Molded article comprising thermoplastic continuous fiber reinforced woven composite, and method for manufacturing same
The thermoplastic continuous fiber reinforced woven body, incorporating a glass fiber composite material with polypropylene resin and flame retardants, addresses the challenge of balancing lightweight, flame retardant, and aesthetic properties in molded products, specifically for electric vehicle battery modules, by using a laminated structure with a non-woven fabric to improve appearance and structural integrity.
Patent Information
- Application Number
- PCT/KR2024/004902
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-31
AI Technical Summary
Thermoplastic continuous fiber reinforced woven materials for molded products, such as electric vehicle battery module protective plates, offer improved flame retardancy, impact resistance, and rigidity but lack desirable appearance characteristics due to protruding fibers and require a solution that balances lightweight properties with aesthetic appeal.
A molded article comprising a thermoplastic continuous fiber reinforced woven body, made by laminating two or more thermoplastic continuous fiber reinforced woven materials with a non-woven fabric, using a glass fiber composite material containing polypropylene resin, piperazine pyrophosphate, phosphazene compound, and zeolite, which are impregnated into tape-shaped glass fibers, and applying a polyethylene terephthalate non-woven fabric to enhance bonding and appearance.
The solution provides a molded article with excellent lightweight properties, flame retardancy, impact resistance, rigidity, and appearance characteristics, meeting the demands for weight reduction and eco-friendliness in the automotive industry while maintaining structural integrity and aesthetic appeal.
Smart Images

Figure KR2024004902_31102024_PF_FP_ABST
Abstract
Description
Molded article comprising thermoplastic continuous fiber reinforced woven fabric and method for manufacturing the same
[0001] The present invention relates to a molded article comprising a thermoplastic continuous fiber-reinforced woven fabric and a method for manufacturing the same. More specifically, the present invention relates to a molded article comprising a thermoplastic continuous fiber-reinforced woven fabric having excellent properties such as lightness, flame retardancy, impact resistance, rigidity, and appearance, and a method for manufacturing the same.
[0002]
[0003] To meet the automotive industry's ever-increasing demand for lightweight and eco-friendly solutions, automotive components are becoming increasingly lightweight, employing plastics instead of metals. There's a strong trend toward eliminating environmentally harmful substances like thermosetting resins and adopting thermoplastics, particularly polypropylene (PP). In particular, technological developments to reduce the weight of electric vehicle components are driving the need for changes in materials, such as the lower protective plates of battery modules for electric vehicles.
[0004] However, when thermoplastic resins are used as materials (such as continuous fiber-reinforced woven fabrics) for molded products (such as lower protective plates for battery modules for electric vehicles) for purposes such as weight reduction, there are problems such as reduced flame retardancy, impact resistance, and rigidity compared to metals or thermosetting resins. Furthermore, when these molded product materials are used alone, there are problems such as poor appearance characteristics, such as the protrusion of reinforcing fibers after molding.
[0005] Therefore, there is a need to develop a molded product that includes a thermoplastic continuous fiber reinforced woven fabric that has excellent properties such as lightness, flame retardancy, impact resistance, rigidity, and appearance, even when using a thermoplastic resin.
[0006] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2020-0033783, etc.
[0007]
[0008] The purpose of the present invention is to provide a molded product including a thermoplastic continuous fiber reinforced woven fabric having excellent properties such as lightness, flame retardancy, impact resistance, rigidity, and appearance.
[0009] Another object of the present invention is to provide a method for manufacturing the above-mentioned molded product.
[0010] The above and other objects of the present invention can all be achieved by the present invention described below.
[0011]
[0012] 1. One aspect of the present invention relates to a molded article. The molded article comprises a woven sheet in which two or more thermoplastic continuous fiber reinforced woven fabrics are laminated; and a nonwoven fabric laminated by heating and pressing on at least one side of the woven sheet; wherein the thermoplastic continuous fiber reinforced woven fabric is characterized in that it is woven using a glass fiber composite material including about 100 parts by weight of glass fiber; about 35 to about 72 parts by weight of polypropylene resin; about 12 to about 35 parts by weight of piperazine pyrophosphate; about 1 to about 20 parts by weight of a phosphazene compound; and about 1 to about 20 parts by weight of zeolite as warp and weft yarns.
[0013] 2. In the above 1 specific example, the polypropylene resin may include at least one of a homo polypropylene resin, a block polypropylene resin, and a random polypropylene resin.
[0014] 3. In the above two specific examples, the weight ratio of the piperazine pyrophosphate and the phosphazene compound may be about 1:0.1 to about 1:0.4.
[0015] 4. In the above 2 or 3 specific examples, the glass fiber composite material may be in the form of a tape in which the glass fiber is impregnated with the polypropylene resin, the piperazine pyrophosphate, the phosphazene compound, and the zeolite.
[0016] 5. In the above specific examples 1 to 4, the glass fiber composite material may be in the form of a tape having a thickness of about 0.2 to about 1.5 mm and a width of about 5 to about 25 mm.
[0017] 6. In the above 1 to 5 specific examples, the thermoplastic continuous fiber reinforced woven fabric may have a void space of about 5 mm × about 5 mm or less in size formed between the warp and warp yarns and between the weft and weft yarns.
[0018] 7. In the above specific examples 1 to 6, the nonwoven fabric may be a polyethylene terephthalate nonwoven fabric having a thickness of about 0.2 to about 1.5 mm.
[0019] 8. In the above 1 to 7 specific examples, the molded product has a density of about 1.40 to about 1.55 g / cm as measured according to ISO 1183-1. 3 It could be.
[0020] 9. In the above 1 to 8 specific examples, the molded product may have a flame retardancy of V-1 or higher on a 2 mm thick specimen measured by the UL-94 vertical test method.
[0021] 10. In the above specific examples 1 to 9, the molded product may have a peak force of about 3.5 to about 6.0 kN of a 60 mm × 60 mm × 2 mm specimen measured at a speed of 4.4 m / s and an impact energy value of 198 J based on a weight of 20 kg according to ISO 6603-2, a total displacement of about 20 to about 35 mm, and an energy absorption amount at a displacement value of 15 mm of about 30 to about 50 J.
[0022] 11. In the above 1 to 10 specific examples, the molded product may have a tensile strength of about 180 to about 270 MPa for a 3 mm thick specimen measured according to ISO 527, and a flexural strength of about 190 to about 280 MPa for a 3 mm thick specimen measured according to ISO 14125.
[0023] 12. In the above specific examples 1 to 11, the molded product may be extinguished naturally without catching fire in a long-term flame retardancy test in which a specimen measuring 330 mm × 330 mm × 2 mm is directly heated with a blue flame for 2 minutes and 10 seconds at a distance of 7 cm using a torch, and then the flame is removed.
[0024] 13. In the above specific examples 1 to 12, the molded product may be a lower protective plate of a battery module for an electric vehicle.
[0025] 14. Another aspect of the present invention relates to a method for manufacturing a molded article. The method comprises the steps of: laminating two or more thermoplastic continuous fiber reinforced woven fabrics, heating and compressing them to manufacture a woven sheet; and laminating a nonwoven fabric on at least one side of the woven sheet, followed by heating and compressing the same; wherein the thermoplastic continuous fiber reinforced woven fabric is characterized in that it is woven using a glass fiber composite material including about 100 parts by weight of glass fiber; about 35 to about 72 parts by weight of polypropylene resin; about 12 to about 35 parts by weight of piperazine pyrophosphate; about 1 to about 20 parts by weight of a phosphazene compound; and about 1 to about 20 parts by weight of zeolite as warp and weft yarns.
[0026]
[0027] The present invention has the effect of providing a molded article including a thermoplastic continuous fiber reinforced woven fabric having excellent lightness, flame retardancy, impact resistance, rigidity, appearance characteristics, etc., and a method for manufacturing the same.
[0028]
[0029] FIG. 1 is a plan view of a thermoplastic continuous fiber reinforced woven fabric according to one specific example of the present invention.
[0030]
[0031] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the following embodiments are provided to enable those skilled in the art to fully understand the present invention, and may be modified in various other forms, and the scope of the present invention is not limited to the embodiments described below.
[0032] In order to clearly express the components in the drawings, the sizes of the components, such as their widths and thicknesses, are somewhat enlarged. In addition, although only a portion of the components is illustrated for convenience of explanation, those skilled in the art will be able to easily understand the remaining portions of the components. Furthermore, those skilled in the art will be able to implement the concept of the present invention in various other forms without departing from the technical spirit of the present invention. Overall, the drawings have been described from the observer's perspective, and the terms "upper," "lower," "left," "right," "front," and "back" are based on the drawings. Furthermore, those skilled in the art will be able to implement the concept of the present invention in various other forms without departing from the technical spirit of the present invention. In addition, the same reference numerals in multiple drawings indicate substantially the same elements.
[0033] In addition, singular expressions should be understood to include plural expressions unless the context clearly indicates otherwise, and terms such as "comprises", "have", etc. should be understood to specify the presence of a described feature, number, step, operation, component, part, or combination thereof, but not to exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0034]
[0035] A molded article according to the present invention comprises (A) a woven sheet; and (B) a nonwoven fabric.
[0036] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.
[0037]
[0038] (A) Woven sheet
[0039] A woven sheet according to one specific example of the present invention is capable of improving the lightness, flame retardancy, impact resistance, rigidity, etc. of a molded product even when a thermoplastic resin is applied, and is in the form of two or more thermoplastic continuous fiber reinforced woven sheets laminated.
[0040] FIG. 1 is a plan view of a thermoplastic continuous fiber-reinforced woven fabric according to one embodiment of the present invention. As illustrated in FIG. 1, a thermoplastic continuous fiber-reinforced woven fabric (100) according to one embodiment of the present invention is a woven fabric woven using a tape-shaped glass fiber composite material as warp yarns (110) and weft yarns (120). Such a woven fabric can be manufactured using a known manufacturing method.
[0041] In a specific example, the thermoplastic continuous fiber reinforced woven fabric may have a void (130) of about 5 mm × about 5 mm or less in size formed between warp yarns (110) and warp yarns (110) and weft yarns (120). Within the above range, the void (gap) can be minimized during the manufacture of a molded product, and the thermoplastic continuous fiber reinforced woven fabric may have excellent moldability, flame retardancy, impact resistance, rigidity, etc.
[0042] In a specific example, the glass fiber composite material is a tape-shaped glass fiber composite material that has excellent lightness, flame retardancy, impact resistance, rigidity, etc., even when a thermoplastic resin is applied, and can improve the lightness, flame retardancy, impact resistance, rigidity, etc. of a thermoplastic continuous fiber reinforced woven fabric woven with weft and warp yarns, a woven sheet manufactured by laminating two or more sheets of the glass fiber composite material, and a molded product including the same. The glass fiber composite material includes (a) glass fiber; (b) polypropylene resin; (c) piperazine pyrophosphate; (d) phosphazene compound; and (e) zeolite.
[0043] (a) glass fiber
[0044] According to one specific example of the present invention, glass fiber is impregnated with polypropylene resin, piperazine pyrophosphate, phosphazene compound, and zeolite, thereby forming a tape-shaped glass fiber composite material having excellent lightness, flame retardancy, impact resistance, rigidity, etc.
[0045] In specific embodiments, the glass fibers may be in the form of fibers and may have various cross-sections such as circular, oval, rectangular, etc. For example, the use of fibrous glass fibers having circular and / or rectangular cross-sections may be preferable in terms of mechanical properties.
[0046] In a specific example, when the glass fiber has a circular cross-section, the diameter measured by a scanning electron microscope (manufacturer: JEOL, device name: JSM-6390A) may be about 5 to about 20 ㎛, for example, about 7 to about 15 ㎛, and when the glass fiber has a rectangular cross-section, the aspect ratio (major axis of the cross-section / minor axis of the cross-section) may be about 1.5 to about 10, for example, about 2 to about 8, and the minor axis of the rectangular cross-section may be about 2 to about 10 ㎛, for example, about 4 to about 8 ㎛. The glass fiber may have a length before processing of about 1 to about 30 mm, for example, about 2 to about 16 mm. In the above range, the productivity, impregnation property, etc. of the glass fiber composite material may be excellent.
[0047] In a specific example, the glass fiber may be treated with a conventional surface treatment agent. The surface treatment agent may include, but is not limited to, a silane compound, a urethane compound, an epoxy compound, or the like.
[0048] (b) polypropylene resin
[0049] According to one specific example of the present invention, a polypropylene resin can be impregnated with piperazine pyrophosphate, a phosphazene compound, and zeolite into the glass fiber to form a tape-shaped glass fiber composite material having excellent lightness, flame retardancy, impact resistance, rigidity, etc., and a polypropylene resin applied to a typical thermoplastic resin composition can be used.
[0050] In a specific example, the polypropylene resin may include at least one of a homopolypropylene resin, a block polypropylene resin, and a random polypropylene resin. Here, the block polypropylene resin may be a block polypropylene resin composed of a homopolypropylene block and an ethylene-propylene copolymer block and / or a homopolyethylene block, and the random polypropylene resin may be a propylene-ethylene random copolymer.
[0051] In a specific example, the polypropylene resin may have a melt flow index (MI) of about 1 to about 1,600 g / 10 min, for example, about 5 to about 1,400 g / 10 min, measured under conditions of 230°C and a load of 2.16 kg according to ASTM D1238. Within this range, the mechanical properties and molding processability of the glass fiber composite material may be excellent.
[0052] In a specific example, the polypropylene resin may be included in an amount of about 35 to about 72 parts by weight, for example, about 36 to about 70 parts by weight, based on about 100 parts by weight of the glass fiber. If the content of the polypropylene resin is less than about 35 parts by weight based on about 100 parts by weight of the glass fiber, there is a concern that manufacturing may be impossible due to single yarns of the glass fiber, or that the lightness, impregnation property, and formability of the glass fiber composite material may be reduced. If it exceeds about 72 parts by weight, there is a concern that the flame retardancy, impact resistance, and rigidity of the glass fiber composite material may be reduced.
[0053] (c) piperazine pyrophosphate
[0054] According to one specific example of the present invention, piperazine pyrophosphate can be impregnated into the glass fiber together with the polypropylene resin, the phosphazene compound, and the zeolite to form a tape-shaped glass fiber composite material having excellent lightness, flame retardancy, impact resistance, rigidity, etc., and piperazine pyrophosphate, which is a phosphorus-based flame retardant, can be used.
[0055] In a specific example, the piperazine pyrophosphate may be included in an amount of about 12 to about 35 parts by weight, for example, about 15 to about 33 parts by weight, based on about 100 parts by weight of the glass fiber. If the content of the piperazine pyrophosphate is less than about 12 parts by weight based on about 100 parts by weight of the glass fiber, there is a concern that the flame retardancy, etc. of the glass fiber composite material may be reduced, and if it exceeds about 35 parts by weight, there is a concern that the impact resistance, rigidity, formability, etc. of the glass fiber composite material may be reduced.
[0056] In a specific example, the weight ratio of the polypropylene resin and the piperazine pyrophosphate (polypropylene resin:piperazine pyrophosphate) may be from about 1:0.2 to about 1:1, for example from about 1:0.25 to about 1:0.90. In this range, the flame retardancy, impact resistance, rigidity, impregnation property, etc. of the glass fiber composite material may be more excellent.
[0057] (d) phosphazene compounds
[0058] According to one specific example of the present invention, a phosphazene compound can be impregnated into the glass fiber together with the polypropylene resin, the piperazine pyrophosphate, and the zeolite to form a tape-shaped glass fiber composite material having excellent lightness, flame retardancy, impact resistance, rigidity, etc., and a phosphazene compound used in a typical flame retardant thermoplastic resin composition can be used.
[0059] In a specific example, the phosphazene compound may include a phosphazene compound represented by the following chemical formula 1.
[0060] [Chemical Formula 1]
[0061]
[0062] In the above chemical formula 1, R1, R2, R3, R4, R5 and R6 are each independently a hydrogen atom, a halogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 7 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted heterocycloalkyl group having 2 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an aryl group or aryloxy group having 6 to 20 carbon atoms, a heteroaryl group having 5 to 20 carbon atoms, a substituted or unsubstituted alkoxycarbonylalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted carbonylalkyl group having 2 to 10 carbon atoms, an amino group or a hydroxy group.
[0063] Here, the above “substitution” means that a hydrogen atom is replaced with a substituent such as an alkyl group having 1 to 10 carbon atoms, a halogen atom, a nitro group, a cyano group, a hydroxy group, an amino group, an aryl group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a heterocycloalkyl group having 3 to 10 carbon atoms, a heteroaryl group having 4 to 10 carbon atoms, or a combination thereof.
[0064] In addition, the substituents including the above "alkyl", "alkoxy" and other "alkyl" moieties include both straight-chain and branched forms, "alkenyl" includes both straight-chain and branched forms having 2 to 8 carbon atoms and containing at least one double bond, and the above "cycloalkyl" includes all saturated monocyclic or saturated bicyclic ring structures having 3 to 20 carbon atoms. The above "aryl" is an organic radical having a ring structure derived from an aromatic hydrocarbon by removal of one hydrogen atom, and includes a single or fused ring system, suitably including 4 to 7, preferably 5 or 6 ring skeletal atoms in each ring. Specifically, phenyl, naphthyl, biphenyl, tolyl, etc. can be exemplified.
[0065] The above "heterocycloalkyl" means a cycloalkyl group containing 1 to 3 heteroatoms selected from N, O, and S as saturated cyclic hydrocarbon skeletal atoms, and the remaining saturated monocyclic or bicyclic ring skeletal atoms are carbon, and is selected from pyrrolidinyl, azetidinyl, pyrazolidinyl, oxazolidinyl, piperidinyl, piperazinyl, morpholinyl, thiomorpholinyl, thiazolidinyl, hydantoinyl, valerolactamyl, oxiranyl, oxetanyl, dioxolanyl, dioxanyl, oxathiolanyl, oxathianyl, dithianyl, dihydrofuranyl, tetrahydrofuranyl, dihydropyranyl, tetrahydropyranyl, tetrahydropyridinyl, tetrahydropyrimidinyl, tetrahydrothiophenyl, tetrahydrothiopyranyl, diazepanyl, Examples include azepanil.
[0066] The above "heteroaryl" refers to an aryl group having 1 to 3 heteroatoms selected from N, O, and S as aromatic ring skeletal atoms, and the remaining aromatic ring skeletal atoms are carbon, and the heteroaryl group includes a divalent aryl group in which the heteroatoms in the ring are oxidized or quaternized to form, for example, an N-oxide or a quaternary salt. Specifically, examples thereof include furyl, thienyl, pyrrolyl, pyranyl, imidazolyl, pyrazolyl, thiazolyl, thiadiazolyl, isothiazolyl, isoxazolyl, oxazolyl, oxadiazolyl, triazinyl, tetrazinyl, triazolyl, tetrazolyl, furazanyl, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, and the like.
[0067] In a specific example, the phosphazene compound may be included in an amount of about 1 to about 20 parts by weight, for example, about 2 to about 15 parts by weight, relative to about 100 parts by weight of the glass fiber. If the content of the phosphazene compound is less than about 1 part by weight relative to about 100 parts by weight of the glass fiber, there is a concern that the flame retardancy, etc. of the glass fiber composite material may be reduced, and if it exceeds about 20 parts by weight, there is a concern that the productivity, impact resistance, rigidity, etc. of the glass fiber composite material may be reduced.
[0068] In a specific example, the weight ratio of the piperazine pyrophosphate and the phosphazene compound (piperazine pyrophosphate:phosphazene compound) may be from about 1:0.1 to about 1:0.4, for example from about 1:0.13 to about 1:0.35. In this range, the flame retardancy, productivity, impregnation property, etc. of the glass fiber composite material may be more excellent.
[0069] (e) zeolite
[0070] Zeolite according to one specific example of the present invention can be impregnated with the glass fiber together with the polypropylene resin, the piperazine pyrophosphate, and the phosphazene compound to form a tape-shaped glass fiber composite material having excellent lightness, flame retardancy, impact resistance, rigidity, etc., and a zeolite used in a typical thermoplastic resin composition can be used.
[0071] In a specific example, the zeolite may be a porous particle having a pore size of about 2 to about 8 nm, for example, about 3 to about 6 nm, and an average particle size of about 1 to about 7 μm, for example, about 3 to about 5 μm. Within this range, the productivity, impregnation property, etc. of the glass fiber composite material may be excellent. Here, the average particle size of the zeolite was determined by obtaining a particle size distribution using a laser diffraction scattering method, and then the particle diameter at 50% of the accumulated value was taken as the average particle size.
[0072] In a specific example, the zeolite may be included in an amount of about 1 to about 20 parts by weight, for example, about 2 to about 15 parts by weight, relative to about 100 parts by weight of the glass fiber. If the content of the zeolite is less than about 1 part by weight relative to about 100 parts by weight of the glass fiber, there is a concern that the impact resistance, rigidity, etc. of the glass fiber composite material may be reduced, and if it exceeds about 20 parts by weight, there is a concern that the productivity, impregnation, etc. of the glass fiber composite material may be reduced.
[0073] In a specific example, the weight ratio of the polypropylene resin and the zeolite (polypropylene resin: zeolite) may be from about 1:0.05 to about 1:0.40, for example from about 1:0.06 to about 1:0.30. In this range, the impregnation property, impact resistance, rigidity, etc. of the glass fiber composite material may be more excellent.
[0074] A glass fiber composite material according to one specific example of the present invention may be in the form of a tape in which the glass fiber is impregnated with the polypropylene resin, the piperazine pyrophosphate, the phosphazene compound, and the zeolite, and may have a thickness of about 0.2 to about 1.5 mm, for example, about 0.3 to about 1.1 mm, and a width of about 5 to about 25 mm, for example, about 7 to about 20 mm. Within the above range, the flame retardancy, impact resistance, rigidity, etc. of the glass fiber composite material may be excellent.
[0075] In a specific example, the glass fiber composite material can be manufactured by a known manufacturing method, and for example, can be manufactured using a manufacturing device disclosed in Korean Patent Publication No. 10-2018-0035064.
[0076]
[0077] (B) Nonwoven fabric
[0078] A nonwoven fabric according to one specific example of the present invention can be applied together with the woven sheet to improve the appearance properties of a molded product, etc.
[0079] In a specific example, the nonwoven fabric may have a thickness of about 0.2 to about 1.5 mm, for example, about 0.5 to about 1.0 mm. Within this range, the final product may not experience peeling due to interface bonding issues with the woven sheet, and may exhibit excellent appearance properties.
[0080] In a specific example, the nonwoven fabric may be a polyethylene terephthalate nonwoven fabric. When a polyethylene terephthalate nonwoven fabric is used as the nonwoven fabric, the melting point is higher than that of the polypropylene resin, which is the base resin of the woven sheet, so that the shape of the nonwoven fabric can be maintained even during molding, and when manufacturing a molded product, the polypropylene resin of the melted woven sheet permeates the nonwoven fabric during the heating and compression process, thereby improving the bonding performance between the nonwoven fabric and the woven sheet. In addition, by permeating the flame retardant system (piperazine pyrophosphate, phosphazene compound, etc.) of the woven sheet into the nonwoven fabric together with the polypropylene resin, the flame retardancy of the woven sheet can also be shared. In other words, even if a non-flame retardant general nonwoven fabric is used instead of a flame retardant nonwoven fabric, the flame retardancy performance can be maintained.
[0081] In a specific example, the nonwoven fabric may be a conventional flame-retardant nonwoven fabric, for example, a flame-retardant polyethylene terephthalate nonwoven fabric. In this case, the flame-retardant properties of the molded product may be improved.
[0082]
[0083] A molded article according to one specific example of the present invention can be manufactured by laminating two or more thermoplastic continuous fiber reinforced woven fabrics, heating and compressing them to produce a woven sheet, and then laminating the nonwoven fabric on at least one side of the woven sheet, followed by heating and compressing the same. Such molding methods are well known to those skilled in the art to which the present invention pertains.
[0084] In a specific example, when manufacturing the woven sheet, heating and pressing may be performed by pressing with a pressing roller at about 180 to about 260°C, for example, pressing may be performed using a pressing roller or the like at about 230 to about 260°C. In the above temperature range, the peeling resistance, mechanical properties, etc. of the woven sheet may be excellent.
[0085] In a specific example, the heating and pressing after laminating the nonwoven fabric may be performed using a press molding machine at about 230 to about 260°C. Within this temperature range, the bonding performance of the woven sheet and the nonwoven fabric may be excellent, the woven sheet and the nonwoven fabric may share flame retardancy performance, and the appearance characteristics of the molded product may be excellent. The press molding machine may be a press molding machine of about 2,000 to about 3,000 tons, but is not limited thereto.
[0086] In a specific example, the molded article has a density of about 1.40 to about 1.55 g / cm as measured according to ISO 1183-1. 3 , for example, about 1.41 to about 1.54 g / cm 3 It could be.
[0087] In a specific example, the molded product may have a flame retardancy of V-1 or higher on a 2 mm thick specimen measured by the UL-94 vertical test method.
[0088] In a specific example, the molded article may have a peak force of about 3.5 to about 6.0 kN, for example, about 3.6 to about 5.0 kN, of a 60 mm × 60 mm × 2 mm specimen measured at a speed of 4.4 m / s and an impact energy value of 198 J based on a weight of 20 kg according to ISO 6603-2, a total displacement of about 20 to about 35 mm, for example, about 22 to about 35 mm, and an energy absorption at a displacement value of 15 mm of about 30 to about 50 J, for example, about 30 to about 45 J.
[0089] In a specific example, the molded article may have a tensile strength of about 180 to about 270 MPa, for example, about 181 to about 260 MPa, of a 3 mm thick specimen measured according to ISO 527.
[0090] In a specific example, the molded article may have a flexural strength of about 190 to about 280 MPa, for example, about 191 to about 270 MPa, of a 3 mm thick specimen measured according to ISO 14125.
[0091] In a specific example, the molded product may be capable of being extinguished spontaneously without catching fire in a long-term flame retardancy test in which a specimen measuring 330 mm × 330 mm × 2 mm is directly heated with a blue flame for 2 minutes and 10 seconds at a distance of 7 cm using a torch, and then the flame is removed.
[0092] In a specific example, the molded product has excellent properties such as light weight, flame retardancy, impact resistance, rigidity, appearance characteristics, and balance of these properties, and is therefore useful as interior and exterior materials for electronic devices, interior and exterior materials for automobiles, structural materials, and the like, and is particularly useful as a lower protective plate for a battery module for an electric vehicle.
[0093]
[0094] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.
[0095]
[0096] Example
[0097] Below, the specifications of each component used in the examples and comparative examples are as follows.
[0098] (A) Glass fiber
[0099] Circular cross-section glass fiber (Manufacturer: Owens Corning, Product Name: SE4121 HP) was used.
[0100] (B) Polypropylene resin
[0101] Homopolypropylene resin (Manufacturer: LG Chemical, Product Name: H7914A) was used.
[0102] (C) Phosphorus nitrogen compounds
[0103] (C1) Piperazine pyrophosphate (Manufacturer: Kempia, Product name: FR220N) was used.
[0104] (C2) Melamine pyrophosphate (Manufacturer: Kempia, Product name: MPP-D) was used.
[0105] (D) Inheritance compound
[0106] (D1) Phosphazene compound (Manufacturer: Kempia, Product name: FRPPZ) was used.
[0107] (D2) Bisphenol-A diphosphate (manufacturer: Jiangsu Yoke Technology, product name: Yoke BDP) was used.
[0108] (E) Zeolite
[0109] Zeolite (Manufacturer: Huin Chemical, Product Name: APS 30) was used.
[0110]
[0111] Examples 1 to 3 and Comparative Examples 1 to 6
[0112] Using the above-mentioned components in the amounts as described in Tables 1 and 2 below, glass fibers were impregnated with polypropylene resin, phosphorus-based compounds (piperazine pyrophosphate or melamine pyrophosphate), phosphorus-based compounds (phosphazene compounds or bisphenol-A diphosphate), and zeolite to manufacture a tape-shaped glass fiber composite material (continuous fiber-reinforced composite material (CFT)) having a thickness of about 0.4 mm and a width of about 11 mm by a known method, and the manufactured glass fiber composite material was woven using weft and warp yarns, such that a void space of about 2 mm × about 2 mm or less in size was formed between the glass fiber composite materials, thereby manufacturing a thermoplastic continuous fiber-reinforced woven body.
[0113] Next, after laminating several sheets of the thermoplastic continuous fiber reinforced woven fabric according to the thickness of the specimen, a polyethylene terephthalate nonwoven fabric (manufacturer: Hoan, product name: Chemical Nonwoven Fabric) was laminated on one side (the side visible to the outside after molding) of the woven fabric laminated sheet according to whether or not a nonwoven fabric was applied in Tables 1 and 2 below, and after preheating before molding, a flat molded product was manufactured by compression molding with a hot press and a cooling press, and a numerically controlled machine tool (NC machine) was used to cut the product to meet the specifications to manufacture a specimen for measuring the physical properties. The physical properties of the manufactured specimen for measuring the physical properties were evaluated by the following method, and the results are shown in Tables 1 and 2 below.
[0114]
[0115] Method of measuring physical properties
[0116] (1) Lightness: Density (unit: g / cm) according to ISO 1183-1 3 ) was measured.
[0117] (2) Flame retardancy: The flame retardancy (unit: grade) of a 2 mm thick specimen was measured using the UL-94 vertical test method.
[0118] (3) Impact resistance: According to ISO 6603-2, the surface impact strength was measured by measuring the peak force (unit: kN), total displacement (unit: mm), and energy absorption (unit: J) at 15 mm displacement of a 60 mm × 60 mm × 2 mm specimen at a speed of 4.4 m / s and an impact energy value of 198 J based on a weight of 20 kg.
[0119] (4) Stiffness: The tensile strength (unit: MPa) of a 3 mm thick specimen was measured according to ISO 527.
[0120] (5) Stiffness: The flexural strength (unit: MPa) of a 3 mm thick specimen was measured according to ISO 14125.
[0121] (6) Long-term flame retardancy: A long-term flame retardancy test was conducted by directly heating a 330 mm × 330 mm × 2 mm specimen with a blue flame at a distance of 7 cm for 2 minutes and 10 seconds using a torch, and then removing the flame. If the specimen did not catch fire after the flame was removed and extinguished spontaneously, it was evaluated as Pass, and if the specimen caught fire, it was evaluated as Fail.
[0122] (7) Appearance characteristics: The appearance of the molded product was visually evaluated to check for protrusion of glass fibers, tearing of non-woven fabric, exposure of woven laminated sheets, and occurrence of cracks / breakage.
[0123]
[0124] Example 123 (A) (parts by weight) 100 100 100 (B) (parts by weight) 45.55 4.550 (C1) (parts by weight) 25.51 8.230 (C2) (parts by weight) --- (D1) (parts by weight) 3.6 5.510 (D2) (parts by weight) --- (E) (parts by weight) 7.3 3.6 10 Non-woven fabric application application application application density (g / cm) 3 )1.511.471.45Flammability (Grade)V-0V-1V-1Peak Force (kN)4.44.23.7Total Displacement (mm)262832Energy Absorption @ 15 mm (J)423932Tensile Strength (MPa)245205185Flexural Strength (MPa)274220215Long-Term Flame RetardancyPassPassPassAppearance CharacteristicsPassPassPass
[0125]
[0126] Comparative Example 123456 (A) (parts by weight) 100 100 100 100 100 100 (B) (parts by weight) 31.77 3.36 6.74 5.55 4.54 1.8 (C1) (parts by weight) 25 31.13 7.8--30.9 (C2) (parts by weight)---7.35.5-(D1) (parts by weight) 58.9 8.9--9.1 (D2) (parts by weight)---21.81 8.2-(E) (parts by weight) 58.9 8.9 7.33.6- Non-woven fabric application Not applied Not applied Not applied Not applied Not applied Not applied Density (g / cm) 3)Not manufacturable1.411.43Not manufacturable1.52Flammability (grade)FailV-1V-1Peak force (kN)3.32.83.3Total displacement (mm)383736Energy absorption @ 15 mm (J)272829Tensile strength (MPa)165170171Flexural strength (MPa)173171166Long-term flame retardancyFailPassPassAppearance evaluationFailFailFail
[0127]
[0128] From the above results, it can be seen that the glass fiber composite material, thermoplastic continuous fiber reinforced woven fabric and molded article of the present invention are all excellent in terms of lightness (density), flame retardancy, impact resistance (peak force, total displacement, energy absorption at 15 mm displacement value), rigidity (tensile strength, flexural strength), appearance characteristics, and balance of these physical properties.
[0129] On the other hand, in the case of Comparative Example 1, where a small amount of polypropylene resin was applied, the friction between the nozzle and the glass fiber increased, resulting in glass fiber breakage, making it impossible to manufacture a tape-shaped glass fiber composite material. In the case of Comparative Example 2, where an excessive amount of polypropylene resin was applied, it was found that flame retardancy, impact resistance, rigidity, etc. were reduced. In the case of Comparative Example 3, where an excessive amount of piperazine pyrophosphate was applied, it was found that impact resistance, rigidity, etc. were reduced. In the case of Comparative Examples 4 and 5, where melamine pyrophosphate (C2) and bisphenol-A diphosphate (D2) were applied instead of the piperazine pyrophosphate and phosphazene compound of the present invention, respectively, it was impossible to manufacture a tape-shaped glass fiber composite material due to increased viscosity and decreased wetting properties. In the case of Comparative Example 6, where zeolite was not applied, it was found that impact resistance, rigidity, etc. were reduced. In addition, since Comparative Examples 2, 3, and 6 did not apply non-woven fabric, the woven sheet was exposed, and accordingly, it can be seen that the appearance characteristics were deteriorated, such as glass fibers protruding from the surface of the molded product specimen for measuring physical properties.
[0130]
[0131] The present invention has been described with reference to exemplary embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.
Claims
A woven sheet comprising 1.2 or more layers of thermoplastic continuous fiber reinforced woven fabrics; and A nonwoven fabric laminated by heating and pressing on at least one side of the above woven sheet; The thermoplastic continuous fiber reinforced woven fabric is characterized by being woven using a glass fiber composite material as warp and weft yarns, wherein the glass fiber composite material comprises about 100 parts by weight of glass fiber; about 35 to about 72 parts by weight of polypropylene resin; about 12 to about 35 parts by weight of piperazine pyrophosphate; about 1 to about 20 parts by weight of phosphazene compound; and about 1 to about 20 parts by weight of zeolite.
2. A molded product according to claim 1, characterized in that the polypropylene resin comprises at least one of homo polypropylene resin, block polypropylene resin, and random polypropylene resin.
3. A molded product according to claim 1 or 2, characterized in that the weight ratio of the piperazine pyrophosphate and the phosphazene compound is about 1:0.1 to about 1:0.
4.
4. A molded product according to any one of claims 1 to 3, wherein the glass fiber composite material is in the form of a tape in which the glass fiber is impregnated with the polypropylene resin, the piperazine pyrophosphate, the phosphazene compound, and the zeolite.
5. A molded product according to any one of claims 1 to 4, wherein the glass fiber composite material is in the form of a tape having a thickness of about 0.2 to about 1.5 mm and a width of about 5 to about 25 mm.
6. A molded product according to any one of claims 1 to 5, wherein the thermoplastic continuous fiber reinforced woven fabric has a void space of about 5 mm × about 5 mm or less in size formed between the warp and warp yarns and between the weft and weft yarns.
7. A molded product according to any one of claims 1 to 6, characterized in that the nonwoven fabric is a polyethylene terephthalate nonwoven fabric having a thickness of about 0.2 to about 1.5 mm.
8. In any one of paragraphs 1 to 7, the molded product has a density of about 1.40 to about 1.55 g / cm as measured according to ISO 1183-1. 3 A molded product characterized by:
9. A molded product according to any one of clauses 1 to 8, characterized in that the molded product has a flame retardancy of V-1 or higher on a 2 mm thick specimen measured by the UL-94 vertical test method.
10. A molded product according to any one of claims 1 to 9, characterized in that the molded product has a peak force of about 3.5 to about 6.0 kN, a total displacement of about 20 to about 35 mm, and an energy absorption at a displacement value of 15 mm, measured at an impact energy value of 198 J based on a speed of 4.4 m / s and a weight of 20 kg in accordance with ISO 6603-2, of a 60 mm × 60 mm × 2 mm specimen.
11. A molded product according to any one of claims 1 to 10, characterized in that the molded product has a tensile strength of about 180 to about 270 MPa for a 3 mm thick specimen measured according to ISO 527, and a flexural strength of about 190 to about 280 MPa for a 3 mm thick specimen measured according to ISO 14125.
12. A molded product according to any one of claims 1 to 11, characterized in that the molded product does not catch fire and is extinguished naturally in a long-term flame retardancy test in which a specimen measuring 330 mm × 330 mm × 2 mm is directly heated with a blue flame for 2 minutes and 10 seconds at a distance of 7 cm using a torch, and then the flame is removed.
13. A molded product according to any one of claims 1 to 12, characterized in that the molded product is a lower protective plate of a battery module for an electric vehicle.
14. Laminating two or more thermoplastic continuous fiber reinforced woven fabrics, heating and compressing to produce a woven fabric sheet; and A step of laminating a nonwoven fabric on at least one side of the above woven sheet, and then heating and pressing it; A method for manufacturing a molded article, characterized in that the thermoplastic continuous fiber reinforced woven fabric is woven using a glass fiber composite material including about 100 parts by weight of glass fiber; about 35 to about 72 parts by weight of polypropylene resin; about 12 to about 35 parts by weight of piperazine pyrophosphate; about 1 to about 20 parts by weight of a phosphazene compound; and about 1 to about 20 parts by weight of zeolite as warp and weft yarns.
Citation Information
Patent Citations
Apparatus for manufacturing long fiber reinforced thermoplastic
KR1020180035064A
Mouse holder
KR1020210117502A
Manufacturing method of high temperature resistant sound absorbing materials for vehicle
KR101417394B1
Improved flame retardant polymer compositions
KR101939228B1
Nonflammable Material for Outdoor
KR102423133B1