190 nm. When the second acrylic emulsion is in the form of an emulsion dispersed in deionized water, it has the effect of reducing the volatile organic compound (VOC) content of the peelable composition, and when the average particle diameter is within the above range, the appearance and particle stability are good.

[0051] The second acrylic emulsion contains a solid content of 40 to 50 wt%, or 43 to 47 wt%, based on the total weight of the second acrylic emulsion. When the solid content of the second acrylic emulsion is within the above range, it has an excellent workability effect.

[0052] The second acrylic emulsion may have an acid value (Av) of 1 to 10 mgKOH / g, or 3 to 8 mgKOH / g. When the acid value of the second acrylic emulsion is within the above range, the reactivity of the composition containing it can be adjusted to improve the appearance properties of the film manufactured therefrom. When the acid value of the second acrylic emulsion is below the above range, the resin stability may be lowered, which may cause a problem of lowering the storability of the peelable composition. When the acid value exceeds the above range, the viscosity of the composition may be increased due to increased resin cohesion, which may cause a problem of lowering the workability and water resistance of the film.

[0053] The second acrylic emulsion may have a pH of 7 to 10, or 8 to 10. When the pH of the second acrylic emulsion is within the above range, the viscosity of the peelable composition for film protection is appropriate, thereby improving workability and storability. When the pH of the second acrylic emulsion is outside the above range, the viscosity of the composition is low, resulting in insufficient workability, which may cause a problem of deterioration in the appearance characteristics of the produced film.

[0054] The second acrylic emulsion may be included in the composition in an amount of 25 to 34 wt%, or 25 to 32 wt%, based on the total weight of the peelable composition for film protection. When the second acrylic emulsion is included within the above content range, it has the effect of improving the tensile strength, peel strength, water resistance, and elongation of the film. When the content of the second acrylic emulsion is less than the above range, the crosslinking density of the film decreases, which may cause problems such as lowering the tensile strength, chemical resistance, and water resistance, and when it exceeds the above range, drying may proceed quickly, resulting in insufficient workability, which may cause problems such as lowering the appearance and tensile strength of the film, and increasing the amount of residue after film detachment.

[0055] When the mixing ratio of the first acrylic emulsion and the second acrylic emulsion falls within the above-mentioned range, the film can be cleanly removed without residue after removal by maintaining appropriate drying properties and having appropriate adhesion to the body coating.

[0056] solvent

[0057] The solvent is water, which can be ion-exchanged water, distilled water, or ultrapure deionized water.

[0058] The water solvent may be included in each acrylic emulsion in an amount of 20 to 40 wt% based on the total weight of each emulsion during the preparation of the first and second acrylic emulsions.

[0059] Meanwhile, when preparing a peelable composition for film protection, the water solvent may be included in an amount of 0.1 to 10 wt%, or 0.3 to 3 wt%, based on the total weight of the peelable composition for film protection. When used within the above range, viscosity control can be facilitated, and the smoothness and workability of the film protection film using the peelable composition for film protection can be excellent.

[0060] additives

[0061] The peelable composition for film protection of the present invention may include one or more additives selected from the group consisting of a neutralizing agent, a dispersing agent, a release agent, an antifreeze agent, an antifoaming agent, and a thickener.

[0062] Additives may be added to a peelable composition for film protection in a predetermined content range for the purpose of providing additional effects such as improving wettability and leveling properties during painting.

[0063] Based on the total weight of the strippable composition for coating protection, the neutralizer may be included in an amount of 0.1 to 2 wt% or 0.1 to 1 wt%, the antifreeze may be included in an amount of 0.1 to 5 wt% or 0.3 to 3 wt%, the defoaming agent may be included in an amount of 0.1 to 3 wt% or 0.3 to 2 wt%, the thickener may be included in an amount of 0.1 to 3 wt% or 0.3 to 2 wt%, the release agent may be included in an amount of 0.1 to 5 wt% or 0.3 to 3 wt%, and the dispersing agent may be included in an amount of 0.1 to 2 wt% or 0.1 to 1 wt%.

[0064] Here, the release agent is included in the peelable composition for film protection separately from the release agent included in the first acrylic emulsion.

[0065] <Screen protection film>

[0066] In another aspect, the present invention can provide a coating protection film manufactured from a peelable composition for coating protection that is easy to peel and has excellent adhesive strength to protect the coating surface of an automobile or heavy equipment, etc.

[0067] The coating protective film of the present invention can be manufactured by curing the peelable composition for coating protective film of the present invention.

[0068] Specifically, the peelable composition for film protection of the present invention can be applied to a thickness of 10 to 100 μm on a conductor by spraying, brushing, or roller, and then cured by drying at room temperature, curing in an oven, or curing with an IR lamp, etc., to form a film protection film.

[0069] <Experimental Example>

[0070] Hereinafter, the present invention will be described in more detail through experimental examples.

[0071] In the present invention, experimental examples include working examples and comparative examples, and the experimental examples are only intended to help understand the present invention and do not limit the scope of the present invention in any way.

[0072] Preparation of first and second acrylic emulsions

[0073] The first and second acrylic emulsions were prepared according to the following procedure with the compositions shown in Table 1.

[0074] 1) Place PART1 in the reactor and heat to 80℃.

[0075] 2) PART3 Mix in advance to make a pre-emulsion.

[0076] 3) When the temperature reaches 80℃, add 10% of the pre-emulsion and maintain for 10 minutes.

[0077] 4) PART2: Keep for 10 minutes after adding.

[0078] 5) Add the rest of PART3 for 30 minutes and then maintain for 30 minutes.

[0079] 6) After adding PART4, keep for 30 minutes.

[0080] 7) After cooling to below 40℃, add PART5 and keep for 10 minutes.

[0081] 8-1) For the second acrylic emulsion: Add PART6 at 40℃ or lower and maintain for 30 minutes.

[0082] 8-2) For the first acrylic emulsion: After adding PART7, keep for 30 minutes.

[0083]

[0084] Specific ingredients used in the preparation of the first and second acrylic emulsions in Table 1 are shown in Table 2 below.

[0085]

[0086] Manufacturing of a peelable composition for coating protection

[0087] A peelable composition for film protection was manufactured by sequentially adding solvent and additives while stirring after adding the first and second acrylic emulsions manufactured previously, according to the compositions shown in Tables 3 and 4 below.

[0088]

[0089]

[0090] Specific ingredients used in the preparation of the peelable compositions for film protection of Tables 3 and 4 are shown in Table 5 below.

[0091]

[0092] Formation of a protective film on the coating

[0093] A peelable composition for coating protection, manufactured by mixing the compositions in Tables 3 and 4, was applied to a substrate coated with automotive clear paint by spraying at a coating thickness of 50 μm, and then cured at 80°C for 3 minutes to form a coating protection film.

[0094] Physical property evaluation

[0095] The physical properties of the manufactured coating protective film were evaluated using the method below, and the results are shown in Tables 6 and 7.

[0096] 1) Peel strength: The adhesive strength and peel performance were evaluated by measuring the force when peeling the film. A film measuring 25 mm x 50 mm (width x length) and 50 μm in thickness was cured at 80°C for 3 minutes and measured 24 hours later. The measurement was made using a UTM (Universal Testing Machine) at a tensile speed of 300 mm / min and a peel direction of 180 degrees. A peel strength of 0.6 to 2.0 N was evaluated as good.

[0097] 2) Tensile strength: The tensile strength, which is the toughness and toughness of the film, was measured. A film with a size of 25 mm x 50 mm (width x length) and a film thickness of 50 μm was measured using a UTM (Universal Testing Machine) at 23°C and RH 65%. Wmax / A0 (Wmax: maximum tensile load, A0: cross-sectional area). A tensile strength of 10 N or more was evaluated as good.

[0098] 3) Elongation: The elongation, which is the extent to which the film stretches, was measured. A film measuring 25 mm x 50 mm (width x length) and 50 μm thick was measured using a UTM (Universal Testing Machine) at 23°C and RH 65%.

[0099] (L-L0)x100 / L0.(L: length before film breaks, L O :initial length of the film)

[0100] If the elongation rate is 200% or higher, it is evaluated as good.

[0101] 4) Water resistance: Measured after 100 hours at 50℃, RH 98% and 1 hour at room temperature. If there is no residue, discoloration, foreign texture, or appearance abnormality on the adherend after film removal, and there is no breakage of the film, it is evaluated as good.

[0102] 5) Chemical resistance: After dropping 0.5 mL of gasoline, the appearance was measured at 70℃ for 3 hours. If there were no abnormalities in appearance, such as discoloration or swelling, on the painted surface after removing the film, it was evaluated as good.

[0103]

[0104]

[0105] As shown in Tables 6 and 7, the coating protective film had good properties in Experimental Examples 1 to 3, somewhat inferior properties in Experimental Examples 4 and 5, and inferior properties in Experimental Examples 6 to 16. Specifically, Experimental Example 6, in which the content of acrylonitrile monomer in the first acrylic emulsion was less than the content of acrylonitrile monomer, was inferior in tensile strength, elongation, chemical resistance and water resistance, Experimental Example 7, in which the content of acrylonitrile monomer in the first acrylic emulsion was greater than the content of acrylonitrile monomer, was inferior in peelability, Experimental Example 8, in which the second acrylic emulsion did not contain a zinc oxide hardener, was inferior in tensile strength, elongation, chemical resistance and water resistance, Experimental Example 9, in which the content of a zinc oxide hardener in the second acrylic emulsion was greater than the content of acrylonitrile monomer, was inferior in elongation and chemical resistance, Experimental Example 10, in which the glass transition temperature of the first acrylic emulsion was less than the range and Experimental Example 11, in which the glass transition temperature of the first acrylic emulsion was greater than the range, were inferior in at least one property in tensile strength, elongation or water resistance, and Experimental Example 12, in which the first acrylic emulsion did not contain an amino-modified fatty acid-based release agent and Experimental Example 13, in which the content was greater than the content of a release agent in the first acrylic emulsion, was inferior in peelability or The peel strength was low, so the adhesion was poor. Experimental example 14, which did not use the second acrylic emulsion but used one type of acrylic emulsion, had poor chemical resistance and water resistance. Experimental example 15, which did not use the first acrylic emulsion but used one type of acrylic emulsion, had poor adhesion and tensile strength. Experimental example 16, which used an acrylic emulsion that did not contain an amino-modified fatty acid-based release agent or a zinc oxide hardener, had poor adhesion and chemical resistance.

[0106] Hereinafter, various embodiments of the present invention will be described.

[0107] (1) A peelable composition for protecting a coating film, comprising a first acrylic emulsion and a second acrylic emulsion, wherein the first acrylic emulsion comprises an amino-modified fatty acid-based release agent, and the second acrylic emulsion comprises a zinc oxide (ZnO) curing agent.

[0108] (2) A peelable composition for protecting a coating film, wherein the first acrylic emulsion comprises 30 to 50 parts by weight of an acrylonitrile monomer and 1 to 5 parts by weight of an amino-modified fatty acid-based release agent based on 100 parts by weight of the total amount of monomers contained in the first acrylic emulsion.

[0109] (3) A peelable composition for protecting a coating film, wherein the second acrylic emulsion contains 5 to 20 parts by weight of a zinc oxide (ZnO) hardener based on 100 parts by weight of the total amount of monomers contained in the second acrylic emulsion.

[0110] (4) A peelable composition for protecting a coating film, wherein the first acrylic emulsion has a glass transition temperature (Tg) of -15 to 20°C, a solid content of 40 to 50 wt% based on the total weight of the first acrylic emulsion, a viscosity at 25°C of 30 to 200 cPs, an acid value of 1 to 10 mgKOH / g, a pH of 7 to 10, a weight average molecular weight (Mw) of 100,000 to 200,000 g / mol, and an average particle diameter of 100 to 200 nm.

[0111] (5) A peelable composition for protecting a coating film, wherein the second acrylic emulsion has a glass transition temperature (Tg) of 40 to 60°C, a solid content of 40 to 50 wt% based on the total weight of the second acrylic emulsion, a viscosity at 25°C of 150 to 500 cPs, an acid value of 1 to 10 mgKOH / g, a pH of 7 to 10, a weight average molecular weight (Mw) of 200,000 to 300,000 g / mol, and an average particle diameter of 150 to 200 nm.

[0112] (6) A peelable composition for film protection, comprising 60 to 70 wt% of a first acrylic emulsion and 25 to 34 wt% of a second acrylic emulsion based on the total weight of the peelable composition for film protection.

[0113] (7) A coating protection film manufactured by curing a peelable composition for coating protection according to the present invention.

Claims

1. Contains a first acrylic emulsion and a second acrylic emulsion, The first acrylic emulsion contains an amino-modified fatty acid-based release agent, A second acrylic emulsion is a peelable composition for protecting a coating film, comprising a zinc oxide (ZnO) curing agent.

2. In claim 1, A peelable composition for protecting a coating film, wherein the first acrylic emulsion comprises 30 to 50 parts by weight of an acrylonitrile monomer and 1 to 5 parts by weight of an amino-modified fatty acid-based release agent based on 100 parts by weight of the total amount of monomers contained in the first acrylic emulsion.

3. In claim 1, A second acrylic emulsion is a peelable composition for protecting a coating film, comprising 5 to 20 parts by weight of a zinc oxide (ZnO) hardener based on 100 parts by weight of the total amount of monomers contained in the second acrylic emulsion.

4. In claim 1, A peelable composition for protecting a coating film, wherein the first acrylic emulsion has a glass transition temperature (Tg) of -15 to 20°C, a solid content of 40 to 50 wt% based on the total weight of the first acrylic emulsion, a viscosity at 25°C of 30 to 200 cPs, an acid value of 1 to 10 mgKOH / g, a pH of 7 to 10, a weight average molecular weight (Mw) of 100,000 to 200,000 g / mol, and an average particle diameter of 100 to 200 nm.

5. In claim 1, A peelable composition for protecting a coating film, wherein the second acrylic emulsion has a glass transition temperature (Tg) of 40 to 60°C, a solid content of 40 to 50 wt% based on the total weight of the second acrylic emulsion, a viscosity at 25°C of 150 to 500 cPs, an acid value of 1 to 10 mgKOH / g, a pH of 7 to 10, a weight average molecular weight (Mw) of 200,000 to 300,000 g / mol, and an average particle diameter of 150 to 200 nm.

6. In claim 1, A peelable composition for film protection, comprising 60 to 70 wt% of a first acrylic emulsion and 25 to 34 wt% of a second acrylic emulsion, based on the total weight of the peelable composition for film protection.

Citation Information

Patent Citations

  • Aqueous strippable paint

    JP1985161465A

  • Releasable film

    JP2019209675A

  • Thermosetting release coating agent and laminate, and method for producing laminate

    JP2021098845A

  • Removable pressure-sensitive adhesive composition, removable pressure-sensitive adhesive layer, and removable pressure-sensitive adhesive sheet

    KR1020130031216A

  • Acrylic adhesive sheet, adhesive tape for medical treatment and method of producing the same

    KR1020160077753A